Anode active materil for lithium secondary battery, manufacturing method of the same and lithium secondary battery comprising the same

A coated secondary particle structure of natural graphite with specific density and orientation ratios addresses the swelling and output issues in lithium-ion batteries, enhancing lifespan and performance.

KR103046669B1Active Publication Date: 2026-11-10POSCO FUTURE M CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020240151879
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2026-11-10
Estimated Expiration
2044-10-31

AI Technical Summary

Technical Problem

Existing lithium-ion secondary batteries using natural graphite as a negative electrode material face challenges with high swelling rates, irreversible reactions, and reduced output characteristics due to the plate-like shape and increased surface area, leading to degraded long-term lifespan.

Method used

A negative electrode active material comprising a first material with a tap density of 0.80 g/cc or less and a second material with a tap density of 0.81 g/cc or more, where the first material has an orientation peak intensity ratio of 75 or more, is manufactured by mixing primary particles with amorphous carbon, pressurizing, crushing, and heat-treating to form a coated secondary particle structure.

Benefits of technology

The solution results in a negative electrode active material with improved lithium ion conductivity, reduced swelling, and enhanced electrochemical properties, such as increased lifespan and output characteristics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present embodiments relate to a negative electrode active material for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery including the same. A negative electrode active material for a lithium secondary battery according to one embodiment comprises: a first negative electrode active material having a tap density of 0.80 g / cc or less; and a second negative electrode active material having a tap density of 0.81 g / cc or more; wherein the first negative electrode active material may have an orientation peak intensity ratio (I110 / I004) of 75 or more when analyzing an XRD pattern.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present embodiments relate to a negative electrode active material for a lithium secondary battery, a method for manufacturing the same, and a lithium secondary battery including the same. Background Technology

[0002] Due to technological development and increasing demand for mobile devices, as well as the rapid rise of electric vehicles (EVs), the demand for lithium-ion batteries as an energy source for these devices is increasing rapidly.

[0003] As the negative electrode active material for such lithium-ion secondary batteries, graphite-based materials such as synthetic graphite and natural graphite are generally used. These materials reversibly accept or supply lithium ions while maintaining structural and electrical properties, and possess chemical potential characteristics nearly similar to metallic lithium during lithium ion insertion and extraction.

[0004] Artificial graphite has a higher charge-to-discharge efficiency than natural graphite and exhibits excellent lifespan characteristics due to less swelling during charging and discharging. However, it has a lower reversible capacity compared to natural graphite, and its hard grains make rolling difficult during electrode manufacturing. Additionally, it has the problem of poor orientation due to minimal shape change. In particular, it has the disadvantage of high manufacturing costs as it requires graphitization heat treatment at around 3,000°C.

[0005] In contrast, natural graphite is widely used as a negative electrode active material because it is cheaper than synthetic graphite, has a high reversible capacity, and exhibits similar electrochemical properties.

[0006] However, since natural graphite generally has a plate-like shape, it has a large surface area and exposed edges. Consequently, the penetration or decomposition of electrolytes causes the edges to peel off or break, leading to significant irreversible reactions and an increased expansion rate, which degrades long-term lifespan characteristics.

[0007] To address this, a method using spherical natural graphite has been proposed; however, in this case, the increase in internal pores leads to longer lithium diffusion distances and larger particle sizes, resulting in a problem of reduced output characteristics when applied to batteries.

[0008] Therefore, there is an urgent need to develop technology capable of realizing lithium secondary batteries with excellent long-term lifespan and output characteristics while using natural graphite. The problem to be solved

[0009] The present embodiment aims to provide a negative electrode active material for a lithium secondary battery that has excellent lifespan and output characteristics while reducing the swelling rate, a method for manufacturing the same, and a lithium secondary battery including the same. means of solving the problem

[0010] A negative electrode active material for a lithium secondary battery according to one embodiment comprises: a first negative electrode active material having a tap density of 0.80 g / cc or less; and a second negative electrode active material having a tap density of 0.81 g / cc or more; wherein the first negative electrode active material may have an orientation peak intensity ratio (I110 / I004) of 75 or more when analyzing an XRD pattern.

[0011] A method for manufacturing a negative electrode active material for a lithium secondary battery according to another embodiment may be manufactured by mixing a first negative electrode active material and a second negative electrode active material to produce a negative electrode active material, wherein the second negative electrode active material is manufactured by a method comprising: a step of sphericalizing natural graphite powder to a high density; and a step of coating the high density sphericalized natural graphite powder by mixing a second amorphous carbon; and wherein the first negative electrode active material may be manufactured by a method comprising: a step of preparing primary particles having an average particle size (D50) of 3 to 5 μm; a step of mixing the primary particles and the first amorphous carbon to produce a mixture; a step of pressurizing the mixture at a temperature of 50°C or higher to produce a molded body; a step of crushing the molded body; and a step of heat-treating the crushed molded body. Effects of the invention

[0012] According to the present embodiment, by providing a negative electrode active material comprising a first negative electrode active material having a tap density of 0.80 g / cc or less and a second negative electrode active material having a tap density of 0.81 g / cc or more, a negative electrode active material with excellent lifespan and output characteristics and reduced swelling occurrence rate can be realized. Specific details for implementing the invention

[0013] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.

[0014] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of "comprising" specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.

[0015] When it is stated that one part is "above" or "on" another part, it may be directly above or on the other part, or other parts may be involved in between. In contrast, when it is stated that one part is "directly above" another part, no other parts are interposed in between.

[0016] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0017] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.

[0018] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.

[0019] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0021] Negative active material for lithium secondary batteries

[0022] A negative electrode active material for a lithium secondary battery according to one embodiment comprises: a first negative electrode active material having a tap density of 0.80 g / cc or less; and a second negative electrode active material having a tap density of 0.81 g / cc or more; wherein the first negative electrode active material may have an orientation peak intensity ratio (I110 / I004) of 75 or more when analyzing an XRD pattern.

[0023] The negative electrode active material of the present embodiment may include a first negative electrode active material and a second negative electrode active material.

[0024] At this time, the weight ratio of the first cathode active material and the second cathode active material may be in the range of 1:9 to 5:5, more specifically 2:8 to 4:6. When the weight ratio of the first and second cathode active materials satisfies the above range, a cathode active material can be realized that has excellent electrochemical properties such as capacity, lifespan, and output characteristics, while simultaneously having a significantly reduced swelling rate.

