Method for preparing graft copolymer containing natural rubber and thermoplastic resin composition comprising the same

By crosslinking natural rubber latex with a multi-double-bond agent and emulsion polymerizing with butadiene rubber, the method addresses low mechanical and gloss issues in ABS resin production, achieving reduced emissions and improved productivity.

KR103046275B1Active Publication Date: 2026-11-11KOREA KUMHO PETROCHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020240143764
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2026-11-11
Estimated Expiration
2044-10-21

AI Technical Summary

Technical Problem

Existing methods for producing ABS resin using natural rubber latex face issues such as insufficient crosslinking density, leading to low mechanical properties and poor gloss, and require additional equipment and complex processes, which increase costs and environmental impact.

Method used

A method involving crosslinking natural rubber latex with a crosslinking agent having three or more double bonds, mixing it with butadiene rubber latex, and emulsion polymerizing with a monomer mixture to produce a graft copolymer, using existing equipment and bio-based materials to enhance mechanical and appearance properties.

Benefits of technology

This approach reduces greenhouse gas emissions, maintains excellent mechanical properties and gloss, and improves productivity by utilizing existing equipment without additional costs or complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024114149011-PAT00001
    Figure 112024114149011-PAT00001
  • Figure 112024114149011-PAT00002
    Figure 112024114149011-PAT00002
Patent Text Reader

Abstract

A method for manufacturing a natural rubber-containing graft copolymer is provided, comprising the steps of: crosslinking a natural rubber latex with a crosslinking agent to obtain a crosslinked natural rubber latex having a gel content of 50 to 95%; mixing the crosslinked natural rubber latex with butadiene rubber latex to obtain a mixed rubber latex; and mixing the mixed rubber latex with a monomer mixture and emulsion polymerizing to obtain a graft copolymer; and a thermoplastic resin composition comprising the natural rubber-containing graft copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a natural rubber-containing graft copolymer and a thermoplastic resin composition comprising the natural rubber-containing graft copolymer. Background Technology

[0002] The issues of climate change and global warming are intensifying worldwide, leading to various efforts across multiple industrial sectors aimed at reducing greenhouse gas emissions, recycling resources, and achieving sustainable development. In particular, as the petrochemical industry is identified as a major source of carbon emissions due to its reliance on fossil fuel-based raw materials, research on transitioning to eco-friendly materials and on circular manufacturing and recycling technologies is continuously underway. This is regarded as a crucial strategy to reduce carbon emissions throughout a product's life cycle and minimize its environmental impact.

[0003] Among various thermoplastic resins, ABS (acrylonitrile-butadiene-styrene) resin is widely used in diverse fields, such as automotive parts, electronic device casings, and home appliances, due to its excellent mechanical strength and superior appearance quality. However, since ABS resin is primarily manufactured using fossil fuel-based raw materials, it presents a problem in that significant amounts of greenhouse gases are generated during the production and disposal processes. Accordingly, various studies and technological developments are being attempted to reduce the environmental impact of ABS resin.

[0004] One such method is recycling technology, with mechanical and chemical recycling being the representative approaches. Mechanical recycling involves collecting waste plastics, separating, washing, and processing them to remake products; it is relatively simple and cost-effective. However, this process can lead to a degradation of material properties due to repetitive processing, and residual impurities may compromise product quality. Chemical recycling involves breaking down waste plastics into their original monomers or other compounds for reuse; while it offers the advantage of securing high-quality recycled materials, its commercial application is limited due to complex processes and high energy consumption. Furthermore, concerns have been raised regarding the high costs and environmental side effects associated with this process.

[0005] To address these issues, the development of materials utilizing bio-based raw materials is gaining increasing attention. Bio-based raw materials are sustainable resources that can replace fossil fuels and contribute to reducing carbon emissions and minimizing environmental impact during the production process. Natural rubber latex is one such bio-based raw material; extracted from natural resources, it is renewable and offers excellent elasticity and durability.

