Method for producing polyester resin

By esterifying dicarboxylic acid and aliphatic diol with triphenylphosphine oxide during advanced stages, the method achieves efficient and cost-effective flame retardancy in polyester resins, addressing the inefficiencies of existing methods.

KR103045831B1Active Publication Date: 2026-11-06LG CHEM LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020210155690
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-11-12
Publication Date
2026-11-06
Estimated Expiration
2041-11-12

AI Technical Summary

Technical Problem

Existing methods for manufacturing polyester resins with flame retardancy are costly and inefficient, particularly due to the limitations of reactive flame retardants and the need to replace halogen-based materials, while additive methods compounding processes reduce productivity.

Method used

A method involving esterification of dicarboxylic acid or its derivative and an aliphatic diol with a catalyst, followed by the addition of triphenylphosphine oxide at 0.1 to 15.0 weight% during the esterification reaction's advanced stage, and subsequent polycondensation, ensures even dispersion and improved flame retardancy without altering the resin's properties.

Benefits of technology

This method enhances flame retardancy, improves productivity, and reduces costs by allowing wide applicability across various polyesters without requiring specific polymerization conditions, maintaining production stability and maximizing the flame retardant effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a polyester resin. The method for manufacturing the polyester resin can provide a polyester resin having excellent flame retardancy while improving productivity and reducing costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a polyester resin. More specifically, it relates to a method for manufacturing a polyester resin having excellent flame retardancy while improving productivity and reducing costs. Background Technology

[0002] Most flame-retardant materials have been manufactured through the mixing and addition of additives via post-processing steps such as compounding. Consequently, there are structural limitations where the introduction of additional processes leads to disadvantages in productivity and increased costs. Furthermore, since a precise quantitative level of flame retardant must be added in proportion to achieve flame retardancy, there is a burden of increased costs when manufacturing highly flame-retardant materials.

[0003] Materials primarily used as flame retardants fall into two main categories: reactive and additive types. Among these, reactive flame retardants can be viewed as co-monomers that possess functional groups within their molecules and exhibit flame retardancy by directly reacting with polymer resins to form chemical bonds within their chains, whereas additive flame retardants simply mix into the polymer resin and physically disperse to produce a flame retardant effect.

[0004] Among these, reactive flame retardants have the advantage of minimal physical state changes after processing, such as migration; however, there are limitations on the applicable content when manufacturing flame-retardant materials using reactive flame retardants, and excessive application may render the polymerization of the material impossible. Furthermore, because reactive flame retardants bond directly to polymer chains, they can cause significant changes to the intrinsic properties of the polymer resin.

[0005] Therefore, reactive flame retardants are difficult to apply widely because specific polymerization conditions are required for their addition. For example, reactive flame retardants used in PET polyesters are difficult to use in PBT polymerization because the PBT polymerization conditions are unsuitable for initiating the reactive flame retardant. In other words, the use of reactive flame retardants presents difficulties such as content limitations, changes in physical properties, and poor scalability.

[0006] Furthermore, due to recent environmental issues, the use of halogen-based flame retardants, which have traditionally been the mainstream, is being restricted, creating a need to replace them with non-halogen flame retardant materials.

[0007] Therefore, there is a need to develop a new method for manufacturing polyester resins that efficiently and effectively imparts flame retardancy. The problem to be solved

[0008] The present invention provides a method for manufacturing a polyester resin having excellent flame retardancy while improving productivity and reducing costs. means of solving the problem

[0009] The present specification provides a method for producing a polyester resin, comprising the steps of: esterifying a dicarboxylic acid or a derivative thereof and an aliphatic diol in the presence of a catalyst including a titanium-based catalyst or a tin-based catalyst; adding triphenylphosphine oxide in an amount of 0.1 to 15.0 weight% of the theoretical production amount of the polyester resin at a time when the esterification reaction has progressed by 80% or more; and polycondensing the esterification reaction product.

[0011] A method for manufacturing a polyester resin according to a specific embodiment of the invention will be described in more detail below.