[0025] The first cathode active material comprises natural graphite particles in the form of secondary particles including primary particles having an average particle size (D50) of 3 to 5 μm, and a first coating layer located on the surface of the natural graphite particles, and the interior of the natural graphite particles in the form of secondary particles and the first coating layer may include a first amorphous carbon.

[0026] In this way, since the first amorphous carbon is evenly positioned inside the natural graphite particles in the form of secondary particles and at the same time forms a first coating layer on the surface, side reactions of the natural graphite with respect to the electrolyte are suppressed, irreversible reactions are reduced, and lithium ion conductivity is improved, thereby improving electrochemical characteristics such as the output and lifespan of the battery.

[0027] At this time, the content of the first amorphous carbon may be in the range of 1% to 30% by weight, more specifically 5% to 25% by weight, or 10% to 20% by weight, based on the total weight of the first negative electrode active material. When the content of the first amorphous carbon satisfies the above range, the primary particles are effectively assembled into the form of secondary particles and a surface coating layer is formed at the same time, which can reduce side reactions and improve lithium ion conductivity, and improve the output and lifespan characteristics of the lithium secondary battery.

[0028] At this time, the first amorphous carbon may include, for example, one or more selected from the group consisting of petroleum-based pitch, coal-based pitch, mesophase pitch, heavy oil, light oil, polyvinyl alcohol (PVA), polyvinyl chloride (PVC), sucrose, phenol resin, furan resin, furfuryl alcohol, polyacrylonitrile, cellulose, styrene, polyimide, epoxy resin, and glucose. However, the present invention is not limited to the aforementioned types of first amorphous carbon. If there are other types of amorphous carbon applicable to the present invention in addition to the aforementioned types, the invention may be extended to include such types.

[0029] In the first negative electrode active material, the thickness of the first coating layer located on the surface of the natural graphite particles in the form of secondary particles may be 5 to 20 nm. If the thickness of the first coating layer is too small, there is an advantage in reducing resistance when lithium ions are inserted into / extracted from the graphite, but it is impossible to ensure coating uniformity and problems such as increased side reactions due to non-uniform coating may occur. If the thickness of the first coating layer is too large, it is difficult for lithium ions to be inserted and extracted, which may lead to problems such as increased negative electrode resistance and reduced lifespan.

[0030] Meanwhile, the first cathode active material may have an orientation degree (I110 / I004) of 75 or higher when analyzed by XRD pattern, more specifically 75 to 110, 75 to 105, or 78 to 100.

[0031] As the orientation (I110 / I004) of the first negative electrode active material satisfies the above range, the directionality of the graphite layer edge portion within the graphite particle can be diversified, allowing for smoother movement of lithium ions, and thereby maximizing the initial efficiency of the battery.

[0032] In this specification, the degree of orientation can be determined using JCPDS (ASTM) data, which is standard data obtained by X-ray diffraction, as an indicator, and refers to the value obtained by measuring the (004) plane and (110) plane of the negative electrode active material by XRD and dividing the peak intensity value of the (110) plane by the peak intensity value of the (004) plane.

[0033] At this time, specifically, plane (110) represents the range of 76.5 degrees < 2θ < 78.5 degrees, plane (004) represents the range of 53.5 < 2θ < 56.0 degrees, and 2θ represents the diffraction angle.

[0034] Meanwhile, the degree of orientation within the above range is noteworthy as it is significantly improved compared to the values ​​observed in conventional natural graphite cathode active materials, and this can be easily obtained through a pressurization process on natural graphite. This will be explained in more detail in the manufacturing method described later.

[0035] Next, the BET (Brunauer-Emmett-Teller) specific surface area of ​​the first cathode active material is 3.0 m² 2 / g or more, 3.0 to 8.0m 2 / g or 3.5 to 7.0 m 2 / g can be in the range.

[0036] In this specification, the BET specific surface area can be measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).

[0037] If the specific surface area of ​​the first negative electrode active material is too small, problems such as reduced lifespan due to increased resistance of the negative electrode material may occur, as there is an excessive amount of surface coating material; or if the crystal orientation of the graphite layer edge is unidirectional, problems such as limited lithium insertion and extraction may occur, leading to deterioration of output characteristics. On the other hand, if the specific surface area of ​​the first negative electrode active material is too large, problems such as reduced battery lifespan may occur due to excessive film (SEI) formation and side reactions at the surface graphite layer edge.

[0038] The tap density of the first negative electrode active material may be 0.80 g / cc or less, more specifically, in the range of 0.10 g / cc to 0.80 g / cc, 0.50 g / cc to 0.80 g / cc, or 0.65 g / cc to 0.80 g / cc. As the tap density satisfies the above range, deformation is minimized even when pressed at a constant pressure during electrode manufacturing after mixing with the second negative electrode active material, thereby suppressing expansion due to charging and discharging.

[0039] In this specification, the tap density can be measured using the AT-2 model of Quantachrome, and can be measured by filling a test container with a sample with a volume of 20 ml, tapping it 3,000 times, and then measuring the volume and weight of the sample.

[0040] In addition, the first negative electrode active material may satisfy the following Equation 1.

[0041] [Equation 1]

[0042] 2.5 ≤ [D90] / [D10] ≤ 6.5

[0043] In the above Equation 1, [D10] and [D90] represent particle sizes corresponding to 10% and 90% of the cumulative volume of the first cathode active material measured using the Laser Diffraction Method.

[0044] The above Equation 1 is a value corresponding to the ratio of the particle size corresponding to 90% to the particle size corresponding to 10% of the cumulative volume of the first cathode active material, and may be an indicator representing the uniformity of the particles. Specifically, the above Equation 1 may be 3.0 to 6.0, 3.5 to 5.8, or 3.8 to 5.4.

[0045] If the above Equation 1 exceeds the upper limit of the aforementioned range, there is a problem in that the proportion of granules increases, and relatively large particles exist within the limited electrode thickness, which can induce non-uniformity of the electrode.

[0046] In addition, if the above Equation 1 deviates from the lower limit of the aforementioned range, there is a problem in that the powder specific surface area increases as the proportion of fine particles increases, and processability decreases during slurry preparation and coating.