[0006] Patent Document 1 describes prior art related to this. Patent Document 1 proposes a method for producing ABS resin by crosslinking natural rubber latex using divinylbenzene (DVB) and then mixing a separately prepared graft copolymer with an existing graft copolymer. However, this method has several limitations. Divinylbenzene is a crosslinking agent with two unsaturated double bonds, and it has the disadvantage that the crosslinking density is insufficient, resulting in low mechanical properties of the final ABS resin and poor gloss characteristics. Furthermore, additional equipment and reaction vessels are required to prepare a separate graft copolymer and then mix it with an existing product, which complicates the production process and causes costs to increase. Prior art literature

[0007] International Open Publication No. WO 2012 / 161667 The problem to be solved

[0008] The present invention is intended to solve the problems of the aforementioned prior art, and one of the various objectives of the present invention is to provide a method for manufacturing a natural rubber-containing graft copolymer that is environmentally friendly and highly productive using natural raw materials.

[0009] Another objective of the present invention is to provide a thermoplastic resin composition having excellent mechanical properties and appearance characteristics. means of solving the problem

[0010] According to one aspect, a method for manufacturing a natural rubber-containing graft copolymer is provided, comprising the steps of: crosslinking a natural rubber latex with a crosslinking agent to obtain a crosslinked natural rubber latex having a gel content of 50 to 95%; mixing the crosslinked natural rubber latex with butadiene rubber latex to obtain a mixed rubber latex; and mixing the mixed rubber latex with a monomer mixture and emulsion polymerizing to obtain a graft copolymer.

[0011] In one embodiment, the crosslinking agent may have three or more double bonds.

[0012] In one embodiment, the crosslinking agent having three or more double bonds may be at least one selected from the group consisting of trialyl isocyanurate, trialyl cyanurate, trialyl trimetate, trimethylolpropane triacrylate, and trialylamine.

[0013] In one embodiment, the content of the crosslinking agent may be 0.1 to 2 weight percent based on 100 weight percent of the natural rubber latex.

[0014] In one embodiment, the gel content of the butadiene rubber latex may be 75 to 90%.

[0015] In one embodiment, the rubber particle size of the butadiene rubber latex may be 1,000 to 4,000 Å.

[0016] In one embodiment, the mixed rubber latex may include the cross-linked natural rubber latex and the butadiene rubber latex in a weight ratio of 20:80 to 80:20.

[0017] In one embodiment, in the step of obtaining the graft copolymer, the mixed rubber latex and the monomer mixture may be mixed in a weight ratio of 40:60 to 70:30.

[0018] In one embodiment, the monomer mixture may include an aromatic vinyl monomer and an unsaturated nitrile monomer in a weight ratio of 70:30 to 80:20.

[0019] In one embodiment, the graft rate of the graft copolymer may be 25 to 60%.

[0020] According to another aspect, a natural rubber-containing graft copolymer produced by the above-described manufacturing method is provided.

[0021] According to another aspect, a thermoplastic resin composition is provided comprising 20 to 50 weight% of the natural rubber-containing graft copolymer and 50 to 80 weight% of an aromatic vinyl compound-unsaturated nitrile compound copolymer. Effects of the invention

[0022] According to the present invention, there is an advantage in that greenhouse gas emissions can be reduced by converting fossil fuels into bio-fuels.

[0023] According to the present invention, the same equipment as the existing graft copolymer manufacturing equipment can be used as is without additional equipment, so there is an advantage of excellent productivity.

[0024] According to the present invention, there is an advantage of being able to provide a thermoplastic resin having excellent gloss and adhesion properties without a reduction in mechanical properties.

[0025] The effects of the present invention are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configuration described in the description of the invention or the claims. Specific details for implementing the invention

[0026] The present invention will be described below based on specific examples. However, the details described in this specification may be implemented in various different forms and are therefore not limited to the embodiments described herein.

[0027] Throughout the specification, when a part is described as "including" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but rather allows for the inclusion of additional components.

[0028] When a range of numerical values ​​is described in this specification, unless a specific range is otherwise described, the value has the precision of significant figures provided according to the standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.

[0029] Terms including ordinal numbers, such as ‘first’ or ‘second’ as used in this specification, may be used to describe various components or steps, but such components or steps should not be limited by ordinal numbers. Terms including ordinal numbers should be interpreted solely for the purpose of distinguishing one component or step from other components or steps.

[0030] Method for manufacturing a natural rubber-containing graft copolymer

[0031] A method for manufacturing a natural rubber-containing graft copolymer, which is one aspect of the present invention, comprises: (a) a step of crosslinking a natural rubber latex with a crosslinking agent to obtain a crosslinked natural rubber latex having a gel content of 50 to 90%; (b) a step of mixing the crosslinked natural rubber latex with butadiene rubber latex to obtain a mixed rubber latex; and (c) a step of mixing the mixed rubber latex with a monomer mixture and emulsion polymerizing to obtain a graft copolymer.