[0012] The terms used herein are merely for describing exemplary embodiments and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, terms such as “comprising,” “comprising,” or “having” are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0013] The present invention is capable of various modifications and may take various forms, and specific embodiments are illustrated and described in detail below. However, this is not intended to limit the invention to the specific disclosed forms, and it should be understood that the invention includes all modifications, equivalents, and substitutions that fall within the spirit and scope of the invention.

[0015] According to one embodiment of the invention, a method for producing a polyester resin may be provided, comprising the steps of: esterifying a dicarboxylic acid or a derivative thereof and an aliphatic diol in the presence of a catalyst including a titanium-based catalyst or a tin-based catalyst; adding triphenylphosphine oxide in an amount of 0.1 to 15.0 weight% of the theoretical production amount of the polyester resin at a time when the esterification reaction has progressed by 80% or more; and polycondensing the esterification reaction product.

[0016] The inventors conducted research on a method for manufacturing a polyester resin and confirmed through experiments that if triphenylphosphine oxide is added to the reaction solution in a predetermined amount at the end of the esterification reaction, for example when the reaction has progressed by 80% or more, and the product of the esterification reaction is polycondensed, a polyester resin with excellent flame retardancy and improved productivity and reduced cost can be manufactured, and thus completed the invention.

[0017] The method for manufacturing a polyester resin according to the above embodiment includes the step of adding triphenylphosphine oxide in a predetermined amount at a specific time. The triphenylphosphine oxide (TPPO) is an additive flame retardant and exists in a physically dispersed state within the resulting polyester, thereby improving production stability without causing significant changes to the physical properties of the raw material and enabling excellent and efficient flame retardancy to be expressed in the manufactured polyester resin.

[0018] In addition, the polyester manufacturing method of the above embodiment is advantageous for increasing the content compared to when using a reactive flame retardant, and since it does not require specific polymerization conditions for initiating the flame retardant, it can be widely used in the manufacture of various polyesters. Furthermore, compared to conventional post-processing processes such as compounding, the manufacturing process is simplified, productivity is improved, and the flame retardant effect can be maximized excellently and efficiently.

[0019] In the above method for manufacturing the polyester resin, at the end of the esterification reaction, for example, when the esterification reaction has progressed 80% or more, the amount may be added in an amount of 0.1% or more, or 0.2% or more, or 0.3% or more with respect to the theoretical production amount of the polyester resin, and in an amount of 15% or less, or 12% or less, or 10% or less. Or it may be added in an amount of 0.1 to 15.0%, or 0.2 to 12.0%, or 0.3 to 10.0%.

[0020] Meanwhile, the theoretically expected production amount (weight) of polyester resin can be calculated from the following mathematical formula 1.

[0021] [Mathematical Formula 1]

[0022] Theoretical yield of polyester resin = (Usage of dicarboxylic acid or its derivative (g) / Molecular weight of dicarboxylic acid or its derivative (g / mol)) x Molecular weight of polyester repeating unit (g / mol)

[0024] If the content of the added triphenylphosphine oxide is less than 0.1 weight% relative to the theoretical production amount of the polyester resin, there may be a problem that the flame retardancy of the polyester resin produced is insufficient, and if the content of the triphenylphosphine oxide exceeds 15 weight% relative to the theoretical production amount of the polyester resin, there is a concern that the polymerization reactivity of the polyester resin will decrease, thereby reducing productivity.

[0025] At this time, the point in time when the esterification reaction has proceeded by 80% or more means the point in time when the dicarboxylic acid or its derivative has reacted by 80% or more, and the extent of the esterification reaction can be calculated from the theoretical amount of water or alcohol produced as a byproduct.

[0026] In other words, the theoretical amount of water or alcohol produced as a byproduct of the esterification reaction can be calculated from the content of the starting material input into the reaction, and the extent of the reaction can be determined by measuring and comparing the amount of water or alcohol produced during the reaction.

[0027] For example, if the theoretical production amount of water or alcohol is 100 ml, triphenylphosphine oxide can be added at the point when 80 ml or more of byproduct is produced during the reaction.

[0028] At this time, the theoretical amount of the above byproduct (water or alcohol) can be calculated from the following mathematical formula 2.