[0047] In one embodiment, the particle size (D10) corresponding to 10% of the volume accumulation of the first negative electrode active material may be 1 μm to 9 μm, more specifically 3 μm to 7 μm or 4.5 μm to 6.5 μm.

[0048] In one embodiment, the particle size (D90) corresponding to 90% of the volume accumulation of the first negative electrode active material may be 15㎛ to 35㎛, more specifically 20㎛ to 30㎛ or 23㎛ to 28㎛.

[0049] By satisfying the aforementioned range for the volume accumulation of the first negative electrode active material, it is possible to manufacture a stable negative electrode active material when mixed with the second negative electrode active material, and by using this, a lithium secondary battery with excellent lifespan characteristics and output characteristics can be manufactured.

[0050] In addition, the first negative electrode active material may have an average particle size (D50) of 9 to 15 μm, more specifically 10 to 14 μm or 11 to 13 μm. If the average particle size (D50) of the first negative electrode active material is too small, there may be a problem where side reactions with the electrolyte increase as the specific surface area increases. If the average particle size (D50) of the first negative electrode active material is too large, there may be a problem where the output characteristics deteriorate as the lithium diffusion distance increases.

[0051] Next, the second cathode active material comprises natural graphite and a second coating layer located on the surface of the natural graphite, and the second coating layer may comprise a second amorphous carbon.

[0052] The second amorphous carbon may be of the same type as the first amorphous carbon or a different type. Since the type of the second amorphous carbon is the same as that of the first amorphous carbon, it will be omitted here.

[0053] The content of the second amorphous carbon may be in the range of 1 to 20 weight%, more specifically 1 to 10 weight% or 3 to 8 weight%, based on the total weight of the second negative electrode active material. When the content of the second amorphous carbon satisfies the above range, other physical properties of the second negative electrode active material, such as BET and tap density, can be appropriately implemented to satisfy the range of this embodiment.

[0054] The BET (Brunauer-Emmett-Teller) specific surface area of ​​the second cathode active material is 3 m² 2 / g or less, more specifically 1 to 3 m 2 / g or 1.5 to 2.7 m 2 / g can be in the range.

[0055] In addition, the tap density of the second negative electrode active material may be 0.81 g / cc or higher, more specifically in the range of 0.81 to 2.5 g / cc, 1.0 to 2.0 g / cc, or 1.0 to 1.5 g / cc.

[0056] When the BET specific surface area and tap density satisfy the above range, when the first cathode active material is mixed with the second cathode active material as in the present embodiment, the BET and orientation can be appropriately implemented to satisfy the range of the present embodiment.

[0057] The above second negative electrode active material may have an average particle size (D50) of 10 to 20 μm, more specifically 12 to 18 μm or 13 to 17 μm. When the average particle size (D50) of the second negative electrode active material satisfies the above range, a negative electrode active material can be manufactured by mixing it with the first negative electrode active material in an appropriate ratio, thereby suppressing side reactions in the electrolyte while producing a lithium secondary battery with excellent output characteristics.

[0058] Meanwhile, the BET (Brunauer-Emmett-Teller) specific surface area of ​​the negative electrode active material of the present embodiment is 3.5 to 4.5 m² 2 / g can be in the range.

[0059] In addition, the negative electrode active material of this embodiment may have an orientation peak intensity ratio (I110 / I004) in the range of 70 to 85 when analyzing the XRD pattern.

[0060] When the specific surface area and orientation peak intensity satisfy the above ranges, a lithium secondary battery with excellent electrochemical properties and improved stability can be realized.

[0061] As described above, in this embodiment, by including a first negative electrode active material having a tap density of 0.80 g / cc or less and a second negative electrode active material having a tap density of 0.81 g / cc or more, a negative electrode active material with excellent lifespan and output characteristics and reduced swelling occurrence rate can be realized.

[0063] Method for manufacturing a negative electrode active material for a lithium secondary battery

[0064] A method for manufacturing a negative electrode active material for a lithium secondary battery according to another embodiment may be manufactured by mixing a first negative electrode active material and a second negative electrode active material.

[0065] At this time, the first cathode active material may be manufactured by a method comprising the steps of: preparing primary particles having an average particle size (D50) of 3 to 5 μm; mixing the primary particles and the first amorphous carbon to produce a mixture; pressurizing the mixture at a temperature of 50°C or higher to produce a molded body; crushing the molded body; and heat-treating the crushed molded body.

[0066] The second cathode active material may be manufactured by a method comprising the steps of: spherizing natural graphite powder into high-density spheres; and mixing and coating the high-density spherical natural graphite powder with a second amorphous carbon.

[0067] Hereinafter, a method for manufacturing a negative electrode active material for a lithium secondary battery according to another embodiment will be described in detail step by step.

[0068] The method for manufacturing the first cathode active material is as follows.

[0069] First, a step of preparing primary particles having an average particle size (D50) of 3 to 5 μm can be performed.

[0070] Typically, the yield of the process for manufacturing commercial natural graphite is around 30%. By utilizing the fine particles generated during the process of manufacturing commercial natural graphite as the primary particles of this embodiment to manufacture the cathode active material, there is an advantage in that production costs can be reduced.

[0071] The average particle size of the primary particles may be in the range of 3 to 5 μm, more specifically 3.5 to 4.5 μm.

[0072] Next, a step of preparing a mixture by mixing primary particles and first amorphous carbon can be performed.

[0073] The BET (Brunauer-Emmett-Teller) specific surface area of ​​the above primary particle is 15 m² 2 / g or more, more specifically 15 m 2 / g to 30 m2 / g or 18 m 2 / g to 25 m 2 / g can be in the range.

[0074] In addition, the tap density of the primary particles may be in the range of 0.05 to 0.5 g / cc, more specifically 0.1 to 0.35 g / cc or 0.15 to 0.30 g / cc.

[0075] When the average particle size, BET, and tap density of the primary particles satisfy the above ranges, a cathode active material with excellent lifespan and output characteristics can be manufactured by the pressurization process described later.

[0076] The above primary particle may satisfy the following Equation 2.

[0077] [Equation 2]

[0078] 2.5 ≤ [D90] / [D10] ≤ 6.5

[0079] In Equation 2 above, [D10] and [D90] represent particle sizes corresponding to 10% and 90% of the volume accumulation of primary particles measured using the Laser Diffraction Method.

