Iron-based composite phosphate cathode material and method of manufacturing the same, cathode sheet and sodium ion battery

By controlling the viscosity and performing drying and sintering, a uniform nano-sized iron-based composite phosphate cathode material is produced, enhancing the cycle and safety performance of sodium ion batteries while addressing manufacturing costs and environmental issues.

KR103045815B1Active Publication Date: 2026-11-06HUBEI WANRUN NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020247010444
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-14
Filing Date
2023-03-08
Publication Date
2026-11-06
Estimated Expiration
2043-03-08

AI Technical Summary

Technical Problem

Existing sodium-ion battery cathode materials like Na4Fe3(PO4)2P2O7 face high manufacturing costs and environmental pollution due to the use of water-soluble salts, hindering industrial development.

Method used

A method is developed to control the viscosity of a solution using a specific solid-liquid ratio, dissolve solid reactants uniformly, and perform drying and sintering to produce a homogeneous iron-based composite phosphate cathode material with nano-sized spherical particles.

Benefits of technology

The method results in a uniform, nano-sized cathode material with improved cycle and safety performance in sodium ion batteries, reducing manufacturing costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024034648948-PCT00001_ABST
    Figure 112024034648948-PCT00001_ABST
Patent Text Reader

Abstract

The present invention relates to the field of sodium ion battery material technology, and specifically to an iron-based composite phosphate cathode material, a method for manufacturing the same, a cathode sheet, and a sodium ion battery. A method for manufacturing an iron-based composite phosphate cathode material comprises uniformly mixing a sodium source, a phosphorus source, a carbon source, and water, and then mixing with iron phosphate to obtain a first mixing system; grinding the first mixing system to obtain a second mixing system, and then performing drying and sintering; the total mass of the Na element, Fe element, (PO4)3-, and carbon source in the first mixing system is 30-40% of the mass of water; and the viscosity of the second mixing system is 300 Pa.S or higher. The above method allows for the dissolution of solid reactants during the grinding process to obtain a uniform reaction function, and additionally, by performing drying and sintering, an iron-based composite phosphate cathode material can be obtained, and the material is a nano-spherical particle of uniform size.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure claims priority to a Chinese patent application filed with the Chinese Intellectual Property Office on March 14, 2022, with application number CN202210247605.5 and titled 'Iron-based composite phosphate cathode material and method for manufacturing the same, cathode sheet and sodium ion battery', the entire contents of which are incorporated by reference into the present disclosure.

[0002] The present disclosure relates to the field of sodium ion battery material technology, specifically to an iron-based composite phosphate cathode material and a method for manufacturing the same, a cathode sheet and a sodium ion battery. Background Technology

[0003] In recent years, people have actively developed clean energy sources such as solar, wind, and hydroelectric energy. However, these clean energies have drawbacks, such as high variability, low stability, and intermittent supply; therefore, the integration and conversion of large-scale energy storage devices are necessary for their rational use. Among existing energy storage technologies, rechargeable batteries have been recognized as one of the ideal choices for large-scale energy storage due to their high flexibility and energy conversion efficiency. Although lithium-ion batteries have achieved great success in the fields of portable electronic devices and electric vehicles due to their high energy density and excellent cycle stability, they cannot meet the low-cost requirements of large-scale energy storage due to the scarcity and uneven distribution of lithium resources. In contrast, sodium-ion batteries possess a similar operating principle to lithium-ion batteries, yet their reserves are more abundant and widely distributed. Considering the requirement that the cost of large-scale energy storage devices exceeds energy density, sodium-ion batteries have been recognized as a potential candidate for large-scale energy storage systems.

[0004] Although a large number of sodium-ion battery cathode materials have been reported to date, only a small fraction of materials, such as vanadium-based phosphates, iron-based phosphates, and Prussian blue analogs, have exhibited excellent electrochemical properties. Furthermore, in the process of commercializing laboratory results, these materials also face some serious problems, such as the high toxicity and high cost of vanadium-based materials and the structural instability of Prussian blue analogs. Among iron-based phosphates, Na4Fe3(PO4)2P2O7 offers low cost, environmental friendliness, and a high theoretical capacity (129 mAh g⁻¹). -1 ), high average operating voltage (3.1VS.Na + It has been recognized as the most potential material for sodium-ion battery cathode materials, combining all the advantages of iron-based phosphates, such as low volume expansion (4% reduction). However, Na4Fe3(PO4)2P2O7 does not contribute to industrial development in terms of raw material manufacturing costs because the synthesis process always uses salts that are easily soluble in water, resulting in high process costs and severe environmental pollution from decomposition products. Therefore, finding a more economical manufacturing process could help with the batch production of Na4Fe3(PO4)2P2O7. The problem to be solved