[0029] [Mathematical Formula 2]

[0030] Theoretical amount of byproduct = (Usage of dicarboxylic acid or its derivative (g) x 2 x Molecular weight of byproduct (g / mol)) / (Molecular weight of dicarboxylic acid or its derivative (g / mol))

[0032] That is, twice the number of moles of the dicarboxylic acid or its derivative added as byproducts is theoretically produced, and based on this, the actual amount of byproducts produced can be measured to calculate the extent of the reaction.

[0033] Since triphenylphosphine oxide is introduced when the above esterification reaction has progressed to 80% or more, 90% or more, or 99% or more, it is possible to prevent the deterioration of the purity of the esterification reaction due to potential side reactions, and there is an advantage in the maintenance of the esterification reactor in the production process.

[0034] Meanwhile, at the point where the esterification reaction is 80% or more complete, the viscosity of the reaction solution may be 10 cP or more, or 15 cP or more, or 20 cP or more, and 50 cP or less, or 45 cP or less, or 40 cP or less. Or it may be 10 to 50 cP, or 15 to 45 cP, or 20 to 40 cP.

[0035] The above reaction solution refers to the total amount of material in the reactor, including all products generated as a catalyst carries out an esterification reaction with a dicarboxylic acid or its derivative, an aliphatic diol, unreacted reactants, and intermediates.

[0036] When the above reaction solution has a predetermined viscosity, if triphenylphosphine oxide is added in a specific amount, the triphenylphosphine oxide is evenly dispersed within the final polyester resin formed, thereby maximizing the flame retardant effect.

[0037] If the viscosity of the above reaction solution is less than 10 cP, the esterification reaction is not sufficiently carried out, which may lead to an increase in the amount of unreacted raw material and a decrease in productivity; if it exceeds 50 cP, it may be difficult for triphenylphosphine oxide to be evenly dispersed within the reaction solution, which may reduce the flame retardancy of the resulting polyester resin. In particular, this problem may worsen as the content of added triphenylphosphine oxide increases.

[0038] Meanwhile, the method of adding the above triphenylphosphine oxide is not limited, and it can be added when the esterification reaction has progressed more than 80% and the weak vacuum in the esterification reactor has been released through nitrogen purging, or it can also be added through an automated injection facility while maintaining a weak vacuum.

[0039] In addition, for ease of introduction, the triphenylphosphine oxide may be introduced in a liquid state dissolved in an aliphatic diol, or it may be introduced in a solid state (powder).

[0040] Meanwhile, the above esterification reaction may be carried out for about 30 minutes to 240 minutes, or 2 hours to 3 hours, at a temperature of 180 to 280 ℃, or 200 to 260 ℃, or 220 to 240 ℃ and a pressure of 250 to 550 torr, or 300 to 500 torr, or 350 to 450 torr.

[0041] Within this range, the esterification reaction can proceed sufficiently, and side reactions such as thermal decomposition can be minimized.

[0042] If the reaction is carried out under atmospheric pressure (760 torr), the evaporation rate of the aliphatic diol may decrease, but the conversion rate of the esterification reaction may decrease; if carried out under reduced pressure, the evaporation rate of the aliphatic diol may be too high, making it impossible to maintain an appropriate molar ratio of the dicarboxylic acid or its derivative and the aliphatic diol.

[0043] The above esterification reaction conditions can be appropriately adjusted according to the specific characteristics of the polyester being manufactured, the molar ratio of the dicarboxylic acid or its derivative and the aliphatic diol, or process conditions, etc.

[0044] In addition, the above esterification reaction can be carried out in a batch or continuous manner, and each raw material can be introduced separately or in the form of a slurry in which a dicarboxylic acid or a derivative thereof is mixed with an aliphatic diol.

[0045] The above dicarboxylic acid or derivative thereof is a term referring to one or more of dicarboxylic acid and its derivatives, and the derivative of the dicarboxylic acid means a dicarboxylic acid alkyl ester or a dicarboxylic acid anhydride.

[0046] In a manufacturing method according to one embodiment, one or more selected from the group consisting of terephthalic acid, dimethyl terephthalate, isophthalic acid, dimethyl isophthalate, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, 1,5-naphthalene dicarboxylic acid, dimethyl 1,5-naphthalene dicarboxylate, 1,4-cyclohexane dicarboxylic acid, and dimethyl 1,4-cyclohexane dicarboxylate may be used as the dicarboxylic acid or a derivative thereof. Among these, it is preferable to use terephthalic acid or dimethyl terephthalate.

