Polymer Composite for Battery Thermal Barrier, Composite Hydrogel-Based Fire-Resistant Pressure Pad Including the Same, Method of Manufacturing the Pad, and Battery Module Including the Pad
A polymer composite with dual network structure and crosslinks addresses the limitations of conventional insulators by providing thermal insulation, flame retardancy, and mechanical support to prevent thermal runaway in battery modules.
Patent Information
- Application Number
- KR1020260130839
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-07-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-07-15
AI Technical Summary
Conventional insulating materials and hydrogels fail to simultaneously provide effective heat absorption, flame retardancy, and surface pressure responsiveness during thermal runaway in battery modules, leading to potential fire or explosion risks.
A polymer composite comprising anionic and nonionic hydrophilic polymers, flame-retardant inorganic fillers, and additives, forming a dual network structure with physical and chemical crosslinks, which maintains a gel or porous solid state to suppress thermal runaway and accommodate cell expansion.
The composite provides simultaneous thermal insulation, flame retardancy, and mechanical reinforcement, effectively suppressing thermal runaway propagation and maintaining surface pressure between battery cells.
Smart Images

Figure 112026086577173-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a polymer composite for battery heat insulation, a composite hydrogel-based pressure-resistant pad including the same, a method for manufacturing the pad, and a battery module including the pad. Background Technology
[0003] Lithium-ion batteries are used in various fields, such as electric vehicles, energy storage devices, and portable electronic devices, due to their high energy density and excellent output characteristics. In particular, in applications requiring high output and capacity, such as electric vehicles or energy storage devices, multiple battery cells are electrically connected to form battery modules or battery packs.
[0004] However, lithium secondary batteries can generate abnormal heat due to various causes such as overcharging, internal short circuits, external impacts, manufacturing defects, overcurrents, and high-temperature environments. If this heat generation progresses beyond a certain level, a chain reaction of electrolyte decomposition, electrode reactions, gas generation, and pressure rise may occur, leading to thermal runaway.
[0005] Since multiple battery cells are densely arranged in a battery module or battery pack, if thermal runaway occurs in any one battery cell, heat and flames can propagate to adjacent battery cells. Consequently, there is a risk that abnormal heating in a single cell could escalate into a fire or explosion of the entire battery module or battery pack.
[0006] To address these problems, techniques have been proposed to place insulating materials, inorganic fibers, mica sheets, aerogel sheets, flame-retardant resin pads, or moisture-containing heat-absorbing materials between battery cells. However, while simple inorganic insulating materials may offer excellent heat insulation at high temperatures, their ability to endothermally mitigate the initial temperature rise is limited. Additionally, while simple moisture-containing hydrogels can be expected to provide an initial endothermic effect due to moisture vaporization, structural stability or continuous heat insulation may deteriorate after the moisture is lost.
[0007] In addition, pads placed between battery cells need not only suppress the propagation of thermal runaway but also accommodate the expansion of battery cells due to charging, discharging, or aging, and maintain stable surface pressure between cells. However, conventional simple thermal insulation sheets or simple hydrogel materials have limitations in simultaneously satisfying heat absorption, flame retardancy, heat insulation, and surface pressure responsiveness in a thermal runaway environment.
[0008] Accordingly, a new fireproof pad is required that can be placed between battery cells or modules, absorbs heat through the vaporization of moisture during the initial stage of thermal runaway, forms a carbonized layer or ceramic shielding film using flame-retardant additives and inorganic fillers in high-temperature environments, and maintains a gel state or porous solid state even when deformed by external forces.
[0009] The aforementioned background technology is one that the inventor possessed or acquired in the process of deriving the disclosure of the present invention, and it cannot be considered as prior art disclosed to the general public prior to the filing of this application. The problem to be solved
[0011] The present invention aims to solve the aforementioned problems, and the objective of the present invention is to provide a polymer composite for battery thermal insulation that can be applied between battery cells or battery modules to simultaneously secure thermal runaway propagation suppression performance and surface pressure response performance.
[0012] Another objective of the present invention is to provide a composite hydrogel-based pressure-resistant pad that can accommodate compressive deformation due to cell expansion between battery cells while suppressing the propagation of heat, flames, and high-temperature gases during battery thermal runaway.
[0013] Another objective of the present invention is to provide a method for manufacturing a composite hydrogel-based refractory pressure pad having shape retention, moisture retention, and thermal runaway propagation suppression performance by uniformly dispersing a flame-retardant inorganic filler and a flame-retardant additive within a hydrophilic polymer network and inducing physical crosslinking and chemical crosslinking together.
[0014] Another objective of the present invention is to provide a battery module that can mitigate changes in surface pressure due to cell expansion during normal operation and suppress the propagation of thermal runaway to adjacent cells in abnormal thermal runaway situations by placing a composite hydrogel-based surface pressure-resistant pad between adjacent battery cells.
[0015] However, the problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below. means of solving the problem
[0017] A polymer composite for battery heat insulation according to one embodiment of the present invention comprises: a first anionic hydrophilic polymer comprising a carboxyl group, a sulfonic acid group, a phosphate group, or a salt thereof; a second nonionic or weakly ionic hydrophilic polymer that is mixable with the first polymer; a flame-retardant inorganic filler; a flame-retardant additive; and water; wherein the first polymer and the second polymer form a polymer network that retains the water, the flame-retardant inorganic filler is dispersed within the polymer network, the inorganic thermal insulation material and a ceramicization-inducing material are included, the flame-retardant additive is dispersed within the polymer network, and the polymer composite is provided in a water-containing hydrogel state or in a dry state from which at least a portion of the water is removed from the polymer composite in the water-containing hydrogel state, the polymer composite in the water-containing hydrogel state maintains a gel state at room temperature, and the polymer composite in the dry state maintains a porous solid state at room temperature.
[0018] In one embodiment, the anionic hydrophilic first polymer may comprise at least one selected from the group consisting of cellulose derivatives, alginate, polyacrylic polymers, polymethacrylic copolymers, polyvinylsulfonic acid, and polystyrenesulfonic acid.
[0019] In one embodiment, the nonionic or weakly ionic hydrophilic second polymer may comprise at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, hydroxyethylcellulose, hydroxypropylcellulose, and polyvinylamine.
[0020] In one embodiment, the first polymer and the second polymer may form a dual network structure in which physical crosslinking and chemical crosslinking are combined.
[0021] In one embodiment, the physical crosslink may include a metal ion-mediated ion crosslink, a dynamic borate ester crosslink, or both.
[0022] In one embodiment, the chemical crosslink is induced by a chemical component, and the metal ion-mediated ion crosslink may include at least one selected from the group consisting of calcium ions, magnesium ions, aluminum ions, iron ions, and zinc ions.
[0023] In one embodiment, the dynamic borate ester crosslink may be formed by a reaction between boric acid, borate, or a combination thereof and a hydroxyl group contained in the first polymer or the second polymer.
[0024] In one embodiment, the chemical crosslinking component may include an organic acid, a radical initiator, a polyfunctional crosslinking agent, or a combination thereof.
[0025] In one embodiment, the chemical crosslinking component may include ammonium persulfate, methylenebisacrylamide, or a combination thereof.
[0026] In one embodiment, the flame-retardant inorganic filler may comprise at least one selected from the group consisting of silica, silica aerogel, aluminosilicate, mica, clay, aluminum oxide, magnesium oxide, zirconium oxide, glass frit, and calcium phosphate-based compounds.
[0027] In one embodiment, the calcium phosphate-based compound comprises hydroxyapatite, tricalcium phosphate, or a mixture thereof, and the calcium phosphate-based compound may be softened, melted, or sintered in a high-temperature environment caused by battery thermal runaway to form an inorganic ceramic shielding film by combining with the inorganic insulating material.
[0028] In one embodiment, the flame retardant additive may comprise at least one selected from the group consisting of phosphorus-based flame retardants, nitrogen-based flame retardants, metal hydroxide-based flame retardants, phosphorus and nitrogen-based inflatable flame retardants, and condensation-type flame retardants comprising phosphorus, nitrogen, and carbon.
[0029] In one embodiment, the flame-retardant additive may perform at least one flame-retardant action among a dehydration reaction, release of non-combustible gas, foaming, or formation of a carbonized layer upon exposure to a flame.
[0030] In one embodiment, the content of the flame-retardant inorganic filler may be 10 to 300 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer.
[0031] In one embodiment, the content of the flame-retardant additive may be 3 to 200 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer.
[0032] In one embodiment, the water content may be 10 to 95 parts by weight based on 100 parts by weight of the total composition.
[0033] In one embodiment, the polymer composite for battery heat insulation has a porous structure containing pores of 1 nm to 500 μm inside, and the porosity of the polymer composite in a dry state may be 10 volume% to 90 volume%.
[0034] In one embodiment, the polymer composite for battery heat insulation may be capable of reabsorbing moisture at least 10 times its own mass at 23°C and 50% relative humidity.