[0080] Equation 2 above is a value corresponding to the ratio of the particle size corresponding to 90% to the particle size corresponding to 10% of the volume accumulation of primary particles, and may be an indicator representing the uniformity of the particles.

[0081] If the value of Equation 2 above satisfies the above range, the average particle size, BET, and tap density of the first cathode active material described above can be easily controlled to the range of this embodiment.

[0082] The particle size (D10) corresponding to 10% of the volume accumulation of the primary particles may be 0.5㎛ to 3.0㎛, more specifically 1.0㎛ to 2.0㎛.

[0083] The particle diameter (D90) corresponding to 90% of the volume accumulation of the primary particles may be 5㎛ to 9㎛, more specifically 6㎛ to 8㎛.

[0084] By satisfying the volume accumulation amount of the primary particles within the aforementioned range, it is possible to manufacture a stable first negative electrode active material by mixing them, and by mixing this with a second negative electrode active material manufactured by the method described below, it is possible to manufacture a lithium secondary battery with excellent lifespan characteristics and output characteristics, while simultaneously reducing the swelling rate.

[0085] Next, the step of preparing a mixture by mixing the primary particles and the first amorphous carbon can be performed.

[0086] The type and content of the first amorphous carbon used in the preparation of the mixture are the same as those previously mentioned, so they will be omitted here.

[0087] Afterwards, the step of manufacturing a molded body by pressurizing the above mixture at a temperature of 50°C or higher can be performed.

[0088] The above pressurization may be a step of applying pressure to high-density spherical natural graphite powder, and may be isotropic pressurization. Through the above pressurization, voids within the cathode active material can be reduced to further decrease the pore size and increase the tap density of the active material. In addition, the specific surface area of ​​the active material can be efficiently reduced.

[0089] The above pressurization can be performed in a temperature range of 100°C to 300°C, more specifically 100°C to 200°C. When the pressurization process is performed to satisfy the above temperature range, the first amorphous carbon can be appropriately melted into a liquid state to increase the bonding force between the primary particles and can be evenly distributed on the surface of the primary particles, that is, inside the secondary particles.

[0090] Natural graphite with a small average particle size (D50) has a low density and a large specific surface area, which presents a problem in that a molded body is not formed well when assembled using a spheroidizer or a granulator. However, in this embodiment, as described above, by performing a pressurization process by simultaneously applying a certain temperature and pressure, a densely assembled molded body can be obtained in which the first amorphous carbon is evenly distributed within the molded body.

[0091] Next, the above pressurization can be performed at a pressure of 120 to 330 MPa, and more specifically, at a pressure of 140 to 310 MPa. When the pressure satisfies the above range during pressurization, the primary particles of the first cathode active material in this embodiment can be densely assembled, and at the same time, the pore size within the first cathode active material can be effectively reduced.

[0092] The above-mentioned pressurization can be performed through a Warm Isostatic Press (WIP) or a Hot Isostatic Press (HIP). In this case, the graphite can be pressed in a uniform direction, which may have the advantage of more preferably realizing effects such as improved orientation.

[0093] Afterwards, a step of crushing the above-mentioned molded body can be performed.

[0094] The above grinding step may be a step of grinding while controlling the particle size of the molded body.

[0095] In one embodiment, the grinding step may be controlled by physical impact. The physical impact may utilize equipment that utilizes physical impact, such as a pin mill, a jet mill, an air classifier mill (or air current classification mill), or a roller mill. The pin mill may grind particles by impact and shear caused by a rotating rotor equipped with fixed pins that rotates. The jet mill may grind particles directly by utilizing collisions between particles. The air classifier may grind particles or classify them according to specific gravity using an airflow. The roller mill may grind particles by feeding, compressing, and grinding them between two or more rollers rotating in opposite directions.

[0096] At this time, the grinding can be performed at a stirring speed of 1500 to 4500 rpm, and more specifically, at a stirring speed of 2000 to 4000 rpm. When the stirring speed during grinding satisfies the above range, the various physical properties, including the average particle size and tap density of the first cathode active material, can be more easily realized within the range according to the present embodiment.

[0097] Next, the step of manufacturing a negative electrode active material in the form of secondary particles containing multiple primary particles and having a coating layer formed on the surface can be performed by heat-treating the crushed molded body.

[0098] The above heat treatment step may include heat treatment at 900 to 1500°C in a gas atmosphere of hydrogen, nitrogen, argon, or a mixture thereof.

[0099] More specifically, the heat treatment temperature may be 950 to 1450℃, 1000 to 1400℃, or 1100 to 1300℃.

[0100] When the above heat treatment temperature falls within the aforementioned range, impurities remaining in the amorphous carbon can be removed and the binding force between primary particles can be further improved, and a negative electrode active material with excellent sphericity can be manufactured by properly binding.

[0101] In addition, if the heat treatment temperature is below the lower limit, impurities contained in the amorphous carbon are not effectively removed, which may result in a problem of low lithium ion conductivity of the negative electrode active material. Furthermore, if the heat treatment temperature exceeds the upper limit of the aforementioned range, there may be a problem of high process costs compared to the improvement in the physical properties and electrochemical characteristics of the negative electrode active material.

[0102] Next, the method for manufacturing the second cathode active material is as follows.

[0103] First, a step of sphericalizing natural graphite powder into high-density particles can be performed.

[0104] The above high-density spheroidization may include a step of first spheroidizing natural graphite powder; and a step of secondarily re-spheroidizing the first spheroidized natural graphite powder.

[0105] The step of first spheroidizing the natural graphite particles may involve spheroidizing plate-shaped natural graphite particles. The step of first spheroidizing the natural graphite particles may be spheroidized through a general method of spheroidizing plate-shaped graphite particles. Through the first spheroidization, the degree of spheroidization of the natural graphite raw material powder may be primarily improved.

[0106] The step of secondarily respherifying the first spherical natural graphite particles may be a step of further sphericalizing the first spherical natural graphite particles using a mechanical spherical method. Through secondary respherification, the degree of sphericity of the natural graphite can be maximized, the porosity can be reduced, and the degree of orientation (I110 / I004 orientation peak intensity ratio) and tap density can be improved.

