Adhesive Composition for road safety facilities
The two-component adhesive composition for road safety facilities addresses adhesion and durability issues by using specific resins and additives, providing enhanced resistance to environmental stress and reducing accident risks.
Patent Information
- Application Number
- KR1020240160725
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-11-13
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-11-13
AI Technical Summary
Existing adhesive compositions for road safety facilities face issues with adhesion strength, durability, and resistance to harsh environmental conditions, including temperature cracks, wear, and weathering, leading to potential secondary accidents and construction difficulties.
A two-component adhesive composition comprising bisphenol A diglycidyl ether epoxy resin, CTBN epoxy resin, cellulose partial carbonized body, mercaptoalkoxysilane, carbon fiber chips, and a curing agent, along with additives like adhesion enhancers and core-shell resins, tailored for specific surface conditions to enhance adhesion, flexibility, and resistance to physical vibrations.
The composition exhibits excellent adhesion strength, temperature crack resistance, wear resistance, and weather resistance, ensuring durability and reducing the risk of secondary accidents even in harsh environments.
Smart Images

Figure 112024124649141-PAT00001
Abstract
Description
Technology Field
[0001] The present invention relates to an adhesive composition for road safety facilities, and more specifically, to an adhesive composition for road safety facilities that has excellent adhesion strength and temperature crack resistance, and excellent weather resistance and wear resistance even in harsh environments. Background Technology
[0003] There are traffic safety facilities attached to roads and other surfaces in traffic environments where vehicles move. A representative example is the road marker, which is a facility installed on the road surface used to guide drivers' attention and promote traffic safety during nighttime or inclement weather. The road marker may be installed on road center lines, lane boundaries, dedicated lanes, road obstacles, safety zones, etc.
[0004] Methods for attaching traffic safety facilities, such as road markers, to the surface of asphalt or concrete paved roads are broadly classified into methods using anchor-type structures or methods using heat-fusion adhesives.
[0005] The anchor-type attachment method is a method in which attachment strength is achieved by inserting and tightening bolts between traffic safety facilities and the road surface. However, there are issues such as the long construction process, the occurrence of potholes due to water infiltration caused by perforation of the road pavement, early loss of bonding strength due to repeated traffic loads, and the risk of secondary traffic accidents caused by bolts being pulled out.
[0006] In addition, the method of using heat-fusion adhesives involves the development of bond strength through mechanical bonding, which requires high-temperature construction of 200°C or higher, making construction difficult and causing problems such as deterioration damage to asphalt pavement materials and maintaining a completely dry state of the bonding surface.
[0007] To resolve this problem, Korean registered patent No. 10-2191001 proposed an adhesive composition based on a rubber-modified and silane-treated epoxy resin and utilizing glass fiber fragments to enhance adhesion.
[0008] However, the aforementioned prior patent also had the disadvantage that it could not guarantee reliability under harsh environments and its durability was significantly reduced due to physical vibrations such as wind.
[0009] Therefore, there is a demand for adhesive compositions that possess excellent durability, flexibility, and chemical resistance, including not only adhesion strength and thermal crack resistance but also wear resistance and weather resistance. Prior art literature
[0011] Republic of Korea Registered Patent No. 10-1260500 Republic of Korea Registered Patent No. 10-1568970 Republic of Korea Registered Patent No. 10-2191001 The problem to be solved
[0012] Accordingly, the objective of the present invention is to provide an adhesive composition for road safety facilities that has excellent adhesion strength and temperature crack resistance, and excellent weather resistance and wear resistance even in harsh environments. means of solving the problem
[0014] The adhesive composition for road safety facilities according to the present invention for achieving the above-mentioned purpose is a two-component adhesive composition comprising a main component and a curing agent, wherein the main component comprises 100 parts by weight of bisphenol A diglycidyl ether epoxy resin; 80 to 100 parts by weight of CTBN (Carboxylic Terminated Butadiene Acrylonitrile) epoxy resin; 10 to 30 parts by weight of a cellulose partial carbonized body surface-treated with 2-ethylhexyl acrylate; 10 to 30 parts by weight of mercaptoalkoxysilane; and 10 to 30 parts by weight of carbon fiber chip powder.