[0035] A composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention comprises a polymer composite for battery heat insulation according to one embodiment of the present invention and is placed between cells or modules of a lithium battery to control thermal runaway.
[0036] In one embodiment, the polymer composite for battery heat insulation may be in the form of a composite infiltrated or impregnated into a sheet or nonwoven fabric composed of glass fiber, ceramic fiber, carbon fiber, aramid fiber, polyolefin fiber, polyester fiber, or a mixture thereof.
[0037] In one embodiment, the composite hydrogel-based pressure-resistant pad may have a thickness of 0.5 mm to 10 mm.
[0038] A method for manufacturing a composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention comprises: a step of preparing a polymer mixture comprising an anionic hydrophilic first polymer comprising a carboxyl group, a sulfonic acid group, a phosphate group, or a salt thereof, and a nonionic or weakly ionic hydrophilic second polymer that is mixable with said first polymer; a step of preparing a hydrogel precursor composition by dispersing a flame-retardant inorganic filler comprising an inorganic thermal insulation material and a ceramicization-inducing material and a flame-retardant additive in said polymer mixture; a step of supplying said hydrogel precursor composition in a sheet shape or infiltrating or impregnating it into a sheet or nonwoven fabric; and a step of forming a composite hydrogel-based pressure-resistant pad in a moisture-containing hydrogel state by inducing physical crosslinking and chemical crosslinking in said hydrogel precursor composition supplied in a sheet shape or infiltrating or impregnating it into said sheet or nonwoven fabric.
[0039] In one embodiment, the step of preparing the polymer mixture may include adding 3 to 5 parts by weight of carboxymethylcellulose and 5 to 8 parts by weight of polyvinyl alcohol to 87 to 92 parts by weight of water, and then stirring at 50°C to 80°C for 0.5 to 1 hour.
[0040] In one embodiment, the step of forming the composite hydrogel-based pressure-resistant pad may include: a step of forming a physical crosslink to at least one of the first polymer and the second polymer using a metal ion or a borate; and a step of forming a chemical crosslink to at least one of the first polymer and the second polymer using a chemical crosslinking component.
[0041] A battery module according to another embodiment of the present invention comprises: a plurality of battery cells; and a composite hydrogel-based pressure-resistant pad according to one embodiment of the present invention disposed between adjacent battery cells among the plurality of battery cells.
[0042] In one embodiment, the plurality of battery cells are lithium secondary battery cells, and the polymer composite for battery thermal insulation may accommodate compressive deformation due to cell expansion between adjacent battery cells while suppressing the propagation of heat and flame during thermal runaway. Effects of the invention
[0044] Unlike simple moisture-containing hydrogels or simple inorganic thermal insulation materials, the polymer composite for battery thermal insulation according to one embodiment of the present invention can simultaneously secure a temperature rise suppression effect due to moisture vaporization, a flame-retardant effect due to a flame-retardant additive, a high-temperature thermal insulation effect due to a flame-retardant inorganic filler, and shape retention in a moisture-containing hydrogel state or a dry state. Accordingly, the polymer composite can improve thermal runaway propagation suppression performance, handling, and assembly stability as a material for a pressure-resistant pad applied between battery cells or modules.
[0045] A composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention can simultaneously secure the action of suppressing temperature rise caused by moisture vaporization of a polymer composite for battery heat insulation, the action of flame retardant by a flame-retardant additive, the action of high-temperature heat insulation by a flame-retardant inorganic filler, and mechanical reinforcement by a fiber sheet or nonwoven fabric. Accordingly, the composite hydrogel-based pressure-resistant pad can stably maintain surface pressure between battery cells while effectively suppressing the propagation of heat, flames, and high-temperature gases in the event of thermal runaway.
[0046] A method for manufacturing a composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention can produce a pad having moisture retention, shape retention, tolerance to compression deformation, and thermal runaway propagation suppression performance by uniformly dispersing a flame-retardant inorganic filler and a flame-retardant additive within a polymer network composed of a hydrophilic first polymer and a hydrophilic second polymer, and inducing both physical and chemical crosslinking. Additionally, by infiltrating or impregnating a fiber sheet or nonwoven fabric as needed, or by converting it into a dry body, it is possible to simultaneously secure handling properties, mechanical reinforcement, and high-temperature heat insulation suitable for battery module assembly processes.
[0047] A battery module according to another embodiment of the present invention can accommodate compressive deformation due to cell expansion and improve surface pressure uniformity between cells during normal operation by placing a composite hydrogel-based pressure-resistant pad between adjacent battery cells, and can suppress the propagation of heat, flame, and high-temperature gas in abnormal thermal runaway situations. Accordingly, the battery module can simultaneously improve cell stacking stability, thermal management stability, and thermal runaway propagation suppression performance. Brief explanation of the drawing
[0049] FIG. 1 is a flowchart illustrating a method for manufacturing a composite hydrogel-based pressure-resistant pad according to one embodiment of the present invention. Specific details for implementing the invention
[0050] Hereinafter, embodiments are described in detail with reference to the attached drawings. However, various modifications may be made to the embodiments, and thus the scope of the patent application is not limited or restricted by these embodiments. It should be understood that all modifications, equivalents, and substitutions to the embodiments are included within the scope of the rights.
[0051] The terms used in the embodiments are for illustrative purposes only and should not be interpreted as intended to be limiting. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as "comprising" or "having" are intended to indicate the existence of the features, numbers, steps, actions, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof.
[0052] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the embodiments pertain. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this application.
[0054] In addition, when describing with reference to the attached drawings, identical components are assigned the same reference numeral regardless of drawing symbols, and redundant descriptions thereof are omitted. In describing the embodiments, if it is determined that a detailed description of related prior art could unnecessarily obscure the essence of the embodiments, such detailed description is omitted.
[0055] In addition, terms such as first, second, A, B, (a), (b), etc. may be used when describing the components of the embodiments. These terms are used merely to distinguish the components from other components, and the essence, order, or sequence of the components is not limited by the terms.
[0056] Components included in any one embodiment and components having common functions shall be described using the same names in other embodiments. Unless otherwise stated, the description in any one embodiment may also apply to other embodiments, and specific descriptions shall be omitted to the extent of overlap.
[0057] In this specification, the term "pressure-resistant pad" may refer to a pad-shaped member disposed between battery cells or battery modules to accommodate compressive deformation resulting from the expansion of battery cells or to buffer or maintain surface pressure, thereby suppressing the propagation of heat, flames, and high-temperature gases during battery thermal runaway. Accordingly, the pressure-resistant pad may perform both the function of a fire-resistant pad that provides heat insulation or flame retardant functions and the function of a surface pressure pad that controls or buffers surface pressure between battery cells.
[0059] Hereinafter, the polymer composite for battery thermal insulation, the method for manufacturing the same, and the battery module including the same according to the present invention will be described in detail with reference to the examples and drawings. However, the present invention is not limited to these examples and drawings.
[0061] A polymer composite for battery heat insulation according to one embodiment of the present invention may comprise an anionic hydrophilic first polymer comprising a carboxyl group, a sulfonic acid group, a phosphate group, or a salt thereof, a nonionic or weakly ionic hydrophilic second polymer that is mixable with the first polymer, a flame-retardant inorganic filler, a flame-retardant additive, and water.
[0062] The first polymer and the second polymer may form a polymer network that retains water. The flame-retardant inorganic filler may be dispersed within the polymer network and may include an inorganic insulating material and a ceramicization-inducing material. The flame-retardant additive may be dispersed within the polymer network.
[0063] The polymer composite is provided in a water-containing hydrogel state or in a dry state from which at least a portion of the water is removed from the polymer composite in the water-containing hydrogel state, and the polymer composite in the water-containing hydrogel state maintains a gel state at room temperature, and the polymer composite in the dry state maintains a porous solid state at room temperature.
[0064] The above-mentioned anionic hydrophilic first polymer may include carboxyl groups, sulfonic acid groups, phosphate groups, or salts thereof. By including these, it has excellent affinity for water and can interact with metal ions or other crosslinking components. Accordingly, the first polymer can improve the water retention, ionic crosslinking, and gel-forming properties of the polymer composite.
[0065] The above-mentioned anionic hydrophilic first polymer may include at least one selected from the group consisting of cellulose derivatives, alginates, polyacrylic polymers, polymethacrylic copolymers, polyvinylsulfonic acid, and polystyrenesulfonic acid.
[0066] For example, the cellulose derivative may include carboxymethylcellulose, carboxyethylcellulose, or salts thereof. The alginate may include sodium alginate, calcium alginate, or a combination thereof. The polyacrylic polymer may include polyacrylic acid, polyacrylate, polyacrylic acid copolymer, or a combination thereof.
[0067] The above nonionic or weakly ionic hydrophilic second polymer can be mixed with the first polymer to complement the mechanical stability, film-forming ability, compression recovery ability, and moisture retention ability of the polymer network.
