Hybrid battery electrode composite comprising transition metal oxide nanoclusters and reduced graphene oxide, and hybrid battery comprising the same
A hybrid electrode composite of reduced graphene oxide and transition metal oxide nanoclusters addresses lithium-ion battery degradation by enhancing lithium ion and pseudocapacitor reactions, achieving high capacity and long-term stability.
Patent Information
- Application Number
- KR1020250091413
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-07-08
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-07-08
AI Technical Summary
Lithium-ion batteries experience rapid output degradation and lifespan reduction under high-speed charging and discharging due to diffusion resistance and reduced interfacial reactions, and conventional pseudocapacitor electrodes suffer from limited electrochemical reactivity and structural instability.
A hybrid electrode composite comprising reduced graphene oxide sheets and transition metal oxide nanoclusters, where the graphene oxide sheet facilitates lithium ion insertion and extraction reactions, and the nanoclusters enable pseudocapacitor reactions, with optimized electron and ion transport pathways.
The composite achieves high capacity, fast reaction rates, and excellent cycle life by simultaneously utilizing lithium ion insertion-extraction and pseudocapacitor reactions, maintaining over 80% of initial capacity after 500 charge-discharge cycles and supporting high-speed charge-discharge characteristics.
Smart Images

Figure 112025076744302-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an electrode composite for a hybrid battery comprising a transition metal oxide nanocluster and reduced graphene oxide, and a hybrid battery comprising the same. Background Technology
[0002] Lithium-ion batteries are widely used in various energy storage devices due to their high energy density and long lifespan. However, under high-speed charging and discharging conditions, output performance decreases rapidly due to factors such as diffusion resistance and reduced interfacial reaction, leading to problems with reduced battery efficiency and lifespan.
[0003] As one approach to solving these problems, pseudocapacitor electrode materials based on transition metal oxides are attracting attention. Pseudocapacitors offer the advantage of providing higher specific capacitance and output characteristics than electric double layer capacitors, while minimizing diffusion delay through rapid surface reactions. In particular, transition metal oxides can exhibit high charge storage capacity through reversible oxidation-reduction reactions.
[0004] However, conventional pseudocapacitor electrodes are often composed of a single oxide structure, which limits electrochemical reactivity and reduces structural stability, making it difficult to ensure a long lifespan. Additionally, oxides synthesized in the form of nanoparticles suffer from reduced effective reaction surface area due to aggregation or non-uniform contact with the electrolyte.
[0005] Accordingly, there is a growing need for composite structures based on porous transition metal oxide nanoclusters combined with conductive supports capable of insertion-extraction reactions. These composite structures can simultaneously realize lithium-ion-based insertion reactions and metal oxide-based pseudocapacitor reactions, making them a focus of attention as next-generation energy storage materials capable of satisfying high capacity, high power, and long lifespan characteristics. Prior art literature
[0006] Republic of Korea Registered Patent No. 10-2177266 (2020.11.04.) The problem to be solved
[0007] The present invention aims to solve the problems of output degradation and lifespan reduction in existing lithium secondary batteries by providing a hybrid electrode structure capable of utilizing both the insertion-extraction reaction of lithium ions and the oxidation-reduction reaction of transition metal ions.
[0008] In addition, the present invention aims to provide an electrode composite that enables a pseudocapacitor reaction to be effectively implemented by preventing the aggregation of transition metal oxide nanoparticles and optimizing the transport pathways of electrons and ions. means of solving the problem
[0009] To solve the above-mentioned problem, the present invention provides an electrode composite for a hybrid battery capable of storing electrochemical energy by simultaneously utilizing the insertion and extraction reaction of lithium ions (lithium secondary battery reaction) and the oxidation and reduction reaction of transition metal ions (pseudocapacitor reaction).
[0010] The electrode composite for a hybrid battery according to the present invention is composed of a structure including a reduced graphene oxide sheet and a transition metal oxide nanocluster. The reduced graphene oxide sheet functions as an electrochemically active component that performs lithium ion insertion and extraction reactions at an interlayer structure or defect site, and can provide an electron transport path at the interface with the transition metal oxide nanocluster. In addition, the reduced graphene oxide sheet may be configured such that the current attributable to pseudocapacitor reactions accounts for 50% or more of the current generated during the electrochemical charging and discharging process.
[0011] The transition metal oxide nanoclusters included in the electrode composite are structures formed by the aggregation of multiple transition metal oxide nanocrystals, and grain boundaries may be formed at the contact surfaces between the nanocrystals. The size of the transition metal oxide nanocrystals may be limited to a range of 1 nm or more and 10 nm or less, and the grain boundaries may occupy 50% or more of the total surface area. The electrode composite for the hybrid battery may be formed of spherical particles having a hollow structure with an average particle size of 400 nm to 1,000 nm.
[0012] The above transition metal oxide nanocluster can be formed into a shell structure including a hollow, and the thickness of the shell can be set to a range of 20 nm or more and 40 nm or less, and the size of the entire nanocluster can be set to a range of 1 nm or more and 100 nm or less.
[0013] The present invention also provides a hybrid secondary battery comprising an electrode composite for a hybrid battery as described above, wherein the hybrid secondary battery has a current density of 100 mA g during charging and discharging. -1 1,500mAh g under conditions -1 The above cost amount can be represented. Effects of the invention
[0014] The electrode composite for a hybrid battery according to the present invention performs a lithium ion insertion-extraction reaction (lithium secondary battery reaction) through a reduced graphene oxide sheet and induces a pseudocapacitor reaction by utilizing the grain boundaries and amorphous regions of transition metal oxide nanoclusters, thereby providing the advantage of simultaneously securing a high capacity, a fast reaction rate, and an excellent cycle life.
[0015] In particular, the composite according to the present invention is 100 mA g -1 1,500 mAh g at a current density -1 It exhibits the above capacity and can secure long-term stability by maintaining more than 80% of the initial capacity even after more than 500 charge-discharge cycles. Brief explanation of the drawing
[0016] FIG. 1 is a schematic diagram of an electrostatic interaction-based layer-by-layer self-assembly (LBL) method for manufacturing an example. Figure 2 shows the X-ray diffraction (PXRD) patterns of the comparative example and the example. Figure 3 is the FTIR spectrum of the comparative example and the example. Figure 4 shows the thermogravimetric analysis (TGA) results of the example. Figure 5 is the XANES spectrum for the Ni and Fe K-edge. Figure 6 is the XANES linear combination fitting (LCF) result of the example. Figure 7 shows the k for the Fe and Ni K-edges. 3 This is the weighted EXAFS spectrum. Figure 8 is the Fourier transform (FT) spectrum for the Fe and Ni K-edges. Figure 9 shows the wavelet transform (WT) analysis results for Ni and Fe K-edges. Figure 10 is a Scanning Electron Microscope (SEM) image of a PS bead template. Figure 11 is an SEM image of a hollow formed by a reduced graphene sheet. Figure 12 is a TEM (Transmission Electron Microscope) image of an example. Figure 13 shows the HRTEM (High Resolution Transmission Electron Microscope) image, FFT (Fast Fourier Transform), and inverse transform image of the embodiment. Figure 14 shows the HRTEM image, FFT and inverse transform image of the example and the analysis results of crystalline NiO particles observed at local locations. FIG. 15 is a graph showing the discharge capacity and Coulomb efficiency of the example and comparative example measured at various current densities, and a schematic diagram showing the process of the example forming a stable SEI in the initial cycle. Figure 16 is a graph comparing the charge-discharge curves and long-term charge-discharge performance of the example and comparative example. Figure 17 shows the results of comparing high-speed reaction rates by calculating the Peukert constant. Figure 18 shows the results of measuring the long-term charge / discharge performance and SOC attainment time according to the C-rate of the example. FIG. 19 shows (a) the initial 15-cycle cyclic voltammetry (CV) curve of the example, (b) the CV curve under various scan rate conditions in the range of 0.1–0.8 mV / s, (c) the CV curve measured under the same conditions after 100 cycles, and (d) the Cottrell plot (i(V) / v 1 / 2 vs v 1 / 2 This shows the analysis of diffusion dominance / pseudocapacitor contribution through ). Figure 20 shows the results of quantitative separation of the diffusion-controlled / pseudocapacitor-controlled reaction in the example. Figure 21 shows the results of measuring the pseudocapacitor contribution rate among the capacitances of the examples and comparative examples. FIG. 22 is a schematic diagram illustrating that the polycrystalline interface structure formed by the phase transition of NiFe-LDH into transition metal oxide nanoclusters contributes to the enhanced pseudocapacitor behavior. Figure 23 shows the results of Electrochemical Impedance Spectroscopy (EIS) measurements of the examples and comparative examples as a Nyquist plot. Figure 24 shows the results of the Distribution of Relaxation Time (DRT) analysis of the examples and comparative examples. Figure 25 shows the results of extracting the resistance configurations of the example and comparative example based on an equivalent circuit model. Figure 26 shows the results of comparing the Warburg coefficients of the example and the comparative example. Figure 27 shows the results of comparing the Warburg coefficients of the example and the comparative example. FIG. 28 is a schematic diagram explaining (d) the degradation mechanism and structural stability of the electrode during charging and discharging, and (e) a schematic diagram showing the difference in lithium diffusion rate according to the structural difference between the example and the comparative example. Specific details for implementing the invention
[0017] The following describes in detail an electrode composite for a hybrid battery comprising transition metal oxide nanoclusters and reduced graphene oxide according to the present invention, and a hybrid battery comprising the same. The drawings presented below are provided as examples to ensure that the concept of the present invention is sufficiently conveyed to those skilled in the art. Accordingly, the present invention is not limited to the drawings presented below and may be embodied in other forms, and the drawings presented below may be exaggerated to clarify the concept of the present invention. In this case, unless otherwise defined, technical and scientific terms used in the present invention have the meaning commonly understood by those skilled in the art to which this invention pertains, and descriptions of known functions and configurations that could unnecessarily obscure the essence of the present invention are omitted in the following description and attached drawings.
