Symmetric dissimilar material weld bead and a secondary battery module including same the weld bead
A symmetrical dissimilar metal weld bead with controlled concentration and geometric symmetry addresses the issues of asymmetrical welds in secondary batteries, improving mechanical properties and reliability by minimizing crack formation and intermetallic compounds.
Patent Information
- Application Number
- KR1020220149372
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-10
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-11-10
AI Technical Summary
Existing laser welding methods for connecting dissimilar metals in secondary batteries result in asymmetrical weld beads with high welding defects, leading to variations in tensile strength, reduced mechanical properties, and increased crack formation, which compromises the reliability and safety of the battery.
A symmetrical dissimilar metal weld bead is formed by controlling the concentration deviation and geometric symmetry of the weld bead, ensuring a copper concentration deviation of less than 5 wt% and satisfying specific geometric ratios, thereby minimizing intermetallic compound formation and crack occurrence.
The symmetrical weld bead enhances mechanical properties, electrical characteristics, and welding reliability by suppressing high-temperature, low-temperature, and embrittlement cracking, ensuring stable welding quality and long-term battery reliability.
Smart Images

Figure 112022119573206-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a secondary battery module, and more specifically, to a symmetrically shaped dissimilar metal weld bead having improved mechanical properties and electrical characteristics, and having improved long-term reliability by suppressing crack formation at the welded area, and a secondary battery module including said weld bead. Background Technology
[0002] Recently, requirements for high-capacity and high-output secondary batteries have been increasing, necessitating the development of secondary batteries that meet these specifications by requiring high energy density, high performance, and a high level of reliability. When configuring the positive and negative electrodes in the fabrication of secondary batteries, a bonding of the electrodes is required to electrically connect cells; generally, heterogeneous bonding methods using materials such as aluminum and copper are widely used. Since both aluminum and copper materials possess excellent electrical and thermal conductivity, they are widely used in electronic and electrical components and heat dissipation components. Furthermore, recently, bonded structures combining copper and aluminum materials are in demand from the perspective of miniaturizing and lightweighting these electronic and electrical components and heat dissipation components.
[0003] In particular, regarding electrical connection methods between cells requiring a high level of reliability, various methods such as ultrasonic welding, laser welding, and mechanical (bolt / nut) joining are used; however, to meet the increasingly high energy density requirements, laser welding is being used as the most common joining method.
[0004] Meanwhile, when laser welding dissimilar materials, intermetallic compounds (IMCs) are generated. Since intermetallic compounds (IMCs) have high electrical resistance and hardness, they can adversely affect the mechanical properties of the weld, such as brittleness, and may also adversely affect battery characteristics due to increased resistance when electrically connecting battery cells.
[0005] Furthermore, defects such as weld cracks may occur in the weld zone during laser welding; known types of such weld cracks include high-temperature cracks, low-temperature cracks, or embrittlement cracks. High-temperature cracks refer to cracks that occur at high temperatures during the welding process or at relatively high temperatures when the weld bead solidifies. Low-temperature cracks generally refer to cracks that occur at room temperature after the welding process, primarily occurring in the heat-affected zone. Embrittlement cracks refer to cracks that occur when stress is applied while grain boundaries are weakened by the precipitation of intermetallic compounds (IMCs); these cracks primarily refer to those that occur during the actual use of the secondary battery module after welding. Since the occurrence of any one of these high-temperature, low-temperature, or embrittlement cracks causes serious defects in the weld zone, it is necessary to eliminate factors that induce cracking from the perspective of long-term battery reliability.
[0006] Various laser welding methods are used to solve the above problems, such as overlapping welding of a single or multiple electrode tabs and a busbar; however, there are limitations such as high welding defects including under-welding after welding, and the need to bend and cut multiple electrode tabs within a unit module for welding leads to increased process steps and higher management costs. Furthermore, an asymmetrical weld bead is formed, resulting in large variations in tensile strength and degraded mechanical properties, making it difficult to ensure stable welding quality.
[0007] In addition, the formation of low-quality weld beads with low uniformity makes it impossible to secure a product safety factor corresponding to requirements such as vibration and impact resistance tests, and fails to suppress the occurrence of high-temperature cracking, low-temperature cracking, or embrittlement cracking, resulting in reduced welding reliability and long-term battery reliability.
[0008] Therefore, there is an urgent need for technology capable of ensuring stable welding quality, as well as excellent mechanical properties, electrical characteristics, and welding reliability. The problem to be solved
[0009] The present disclosure aims to provide a symmetrically shaped dissimilar metal weld bead capable of having a weld portion having excellent mechanical properties and electrical characteristics, and a secondary battery module including said weld bead.
[0010] In addition, the present disclosure aims to provide a symmetrically shaped dissimilar metal weld bead that suppresses crack formation in the weld bead, thereby improving welding reliability and long-term reliability of the battery, and a secondary battery module including said weld bead.
[0011] Furthermore, the technical problems to be solved in this disclosure are not limited to those mentioned above, and other technical problems not mentioned will be clearly understood by those skilled in the art to which this invention belongs from the description below. means of solving the problem
[0012] The present disclosure provides a secondary battery module comprising a plurality of battery cells each including an electrode tab, and a bus bar connected to the plurality of electrode tabs to electrically connect the plurality of battery cells to each other, wherein the bus bar comprises a plate having a plurality of holes formed therein, wherein the electrode tabs of the plurality of battery cells are inserted into at least some of the plurality of holes of the plate, and the electrode tabs inserted into the holes and the plate are joined to each other by a welding bead, wherein the welding bead comprises one or more welding beads, and wherein the welding bead satisfies the following Equation 1 for a concentration deviation (△C).
[0013] [Equation 1]
[0014] Concentration deviation (△C) < 5 wt%
[0015] (In the above Equation 1, the concentration deviation (△C) refers to the difference between the average copper concentration (C1) on the left side and the average copper concentration (C2) on the right side, based on the centerline of the hole in the weld bead cross-section in the thickness direction of the plate.)
