Method for manufacturing monodispersed polymer polyols
A method for producing monodisperse polymer polyols using a dispersion stabilizer with specific polyether polyol properties and batch polymerization addresses non-uniformity and quality issues, achieving stable polymerization and cost-effective production of high-quality polyurethane products.
Patent Information
- Application Number
- KR1020240147282
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-10-25
AI Technical Summary
Conventional methods for manufacturing polymer polyols result in non-uniform particle sizes and quality degradation due to the use of chain transfer agents and organic diluents, leading to VOCs and odor generation, and require acrylonitrile to improve graft efficiency, increasing production costs.
A method involving the production of a dispersion stabilizer by reacting a reactive unsaturated compound with a polyether polyol having specific hydroxyl and ethylene oxide content, followed by batch polymerization of a mixture containing a base polyol, aromatic vinyl monomer, and initiator, to produce a monodisperse polymer polyol.
The method achieves excellent dispersion and polymerization stability, enabling the production of high-quality polyurethane molded articles without acrylonitrile, reducing production costs and environmental impact.
Abstract
Description
Technology Field
[0001] This specification relates to a method for manufacturing a monodisperse polymer polyol. Background Technology
[0002] Polymer polyols (POPs), also known as copolymer polyols (CPPs), are generally used to enhance the hardness and breathability of polyurethanes. Recently, as the use of polyurethane in automotive seats, furniture, and the like has increased, there is also a growing need for methods to manufacture high-quality polymer polyols at low production costs.
[0003] Conventional methods for manufacturing polymer polyols involve mixing a certain amount of styrene monomer (SM) and acrylonitrile (AN) with a base polyol and continuously adding this mixture to a reactor filled with the remaining base polyol while maintaining a polymerization temperature at a constant rate to disperse polydisperse SAN particles, which are copolymers of styrene monomer and acrylonitrile, into the base polyol. While this method of continuous monomer addition has the advantage of effectively dissipating the polymerization heat generated in large quantities, particularly during the polymerization of acrylonitrile, it has the disadvantages that the particle size of the formed polymer particles is non-uniform due to the monomer being added during the polymerization process, and that chain transfer agents or organic diluents must be used to address the rapid viscosity changes that occur during the continuous addition of monomers. These chain transfer agents and organic diluents are the cause of VOCs and odor generation in the product.
[0004] Polymerization stabilizers used in the manufacture of polymer polyols are macromonomers containing reactive unsaturated groups capable of copolymerizing with polymerizable monomers at the polyol terminals. They play a role in improving the steric stability of the resulting particles by forming graft copolymers during polymerization. However, styrene monomers have low graft efficiency with polymerization stabilizers; when used alone, this leads to a decrease in the quality of the polymer polyol due to problems such as high viscosity resulting from reduced steric stability and an increase in the production of soluble oligomers. To address this, acrylonitrile is used, which has relatively high graft efficiency and can reduce the production of soluble oligomers by copolymerizing with styrene monomers; however, this causes an increase in the production cost of polymer polyols.
[0005] Meanwhile, the polymerization stabilizers used in the manufacture of conventional polymer polyols are designed for the manufacture of styrene-acrylonitrile copolymers, and when used in the manufacture of polymer polyols containing only polymers derived from aromatic vinyl monomers, the monomers may not polymerize well or the stability of the polymer may be insufficient, which may lead to a deterioration in the physical properties of the polyurethane foam. The problem to be solved
[0006] The details described in this specification were devised in consideration of the problems of the aforementioned prior art, and one objective is to provide a method for manufacturing a polymer polyol that exhibits excellent dispersion stability even during homopolymerization of aromatic vinyl monomers, thereby preventing degradation of the quality of the final product. means of solving the problem
[0007] According to one aspect of the present specification, a method for producing a monodisperse polymer polyol is provided, comprising: (a) a step of producing a dispersion stabilizer by reacting a reactive unsaturated compound in the presence of a polyether polyol having a hydroxyl value of 50 to 70 mgKOH / g and an ethylene oxide content of 1% or more and less than 20% by weight; and (b) a step of producing a monodisperse polymer polyol by polymerizing a mixture prepared by adding a base polyol, an aromatic vinyl monomer, an initiator, and the dispersion stabilizer in batches.
[0008] In one embodiment, the hydroxyl value of the polyether polyol may be 50 to 60 mgKOH / g.
[0009] In addition, the ethylene oxide content of the polyether polyol may be 5 to 15 weight percent.
[0010] In one embodiment, the polyol described above may be a polyol having a hydroxyl value of 20 to 80 mgKOH / g and an ethylene oxide content of 5 to 30 weight%.
[0011] Here, the reactive unsaturated compound may be at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, itaconic acid, citraconic acid, citraconic anhydride, phthalic acid, phthalic anhydride, hydroxyalkyl acrylate and methacrylate.
[0012] Meanwhile, the above aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, divinylnaphthalene, divinylbenzene, trivinylbenzene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene primary It may be at least one selected from the group consisting of styrene functionalized with amines, styrene functionalized with secondary amines, and styrene functionalized with tertiary amines.
[0013] Meanwhile, the solid content of the above polymer polyol may be 10 to 70 weight percent.
[0014] In addition, the average particle size of the polymer polyol may be 0.8 to 1.5 μm.