[0068] The second polymer can form hydrogen bonds, chain entanglements, physical crosslinking, or chemical crosslinking with the first polymer, and accordingly, shape stability against external forces can be improved compared to a single polymer-based hydrogel.
[0069] The above nonionic or weakly ionic hydrophilic second polymer may include at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, hydroxyethylcellulose, hydroxypropylcellulose, and polyvinylamine.
[0070] In one embodiment, the weight ratio of the first polymer and the second polymer may be 10:90 to 90:10, and preferably 30:70 to 70:30. If the content of the first polymer is excessively low, the ionic crosslinkability or moisture retention may not be sufficient, and if the content of the second polymer is excessively low, mechanical stability or film formation ability may be reduced.
[0071] The first polymer and the second polymer can form a dual network structure in which physical crosslinking and chemical crosslinking are combined.
[0072] The physical crosslinking may include metal ion-mediated ionic crosslinking, dynamic borate ester crosslinking, or both. The metal ion-mediated ionic crosslinking may be formed by ionic or coordinate bonding between a metal ion and a carboxyl group, sulfonic acid group, phosphate group, or salt thereof contained in the first polymer. The metal ion-mediated ionic crosslinking may be formed by at least one selected from the group consisting of calcium ions, magnesium ions, aluminum ions, iron ions, and zinc ions. The metal ions may be provided in the form of chlorides, nitrates, sulfates, lactates, gluconates, or acetates, but are not limited thereto.
[0073] The dynamic borate ester crosslink above can be formed by a reaction between boric acid, borate, or a combination thereof and a hydroxyl group included in the first polymer or the second polymer. For example, if the second polymer includes polyvinyl alcohol, a dynamic borate ester bond can be formed between the hydroxyl group of polyvinyl alcohol and boric acid or borate. Since such a dynamic crosslink can be temporarily dissociated by an external force and then re-bonded, it can improve the deformation responsiveness, self-healing ability, and compression recovery ability of the polymer composite.
[0074] The above chemical crosslinking may be induced by a chemical crosslinking component. The chemical crosslinking component may include an organic acid, a radical initiator, a polyfunctional crosslinking agent, or a combination thereof. For example, the chemical crosslinking component may include ammonium persulfate, methylenebisacrylamide, or a combination thereof.
[0075] The above organic acid may include citric acid, tartaric acid, malic acid, succinic acid, glutaric acid, adipic acid, oxalic acid, or a combination thereof.
[0076] The chemical crosslinking component can provide chemical bonding points or crosslinking points between the first polymer or the second polymer, and accordingly, can improve the structural stability, gel state retention, and shape retention in a repeated compression environment of the polymer network.
[0077] The flame-retardant inorganic filler may be dispersed in the first polymer and the second polymer. The flame-retardant inorganic filler may function as an inorganic insulating material that blocks or delays the heat conduction path of the polymer composite, and simultaneously function as a ceramicization-inducing material to form an inorganic shielding layer or a ceramic shielding film in a high-temperature environment. The flame-retardant inorganic filler may be provided in the form of a single particle that simultaneously performs the functions of an inorganic insulating material and a ceramicization-inducing material, or in the form of a mixture of a particle functioning as an inorganic insulating material and a particle functioning as a ceramicization-inducing material.
[0078] The flame-retardant inorganic filler may comprise at least one selected from the group consisting of silica, silica aerogel, aluminosilicate, mica, clay, aluminum oxide, magnesium oxide, zirconium oxide, glass frit, and calcium phosphate-based compounds. The silica or silica aerogel may improve thermal insulation through low thermal conductivity and a porous structure. The aluminosilicate, mica, or clay may improve heat insulation by increasing the path of heat and flame movement through a layered or plate-like structure. The aluminum oxide, magnesium oxide, or zirconium oxide may improve the structural stability of the inorganic residue layer in a thermal runaway environment due to its excellent high-temperature stability. The glass frit may soften or melt at high temperatures and act as a binder to bind surrounding inorganic particles.
[0079] The calcium phosphate-based compound may include hydroxyapatite, tricalcium phosphate, or a mixture thereof. The calcium phosphate-based compound may be softened, melted, or sintered in a high-temperature environment caused by battery thermal runaway to form an inorganic ceramic shield by combining with the inorganic insulating material. The inorganic ceramic shield may remain even after the moisture in the hydrogel has vaporized, thereby physically blocking or delaying the movement of heat, flame, high-temperature gas, or molten material.
[0080] The flame-retardant additive may be dispersed in the first polymer and the second polymer. When exposed to flame or high temperature, the flame-retardant additive may perform a flame-retardant action according to the type of flame retardant, such as a dehydration reaction, a foaming reaction, the release of non-combustible gas, the formation of a carbonized layer, or a combination thereof. Accordingly, the flame-retardant additive may suppress the temperature rise during the initial stages of battery thermal runaway and delay the combustion or decomposition of the polymer network in a high-temperature environment.
[0081] The flame retardant additive may include at least one selected from the group consisting of phosphorus-based flame retardants, nitrogen-based flame retardants, metal hydroxide-based flame retardants, phosphorus and nitrogen-based inflatable flame retardants, and condensation-type flame retardants containing phosphorus, nitrogen, and carbon. For example, the phosphorus-based flame retardant may include phosphates, polyphosphates, organophosphorus compounds, or combinations thereof. The nitrogen-based flame retardant may include melamine, melamine cyanurate, melamine phosphate, guanidine-based compounds, or combinations thereof. The metal hydroxide-based flame retardant may include aluminum hydroxide, magnesium hydroxide, or combinations thereof. The phosphorus and nitrogen-based inflatable flame retardant may include an inflatable flame retardant system comprising an acid source, a foaming source, and a carbon source. The condensation-type flame retardant containing phosphorus, nitrogen, and carbon may include a condensation-reactive flame retardant system capable of forming a carbonized layer or an expanded carbonized layer at high temperatures.
[0082] The flame-retardant additive may release water vapor or form a carbon layer through a dehydration reaction upon exposure to a flame. The water vapor may lower the temperature around the flame, dilute the concentration of oxygen or flammable gases, and suppress the combustion of high-temperature gases generated by thermal runaway. The carbon layer may be formed on or inside the polymer composite to delay heat transfer and, together with the flame-retardant inorganic filler, form a composite shielding layer. In one embodiment, the hydroxycarbonate-based flame retardant may release moisture or carbon dioxide as it decomposes at high temperatures and may contribute to the formation of a heat-insulating layer or an inorganic residual layer by forming residual inorganic components after decomposition.
[0083] The content of the flame-retardant inorganic filler may be 10 to 300 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer. For example, the content of the flame-retardant inorganic filler may be 20 to 280 parts by weight, 30 to 250 parts by weight, 40 to 220 parts by weight, 50 to 200 parts by weight, 60 to 180 parts by weight, 70 to 160 parts by weight, or 80 to 150 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer.
[0084] If the content of the flame-retardant inorganic filler is less than 10 parts by weight, it may be difficult to secure sufficient thermal insulation, inorganic residual layer formation, or ceramic shielding film formation. If the content of the flame-retardant inorganic filler exceeds 300 parts by weight, the gel formation, flexibility, compression recovery, or moisture retention of the polymer composite may be reduced.
[0085] In one embodiment, when the content of the flame-retardant inorganic filler is 30 to 250 parts by weight, the inorganic thermal insulation and the shape stability of the polymer network can be secured in a balanced manner. In another embodiment, when the content of the flame-retardant inorganic filler is 50 to 200 parts by weight, the formation ability of the inorganic residual layer or inorganic ceramic shielding film in a high-temperature environment due to battery thermal runaway can be improved. In yet another embodiment, when the content of the flame-retardant inorganic filler is 80 to 150 parts by weight, it may be advantageous to simultaneously secure the compressive deformation tolerance, moisture retention, and thermal insulation properties of the polymer composite.
[0086] The content of the flame-retardant additive may be 3 to 200 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer. For example, the content of the flame-retardant additive may be 5 to 180 parts by weight, 10 to 180 parts by weight, 15 to 160 parts by weight, 20 to 150 parts by weight, 25 to 130 parts by weight, 30 to 120 parts by weight, 40 to 100 parts by weight, or 50 to 90 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer.
[0087] If the content of the flame-retardant additive is less than 3 parts by weight, it may be difficult to secure sufficient dehydration reaction, release of non-flammable gas, foaming action, or carbon layer formation effect during battery thermal runaway or exposure to flame. On the other hand, if the content of the flame-retardant additive exceeds 200 parts by weight, the dispersibility of the additive within the polymer network may be reduced, or the gel-forming ability, moisture retention, flexibility, compression recovery, or shape retention of the polymer composite may be reduced.