[0016] In one embodiment, the weld bead may satisfy a concentration deviation (△C) of 3 weight% or less.
[0017] In one embodiment, the concentration deviation (△C) may be measured through SEM-EDS (SEM, Scanning Electron Microscope, EDS, energy dispersive X-ray spectroscopy).
[0018] In one embodiment, the weld bead may be a symmetrical weld bead that is symmetrical with respect to the centerline of the hole in the weld bead cross-section in the thickness direction of the plate.
[0019] In one embodiment, the weld bead having the symmetry may satisfy the following Equations 2 and 3.
[0020] [Equation 2]
[0021] 0.90L2 ≤ L1 ≤ 1.1L2
[0022] [Equation 3]
[0023] 0.90D2 ≤ D1 ≤ 1.1D2
[0024] (In the above Equations 2 and 3, L1 and L2 represent the shortest distance from the intersection point (P100, P200) to the boundary point (P1, P2), and D1 and D2 represent the distance from the intersection point (P100, P200) to the bonding interface of the weld bead perpendicular to L1 and L2. In this case, the boundary point (P1, P2) refers to the boundary point (P1, P2) on the left and right sides where the bonding interface of the weld bead meets the surface of the weld bead, and the intersection point (P100, P200) refers to the intersection point (P100, P200) on the left and right sides where a line perpendicular from the boundary point (P1, P2) to the centerline of the hole and a virtual line (L100, L200) extending the boundary surface of the electrode tab intersect perpendicularly.)
[0025] In one embodiment, the weld bead may include a cover portion having a convex shape covering the hole in the weld bead cross-section in the thickness direction of the plate; and a column portion inserted into the hole.
[0026] In one embodiment, the electrode tab may be made of aluminum, and the plate may be made of copper.
[0027] In one embodiment, the welding bead may have a copper concentration of 40 weight% or less.
[0028] In one embodiment, the welding bead may have a plate dilution rate of 40% or less.
[0029] In one embodiment, the battery cell may be a secondary battery module that is a pouch-type battery cell. Effects of the invention
[0030] A symmetrical heterogeneous metal welding bead according to the present disclosure and a secondary battery module including said welding bead can ensure stable welding quality by improving mechanical properties and electrical characteristics.
[0031] A symmetrical dissimilar metal welding bead according to the present disclosure and a secondary battery module including said welding bead can improve welding reliability and long-term reliability of the battery by suppressing the occurrence of high-temperature cracking, low-temperature cracking, and embrittlement cracking in the welding bead.
[0032] A symmetrical heterogeneous metal welding bead according to the present disclosure and a secondary battery module including said welding bead can minimize the formation of intermetallic compounds (IMCs) in the welding bead. Brief explanation of the drawing
[0033] FIG. 1 is a drawing illustrating a virtual plane forming a weld bead cross-section in the thickness direction of a plate according to one embodiment. FIG. 2 is a schematic cross-sectional view showing that, according to one embodiment, a weld bead is formed together with the plate by heating and melting the electrode tab end penetrating the hole of the plate with a laser. Figure 3 shows the left and right sides with respect to the centerline of the hole in the weld bead cross-section in the thickness direction of the plate according to one embodiment. FIG. 4 shows the intersection points (P100, P200) on the left and right sides where a line extending vertically from the boundary points (P1, P2) on the left and right sides, where the bonding interface of the weld bead and the surface of the weld bead meet, to the centerline of the hole and a virtual line (L100, L200) extending the boundary surface of the electrode tab intersects vertically in the weld bead cross-section in the thickness direction of the plate according to one embodiment. FIG. 5 shows L1 and L2, which are the shortest distances from the intersection point (P100, P200) to the boundary point (P1, P2), according to one embodiment, and D1 and D2, which are distances from the intersection point (P100, P200) to the joint interface of the weld bead perpendicular to L1 and L2. FIG. 6 is a drawing showing a welding process using a laser according to one embodiment. FIG. 7 is a drawing showing a bus bar included in a secondary battery module according to one embodiment. FIG. 8 is a drawing showing a secondary battery module having a weld bead according to one embodiment. Figure 9 shows an optical microscope (OM) image of a weld bead according to Example 2. Figure 10 shows an optical microscope (OM) image of a weld bead according to Comparative Example 1. Specific details for implementing the invention
[0034] The secondary battery module of the present invention will be described in detail below with reference to the attached drawings. The drawings presented below are provided as examples to ensure that the concept of the present invention is sufficiently conveyed to those skilled in the art. Accordingly, the present invention is not limited to the drawings presented below and may be embodied in other forms, and the drawings presented below may be exaggerated to clarify the concept of the present invention. Unless otherwise defined, technical and scientific terms used herein shall have the meaning commonly understood by those skilled in the art to which this invention pertains, and descriptions of known functions and configurations that could unnecessarily obscure the essence of the present invention in the following description and attached drawings are omitted.
[0035] Additionally, the singular form used in the specification and the appended claims may be intended to include the plural form unless specifically indicated otherwise in the context.
[0036] In this specification and the appended claims, terms such as "first," "second," etc. are used not in a limiting sense, but for the purpose of distinguishing one component from another.
[0037] In this specification and the appended claims, terms such as "include" or "have" mean that the features or components described in the specification exist, and unless specifically limited, this does not preclude the possibility that one or more other features or components may be added.
[0038] In this specification and the appended claims, when a part such as a film (layer), region, or component is described as being on or above another part, it includes not only cases where it is directly above in contact with the other part, but also cases where another film (layer), other region, or other component is interposed therein.
[0039] Unless otherwise specified in this specification, the term "crack" includes high-temperature cracking, low-temperature cracking, or embrittlement cracking.
[0040] When laser welding dissimilar materials, intermetallic compounds (IMCs) are generated. Since IMCs possess properties such as high electrical resistance and hardness, they adversely affect the mechanical properties of the weld, such as causing brittleness, and may also negatively affect battery performance due to increased resistance during electrical connections between battery cells. Furthermore, since the occurrence of high-temperature cracking, low-temperature cracking, or embrittlement cracking in the weld can cause serious defects, it is necessary to eliminate factors that cause cracking from the perspective of long-term battery reliability.