[0005] The purpose of the present disclosure is to provide a method for manufacturing an iron-based composite phosphate cathode material by controlling the viscosity of a solution using an appropriate solid / liquid ratio, realizing the dissolution of solid reactants during a polishing process to obtain a homogeneous reaction function, and obtaining a final product through additional drying and sintering.

[0006] Another object of the present disclosure is to provide an iron-based composite phosphate cathode material produced by the method for producing the iron-based composite phosphate cathode material described above.

[0007] Another objective of the present disclosure is to provide an anode sheet comprising the above anode material.

[0008] Another object of the present disclosure is to provide a sodium ion battery comprising the anode sheet. means of solving the problem

[0009] To achieve the above objectives of the present disclosure, the following technical measures are used in particular.

[0010] The present disclosure comprises the steps of: uniformly mixing a sodium source, a phosphorus source, a carbon source, and water, and then mixing with iron phosphate to obtain a first mixed system; grinding the first mixed system to obtain a second mixed system, and then performing drying and sintering;

[0011] In the first mixing system above, Na element, Fe element, (PO4) 3- The total mass of the carbon source is 30 to 40% of the mass of the water; and the viscosity of the second mixing system is 300 Pa.S or higher. A method for manufacturing an iron-based composite phosphate cathode material is provided.

[0012] Optionally, the sodium source comprises at least one of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, and sodium phosphate;

[0013] Optionally, the phosphorus source comprises at least one of sodium dihydrogen phosphate, sodium phosphate, and phosphoric acid;

[0014] Optionally, the carbon source comprises at least one of citric acid, glucose, sucrose, and polyethylene glycol;

[0015] Optionally, the molar ratio of the phosphorus source, sodium source, and carbon source is 1: (2.8–3.2): (1–10).

[0016] Optionally, the molar ratio of Fe to P in the iron phosphate is 0.97 to 1;

[0017] Optionally, the iron phosphate comprises micrometer-sized particles and / or nanometer-sized coacervates.

[0018] Optionally, in the second mixing system, the particle size D90 of the iron phosphate is 0.05 to 0.15 μm.

[0019] Optionally, the viscosity of the second mixing system is 300 to 400 Pa.S.

[0020] Optionally, the drying comprises spray drying;

[0021] Optionally, the drying temperature is 80 to 120°C and the drying time is 5 to 10 hours.

[0022] Optionally, the sintering comprises performing a first sintering treatment under conditions of 290–310°C and performing a second sintering treatment by increasing the temperature to 550–600°C;

[0023] Optionally, the time of the first sintering treatment is 3 to 5 hours, and the time of the second sintering treatment is 10 to 12 hours;

[0024] Optionally, the heating rate of the above heating is 2 to 5℃ / min.

[0025] The present invention provides an iron-based composite phosphate cathode material manufactured by the above-described method for manufacturing an iron-based composite phosphate cathode material.

[0026] Optionally, the iron-based composite phosphate cathode material is a spherical particle, and the particle size is 100 to 200 nm.

[0027] The present disclosure also provides an anode sheet comprising the above anode material.

[0028] The present disclosure also provides a sodium ion battery comprising the anode sheet. Effects of the invention

[0029] Compared to prior art, the beneficial effects of the present disclosure are as follows.

[0030] (1) In the present disclosure, the viscosity of the solution is controlled using an appropriate solid-liquid ratio, and then the solid reactant is dissolved during the polishing process to obtain a uniform reaction function, and an iron-based composite phosphate cathode material is obtained through additional drying and sintering. The material is a nano-spherical particle with a particle size of 100 to 200 nm, is uniform in size, and has excellent electrochemical properties.