[0088] In one embodiment, when the content of the flame-retardant additive is 15 to 160 parts by weight, a balance of flame-retardant action and mechanical stability of the polymer network can be secured. In another embodiment, when the content of the flame-retardant additive is 20 to 150 parts by weight, the effect of releasing water vapor or forming a carbonized layer upon exposure to flame can be enhanced. In yet another embodiment, when the content of the flame-retardant additive is 40 to 100 parts by weight, it may be advantageous to simultaneously secure moisture retention, compressive deformation tolerance, and flame retardancy of the polymer composite.
[0089] The water content may be 10 to 95 parts by weight based on 100 parts by weight of the total composition. For example, the water content may be 10 to 90 parts by weight, 15 to 85 parts by weight, 20 to 80 parts by weight, 25 to 75 parts by weight, 30 to 70 parts by weight, 35 to 65 parts by weight, or 40 to 60 parts by weight based on 100 parts by weight of the total composition.
[0090] If the water content is less than 10 parts by weight, the effect of suppressing the temperature rise due to the vaporization of water during the initial stage of battery thermal runaway may not be sufficient, and the gel state retention or moisture-based buffering ability of the polymer composite may be reduced. On the other hand, if the water content exceeds 95 parts by weight, the solid content of the polymer network becomes relatively low, and shape retention, compressive strength, surface pressure retention, or handling ability may be reduced.
[0091] In one embodiment, when the water content is 20 to 80 parts by weight, the ability to suppress temperature rise due to moisture vaporization and the shape stability of the polymer composite can be secured in a balanced manner. In another embodiment, when the water content is 30 to 70 parts by weight, the ability to accept compression deformation and moisture retention required as a pressure-resistant pad placed between battery cells can be improved. In yet another embodiment, when the water content is 40 to 60 parts by weight, it may be advantageous to simultaneously secure gel state maintenance, handling properties, and the ability to suppress temperature rise at the beginning of thermal runaway.
[0092] When the above-described polymer composite for battery heat insulation is provided in a dry state, the polymer composite in the dry state may have a porous structure containing pores of 1 nm to 500 μm inside. For example, the size of the pores may be 5 nm to 300 μm, 10 nm to 200 μm, 50 nm to 100 μm, 100 nm to 50 μm, 500 nm to 30 μm, 1 μm to 20 μm, or 2 μm to 10 μm.
[0093] The above pores may be formed during the process in which at least a portion of the water is removed from the polymer composite in the dry state.
[0094] The above pores can improve the lightweighting, moisture reabsorption, thermal insulation, and compressive deformation tolerance of the polymer composite for battery thermal insulation. In addition, the above pores act as pathways for water vapor, non-combustible gases, or decomposition gases generated in a thermal runaway environment, thereby mitigating local pressure increases within the polymer composite.
[0095] In one embodiment, when the polymer composite in the dry state contains micropores of 1 nm to 100 nm, moisture reabsorption and moisture retention due to capillary action may be improved. In another embodiment, when the polymer composite in the dry state contains pores of greater than 100 nm to 10 μm, thermal insulation, moisture reabsorption, and mechanical stability may be secured in balance. In yet another embodiment, when the polymer composite in the dry state contains pores of greater than 10 μm to 500 μm, compressive deformation tolerance and gas release may be improved.
[0096] If the size of the pores is less than 1 nm, moisture reabsorption or gas diffusion may be limited, and if the size of the pores exceeds 500 μm, the compressive strength, shape retention, or durability of the polymer composite in the dry state may be reduced.
[0097] The porosity of the polymer composite in the dry state may be 10 volume% to 90 volume%. For example, the porosity may be 15 volume% to 85 volume%, 20 volume% to 80 volume%, 25 volume% to 75 volume%, 30 volume% to 70 volume%, 35 volume% to 65 volume%, or 40 volume% to 60 volume%.
[0098] The above porosity can affect the moisture reabsorption, thermal insulation, lightweight properties, compressive deformation tolerance, and shape retention of the polymer composite in the dry state. As the porosity increases, the moisture reabsorption space and heat transfer resistance may increase, thereby improving moisture reabsorption and thermal insulation. On the other hand, if the porosity increases excessively, the continuity of the polymer network deteriorates, which may lead to a decrease in compressive strength, durability, and surface pressure retention.
[0099] If the above porosity is less than 10 volume%, it may be difficult to secure sufficient moisture reabsorption, lightness, or thermal insulation of the polymer composite in the dry state. On the other hand, if the above porosity exceeds 90 volume%, the compressive strength, shape retention, or handling properties of the polymer composite in the dry state may be reduced.
[0100] In one embodiment, when the porosity is 20 volume% to 80 volume%, moisture reabsorption and shape stability can be secured in a balanced manner. In another embodiment, when the porosity is 30 volume% to 70 volume%, the compressive deformation tolerance, thermal insulation, and mechanical durability required as a pressure-resistant pad placed between battery cells can be improved. In yet another embodiment, when the porosity is 40 volume% to 60 volume%, it may be advantageous to simultaneously secure handling in a dry state, moisture reabsorption, and thermal insulation.
[0101] The polymer composite in the above dry state can reabsorb moisture at least 10 times its own mass at 23°C and 50% relative humidity. For example, the polymer composite in the above dry state can reabsorb moisture at least 10 times, 15 times, 20 times, 30 times, 40 times, or 50 times its own mass at 23°C and 50% relative humidity. Additionally, the polymer composite in the above dry state can reabsorb moisture at least 10 to 200 times, 15 to 150 times, 20 to 100 times, or 30 to 80 times its own mass under conditions of contact with moisture or immersion in water.
[0102] The above moisture reabsorption capability may mean that the polymer composite for battery thermal insulation can be handled in a porous solid state during storage or assembly, while being converted into a polymer composite in a moisture-containing hydrogel state by reabsorbing moisture before or during use. Accordingly, the polymer composite can secure excellent handling, dimensional stability, and storage stability in a dry state, and after moisture reabsorption, it can perform a function to suppress the temperature rise caused by the vaporization of water during the initial stage of battery thermal runaway.
[0103] The above moisture reabsorption can be realized by the hydrophilic functional groups of the first polymer and the second polymer, the double cross-linked structure of the polymer network, and the porous structure formed inside the polymer composite in the dry state. For example, carboxyl groups, sulfonic acid groups, phosphate groups, or salts thereof included in the first polymer can form ionic interactions or hydrogen bonds with water, and hydroxyl groups, amide groups, ether groups, or amine groups included in the second polymer can form hydrogen bonds with water to contribute to moisture reabsorption and moisture retention.
[0104] In addition, the pores inside the polymer composite in the dry state can act as pathways for moisture penetration and moisture storage spaces. Accordingly, when the polymer composite in the dry state comes into contact with moisture, it rapidly absorbs water into the pores and can be converted into a moisture-containing hydrogel state through the swelling of the polymer network.
[0105] If the amount of moisture reabsorbed by the polymer composite in the above dry state is less than 10 times its own mass, it may be difficult to secure the temperature rise effect resulting from sufficient moisture vaporization during the initial stage of battery thermal runaway after reabsorption. On the other hand, if the amount of moisture reabsorbed is excessively large, the dimensional change of the polymer composite after reabsorption may increase, or the surface pressure retention or shape stability required between battery cells may decrease. Therefore, moisture reabsorption and shape stability can be controlled in a balanced manner by adjusting the crosslinking density, porosity, and inorganic filler content of the polymer network.
[0106] In one embodiment, when the polymer composite for battery thermal insulation reabsorbs moisture 10 to 100 times its own mass, the ability to suppress the initial temperature rise of thermal runaway and the shape stability of the pad can be secured in a balanced manner. In another embodiment, when the polymer composite in a dry state reabsorbs moisture 20 to 80 times its own mass, the moisture retention, compressive deformation tolerance, and thermal insulation properties required for a pressure-resistant pad placed between battery cells can be improved.
[0107] The above-described polymer composite for battery thermal insulation can perform a stepwise or complex thermal insulation mechanism in a battery thermal runaway environment. For example, at the initial stage of thermal runaway, the water contained in the polymer composite can absorb heat as it vaporizes, thereby suppressing a rapid rise in temperature. Subsequently, as the temperature rises, the flame-retardant additive can delay flame propagation and the combustion of the polymer network by performing reactions such as dehydration, foaming, release of non-combustible gases, or the formation of a carbonized layer. Furthermore, in a high-temperature environment, the flame-retardant inorganic filler can form a residual inorganic layer or an inorganic ceramic shield, thereby providing continuous thermal insulation even after the moisture has been lost.
[0108] Unlike simple moisture-containing hydrogels or simple inorganic thermal insulation materials, the polymer composite for battery thermal insulation according to one embodiment of the present invention can simultaneously secure a temperature rise suppression effect due to moisture vaporization, a flame-retardant effect by a flame-retardant additive, a high-temperature thermal insulation effect by a flame-retardant inorganic filler, and shape retention in a moisture-containing hydrogel state or a dry state. Accordingly, the polymer composite can improve thermal runaway propagation suppression performance, handling, and assembly stability as a material for a pressure-resistant pad applied between battery cells or modules.