[0041] Various laser welding methods are used to solve the above problem, such as overlapping welding of a single or multiple electrode tabs and a busbar, but there are limitations such as high welding defects including weak welding after welding, and there is a problem that the process increases and management costs rise because multiple electrode tabs within a unit module need to be bent and cut for welding.
[0042] Furthermore, the formation of asymmetric weld beads results in large variations in tensile strength and deterioration of mechanical properties, making it difficult to ensure stable weld quality. Additionally, the formation of low-quality weld beads with low uniformity makes it impossible to secure a product safety factor corresponding to requirements such as vibration and impact resistance tests. Moreover, the failure to suppress the occurrence of high-temperature cracking, low-temperature cracking, or embrittlement cracking leads to reduced weld reliability and the long-term reliability of the battery.
[0043] Accordingly, the present invention aims to solve the above problem by providing a secondary battery module comprising a plurality of battery cells each including an electrode tab, a bus bar connected to the plurality of electrode tabs to electrically connect the plurality of battery cells to each other, wherein the bus bar includes a plate having a plurality of holes formed therein, wherein each electrode tab of the plurality of battery cells is inserted into at least some of the plurality of holes of the plate, and the electrode tab inserted into the hole and the plate are joined to each other by a welding bead, wherein the welding bead includes one or more welding beads, and wherein the welding bead satisfies the concentration deviation (△C) of the following Equation 1.
[0044] [Equation 1]
[0045] Concentration deviation (△C) < 5 wt%
[0046] (In the above Equation 1, the concentration deviation (△C) refers to the difference between the average copper concentration (C1) on the left side and the average copper concentration (C2) on the right side, based on the centerline of the hole in the weld bead cross-section in the thickness direction of the plate.)
[0047] Specifically, the cross-section of the weld bead (170) in the thickness direction of the plate refers to a cross-section cut by a virtual plane parallel to the thickness direction of the plate (a virtual plane having the thickness direction in-plane), and may refer to a weld cross-section cut such that the area of the weld bead (170) is minimized. Referring to FIG. 1, the virtual plane (p) that forms the cross-section of the weld bead (170) may refer to a virtual plane that is parallel to the thickness direction (t1) of the plate (150) and simultaneously parallel to the thickness direction (t2) of the electrode tab (120), and the cross-section of the weld bead (170) may refer to a cross-section cut by the aforementioned virtual plane (p).
[0048] FIG. 2 is a schematic cross-sectional view showing that, according to one embodiment, a weld bead (170) is formed by heating and melting the end of an electrode tab (120) that penetrates a hole (150c) of a plate (150a) of a busbar with a laser. At this time, the centerline (CL) of the hole (150c) may be the same as the centerline (CL) of the battery tab as the battery tab is inserted into the hole.
[0049] The concentration deviation (△C) is particularly important when the electrode tab and the plate are heterogeneous metals of different materials (metal materials). As in the embodiment described below, when the electrode tab is made of aluminum and the busbar is made of copper, when the concentration deviation (△C) satisfies 5 weight% or less, the mechanical properties and electrical characteristics of the weld bead (170) can be significantly improved, and the uniformity of the weld bead is excellent, thereby suppressing the occurrence of cracks such as high-temperature cracks, low-temperature cracks, or embrittlement cracks, and thus improving long-term reliability. Preferably, the weld bead may satisfy a concentration deviation (△C) of 4 weight% or less, and more preferably, may satisfy a concentration deviation (△C) of 3 weight% or less.
[0050] In one embodiment, the concentration deviation (△C) can be measured through SEM-EDS analysis (SEM, Scanning Electron Microscope, EDS, energy dispersive X-ray spectroscopy). The EDS (energy dispersive X-ray spectroscopy) is equipment used by attaching a detector to a scanning electron microscope (SEM), and composition analysis over the entire weld can be quantified by detecting characteristic X-rays among various signals emitted by the interaction between the sample surface and the electron beam. Specifically, through SEM-EDS analysis, as shown in FIG. 3, the average copper concentration (C1) on the left side and the average copper concentration (C2) on the right side are measured respectively with respect to the centerline of the hole in the weld bead cross-section in the thickness direction of the plate, and the concentration deviation (△C) can be derived by calculating the difference between them, IC1-C2I.
[0051] In one embodiment, the weld bead may be a symmetrical weld bead, which is symmetrical with respect to the centerline of the hole in the weld bead cross-section in the thickness direction of the plate. When the concentration deviation (△C) satisfies 5 weight% or less as in Equation 1 and satisfies morphological symmetry such as left-right symmetry, the formation of intermetallic compounds (IMCs) is prevented, thereby exhibiting excellent tensile strength and mechanical properties. Furthermore, since the uniformity of the weld bead is significantly superior, the occurrence of high-temperature cracks, low-temperature cracks, or embrittlement cracks can all be suppressed, thus improving welding reliability and the long-term reliability of the battery.
[0052] In one embodiment, the weld bead having the symmetry may satisfy the following Equations 2 and 3.
[0053] [Equation 2]
[0054] 0.90L2 ≤ L1 ≤ 1.1L2
[0055] [Equation 3]
[0056] 0.90D2 ≤ D1 ≤ 1.1D2
[0057] (In the above Equations 2 and 3, L1 and L2 represent the shortest distance from the intersection point (P100, P200) to the boundary point (P1, P2), and D1 and D2 represent the distance from the intersection point (P100, P200) to the bonding interface of the weld bead perpendicular to L1 and L2. In this case, the boundary point (P1, P2) refers to the boundary point (P1, P2) on the left and right sides where the bonding interface of the weld bead meets the surface of the weld bead, and the intersection point (P100, P200) refers to the intersection point (P100, P200) on the left and right sides where a line perpendicular from the boundary point (P1, P2) to the centerline of the hole and a virtual line (L100, L200) extending the boundary surface of the electrode tab intersect perpendicularly.)