[0032] Natural rubber can be ordinary natural rubber or modified natural rubber.

[0033] Any natural rubber known as natural rubber can be used, and its country of origin is not limited. Natural rubber contains cis-1,4-polyisoprene as the main component, but may also contain trans-1,4-polyisoprene depending on the required characteristics. Therefore, in addition to natural rubber containing cis-1,4-polyisoprene as the main component, natural rubber may also include natural rubber containing trans-1,4-isoprene as the main component, such as balata, a type of rubber from the Sapotaceae family in South America.

[0034] Modified natural rubber refers to ordinary natural rubber that has been modified or refined. Examples of modified natural rubber include epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR), and hydrogenated natural rubber.

[0035] The crosslinking agent may refer to a monomer having three or more double bonds. A monomer having three or more double bonds may be, for example, at least one selected from the group consisting of trialyl isocyanurate, trialyl cyanurate, trialyl trimetate, trimethylolpropane triacrylate, and trialylamine, but is not limited thereto.

[0036] Butadiene rubber may refer to rubber polymerized from butadiene monomers, or rubber copolymerized from butadiene and a small amount of vinyl monomer copolymerizable with butadiene. Vinyl monomer copolymerizable with butadiene may be, for example, styrene or acrylonitrile, but is not limited thereto. When butadiene rubber contains monomer copolymerizable with butadiene, the content thereof is preferably 30% or less, more preferably 25% or less, even more preferably 20% or less, and most preferably 10% or less.

[0037] A monomer mixture may refer to a mixture of aromatic vinyl monomers and unsaturated nitrile monomers.

[0038] The aromatic vinyl monomer may be one or more selected from the group consisting of styrene, t-butylstyrene, halogen-substituted styrene, 3-methylstyrene, 4-methylstyrene, 4-propylstyrene, 2,3-dimethylstyrene, 2,4-dimethylstyrene, α-methylstyrene, α-ethylstyrene, methyl α-methylstyrene, 1-vinylnaphthalene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, and 1-vinyl-5-hexylnaphthalene, and preferably styrene, but is not limited thereto.

[0039] The unsaturated nitrile monomer may be one or more selected from the group consisting of acrylonitrile, methacrylonitrile, ethacrylonitrile, phenylacrylonitrile, and α-chloroacrylonitrile, and preferably may be acrylonitrile, but is not limited thereto.

[0040] (a) Step to obtain cross-linked natural rubber latex

[0041] (a) Step may be a step of adding natural rubber latex, a crosslinking agent, a polymerization initiator, and an emulsifier in batches or in succession, and crosslinking the natural rubber at a temperature of 50 to 80°C.

[0042] The crosslinking agent is a monomer having three or more double bonds, and may be at least one selected from the group consisting of, for example, trialyl isocyanurate, trialyl cyanurate, trialyl trimetate, trimethylolpropane triacrylate, and trialylamine, and preferably, considering aspects of polymerization stability, it may be trialyl isocyanurate.

[0043] The content of the crosslinking agent may be 0.1 to 2 weight% based on 100 weight% of natural rubber latex, preferably 0.2 to 1.8 weight%, and more preferably 0.4 to 1.6 weight%, but is not limited thereto. If the content of the crosslinking agent is excessively low, the crosslinking density may decrease, which may degrade the appearance quality, and conversely, if the content is excessively high, the impact strength of the resin may decrease due to excessive crosslinking density.

[0044] The polymerization initiator may be a hydrophilic initiator or a lipophilic initiator, and it is preferable to use a hydroperoxide-based redox initiator considering the ease of controlling crosslinking density and the possibility of simultaneous use with the graft reaction described later. As a hydroperoxide-based initiator, for example, at least one organic peroxide selected from the group consisting of tert-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, methylcyclohexyl hydroperoxide, p-menethane hydroperoxide, and 1,1,3,3-tetramethylbutyl hydroperoxide, and at least one inorganic peroxide selected from the group consisting of potassium persulfate and sodium persulfate may be used alone or in combination, but is not limited thereto.

[0045] The content of the polymerization initiator may be 0.1 to 2.0 wt% based on 100 wt% of natural rubber latex. For example, it may be 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2.0 wt%, or a value between two of these values, but is not limited thereto. If the content of the polymerization initiator is excessively low, it may be difficult for the crosslinking reaction to proceed smoothly, and conversely, if the content is excessively high, the impact strength of the resin may decrease due to excessive crosslinking density.