[0015] Here, the unsaturated nitrile-based compound in the polymer polyol may be less than 1 weight%.
[0016] According to another aspect of the present specification, a monodisperse polymer polyol is provided, comprising: a polyol having a hydroxyl value of 30 to 60 mgKOH / g and an ethylene oxide content of 1 to 30 weight%; and a polymer derived from an aromatic vinyl monomer dispersed in the polyol, wherein the unsaturated nitrile compound is less than 1 weight%.
[0017] According to another aspect of the present specification, a polyurethane molded article is provided, prepared by reacting the aforementioned monodisperse polymer polyol with an isocyanate compound. Effects of the invention
[0018] According to one aspect, a method for manufacturing a polymer polyol can be provided, which has excellent dispersion stability and polymerization stability effects even during homopolymerization of aromatic vinyl monomers, thereby enabling the production of a high-quality polyurethane molded article regardless of the characteristics of the base polyol.
[0019] The effects of one aspect of this specification are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configurations described in the detailed description or claims of this specification. Specific details for implementing the invention
[0020] Hereinafter, one aspect of this specification will be described. However, the details described in this specification may be implemented in various different forms and are therefore not limited to the embodiments described herein. Furthermore, to clearly explain one aspect of this specification, parts unrelated to the description have been omitted.
[0021] Throughout the specification, when it is stated that a part is "connected" to another part, this includes not only cases where they are "directly connected," but also cases where they are "indirectly connected" with other members interposed between them. Furthermore, when it is stated that a part "includes" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but rather allows for the inclusion of additional components.
[0022] When a range of numerical values is described in this specification, unless a specific range is otherwise described, the value has the precision of significant figures provided according to the standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.
[0023] In this specification, “polymer polyol” is also referred to as copolymer polyol and is a product in which granulated organic or inorganic fillers are dispersed in a specific amount in a liquid base polyol. A polyol prepared by dispersing and polymerizing polymer particles in a polyether polyol is also a type thereof.
[0024] “Polyurethane” is a polymer material containing a large amount of urethane (-NHCOO) bonds. It is generally used by molding and processing it into a lightweight, honeycomb-shaped foam through a polymer reaction that generates bubbles. “Polyurethane foam” is typically classified into flexible, rigid, and semi-rigid types.
[0025] "Dispersion polymerization" is a polymerization method that uses a solvent, dispersion stabilizer, and polymerization initiator that are soluble in the monomer but insoluble in the resulting polymer. In this method, all components are dissolved in a single phase at the beginning of the reaction, but as polymerization proceeds, the polymer product precipitates, and a product with particle sizes ranging from hundreds of nanometers to tens of microns is obtained through the action of the dispersion stabilizer.
[0026] “Hydroxyl value (OH-Value, OHV),” also known as the hydroxyl number, refers to the weight of mg of potassium hydroxide (KOH) equivalent to the OH groups present in 1 g of polyol, and can be expressed in units of mgKOH / g. This hydroxyl value can be measured by various methods. For example, it can be analyzed using a near-infrared (NIR) spectrometer. Such analysis can be performed in accordance with ASTM D6342 to ISO 15063.
[0027] "Mono-disperse" refers to a case in a dispersion system where the individual particles of the dispersed phase are of uniform size. Polymers obtained by ordinary methods are polydisperse systems with a distribution of molecular weight; in contrast, a system with practically no distribution is called a monodisperse system. Methods include directly obtaining a system close to monodisperse through living polymerization, or converting a polydisperse system into a system close to monodisperse through fractionation.
[0029] Method for manufacturing monodisperse polymer polyol
[0030] A method for preparing a monodisperse polymer polyol according to one aspect of the present specification may comprise: (a) a step of preparing a dispersion stabilizer by reacting a reactive unsaturated compound in the presence of a polyether polyol having a hydroxyl value of 50 to 70 mgKOH / g and an ethylene oxide content of 1% or more and less than 20% by weight; and (b) a step of preparing a monodisperse polymer polyol by polymerizing a mixture prepared by adding a base polyol, an aromatic vinyl monomer, an initiator, and the dispersion stabilizer in a batch.
[0031] Step (a) above may be a step of preparing a dispersion stabilizer suitable for the polymerization of aromatic vinyl monomers.
[0032] In the conventional preparation of monodisperse polymer polyols, a dispersion stabilizer in the form of a macromer was used, which has graft sites on the polyol chain that can bind to a styrene-acrylonitrile copolymer. The dispersion stabilizer contains double bonds that can undergo graft reactions with aromatic vinyl monomers and exists on the surface of the aromatic vinyl polymer in a hair-like form, thereby suppressing aggregation between polymer particles.
[0033] Typically, methods for imparting double bonds to dispersion stabilizers include reacting compounds such as maleic anhydride or phthalic anhydride with a polyol to directly impart double bonds to the polyol chain, or reacting hydroxyalkyl acrylate or methacrylate with an isocyanate to form double bonds, and then preparing a macromer through a prepolymer reaction with the polyol.
[0034] Dispersion stabilizers are mixtures of styrene and acrylonitrile and can be advantageous for forming a stable polymer structure. Styrene-acrylonitrile copolymers are used in various fields because they possess high strength and excellent durability. Conventional dispersion stabilizers can sufficiently bind to styrene-acrylonitrile copolymers, resulting in small and uniform particle sizes, which can be used to manufacture polyurethane foam with excellent mechanical properties.