[0018] The present invention provides an electrode composite for a hybrid battery characterized by comprising transition metal oxide nanoclusters dispersed on a reduced graphene oxide sheet.
[0019] The electrode composite for the hybrid battery described above may store electrochemical energy through the insertion-extraction reaction of lithium ions (lithium secondary battery reaction) and the oxidation-reduction reaction of transition metal ions (pseudocapacitor reaction).
[0020] More specifically, the reduced graphene oxide sheet and the transition metal oxide nanocluster are subcomponents with different structural characteristics, and the transition metal oxide nanocluster is continuously formed on the outer edge of the sheet, and can form a single secondary particle structure by closely bonding them along the interface.
[0021] The above-mentioned reduced graphene oxide sheet may be composed of a multilayer carbon structure (rGO-HS) having a hollow structure and may function as an electrochemically active component that performs lithium ion insertion and extraction reactions. The above-mentioned reduced graphene oxide sheet has a multilayer structure, and more specifically, may be formed in an irregularly stacked turbostratic form.
[0022] The interlayer spacing of the above-described reduced graphene oxide sheet can be distributed in a range of 0.33 nm to 0.56 nm. This is a structural requirement to secure a sufficient diffusion path for lithium ions to be inserted between the graphene layers. If the interlayer spacing of the above-described reduced graphene oxide sheet is less than 0.33 nm, it is difficult for lithium ions to be effectively inserted between the layers, which may lead to a decrease in the reactivity of the insertion reaction; conversely, if it exceeds 0.56 nm, the layer structure may become excessively relaxed, potentially causing a decrease in conductivity and structural stability issues. More preferably, the interlayer spacing of the above-described reduced graphene oxide sheet is 0.35 nm to 0.50 nm, and even more preferably 0.40 nm to 0.45 nm.
[0023] At that time, the number of stacked reduced graphene oxide sheets in the electrode composite for the hybrid battery may be limited to 10 layers or less. This is because as the number of stacked layers increases, the effective area for inserting lithium ions decreases, and ion diffusion into the inner layers may be inhibited. A multilayer structure of 10 layers or less provides a physical distance that allows lithium ions to efficiently pass between each layer, while simultaneously suppressing sheet aggregation phenomena, which is advantageous for maintaining surface reactivity. The above limitation corresponds to a structural condition for maximizing the ion diffusivity and electrochemical active area of the multilayer reduced graphene oxide sheets.
[0024] Meanwhile, the reduced graphene oxide sheet has a structure in which a plurality of graphene layers are stacked, and the interlayer spacing refers to a local gap between two adjacent graphene layers and is a concept distinct from the total stacking thickness determined by the number of layers in the entire sheet. For example, if the interlayer spacing is maintained at an average level of about 0.42 nm, the total thickness in a stacked structure of 10 layers or less can be formed in a range of about 4.10 nm to 4.30 nm. Therefore, the limitation of the range for the interlayer spacing and the number of layers can be understood as a physical condition for achieving a balance of reactivity of the intercalation reaction, securing an electron conduction path, and structural stability.
[0025] The above-mentioned reduced graphene oxide sheet undergoes a deoxygenation reaction during the high-temperature heat treatment of graphene oxide, and various defect structures may be generated during this process. The defects formed within the reduced graphene oxide sheet are sp² resulting from the removal of oxygen groups. 3 These defects may consist of bond breakage, atomic defects within the lattice, pore formation, and exposure of edge regions, and these defects can reduce local electron density within the reduced graphene oxide sheet, thereby forming highly reactive active sites favorable for lithium ion adsorption or reaction.
[0026] Defects may be generated in the aforementioned reduced graphene oxide sheet during the thermal reduction process. Defects within the reduced graphene oxide sheet can be attributed to bond breakage, pore formation, or oxygen removal, which may result in the formation of highly reactive regions with low electron density. These defects within the reduced graphene oxide sheet can act as active sites capable of inducing localized adsorption or surface reactions of lithium ions. Therefore, the reduced graphene oxide sheet can function as an electrochemical active material capable of substantially contributing to lithium ion-based electrochemical storage reactions, going beyond a simple conductive support.
[0027] The reduced graphene oxide sheet can form a structure that adheres closely to the interface with the transition metal oxide nanocluster, and the interface can be stably maintained by physical adsorption and partial chemical bonding. The reduced graphene oxide sheet is a conductive carbon material having a continuous π-bond electron structure and can function as an electron flow path that transmits electrons generated from the transition metal oxide nanocluster to an external circuit.
[0028] An electron density imbalance may be formed at the contact interface between the reduced graphene oxide sheet and the transition metal oxide nanocluster, thereby inducing electron transfer from the transition metal oxide nanocluster to the reduced graphene oxide sheet. This electron transfer can be realized through a path extending from the interface along the reduced graphene oxide sheet to the external current collector, which can contribute to minimizing electron conduction losses within the electrode and improving the responsiveness of the overall electrochemical reaction.
[0029] In particular, the interface may have a structure in which a multilayer carbon lattice of a reduced graphene oxide sheet locally contacts a structure in which multiple transition metal oxide nanocrystals are aggregated; this complex contact structure can serve as an integrated reaction platform capable of simultaneously providing surface diffusion pathways for both electrons and lithium ions. Accordingly, the interface structure goes beyond simple structural bonding and becomes a key element that can contribute to improving the electrochemical reactivity and output characteristics of electrode composites for hybrid batteries.