[0047] Meanwhile, the above-mentioned aliphatic diol may specifically be an aliphatic diol having a molecular weight of 50 to 300 g / mol. As such aliphatic diol, one or more selected from the group consisting of ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol may be used. Among these, it is preferable to use 1,4-butanediol.

[0048] Unless otherwise noted, the molecular weight of the above-mentioned aliphatic diol can be measured at 40°C by gel permeation chromatography (GPC) after dissolving the sample in tetrahydrofuran, for example, and polystyrene can be used as a standard material.

[0049] In the above esterification reaction, the molar ratio of the dicarboxylic acid or its derivative to the aliphatic diol may be 1.2:1 to 2.2:1, or 1.4:1 to 2.0:1, or 1.6:1 to 1.8:1. Within this range, the reaction balance is excellent, allowing the reaction to proceed smoothly.

[0050] If the molar ratio of the above dicarboxylic acid or its derivative to the aliphatic diol is less than 1.2:1, the esterification reaction may be reduced, which may lower the productivity of the resin, and if the molar ratio of the above dicarboxylic acid or its derivative to the aliphatic diol exceeds 2.2:1, there may be problems with the quality of the resin due to side reactions caused by excessive reactivity.

[0051] Meanwhile, the esterification reaction in which a dicarboxylic acid or its derivative reacts with an aliphatic diol is carried out in the presence of a catalyst, and the catalyst may be a material known in the art.

[0052] Specifically, the catalyst may be a catalyst comprising titanium or tin as an active metal, and more specifically, the catalyst may be a titanium-based catalyst such as tetrabutyltitanate (TBT), tetraethyltitanate, or tetra(isopropyl)titanate; or a tin-based catalyst such as n-butylstanoic acid, octylstanoic acid, dimethyltin oxide, dibutyltin oxide, dioctyltin oxide, diphenyltin oxide, tri-n-butyltin acetate, tri-n-butyltin chloride, or tri-n-butyltin fluoride. In addition, in addition to the catalysts mentioned above, catalysts such as oxides or acetates comprising Mg, Ca, Mn, Zn, Pb, Zr, etc., as active metals may be used alone or in combination. Among these, a titanium-based catalyst such as TBT may be preferably used.

[0053] The catalyst may be used in an amount of 0.01 to 1 part by weight, or 0.03 to 0.7 parts by weight, or 0.05 to 0.5 parts by weight, based on a total of 100 parts by weight of the dicarboxylic acid or its derivative, aliphatic diol, and catalyst, and reaction efficiency may be maximized within this range.

[0054] Meanwhile, at the point when the above esterification reaction has progressed by more than 80%, the addition of triphenylphosphine oxide can be carried out for 10 to 40 minutes, or 20 to 30 minutes, at a pressure of 250 to 550 torr, or 350 to 450 torr.

[0055] In addition, the addition of the triphenylphosphine oxide may be carried out at a temperature of 180 to 280 ℃, 200 to 260 ℃, or 220 to 240 ℃ for 10 to 40 minutes, or 20 to 30 minutes.

[0056] As described above, after carrying out the esterification reaction at a predetermined temperature and pressure, triphenylphosphine oxide is added when the esterification reaction has progressed by more than 80%, and then a polycondensation reaction is carried out at the temperature and pressure described below.

[0057] At this time, if the pressure is reduced for a sufficient period after adding the triphenylphosphine oxide and then the temperature is increased to change to the expansion condensation reaction conditions, the triphenylphosphine oxide can be sufficiently mixed into the esterification reaction product and physically dispersed appropriately, and since there is no abrupt change in reaction conditions, changes in physical properties are minimal and production stability can be improved.

[0058] Meanwhile, the above polycondensation reaction may be carried out for about 30 minutes to 5 hours, or 1 to 3 hours, at a temperature of 200 to 300 ℃, or 220 to 280 ℃, or 240 to 260 ℃ and a pressure of 0.1 to 1 torr.