[0035] As described above, using conventional polyol-based macromers allows even monomers that are difficult to undergo chain transfer reactions, such as styrene, to be dispersed into stable polymer particles through radical polymerization. However, if styrene is used alone without acrylonitrile, the rate of the chain transfer reaction is slow, which reduces reactivity with the dispersion stabilizer; consequently, this increases reaction time and lowers the conversion rate. Therefore, this type of dispersion stabilizer presents a problem where the physical properties of the polyurethane foam deteriorate depending on the type of base polyol. In other words, monodisperse polymer polyols to which conventional dispersion stabilizers are applied fail to sufficiently bond with polystyrene, making the performance of the polyurethane foam prone to degradation.
[0036] This may be because conventional dispersion stabilizers are suitable for styrene-acrylonitrile copolymers and do not have sufficient reactivity with styrene, which reduces the particle stability of polystyrene within the monodisperse polymer polyol. Additionally, when a highly polar base polyol is applied, styrene does not dissolve well, which reduces the stability of dispersion polymerization and can cause a decrease in the physical properties of the final product.
[0037] The polyether polyol of step (a) above may have a hydroxyl value (OHV) of 50 to 70 mgKOH / g, for example, 50 mgKOH / g, 52 mgKOH / g, 54 mgKOH / g, 56 mgKOH / g, 58 mgKOH / g, 60 mgKOH / g, 62 mgKOH / g, 64 mgKOH / g, 66 mgKOH / g, 68 mgKOH / g, 70 mgKOH / g, or a range between two of these values.
[0038] If the hydroxyl group of a polyol is high, the molecular weight may be low. On the other hand, if the hydroxyl group is low, the molecular weight may be high.
[0039] If the chain length of the polyether polyol constituting the dispersion stabilizer becomes excessively long, the concentration of functional groups decreases, and as a result, aromatic vinyl monomers with slow chain transfer reaction rates may find it difficult to react sufficiently. On the other hand, if the molecular weight of the polyether polyol is excessively small, the hairs of the prepared dispersion stabilizer become short, which may degrade its performance as a dispersion stabilizer.
[0040] In one embodiment, the hydroxyl value of the polyether polyol is 50 to 60 mgKOH / g. For example, it may be 50 mgKOH / g, 52 mgKOH / g, 54 mgKOH / g, 56 mgKOH / g, 58 mgKOH / g, 60 mgKOH / g, or a range between two of these values, but is not limited thereto.
[0041] If the hydroxyl group of the above polyether polyol is adjusted to an appropriate range, it can easily react with aromatic vinyl monomers to form a polymer more stably, and the performance of the prepared dispersion stabilizer can be excellent.
[0042] The ethylene oxide content of the polyether polyol may refer to the ratio of the ethylene oxide compound added during the synthesis of each polyol. The polyether polyol may be a polyether polyol prepared by adding ethylene oxide and propylene oxide to an initiator having two or more active hydrogens (-OH, -NH2), but is not limited thereto.
[0043] If the ethylene oxide content is high, the polarity of the dispersion stabilizer may increase. When a dispersion stabilizer with a high ethylene oxide content is applied to a polymer polyol, it has a low affinity for non-polar polymer particles, which may increase the spacing between polymer particles. When a dispersion stabilizer with a low ethylene oxide content is applied to a polymer polyol, it has a high affinity for polymer particles, which may reduce the spacing between polymer particles and cause aggregation. If the polarity of the dispersion stabilizer is very high, it can be applied as a dispersion stabilizer for rigid polymer polyols.
[0044] Meanwhile, the polyether polyol of step (a) above has an ethylene oxide content of 1 wt% or more and less than 20 wt%, for example, 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, 10.5 wt%, 11 wt%, 11.5 wt%, 12 wt%, 12.5 wt%, 13 wt%, 13.5 wt%, 14 wt%, 14.5 wt%, 15 wt%, 15.5 wt%, 16 wt%, 16.5 wt%, It may be 17 wt%, 17.5 wt%, 18 wt%, 18.5 wt%, 19 wt%, 19.5 wt%, 19.9 wt%, or a range between two of these values.
[0045] If the polarity of the above polyether polyol is too high, the affinity with non-polar aromatic vinyl monomers is reduced, which may lower polymerization stability. Conversely, if the polarity of the above polyether polyol is too low, reactivity is reduced, which shortens the hair of the dispersion stabilizer and may result in insufficient performance.
[0046] In one embodiment, the ethylene oxide content of the polyether polyol may be 5 to 15 wt%, for example, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, 10.5 wt%, 11 wt%, 11.5 wt%, 12 wt%, 12.5 wt%, 13 wt%, 13.5 wt%, 14 wt%, 14.5 wt%, 15 wt%, or a range between two of these values, but is not limited thereto.
[0047] By adjusting the ethylene oxide content of the above polyether polyol to an appropriate range, the affinity with aromatic vinyl monomers is increased, allowing for the more stable formation of the polymer and excellent performance of the prepared dispersion stabilizer. As a result, a high-quality monodisperse polymer polyol can be produced regardless of the characteristics of the base polyol.