[0030] Furthermore, the reduced graphene oxide sheet can make a certain level of auxiliary contribution to the pseudocapacitor reaction. For example, in cyclic voltammetry (CV) using the reduced graphene oxide sheet as a working electrode, the current ratio attributable to the pseudocapacitor reaction depending on the scan rate can be expressed as follows: 0.1 mV s⁻¹ -1 At 52% or more and 54% or less, 0.2 mV s -1 At 57% or more and 60% or less, 0.4 mV s -1 At 62% or more and 65% or less, 0.6 mV s -1 At 66% or more and 69% or less, 0.8 mV s -1 73% or more and 75% or less. This suggests that defects or edge structures within the reduced graphene oxide sheet act as active sites that can contribute to electrochemical reactions, particularly pseudocapacitor activity. Meanwhile, within the entire composite, the oxidation-reduction reaction of transition metal oxide nanoclusters leads the pseudocapacitor properties, and the reduced graphene oxide sheet can function as a supporting component.
[0031] The transition metal oxide nanocluster may be a porous oxide layer continuously formed along the outer edge of a reduced graphene oxide sheet, and may be included as an electrochemically active component that performs an oxidation-reduction reaction (pseudocapacitor reaction) of transition metal ions within an electrode composite for a hybrid battery.
[0032] The above transition metal oxide nanoclusters may be composed of oxides of transition metals such as nickel (Ni), iron (Fe), cobalt (Co), and manganese (Mn), and may be formed based on a transition metal hydroxide precursor by heat treatment of said precursor. During the heat treatment process, the hydroxide undergoes dehydration and rearrangement to be converted into an oxide phase, and examples of transition metal oxides may be in the form of single or complex oxides such as a-NiO, NiFe2O4, Co3O4, and Mn3O4. Preferably, a complex oxide structure composed of a-NiO and NiFe2O4 may be formed. Such oxides can exhibit rapid surface charge storage characteristics through reversible oxidation-reduction reactions of transition metal ions.
[0033] At this time, the a-NiO and NiFe2O4 may be included in a ratio of a-NiO:NiFe2O4 of 2.5:1 or more and 3.5:1 or less based on the total weight ratio. Based on structural characteristics having a high specific surface area and grain boundary density, the transition metal oxide nanoclusters can act as active sites where surface reactions of electrons and lithium ions are concentrated. This structure can contribute to improving the reaction rate of electrochemical reactions and securing high-speed charge and discharge characteristics.
[0034] The transition metal oxide nanocluster can be formed as a structure in which a plurality of transition metal oxide nanocrystals are aggregated. The transition metal oxide nanocrystals may have a uniform size distribution, and their size may be broadly limited to a range of 3 nm to 12 nm, more preferably 4 nm to 11 nm, and even more preferably 5 nm to 10 nm. Grain boundaries may be formed between the transition metal oxide nanocrystals, and these grain boundaries may act as surface active sites where lithium ions can be selectively adsorbed or reacted. In particular, the transition metal oxide nanocluster can provide major active sites for pseudocapacitor reactions by having a high grain boundary density.
[0035] The electrode composite for the hybrid battery described above may include a reduced graphene oxide sheet having a hollow structure. The hollow structure is formed by hydrothermally reacting graphene oxide using polymer beads as a template during the manufacturing process, and then removing the polymer beads through heat treatment. The reduced graphene oxide sheet formed at this time has a shell structure composed of multilayer carbon sheets and can function as an outer shell surrounding the interior of the hollow. The electrode composite for the hybrid battery described above may be formed of spherical particles having a hollow structure with an average particle size of 400 nm to 1,000 nm.
[0036] The thickness of the shell structure can be maintained within a range of 20 nm or more and 40 nm or less, more preferably 23 nm or more and 35 nm or less, and even more preferably 25 nm or more and 32 nm or less. This thickness range is a condition for providing structural characteristics capable of withstanding mechanical stress generated during electrochemical reactions while maintaining the mechanical stability of the hollow structure. If the shell thickness is less than 20 nm, there is a risk of structural collapse or rupture, and conversely, if it exceeds 40 nm, the electron and ion diffusion resistance increases, which may lead to a decrease in the reaction rate.
[0037] Meanwhile, due to shrinkage stress and gas release occurring during the heat treatment process, localized ruptures or fine crusts or fragments may be generated on the shell surface. These fragments exist in the form of fine particles composed of aggregated transition metal oxide nanocrystals and may attach to the inner or outer walls of the hollow structure or act as independent secondary particles within the electrode. These fragments can contribute to the improvement of electrochemical reaction uniformity and reaction rate by expanding the reaction surface area and increasing the electrolyte penetration pathways.
[0038] A transition metal oxide nanocluster layer formed by heat treatment after depositing a transition metal dihydroxide precursor may exist on the outer surface of the above-mentioned reduced graphene oxide sheet. The above-mentioned transition metal oxide nanocluster is a porous oxide layer composed of α-NiO and NiFe2O4, formed by being continuously coated on the reduced graphene oxide sheet. This structure may have a size ranging from 500 nm to 700 nm in terms of outer diameter, more preferably from 550 nm to 660 nm, and even more preferably from 560 nm to 640 nm. If the outer diameter is less than 500 nm, it is difficult to secure internal space within the particle, which may limit electrolyte penetration, and if it exceeds 700 nm, dispersion stability within the electrode may be reduced.
[0039] The above transition metal oxide nanoclusters may have a porous structure containing numerous micropores internally, which can be advantageous for electrolyte penetration and increasing the reaction surface area. In addition, the composite structure of transition metal oxide nanocrystals and amorphous oxides can provide an electrochemical environment in which lithium ion diffusion and electron transfer can occur simultaneously and easily within the electrode.
[0040] Transition metal oxide nanoclusters can form a closely bonded structure at the interface with the reduced graphene oxide sheet, and said interface can provide a continuous electron transfer pathway. This interface structure facilitates the smooth flow of electrons from the external circuit to the internal active site where electrochemical reactions occur, thereby contributing to the improvement of reaction uniformity and response characteristics of the entire electrode composite.
[0041] In particular, the interface can be realized as a composite contact structure formed by the close contact of a porous layer formed by transition metal oxide nanocrystals and a reduced graphene oxide sheet with a multilayer carbon structure. Such a structure functions as an integrated reaction platform that simultaneously provides a surface diffusion pathway for lithium ions as well as electron transfer, and can effectively contribute to improving the high-speed charge / discharge characteristics and output characteristics of the electrode composite.
[0042] The electrode composite for a hybrid battery according to the present invention can be used as an electrode active material, particularly a negative electrode active material, for a lithium secondary battery by simultaneously performing the insertion and extraction reaction of lithium ions (insertion-type reaction) and the oxidation and reduction reaction of transition metal ions (pseudocapacitor reaction) through the structure described above. Furthermore, the electrode composite for a hybrid battery implements a dual electrochemical reaction mechanism, thereby improving overall reaction uniformity and enabling it to function as a hybrid battery platform that provides high capacity and excellent cycle life.
[0043] More specifically, the electrode composite for a hybrid battery according to the present invention has a current density of 100 mA g -1 1,500mAh g at the standard -1 It can exhibit a specific capacity exceeding this amount, representing a significant improvement in energy storage capability compared to conventional electrodes based on a single reaction mechanism. Furthermore, the structural flexibility based on the porous structure and hollow shell effectively responds to volume expansion and stress changes occurring during charging and discharging, maintaining approximately 1,000 mAh g even after 1,000 cycles at 1C. -1 It can maintain a capacity of over 280mAh g even at an ultra-high rate of 50C. -1 Excellent cycle life characteristics, such as exhibiting the above capacity, can be secured.
[0044] The method for manufacturing an electrode composite for a hybrid battery according to the present invention may comprise: A) a step of preparing a graphene oxide dispersion; B) a step of performing a hydrothermal reaction by adding a reducing agent to the dispersion; C) a step of forming a graphene sheet with a hollow structure; D) a step of performing a thermal reduction treatment on the hollow graphene sheet; E) a step of depositing a metal dihydroxide; F) a step of heat-treating the composite after the deposition is completed; and G) a step of recovering the composite.
[0045] In step A) above, graphene oxide (GO) powder is dispersed in deionized water to form a uniform colloidal solution. Preferably, the solution is formed at a ratio of 0.5 to 2.0 mL of deionized water per 1 mg of GO, and ultrasonic treatment is performed to induce uniform dispersion of GO. At this time, the ultrasonic treatment may be performed for 20 to 60 minutes.