[0107] The mechanical spheroidization method of the above secondary respheroidization can be performed through one or more methods selected from the group consisting of Air Classifying milling, Spheronizing milling, Grinding milling, mechanofusion milling, planetary milling, Hybridization milling, shape milling, and high speed milling.

[0108] The above secondary respheroidization can be performed at a rotational speed of 500 to 6000 rpm, and more specifically, at 700 to 4000 rpm or 800 to 2000 rpm. If the rotational speed is too slow during high-density spheroidization, the ratio of the degree of spheroidization and the orientation peak intensity (I110 / I004) of the natural graphite may be obtained to be too small. If the rotational speed is too fast during high-density spheroidization, the ratio of the degree of spheroidization and the orientation peak intensity (I110 / I004) of the natural graphite may be obtained to be large, but the natural graphite may be destroyed due to excessive processing.

[0109] Subsequently, a step of mixing and coating the high-density spherical natural graphite powder with a second amorphous carbon can be performed.

[0110] The second amorphous carbon may be of the same type as the first amorphous carbon or a different type. Since the type of the second amorphous carbon is the same as that of the first amorphous carbon, it will be omitted here.

[0111] Meanwhile, the amount of the second amorphous carbon added may be in the range of 1 to 20 weight% based on the total weight of the second negative electrode active material, more specifically, 1 to 10 weight% or 3 to 8 weight%. When the content of the second amorphous carbon satisfies the above range, other physical properties of the second negative electrode active material, such as BET and tap density, can be appropriately implemented to satisfy the range of this embodiment.

[0112] Next, the coating step can be performed by heat treatment at a temperature of 1000 to 1400°C, and more specifically, at a temperature of 1100 to 1300°C. If the coating heat treatment temperature is too low, there may be a problem of reduced performance due to side reactions with the electrolyte caused by functional groups remaining on the surface of the active material. If the coating heat treatment temperature is too high, process costs may increase.

[0113] In this embodiment, excellent electrochemical characteristics and stability can be secured by mixing a first cathode active material, which is manufactured by pressing primary particles with an average particle size (D50) of 3 to 5 μm at a temperature of 50°C or higher and then crushing them, and a second cathode active material, which is manufactured by high-density spherical shaping, in an appropriate ratio.

[0115] Cathode and lithium secondary battery

[0116] In another embodiment, a negative electrode for a lithium secondary battery comprising the aforementioned negative electrode active material is provided.

[0117] A negative electrode for a lithium secondary battery according to another embodiment of the present invention may more specifically include a negative electrode current collector; and a negative electrode active material layer located on the negative electrode current collector and comprising the aforementioned negative electrode active material for a lithium secondary battery.

[0118] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0119] The above-mentioned cathode active material layer may optionally include a binder and / or a conductive material together with the cathode active material.

[0120] The above binder serves to improve adhesion between negative electrode active material particles and adhesion between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The above binder may be included in an amount of 1 to 30 weight% based on the total weight of the negative electrode active material layer.

[0121] The above conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special restrictions as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The above conductive material may typically be included in an amount of 1 to 30 weight% relative to the total weight of the negative electrode active material layer.

[0122] A negative electrode for a lithium secondary battery according to one embodiment of the present invention can be manufactured according to a conventional negative electrode manufacturing method, except for using the negative electrode active material described above.

[0123] Specifically, it can be manufactured by applying a composition for forming a negative electrode active material layer, comprising the aforementioned negative electrode active material and optionally a binder, a conductive material, and a solvent, onto a negative electrode current collector, followed by rolling and drying. At this time, the types and contents of the negative electrode active material, binder, and conductive material are as described above.

[0124] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that dissolves or disperses the cathode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for cathode manufacturing.

[0125] Alternatively, the cathode may be manufactured by casting the composition for forming the cathode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto a cathode current collector.

[0127] Another embodiment of the present invention provides a lithium secondary battery comprising the negative electrode.

[0128] A lithium secondary battery according to another embodiment of the present invention may, more specifically, include a positive electrode, a negative electrode positioned opposite to the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

[0129] The above cathode is as described above.

[0130] Additionally, the lithium secondary battery may optionally further include a battery container housing an electrode assembly of a positive electrode, a negative electrode, and a separator, and a sealing member sealing the battery container.

[0132] The above positive electrode may include a positive current collector and a positive active material layer disposed on the positive current collector, and the positive active material layer may include a positive active material.

[0133] The above positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the positive current collector to increase the adhesion of the positive active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0134] As the above-mentioned cathode active material, a compound capable of reversibly intercalating and deintercalating lithium (a lithated intercalation compound) may be used. Specifically, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used, and specific examples thereof may include compounds represented by any one of the following chemical formulas:

[0135] Li a A 1-b B b D2(wherein 0.90 ≤ a ≤ 1.8, and 0 ≤ b ≤ 0.5); Li a E 1-b B b O 2-c D c (In the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); LiE 2-b B b O 4-c D c (In the above equation, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α(In the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Co b B c O 2-α T α (In the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Co b B c O 2-α T2(wherein, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c D α (In the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α ≤ 2); Li a Ni 1-b-c Mn b B c O 2-α T α (In the above equation, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni 1-b-c Mn b B c O 2-α T2(wherein, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05, 0 < α < 2); Li a Ni b E c G d O2(wherein 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0.001 ≤ d ≤ 0.1); Li a Ni b Co c Mn dGeO2(wherein the above formula, 0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0.001 ≤ e ≤ 0.1); Li a NiG b O2(in the above equation, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2(in the above equation, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a MnG b O2(in the above equation, 0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4(wherein 0.90 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0 ≤ f ≤ 2); Li (3-f) Fe2(PO4)3(0 ≤ f ≤ 2); and LiFePO4.

[0136] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; T is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I is Cr, V, Fe, Sc, Y, or a combination thereof; and J may be V, Cr, Mn, Co, Ni, Cu, or a combination thereof.

[0137] Of course, the compound having a coating layer on its surface or the compound having a coating layer may also be used in combination.