[0048] The above dispersion stabilizer can be prepared by reacting the polyether polyol and the reactive unsaturated compound in the presence of a catalyst.
[0049] As the catalyst, inorganic bases such as hydroxides of alkali metals or alkaline earth metals, weak salts of alkali metals or alkaline earth metals, organic bases such as quaternary ammonium hydroxides, 4-dimethylaminopyridine, 4-pyrrolidinopyridine, and imidazole, acids such as hydrochloric acid, sulfuric acid, and phosphoric acid, and organotin compounds such as dibutyltin dilaurate, dibutyltin diacetate, dibutyltin dioctoeate, dibutyltin dibutoxide, dibutyltin dimethoxide, tin dilaurate, tin diacetate, tin dioctoeate, tin 2-ethylhexanoate, tin dibutoxide, and tin dimethoxide may be used, but are not limited thereto.
[0050] In one example, the unsaturated reactive compound may be a reactive unsaturated compound having one or more carbon-carbon double bonds and two or more carbon-oxygen double bonds, but is not limited thereto.
[0051] In one example, the unsaturated reactive compound may be at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, itaconic acid, citraconic acid, citraconic anhydride, phthalic acid, phthalic anhydride, hydroxyalkyl acrylate and methacrylate, but is not limited thereto.
[0052] Based on 100 parts by weight of the polyether polyol, the content of the reactive unsaturated compound may be 1 to 5 parts by weight, for example, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, or a range between two of these values. Using a dispersion stabilizer prepared by introducing a small amount of reactive unsaturated compound into the polyol can improve the dispersion stability of the solid component during the production of the polymer polyol.
[0053] The reaction temperature suitable for manufacturing the above dispersion stabilizer may be 80 to 150°C, for example, 80°C, 82.5°C, 85°C, 87.5°C, 90°C, 92.5°C, 95°C, 97.5°C, 100°C, 102.5°C, 105°C, 107.5°C, 110°C, 112.5°C, 115°C, 117.5°C, 120°C, 122.5°C, 125°C, 127.5°C, 130°C, 132.5°C, 135°C, 137.5°C, 140°C, 142.5°C, 145°C, 147.5°C, 150°C, or a range between two of these values. The reaction may be carried out in a reactor capable of performing stirring and pressurization.
[0054] Step (b) above may involve preparing a polymer polyol by polymerizing an aromatic vinyl monomer dissolved in a base polyol in the presence of the aforementioned dispersion stabilizer. As a result, the polymer polyol may be in a form in which polymer particles derived from the aromatic vinyl monomer are stably dispersed in a liquid base polyol. A polyurethane foam prepared using such a polymer polyol may have excellent mechanical properties and breathability.
[0055] Here, the polyol described above and the aromatic vinyl monomer may be added in a weight ratio of 30 to 70:70 to 30, for example, 30:70, 32.5:67.5, 35:65, 37.5:62.5, 40:60, 42.5:57.5, 45:55, 47.5:52.5, 50:50, 52.5:47.5, 55:45, 57.5:42.5, 60:40, 62.5:37.5, 65:35, 67.5:32.5, 70:30, or a range between two of these values.
[0056] If the ratio of the polyol described above and the aromatic vinyl monomer falls outside the above range, the solid content of the polymer polyol increases excessively, causing aggregation or a decrease in the hardness of the final product, the polyurethane foam.
[0057] Meanwhile, conventional methods for manufacturing polymer polyols cause problems such as aggregation, formation of soluble oligomers, and deterioration of product quality during the homopolymerization of aromatic vinyl monomers, whereas the above manufacturing method can produce high-quality polymer polyols even when aromatic vinyl monomers are added alone.
[0058] In step (b) above, the aromatic vinyl monomer included in the mixture may react to form a polymer, and then the polymer may be granulated to form polymer polyol particles dispersed in the base polyol included in the mixture. Additionally, the aromatic vinyl monomer included in the mixture may be gradually consumed as it polymerizes into the base polyol, that is, polymer polyol particles may be formed in a manner substantially similar to addition polymerization.
[0059] Here, the polymer derived from the aromatic vinyl monomer can be polymerized in a monodisperse form. In this way, when a certain amount of monomer is homopolymerized, the amount of soluble oligomers produced can be reduced without using unsaturated nitrile monomers as in the past.
[0060] Independent of the reaction mechanism of the aromatic vinyl monomer included in the above mixture, the base polyol and the aromatic vinyl monomer, which are raw materials for the manufacture of the polymer polyol, may be fed into the reactor in a single batch rather than being fed in divided or continuous. This single-batch feeding method has the advantage of simplifying the process compared to the conventional continuous feeding method. Furthermore, this single-batch feeding method can improve stability by unifying the timing of polymer formation, thereby ensuring that the particles have a monodisperse distribution.
[0061] The polyol described above may be a polyether polyol obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to polyhydric alcohols such as propylene glycol and glycerin, but any polyol suitable for manufacturing polymer polyols may be used without limitation.