[0058] Referring to FIG. 4, the intersection points (P100, P200) on the left and right sides, where a line perpendicular from the boundary points (P1, P2) on the left and right sides where the joint interface of the weld bead and the surface of the weld bead meet to the center line (CL) of the hole and a virtual line (L100, L200) extending from the boundary surface of the electrode tab intersect perpendicularly.
[0059] Based on this, as shown in FIG. 5, L1 and L2, which are the shortest distances from the intersection points (P100, P200) to the boundary points (P1, P2), and D1 and D2, which are distances from the intersection points (P100, P200) to the joint interface of the weld bead perpendicular to L1 and L2, can be derived. When molten metal originating from welding base materials such as electrode tabs and plates (busbars) is cooled to form a weld bead (170), it can have geometric symmetry by satisfying Equations 2 and 3, and the weld can exhibit uniform tensile strength and excellent mechanical properties, and stable welding quality can be secured by minimizing welding defects. Specifically, Equation 2 may be 0.95L2 ≤ L1 ≤ 1.05L2, and Equation 3 may be 0.95D2 ≤ D1 ≤ 1.05D2; more specifically, Equation 2 may be 0.98L2 ≤ L1 ≤ It can be 1.02L2, and Equation 3 can be 0.98D2 ≤ D1 ≤ 1.02D2.
[0060] In the above Equations 2 and 3, L1, L2, D1, and D2 can be measured through optical microscope image analysis (OM). Specifically, after undergoing specimen pretreatment processes such as cutting the weld specimen, fabricating and mounting the mold, and polishing the specimen surface, the specimen can be observed with an optical microscope to acquire an image and derived based on this.
[0061] The weld bead (170) having the above symmetry satisfies Equation 1 and can also satisfy Equations 2 and 3. By satisfying all of these, the occurrence of high-temperature cracks, low-temperature cracks, or embrittlement cracks can be suppressed, thereby improving welding reliability and long-term reliability of the battery. Furthermore, the formation of intermetallic compounds (IMCs) can be minimized, and electrical properties such as excellent tensile strength, mechanical properties, and reduced electrical resistance can be further improved, thereby ensuring stable welding quality.
[0062] In one embodiment, the weld bead (170) may include a cover portion having a convex shape covering the hole (150c) in the cross-section of the weld bead (170) in the thickness direction of the plate, and a column portion inserted into the hole (150c). Specifically, the column portion refers to an area inserted into the hole (150c) below, based on the line connecting the boundary points (P1, P2) of the left and right sides where the bonding interface of the weld bead meets the surface of the weld bead. Unlike conventional techniques such as overlapping welding methods during laser welding, the present disclosure performs welding by protruding an electrode tab through the plate and then irradiating a laser beam onto the protruding weld portion. By the welding method, a weld bead (170) shape including a cover portion and a column portion can be created. Specifically, a stacked body containing a certain number of cells is formed by stacking unit cells, and subsequently, the plate can be assembled in the direction in which the electrode tab is inserted for electrical connection. At this time, the plate has a predetermined gap through which a pre-processed electrode tab can pass, and is provided with a hole (slot) corresponding to each electrode tab, and may have a surface that protrudes in a predetermined direction of passage of the electrode tab along the outer circumference of the hole (150c). After assembly in this way, the electrode tab protrudes through the plate, and then a laser beam can be irradiated onto the protruding weld to perform welding.
[0063] In detail, as shown in FIG. 6, when irradiating a laser beam (L), it may be desirable to search for a laser irradiation position such that the protrusion amount (tolerance, G) of the electrode tab penetrating the plate becomes 2.0 mm or less, thereby finally selecting the laser irradiation position and performing automatic welding. At this time, it may be desirable to perform welding by automatically adjusting the laser irradiation position and output according to the electrode protrusion amount within the tolerance range, with the laser output in the range of 15 to 30 J / mm. When welding is performed by the above welding method, a weld bead having high uniformity and symmetry can be formed that further satisfies Equations 1, 2, and 3. It may be desirable to make the tolerance 1 mm or less, and it may be more desirable to make it 0.5 mm or less. It may be desirable to set the laser output in the range of 15 to 25 J / mm, and more preferably, it may be more desirable to set it in the range of 15 to 20 J / mm.
[0064] When the molten metal originating from the welding base material is cooled to form a welding bead (170) during laser welding, various welding beads (170) are formed depending on the thickness, material, protrusion amount of the electrode tab, the material of the plate, the plating material and thickness, the welding length, the welding speed, the laser power, and the laser irradiation pattern. In particular, the shape of the welding bead (170), including the cover portion and the column portion, can affect the mechanical properties of the weld. As the concentration deviation of the welding bead (170) satisfies Equation 1 and simultaneously satisfies geometric symmetry, it can secure stable welding quality by having excellent mechanical properties and electrical characteristics.
[0065] In one embodiment, the plate dilution rate of the weld bead (170) may be 40% or less. When welding dissimilar materials, mechanical properties may be improved without substantial deterioration of electrical properties depending on the composition of the weld bead (170), for example, the copper-aluminum dilution rate in the case of copper-aluminum dissimilar materials. Generally, the dilution rate indicates the degree of contribution of each weld base material (in the case of the present invention, the plate and electrode tab) to the overall weld with or without the addition of filler, and can be measured as the area where each component is melted and mixed in a cross-sectional image of the weld metal. It is known that this dilution rate varies depending on the welding heat input, thermal properties, initial joint shape, and dimensions. When welding dissimilar materials, such as when the electrode tab is made of aluminum and the busbar is made of copper, the amount of melting of the copper plate (busbar) increases, which may cause the tab to form an intermetallic compound (IMC) at the copper-aluminum interface. In one embodiment of the present disclosure, when the dilution rate of the plate is 40% or less, the formation of intermetallic compounds (IMCs) and cracking in the weldment can be minimized, and such a weld bead (170) has the advantage of reducing cracking and forming a stronger weldment. Specifically, the dilution rate of the plate in the weld bead (170) may be 20% or less, and more specifically, 1 to 5%.