[0046] If the amount of deionized water mixed in the above-mentioned colloidal solution is less than the range specified above, the degree of dispersion may increase, but the viscosity of the solution may increase, which may hinder diffusion within the solvent during subsequent hydrothermal reactions. This leads to a decrease in the uniformity of the reaction and, consequently, may have a negative impact on the structural stability and surface activity of the rGO sheet formed. Conversely, if the amount of deionized water mixed in excessively exceeds the range specified above, the average inter-particle distance of GO increases, reducing inter-particle interactions and diluting the dispersion concentration, which may lower the efficiency of the electrostatic adsorption reaction. This can lead to a decrease in alignment between graphene sheets, thinning, or asymmetric particle growth, and may cause a deterioration in the mechanical and electrical properties of the final electrode composite.
[0047] In addition, ultrasonic treatment is intended to prevent re-aggregation of GO particles and improve lamellar alignment in subsequent processes, and a certain level of dispersion is possible even if ultrasonic treatment is omitted. However, since quality variation may increase in terms of long-term storage stability and repeatability, it is recommended to perform it to improve dispersion stability and particle uniformity.
[0048] In step B) above, a reducing agent is added at a concentration of 0.025 to 0.125 mL per 1 mg of GO in the dispersed GO solution, and a hydrothermal reaction is performed at 100 to 140°C for 8 to 12 hours. In this process, GO is converted into reduced graphene oxide (rGO) through thermal reduction.
[0049] At this time, it is preferable to use an organic acid series as the reducing agent, for example, ascorbic acid, citric acid, tannic acid, and gallic acid may be used. Preferably, ascorbic acid is used because it has high reduction efficiency and low reaction by-products, which minimizes the accumulation of impurities and is advantageous for ensuring structural compatibility and electrochemical stability. However, the reducing agent is not necessarily limited to the organic acid series mentioned above, and reducing agents such as hydrazine hydrate, sodium nitrite, sodium sulfate, or ethylene glycol may also be used as needed.
[0050] In step C) above, to implement a hollow structure, polymer beads are dispersed in an organic solvent, and after adding the reduced graphene oxide dispersion in a weight ratio of 1:20 to 1:10 based on the polymer beads, a hydrothermal reaction can be performed.
[0051] The above polymer beads may be composed of polystyrene (PS), polymethyl methacrylate (PMMA), polyurethane, etc., and the organic solvent may be selected from formamide, dimethylformamide (DMF), ethanol, etc. Preferably, the polymer beads are polystyrene (PS), and in particular, it is preferable that the surface be modified with polyethyleneimine (PEI), so as to induce electrostatic self-assembly between reduced graphene oxide and the polymer beads. More specifically, reduced graphene oxide contains numerous oxygen-containing functional groups such as carboxyl groups and hydroxyl groups, and thus has the characteristic of being negatively charged in a neutral environment (pH=6~8). However, since the surface of polystyrene is hydrophobic, there is little electrostatic interaction, so direct adsorption with reduced graphene oxide does not occur easily. Therefore, when the surface of polystyrene is modified with PEI, a polymer containing a large amount of amine groups, and charged with a positive charge, electrostatic attraction occurs between the reduced graphene oxide and the polymer beads, and through this, the reduced graphene oxide can be easily bonded and stacked on the polymer beads.
[0052] The above mixture can be maintained in a sealed state in a hydrothermal reaction device at a temperature of 100°C to 140°C for 6 to 12 hours, and more preferably, by carrying out the reaction at a temperature of 110°C to 130°C for about 10 hours, uniform stacking and structural immobilization of reduced graphene oxide on the surface of polymer beads can be induced. After the hydrothermal reaction is completed, the polymer beads are removed by chemical dissolution or thermal decomposition, and a reduced graphene sheet (rGO-HS) with a hollow internal structure is obtained.
[0053] In step D) above, by heat-treating the rGO-HS obtained by the hydrothermal reaction at a temperature of 400 to 500°C for 1 to 3 hours under an argon atmosphere, the reduction of graphene oxide and simultaneous thermal decomposition of the polymer beads can be removed, and a hollow structure can be formed inside the structure while simultaneously removing residual oxygen groups, thereby improving electrical conductivity and structural stability. Preferably, heat treatment is performed at 450 to 480°C for 1 to 3 hours, at which time the polymer beads are completely removed as volatile decomposition products.
[0054] In step E) above, the rGO-HS composite can be introduced into a reaction vessel, and a transition metal nitrate aqueous solution can be added to carry out the reaction. The type of transition metal is as described above, and preferably, a nickel and iron nitrate aqueous solution can be added to carry out the reaction. Specifically, the molar ratio of transition metal ions in the transition metal nitrate aqueous solution can be set to Ni:Fe = 1:1 to 3:1, and the total metal ion concentration can be set in the range of 0.01 to 0.05 M, preferably 0.02 to 0.04 M. Subsequently, hexamethylenetetramine (HMT) is added at a concentration of 0.02 to 0.08 M, preferably 0.03 to 0.06 M, and the reaction is carried out at a temperature of 80 to 100°C for 6 to 12 hours, thereby inducing the uniform deposition of nickel-iron dihydroxide (NiFe-LDH) on the surface of the rGO-HS by electrostatic interaction.
[0055] In step F) above, the composite with the deposited metal double hydroxide is heat-treated at a temperature of 450 to 500°C for 1.5 to 3 hours in an argon or nitrogen atmosphere. Through this process, NiFe-LDH is converted into crystalline NiFe2O4, and some Ni ions are formed into amorphous a-NiO to form transition metal oxide nanoclusters.
[0056] In step G) above, the electrode composite for the hybrid battery generated after heat treatment is recovered through centrifugation or filtration, and after repeated washing with deionized water, is secured in a solid state through freeze-drying or vacuum drying. The final product is powdered into a form suitable for use as an electrode material.
[0057] In addition, the present invention provides a hybrid battery comprising the electrode composite for the hybrid battery.
[0058] The electrode composite for the hybrid battery described above may be included as a negative electrode material (negative active material) of the hybrid battery, and the negative electrode of the hybrid battery may further include a conductive material, a binder, and a negative current collector.
[0059] The above conductive material is a material for imparting electronic conductivity and may include carbon-based materials such as graphite, carbon black, super py, acetylene black, carbon fiber, carbon nanotube, graphene; metal powders such as copper, nickel, aluminum, silver; conductive whiskers such as zinc oxide, potassium titanate; conductive metal oxides; conductive polymers, etc., and any one or more of the above may be used.
[0060] The above binder is a resin-based polymer that fixes the negative electrode active material and the conductive material to the current collector, and one or more of binders known in the art, such as polyvinylidene fluoride (PVdF), carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), and Teflon (PTFE), may be used.
[0061] The above-mentioned cathode current collector is configured to provide an electrical path between the cathode active material and the power source, and it is preferable to use copper processed into a form such as copper foil or copper mesh.
[0062] The above hybrid battery may include a positive electrode, an electrolyte, and a separator in addition to the above negative electrode.
[0063] The above-mentioned positive electrode may include a positive electrode active material, a conductive material, a binder, and a positive electrode current collector, and the positive electrode active material may be selected from known active materials for lithium secondary batteries, such as lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), nickel cobalt manganese-based (NCM), nickel cobalt aluminum-based (NCA), and lithium iron phosphate (LiFePO4).
[0064] Since the conductive material, binder, and current collector for the anode are identical to the composition of the cathode, a repeated explanation is omitted; in particular, a conductive metal in the form of aluminum foil or aluminum mesh can be used as the anode current collector.
[0065] The above electrolyte may be composed of a lithium salt, an organic solvent that dissolves or contains the same, a polymer matrix, or an all-solid electrolyte, and lithium salts such as LiPF6, LiBF4, LiClO4, and LiN(CF3SO2)2 may be used as the lithium salt, and the organic solvent may be a carbonate-based mixture such as ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and fluoroethylene carbonate (FEC).