[0015] The above subject further comprises 1 to 10 parts by weight of an adhesion enhancer, wherein the adhesion enhancer is characterized as being one or more of naphthalic anhydride, phosphoric anhydride, maleic anhydride, phthalic anhydride, acetic anhydride, itaconic anhydride, chlorendic anhydride, boric anhydride, and trimellitic anhydride.
[0016] The above subject is characterized by further including 1 to 10 parts by weight of epoxidized silane.
[0017] The above subject further comprises 10 to 30 parts by weight of a core-shell resin, wherein the core-shell resin is characterized in that elastic rubber particles exist as a core, and a hard acrylic resin surrounds the surface of the rubber particles to form a shell.
[0018] The above curing agent is an amine-based curing agent, characterized by applying an aliphatic amine when the surface condition of the object to be attached is dry, and a ketimine compound when the surface condition is wet.
[0019] The above curing agent is characterized by further including 1 to 10 parts by weight of Hastelloy per 100 parts by weight of the above amine-based curing agent. Effects of the invention
[0021] According to the adhesive composition for road safety facilities of the present invention, not only adhesive strength and resistance to temperature cracking, but also durability such as wear resistance and weather resistance, flexibility, and chemical resistance are excellent, and durability against physical vibrations such as wind is also excellent, so there is an advantage of excellent reliability even under harsh environments. In addition, when using the adhesive composition according to the present invention for on-site construction, the possibility of causing secondary accidents that may occur when the bonding force of bolts fastened to a base material sensitive to temperature changes loosens due to repeated external loads can be reduced. Specific details for implementing the invention
[0023] The present invention will be described in detail below.
[0024] The adhesive composition according to the present invention is used in road safety facilities such as road markers.
[0025] The above adhesive composition is a two-component type consisting of a main component and a curing agent. By using bisphenol A diglycidyl ether epoxy resin and CTBN epoxy resin together as the main resin of the main component, not only is adhesion and durability improved, but elasticity and flexibility are also secured to increase durability, and other additives are used to significantly improve wear resistance, strength, chemical resistance, and durability.
[0026] In addition, depending on the condition of the attachment surface (wet, dry, or temperature conditions), different curing agents are selectively used or their mixing ratios are varied, and the adhesion is further enhanced through functional additives.
[0028] The subject of the present invention is described.
[0029] The above subject comprises 100 parts by weight of bisphenol A diglycidyl ether epoxy resin; 80 to 100 parts by weight of CTBN epoxy resin; 10 to 30 parts by weight of a cellulose partial carbonized body surface-treated with 2-ethylhexyl acrylate; 10 to 30 parts by weight of mercaptoalkoxysilane; and 10 to 30 parts by weight of carbon fiber chip powder.
[0031] The above-mentioned bisphenol A diglycidyl ether epoxy resin not only has excellent adhesion and strength, but also excellent durability and weather resistance as it is hardly affected by the external environment. This bisphenol A diglycidyl ether epoxy resin generally refers to an epoxy prepolymer having the structure of Chemical Formula 1 below.
[0032] [Chemical Formula 1]
[0033]
[0034] In the above [Chemical Formula 1], n is a positive number in the range of 1 to 25, and the softening point of the epoxy is determined according to the size of n.
[0035] The epoxy prepolymer that can be used as the above bisphenol A diglycidyl ether epoxy resin may be any epoxy commonly used in the relevant technical field without any special restrictions. For example, the above bisphenol A diglycidyl ether epoxy resin may be E-20 (601) from Henkel Japan or YD-128 from Kookdo Chemical Co., Ltd., having an equivalent weight of 180 to 220 (g / eq) and a viscosity of 8,000 to 15,000 (cps, at 25℃). Hereinafter, 'parts by weight' in the main text is based on 100 parts by weight of the above bisphenol A diglycidyl ether epoxy resin.
[0037] In addition, the above CTBN (Carboxylic Terminated Butadiene Acrylonitrile) epoxy resin is produced by adding carboxylterminated butadiene acrylonitrile rubber to a trifunctional aliphatic epoxy resin, thereby improving elasticity, adhesion, impact resistance, etc., which are lacking in bisphenol A diglycidyl ether epoxy resin. Specific examples of the above CTBN epoxy resin include KR-818, KR-450, KR-207, KR-170, KR104, and KR-100 sold by Kookdo Chemical Co., Ltd.