[0046] The emulsifier may be at least one selected from the group consisting of, for example, potassium oleate, sodium oleate, fatty acid soap, alkali salt of rosin acid, alkylaryl sulfonate, alkali methylalkyl sulfate, sulfonated alkyl ester, and alkali alkylsulfosuccinate, but is not limited thereto.

[0047] The content of the emulsifier may be 0.1 to 3.0 weight% based on 100 weight% of natural rubber latex. For example, it may be 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2.0 wt%, 2.1 wt%, 2.2 wt%, 2.3 wt%, 2.4 wt%, 2.5 wt%, 2.6 wt%, 2.7 wt%, 2.8 wt%, 2.9 wt%, 3.0 wt%, or a value between two of these values, but is not limited thereto. If the emulsifier content is excessively low, the stability of the latex decreases, which may lead to excessive coagulation; conversely, if the content is excessively high, the thermal stability of the final product may be reduced.

[0048] The temperature of the crosslinking reaction may be 50 to 80°C, preferably 55 to 75°C, and more preferably 60 to 70°C. If the crosslinking reaction temperature is excessively low, the crosslinking density may decrease, and conversely, if the temperature is excessively high, the crosslinking density may increase excessively and an excessive amount of coagulated material may be produced.

[0049] The gel content of the cross-linked natural rubber latex may be 50 to 95%, preferably 60 to 90%, and more preferably 70 to 88%. If the gel content of the cross-linked natural rubber latex is excessively low, the dispersibility in the final ABS resin may be reduced, which may result in a decrease in mechanical properties and appearance quality, while conversely, if the content is excessively high, the impact strength may be reduced.

[0050] (b) Step to obtain mixed rubber latex

[0051] (b) Step may be a step of obtaining a mixed rubber latex by mixing the aforementioned cross-linked natural rubber latex and butadiene rubber latex.

[0052] The gel content of the butadiene rubber latex may be 75 to 90%. For example, it may be 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, or a value between two of these values, but is not limited thereto.

[0053] The rubber particle size of butadiene rubber latex can be 1,000 to 4,000 Å. For example, 1,000Å, 1,100Å, 1,200Å, 1,300Å, 1,400Å, 1,500Å, 1,600Å, 1,700Å, 1,800Å, 1,900Å, 2,000Å, 2,100Å, 2,200Å, 2,300Å, 2,400Å, 2,500Å, 2,600Å, 2,700Å, 2,800Å, 2,900Å, 3,000Å, 3,100Å, 3,200Å, 3,300Å, 3,400Å, 3,500Å, 3,600Å, 3,700Å, 3,800Å, 3,900Å, It may be 4,000 Å, or a value between two of these values, but is not limited thereto.

[0054] The mixed rubber latex may contain cross-linked natural rubber latex and butadiene rubber latex in a weight ratio of 20:80 to 80:20, preferably in a weight ratio of 25:75 to 75:25, more preferably in a weight ratio of 30:70 to 70:30, even more preferably in a weight ratio of 35:65 to 65:35, and most preferably in a weight ratio of 40:60 to 60:40, but is not limited thereto. If the content of cross-linked natural rubber latex is excessively low, the content of bio-raw materials may be insufficient, and conversely, if the content is excessively high, the colorability of the ABS resin may be reduced.

[0055] (c) Step to obtain a graft copolymer

[0056] (c) Step (c) may include: (c1) a step of initiating a reaction by introducing a mixed rubber latex, a first monomer mixture, a first polymerization initiator, a first emulsifier, an activator, and a molecular weight regulator into a reactor in a batch or sequentially; (c2) a step of additionally supplying a second monomer mixture, a second polymerization initiator, and a second emulsifier into the reactor in sequentially, respectively; and (c3) a step of terminating the reaction when the conversion rate of the monomer reaches 90% or more (e.g., 99%). Here, the first and second monomer mixtures have the same composition and are distinguished only by the order of introduction, and the same applies to the first and second polymerization initiators and the first and second emulsifiers.

[0057] The mixing ratio (weight ratio) of the mixed rubber latex and monomer mixture may be 40:60 to 70:30, preferably 45:55 to 65:35, and more preferably 50:50 to 60:40, but is not limited thereto. If the content of the mixed rubber latex is excessively low, productivity may decrease, and conversely, if the content is excessively high, it may be difficult to achieve an efficient graft rate.