[0066] In addition, the above electrolyte may further include additives, viscosity modifiers, flame retardants, etc., and when using a polymer matrix, polymers such as polyethylene oxide (PEO), polyvinylidene fluoride (PVdF), and polyacrylonitrile (PAN), or copolymers mixed therewith may be used.
[0067] The above separator prevents electrical short circuits between electrodes and enables selective movement of ions, and may be composed of a porous thin film such as polyethylene (PE) or polypropylene (PP), or a composite separator coated with ceramic thereon.
[0068] The initial discharge capacity of the hybrid battery configured as above is 100 mAg -1 900 to 1,800 mAhg based on current density -1 , preferably 1,100 to 1,500 mAhg -1 , more preferably 1,250 to 1,300 mAhg -1 It can represent the value of.
[0069] In addition, under the same conditions, the initial charging capacity is 1,100 to 2,000 mAhg -1 , preferably 1,300 to 1,700 mAhg -1, more preferably 1,500 to 1,600 mAhg -1 It could be.
[0070] Accordingly, the initial Coulombic efficiency (CE) can be formed at a level of 60 to 90%, preferably 75 to 85%, and more preferably 80 to 83%.
[0071] This initial efficiency is primarily determined by the formation of a Solid Electrolyte Interphase (SEI) layer and irreversible reactions. The composite according to the present invention forms a uniform and stable SEI layer through a hydrothermal process and a heat treatment process, thereby increasing the CE to over 99% within 3 to 5 cycles and subsequently maintaining a stable efficiency of over 99.4% on average over the long term. Consequently, the electrode composite of the present invention achieves high initial capacity and rapid efficiency stabilization characteristics simultaneously, making it applicable as an electrode material for high-performance lithium secondary batteries that considers both energy density and cycle life.
[0072] The electrode composite for a hybrid battery according to the present invention can maintain a stable discharge capacity even under various current density conditions (C-rate) and can exhibit excellent responsiveness in high-speed charge and discharge characteristics.
[0073] The discharge capacity of the above hybrid battery is 900 to 1,200 mAhg under the 1C condition when the charge / discharge rate is varied from 1C to 50C. -1 , preferably 950 to 1,100 mAhg -1 , more preferably 1,000 to 1,050 mAhg -1 , 600 to 850 mAhg under 5C conditions -1 , preferably 650 to 800 mAhg -1 , more preferably 700 to 750 mAhg -1 , 450 to 700 mAhg under 10C conditions -1 , preferably 500 to 650 mAhg-1 , more preferably 550 to 600 mAhg -1 , 300 to 450 mAhg under 30C conditions -1 , preferably 320 to 400 mAhg -1 , more preferably 340 to 380 mAhg -1 , 250 to 330 mAhg under 50C conditions -1 , preferably 270 to 310 mAhg -1 , more preferably 280 to 300 mAhg -1 It can represent the value of.
[0074] These high-rate characteristics can be interpreted as the result of the organic combination of structural properties, such as the high electrical conductivity of the reduced graphene oxide sheet, rapid ion diffusion pathways due to the porous hollow structure, and enhanced interfacial reactivity between transition metal oxide nanoclusters.
[0075] The hybrid battery of the present invention can exhibit reactivation characteristics that recover to a capacity greater than the initial capacity even when switched back to low-rate conditions after performing charge and discharge under high-rate conditions.
[0076] After the initial capacity measurement, the above hybrid battery sequentially increases the current density to a maximum of 20,000 mAg -1 After undergoing high-rate discharge conditions up to (approx. 25C), again 100mAg -1 When switched to a low rate, the dose recovery rate may show a value of 120 to 180% relative to the initial dose, preferably 140 to 170%, and more preferably 160 to 170%.
[0077] In particular, the initial discharge capacity is approximately 1,280 mAhg -1 Under these conditions, the recovered capacity is 1,600 to 1,700 mAhg -1 , preferably 1,650 to 1,690 mAhg -1It is possible to reach this level. This high recovery rate can be interpreted as being due to the fact that internal active surfaces that were not exposed during high-speed charging and discharging are newly activated in subsequent cycles, thereby increasing the reaction area within the electrode and expanding the electrochemically available region.
[0078] The electrode composite for a hybrid battery according to the present invention can rapidly reach the State of Charge (SOC) even under high-speed charging conditions and exhibits excellent response speed under high current density conditions.
[0079] For example, under 10C conditions (approx. 8,000 mAg -1 When charging at a current density, the SOC can reach a level of 40 to 65%, preferably 50 to 60%, and more preferably 55 to 57% within 6 minutes.
[0080] These high-speed charging characteristics can be understood as the result of the combined effects of securing rapid ion diffusion pathways based on the porous hollow structure within the electrode composite, increasing electron transfer efficiency through a conductive network based on reduced graphene oxide sheets, and low electrode resistance characteristics due to a stable interfacial structure.
[0081] In addition, the hybrid battery of the present invention has an excellent discharge capacity retention rate even under long-term repeated charge and discharge conditions, and can exhibit excellent cycle stability even in high-output environments.
[0082] For example, when repeated charge and discharge cycles of 500 to 1,000 or more are performed in a current density range of 1C to 50C, the discharge capacity under the 1C condition is 800 to 1,200 mAhg -1 , preferably 900 to 1,100 mAhg -1 , more preferably 1,000 to 1,050 mAhg -1 It can be maintained at a level of 400 to 700 mAhg under 10C conditions. -1, preferably 450 to 650 mAhg -1 , more preferably 500 to 600 mAhg -1 , 250 to 320 mAhg even under 50C conditions -1 , preferably 270 to 310 mAhg -1 , more preferably 280 to 300 mAhg -1 It can maintain the discharge capacity. Such long-term durability can be interpreted as being realized by the stable crystal structure of the metal oxide, improved interfacial adhesion within the electrode, and the stabilization of the SEI layer during the cycling process. In particular, by maintaining a constant level of charge and discharge performance without structural collapse or a sharp drop in capacity even after cycling, the composite of the present invention can be evaluated as a durability-focused material suitable for high-power lithium-ion hybrid batteries.
[0083] The hybrid battery of the present invention can utilize not only the insertion-extraction reaction of lithium ions but also an interface-based rapid charge storage reaction (pseudocapacitor reaction) as the main electrochemical mechanism.
[0084] For example, the b value derived from the log(i)-log(v) relationship measured by cyclic voltammetry (CV) analysis may be 0.70 to 0.95, preferably 0.80 to 0.90, more preferably 0.83 to 0.86 based on the reduction peak, and 0.80 to 1.00, preferably 0.85 to 0.95, more preferably 0.89 to 0.92 based on the oxidation peak. This implies that the current follows a quasi-linear relationship in which it increases with powers of the scan rate, and represents a mixed charge storage mechanism in which diffusion-dominated reactions (lithium secondary battery reactions) and capacitance-dominated reactions (pseudocapacitor reactions) are mixed.
[0085] In particular, scan speed 0.6mVs -1As a result of quantitative analysis in, the contribution rate of the pseudocapacitor reaction to the total current can reach a level of 60 to 85%, preferably 70 to 80%, and more preferably 73 to 75%.
[0086] In addition, as the scan speed increases, the capacitance-based contribution rate also gradually increases, and can increase to 80 to 90%, preferably 85 to 90%, and more preferably 87 to 90% based on measurements after a cycle.
[0087] Also, scan speed 0.8mVs -1 As a result of comparing different electrodes, the electrode composite of the present invention (Example) records a pseudocapacitor contribution rate that is 5 to 15% higher than that of other electrodes (Comparative Example), and these results suggest that the rapid reaction characteristics of electrons and ions occurring at the interface between the graphene sheet and the metal oxide act as a major component of the current.