[0066] To explain in detail the dilution rates of the electrode tab and the plate, respectively, when the electrode tab is used as the first base material for welding and the plate is used as the second base material for welding, the dilution rate of the first base material may be 70 to 99% and the dilution rate of the second base material may be 1 to 30%, specifically, the dilution rate of the first base material may be 85 to 99% and the dilution rate of the second base material may be 1 to 15%, and more specifically, the dilution rate of the first base material may be 95 to 99% and the dilution rate of the second base material may be 1 to 5%.
[0067] The above-mentioned weld bead (170) may have a copper content of 40 weight% or less. If copper is included in excess, the probability of forming intermetallic compounds (IMCs) increases, and the increase in brittleness due to precipitation may cause a decrease in strength or ductility of the weld bead. Within the above range, the occurrence of intermetallic compounds (IMCs) is minimized, thereby enabling stable weld quality and minimizing crack formation. Specifically, the copper content may be 20 weight% or less, and more specifically, 1 to 5 weight% or less.
[0068] A surface plating layer may be formed on the electrode tab, which is the first base material (welding base material), and / or the plate, which is the second base material. That is, the electrode tab and / or plate may include a surface plating layer, and in particular, the electrode tab, which must ensure electrochemical stability with respect to the electrolyte, may include a surface plating layer. As is known, the surface plating layer for ensuring electrochemical stability with respect to the electrolyte may include Ni, Sn, Si, Mg, Fe, Mn, Zn, Cr, Li, Ca, or alloys thereof. If a surface plating layer is present on the electrode tab and / or plate, the dilution rate of the surface plating layer itself can also be calculated through component analysis of the weld bead (170) containing the aforementioned first base material, second base material, and plating components. As described above, the compositional components of the weld metal (welding bead) throughout the weld can be quantified by Energy Dispersive Spectroscopy (EDS) with respect to various process factors.
[0069] In one embodiment, the electrode tab may be made of aluminum, and the plate may be made of copper. In this case, the aluminum material may be aluminum with a purity of 50 wt% or more, specifically aluminum with a purity of 55 wt% or more, 99 wt% or more, or 99.5 wt% or more. In one embodiment, the aluminum material may be industrial pure aluminum, and commercial examples may include the Aluminum 1000 series, such as Aluminum 1050, Aluminum 1100, or Aluminum 1200. The copper material may be copper with a purity of 58 wt% or more, 99 wt% or more, or 99.3 wt% or more. In one embodiment, the copper material may be industrial pure copper, and commercial examples may include the C10100 to C13000 series, such as C11000, C10100, C10200, C12500, etc. However, this is merely an example, and if necessary, the electrode tab may be made of copper and the plate of aluminum.
[0070] The present invention will be described in detail below with reference to the attached drawings.
[0071] FIG. 7 is a drawing showing a bus bar (150) provided in a secondary battery module according to one embodiment of the present disclosure, and FIG. 8 is a drawing showing a secondary battery module having a weld bead (170) according to one embodiment of the present disclosure.
[0072] As shown in one embodiment of FIG. 7(a), the secondary battery module of the present invention includes a bus bar (150), and the bus bar (150) is configured to include a plate (150a) and a hole (150c) formed in the plate. At this time, the plate may include a plurality of holes (150c) capable of accommodating each of a plurality of electrode tabs (120), and each hole (150c) may have a shape and size corresponding to the cross-section of the electrode tab (120) so that the end of the electrode tab (120) can be inserted into the hole (150c).
[0073] As in one embodiment illustrated in FIG. 7(b), each hole (150c) may include an insertion part (151) with one side open so that an electrode tab (120) can be slidably inserted. Specifically, the insertion part may have a tapered shape that widens toward the open side so that the electrode tab (120) can be easily slidably inserted into the hole (150c), but the shape of the insertion part (151) is not limited thereto. As shown in FIG. 7(a), when both ends of the hole (150c) are closed, the electrode tab (120) can be inserted into the hole (150c) of the plate (150a) in the protruding direction of the electrode tab (120). As shown in FIG. 7(b), when one end of the hole (150c) is open, the electrode tab (120) can be inserted into the hole (150c) of the plate (150a) in the upright direction (width direction) of the electrode tab (120) through the insertion part (151). One or more holes (150c) are formed in the plate (150a), and the electrode tab (120) inserted into each hole (150c) can be welded to electrically connect a plurality of welded battery cells (110).
[0074] As shown in FIG. 8, the secondary battery module according to the present disclosure may be configured to include a plurality of battery cells (110) and electrode tabs (120) drawn from the battery cells (110). The battery cells (110) are connected by inserting the electrode tabs (120) into holes (150c) formed in a plate (150a) and then welding them, so as not to separately modify the shape of the electrode tabs (120) as in the prior art. In addition, one or more holes (150c) may be formed in the plate (150a) to correspond to the number of battery cells (110) to be connected. Therefore, to electrically connect the battery cells (110), the battery cells (110) can be electrically connected without changing the shape of the electrode tabs (120), regardless of the number of battery cells (110) to be connected.
[0075] That is, in the present disclosure, the plate (150a) forming the busbar (150) includes one or more holes (150c) having a predetermined spacing, and a plurality of battery cells (110) can be electrically connected by welding an electrode tab (120) that is inserted and penetrates the hole (150c). At this time, since an electrode tab (120) (120) can be inserted and welded into each hole (150c), a plurality of battery cells (110) welded through the busbar (150) can be electrically connected. In the present disclosure, the hole (150c) may be formed in a slit shape.
[0076] Meanwhile, in the secondary battery module of the present disclosure, after penetrating the electrode tab (120) into the hole (150c) of the plate, laser welding can be performed to obtain a weld bead (170) of various shapes. When the weld bead (170) has the specific shape and size described below, mechanical properties including tensile strength can be further improved without deterioration of electrical properties, and the resistance of the module can be reduced. The specific shape and size of the weld bead (170) described below should be understood within a range that does not contradict the content applied supplementarily in addition to the concentration deviation (△C) such as Equation 1 described above or the geometric symmetry such as Equations 2 and 3.