[0058] The monomer mixture may contain aromatic vinyl monomers and unsaturated nitrile monomers in a weight ratio of 70:30 to 80:20, but is not limited thereto. If the content of aromatic vinyl monomers is excessively low, it may be difficult to mix with SAN resin obtained by bulk or solution polymerization, or the impact strength may be significantly reduced; conversely, if the content is excessively high, it may be difficult to mix with SAN resin obtained by bulk or solution polymerization, or there is a risk that the natural color may turn yellow.

[0059] The content of the first monomer mixture may be 15 to 30 weight percent based on 100 weight percent of the total monomer mixture (first and second monomer mixture). If the content of the first monomer mixture is excessively low, mechanical properties may deteriorate, and if the content is excessively high, it may be difficult to control the heat of reaction.

[0060] The polymerization initiator may be a hydroperoxide-based redoxy initiator, and its content may be 0.1 to 0.5 weight% based on 100 weight% of the total monomer mixture (mixture of first and second monomers).

[0061] The content of the first polymerization initiator may be 30 to 40 weight% based on 100 weight% of the total polymerization initiator (first and second polymerization initiators), but is not limited thereto. If the content of the first polymerization initiator is excessively low, the graft rate may decrease, and conversely, if the content is excessively high, a low molecular weight graft copolymer may be obtained, which may result in a decrease in mechanical properties.

[0062] The emulsifier may be at least one selected from the group consisting of, for example, potassium oleate, sodium oleate, fatty acid soap, alkali salt of rosin acid, alkylaryl sulfonate, alkali methylalkyl sulfate, sulfonated alkyl ester, and alkali alkylsulfosuccinate, but is not limited thereto.

[0063] The content of the emulsifier may be 0.1 to 5 weight percent based on 100 weight percent of the total monomer mixture (first and second monomer mixture), but is not limited thereto. If the content of the emulsifier is excessively low, the stability of the latex may decrease and the amount of solidified material may increase, and conversely, if the content is excessively high, the impact resistance of the final product may decrease.

[0064] The activator enables the polymerization reaction even at temperatures of 50°C or lower, and also plays a role in promoting the polymerization reaction and improving the graft rate depending on the amount used. The activator may be, for example, one or more selected from the group consisting of sodium formaldehyde sulfoxylate, sodium ethylenediamine tetraacetate, ferrous sulfate, lactose, dextrose, sodium pyrrophosphate, and sodium sulfate, and preferably may be lactose, sodium pyrrophosphate, and ferrous sulfate, but is not limited thereto.

[0065] The content of the activator may be 0.051 to 0.51 weight% based on 100 weight% of the total monomer mixture (first and second monomer mixture), preferably 0.03 to 0.3 weight% of lactose, 0.02 to 0.2 weight% of sodium pyrrophosphate, and 0.001 to 0.01 weight% of ferrous sulfate, but is not limited thereto. If the content of the activator is excessively low or high, it may be difficult to balance the mechanical properties.

[0066] The molecular weight regulator may be a mercaptan-based molecular weight regulator, and may be, for example, one or more selected from the group consisting of n-decyl mercaptan, n-dodecyl mercaptan, t-dodecyl mercaptan and n-octadecyl mercaptan, but is not limited thereto.

[0067] The content of the molecular weight regulator may be 0.1 to 1 weight% based on 100 weight% of the total monomer mixture (first and second monomer mixture), and preferably 0.2 to 0.8 weight%. If the content of the molecular weight regulator is excessively low, the gloss improvement effect may be insufficient, and conversely, if the content is excessively high, mechanical properties may be degraded.

[0068] After the reaction is finished, the mixture can be coagulated with a coagulant such as sulfuric acid, MgSO4, CaCl2, or Al2(SO4)3, then washed, dehydrated, and dried to obtain a graft copolymer in powder form.

[0069] The graft rate of the graft copolymer may be 25 to 60%, preferably 30 to 55%, but is not limited thereto. If the graft rate is excessively low or high, the rubber particles may not be evenly distributed when manufacturing a thermoplastic resin using it, which may result in reduced gloss and color.

[0070] Natural rubber-containing graft copolymer and thermoplastic resin composition

[0071] A natural rubber-containing graft copolymer, which is another aspect of the present invention, may be manufactured by the aforementioned manufacturing method.