[0038] It is preferable that the above CTBN epoxy resin be included in the main component in an amount of 80 to 100 parts by weight, because if the content is less than 80 parts by weight, the effect of improving impact strength and adhesive strength is negligible, and if it exceeds 100 parts by weight, the overall physical properties are degraded.
[0040] The cellulose partial carbonized body surface-treated with the above-mentioned 2-ethylhexyl acrylate removes the non-cellulose portion within the cellulose particles to enhance physical properties, while particularly increasing flexibility to improve the durability, weather resistance, and temperature crack resistance of the composition, and prevents a decrease in adhesive strength through surface treatment. Specifically, this partial carbonization method involves carbonizing the cellulose particles at a temperature of 200 to 500°C for 30 to 180 minutes. Through this carbonization, only the moisture and low molecular weight portions within the cellulose particles are removed, thereby condensing the high molecular weight components with superior physical properties into a stronger structure. At this time, it is preferable to perform the carbonization in a vacuum atmosphere (approximately 3 to 100 torr). Then, the carbonized material is ground to 150 to 200 mesh.
[0041] In addition, after partial carbonization in the manner described above, it is more preferable to mix 2-ethylhexyl acrylate (2-EHA) with the partially carbonized material in a weight ratio of 1:1 to 2 and mill at a speed of 300 to 3,000 rpm so that the partially carbonized material and 2-ethylhexyl acrylate are finely bonded. It is sufficient for the particle size of the partially carbonized material to be approximately 150 to 300 mesh.
[0042] At this time, it is preferable to include 10 to 30 parts by weight of the cellulose partial carbonized body surface-treated with the above 2-ethylhexyl acrylate, because if the amount used is too small, the effect is negligible, and if it is excessive, the adhesive strength may decrease.
[0044] The above mercaptoalkoxysilane significantly improves the adhesive strength of the composition, and as a specific example, 3-mercaptopropyltrimethoxysilane can be used.
[0045] The above mercaptoalkoxysilane is included in the main component in an amount of 10 to 30 parts by weight, because if the content is less than 10 parts by weight, the effect is negligible, and if it exceeds 30 parts by weight, it becomes an excess amount, which lowers the overall physical properties.
[0047] The above carbon fiber chips improve physical properties such as overall strength, wear resistance, weather resistance, and durability. However, using carbon fibers alone has the disadvantage that their adhesion is reduced. Therefore, in the present invention, it is preferable to use carbon fibers that have been plasma treated, treated with mercaptoalkoxysilane, dried, and then ground to a size of 0.1 to 100 μm. More specifically, it is preferable to inject air, oxygen, nitrogen, or a combined gas thereof into the carbon fibers at a rate of 1 to 20 cc / min, apply a voltage of 50 to 100 W to plasma treat the carbon fibers for 0.1 to 5 minutes, immerse and stir the carbon fibers in 2 to 3 times their volume of a mercaptoalkoxysilane coating solution at a temperature of about 20 to 30°C for 1 to 10 minutes, dry the carbon fibers, and then grind them to a size of 0.1 to 100 μm. At this time, it is sufficient to use a mercaptoalkoxysilane coating solution with a concentration of 1 to 50 wt% for the coating, and distilled water or the like may be used as the solvent.
[0048] The above carbon fiber chips are included in the main component in an amount of 1 to 10 parts by weight. This is because if the content is less than 1 part by weight, the effect is negligible, and if it exceeds 10 parts by weight, it becomes an excess amount, which degrades the overall physical properties.
[0050] In addition, the curing agent according to the present invention is an amine-based curing agent generally used in the field, and its type is not specifically limited. For example, amines containing active hydrogen, such as aliphatic amines like diethyltriamine, triethyltetramine, and polyoxypropylenediamine; cyclic amines; ketamines produced by the condensation reaction of amines and ketones; modified resins such as polyamineamides, polyamidoamines, phenol-modified amines, and epoxy-added amines using these amines; or the product of the condensation reaction of a polyamine and a dimer fatty acid may be used as a curing agent. Hereinafter, 'parts by weight' in the curing agent is based on 100 parts by weight of the above amine-based curing agent.
[0051] More specifically, in the present invention, the curing agent may be used differently depending on the surface condition (wet or dry) of the object to be attached at the site. When the object is in a dry state, it is most preferable to use an aliphatic amine such as diethyltriamine, triethyltetramine, or polyoxypropylenediamine, considering the adhesive strength. In addition, when the surface of the object to be attached at the site is moist, it is most preferable to use a blocked amine-based curing agent, i.e., a ketimine compound. This is because the ketimine compound dissociates into a ketone and an amine upon contact with moisture, and the dissociated amine acts as a curing agent. At this time, the type of ketimine compound is not limited, and for example, commercially available EH-235RSA of Asahi Denka can be used.