[0110] A composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention may include a polymer composite for battery heat insulation according to one embodiment of the present invention. The composite hydrogel-based pressure-resistant pad may be placed between cells or modules of a lithium battery to suppress thermal runaway generated in any one battery cell from propagating to an adjacent battery cell or module.
[0111] The composite hydrogel-based pressure-resistant pad may be a sheet-type, film-type, pad-type, or mat-type member disposed in the gap between battery cells. The composite hydrogel-based pressure-resistant pad may be interposed between the opposing surfaces of adjacent battery cells and may buffer or maintain the surface pressure between battery cells while accommodating thickness-direction expansion due to charging, discharging, or aging of the battery cells. Accordingly, the composite hydrogel-based pressure-resistant pad may function not only as a thermal insulation member but also as a pressure equalization member or expansion buffering member between cells within the battery module.
[0112] The above composite hydrogel-based pressure-resistant pad may include a polymer composite in a water-containing hydrogel state. In this case, the composite hydrogel-based pressure-resistant pad can perform an endothermic action in the initial stage of battery thermal runaway by utilizing water retained within the hydrogel. Additionally, the above composite hydrogel-based pressure-resistant pad may include a polymer composite in a dry state. In this case, the composite hydrogel-based pressure-resistant pad may have excellent handling properties during assembly and storage as a porous solid, and can secure endothermic properties in the initial stage of thermal runaway by reabsorbing moisture before or during use.
[0113] The polymer composite for battery heat insulation may be in the form of a composite infiltrated or impregnated into a sheet or nonwoven fabric composed of glass fibers, ceramic fibers, carbon fibers, aramid fibers, polyolefin fibers, polyester fibers, or a mixture thereof. The sheet or nonwoven fabric may function as a reinforcing substrate that supports the polymer composite and may improve the tensile strength, handling properties, dimensional stability, and tear resistance of the composite hydrogel-based pressure-resistant pad.
[0114] The glass fibers or ceramic fibers mentioned above can provide excellent heat resistance and dimensional stability in high-temperature environments. The carbon fibers mentioned above can improve mechanical strength and shape retention. The aramid fibers mentioned above can improve heat resistance, impact resistance, and tensile strength. The polyolefin fibers or polyester fibers mentioned above can improve the flexibility, processability, and cost-effectiveness of the pad. These fibers may be used individually or in a mixture of multiple types.
[0115] The sheet or nonwoven fabric may be in the form of a woven fabric, knitted fabric, nonwoven fabric, felt, mesh, porous film, or a laminate thereof. The sheet or nonwoven fabric may have a porous structure in which a polymer composite can penetrate into internal pores or be attached to the fiber surface. Accordingly, the polymer composite may be impregnated into the interior of the sheet or nonwoven fabric, or may be disposed simultaneously on the surface and inside the sheet or nonwoven fabric.
[0116] When the polymer composite is infiltrated or impregnated into the sheet or nonwoven fabric, the mechanical bonding strength between the polymer composite and the fiber substrate can be improved. In addition, even after some of the polymer components decompose or moisture vaporizes in a thermal runaway environment, the sheet or nonwoven fabric can support the residual inorganic layer, carbonized layer, or inorganic ceramic shielding film. Accordingly, the composite hydrogel-based pressure-resistant pad can suppress the collapse or detachment of the shielding layer even in a high-temperature environment and provide continuous heat-blocking performance.
[0117] The above composite hydrogel-based pressure-resistant pad may be formed as a single-layer structure, or, if necessary, as a multilayer structure in which multiple layers are stacked. For example, the above composite hydrogel-based pressure-resistant pad may include a single composite layer in which the polymer composite is impregnated into a single sheet or nonwoven fabric. As another example, the above composite hydrogel-based pressure-resistant pad may have a structure in which multiple composite layers comprising different fiber substrates or polymer composites of different compositions are stacked. In this case, the thermal insulation performance, compression characteristics, or moisture retention in the thickness direction can be controlled by varying the inorganic filler content, moisture content, porosity, or flame-retardant additive content of each layer.
[0118] The above composite hydrogel-based pressure-resistant pad may have a thickness of 0.5 mm to 10 mm. For example, the thickness of the above composite hydrogel-based pressure-resistant pad may be 0.5 mm to 8 mm, 0.8 mm to 6 mm, 1 mm to 5 mm, 1.5 mm to 4 mm, or 2 mm to 3 mm. If the thickness is less than 0.5 mm, it may be difficult to secure sufficient moisture retention, an inorganic shielding layer formation amount, or compression buffering. On the other hand, if the thickness exceeds 10 mm, the cell stacking density within the battery module may decrease, or the volumetric energy density of the module may decrease.
[0119] The composite hydrogel-based pressure-resistant pad can be placed between battery cells in a compressed state. For example, the composite hydrogel-based pressure-resistant pad can be placed at a compression rate of 5% to 50% relative to its initial thickness. Even in a compressed state, the composite hydrogel-based pressure-resistant pad can maintain its shape through a polymer network, fiber substrate, and porous structure, and can be deformed elastically or viscoelastically according to the expansion or contraction of the battery cells.
[0120] The above composite hydrogel-based pressure-resistant pad may be positioned to cover the entire surface of one side of the battery cell, or may be selectively positioned in a part of the battery cell, for example, in the center where there is a high risk of thermal runaway propagation, around the electrode tab, around the vent, or in an area where there is high contact pressure between cells. Additionally, the above composite hydrogel-based pressure-resistant pad may be positioned between the battery cell and the module frame, between the battery cell and the cooling plate, or between adjacent battery modules.
[0121] A composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention can simultaneously secure the action of suppressing temperature rise caused by moisture vaporization of a polymer composite for battery heat insulation, the action of flame retardant by a flame-retardant additive, the action of high-temperature heat insulation by a flame-retardant inorganic filler, and mechanical reinforcement by a fiber sheet or nonwoven fabric. Accordingly, the composite hydrogel-based pressure-resistant pad can stably maintain surface pressure between battery cells while effectively suppressing the propagation of heat, flames, and high-temperature gases in the event of thermal runaway.
[0123] A method for manufacturing a composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention comprises: a step of preparing a polymer mixture comprising an anionic hydrophilic first polymer comprising a carboxyl group, a sulfonic acid group, a phosphate group, or a salt thereof, and a nonionic or weakly ionic hydrophilic second polymer that is mixable with said first polymer; a step of preparing a hydrogel precursor composition by dispersing a flame-retardant inorganic filler comprising an inorganic thermal insulation material and a ceramicization-inducing material and a flame-retardant additive in said polymer mixture; a step of supplying said hydrogel precursor composition in a sheet shape or infiltrating or impregnating it into a sheet or nonwoven fabric; and a step of forming a composite hydrogel-based pressure-resistant pad in a moisture-containing hydrogel state by inducing physical crosslinking and chemical crosslinking in said hydrogel precursor composition supplied in a sheet shape or infiltrating or impregnating it into said sheet or nonwoven fabric.
[0124] Referring to FIG. 1, a method for manufacturing a composite hydrogel-based pressure-resistant pad according to one embodiment of the present invention may include a step of manufacturing a polymer mixture (110), a step of manufacturing a hydrogel precursor composition (120), a step of supplying in a sheet shape or infiltrating or impregnating into a sheet or nonwoven fabric (130), and a step of forming a composite hydrogel-based pressure-resistant pad (140). Additionally, the manufacturing method may further include, as necessary, a step of forming a dried body, a step of infiltrating or impregnating into a fiber sheet or nonwoven fabric, a cutting step, a thickness adjustment step, or a moisture reabsorption step.
[0125] The step (110) of preparing the polymer mixture above may be a step of preparing a polymer mixture by dissolving or dispersing an anionic hydrophilic first polymer and a nonionic or weakly ionic hydrophilic second polymer in a solvent. The solvent may include water, and may further include an alcohol-based solvent, a glycol-based solvent, or a mixture thereof as needed. In one embodiment, the solvent may be water.
[0126] The above-mentioned anionic hydrophilic first polymer may include carboxyl groups, sulfonic acid groups, phosphate groups, or salts thereof. The above-mentioned first polymer may absorb or retain water within a polymer mixture and may form the basic framework of a polymer network through ionic crosslinking or coordination bonding with metal ions. The above-mentioned first polymer may include cellulose derivatives, alginates, polyacrylic polymers, polymethacrylic copolymers, polyvinylsulfonic acid, polystyrenesulfonic acid, or combinations thereof.
[0127] The above nonionic or weakly ionic hydrophilic second polymer can be mixed with the first polymer to complement the flexibility, mechanical stability, and moisture retention of the polymer network. The second polymer may include polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, hydroxyethylcellulose, hydroxypropylcellulose, polyvinylamine, or a combination thereof.