[0072] A thermoplastic resin composition, which is another aspect of the present invention, may comprise 20 to 50 weight% of the aforementioned natural rubber-containing graft copolymer and 50 to 80 weight% of an aromatic vinyl compound-unsaturated nitrile compound copolymer. If the content of the natural rubber-containing graft copolymer is excessively low, the impact strength may be reduced, and conversely, if the content is excessively high, a decrease in processability and surface gloss may occur.

[0073] The embodiments of this specification will be described in more detail below. However, the following experimental results represent only representative results among the above embodiments, and the scope and content of this specification should not be interpreted as being narrowed or limited by the embodiments. The respective effects of various embodiments of this specification not explicitly presented below will be described in detail in the relevant sections.

[0074] Example 1

[0075] (a) Preparation of cross-linked natural rubber latex

[0076] 100 parts by weight of ion-exchanged water, 100 parts by weight of natural rubber latex, 1 part by weight of triallyl cyanurate, 1 part by weight of tert-butyl hydroperoxide, 0.12 parts by weight of lactose, 0.05 parts by weight of sodium pyrrophosphate, 0.002 parts by weight of ferrous sulfide, and 1 part by weight of potassium oleate were added in a batch to a nitrogen-substituted polymerization reactor, and reacted at 70°C for 5 hours. The gel content of the natural rubber latex produced was 80%.

[0077] (b) Preparation of mixed rubber latex

[0078] 50 parts by weight of the above-prepared natural rubber latex and 50 parts by weight of butadiene rubber latex were mixed. Ag-1004 from Kumho Petrochemical Co., Ltd. was used as the butadiene rubber latex, and the gel content was 88% and the rubber particle size was 3300 Å.

[0079] (c) Preparation of graft copolymer

[0080] 60 parts by weight of the above-prepared mixed rubber latex were administered through a heat exchanger at 65°C, and 7.5 parts by weight of styrene monomer, 2.5 parts by weight of acrylonitrile monomer, 0.1 parts by weight of tertiary butyl hydroperoxide, 0.12 parts by weight of lactose, 0.05 parts by weight of sodium pyrrophosphate, 0.002 parts by weight of ferrous sulfide, 0.35 parts by weight of potassium oleate, and 0.2 parts by weight of tertiary dodecyl mercaptan were administered continuously or in batches for 45 minutes. After 45 minutes, the temperature inside the reactor was 65°C.

[0081] Subsequently, 22.5 parts by weight of styrene monomer, 7.5 parts by weight of acrylonitrile monomer, 0.2 parts by weight of tert-butyl hydroperoxide, and 0.8 parts by weight of potassium oleate were continuously added for 210 minutes. During this time, the reaction temperature was raised from 65°C to 75°C. To achieve a final monomer conversion rate of over 99%, the mixture was aged for 60 minutes after continuous addition to obtain a graft copolymer latex. Afterward, the mixture was aggregated with magnesium sulfate (MgSO4), followed by washing, dehydration, and drying to obtain a powdered graft copolymer resin. The graft rate of the prepared graft copolymer was 40%.

[0082] Example 2

[0083] (a) Preparation of cross-linked natural rubber latex

[0084] A cross-linked natural rubber latex was prepared in the same manner as in Example 1, except that 1.5 parts by weight of triallyl cyanurate, 1.5 parts by weight of tert-butyl hydroperoxide, and 2.5 parts by weight of potassium oleate were used. The gel content of the prepared natural rubber latex was 87%.

[0085] (b) Preparation of mixed rubber latex

[0086] A mixed rubber latex was prepared in the same manner as in Example 1, except that 70 parts by weight of natural rubber latex and 30 parts by weight of butadiene rubber latex were mixed.

[0087] (c) Preparation of graft copolymer

[0088] A graft copolymer was prepared in the same manner as in Example 1, and the graft rate of the prepared graft copolymer was 50%.

[0089] Example 3

[0090] (a) Preparation of cross-linked natural rubber latex

[0091] A cross-linked natural rubber latex was prepared in the same manner as in Example 1, except that 0.5 parts by weight of triallyl cyanurate, 0.5 parts by weight of tert-butyl hydroperoxide, and 0.5 parts by weight of potassium oleate were used. The gel content of the prepared natural rubber latex was 70%.