[0053] In the present invention, it is preferable that the main component and the hardener be mixed and used in a weight ratio of 10:1 to 5, because if the content falls outside the above range, it is difficult to achieve sufficient adhesion and strength. At this time, it is obvious that a small amount of water may be added as needed, that is, in the case of a wet surface. Furthermore, it is preferable to slightly increase the amount of hardener within the above weight ratio when the surface temperature of the object to be attached at the site is low, and to slightly decrease the amount of hardener within the above weight ratio when the surface temperature is high; this is determined by adjusting within the above range according to the site conditions.
[0054] In addition, the adhesive composition of the present invention is mixed at room temperature and applied to a thickness of about 300 to 1000 μm, then installed and compressed by installing a road safety facility, and can be used by curing at room temperature for 30 minutes to 10 hours, so the implementation is not limited.
[0056] As previously explained, the adhesive composition of the present invention configured as described above has the advantage of excellent reliability even in harsh environments, as it exhibits not only adhesive strength and resistance to temperature cracking but also excellent durability and flexibility, such as wear resistance and weather resistance, as well as excellent durability against physical vibrations such as wind.
[0058] Meanwhile, in the present invention, it is preferable that the subject further includes an adhesion enhancer. The adhesion enhancer is an additive that significantly improves adhesion, and one or more of naphthalic anhydride, phosphoric anhydride, maleic anhydride, phthalic anhydride, acetic anhydride, itaconic anhydride, chlorendic anhydride, boric anhydride, and trimellitic anhydride may be used.
[0059] It is preferable that the above adhesive strength enhancer be included in the main component in an amount of 1 to 10 parts by weight, because if the content is less than 1 part by weight, the effect is negligible, and if it exceeds 10 parts by weight, it becomes an excess amount, which may actually lower the overall physical properties.
[0061] In addition, it is desirable that the above subject further includes an epoxidized silane.
[0062] The above-mentioned epoxidized silane not only shortens the curing time but also increases adhesion and resistance to temperature cracking. As for such epoxidized silanes, one or more of β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxypropylmethyltriethoxysilane, 3-glycidyloxypropyltriethoxysilane (GLYEO), and 3-glycidyloxypropyltrimethoxysilane (GLYMO) may be used.
[0063] It is preferable that the above-mentioned epoxidized silane be included in the main component in an amount of 1 to 10 parts by weight, because if the content is less than 1 part by weight, the effect is negligible, and if it exceeds 10 parts by weight, it becomes an excess amount, which may actually lower the overall physical properties.
[0065] It is desirable that the above subject further includes a core-shell resin.
[0066] The core-shell resin described above is composed of an elastic core polymer and a hard shell polymer; that is, it is a resin that forms a core-shell structure in which elastic rubber particles exist as a core and a hard acrylic resin surrounds the surface of the rubber particles to form a shell. More specifically, butadiene rubber particles or styrene-butadiene rubber particles may be used as the core material, and polymethyl methacrylate (PMMA) or acrylonitrile (AN) may be used as the shell material. The core-shell resin is expected to have the effect of reinforcing impact strength while the rubber core absorbs the impact upon external impact. In other words, this can improve resistance to temperature cracking as well as weather resistance in harsh environments.
[0067] It is preferable that the above core-shell resin be included in the main component in an amount of 10 to 30 parts by weight, because if the content is less than 10 parts by weight, the effect is negligible, and if it is in excess, there may be a problem of relatively reduced shear adhesion.
[0069] In addition, the curing agent is characterized by further including 1 to 10 parts by weight of Hastelloy.
[0070] The above Hastelloy is an alloy in which 10 to 35 weight percent of molybdenum is mixed with nickel, and it functions to significantly improve physical properties such as strength, wear resistance, corrosion resistance, chemical resistance, durability, and heat resistance.
[0071] This Hastelloy is included in the curing agent in an amount of 1 to 10 parts by weight, because if the content is too low, the effect is negligible, and if it is excessive, the adhesion is reduced.