[0077] Specifically, the weld bead (170) may have a width (W) and a height (H) that satisfy the following formulas 4 and 5.
[0078] [Equation 4]
[0079] 0 < W < 7T
[0080] In Equation 4, W is the width of the weld bead (170) based on the cross-section of the weld bead (170) in the thickness direction of the plate, and T is the thickness of the electrode tab.
[0081] [Equation 5]
[0082] 0 < H < 3T
[0083] In Equation 5, H is the height of the weld bead (170) based on the cross-section of the weld bead (170) in the thickness direction of the plate, and T is the thickness of the electrode tab. At this time, the unit of T may be mm.
[0084] In welding of dissimilar materials, if the width (W) of the weld bead (170) is 7T or more, the formation of an intermetallic compound (IMC) between the dissimilar materials may be induced. In one embodiment, when the electrode tab is made of aluminum and the busbar is made of copper, if the width of the weld bead (170) is 7T or more, the amount of melting of the copper plate (busbar) increases, causing the formation of an intermetallic compound (IMC) at the copper-aluminum interface, which may lead to a deterioration in weld quality, such as microcracks and increased resistance within the weld. Additionally, if the height (H) of the weld bead (170) is 3T or more, the length of the column portion of the weld bead (170) becomes shorter, which may cause a problem where the interfacial bonding strength decreases. Specifically, to ensure stable welding quality, the width (W) of the weld bead (170) may be 2T to 6T, more specifically 3T to 6T, and the height (H) may be 0.5T to 2T, more specifically 1T to 2T. When these weld bead (170) widths and heights are satisfied, excellent welding characteristics can be exhibited by having improved tensile strength and low contact resistance.
[0085] The width and height of the aforementioned weld bead (170) directly affect the cross-sectional area of the weld bead (170). Accordingly, in another embodiment, the electrode tab and plate inserted into the hole (150c) are joined together by the weld bead (170), and the weld bead (170) can satisfy the following Equation 6.
[0086] [Equation 6]
[0087] 0 < A < 21T 2
[0088] In Equation 6, A is the cross-sectional area of the weld bead (170) based on the cross-section of the weld bead (170) in the thickness direction of the plate, and T is the thickness of the electrode tab. At this time, the cross-section of the weld bead (170) in the thickness direction of the plate is the same as described above based on Equations 4 and 5.
[0089] The weld bead (170) has a cross-sectional area (A) of 21T 2 It may be less than. If the cross-sectional area is 21T 2 (mm 2 If it is greater than ), various types of problems may occur, such as increased occurrence of intermetallic compounds (IMCs), reduced welding strength, and cracking of the weldment. More specifically, based on the cross-section of the weld bead (170), the cross-sectional area of the weld bead (170) is T 2 Up to 12T 2 It can satisfy the above. When such a weld bead (170) cross-sectional area is satisfied, it can exhibit excellent welding characteristics with improved tensile strength and low contact resistance, and can exhibit consistent welding characteristics without being substantially affected by the specific welding conditions.
[0090] FIG. 2 illustrates forming a weld bead (170) by heating and melting the end of an electrode tab (120) that penetrates the hole (150c) of a plate (150a) of a bus bar (150) according to one embodiment of the present disclosure with a laser.
[0091] As illustrated in FIG. 2, the width (W) of the bead may be the width of the cover portion based on the cross-section of the weld bead (170). Specifically, the width (W) of the bead may be defined as the distance between the two boundary points (P1, P2) on the left and right sides where the joint interface of the weld bead meets the surface of the weld bead. In this case, the example illustrated in FIG. 2 is a case where the two boundary points (P1, P2) on the left and right are located at the same height, so the width of the bead is illustrated as in FIG. 2; however, if the two boundary points (P1, P2) on the left and right are not located at the same height, the width of the bead may be defined as the shortest distance between the two boundary points.
[0092] As illustrated in FIG. 2, the height (H) of the bead may be the maximum height of the cover portion based on the cross-section of the weld bead (170). Specifically, the height (H) of the bead may be the distance (shortest distance) between the highest point of the cover portion and an imaginary line connecting the two boundary points (P1, P2) on the left and right sides where the weld bead's bonding interface and the weld bead's surface meet in the cross-section of the weld bead (170) in the thickness direction of the plate. In this case, since the example illustrated in FIG. 2 is a case where the two boundary points (P1, P2) on the left and right are located at the same height, the width of the bead is illustrated as in FIG. 2, but the height of the bead may be defined as the shortest distance between the imaginary line connecting the two boundary points and the highest point of the cover portion.
[0093] In one embodiment, the weld bead (170) may further satisfy Equation 7.
[0094] [Equation 7]
[0095] 0.4T ≤ D ≤ 2T
[0096] In Equation 7, D is the penetration depth into the hole (150c) of the weld bead (170) based on the cross-section of the weld bead (170) in the thickness direction of the plate, and T is the thickness of the electrode tab. Specifically, the penetration depth may be the distance (shortest distance) between the imaginary line connecting the two boundary points (P1, P2) on the left and right and the lowest point of the weld bead (170) located inside the hole (150c). The penetration depth may correspond to the length of the column portion. The penetration depth may be a factor related to the mechanical properties due to the shape of the weld bead (170) itself and the dilution rate of the plate. When the penetration depth satisfies a penetration depth of 0.4T to 2T, specifically 0.5T to 1.5T, more specifically 0.5T to 1.0T, the dilution rate of the plate can be controlled to 5% or less, and the mechanical properties can be improved by the shape of the weld bead (170).