[0092] (b) Preparation of mixed rubber latex

[0093] A mixed rubber latex was prepared in the same manner as in Example 1, except that 30 parts by weight of natural rubber latex and 70 parts by weight of butadiene rubber latex were mixed.

[0094] (c) Preparation of graft copolymer

[0095] A graft copolymer was prepared in the same manner as in Example 1, and the graft rate of the prepared graft copolymer was 35%.

[0096] Comparative Example 1

[0097] (a) Preparation of cross-linked natural rubber latex

[0098] A cross-linked natural rubber latex was prepared in the same manner as in Example 1, except that divinylbenzene was used instead of trialyl cyanurate as the cross-linking agent. The gel content of the prepared natural rubber latex was 40%.

[0099] (b) Preparation of mixed rubber latex

[0100] A mixed rubber latex was prepared in the same manner as in Example 1.

[0101] (c) Preparation of graft copolymer

[0102] A graft copolymer was prepared in the same manner as in Example 1, and the graft rate of the prepared graft copolymer was 25%.

[0103] Comparative Example 2

[0104] (a) Preparation of cross-linked natural rubber latex

[0105] A cross-linked natural rubber latex was prepared in the same manner as in Example 1, except that ethylene glycol dimethacrylate (EGDMA) was used instead of trialyl cyanurate as the cross-linking agent. The gel content of the prepared natural rubber latex was 30%.

[0106] (b) Preparation of mixed rubber latex

[0107] A mixed rubber latex was prepared in the same manner as in Example 1.

[0108] (c) Preparation of graft copolymer

[0109] A graft copolymer was prepared in the same manner as in Example 1, and the graft rate of the prepared graft copolymer was 20%.

[0110] Comparative Example 3

[0111] (a) Preparation of cross-linked natural rubber latex

[0112] A cross-linked natural rubber latex was prepared in the same manner as in Example 1.

[0113] (c) Preparation of graft copolymer

[0114] A graft copolymer was prepared in the same manner as in Example 1 using 100% cross-linked natural rubber latex without mixing with butadiene rubber latex, and the graft rate of the prepared graft copolymer was 20%.

[0115] Comparative Example 4

[0116] (a) Preparation of cross-linked natural rubber latex

[0117] A cross-linked natural rubber latex was prepared in the same manner as in Example 1, except that 2.5 parts by weight of triallyl cyanurate were used. The gel content of the prepared natural rubber latex was 95%.

[0118] (b) Preparation of mixed rubber latex

[0119] A mixed rubber latex was prepared in the same manner as in Example 1.

[0120] (c) Preparation of graft copolymer

[0121] A graft copolymer was prepared in the same manner as in Example 1, and the graft rate of the prepared graft copolymer was 45%.

[0122] Table 1 below summarizes the manufacturing conditions and physical properties of the prepared graft copolymers for Examples 1 to 3 and Comparative Examples 1 to 4. Meanwhile, the gel content, rubber particle size, and graft rate were measured and calculated using the following instruments and test methods.

[0123] (1) Gel content

[0124] After coagulating rubber latex using a 1% sulfuric acid solution, washing and drying in a vacuum oven at 50°C for 24 hours, 1 g of the obtained coagulated material was placed in 100 g of toluene and stored in a dark room at room temperature for 48 hours, then separated into a sol and a gel, and the gel content was measured according to the following mathematical formula 1.

[0125] [Mathematical Formula 1]

[0126] (Gel content, %) = (Weight of insoluble matter (gel)) / (Weight of sample) × 100

[0127] (2) Rubber particle size

[0128] Measurements were taken using Nanotrac 150 with the dynamic laser light scattering method.

[0129] (3) Graft rate

[0130] 2g of powdered graft copolymer resin was stirred with 100ml of acetone for 24 hours to dissolve the styrene-based copolymer that was not grafted onto the rubber component, and then the gel and sol were separated by ultracentrifugation and calculated according to the following mathematical formula 2.

[0131] [Mathematical Formula 2]

[0132] (Graft rate) = {(Gel weight) - (Rubber weight)} / (Rubber weight) × 100

[0133]

[0134] Experimental Example

[0135] 30 parts by weight of the graft copolymer resin prepared in Examples 1 to 3 and Comparative Examples 1 to 4, 70 parts by weight of SAN resin having a weight-average molecular weight of 100,000 and an acrylonitrile content of 25%, 0.75 parts by weight of a lubricant, and 0.25 parts by weight of a heat stabilizer were added and mixed, and then extruded and injection molded to produce a specimen having a final rubber content of 15% by weight. Using the specimen, Izod impact strength, tensile strength, surface gloss, and colorability (L) were measured by the following method, and the results are shown in Table 2 below.