[0073] The present invention will be explained more specifically below through examples, comparative examples, and experimental examples. These examples, comparative examples, and experimental examples are intended solely to illustrate the present invention, and it is obvious to those skilled in the art that the scope of the present invention is not limited thereto.
[0075] (Examples and Comparative Examples)
[0076] The compositions of the examples and comparative examples were prepared with the mixing ratios shown in Table 1 below.
[0077] Mixing ratio (g) of examples and comparative examples division Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 subject Bisphenol A diglycidyl ether epoxy resin 100 100 100 100 200 - CTBN epoxy resin 100 100 100 100 - 200 Cellulose partial carbonized material surface-treated with 2-ethylhexyl acrylate 20 20 20 20 20 20 Mercaptoalkoxysilane 20 20 20 20 20 20 carbon fiber chips 20 20 20 20 20 20 Adhesion enhancer - 5 5 6 - - Epoxide silane - 5 5 5 - - Core-shell resin - - 20 20 - - hardener Amine-based curing agent 100 100 100 100 100 100 Hastelloy (7㎛) - - - 5 - -
[0078] YD-128 from Kookdo Chemical Co., Ltd. was used as the bisphenol A diglycidyl ether epoxy resin, KR-450 from Kookdo Chemical Co., Ltd. was used as the CTBN epoxy resin, 3-mercaptopropyl trimethoxysilane was used as the mercaptoalkoxysilane, phosphoric anhydride was used as the adhesion enhancer, γ-glycidoxypropyltrimethoxysilane was used as the epoxidized silane, and a resin in which the surface of butadiene rubber particles is surrounded by acrylonitrile resin was used as the core-shell resin. In addition, triethyltetramine was used as the amine-based curing agent.
[0079] Then, for the cellulose partial carbonized body, 10 kg of cellulose particles with a size of 0.1 to 1 mm and a moisture content of 11.3% were prepared, placed in a stainless steel container and sealed, and partially carbonized at a temperature of 500°C for 2 hours under a vacuum of 50 torr. Subsequently, 2-ethylhexyl acrylate was mixed with the partial carbonized body in a weight ratio of 1:2, and ceramic balls with diameters of 50 mm, 30 mm, and 20 mm were added to the mixture and milled at a speed of 500 rpm for 24 hours. The particle size of the partial carbonized body was 150 to 200 mesh.
[0080] The above carbon fiber chip was prepared by injecting air into the carbon fiber at a rate of 1 to 20 cc / min, applying a voltage of 60 W and plasma treating it for 3 minutes, then immersing and stirring it in 3 times the volume of a 3-mercaptopropyl trimethoxysilane coating solution (20 wt% 3-mercaptopropyl trimethoxysilane, 80 wt% distilled water) at a temperature of 25°C for 10 minutes, drying it at 40°C, and grinding it to 0.1 to 100 μm.
[0082] (Test Example 1)
[0083] A Dolly Test was performed to evaluate the adhesion performance of the composition according to the present invention. Specifically, the main component and the hardener were mixed in a weight ratio of 10:2, coated onto the surface of a test specimen, and the maximum adhesion strength with the test specimen was measured using a Dolly. The results are shown in Table 2 below. At this time, the thickness of the coating film was set to 500 μm.
[0085] Adhesion performance test results (Mpa.s) division marble surface concrete surface Example 1 46.5 28.5 Example 2 49.5 30.1 Example 3 51.2 32.3 Example 4 50.3 31.8 Comparative Example 1 30.1 20.4 Comparative Example 2 32.5 22.5
[0086] As shown in Table 2 above, it was confirmed that Examples 1 to 4 of the present invention had superior adhesion strength compared to Comparative Examples 1 and 2.
[0088] (Test Example 2)
[0089] The shear strength of the composition according to the present invention was evaluated. At this time, the shear strength evaluation was classified into dry specimens and water-immersed specimens, and the shear strength evaluation was performed under a loading condition of a speed of 5 mm / min.
[0091] Shear strength test results (Mpa) division Asphalt concrete (dry state, 25℃) Cement concrete (dry state, 25℃) Example 1 1.31 1.38 Example 2 1.42 1.48 Example 3 1.57 1.52 Example 4 1.74 1.60 Comparative Example 1 0.98 0.74 Comparative Example 2 0.67 0.60
[0092] As shown in Table 3 above, it was confirmed that Examples 1 to 4 of the present invention have superior shear strength compared to Comparative Examples 1 and 2.