[0097] The electrode tab (120) is configured to penetrate a hole (150c) in a direction perpendicular to the surface of the plate (150a), and it is preferable that its thickness be 0.2 mm or more. More specifically, the thickness of the electrode tab (120) may be 0.2 to 1.0 mm. When the electrode tab (120) has a thickness of 0.2 mm or more, it is advantageous to be able to manufacture a weld bead (170) having the spherical shape described above by laser welding, and to manufacture a weld bead (170) in which the dilution rate of the plate is 10% or less.
[0098] In addition, in the present disclosure, the plate (150a) preferably has a thickness of 0.5 mm or more, and in one embodiment, may have a thickness of 0.5 mm to 10 mm, 1 mm to 8 mm, or 1 mm to 6 mm, but is not necessarily limited thereto.
[0099] In one embodiment, the battery cell (110) may be a pouch-type battery cell (110). The pouch-type battery cell (110) may be a battery cell (110) in which an electrode assembly comprising a positive electrode, a negative electrode, and a separator interposed between the positive and negative electrodes is impregnated with an electrolyte (electrolyte) and sealed in a pouch. The pouch may be a multilayer film structure in which a metal film, such as an aluminum film, is interposed between an outer layer film and an inner layer film, but is not limited thereto. In a secondary battery module according to one embodiment, the electrode tabs of each of the multiple pouch-type battery cells (110) stacked in one direction are inserted and welded into each of the holes (150c) of the plate, so that multiple pouch-type battery cells (110) can be electrically connected to each other.
[0100] The present disclosure is described in detail below through examples, but these are for the purpose of providing a more detailed explanation and the scope of the rights is not limited by the following examples.
[0101] Example 1
[0102] According to one embodiment of the present disclosure, a secondary battery module was prepared that includes a weld bead satisfying geometric symmetry, with a concentration deviation (△C) between unit zones of 4 wt% and L1 = 0.92 L2 and D1 = 1.05 D2. Specifically, the weld bead was formed through an automatic laser welding system in which, after inserting an aluminum electrode tab into a hole in a copper plate, a laser irradiation position was searched for and finally selected so that the protrusion amount (tolerance, G) of the electrode tab penetrating the plate was 2.0 mm or less, and welding was performed by automatically adjusting the laser output within the range of 15 to 25 J / mm. The concentration deviation (△C) was derived using an SEM-EDS (SEM, Scanning Electron Microscope, EDS, energy dispersive X-ray spectroscopy) analysis device.
[0103] Example 2
[0104] In Example 1, a secondary battery module was prepared that includes a weld bead satisfying geometric symmetry with a concentration deviation (△C) between unit zones of 2 wt%, L1=0.98L2 and D1=0.98D2. Specifically, the weld bead was formed using an automatic laser welding system in which an aluminum electrode tab is inserted into a hole in a copper plate, a laser output of 15 to 20 J / mm is set, a laser irradiation position is searched for such that the protrusion tolerance (G) of the electrode tab penetrating the plate is 0.5 mm or less, and the laser irradiation position is finally selected to perform welding. An image of the weld bead analyzed by an optical microscope (OM) is shown in FIG. 9.
[0105] Comparative Example 1
[0106] In Example 1, a secondary battery module was prepared that includes a weld bead with a concentration deviation (△C) between unit zones of 12 wt%, L1=1.45L2 and D1=1.30D2. Specifically, the weld bead was formed by overlapping aluminum electrode tabs on a copper plate without holes and then using an overlapping welding method with a laser output of 9 J / mm. An image of the weld bead analyzed by an optical microscope (OM) is shown in FIG. 10.
[0107] Comparative Example 2
[0108] In Example 1, a secondary battery module was prepared that includes a welding bead with a concentration deviation (△C) between unit zones of 9 wt%, L1 = 1.10 L2, and D1 = 1.20 D2. Specifically, the welding bead was formed by inserting an aluminum electrode tab into a hole in a copper plate and then irradiating the protruding part at an oblique angle of about 20 to 35º with respect to the central axis in the longitudinal direction (d1) of the electrode tab with a laser output of 9 J / mm. At this time, the laser irradiation position selection process and the laser output adjustment process based on tolerance position search were both excluded, and only laser welding was performed at a fixed position.
[0109] Evaluation example
[0110] The mechanical properties of the weld bead were evaluated by testing the tensile strength using a universal test machine under conditions of 20 mm / min.
[0111] To evaluate the concentration deviation (△C) and the formation of intermetallic compounds (IMC) in the weld bead, the composition (weight% copper) of the weld bead was quantified and analyzed using SEM-EDS (SEM, Scanning Electron Microscope, EDS, energy dispersive X-ray spectroscopy).
[0112] The morphological symmetry of the weld bead was evaluated by measuring the ratios of L1 and L2 and D1 and D2 using optical microscope image analysis (OM).
[0113] High-temperature cracking was assessed by examining the presence or absence of cracks on the weld bead surface during the above welding process, and was indicated as X if no cracks occurred and O if cracks occurred.
[0114] After performing the above welding process, the weld bead surface was examined for the presence of cracks by leaving it at room temperature (25℃) for 5 days. X was used to indicate no cracks, and O was used to indicate cracks.
[0115] For embrittlement cracking, the occurrence of cracks on the surface of the weld bead was investigated in the actual use evaluation environment of the secondary battery module. X was indicated if no cracks occurred, and O was indicated if cracks occurred. Specifically, the occurrence of cracks was investigated while charging the secondary battery module containing the weld bead at a constant voltage (up to 4.2V) for 5 days under conditions of 0.4 MPa and 60℃.
[0116] The above evaluation results are shown in Table 1 below.
[0117] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Concentration deviation (△C) (weight%) 4 2 12 9 morphological symmetry L1 0.92L2 0.98L2 1.45L2 1.10L2 D1 1.05D2 0.98D2 1.30D1 1.20D2 copper concentration (weight%) 8 4 39 31 Tensile strength (arbitrary) 0.99 1 0.87 0.93 Whether high-temperature cracks occur X X O X Whether low-temperature cracks occur X X O O Whether embrittlement cracks occur X X O O
[0118] Referring to Table 1 above, Example 1 satisfies geometric symmetry (Equations 2 and 3) with a concentration deviation (△C) of 4 wt% (Equation 1), L1=0.92L2 and D1=1.05D2, and with a copper concentration of 8 wt%, it can be inferred that the formation of intermetallic compounds (IMC) is minimized, and no high-temperature cracking, low-temperature cracking, or embrittlement cracking occur, and an excellent weld bead with a tensile strength of 0.99 can be confirmed.