[0128] In the polymer mixture preparation step (110) above, the first polymer and the second polymer may be mixed at room temperature and, if necessary, dissolved or dispersed by heating, stirring, ultrasonic treatment, or high-shear mixing. For example, the polymer mixture may be prepared at a temperature of 20°C to 90°C and stirred for 10 minutes to 24 hours. The temperature and stirring time may be adjusted according to the type, molecular weight, solubility, and target viscosity of the polymers used.
[0129] For example, the step of preparing the polymer mixture may include adding 3 to 5 parts by weight of carboxymethylcellulose and 5 to 8 parts by weight of polyvinyl alcohol to 87 to 92 parts by weight of water, and then stirring at 50°C to 80°C for 0.5 to 1 hour.
[0130] The step (120) of preparing the hydrogel precursor composition above may be a step of dispersing a flame-retardant inorganic filler and a flame-retardant additive in the polymer mixture. The flame-retardant inorganic filler may include an inorganic thermal insulation material and a ceramicization-inducing material. The flame-retardant inorganic filler may include silica, silica aerogel, aluminosilicate, mica, clay, aluminum oxide, magnesium oxide, zirconium oxide, glass frit, calcium phosphate-based compounds, or a combination thereof.
[0131] The flame-retardant additive may include phosphorus-based flame retardants, nitrogen-based flame retardants, metal hydroxide-based flame retardants, phosphorus and nitrogen-based inflatable flame retardants, condensation-type flame retardants containing phosphorus, nitrogen, and carbon, or combinations thereof. The flame-retardant additive may perform dehydration reactions, release of non-flammable gases, foaming, or carbonization layer formation reactions upon battery thermal runaway or exposure to flame.
[0132] In the step (120) of preparing the hydrogel precursor composition, the flame-retardant inorganic filler and flame-retardant additive may be uniformly dispersed within the polymer mixture. For example, the flame-retardant inorganic filler and flame-retardant additive may be dispersed through mechanical stirring, high-shear mixing, roll milling, bead milling, ultrasonic dispersion, or vacuum degassing. Additionally, the flame-retardant inorganic filler and flame-retardant additive may be added to the polymer mixture in the form of a slurry that has been pre-dispersed in a solvent.
[0133] The hydrogel precursor composition may further include a dispersant, a wetting agent, an antifoaming agent, a viscosity modifier, a pH adjuster, or a preservative as needed. The dispersant or wetting agent may inhibit the aggregation of flame-retardant inorganic fillers and flame-retardant additives and induce uniform dispersion within the polymer network. The pH adjuster may adjust the pH of the hydrogel precursor composition so that metal ion crosslinking, borate ester crosslinking, or organic acid crosslinking proceeds appropriately.
[0134] The step (130) of supplying in a sheet shape or infiltrating or impregnating into a sheet or nonwoven fabric may be a step of supplying the hydrogel precursor composition in a sheet shape or infiltrating or impregnating into a sheet or nonwoven fabric. For example, the hydrogel precursor composition may be supplied in a sheet shape by applying, casting, coating, or laminating onto a mold, carrier film, release film, or support substrate. As another example, the hydrogel precursor composition may be infiltrated or impregnated into the internal pores of a sheet or nonwoven fabric made of glass fiber, ceramic fiber, carbon fiber, aramid fiber, polyolefin fiber, polyester fiber, or a mixture thereof.
[0135] The step (140) of forming the above composite hydrogel-based pressure-resistant pad may be a step of inducing physical crosslinking and chemical crosslinking in the hydrogel precursor composition supplied in the form of a sheet or infiltrated or impregnated into the sheet or nonwoven fabric to form a composite hydrogel-based pressure-resistant pad in a moisture-containing hydrogel state. Accordingly, the hydrogel precursor composition may be crosslinked in a state integrated with the sheet or sheet / nonwoven fabric and formed into a pad shape without necessarily undergoing a separate drying process.
[0136] The above composite hydrogel-based pressure-resistant pad may be provided in a water-containing hydrogel state and may include water, a flame-retardant inorganic filler, and a flame-retardant additive within a polymer network. The water may perform an endothermic action by vaporizing at the beginning of thermal runaway, and the flame-retardant inorganic filler and flame-retardant additive may be dispersed within the polymer network to improve flame retardancy, heat insulation, and shape retention.
[0137] The step (140) of forming the above composite hydrogel-based pressure-resistant pad may include: a step of forming a physical crosslink to at least one of the first polymer and the second polymer using a metal ion or a borate; and a step of forming a chemical crosslink to at least one of the first polymer and the second polymer using a chemical crosslinking component.
[0138] The physical crosslinking may include metal ion-mediated ionic crosslinking, dynamic borate ester crosslinking, or a combination thereof. The metal ion-mediated ionic crosslinking may be formed by calcium ions, magnesium ions, aluminum ions, iron ions, zinc ions, or a combination thereof. For example, the metal ions may be provided in the form of calcium chloride, magnesium chloride, aluminum chloride, iron chloride, zinc chloride, nitrate, sulfate, lactate, gluconate, or acetate.
[0139] The dynamic borate ester crosslinking described above can be formed by a reaction between boric acid, borate, or a combination thereof and a hydroxyl group contained in the first polymer or the second polymer. For example, if the second polymer contains polyvinyl alcohol, deformation responsiveness and compression recovery can be improved by dynamic crosslinking between the hydroxyl group of the polyvinyl alcohol and the boric acid or borate.
[0140] The chemical crosslinking component may include an organic acid, a radical initiator, a multifunctional crosslinking agent, or a combination thereof. For example, the chemical crosslinking component may include ammonium persulfate, methylenebisacrylamide, or a combination thereof.
[0141] As another example, the chemical crosslinking component may include citric acid, tartaric acid, malic acid, succinic acid, glutaric acid, adipic acid, oxalic acid, or a combination thereof. The chemical crosslinking component may provide chemical bonding points or crosslinking points of the first polymer or the second polymer, thereby improving the structural stability, gel state retention, and shape retention in a repeated compression environment of the polymer network.
[0142] The physical crosslinking and chemical crosslinking described above may be performed sequentially, or at least partially simultaneously. For example, a metal ion or borate may be added first to form an initial gel structure in the hydrogel precursor composition, and then chemical crosslinking may be performed using a chemical crosslinking component. As another example, physical crosslinking may be induced by mixing the chemical crosslinking component first and then adding the metal ion or borate. As yet another example, physical crosslinking and chemical crosslinking may be performed in parallel by adding the metal ion, borate, and chemical crosslinking component together.
[0143] The step (140) of forming the composite hydrogel-based refractory pressure pad above may be a step of forming a composite hydrogel-based refractory pressure pad in a moisture-containing hydrogel state by inducing physical crosslinking and chemical crosslinking in the hydrogel precursor composition supplied in the form of a sheet or infiltrated or impregnated in the sheet or nonwoven fabric.
[0144] In the step (140) of forming the composite hydrogel-based pressure-resistant pad, the hydrogel precursor composition may be crosslinked while maintaining a sheet shape or a shape integrated with the sheet and nonwoven fabric. Accordingly, the hydrogel precursor composition may be directly formed into a pad in a moisture-containing hydrogel state without necessarily undergoing a separate drying process.
[0145] The physical and chemical crosslinking described above may be induced after the hydrogel precursor composition is supplied in a sheet form. In another embodiment, the physical and chemical crosslinking may be induced after the hydrogel precursor composition is infiltrated or impregnated into a sheet or nonwoven fabric. In yet another embodiment, at least a portion of the physical and chemical crosslinking may proceed simultaneously with the sheeting or impregnation of the hydrogel precursor composition.
[0146] The step (140) of forming the composite hydrogel-based refractory pressure pad may include crosslinking within a mold, crosslinking on a carrier film, crosslinking on a release film, crosslinking within a coating layer, crosslinking within a sheet or nonwoven fabric, crosslinking under a roll press pressure state, or crosslinking under a lamination state. For example, the hydrogel precursor composition may be supplied onto a mold, a carrier film, or a release film to have a constant thickness and then crosslinked. As another example, the hydrogel precursor composition may be crosslinked while penetrating or impregnating into the internal pores of a sheet or nonwoven fabric to form a composite hydrogel-based refractory pressure pad integrated with the sheet or nonwoven fabric.
[0147] The composite hydrogel-based surface pressure-resistant pad can be molded to have a thickness of 0.5 mm to 10 mm. For example, the composite hydrogel-based surface pressure-resistant pad can be molded to have a thickness of 0.5 mm to 8 mm, 0.8 mm to 6 mm, 1 mm to 5 mm, 1.5 mm to 4 mm, or 2 mm to 3 mm. The thickness can be adjusted considering the gap between battery cells, the required surface pressure, thermal insulation performance, and module energy density.