[0138] The above coating layer may include at least one coating element compound selected from the group consisting of oxides of coating elements, hydroxides of coating elements, oxyhydroxides of coating elements, oxycarbonates of coating elements, and hydroxycarbonates of coating elements. The compounds forming these coating layers may be amorphous or crystalline. As coating elements included in the above coating layer, Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof may be used. For the coating layer formation process, any coating method may be used as long as the compound can be coated using these elements in a way that does not adversely affect the physical properties of the cathode active material (e.g., spray coating, immersion method, etc.). Since this is a matter that is well understood by those engaged in the relevant field, a detailed explanation will be omitted.

[0139] The above positive active material layer may further include a binder and / or a conductive material together with the aforementioned positive active material.

[0141] The above binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof. One of these alone or a mixture of two or more may be used, but is not limited thereto. The above binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.

[0142] The above conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special limitations as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used, but is not limited thereto. The above conductive material may typically be included in an amount of 1 to 30 weight% relative to the total weight of the positive electrode active material layer.

[0143] The above anode can be manufactured according to a conventional anode manufacturing method.

[0144] Specifically, the anode can be manufactured by applying a composition for forming an anode active material layer, comprising an anode active material and optionally a binder, conductive material, or solvent as needed, onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the anode active material, binder, and conductive material are as described above.

[0145] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that allows for the dissolution or dispersion of the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.

[0146] Alternatively, the anode may be manufactured by casting the composition for forming the anode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.

[0148] The above separator separates the positive and negative electrodes and provides a pathway for the movement of lithium ions. It can be used without special restrictions as long as it is typically used as a separator in a lithium secondary battery, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.

[0150] The above electrolytes may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which can be used in the manufacture of lithium secondary batteries, but are not limited thereto.

[0151] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.

[0152] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.

[0153] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.

[0154] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, haloalkylene carbonate-based compounds like difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexamethylphosphate triamide, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the additive may be included in an amount of 0.1 to 5 weight% based on the total weight of the electrolyte.

[0155] As described above, since the lithium secondary battery containing the negative electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, it can be usefully applied to portable devices such as mobile phones, laptop computers, and digital cameras, as well as electric vehicles such as hybrid electric vehicles (HEVs).

[0157] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0159] Example 1

[0160] (1) Preparation of the first cathode active material

[0161] (Preparation of raw materials) Petroleum-based pitch was prepared using fine powder (primary particles) and amorphous carbon having particle size distribution, tap density, and BET values ​​as shown in Table 1 below.

[0162] (Mixing) A mixture was prepared by mixing the prepared fine powder and petroleum-based pitch. At this time, 10% by weight of petroleum-based pitch was mixed based on the mixture.

[0163] After (pressurization), the above mixture was filled into a molding mold, and a molded body was manufactured through a Warm Isostatic Press (WIP) process. At this time, the applied pressure was 300 MPa, the temperature was 150℃, and the execution time was 5 minutes.

[0164] After (grinding), the molded body was ground using a pin mill to produce a negative electrode active material with an average particle size (D50) of 11.9 μm. At this time, the stirring speed during pin milling was set to 3000 rpm.

[0165] (Heat treatment) Next, the crushed molded body was heat-treated at a temperature of 1200°C for 12 hours.

[0166] (2) Preparation of second cathode active material

[0167] (Preparation of natural graphite powder and high-density spheroidization) A primary spheroidized natural graphite powder with an average particle size (D50) of 16 μm was prepared. Subsequently, the natural graphite powder was subjected to a secondary mechanical spheroidization treatment at 1,000 rpm for 15 minutes in a spheroidizer, and fine and coarse particles were removed through air stream classification and sieving classification to produce a re-spheroidized high-density spheroidized natural graphite powder with an average particle size (D50) of 14.3 μm.

[0168] After (coating), high-density spherical natural graphite powder and petroleum-based pitch were mixed, and a coating heat treatment was performed at a temperature of 1200°C for 12 hours to produce a natural graphite negative electrode active material with a coating layer formed. At this time, the amount of petroleum-based pitch added was appropriately adjusted so that the amorphous carbon was 5% by weight based on the total weight of the negative electrode active material.

[0169] (3) Preparation of cathode active material

[0170] A negative electrode active material was prepared by mixing 30 wt% of the first negative electrode active material and 70 wt% of the second negative electrode active material based on the total weight of the negative electrode active material.

[0171] (4) Cathode manufacturing

[0172] A negative electrode active material powder produced by the above method, a conductive material, a binder (styrene butadiene rubber - SBR), and a thickener (carboxymethylcellulose - CMC) were mixed in a mass ratio of 96.3:1:1.5:1.2, and water was added to prepare a negative electrode active material slurry. The negative electrode active material slurry was coated onto a copper (Cu) foil current collector, and then dried and rolled to manufacture a negative electrode. At this time, the loading of the negative electrode was 3.6 mAh / cm² 2 It was manufactured to be this way.

[0173] (5) Lithium secondary battery manufacturing

[0174] As a positive electrode active material, NCM (Ni 65 wt%), a conductive material, and KF1100 as a binder were mixed in a weight ratio of 96:2:2, and water was added to prepare a positive electrode slurry. The positive electrode slurry was coated onto aluminum foil, and the electrode was manufactured by vacuum drying and rolling at approximately 120°C for 12 hours. At this time, the loading of the positive electrode was 3.3 mAh / cm² 2 It was manufactured to be this way.

[0175] At this time, a separator made of a porous polypropylene film was inserted between the working electrode and the counter electrode, and as the electrolyte, a mixed solvent was used in which 0.5 wt% of vinylene carbonate (VC) and 1.5 wt% of propane sulfone (PS) were added to the solvent and 1.2 M concentration of LiPF6 was dissolved, with the mixed volumes of ethylene carbonate (EC), propylene carbonate (PC), ethylmethyl carbonate (EMC), and dimethyl carbonate (DMC) having a mixture volume ratio of 25:5:30:35.

[0176] division D10 (㎛) D50(㎛) D90(㎛) Tap density (g / cc) BET(m 2 / g) differential 1.6 4 7 0.21 21.1

[0177] Example 2

[0178] A negative electrode active material and a lithium secondary battery were manufactured in the same manner as in Example 1, except that 20% by weight of petroleum-based pitch was mixed based on the total mixture during the mixing step when manufacturing the first negative electrode active material.

[0180] Comparative Example 1

[0181] (Preparation of raw materials) Petroleum-based pitch was prepared using first graphite and amorphous carbon.