[0119] In addition, Example 2 shows that the weld bead satisfies geometric symmetry (Equations 2 and 3) with a concentration deviation (△C) of 2 wt% (Equation 1), L1=0.98L2 and D1=0.98D2, and with a copper content of 4 wt%, the formation of intermetallic compounds (IMC) is minimized and the weld bead with the best tensile strength can be confirmed.
[0120] On the other hand, Comparative Example 1 does not satisfy Equations 1 to 3 with a concentration deviation (△C) of 12 wt%, L1=1.45L2 and D1=1.30D2, and it can be inferred that a large amount of intermetallic compounds (IMC) are formed as the copper content is 39 wt%, and high-temperature cracking, low-temperature cracking, and embrittlement cracking all occur, and a weld bead with a significantly low tensile strength of 0.87 can be confirmed.
[0121] In addition, Comparative Example 2 has a weld bead with a concentration deviation (△C) of 9 wt%, L1=1.10L2 and D1=1.20D2, which does not satisfy Equation 1, satisfies Equation 2, and does not satisfy Equation 3, and the copper content is 31 wt%. Therefore, it can be inferred that high-temperature cracking does not occur, but low-temperature cracking and embrittlement cracking occur, and that more intermetallic compounds (IMCs) are formed than in Examples 1 and 2, and that a weld bead with a low tensile strength of 0.93 can be confirmed.
[0122] As described above, the present invention has been explained by specific details, limited embodiments, and drawings; however, this is provided merely to aid in a more comprehensive understanding of the invention, and the invention is not limited to the above embodiments. Those skilled in the art can make various modifications and variations from this description.
[0123] Accordingly, the scope of the present invention is not limited to the described embodiments, and all things equivalent to or having equivalent variations to the claims set forth below, as well as the claims set forth below, shall be considered to fall within the scope of the concept of the present invention. Explanation of the symbols
[0124] 110: Battery cell, 120: Battery tab, 150: Busbar, 150a: Plate, 150c: Hole, 151 Insertion part, 151a: Tab connection part, 151b: Groove, t1: Thickness direction of the plate, t2: Thickness direction of the electrode tab, 170 Weld bead, L: Laser, T: Thickness of the electrode tab, H: Height of the weld bead, W: Width of the weld bead, CL: Centerline of the hole, P1: Boundary point on the left side, P2: Boundary point on the right side, P100: Intersection point on the left side, P200: Intersection point on the right side
Claims
Claim 1 A secondary battery module comprising a plurality of battery cells each including an electrode tab, a bus bar connected to the plurality of electrode tabs to electrically connect the plurality of battery cells to each other, wherein the bus bar comprises a plate having a plurality of holes formed therein, wherein the electrode tabs of the plurality of battery cells are inserted so as to protrude through at least a portion of the plurality of holes of the plate and then welded, wherein the welding is performed on the protruding electrode tabs, wherein the electrode tabs inserted into the holes and the plate are joined to each other by a weld bead, wherein the weld bead comprises one or more weld beads, and wherein the concentration deviation (△C) measured by SEM-EDS analysis (SEM, Scanning Electron Microscope, EDS, energy dispersive X-ray spectroscopy) satisfies the following Equation 1. [Equation 1] Concentration deviation (△C) < 5 wt% (wherein the above Equation 1, the concentration deviation (△C) is the average copper concentration (C1) on the left side relative to the centerline of the hole in the cross-section of the weld bead in the thickness direction of the plate and the average on the right side It refers to the difference in copper concentration (C2). Claim 2 A secondary battery module according to claim 1, wherein the welding bead satisfies a concentration deviation (△C) of 3 weight% or less. Claim 3 delete Claim 4 A secondary battery module according to claim 1, wherein the weld bead is a symmetrical weld bead that is symmetrical with respect to the centerline of the hole in the weld bead cross-section in the thickness direction of the plate. Claim 5 In claim 4, a secondary battery module in which the weld bead having the symmetry satisfies the following Equations 2 and 3. [Equation 2] 0.90L2 ≤ L1 ≤ 1.1L2 [Equation 3] 0.90D2 ≤ D1 ≤ 1.1D2 (wherein Equations 2 and 3, L1 and L2 represent the shortest distance from the intersection point (P100, P200) to the boundary point (P1, P2), and D1 and D2 represent the distance from the intersection point (P100, P200) to the bonding interface of the weld bead perpendicular to L1 and L2, wherein the boundary point (P1, P2) represents the boundary point (P1, P2) on the left and right sides where the bonding interface of the weld bead meets the surface of the weld bead, and the intersection point (P100, P200) represents the hole at the boundary point (P1, P2). It refers to the intersection points (P100, P200) on the left and right sides where a line perpendicular to the centerline and an imaginary line (L100, L200) extending from the boundary surface of the electrode tab intersect perpendicularly. Claim 6 A secondary battery module according to claim 1, wherein the weld bead comprises: a cover portion having a convex shape covering the hole in the weld bead cross-section in the thickness direction of the plate; and a column portion inserted into the hole. Claim 7 A secondary battery module according to claim 1, wherein the electrode tab is made of aluminum and the plate is made of copper. Claim 8 In claim 1, the welding bead is a secondary battery module having a copper concentration of 40 weight% or less. Claim 9 In claim 1, the welding bead is a secondary battery module in which the plate dilution rate is 40% or less. Claim 10 In claim 1, the battery cell is a pouch-type battery cell, which is a secondary battery module.
Citation Information
Patent Citations
Method for laser weding of different metals with optimization of welding condition by using intermetallic compound analysis
KR1020190029030A
Battery Module
KR1020210061945A