[0148] The above manufacturing method may further include the steps of cutting, perforating, surface treating, or laminating the composite hydrogel-based pressure-resistant pad. For example, the composite hydrogel-based pressure-resistant pad may be cut into a square, circular, elliptical, or polygonal shape to correspond to the shape of a battery cell. Additionally, the composite hydrogel-based pressure-resistant pad may be processed to include through holes, cuts, or grooves to avoid interference with electrode tabs, vents, fasteners, or cooling structures.
[0149] The composite hydrogel-based pressure-resistant pad manufactured by the above manufacturing method can be stored in a moisture-containing hydrogel state until it is placed between battery cells. For example, the composite hydrogel-based pressure-resistant pad can be stored in a sealed package, a moisture-retaining package, or with a release film attached. Accordingly, the composite hydrogel-based pressure-resistant pad can maintain moisture retention and a gel state until assembly.
[0150] A method for manufacturing a composite hydrogel-based pressure-resistant pad according to another embodiment of the present invention can directly manufacture a composite hydrogel-based pressure-resistant pad in a moisture-containing hydrogel state by dispersing a flame-retardant inorganic filler and a flame-retardant additive in a hydrogel precursor composition comprising a hydrophilic first polymer and a hydrophilic second polymer, and inducing crosslinking while supplying the hydrogel precursor composition in a sheet shape or infiltrating or impregnating it into a sheet or nonwoven fabric. Accordingly, a pad having moisture retention, shape retention, compressive deformation tolerance, and thermal runaway propagation suppression performance can be manufactured without necessarily requiring a separate drying process.
[0152] A battery module according to another embodiment of the present invention may include a plurality of battery cells and a composite hydrogel-based pressure-resistant pad. The composite hydrogel-based pressure-resistant pad may be disposed between adjacent battery cells among the plurality of battery cells.
[0153] The plurality of battery cells may be lithium secondary battery cells. For example, the battery cells may be lithium-ion battery cells, lithium polymer battery cells, lithium metal battery cells, or lithium sulfur battery cells, but are not limited thereto. The battery cells may be pouch-type cells, prismatic cells, or cylindrical cells. In one embodiment, the plurality of battery cells may be pouch-type lithium secondary battery cells, and the composite hydrogel-based pressure-resistant pad may be disposed between the opposing wide surfaces of adjacent pouch-type cells.
[0154] The composite hydrogel-based pressure-resistant pad is interposed between adjacent battery cells to accommodate thickness-direction expansion of the battery cells due to charging / discharging, aging, or gas generation. For example, the composite hydrogel-based pressure-resistant pad may be compressively deformed according to the expansion of the battery cells and may be restored at least partially according to the contraction of the battery cells or changes in external load. Accordingly, the composite hydrogel-based pressure-resistant pad can alleviate localized pressure concentration between the plurality of battery cells and improve the uniformity of surface pressure across the entire cell stack.
[0155] The above-described composite hydrogel-based pressure-resistant pad can accommodate compressive deformation due to cell expansion between adjacent battery cells and suppress the propagation of heat and flames during thermal runaway. Specifically, when thermal runaway occurs in any one battery cell, the polymer composite for battery heat insulation included in the above-described composite hydrogel-based pressure-resistant pad can delay the heat transferred to adjacent battery cells through an endothermic action due to moisture vaporization, a flame-retardant action by a flame-retardant additive, and an action of forming an inorganic shielding layer by a flame-retardant inorganic filler.
[0156] The composite hydrogel-based pressure-resistant pad may be positioned to correspond to the entire opposing surface between adjacent battery cells. In this case, the composite hydrogel-based pressure-resistant pad can disperse surface pressure across the entire surface of the battery cell and block radiant heat, conductive heat, or flame transmitted through the wide surface of the battery cell in the event of thermal runaway. In another embodiment, the composite hydrogel-based pressure-resistant pad may be selectively positioned in a portion of the area between adjacent battery cells. For example, the composite hydrogel-based pressure-resistant pad may be positioned in the center of the battery cell, around the electrode tab, around the vent, in an area where high temperatures are likely to occur, or in an area where inter-cell contact pressure is concentrated.
[0157] The battery module may further include a module housing that accommodates the plurality of battery cells. The module housing can align and fix the plurality of battery cells and protect the plurality of battery cells from external impact. The composite hydrogel-based surface pressure-resistant pad may be placed in a compressed state between the battery cells within the module housing and may maintain a constant surface pressure by the fastening force of the module housing or the restraining force of the cell stack.
[0158] The battery module may further include a cooling member. The cooling member may include a cooling plate, a cooling channel, a heat sink, a thermally conductive pad, or a cooling channel. The composite hydrogel-based pressure-resistant pad is placed between the battery cells to suppress thermal runaway propagation between cells, and the cooling member can dissipate heat generated during normal operation to the outside. Accordingly, the battery module can secure both thermal management performance under normal operating conditions and thermal propagation suppression performance under abnormal thermal runaway conditions.
[0159] The above composite hydrogel-based pressure-resistant pad may be placed not only between the battery cells, but also between the battery cells and the module housing, between the battery cells and the cooling member, or between adjacent cell groups. For example, if the battery module includes a plurality of cell groups, the composite hydrogel-based pressure-resistant pad may be placed between adjacent cells within each cell group or between adjacent cell groups. Accordingly, the battery module can block thermal runaway propagation in stages on a cell-by-cell or cell-group basis.
[0160] The above composite hydrogel-based pressure-resistant pad can be assembled to the battery module in a moisture-containing hydrogel state. In this case, the composite hydrogel-based pressure-resistant pad can perform a moisture vaporization and endothermic function immediately after assembly. Additionally, the composite hydrogel-based pressure-resistant pad may reabsorb moisture through moisture supply or ambient humidity after being assembled to the battery module in a dry state. In this case, the composite hydrogel-based pressure-resistant pad can recover or improve responsiveness to thermal runaway during use while ensuring excellent handling and dimensional stability during the assembly process.
[0161] In the battery module above, the composite hydrogel-based pressure-resistant pad may have compressive deformability capable of accommodating the expansion of the battery cell in the thickness direction. For example, the composite hydrogel-based pressure-resistant pad may accommodate compressive deformation of 5% to 50% relative to the initial thickness. If the compressive deformability is less than 5%, it may be difficult to sufficiently alleviate the increase in surface pressure due to the expansion of the battery cell, and if the compressive deformability exceeds 50%, the shape retention or long-term surface pressure retention of the pad may be reduced.
[0162] The above composite hydrogel-based pressure-resistant pad can maintain the gap between adjacent battery cells for a certain period of time or maintain its shape as a thermal barrier layer even during thermal runaway. For example, even if the polymer component or moisture of the above composite hydrogel-based pressure-resistant pad decreases at high temperatures, the flame-retardant inorganic filler, carbonized layer, fiber substrate, or inorganic ceramic shielding film remains to maintain the shielding structure between adjacent battery cells. Accordingly, the battery module can delay or suppress the sequential propagation of thermal runaway from any one battery cell to adjacent cells.
[0163] A battery module according to another embodiment of the present invention can accommodate compressive deformation due to cell expansion and improve surface pressure uniformity between cells during normal operation by placing a composite hydrogel-based pressure-resistant pad between adjacent battery cells, and can suppress the propagation of heat, flame, and high-temperature gas in abnormal thermal runaway situations. Accordingly, the battery module can simultaneously improve cell stacking stability, thermal management stability, and thermal runaway propagation suppression performance.
[0165] The present invention will be described in detail below with reference to the following examples and comparative examples. However, the technical scope of the present invention is not limited or restricted by such examples.
[0167] [Example]
[0168] Carboxymethylcellulose was prepared as an anionic hydrophilic first polymer, and polyvinyl alcohol was prepared as a nonionic hydrophilic second polymer.
[0169] 3 parts by weight of the first polymer and 5 parts by weight of the second polymer were added to 90 parts by weight of water, and then stirred at 70°C for 0.5 hours to prepare a polymer mixture.
[0170] Subsequently, tricalcium phosphate, calcium phosphate, alumina, magnesia, silica, ceramic fibers, and glass fibers were mixed and added to the polymer mixture as flame-retardant inorganic fillers. Additionally, hydroxycarbonate was added to the polymer mixture as a flame-retardant additive. The flame-retardant additive was added in an amount of 5 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer.
[0171] A hydrogel precursor composition was prepared by stirring a mixture containing a flame-retardant inorganic filler and a flame-retardant additive at 70°C for 0.5 hours.
[0172] 0.4 parts by weight of a dispersant, 0.4 parts by weight of an antifoaming agent, and 0.5 parts by weight of a pH adjuster were further added to the hydrogel precursor composition.