[0182] At this time, the first graphite was prepared by first spheroidizing natural graphite to obtain spherical graphite powder with an average particle size (D50) of 16 μm, and second spheroidization was performed. Specifically, the second spheroidization was performed by treating the spherical graphite powder in a spheronizer at 1000 rpm for 15 minutes. Then, fine and coarse particles were removed through air flow classification and sieving to obtain a high-density spherical product.

[0183] (Mixing) The prepared first graphite and amorphous carbon were mixed. At this time, the mixture was prepared so that the content of petroleum-based pitch was 5% by weight based on the total negative electrode active material.

[0184] (Heat treatment) Next, the above mixture was heat-treated at a temperature of 1200°C for 12 hours to produce a negative electrode active material.

[0186] Experimental Example 1: Evaluation of Cathode Active Material Properties

[0187] (1) Measurement of the ratio of small particles smaller than 5㎛ in the cathode active material using SEM images

[0188] After obtaining an image of the cathode active material prepared according to the above examples and comparative examples at 10,000x magnification and 10kV conditions using a Scanning Electron Microscopy (SEM) analysis device, the ratio of small particles with a diameter of 5㎛ or less was measured based on the scale bar.

[0189] (2) Particle size evaluation

[0190] The particle sizes corresponding to 10%, 50%, 90%, and the maximum value of the volume accumulation of the cathode active material were measured using the laser diffraction method.

[0191] (3) Tap density evaluation

[0192] Tap density was measured using the AT-2 model from Quantachrome. The sample was filled into a test container with a volume of 20 ml, tapped 3,000 times, and then the volume and weight of the sample were measured.

[0193] (4) Specific surface area evaluation

[0194] The specific surface area was measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).

[0195] (5) Orientation measurement

[0196] The area ratio (I110 / I004) was calculated by integrating the peak intensities of the XRD spectra attributable to the (110) plane and (004) plane of the graphite crystal in the XRD pattern obtained from X-ray diffraction measurements. More specifically, the XRD measurement conditions are as follows.

[0197] - Target: Cu(Kα-line) graphite monochromator

[0198] - Slit: Diverging slit = 1 degree, Receiving slit = 0.1 mm, Scattering slit = 1 degree

[0199] - Measurement area and step angle / measurement time:

[0200] - (110) Surface: 76.5 degrees < 2θ < 78.5 degrees, 0.1 degrees / 4.2 seconds

[0201] - (004) plane: 53.5 degrees < 2θ < 56.0 degrees, 0.1 degrees / 4.2 seconds, where 2θ represents the diffraction angle.

[0202] division Second cathode active material (weight%) First cathode active material (weight%) Amorphous carbon content (weight%) of the first cathode active material ~5um (%) D10 (㎛) D50(㎛) D90(㎛) Dmax (㎛) Tap density (g / cc) BET(m2 / g) Orientation (I110 / I004) Example 1 70 30 10 5.5 6.5 14.3 22.7 36 1.05 3.0 76 Example 2 70 30 20 5.6 6.6 14.2 22.6 36 1.04 2.7 80 Comparative Example 1 100 - - 1.5 9.3 14.4 20.9 32 1.17 2.1 -

[0203] Referring to Table 2, it can be seen that the negative electrode active materials of Examples 1 and 2 are appropriately implemented to satisfy the range of this example in terms of particle ratio of 5 μm or less, average particle size, tap density, specific surface area, and shape.

[0205] Experimental Example 2: Evaluation of Electrochemical Characteristics of Lithium Secondary Battery

[0206] (1) Evaluation of initial capacity and initial efficiency

[0207] After fabricating a lithium secondary battery full cell, it was aged at 25°C for 12 hours, and then a charge-discharge test was performed at 25°C. To evaluate the initial capacity, the reference capacity was set to 200 mAh / g, and the battery was charged to 4.25V with a constant current of 0.1C. Then, the voltage was switched to a constant voltage, and charging continued until the terminal current reached 0.05C. After a 10-minute rest time following charging, the battery was discharged until it reached 2.5V with a constant current of 0.1C and a reference capacity of 200 mAh / g.

[0208] (2) Evaluation of output characteristics

[0209] After completing the formation process of the manufactured lithium secondary battery under constant current / constant voltage (CC / CV) conditions at 25°C, the SOC at which lithium metal is electrodeposited was measured by charging under constant current (CC) conditions at a 3C-rate.

[0210] (3) Measurement of the thickness expansion rate of the cathode

[0211] A lithium secondary battery prepared using the negative electrode active material prepared according to Examples 1 and 2 and Comparative Example 1 was charged and discharged 30 times at a rate of 0.5C, and then the battery was recharged to a fully charged state and disassembled. The negative electrode was recovered from the disassembled battery, washed with DEC (diethyl carbonate), and then dried.

[0212] Next, the thickness expansion rate of the cathode before and after charging and discharging was measured using a micrometer, and the results are shown in Table 3.

[0214] division Capacity (mAh / g) Efficiency (%) Output characteristics 3C-rate SOC(%) Expansion rate (%) Example 1 357.4 90.3  41 20 Example 2 356.7 89.7  41 21 Comparative Example 1 360.7 91.9  38 24

[0215] Referring to Table 2, it can be seen that the cathode active materials of Example 1 and Example 2, which include the second cathode active material manufactured by a high-density spherical process and the first cathode active material manufactured by a warm hydrostatic pressing method, have excellent capacity while also improving output characteristics and swelling characteristics.

[0216] In contrast, Comparative Example 1, which uses a negative electrode active material manufactured by a high-density spherical process, has excellent capacity but is inferior to the examples in terms of output characteristics and swelling characteristics.

[0217] Therefore, the negative electrode active material of the present embodiment, comprising a first negative electrode active material manufactured by a high-density spherical process and a second negative electrode active material manufactured by a warm hydrostatic pressing method in an appropriate ratio, has a very advantageous effect in that it can realize a lithium secondary battery with excellent output and swelling characteristics while securing excellent capacity.

[0219] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.