[0031] (2) When the iron-based composite phosphate cathode material manufactured in the present disclosure is applied to a sodium ion battery, the cycle performance and safety performance of the battery can be further improved. Brief explanation of the drawing

[0032] Hereinafter, in order to more clearly explain the specific embodiments of the present disclosure or the technical methods of the prior art, drawings necessary for describing the specific embodiments or prior art will be briefly described. The drawings described below are some embodiments of the present disclosure, and it is obvious that a person skilled in the art can obtain other drawings based on these drawings without any creative labor. FIG. 1 is a scanning electron microscope (SEM) image of an iron-based composite phosphate cathode material obtained in Example 1 of the present disclosure. FIG. 2 is a charge / discharge graph of a battery manufactured with an iron-based composite phosphate cathode material obtained in Example 1 of the present disclosure. Specific details for implementing the invention

[0033] Embodiments of the present disclosure will be described in detail below with reference to examples. However, those skilled in the art will understand that the following examples are merely for illustrative purposes and should not be construed as limiting the scope of the present disclosure. Where specific conditions are not indicated in the examples, the procedure is performed according to existing conditions or conditions recommended by the manufacturer. Where the manufacturer is not indicated on the reagents or equipment used, they are all commercially available products.

[0034] According to one aspect of the present disclosure, the method comprises the steps of: uniformly mixing a sodium source, a phosphorus source, a carbon source, and water, and then mixing with iron phosphate to obtain a first mixed system; grinding the first mixed system to obtain a second mixed system, and then performing drying and sintering;

[0035] In the first mixing system above, Na element, Fe element, (PO4) 3- The present invention relates to a method for manufacturing an iron-based composite phosphate cathode material in which the total mass of the carbon source is 30 to 40% of the mass of the water; and the viscosity of the second mixing system is 300 Pa.S or higher.

[0036] The present disclosure obtains a Na4Fe3(PO4)2P2O7 cathode material, which is an iron-based complex phosphate, by controlling the viscosity of the solution using an appropriate solid-liquid ratio, realizing the dissolution of solid reactants during the polishing process to obtain a uniform reaction function, and then further drying and sintering. The cathode material is a nano-sized spherical particle with a particle size of 100 to 200 nm and is uniform in size.

[0037] In one embodiment, in the first mixing system, Na element, Fe element, (PO4) 3- The total mass of the (phosphate radical) and carbon source is 30 to 40% of the mass of the water, specifically including but not limited to 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, or 39%.

[0038] In one embodiment, the viscosity of the second mixing system is 300 Pa.S or higher. Specifically, it includes, but is not limited to, 310 Pa.S, 320 Pa.S, 330 Pa.S, 350 Pa.S, 360 Pa.S, 380 Pa.S, 400 Pa.S, 420 Pa.S, 450 Pa.S, and 500 Pa.S. In one embodiment, the viscosity of the second mixing system is 300 to 500 Pa.S.

[0039] The above grinding refers to a method of refining and dispersing particles using mechanical force. For example, a sand milling method is used, and the sand milling medium includes at least one of riprap, glass beads, zirconia oxide beads, and zirconia silicate beads.

[0040] In one embodiment, the sodium source comprises at least one of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, and sodium phosphate.

[0041] In one embodiment, the phosphorus source comprises at least one of sodium dihydrogen phosphate, sodium phosphate, and phosphoric acid.

[0042] In one embodiment, the carbon source comprises at least one of citric acid, glucose, sucrose, and polyethylene glycol.

[0043] In one embodiment, the molar ratio of the phosphorus source, sodium source, and carbon source is 1: (2.8~3.2): (1~10).

[0044] In one embodiment, the molar ratio of the phosphorus source, sodium source, and carbon source is 1:3:1, 1:3:2, 1:3:3, 1:3:4, 1:3:5, 1:3:6, 1:3:7, 1:3:10.

[0045] In one embodiment, the molar ratio of Fe to P in the iron phosphate is 0.97 to 1, and, for example, may be 0.98 or 0.99.

[0046] In one embodiment, the iron phosphate is a crystalline or amorphous particle. The iron phosphate comprises micrometer-sized particles and / or nanometer-sized coacervates. A preferred type is a nanometer-sized coacervate.

[0047] In one embodiment, the micrometer-sized particle size of the iron phosphate is 1 to 20 μm, including but not limited to 2 μm, 3 μm, 5 μm, 6 μm, 7 μm, 10 μm, 11 μm, 13 μm, 15 μm, 17 μm, or 20 μm. In one embodiment, the nanometer-sized coacervate particle size of the iron phosphate is 20 to 200 nm, including but not limited to 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 70 nm, 80 nm, 100 nm, 120 nm, 150 nm, 170 nm, 180 nm, and 200 nm.