[0173] Next, calcium chloride (CaCl2) was added to the hydrogel precursor composition as a physical crosslinking agent, and ammonium persulfate and methylene bisacrylamide were added as chemical crosslinking agents, either individually or in combination. For physical crosslinking, 40 parts by weight of a 5 wt% CaCl2 solution were added based on 100 parts by weight of the total of the first and second polymers, and 2 parts by weight of the chemical crosslinking agent were added based on 100 parts by weight of the total of the first and second polymers. The hydrogel precursor composition was reacted at 50°C for 0.5 hours to produce a polymer composite for battery heat insulation containing moisture.
[0174] Subsequently, the hydrogel precursor composition, which was adjusted to the sheet shape or infiltrated or impregnated into the sheet or nonwoven fabric, was reacted at 50°C for 0.5 hours to induce physical and chemical crosslinking. Accordingly, the hydrogel precursor composition was converted into a water-containing hydrogel state while maintaining its sheet shape, thereby producing a composite hydrogel-based refractory pressure pad.
[0175] The manufactured composite hydrogel-based pressure-resistant pad did not undergo a separate drying process and maintained a moisture-containing hydrogel state even after manufacturing. The composite hydrogel-based pressure-resistant pad was able to accommodate compressive deformation while maintaining a gel state at room temperature and had a pad shape that could be placed between battery cells.
[0176] The above composite hydrogel-based pressure-resistant pad was able to perform endothermic action due to moisture vaporization in a battery thermal runaway environment, flame-retardant action due to flame-retardant additives, and heat-insulating action due to flame-retardant inorganic fillers. In addition, when the above composite hydrogel-based pressure-resistant pad is manufactured in a form impregnated into a fiber sheet or nonwoven fabric, the fiber sheet or nonwoven fabric supports the polymer composite in a moisture-containing hydrogel state, thereby improving the handling, shape retention, and mechanical stability of the pad.
[0178] Although the embodiments have been described above with reference to the limited drawings, those skilled in the art can apply various technical modifications and variations based on the above. For example, suitable results may be achieved even if the described techniques are performed in a different order than described, and / or if the components of the described system, structure, device, circuit, etc. are combined or assembled in a form different from described, or replaced or substituted by other components or equivalents.
[0179] Therefore, other implementations, other embodiments, and equivalents to the claims also fall within the scope of the claims set forth below.
Claims
Claim 1 In a polymer composite for battery heat insulation, the polymer composite comprises: an anionic hydrophilic first polymer comprising a carboxyl group, a sulfonic acid group, a phosphate group, or a salt thereof; a nonionic or weakly ionic hydrophilic second polymer that is miscible with the first polymer; a flame-retardant inorganic filler; and a flame-retardant additive. and water; comprising, wherein the first polymer and the second polymer form a polymer network that retains the water, the flame-retardant inorganic filler is dispersed within the polymer network, and comprises an inorganic insulating material and a ceramicization-inducing material, wherein the inorganic insulating material comprises at least one selected from the group consisting of silica, silica aerogel, aluminosilicate, mica, clay, aluminum oxide, magnesium oxide, zirconium oxide, glass frit, and calcium phosphate-based compounds, and the calcium phosphate-based compound comprises hydroxyapatite, tricalcium phosphate, or a mixture thereof, wherein the calcium phosphate-based compound is softened, melted, or sintered in a high-temperature environment caused by battery thermal runaway to combine with the inorganic insulating material to form an inorganic ceramic shield, the flame-retardant additive is dispersed within the polymer network, and the polymer composite is provided in a water-containing hydrogel state or provided in a dry state from which at least a portion of the water has been removed from the polymer composite in the water-containing hydrogel state, and the polymer composite in the water-containing hydrogel state is in a gel state at room temperature Maintaining, the nonionic or weakly ionic hydrophilic second polymer comprises at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethylene oxide, hydroxyethylcellulose, hydroxypropylcellulose, and polyvinylamine, or the first polymer and the second polymer form a dual network structure in which physical crosslinking and chemical crosslinking are combined, the physical crosslinking comprises metal ion-mediated ionic crosslinking, dynamic borate ester crosslinking, or both, the chemical crosslinking is induced by a chemical component, and the metal ion-mediated ionic crosslinking comprises calcium ions,A polymer composite for battery heat insulation comprising at least one selected from the group consisting of magnesium ions, aluminum ions, iron ions, and zinc ions, wherein the dynamic borate ester crosslink is formed by a reaction between boric acid, borate, or a combination thereof and a hydroxyl group contained in the first polymer or the second polymer, wherein the chemical crosslinking component comprises an organic acid, a radical initiator, a polyfunctional crosslinking agent, or a combination thereof, wherein the chemical crosslinking component comprises ammonium persulfate, methylenebisacrylamide, or a combination thereof, or wherein the polymer composite in a dry state is capable of reabsorbing moisture at least 10 times its own mass at 23°C and 50% relative humidity. Claim 2 A polymer composite for battery heat insulation according to claim 1, wherein the anionic hydrophilic first polymer comprises at least one selected from the group consisting of cellulose derivatives, alginate, polyacrylic polymers, polymethacrylic copolymers, polyvinylsulfonic acid, and polystyrenesulfonic acid. Claim 3 delete Claim 4 delete Claim 5 A polymer composite for battery heat insulation according to claim 1, wherein the flame retardant additive comprises at least one selected from the group consisting of phosphorus-based flame retardants, nitrogen-based flame retardants, metal hydroxide-based flame retardants, phosphorus and nitrogen-based expansive flame retardants, and condensation-type flame retardants containing phosphorus, nitrogen, and carbon. Claim 6 A polymer composite for battery heat insulation according to claim 1, wherein the flame-retardant additive performs at least one flame-retardant action among dehydration reaction, release of non-combustible gas, foaming, or formation of a carbon layer upon exposure to flame. Claim 7 A polymer composite for heat insulation of a battery, wherein, in claim 1, the content of the flame-retardant inorganic filler is 10 to 300 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer, the content of the flame-retardant additive is 3 to 200 parts by weight based on 100 parts by weight of the total of the first polymer and the second polymer, and the content of the moisture-containing hydrogel is 10 to 95 parts by weight based on 100 parts by weight of the total composition. Claim 8 A polymer composite for heat insulation of a battery according to claim 1, wherein when the polymer composite for heat insulation of a battery is provided in a dry state, the polymer composite in the dry state has a porous structure having pores of 1 nm to 500 μm inside, and the porosity of the polymer composite in the dry state is 10 volume% to 90 volume%. Claim 9 delete Claim 10 A composite hydrogel-based pressure-resistant pad comprising a polymer composite for battery thermal insulation according to claim 1, disposed between cells or modules of a lithium battery to control thermal runaway. Claim 11 In claim 10, the polymer composite for battery heat insulation is in the form of a composite infiltrated or impregnated into a sheet or nonwoven fabric composed of glass fiber, ceramic fiber, carbon fiber, aramid fiber, polyolefin fiber, polyester fiber, or a mixture thereof, a composite hydrogel-based pressure-resistant pad. Claim 12 In claim 10, the composite hydrogel-based pressure-resistant pad has a thickness of 0.5 mm to 10 mm. Claim 13 A method for manufacturing a composite hydrogel-based refractory pressure pad according to claim 10, comprising: a step of preparing a polymer mixture comprising an anionic hydrophilic first polymer containing a carboxyl group, a sulfonic acid group, a phosphate group, or a salt thereof, and a nonionic or weakly ionic hydrophilic second polymer that is mixable with said first polymer; a step of preparing a hydrogel precursor composition by dispersing a flame-retardant inorganic filler containing an inorganic thermal insulation material and a ceramicization-inducing material and a flame-retardant additive in said polymer mixture; a step of supplying said hydrogel precursor composition in a sheet shape or infiltrating or impregnating it into a sheet or nonwoven fabric; and a step of inducing physical crosslinking and chemical crosslinking in said hydrogel precursor composition supplied in a sheet shape or infiltrating or impregnating it into said sheet or nonwoven fabric to form a composite hydrogel-based refractory pressure pad in a moisture-containing hydrogel state. Claim 14 A method for manufacturing a composite hydrogel-based pressure-resistant pad according to claim 13, wherein the step of forming the composite hydrogel-based pressure-resistant pad comprises: a step of forming a physical crosslink to at least one of the first polymer and the second polymer using a metal ion or a borate; and a step of forming a chemical crosslink to at least one of the first polymer and the second polymer using a chemical crosslinking component. Claim 15 A battery module comprising: a plurality of battery cells; and a composite hydrogel-based pressure-resistant pad according to claim 10 disposed between adjacent battery cells among the plurality of battery cells. Claim 16 A battery module according to claim 15, wherein the plurality of battery cells are lithium secondary battery cells, and the polymer composite for battery thermal insulation accommodates compressive deformation due to cell expansion between adjacent battery cells while suppressing the propagation of heat and flame during thermal runaway.
Citation Information
Patent Citations
Thin fire-resistant sheet having excellent flame-blocking and fire-resistance properties for electric vehicle battery, and manufacturing method thereof
WO2025244230A1
Flame retardant surface pressure pad for battery
WO2026146762A1