Claims

Claim 1 A negative electrode active material for a lithium secondary battery comprising: a first negative electrode active material having a tap density of 0.80 g / cc or less; and a second negative electrode active material having a tap density of 0.81 g / cc or more; wherein the first negative electrode active material has an orientation peak intensity ratio (I110 / I004) of 75 or more when analyzing an XRD pattern, and the first negative electrode active material comprises natural graphite particles in the form of secondary particles including primary particles having an average particle size (D50) of 3 to 5 μm, and a first coating layer located on the surface of the natural graphite particles, and the second negative electrode active material comprises natural graphite and a second coating layer located on the surface of the natural graphite. Claim 2 A negative electrode active material for a lithium secondary battery according to claim 1, wherein the interior of the natural graphite particles in the form of secondary particles of the first negative electrode active material and the first coating layer comprise first amorphous carbon. Claim 3 A negative electrode active material for a lithium secondary battery according to claim 2, wherein the content of the first amorphous carbon is in the range of 1% to 30% by weight based on the total weight of the first negative electrode active material. Claim 4 In claim 1, the BET (Brunauer-Emmett-Teller) specific surface area of ​​the first cathode active material is 3 m² 2 Negative electrode active material for lithium secondary batteries, having a g or more. Claim 5 A negative electrode active material for a lithium secondary battery according to claim 1, wherein the tap density of the first negative electrode active material is 0.10 g / cc to 0.80 g / cc. Claim 6 In claim 1, the first negative electrode active material is a negative electrode active material for a lithium secondary battery satisfying the following Equation 1. [Equation 1] 2.5 ≤ [D90] / [D10] ≤ 6.5 (wherein Equation 1, [D10] and [D90] represent particle sizes corresponding to 10% and 90% of the cumulative volume of the first negative electrode active material measured using the Laser Diffraction Method). Claim 7 A negative electrode active material for a lithium secondary battery according to claim 1, wherein the average particle size (D50) of the first negative electrode active material is 10 to 13 μm. Claim 8 A negative electrode active material for a lithium secondary battery, wherein the second coating layer of the second negative electrode active material comprises second amorphous carbon. Claim 9 A negative electrode active material for a lithium secondary battery according to claim 8, wherein the content of the second amorphous carbon is in the range of 1 to 20 weight% based on the total weight of the second negative electrode active material. Claim 10 In claim 1, the BET (Brunauer-Emmett-Teller) specific surface area of ​​the second cathode active material is 3 m² 2 Negative electrode active material for lithium secondary batteries, with a g or less. Claim 11 A negative electrode active material for a lithium secondary battery according to claim 1, wherein the tap density of the second negative electrode active material is 1.0 g / cc or more. Claim 12 A negative electrode active material for a lithium secondary battery according to claim 1, wherein the weight ratio of the first negative electrode active material and the second negative electrode active material is in the range of 1:9 to 5:

5. Claim 13 In claim 1, the BET (Brunauer-Emmett-Teller) specific surface area of ​​the cathode active material is 3.5 to 4.5 m² 2 Negative active material for lithium secondary batteries in the range of / g. Claim 14 In claim 1, the negative electrode active material is a negative electrode active material for a lithium secondary battery having an orientation peak intensity ratio (I110 / I004) in the range of 70 to 85 when analyzed by XRD pattern. Claim 15 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein the negative electrode active material is manufactured by mixing a first negative electrode active material and a second negative electrode active material, the first negative electrode active material is manufactured by a step of preparing primary particles having an average particle size (D50) of 3 to 5 μm; a step of mixing the primary particles and a first amorphous carbon to manufacture a mixture; a step of pressurizing the mixture at a temperature of 100°C to 300°C to manufacture a molded body; a step of grinding the molded body; and a step of heat-treating the ground molded body; and the second negative electrode active material is manufactured by a method comprising a step of sphericalizing natural graphite powder to a high density; and a step of coating the high-density sphericalized natural graphite powder by mixing it with a second amorphous carbon. Claim 16 A method for manufacturing a negative electrode active material for a lithium secondary battery according to claim 15, wherein the mixing weight ratio of the first negative electrode active material and the second negative electrode active material is in the range of 1:9 to 5:

5. Claim 17 In paragraph 15, the BET (Brunauer-Emmett-Teller) specific surface area of ​​the primary particle is 15 m² 2 A method for manufacturing a negative electrode active material for a lithium secondary battery, having a content of / g or more. Claim 18 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 15, the tap density of the primary particles is in the range of 0.05 to 0.5 g / cc. Claim 19 A method for manufacturing a negative electrode active material for a lithium secondary battery according to claim 15, wherein the primary particles satisfy the following Equation 2. [Equation 2] 2.5 ≤ [D90] / [D10] ≤ 6.5 (wherein Equation 2, [D10] and [D90] represent particle diameters corresponding to 10% and 90% of the cumulative volume of the primary particles measured using the Laser Diffraction Method). Claim 20 delete Claim 21 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 15, the above-mentioned pressurization is performed in a pressure range of 120 to 330 MPa. Claim 22 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 15, the above-mentioned pressurization is performed using a Warm Isostatic Press (WIP) or a Hot Isostatic Press (HIP). Claim 23 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 15, the grinding is performed at a stirring speed of 1500 to 4500 rpm. Claim 24 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 15, the heat treatment is performed at a temperature of 900 to 1500℃. Claim 25 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 15, the high-density spheroidization comprises: a step of first spheroidizing natural graphite powder; and a step of secondarily re-spheroidizing the first spheroidized natural graphite powder. Claim 26 A method for manufacturing a negative electrode active material for a lithium secondary battery, wherein, in claim 15, the coating step is performed by heat treatment at a temperature of 1000 to 1400℃. Claim 27 A negative electrode for a lithium secondary battery comprising the negative electrode active material of claim 1. Claim 28 A lithium secondary battery comprising a negative electrode for a lithium secondary battery according to claim 27.

Citation Information

Patent Citations

  • Carbon material for nonaqueous secondary battery and nonaqueous secondary battery

    JP2015185443A

  • Negative electrode active material for rechargeable lithium battery, method for preparing the same, negative electrode including the same, and rechargeable lithium battery including the negative electrode

    KR1020140140952A

  • Negative electrode active material, method for manufacturing the same, negative electrode and secondary battery comprising the same

    KR1020210071836A

  • Negative active material for rechargeable lithium battery, method of preparing same, and rechargeable lithium battery including the same

    KR1020210111568A

  • Negative electrode for lithium secondary battery and lithium secondary battery comprising the same