[0048] In one embodiment, the particle size D90 of the iron phosphate in the second mixing system is 0.05 to 0.15 μm. In one embodiment, the particle size D90 of the iron phosphate is 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.11 μm, 0.12 μm, 0.13 μm, 0.14 μm, or 0.15 μm.

[0049] In one embodiment, the drying includes spray drying.

[0050] In one embodiment, the drying temperature is 80 to 120°C and the drying time is 5 to 10h. In one embodiment, the drying temperature is 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, or 115°C. The drying time is 6h, 7h, 8h, 9h, or 9.5h.

[0051] In one embodiment, the sintering comprises performing a first sintering treatment under conditions of 290 to 310°C and performing a second sintering treatment by raising the temperature to 550 to 600°C. In one embodiment, the temperature of the first sintering treatment is 292°C, 295°C, 298°C, 300°C, 302°C, 305°C, or 309°C. In one embodiment, the temperature of the second sintering treatment includes, but is not limited to, 555°C, 560°C, 565°C, 570°C, 575°C, 580°C, 585°C, 590°C, 595°C, or 600°C.

[0052] In one embodiment, the time of the first sintering treatment is 3 to 5 hours, and the time of the second sintering treatment is 10 to 12 hours. In one embodiment, the time of the first sintering treatment includes, but is not limited to, 3 hours, 3.5 hours, 4 hours, or 4.5 hours. The time of the second sintering treatment includes, but is not limited to, 10.5 hours, 11 hours, or 11.5 hours.

[0053] Optionally, the heating rate of the above heating is 2 to 5℃ / min. For example, it may be 2.5℃ / min, 3℃ / min, 4℃ / min, or 4.5℃ / min.

[0054] In one embodiment, sintering is performed under protective gas conditions. The protective gas includes nitrogen and an inert gas. The inert gas includes argon, neon, etc.

[0055] The present disclosure further obtains an iron-based composite phosphate cathode material with excellent electrochemical properties through the above sintering conditions.

[0056] According to another aspect of the present disclosure, the present disclosure also relates to an iron-based composite phosphate cathode material produced by the method for producing the iron-based composite phosphate cathode material.

[0057] In one embodiment, the iron-based composite phosphate cathode material is a spherical particle and has a particle size of 100 to 200 nm. In one embodiment, the particle size of the iron-based composite phosphate cathode material includes, but is not limited to, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, or 200 nm.

[0058] According to another aspect of the present disclosure, the present disclosure also relates to an anode sheet comprising the anode material.

[0059] According to another aspect of the present disclosure, the present disclosure also relates to a sodium ion battery comprising the anode sheet.

[0060] The battery of the present disclosure has excellent cycle performance and safety.

[0061] The present disclosure will be further explained below with specific embodiments and comparative examples.

[0062] FIG. 1 is a scanning electron microscope (SEM) image of an iron-based composite phosphate cathode material obtained in Example 1 of the present disclosure. FIG. 2 is a charge-discharge graph of a battery manufactured with the iron-based composite phosphate cathode material obtained in Example 1 of the present disclosure.

[0063] Example 1

[0064] A method for manufacturing an iron-based composite phosphate cathode material includes the following steps.

[0065] Sodium dihydrogen phosphate, sodium acetate, and citrate monohydrate were added to 5 kg of deionized water in a molar ratio of 1:3:2 and stirred continuously until a clear solution was formed. A certain proportion of solid iron phosphate was added to the clear solution to adjust the total solid content to 35%, wherein the iron phosphate was a nanometer-sized coacervate with a particle size of 50–100 nm. Next, sand milling was performed so that the viscosity of the solution gradually increased as the iron phosphate was dispersed in the solution, and sand milling was stopped when the viscosity of the solution reached 300 Pa·S. The solution was then spray-dried at a temperature of 95°C for a duration of 8 hours. Subsequently, the solution was calcined at a high temperature in an N2 atmosphere at a heating rate of 2°C / min, maintained at 300°C for 5 hours, maintained at 550°C for 12 hours, and after natural cooling, an iron-based composite phosphate cathode material was obtained.

[0066] The morphology of the material is analyzed by SEM, and as shown in Figure 1, the material is a nano-spherical particle with a particle size of 100 to 200 nm and is uniform in size.

[0067] Example 2

[0068] A method for manufacturing an iron-based composite phosphate cathode material includes the following steps.