[0059] Within this range, a sufficient increase in molecular weight can be achieved, and side reactions such as thermal decomposition can be minimized.

[0060] If the temperature and pressure conditions of the above polycondensation reaction are exceeded, by-products cannot be effectively removed, and the physical properties of the manufactured polyester resin may deteriorate.

[0061] Meanwhile, in the present invention, a catalyst comprising a titanium-based catalyst or a tin-based catalyst can be introduced not only in the esterification reaction but also together with the triphenylphosphine oxide or in the polycondensation step.

[0062] Specifically, the catalyst may be added to a reaction product containing a dicarboxylic acid or its derivative and an aliphatic diol together with triphenylphosphine oxide at a point when the esterification reaction has progressed by more than 80%, may be added to the esterification reaction product before the start of the polycondensation reaction, or may be added during the esterification reaction step.

[0063] The catalyst introduced together with the above-mentioned triphenylphosphine oxide or during the polycondensation step may be a material known in the art, and specific examples are as described above.

[0064] In addition, various additives known in the technical field to which the present invention belongs may be added during the esterification reaction and polycondensation reaction steps. Specifically, antioxidants such as hindered phenol-based antioxidants, diphenylamine-based antioxidants, or metal complex antioxidants; or light stabilizers such as hindered amine-based light stabilizers; etc. may be added.

[0065] Meanwhile, the polyester produced by the method for manufacturing the polyester resin of the above embodiment can exhibit excellent flame retardancy, with a flame retardancy rating of V-0 measured on a specimen with a thickness of 3.0 mm according to UL 94 standards. Effects of the invention

[0066] According to the present invention, a method for manufacturing a polyester resin having excellent flame retardancy while improving productivity and reducing costs can be provided. Specific details for implementing the invention

[0067] The operation and effects of the invention will be explained in more detail below through specific embodiments. However, these are presented as examples of the invention and do not limit the scope of the invention in any way.

[0069] Example 1

[0070] (1) 1887 g of terephthalic acid, 1739 g of 1,4-butanediol and 0.775 g of tributyltin (TBT) were added to a reactor, and the temperature was raised to 200 ℃ while stirring under reflux and a weak vacuum (350 to 450 torr), and then the etherification reaction was carried out by raising the temperature to 230 ℃ for 2 to 3 hours.

[0071] (2) Afterwards, at the point when the esterification reaction proceeded at 80% or more (water production amount 327 ml), 7.5 g of triphenylphosphine oxide was dissolved in 200 g of 1,4-butanediol (concentration of about 40 wt% based on triphenylphosphine oxide) and then added to the reactor along with 6 g of tributyltin.

[0072] At this time, the added triphenylphosphine oxide was set to 0.3 weight% of the theoretical production amount of the polyester resin below.

[0073] Afterwards, the pressure was slowly reduced to a vacuum of 1 torr or less over 30 to 40 minutes, and the temperature was raised to 255 ℃.

[0074] (3) Polycondensation reaction was performed at a final state of 255 ℃ and 0.3~0.9 torr, and when the polymerization termination torque was reached, the reaction was stopped and the mixture was pressurized and discharged into cold water to obtain pelletized polybutylene terephthalate.

[0076] Example 2

[0077] Polybutylene terephthalate was prepared in the same manner as in Example 1, except that the content of triphenylphosphine oxide in Example 1 was adjusted to 25 g (1.0 wt% of the theoretical production amount of polyester resin).

[0079] Example 3

[0080] Polybutylene terephthalate was prepared in the same manner as in Example 1, except that the content of triphenylphosphine oxide in Example 1 was adjusted to 50 g (2.0 wt% of the theoretical production amount of polyester resin).

[0082] Example 4

[0083] Polybutylene terephthalate was prepared in the same manner as in Example 1, except that the content of triphenylphosphine oxide in Example 1 was adjusted to 125 g (5.0 wt% of the theoretical production amount of polyester resin).

[0085] Example 5

[0086] Polybutylene terephthalate was prepared in the same manner as in Example 1, except that the content of triphenylphosphine oxide in Example 1 was adjusted to 250 g (10.0 wt% of the theoretical production amount of polyester resin).