[0062] In one embodiment, the polyol described above has a hydroxyl value of 20 to 80 mgKOH / g, for example, 20 mgKOH / g, 22 mgKOH / g, 24 mgKOH / g, 26 mgKOH / g, 28 mgKOH / g, 30 mgKOH / g, 32 mgKOH / g, 34 mgKOH / g, 36 mgKOH / g, 38 mgKOH / g, 40 mgKOH / g, 42 mgKOH / g, 44 mgKOH / g, 46 mgKOH / g, 48 mgKOH / g, 50 mgKOH / g, 52 mgKOH / g, 54 mgKOH / g, 56 mgKOH / g, 58 mgKOH / g, 60 mgKOH / g, 62 mgKOH / g, 64 mgKOH / g, 66 mgKOH / g, It may be 68 mgKOH / g, 70 mgKOH / g, 72 mgKOH / g, 74 mgKOH / g, 76 mgKOH / g, 78 mgKOH / g, 80 mgKOH / g, or a range between two of these values. If the hydroxyl value of the polyol described falls outside the above range, aggregation of the polymer polyol may occur.
[0063] Meanwhile, the polyol described above has an ethylene oxide content of 5 to 30 wt%, for example, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, 10.5 wt%, 11 wt%, 11.5 wt%, 12 wt%, 12.5 wt%, 13 wt%, 13.5 wt%, 14 wt%, 14.5 wt%, 15 wt%, 15.5 wt%, 16 wt%, 16.5 wt%, 17 wt%, 17.5 wt%, 18 wt%, 18.5 wt%, 19 wt%, 19.5 wt%, 20 wt%, 20.5 wt%, 21 wt%, It may be a polyol with an amount of 21.5 wt%, 22 wt%, 22.5 wt%, 23 wt%, 23.5 wt%, 24 wt%, 24.5 wt%, 25 wt%, 25.5 wt%, 26 wt%, 26.5 wt%, 27 wt%, 27.5 wt%, 28 wt%, 28.5 wt%, 29 wt%, 29.5 wt%, 30 wt%, or a range between two of these values.
[0064] The above aromatic vinyl monomers are styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, divinylnaphthalene, divinylbenzene, trivinylbenzene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, and diphenylethylene primary amines. It may be at least one selected from the group consisting of functionalized styrene, styrene functionalized with a secondary amine, and styrene functionalized with a tertiary amine.
[0065] As the above initiator, organic peroxide-based initiators such as t-butylperoxy-2-ethylhexanoate, t-butylperpivalate, t-amylperoctoate, 2,5-dimethyl-hexane-2,5-di-per-2-ethylhexoate, t-butylperneodecanoate, and t-butylperbenzoate, or azo-based initiators such as azobisisobutyronitrile (AIBN) and azobismethylbutyronitrile (AMBN) may be used. The content of the initiator may be 0.1 to 2.5 parts by weight based on 100 parts by weight of the total monomer, for example, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight, 2 parts by weight, 2.1 parts by weight, 2.2 parts by weight, 2.3 parts by weight, 2.4 parts by weight, 2.5 parts by weight, or a range between two of these values. If the content of the initiator falls outside the above range, the polymerization rate and dispersion stability may decrease.
[0066] The aforementioned dispersion stabilizer has excellent affinity for aromatic vinyl monomers and can compensate for slow chain transfer reaction rates due to its high functional group concentration, and can provide excellent dispersion stability for polymer particles derived from aromatic vinyl monomers.
[0067] The above dispersion stabilizer provides a dispersion stabilization effect during the initial stage of polymer polyol manufacturing and, based on its high dispersion stability, can also serve as a polymerization stabilizer that provides a buffering effect between the polymers formed during the later stages of manufacturing.
[0068] Based on 100 parts by weight of the above aromatic vinyl monomer, the content of the dispersion stabilizer may be 1 to 10 parts by weight, for example, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, or a range between two of these values. If the content falls outside the above range, aggregation of polymer particles may occur, or the solid content may not reach the required level.
[0069] When preparing the above polymer polyol, a molecular weight regulator or a diluent may be further included. For example, alcohols such as methanol, ethanol, isopropanol, butanol, mercaptans such as ethanethiol, heptanethiol, octanethiol, dodecanethiol, toluene, ethylbenzene, xylene, etc. may be used, but are not limited thereto.
[0070] The polymerization of step (b) above may be performed at 80 to 150°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, or in a range between two of these values. Step (b) above may be performed while continuously stirring.
[0071] The polymerization of step (b) above may be performed for 1 to 30 hours, for example, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours, 30 hours, or for a time between two of these values.
[0072] After the polymerization of step (b) above, the polymerization can be carried out at a temperature equal to or higher than the polymerization temperature for 1 to 10 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, 7.5 hours, 8 hours, 8.5 hours, 9 hours, 9.5 hours, 10 hours, or a time between two of these values. Through this aging process, polymer particles can be stably dispersed within the polyol.
[0073] After the above aging process, a degassing process may be performed to remove unreacted monomers and other additives. Known methods may be applied for this degassing process.
[0074] The above polymer polyol may have a solid content of 10 to 70 wt%, for example, 10 wt%, 12.5 wt%, 15 wt%, 17.5 wt%, 20 wt%, 22.5 wt%, 25 wt%, 27.5 wt%, 30 wt%, 32.5 wt%, 35 wt%, 37.5 wt%, 40 wt%, 42.5 wt%, 45 wt%, 47.5 wt%, 50 wt%, 52.5 wt%, 55 wt%, 57.5 wt%, 60 wt%, 62.5 wt%, 65 wt%, 67.5 wt%, 70 wt%, or a range between two of these values. If the solid content falls outside the above range, the physical properties of the final product may be poor or aggregation of the polymer polyol may occur.