[0094] (Test Example 3)
[0095] The shear adhesive strength of the composition according to the present invention was measured, and high temperature adhesive strength, water-resistant adhesive strength, aging-resistant adhesive strength, and heat cycle adhesive strength were measured (exposure to temperatures of 70~80℃ → 20~25℃ → -30~20℃ → 20~25℃ → 40~50℃ → 20~25℃ for a specified time was considered as one cycle, and performed 5 times).
[0096] In addition, impact peel strength was also measured using an impact tester at room temperature (23℃), high temperature (80℃), and low temperature (-40℃).
[0098] Shear adhesion and impact peel strength test results division Shear adhesion (Mpa) Impact peel strength (N / mm) High temperature (80℃) water resistance Antiaging Heat cycle Room temperature (23℃) High temperature (80℃) Low temperature (-40℃) Example 1 25.2 32.2 32.5 35.5 49.8 52.4 35.9 Example 2 26.5 33.8 33.9 36.7 50.2 53.7 36.8 Example 3 27.1 35.2 35.8 37.5 53.1 55.2 38.1 Example 4 26.7 33.7 33.5 36.9 54.1 56.3 38.9 Comparative Example 1 18.8 26.5 26.8 28.1 35.5 38.5 28.2 Comparative Example 2 19.5 26.9 27.9 29.3 36.5 40.2 25.1
[0099] As shown in Table 4 above, it was confirmed that Examples 1 to 4 of the present invention had superior shear adhesion and impact peel strength compared to Comparative Examples 1 and 2.
[0101] Therefore, it was determined that the adhesive composition according to the present invention has excellent quality and ease of application, and excellent reliability even under harsh environments.
[0103] From the above description, those skilled in the art will understand that various changes and modifications are possible within the scope of the technical concept of the present invention. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be determined by the claims.
Claims
Claim 1 An adhesive composition for road safety facilities comprising a two-component adhesive composition consisting of a main component and a curing agent, wherein the main component comprises: 100 parts by weight of bisphenol A diglycidyl ether epoxy resin; 80 to 100 parts by weight of CTBN (Carboxylic Terminated Butadiene Acrylonitrile) epoxy resin; 10 to 30 parts by weight of a cellulose partial carbonized body surface-treated with 2-ethylhexyl acrylate; 10 to 30 parts by weight of mercapto alkoxysilane; and 10 to 30 parts by weight of carbon fiber chip powder. Claim 2 An adhesive composition for road safety facilities according to claim 1, wherein the subject further comprises 1 to 10 parts by weight of an adhesion enhancer, and the adhesion enhancer is one or more of naphthalic anhydride, phosphoric anhydride, maleic anhydride, phthalic anhydride, acetic anhydride, itaconic anhydride, chlorendic anhydride, boric anhydride, and trimellitic anhydride. Claim 3 An adhesive composition for road safety facilities according to claim 1, characterized in that the subject further comprises 1 to 10 parts by weight of epoxidized silane. Claim 4 An adhesive composition for road safety facilities according to claim 1, wherein the subject further comprises 10 to 30 parts by weight of a core-shell resin, wherein the core-shell resin is characterized in that elastic rubber particles exist as a core and a hard acrylic resin surrounds the surface of the rubber particles to form a shell. Claim 5 An adhesive composition for road safety facilities according to any one of claims 1 to 4, wherein the curing agent is an amine-based curing agent, wherein an aliphatic amine is applied when the surface condition of the object to be attached is dry, and a ketimine compound is applied when the surface condition is wet. Claim 6 An adhesive composition for road safety facilities according to claim 5, characterized in that the curing agent further comprises 1 to 10 parts by weight of Hastelloy per 100 parts by weight of the amine-based curing agent.
Citation Information
Patent Citations
Resin composition and adhesive containing the same
JP2014012778A
Curable compositions containing adhesion promoters
JP2021524517A
Method of manufacturing Polyurethane paints comprising carbonized microfiber-reinforced, Method for manufacturing Polyurethane coating steel pipe using the same and Polyurethane coating steel pipe by the same
KR101811372B1
Polyurethane adhesive composition in improving bonding strength for nylon shoe material
KR1020120118657A
Epoxy structural adhesive resistant to moisture exposure during both uncured and cured periods
KR1020240155849A