[0088] Comparative Example 1

[0089] 50g of triphenylphosphine oxide was added to 950g of polybutylene terephthalate (Tunher, TH6098, etc.) by compounding using a twin-screw extruder. At this time, the temperature was set to 230 to 260 ℃, the screw rotation speed was set to 200 to 350 rpm, and the feed rate was set to 40 to 90 kg / h.

[0091] Comparative Example 2

[0092] Polybutylene terephthalate was prepared in the same manner as in Example 1, except that triphenylphosphine oxide was not added in Example 1.

[0094] Comparative Example 3

[0095] Polybutylene terephthalate was prepared in the same manner as in Example 1, except that 25 g of 3-(hydroxyphenylphosphinyl)propanoic acid (3-HPP) was added instead of triphenylphosphine oxide in Example 1 (1.0 wt%).

[0097] Comparative Example 4

[0098] Polybutylene terephthalate was prepared in the same manner as in Example 1, except that 75 g of 3-(hydroxyphenylphosphinyl)propanoic acid (3.0 wt%) of the theoretical yield of the polyester resin was added instead of triphenylphosphine oxide in Example 1.

[0100] Test Example: Evaluation of Physical Properties of Polyester Resin

[0101] (1) Melt Index

[0102] It was measured at 235°C and under a load of 2.16 kg in accordance with ASTM D1238.

[0104] (2) Melting point (Tm)

[0105] The melting point was measured using a Differential Scanning Calorimeter (DSC, device name: DSC 2920, manufacturer: TA instrument). Specifically, polybutylene terephthalate was heated to 250°C and maintained at that temperature for 5 minutes, then cooled down to 20°C and then increased again, with the rate of temperature increase and decrease each controlled to 10°C / min.

[0107] The melt index and melting point of the polyester resins prepared in the examples and comparative examples were measured using the method described above, and the results are shown in Table 1.

[0108] Polymerization termination torque (Ncm) PC response time (minutes) MI(2.16kg, 235℃) Tm(℃) Example 1 69.0 70.0 20.0 221.2 Example 2 70.0 58.0 9.0 221.4 Example 3 72.0 59.0 7.5 221.0 Example 4 66.0 66.0 20.7 220.6 Example 5 70.0 60.0 14.1 220.3 Comparative Example 1 - - 25.5 220.7 Comparative Example 2 60.0 68.0 12.3 219.9 Comparative Example 3 16.0 150.0 191.0 Unmeasurable Comparative Example 4 0.0 180.0 Unmeasurable Unmeasurable

[0109] Referring to Table 1 above, it can be confirmed that the manufacturing method according to one embodiment of the present invention, which includes the step of adding a predetermined triphenylphosphine oxide and carrying out a polycondensation reaction when the esterification reaction has progressed by more than 80%, has a polymerization rate equal to or greater than that of Comparative Example 2, which did not add triphenylphosphine oxide, and at the same time, does not cause a significant change in basic physical properties such as Tm.

[0110] In addition, Comparative Examples 3 and 4, which used a reactive flame retardant, showed that the reaction time and melt index increased, indicating that the polyester was not polymerized smoothly.

[0112] (3) Flame retardancy (UL 94 Protocol)

[0113] Flame retardancy was evaluated in accordance with the UL 94 standard. Specifically, a flame-retardant specimen with a thickness of 3.0 mm required for the flame retardant test was prepared and evaluated according to the following.

[0114] First, a flame 20 mm high was applied to the specimen for 10 seconds, the combustion time (t1) of the specimen was measured, and the combustion pattern was recorded. Then, after the combustion ended following the first application of the flame, the combustion time (t2) of the specimen was measured again after applying the flame for 10 seconds, and the combustion pattern was recorded. After performing this five times using specimens of the same specifications, the results were evaluated according to the criteria in Table 2 below, and the results are shown in Table 3.