[0075] In addition, the average particle size of the polymer polyol may be 0.8 to 1.5 μm. That is, the polymer derived from the aromatic vinyl monomer may be particles with an average particle size of 0.8 to 1.5 μm, for example, 0.8 μm, 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, or a range between two of these values. The polymer polyol may be one in which polymer particles having the aforementioned average particle size are dispersed on a liquid substrate polyol without aggregating.
[0076] Here, the unsaturated nitrile compound in the polymer polyol may be less than 1% by weight, less than 0.5% by weight, less than 0.1% by weight, or may not contain any unsaturated nitrile compound. The polymer polyol is environmentally friendly as it does not contain unsaturated nitrile compounds such as acrylonitrile and can be manufactured through a simpler process.
[0078] Monodisperse polymer polyols and polyurethane molded bodies
[0079] A polymer polyol according to another aspect of the present specification comprises: a polyol having a hydroxyl value of 30 to 60 mgKOH / g and an ethylene oxide content of 1 to 30 weight%; and a polymer derived from an aromatic vinyl monomer dispersed in the polyol; wherein the unsaturated nitrile compound may be less than 1 weight%.
[0080] Here, the monodisperse polymer polyol comprises the polyether polyol and a component derived from the base polyol, with a hydroxyl value of 30 to 60 mgKOH / g, e.g., 30 mgKOH / g, 32 mgKOH / g, 34 mgKOH / g, 36 mgKOH / g, 38 mgKOH / g, 40 mgKOH / g, 42 mgKOH / g, 44 mgKOH / g, 46 mgKOH / g, 48 mgKOH / g, 50 mgKOH / g, 52 mgKOH / g, 54 mgKOH / g, 56 mgKOH / g, 58 mgKOH / g, 60 mgKOH / g, or a range between two of these values, and an ethylene oxide content of 1 to 30 wt%, e.g., 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, 10.5 wt%, 11 wt%, 11.5 wt%, 12 wt%, 12.5 wt%, 13 wt%, 13.5 wt%, 14 wt%, 14.5 wt%, 15 wt%, 15.5 wt%, 16 wt%, 16.5 wt%, 17 wt%, 17.5 wt%, 18 wt%, 18.5 wt%, 19 wt%, 19.5 wt%, 20 wt%, 20.5 wt%, 21 wt%, It may include a polyol in an amount of 21.5 wt%, 22 wt%, 22.5 wt%, 23 wt%, 23.5 wt%, 24 wt%, 24.5 wt%, 25 wt%, 25.5 wt%, 26 wt%, 26.5 wt%, 27 wt%, 27.5 wt%, 28 wt%, 28.5 wt%, 29 wt%, 29.5 wt%, 30 wt%, or a range between two of these values.
[0081] Here, the polymer derived from the aromatic vinyl monomer may be dispersed in the polyol or bonded to the polymer chain of the polyol.
[0082] The above polymer polyol can be used to replace some or all of the base polyols in known polyurethane systems. In addition to the polyol, the polyurethane system may further include additives such as foam stabilizers, catalysts, blowing agents, and crosslinking agents. These additives may be those known in the industry.
[0083] A polyurethane molded article according to another aspect of the present specification may be prepared by reacting the aforementioned monodisperse polymer polyol with an isocyanate compound.
[0084] For example, the above polyurethane molded article may be a polyurethane foam. The above polymer polyol may be used in the manufacture of polyurethane foam. When the above polymer polyol is applied, mechanical properties, breathability, etc., can be improved compared to when a general polyol is used.
[0085] Polyurethane foam manufactured using the above polymer polyol has improved factors affecting the sensory quality of the final product, such as elasticity, stress relief, and vibration transmission rate, making it suitable for providing comfort.
[0087] The embodiments of this specification will be described in more detail below. However, the following experimental results represent only representative results among the above embodiments, and the scope and content of this specification should not be interpreted as being narrowed or limited by the embodiments. The respective effects of various embodiments of this specification not explicitly presented below will be described in detail in the relevant sections.
[0088] Preparation Example 1
[0089] Example 1
[0090] 1,000 parts by weight of a polyether polyol with an OHV of 56 mgKOH / g and an ethylene oxide (EO) content of 10 wt%, 35 parts by weight of maleic anhydride, and 1 part by weight of sodium hydroxide were introduced into a reactor. A dispersion stabilizer was prepared by stirring for 14 hours under conditions of 130°C and 200 rpm.
[0091] A mixture was prepared by adding 45 parts by weight of styrene monomer, 25 parts by weight of ethylbenzene diluent, 55 parts by weight of a base polyol with an OHV of 56 mgKOH / g and an ethylene oxide content of 7% by weight, and 1 part by weight of the dispersion stabilizer to a stirring tank equipped with a stirrer, and stirring for 5 minutes.
[0092] The above mixture was introduced into a batch reactor equipped with a stirrer, and 0.3 parts by weight of the polymerization initiator azobisisobutyronitrile were mixed and completely dissolved at room temperature, followed by stirring for 10 minutes. Subsequently, the temperature of the reaction mixture was raised to 120°C over 1 hour while stirring at a speed of 250 rpm. The temperature and stirring conditions of the reactor were maintained at 115–125°C and 250 rpm, respectively. After the polymerization was completed, the mixture was aged for 1 hour.