[0088] Hereinafter, through examples, an electrode composite for a hybrid battery comprising transition metal oxide nanoclusters and reduced graphene oxide according to the present invention, and a hybrid battery comprising the same, will be described in more detail. However, the following examples are merely references for explaining the present invention in detail, and the present invention is not limited thereto and can be implemented in various forms.
[0089] Furthermore, unless otherwise defined, all technical and scientific terms have the same meaning as generally understood by one of the art to which the present invention pertains. The terms used in the description herein are merely for the purpose of effectively describing specific embodiments and are not intended to limit the present invention. Additionally, the units of additives not specifically stated in the specification may be in weight percent.
[0090] [Example] rGO / a-NiO / NiFe 2 O 4 -HS
[0091] 40 mg of graphene oxide (GO) was mixed with 50 mL of deionized water and sonicated for 30 minutes. Subsequently, 3.0 mL of ascorbic acid was added, and a hydrothermal reaction was performed at 120°C for 10 hours to produce reduced graphene oxide (rGO). The produced rGO was obtained in powder form through recovery, washing, and freeze-drying.
[0092] Next, polystyrene (PS) nanobeads were dispersed in 20 mL of DIW, and GO was added in the same way to perform the same hydrothermal reaction. Subsequently, hollow-structured rGO-HS was formed through a PS removal process. At this time, additional thermal reduction treatment was performed on the rGO-HS to remove residual oxygen groups and ensure structural stability.
[0093] Subsequently, an aqueous solution of nickel and iron nitrate (Ni:Fe = 2:1) was added to rGO-HS, and a nickel-iron dihydroxide was deposited by hydrolyzing hexamethylenetetramine (HMT). The deposited precursor was heat-treated at 470°C for 2 hours in an argon atmosphere to be converted into a porous oxide layer containing a-NiO and NiFe2O4. The finally obtained rGO / a-NiO / NiFe2O4-HS composite is an electrode composite for a hybrid battery corresponding to an embodiment of the present invention.
[0094] [Comparative Example 1] rGO
[0095] Reduced graphene oxide (rGO) prepared in the initial stage of the example was used as the sole electrode active material.
[0096] [Comparative Example 2] rGO-HS
[0097] Comparative Example 2 used rGO-HS formed based on a PS template as the sole electrode active material.
[0098] [Comparative Example 3] NiO
[0099] Comparative Example 3 used commercial NiO nanoparticles as the sole electrode active material.
[0100] [Comparative Example 4] NiFe 2 O 4
[0101] Comparative Example 4 used commercial nickel-iron oxide (NiFe2O4) nanoparticles as the sole electrode active material.
[0102] [Comparative Example 5] rGO / NiO / NiFe 2 O 4 -Air
[0103] Comparative Example 5 used a sample of the nickel-iron dihydroxide precursor composite of the example, heat-treated at 400°C in an air atmosphere, as a single electrode active material.
[0104] [Characteristic Evaluation Method]
[0105] A. Structural Formation and Analysis of Electrode Composites for Hybrid Batteries
[0106] FIG. 1 is a schematic diagram illustrating the manufacturing process of an exemplary hybrid structure according to the present invention. First, to control the nanostructure, polystyrene (PS) beads surface-modified with polyethyleneimine (PEI) to have a positively charged surface were used as a template. Negatively charged graphene oxide (GO) was electrostatically adsorbed onto the surface of the PEI-treated PS beads by oxygen-containing functional groups (e.g., -COOH, -OH), and positively charged nickel-iron double hydroxide was alternately deposited on the GO layers. By repeating this layered self-assembly process, a GO / nickel-iron double hydroxide multilayer structure was formed, and the composite structure of the example was finally manufactured by heat treatment.
[0107] Heat treatment was performed in an Ar atmosphere, and during this process, oxygen functional groups on the surface of GO were thermally decomposed and removed as CO and CO2 gases, thereby converting GO into reduced graphene (rGO). At the same time, nickel-iron dihydroxide transitioned into crystalline NiFe2O4, undergoing a solid-state transition with partially amorphous α-NiO incorporated, while the Ni:Fe atomic ratio was maintained at 2:1, the same as the initial synthesis ratio.
[0108] Figure 2 shows the PXRD patterns of the precursor containing PS beads and the heat-treated composite. The PS beads are amorphous peaks (2θ It shows 19.5°, which disappears after heat treatment. In the heat-treated example, diffraction peaks of NiFe2O4 (JCPDS No. 10-0325) (27.0°, 35.3°, 43.0°, 56.1°, 62.6°) were confirmed, showing that a metal oxide phase was stably formed after PS removal.
[0109] In the FTIR spectrum of Fig. 3, the PS bead-based precursor is at 695, 1,008, and 1,450 cm⁻¹. -1 It shows peaks corresponding to the benzene ring vibration and CH bending vibration, respectively. However, it can be confirmed that these peaks completely disappear after heat treatment.
[0110] Figure 4 shows the TGA analysis results, and the example obtained after heat treatment showed only a gradual mass reduction due to the oxidation of rGO in the 400–500°C range, and it was confirmed that an inorganic residue of about 15 wt% remained thereafter.
[0111] B. Analysis of Local Structure and Electronic State of Metal Oxide Nanoclusters
[0112] Figure 5 shows the XANES spectra for the Fe and Ni K-edges, respectively, where the edge positions of the examples exhibit similar absorption edges and intensity steps compared to standard materials NiFe2O4 and α-NiO. This confirms that Fe ions exist mainly in an oxidation state of +3 (+2.9) and Ni ions mainly in +2 (+2.2), suggesting that they are stable metal oxide phases that are not excessively electron-deficient or excessively reduced.
[0113] Figure 6 shows the results of decomposing the XANES curve of the sample into standard materials using linear combination fitting (LCF). Through this, the phase ratio of NiFe2O4 and α-NiO within the example was quantitatively derived, and it was experimentally confirmed that a ratio of approximately 2:1 was maintained. This indicates that under heat treatment conditions, nickel-iron dihydroxide is quantitatively converted to NiFe2O4, and some Ni ions exist in the amorphous NiO phase.
[0114] Figures 7 and 8 show the k for the Fe and Ni K-edges, respectively. 3 The weighted EXAFS spectrum and its Fourier transform (FT spectra) reflect local bonding distances due to Fe-O and Ni-O, Fe-Fe and Ni-Fe interactions. The Fe-O peak appears at approximately 1.5 Å, and the Fe-Fe peak at approximately 2.9 Å, which is consistent with the normal spinel structure of NiFe2O4. On the other hand, the Ni-O peak is observed broadly around 2.05 Å, reflecting the characteristics of the amorphous structure. These results support the coexistence of the crystalline NiFe2O4 phase and the amorphous α-NiO phase.
[0115] Finally, Figure 9 shows the wavelet transform (WT) analysis results for the Ni and Fe K-edges, reflecting both k- and R-space resolutions simultaneously. The Fe WT map indicates the presence of crystalline NiFe2O4 with well-preserved Fe-centered oxygen bonding structures. On the other hand, the Ni WT map shows broad peaks, which supports the existence of a-NiO in an amorphous state.
[0116] As such, through XANES and EXAFS analyses, it was demonstrated that the composite of the present invention is simultaneously endowed with structural heterogeneity and electrochemical activity by the coexistence of the crystalline oxide structure of NiFe2O4 and the amorphous phase of α-NiO.
[0117] C. Analysis of the morphology and microstructure of the complex
[0118] Through the FESEM image shown in Fig. 10, it can be confirmed that the fabricated composite consists of uniform spherical particles with an average diameter of approximately 560–640 nm, and that the porous (hollow sphere) structure is well maintained overall. In particular, it can be confirmed that even after heat treatment, the individual particles maintain an independent spherical shape with distinct boundaries and are uniformly distributed without aggregation.
[0119] Figure 11 shows the results of observing the fracture cross-section of a single sphere using high-magnification TEM, where a typical core-void-shell structure is clearly observed. This indicates that the LBL self-assembly method using PS beads as a template operated effectively, and the internal hollow region can be advantageous for securing ion diffusion pathways and absorbing structural expansion.