[0115] Flame retardant rating V-0 V-1 V-2 Individual combustion time (t1 or t2 of individual specimens) 10 seconds or less 30 seconds or less 30 seconds or less Total combustion time of 5 specimens (sum of t1 and t2 of 5 specimens) 50 seconds or less 250 seconds or less 250 seconds or less Whether or not it drops flame-emitting particles doesn't exist doesn't exist is available

[0116] division 1 2 3 4 5 sec rating 1st 2nd 1st 2nd 1st 2nd 1st 2nd 1st 2nd * PBT 4 17 22 200 45 22 33 15 358 - Example 4 4.1 1.7 2.7 1.5 2.1 1.9 2.1 1.8 6.2 2.5 27 V-0 Comparative Example 1 22 8.2 15.8 4.6 2.8 8 28.2 9 31.3 12 142 V-2

[0117] * PBT: PBT TH6098(IV 0.98), PBT Base Resin

[0119] According to Table 3 above, it can be confirmed that the polyester manufacturing method according to one embodiment of the present invention has superior flame retardancy compared to Comparative Example 1, which was manufactured by a compounding method. Meanwhile, in the case of PBT, it was not possible to assign a grade because it had no flame retardancy.

Claims

Claim 1 A method for producing a polyester resin, comprising: a step of esterifying a dicarboxylic acid or its derivative and an aliphatic diol in the presence of a catalyst including a titanium-based catalyst or a tin-based catalyst; a step of adding triphenylphosphine oxide in an amount of 0.1 to 15.0 weight% of the theoretical production amount of the polyester resin before starting the polycondensation reaction at a point when the esterification reaction has proceeded by 80 mol% or more; and a step of polycondensing the esterification reaction product. Claim 2 delete Claim 3 A method for manufacturing a polyester resin according to claim 1, wherein the viscosity of the reaction solution is 10 to 50 cP at the point when the esterification reaction proceeds at 80 mol% or more. Claim 4 A method for manufacturing a polyester resin according to claim 1, wherein the triphenylphosphine oxide is introduced in a liquid or solid state dissolved in an aliphatic diol. Claim 5 A method for manufacturing a polyester resin according to claim 1, wherein the esterification reaction is performed for 30 minutes to 240 minutes at a temperature of 180 to 280 ℃ and a pressure of 250 to 550 torr. Claim 6 A method for manufacturing a polyester resin according to claim 1, wherein the addition of the triphenylphosphine oxide is performed at a pressure of 250 to 550 torr for 10 to 40 minutes. Claim 7 A method for manufacturing a polyester resin according to claim 1, wherein the addition of the triphenylphosphine oxide is performed at a temperature of 180 to 280 ℃ for 10 to 40 minutes. Claim 8 A method for manufacturing a polyester resin according to claim 1, wherein the polycondensation reaction is performed for 30 minutes to 300 minutes at a temperature of 200 to 300 ℃ and a pressure of 0.01 to 1.0 torr. Claim 9 A method for producing a polyester resin according to claim 1, wherein the molar ratio of the dicarboxylic acid or its derivative to the aliphatic diol in the esterification reaction is 1.2:1 to 2.2:

1. Claim 10 A method for manufacturing a polyester resin according to claim 1, wherein the dicarboxylic acid or its derivative is one or more selected from the group consisting of terephthalic acid, dimethyl terephthalate, isophthalic acid, dimethyl isophthalate, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, 1,5-naphthalene dicarboxylic acid, dimethyl 1,5-naphthalene dicarboxylate, 1,4-cyclohexane dicarboxylic acid, and dimethyl 1,4-cyclohexane dicarboxylate. Claim 11 A method for manufacturing a polyester resin according to claim 1, wherein the aliphatic diol is an aliphatic diol having a molecular weight of 50 to 300 g / mol. Claim 12 A method for manufacturing a polyester resin according to claim 1, wherein a catalyst is additionally added together with the triphenylphosphine oxide to a reaction product comprising a dicarboxylic acid or a derivative thereof and an aliphatic diol at a point when the esterification reaction has proceeded by 80 mol% or more. Claim 13 A method for manufacturing a polyester resin according to claim 1, wherein the polyester resin has a flame retardancy rating of V-0 as measured on a specimen having a thickness of 3.0 mm in accordance with UL 94 standards.

Citation Information

Patent Citations

  • Method for manufacturing polyester

    JP2008095078A

  • Process for preparing polybutylene terephthalate

    KR1019920009688B1