[0093] The polymer, after polymerization and aging were completed, was transferred to a purification tank and degassed under reduced pressure for 20 hours at a temperature of 120°C to remove unreacted monomers and ethylbenzene dissolved in the polymer, thereby obtaining a polymer polyol.
[0094] Example 2
[0095] A polymer polyol was prepared in the same manner as in Example 1, except that a base polyol with an OHV of 34 mgKOH / g and an ethylene oxide content of 20 wt% was used.
[0096] Comparative Example 1
[0097] A polymer polyol was prepared in the same manner as in Example 1, except that a dispersion stabilizer was used, which is manufactured from a polyol with a viscosity of 8,000 cps at 25°C and a linearity enhancement process applied, and a mixture of 32 parts by weight of styrene and 13 parts by weight of acrylonitrile was used as the monomer.
[0098] Comparative Example 2
[0099] A polymer polyol was prepared in the same manner as in Example 2, except that a dispersion stabilizer was used, which is manufactured from a polyol with a viscosity of 8,000 cps at 25°C and a linearity enhancement process applied, and a mixture of 32 parts by weight of styrene and 13 parts by weight of acrylonitrile was used as the monomer.
[0100] Comparative Example 3
[0101] A polymer polyol was prepared in the same manner as in Example 1, except that a dispersion stabilizer was used, which is manufactured from a polyol of type 1 with a 25°C viscosity of 8,000 cps and a linearity enhancement process applied, and which is used in the conventional polymerization of styrene and acrylonitrile.
[0102] Comparative Example 4
[0103] A polymer polyol was prepared in the same manner as in Example 2, except that a dispersion stabilizer was used, which is manufactured from a polyol of type 1 and has a 25°C viscosity of 8,000 cps and is used in the polymerization of conventional styrene and acrylonitrile, and to which a linearity enhancement process is applied.
[0104] Comparative Example 5
[0105] A polymer polyol was prepared in the same manner as in Example 1, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 38 mgKOH / g and an ethylene oxide content of 10 wt%.
[0106] Comparative Example 6
[0107] A polymer polyol was prepared in the same manner as in Example 2, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 38 mgKOH / g and an ethylene oxide content of 10 wt%.
[0108] Comparative Example 7
[0109] A polymer polyol was prepared in the same manner as in Example 1, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 84 mgKOH / g and an ethylene oxide content of 10 wt%.
[0110] Comparative Example 8
[0111] A polymer polyol was prepared in the same manner as in Example 2, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 84 mgKOH / g and an ethylene oxide content of 10 wt%.
[0112] Comparative Example 9
[0113] A polymer polyol was prepared in the same manner as in Example 1, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 56 mgKOH / g and an ethylene oxide content of 20 wt%.
[0114] Comparative Example 10
[0115] A polymer polyol was prepared in the same manner as in Example 2, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 56 mgKOH / g and an ethylene oxide content of 20 wt%.
[0116] Comparative Example 11
[0117] A polymer polyol was prepared in the same manner as in Example 1, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 56 mgKOH / g and an ethylene oxide content of 0 wt%.
[0118] Comparative Example 12
[0119] A polymer polyol was prepared in the same manner as in Example 2, except that a dispersion stabilizer was prepared using a polyether polyol with an OHV of 56 mgKOH / g and an ethylene oxide content of 0 wt%.
[0120] The characteristics of the raw materials used in the above examples and comparative examples are shown in Table 1 below.
[0121] - Dispersion stabilizer polyol Polyol Whether acrylonitrile is used OHV(mgKOH / g) EO content (weight%) OHV(mgKOH / g) EO content (weight%) Example 1 56 10 56 7 X Example 2 56 10 34 20 X Comparative Example 1 - - 56 7 O Comparative Example 2 - - 34 20 O Comparative Example 3 - - 56 7 X Comparative Example 4 - - 34 20 X Comparative Example 5 38 10 56 7 X Comparative Example 6 38 10 34 20 X Comparative Example 7 84 10 56 7 X Comparative Example 8 84 10 34 20 X Comparative Example 9 56 20 56 7 X Comparative Example 10 56 20 34 20 X Comparative Example 11 56 0 56 7 X Comparative Example 12 56 0 34 20 X
[0122] The characteristics of the polymer polyols prepared in the examples and comparative examples and the characteristics of the polyurethane foam prepared using them were measured and are shown in Table 2 below.
[0123] -25% ILD (indentation load deflection): Measured by compressing a polyurethane foam, prepared and molded by reacting the above polymer polyol with 4,4'-methylene dibisphenyl diisocyanate (MDI) in a 300×300×100 mm mold, at 25% by volume after curing at room temperature for one day; the unit is kgf / 314cm² 2 all.