[0120] Figure 12 is a high-resolution TEM (HRTEM) image of the composite, showing that metal oxide nanoparticles with different crystal planes are uniformly dispersed on the rGO substrate. Analysis of the crystal lattice spacing revealed that spacings of approximately 0.252 nm and 0.290 nm correspond to the (311) plane of NiFe2O4 and the (111) plane of a-NiO, respectively, which is consistent with the previous XRD and EXAFS results.
[0121] D. High-resolution structural and graphene interface analysis
[0122] The HRTEM image on the left side of Fig. 14 shows a structure in which NiFe2O4 nanoparticles are surrounded by irregularly stacked graphene sheets. Through Fast Fourier Transform (FFT) and inverse transform image analysis, the lattice spacing corresponding to the (311) and (220) crystal planes of the NiFe2O4 particles was measured to be approximately 0.252 nm and 0.290 nm, respectively, which is consistent with PXRD analysis. In addition, the average interlayer spacing of the rGO sheets is distributed from 0.33 to 0.56 nm, and the average spacing was calculated to be approximately 4.21 nm.
[0123] Graphene with such a turbostratic structure provides high flexibility and structural gaps around the particles, significantly improving stress relief due to volume changes of NiFe2O4 particles and interfacial stability during electrochemical reactions. In particular, the graphene layer acts as a protective barrier that blocks electrolyte reactions between particles, while simultaneously acting as an electron and ion transport pathway to maximize reactivity.
[0124] Such an irregular multilayer graphene structure acts as an ideal electrode structure that effectively exposes electrochemical reaction sites while preventing direct exposure of nanoparticles, and makes a decisive contribution to securing high-rate and long-term cycle characteristics.
[0125] Additionally, the right side of Fig. 14 shows the results of observing locally distributed crystalline NiO (c-NiO) nanoparticles within the complex using high-magnification HRTEM. These particles are present in small numbers only in certain regions and are interpreted as FCC-based rock salt structures possessing a typical octahedral (NiO6) structure. According to the results combined with XAS analysis, this NiO exhibits a dual coordination environment in which square planar and rock salt structures coexist; this is determined to have been formed by heat treatment under oxygen-deficient conditions and interfacial effects between the constituent components.
[0126] E. Analysis of Electrochemical Characteristics
[0127] Fig. 15 shows 100–20,000 mA g -1 It shows the charge and discharge curves measured within the range, and the electrode in the example is under low current conditions (100 mA g -1 Approximately 1,278.3 mAh g at ) -1 The capacity was recorded, and 20,000 mA g -1 283.3 mAh g even under extreme conditions -1 maintained. Afterwards, again 100 mA g -1 When switched to, the discharge capacity is 1,687.6 mAh g -1 It was recovered to [amount], which means a capacity recovery rate of 167.2% compared to the initial level. That is, despite the excessive load in the example, these results are interpreted as being due to the electrode reactivation effect and the gradual exposure of the internal active surface.
[0128] In the initial cycle, the Coulomb efficiency of the example was approximately 82.2%, and subsequently rose rapidly to over 99%, recording a stable efficiency of 99.4% on average. In other words, this suggests that after the stable initial SEI formation at the interface between the reduced graphene oxide sheet and the transition metal oxide nanocluster of the example, a stable reaction environment was formed, blocking side reactions with the electrolyte and simultaneously securing initial Coulomb efficiency and long-term cycle stability.
[0129] Figure 16 shows the results of a comparison of long-term charge-discharge performance performed over 560 cycles for the example and comparative example. The electrode of the example is 1,000 mA g -1 At the current density, 763.2 mAh g each at the end of the cycle -1 (Discharged), 759.4 mAh g -1 It maintained a high capacity (charging), which is the reversible capacity based on the second cycle (579.6 / 536.6 mAh g -1 This represents an excellent retention rate of 131.7% / 141.5% compared to ). This demonstrates that the electrical connectivity and charge transfer characteristics between the metal oxide nanoparticles and the graphene interface were stably maintained.
[0130] Meanwhile, among the comparative example electrodes, the electrodes of Comparative Example 1 (rGO) and Comparative Example 2 (rGO-HS) were 295.6 / 294.2 mAh g, respectively. -1 and 89.2 / 89.3 mAh g -1 It exhibited a relatively low capacity. It is determined that the performance of the Comparative Example 1 electrode was further degraded because it did not have a hollow structure and lacked ion storage and transport pathways, and although the Comparative Example 2 electrode has some structural advantages due to its hollow structure, it is determined that capacity acquisition was limited because it does not contain transition metal oxide nanoclusters.
[0131] Next, the electrodes of Comparative Example 3 (NiO) and Comparative Example 4 (NiFe2O4) were 1,000 mA g -1 Under the conditions, a rapid decrease in capacity was observed within the first 100 cycles. More specifically, Comparative Example 3 lost 96.3% of its total capacity, and Comparative Example 4 lost 92.3%. This is analyzed to be due to the unstable formation of the SEI layer caused by the inherently low conductivity and particle aggregate structure of the metal oxide, leading to structural collapse during repeated cycling.
[0132] Finally, Comparative Example 5 (rGO / NiO / NiFe2O4-Air) electrode used the same precursor composite as the example, but was manufactured under conditions of heat treatment at 400°C in an air atmosphere. Consequently, the metal oxide particles agglomerated unevenly, weakening interfacial connectivity with the graphene layer, and the conductivity was significantly reduced due to low residual oxygen and grain boundary density within the structure. As a result, a rapid decrease in capacity occurred within 30 initial cycles. Unlike the example of the present invention, it is determined that the uneven dispersion structure between the metal oxide and graphene and the lack of interfacial bonding strength were the main causes.
[0133] FIG. 17 shows the results of evaluating the long-term performance of the example electrode over 1,000 cycles under various C-rate conditions from 1 to 50 C based on the Peukert constant, with 1,023.1 mAh g under the 1 C condition. -1 , 282.2 mAh g even under 50C conditions -1 It maintained excellent capacitance stability even at high current densities. Overall, the electrode of the example exhibited the most ideal current-capacity relationship (k 1.20) was shown, maintaining the most ideal current-capacity relationship. This means that electrochemical performance degradation is minimized even under high-speed charging and discharging conditions.
[0134] In Fig. 18, the characteristics of the change in State of Charge (SOC) during fast charging were analyzed, and the electrode of the example reached 55.4% SOC within about 6 minutes under 10C conditions. This suggests that charge distribution is uniform within the electrode and that a fast electron-ion transfer pathway is secured.
[0135] Meanwhile, Fig. 19 shows 0.1–0.8 mV s -1It includes the CV curves measured at the scan rate and the results of the log(i)-log(v) relationship analysis. The b values derived from the log(i)-log(v) relationship were found to be 0.84 at the reduction peak and 0.91 at the oxidation peak, reflecting a complex reaction mechanism involving a mixture of diffusion-dominated and capacitance-dominated reactions. In particular, results showing a b value greater than 0.5 indicate the dominance of interface-based charge storage characteristics and suggest a dominant contribution from pseudocapacitor reactions.
[0136] Also, in FIG. 19, i(V) / v 1 / 2 ul v 1 / 2 A Cottrell plot is shown for this, which is the result of quantitatively separating the contribution rates of pseudocapacitors and diffusion-controlled reactions constituting the total current. Through this analysis, it was confirmed that the rapid interfacial reaction of the electrode in the example accounts for most of the total current.
[0137] In Fig. 20, the capacitance-based contribution rate increased sharply with increasing scan speed, reaching up to 87.6% based on measurements after the cycle. This demonstrates that the electrode surface-based charge storage mechanism acts dominantly even under high-speed response conditions.