[0136] a) Izod impact strength test: Measured according to the ASTM D256 method. The thickness of the specimen was 1 / 4 inch.

[0137] b) Tensile strength: Tensile strength was measured using the ASTM D638 method.

[0138] c) Surface gloss: Measured using Micro Haze Plus at a 60-degree angle.

[0139] L) Colorability (L): 0.5 parts by weight of an easily identifiable black colorant was added to 100 parts by weight of thermoplastic resin and injection molded, and each L value was measured using a spectrophotometer (Datacolor 650). A low L value was judged to indicate good colorability.

[0140]

[0141] From Table 2, it can be seen that the thermoplastic resins prepared using the graft copolymers of Examples 1 to 3 have superior gloss and colorability compared to Comparative Examples 1 to 3, and have superior mechanical properties while maintaining superior appearance quality compared to Comparative Example 4.

[0142] The foregoing description of this specification is for illustrative purposes only, and those skilled in the art to which one aspect of this specification pertains will understand that other specific forms can be easily modified without altering the technical concept or essential features described in this specification. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.

[0143] The scope of this specification is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of this specification.

Claims

Claim 1 A method for manufacturing a natural rubber-containing graft copolymer, comprising: a step of crosslinking a natural rubber latex with a crosslinking agent having three or more double bonds to obtain a crosslinked natural rubber latex having a gel content of 50 to 95%; a step of mixing the crosslinked natural rubber latex with butadiene rubber latex to obtain a mixed rubber latex; and a step of mixing the mixed rubber latex with a monomer mixture and emulsion polymerizing to obtain a graft copolymer; wherein the content of the crosslinking agent is 0.1 to 2 weight% based on 100 weight% of the natural rubber latex. Claim 2 delete Claim 3 A method for preparing a natural rubber-containing graft copolymer according to claim 1, wherein the crosslinking agent having three or more double bonds is at least one selected from the group consisting of trialyl isocyanurate, trialyl cyanurate, trialyl trimetate, trimethylolpropane triacrylate, and trialylamine. Claim 4 delete Claim 5 A method for manufacturing a natural rubber-containing graft copolymer according to claim 1, wherein the gel content of the butadiene rubber latex is 75 to 90%. Claim 6 A method for manufacturing a natural rubber-containing graft copolymer according to claim 1, wherein the rubber particle size of the butadiene rubber latex is 1,000 to 4,000 Å. Claim 7 A method for manufacturing a natural rubber-containing graft copolymer according to claim 1, wherein the mixed rubber latex comprises the cross-linked natural rubber latex and the butadiene rubber latex in a weight ratio of 20:80 to 80:

20. Claim 8 A method for manufacturing a natural rubber-containing graft copolymer according to claim 1, wherein, in the step of obtaining the graft copolymer, the mixed rubber latex and the monomer mixture are mixed in a weight ratio of 40:60 to 70:

30. Claim 9 A method for manufacturing a natural rubber-containing graft copolymer according to claim 1, wherein the monomer mixture comprises an aromatic vinyl monomer and an unsaturated nitrile monomer in a weight ratio of 70:30 to 80:

20. Claim 10 A method for manufacturing a natural rubber-containing graft copolymer according to claim 1, wherein the graft rate of the graft copolymer is 25 to 60%. Claim 11 A natural rubber-containing graft copolymer produced by a manufacturing method according to any one of claims 1, 3, and 5 to 10. Claim 12 A thermoplastic resin composition comprising 20 to 50 weight% of the natural rubber-containing graft copolymer of claim 11 and 50 to 80 weight% of an aromatic vinyl compound-unsaturated nitrile compound copolymer.

Citation Information

Patent Citations

  • Natural rubber-containing heat-resistant, easily-coatable thermoplastic resin composition

    JP2014173049A

  • Natural rubber-containing thermoplastic resin composition and molded article thereof

    JP2014234408A

  • Thermoplastic resin composition

    KR1020240129401A

  • Graft copolymer and rubber-reinforced thermoplastic resin composition

    JP2015218328A

  • Natural rubber-containing thermoplastic resin composition and molded article thereof