[0124] - Polymer polyol quality Polymer polyol solid content Polymer Polyol Average Particle Size (㎛) Foam 25% ILD (kgf / 314 cm²) 2 ) Foam tensile strength (kgf / cm²) 2 ) Example 1 Good 45.1 1.2 42 0.94 Example 2 Good 40.2 1.2 29 2.11 Comparative Example 1 Good 45.2 1.2 43 0.97 Comparative Example 2 Good 40.1 1.1 28 2.03 Comparative Example 3 Good 45.3 1.1 42 0.91 Comparative Example 4 Good 40.1 1.7 28 1.65 Comparative Example 5 Good 45.4 1.3 41 0.89 Comparative Example 6 Good 40 2 29 1.7 Comparative Example 7 Bad 45.3 2.8 35 0.65 Comparative Example 8 Bad 40.2 2.7 24 1.41 Comparative Example 9 aggregation Unable to evaluate Comparative Example 10 aggregation Unable to evaluate Comparative Example 11 aggregation Unable to evaluate Comparative Example 12 aggregation Unable to evaluate
[0125] Referring to Tables 1 and 2, the polymer polyol of the example showed performance equivalent to that of the polymer polyol of Comparative Examples 1 and 2, which used acrylonitrile, even though acrylonitrile was not used.
[0126] When using a conventional dispersion stabilizer for styrene-acrylonitrile polymerization without acrylonitrile, there is a problem where the foam properties deteriorate when a highly polar polyol is used as the base polyol (Comparative Example 4).
[0127] Meanwhile, if the molecular weight of the polyol used in the dispersion stabilizer is too high, the physical properties of the foam deteriorate (Comparative Examples 5, 6), and if the molecular weight is too low, the hairs of the dispersion stabilizer become short, which can lead to poor quality (Comparative Examples 7, 8). On the other hand, if the polarity of the dispersion stabilizer is too high, the affinity with the non-polar styrene monomer is low, so no dispersion stabilization effect is observed (Comparative Examples 9, 10). If the polarity of the dispersion stabilizer is too low, the reaction is slow, resulting in the production of a dispersion stabilizer with short hairs, and the dispersion stabilization effect of the polymer polyol is insufficient (Comparative Examples 11, 12).
[0128] The foregoing description of this specification is for illustrative purposes only, and those skilled in the art to which one aspect of this specification pertains will understand that other specific forms can be easily modified without altering the technical concept or essential features described in this specification. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.
[0129] The scope of this specification is defined by the claims, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of this specification.
Claims
Claim 1 (a) a step of preparing a dispersion stabilizer by reacting a reactive unsaturated compound in the presence of a polyether polyol having a hydroxyl value of 50 to 70 mgKOH / g and an ethylene oxide content of 1% or more and less than 20% by weight; and (b) a step of preparing a monodispersed polymer polyol by polymerizing a mixture prepared by adding a base polyol, an aromatic vinyl monomer, an initiator, and the dispersion stabilizer in a batch, wherein the reactive unsaturated compound directly reacts with the polyether polyol to form a bond. Claim 2 A method for producing a monodisperse polymer polyol according to claim 1, wherein the hydroxyl value of the polyether polyol is 50 to 60 mgKOH / g. Claim 3 A method for manufacturing a monodisperse polymer polyol according to claim 1, wherein the ethylene oxide content of the polyether polyol is 5 to 15 weight%. Claim 4 A method for preparing a monodisperse polymer polyol according to claim 1, wherein the reactive unsaturated compound is at least one selected from the group consisting of maleic acid, maleic anhydride, fumaric acid, itaconic acid, citraconic acid, citraconic anhydride, phthalic acid, phthalic anhydride, hydroxyalkyl acrylate, and methacrylate. Claim 5 A method for preparing a monodisperse polymer polyol according to claim 1, wherein the polyol described above has a hydroxyl value of 20 to 80 mgKOH / g and an ethylene oxide content of 5 to 30 wt%. Claim 6 In claim 1, the aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, divinylnaphthalene, divinylbenzene, trivinylbenzene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene A method for preparing a monodisperse polymer polyol, comprising at least one selected from the group consisting of styrene functionalized with a primary amine, styrene functionalized with a secondary amine, and styrene functionalized with a tertiary amine. Claim 7 A method for manufacturing a monodisperse polymer polyol according to claim 1, wherein the solid content of the polymer polyol is 10 to 70 weight%. Claim 8 A method for manufacturing a monodisperse polymer polyol according to claim 1, wherein the average particle size of the polymer polyol is 0.8 to 1.5 μm. Claim 9 A method for manufacturing a monodisperse polymer polyol according to claim 1, wherein the unsaturated nitrile-based compound in the polymer polyol is less than 1% by weight. Claim 10 A monodisperse polymer polyol comprising: a polyol having a hydroxyl value of 30 to 60 mgKOH / g and an ethylene oxide content of 1 to 30 wt%; and a polymer derived from an aromatic vinyl monomer dispersed in the polyol; wherein the unsaturated nitrile compound is less than 1 wt%. Claim 11 A polyurethane molded article prepared by reacting a monodisperse polymer polyol according to paragraph 10 with an isocyanate compound.
Citation Information
Patent Citations
Method for producing macromers and polymer polyols
KR1020220124732A
Stabilizer, polymer polyol prepared using same, and method for preparing the same
KR1020230032145A
Dispersion stabilizer based on at least two types of polyols and method for preparing the same
KR1020240016838A
Polymer polyol, method for producing the same and flexible urethane foam
JP2006219517A
A method for manufacturing monodispersed polymer polyols
KR101997463B1