[0069] Sodium dihydrogen phosphate, sodium acetate, and citrate monohydrate were added to 5 kg of deionized water in a molar ratio of 1:3:5 and stirred continuously until a clear solution was formed. A certain proportion of solid iron phosphate was added to the clear solution to adjust the total solid content to 40%, wherein the iron phosphate was a nanometer-sized coacervate with a particle size of 20–95 nm. Next, sand milling was performed so that the viscosity of the solution gradually increased as the iron phosphate was dispersed in the solution, and sand milling was stopped when the viscosity of the solution reached 350 Pa·S. The solution was then spray-dried at a temperature of 120°C for a duration of 10 hours. Subsequently, the solution was calcined at a high temperature in an inert N2 atmosphere at a heating rate of 5°C / min, maintained at 300°C for 4 hours, maintained at 600°C for 10 hours, and after natural cooling, an iron-based composite phosphate cathode material was obtained.

[0070] Example 3

[0071] A method for manufacturing an iron-based composite phosphate cathode material includes the following steps.

[0072] Sodium dihydrogen phosphate, sodium acetate, and citrate monohydrate were added to 5 kg of deionized water in a molar ratio of 1:3:10 and stirred continuously until a clear solution was formed. A certain proportion of solid iron phosphate was added to the clear solution to adjust the total solid content to 30%, wherein the iron phosphate was a nanometer-sized coacervate with a particle size of 75–95 nm. Next, sand milling was performed so that the viscosity of the solution gradually increased as the iron phosphate was dispersed in the solution, and sand milling was stopped when the viscosity of the solution reached 400 Pa·S. The solution was then spray-dried at a spray-drying temperature of 80°C for a duration of 6 hours. Subsequently, the solution was calcined at a high temperature in an inert N2 atmosphere at a heating rate of 2.5°C / min, maintained at 290°C for 4.5 hours, and maintained at 585°C for 11 hours. After natural cooling, an iron-based composite phosphate cathode material was obtained.

[0073] Example 4

[0074] In the method for manufacturing an iron-based composite phosphate cathode material, the sodium source is sodium oxalate, the phosphorus source is sodium phosphate, and the carbon sources are glucose and citric acid, and the molar ratio of sodium oxalate, sodium phosphate, glucose, and citric acid is 0.5:1:1:2.5, and other conditions except for the above are the same as in Example 1.

[0075] Example 5

[0076] In the method for manufacturing an iron-based composite phosphate cathode material, the sodium source is sodium citrate, the phosphorus source is phosphoric acid, and the carbon sources are polyethylene glycol, glucose, and sucrose, and the molar ratio of sodium citrate, phosphoric acid, polyethylene glycol, glucose, and sucrose is 1:1:0.1:1:1.5, and other conditions except for the above are the same as in Example 1.

[0077] Comparative Example 1

[0078] In the method for manufacturing an iron-based composite phosphate cathode material, the total solid content is controlled to 25%, and sand milling is stopped when the viscosity of the solution reaches 250 Pa.S. Other conditions, excluding the above, are the same as in Example 1.

[0079] Comparative Example 2

[0080] In the method for manufacturing an iron-based composite phosphate cathode material, the total solid content is controlled to 45%, and sand milling is stopped when the viscosity of the solution reaches 280 Pa.S. Other conditions, excluding the above, are the same as in Example 1.

[0081] Experimental Example

[0082] The cathode materials of the examples and comparative examples were taken and mixed with acetylene black and PVDF, respectively. The mass ratio of the cathode material, acetylene black, and PVDF was 70:20:10. After coating the mixture onto an aluminum foil with a diameter of 19 mm, the aluminum foil was vacuum dried at 120°C for 12 hours to obtain a cathode sheet. A metallic sodium was used as the counter electrode, 1 mol / L NaClO4 vinyl carbonate / diethyl carbonate (volume ratio 1:1) was used as the electrolyte, the separator was Cellgard 2035, and the cells were assembled into a button cell in a glove box. The battery model was CR2016. A constant current charge / discharge test was performed on the battery, and the current density was 26 mA / g. The test results are as shown in Fig. 2, and the reversible specific capacity in the voltage range of 2.0 to 4.3 V is 109 mAh / g.

[0083] Performance tests for primary effect and capacity retention rate were performed on the batteries of the examples and comparative examples, and the results are shown in Table 1.