[0138] The left graph of Fig. 21 shows the results of comparing the capacitance-based charge storage contribution rates between the Example, Comparative Example 1, and Comparative Example 2 under pre-cycle conditions. Scan rate 0.8 mV s -1Under the conditions, it was analyzed that 78.6% of the total current of the example electrode was attributed to capacitance, which is the highest percentage compared to the electrode of Comparative Example 1 (63.0%) and the electrode of Comparative Example 2 (74.4%). These results suggest that the interfacial reaction-based charge storage pathway was effectively expanded by the uniform dispersion of NiFe2O4 and α-NiO nanoparticles on the rGO sheet. In particular, it can be confirmed that the pseudocapacitor reaction, activated by the multiple oxidation state transition of the metal oxide, acts as a major component of the current.
[0139] In addition, the graph on the right in Fig. 21 shows the results of comparing the change in capacitance contribution rate after long-term cycling for identical electrodes. The pseudocapacitor contribution rate of the electrode in the example increased from an initial 78.6% to 87.6%. On the other hand, the electrode in Comparative Example 2 increased from 74.4% to 82.2%, and the electrode in Comparative Example 1 increased from 63.0% to 70.2%, respectively. This increase in contribution rate reflects a kinetic evolution in which the proportion of capacitor-dominated reactions replaces diffusion-dominated reactions as active sites within the electrode are gradually exposed and interfacial reactivity improves during the long-term charging and discharging process. In particular, the composite electrode according to the present invention demonstrates that the interface-based charge storage mechanism is further strengthened even after cycling, thereby securing superiority in terms of long-term stability and high-rate reactivity.
[0140] FIG. 22 shows that nickel-iron double hydroxide is converted into a-NiO / NiFe2O4 nanoparticles through heat treatment and changes into a structure having multiple grain boundaries. From these structural features, the present invention can improve interface-based charge storage capacity and provide fast pseudocapacitor responsiveness without diffusion delay.
[0141] F. Analysis of High-Rate Charge / Discharge Characteristics
[0142] Figure 23 shows the Nyquist plot for each electrode. The intersection observed in the high-frequency region represents the ionic conductivity of the electrolyte and the interfacial contact resistance (R) of the cell components. s It corresponds to ), and the semicircle in the high-mid frequency region is SEI formation and interfacial charge transfer resistance (R ct Reflects the ) component. In the example, as the cycle progresses, the electrode R s It shows a gradual decreasing trend, suggesting that the internal resistance decreases as the SEI layer and electrode structure stabilize during the initial cycle.
[0143] In addition, the Distribution of Relaxation Time (DRT) analysis results in Fig. 24 show the ion transport resistance (R) within the SEI. f , τ1) and charge transfer resistance (R) at the electrolyte-active material interface ct , τ2) were derived by isolating them individually. The electrode in the example showed an increase in the τ2 peak immediately after the initial discharge of the cycle, but then gradually decreased, maintaining stable electrochemical characteristics, which indicates that a reversible charge transfer path at the internal interface was secured.
[0144] H. Analysis of Lithium Diffusion Mechanisms Based on Electrode Impedance and Structure
[0145] Figure 25 summarizes the results of each impedance parameter derived by applying an equivalent circuit-based model to the electrodes of the Example, Comparative Example 1, and Comparative Example 2. Through this analysis, the electrode of the Example is R s (Series resistance), R ct It recorded the lowest values for all (charge transfer resistance), suggesting excellent electrical continuity and interfacial stability within the electrode.
[0146] Figure 26 shows the results of comparing the change in the Warburg coefficient over the course of a cycle. After 100 cycles, the Warburg coefficient of the electrode of the example decreased to about 30-40% of that of Comparative Example 1 and Comparative Example 2. This means that even during repeated charging and discharging, the electrode of the present invention maintains low lithium diffusion resistance and the ion transport pathway is gradually optimized.
[0147] Figure 27 compares the Warburg coefficients of metal oxide-based electrodes (Example, Comparative Example 3, Comparative Example 4), showing that the structure of the Example, in which a non-simultaneous phase mixed structure (a-NiO and NiFe2O4) is uniformly dispersed, is advantageous in terms of lithium diffusion performance compared to a single-phase electrode. Therefore, the Example maintained the lowest Warburg coefficient among these electrodes.
[0148] Figure 28 (d) illustrates the mechanism of increasing electrode resistance and decreasing capacity that occurs as the SEI layer is repeatedly destroyed and reformed during electrode charge-discharge cycles. While conventional transition metal oxide-based electrodes show significant performance degradation in long-term cycles due to structural expansion and SEI instability, the electrode of the present invention enables stable SEI formation through a porous hollow structure and a flexible matrix of rGO, thereby ensuring an excellent capacity retention rate even in long-term cycles.
[0149] Finally, FIG. 28(e) is a schematic diagram illustrating the difference in lithium ion diffusion pathways between Comparative Example 1, Comparative Example 2, and the Example electrodes. In a single rGO structure, ion diffusion is restricted due to the recombination phenomenon between graphene sheets, whereas in a composite electrode where NiFe2O4 and α-NiO nanoparticles act as spacers, the spacing between sheets is maintained, allowing lithium ions to be inserted and extracted more smoothly. These structural advantages directly contribute to the high-speed charge / discharge characteristics and long-term durability of the electrodes.
[0150] Although the present invention has been described above through specific details and limited embodiments, this is provided merely to aid in the overall understanding of the invention, and the invention is not limited to the above embodiments. Those skilled in the art can make various modifications and variations from this description.
[0151] Accordingly, the scope of the present invention is not limited to the described embodiments, and all things equivalent to or having equivalent variations to the claims set forth below, as well as the claims set forth below, shall be considered to fall within the scope of the concept of the present invention.
Claims
Claim 1 An electrode composite for a hybrid battery that stores electrochemical energy through the insertion-extraction reaction of lithium ions (lithium secondary battery reaction) and the oxidation-reduction reaction of transition metal ions (pseudocapacitor reaction), comprising a reduced graphene oxide sheet and a transition metal oxide nanocluster, wherein the transition metal oxide nanocluster is formed by the aggregation of transition metal oxide nanocrystals, grain boundaries are formed between the nanocrystals, and the ratio of grain boundaries to the total surface area of the transition metal oxide nanocluster is 50% or more. Claim 2 An electrode composite for a hybrid battery according to claim 1, characterized in that the reduced graphene oxide sheet performs lithium ion insertion and extraction reactions at an interlayer structure or defect site. Claim 3 An electrode composite for a hybrid battery according to claim 1, characterized in that the reduced graphene oxide sheet forms an electron transfer pathway at the contact interface with a transition metal oxide nanocluster due to π-π interaction or a difference in binding energy. Claim 4 An electrode composite for a hybrid battery according to claim 1, characterized in that the reduced graphene oxide sheet accounts for 50% or more of the current generated during the electrochemical charging and discharging process, which is attributable to a pseudocapacitor reaction. Claim 5 delete Claim 6 delete Claim 7 An electrode composite for a hybrid battery according to claim 1, characterized in that the size of the transition metal oxide nanocrystals forming the transition metal oxide nanocluster is 1 nm to 10 nm. Claim 8 A hybrid battery electrode composite according to claim 1, characterized in that the electrode composite for the hybrid battery has a hollow structure. Claim 9 An electrode composite for a hybrid battery according to claim 8, wherein the hollow comprises a shell having a thickness of 20 nm to 40 nm. Claim 10 In claim 8, the electrode composite for a hybrid battery is formed of spherical particles having a hollow structure with an average particle size of 400 nm to 1,000 nm. Claim 11 A method for manufacturing an electrode composite for a hybrid battery according to any one of claims 1 to 4 and 7 to 10. Claim 12 A hybrid secondary battery comprising an electrode composite for a hybrid battery according to any one of claims 1 to 4 and 7 to 10. Claim 13 In Clause 12, the above-mentioned hybrid secondary battery has a current density of 100 mAg during charging and discharging. -1 The capacity based on 1,500mAh g -1 Lee Sang-in hybrid secondary battery.
Citation Information
Patent Citations
Two-dimensional nanosheets and methods of making and use thereof
US20160254528A1