[0084] Battery performance test results By group 0.2C charging (mAh / g) 0.2C discharge (mAh / g) First cycle efficiency (%) 500-Cycle Retention Rate (%) Example 1 118 109 92 98 Example 2 115 106 92 96 Example 3 120 112 93 96 Comparative Example 1 92 90 98 89 Comparative Example 2 99 96 97 90

[0085] As can be seen from Table 1, the present disclosure controls the viscosity of the solution using an appropriate solid-liquid ratio, then realizes the dissolution of solid reactants during the polishing process to obtain a homogeneous reaction function, and the cathode material obtained through additional drying and sintering has excellent primary effects and capacity retention rate. The solid-liquid ratio and solution viscosity of Comparative Example 1 and Comparative Example 2 are not within the scope of protection of the present disclosure, and the capacity retention rate of the obtained cathode material is much different from the capacity retention rate of the cathode material of the present application.

[0086] Finally, it must be noted that the above embodiments are intended to illustrate the technical solutions of the present disclosure and are not limiting. Although the present disclosure has been described in detail with reference to each of the above embodiments, those skilled in the art should understand that the technical solutions described in each of the above embodiments may be modified or that some or all of the technical features may be replaced with equivalents, and such modifications or replacements do not deviate from the scope of the technical solutions of each of the embodiments of the present disclosure in terms of the essence of such technical solutions.

Claims

Claim 1 A method for manufacturing an iron-based composite phosphate cathode material comprises the steps of: uniformly mixing a sodium source, a phosphorus source, a carbon source, and water, and then mixing with iron phosphate to obtain a first mixing system; grinding the first mixing system to obtain a second mixing system, and then performing drying and sintering; wherein in the first mixing system, Na element, Fe element, (PO4) 3- A method for manufacturing an iron-based composite phosphate cathode material, characterized in that the total mass of the carbon source is 30 to 40% of the mass of the water; the viscosity of the second mixing system is 300 Pa.S or higher; and the sintering comprises performing a first sintering treatment under conditions of 290 to 310°C and performing a second sintering treatment by raising the temperature to 550 to 600°C. Claim 2 A method for manufacturing an iron-based composite phosphate cathode material according to claim 1, wherein the manufacturing method comprises at least one of the following technical features: (1) the sodium source comprises at least one of sodium acetate, sodium nitrate, sodium oxalate, sodium citrate, and sodium phosphate; (2) the phosphorus source comprises at least one of sodium dihydrogen phosphate, sodium phosphate, and phosphoric acid; (3) the carbon source comprises at least one of citric acid, glucose, sucrose, and polyethylene glycol; and (4) the molar ratio of the phosphorus source, the sodium source, and the carbon source is 1: (2.8~3.2): (1~10). Claim 3 A method for manufacturing an iron-based composite phosphate cathode material according to claim 1, wherein the manufacturing method comprises: (1) a molar ratio of Fe to P in the iron phosphate of 0.97 to 1; and (2) at least one of the technical features comprising the iron phosphate of micrometer-sized particles and / or nanometer-sized coacervates. Claim 4 A method for manufacturing an iron-based composite phosphate cathode material according to claim 1, characterized in that the particle size D90 of the iron phosphate in the second mixing system is 0.05μm to 0.15μm. Claim 5 A method for manufacturing an iron-based composite phosphate cathode material according to claim 1, characterized in that the viscosity of the second mixing system is 300 Pa.S to 400 Pa.S. Claim 6 A method for manufacturing an iron-based composite phosphate cathode material according to claim 1, wherein the manufacturing method comprises at least one of the following technical features: (1) the drying includes spray drying; and (2) the drying temperature is 80℃ to 120℃ and the drying time is 5h to 10h. Claim 7 A method for manufacturing an iron-based composite phosphate cathode material according to claim 1, wherein the manufacturing method comprises at least one of the following technical features: (1) the time of the first sintering treatment is 3h to 5h and the time of the second sintering treatment is 10h to 12h; and (2) the heating rate of the heating is 2℃ / min to 5℃ / min. Claim 8 delete Claim 9 delete Claim 10 delete

Citation Information

Patent Citations

  • Method for preparing Na4Fe3 (PO4) 2 (P2O7) by homogeneous phase method and application

    CN113060713A

  • Carbon-coated sodium ferrous fluorophosphate positive electrode active material, preparation thereof and application of carbon-coated sodium ferrous fluorophosphate positive electrode active material in sodium ion battery