Manufacturing method of cathode active material precursor for lithium secondary battery

By controlling co-precipitation conditions with specific ammonia and caustic soda ratios, the method improves lithium ion mobility and electrochemical performance of cathode active materials made from recycled lithium secondary battery materials, addressing impurity-related performance degradation.

KR103046673B1Active Publication Date: 2026-11-10RES INST OF IND SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020220113581
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-09-07
Publication Date
2026-11-10
Estimated Expiration
2042-09-07

Smart Images

  • Figure 112022094449659-PAT00003_ABST
    Figure 112022094449659-PAT00003_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a positive electrode active material precursor for a lithium secondary battery from a spent lithium secondary battery, comprising the steps of: preparing a recycled liquid raw material containing a liquid nickel raw material, a cobalt raw material, and a manganese raw material extracted from a spent lithium secondary battery, wherein the impurity content of each of the nickel raw material, the cobalt raw material, and the manganese raw material is 100 ppm or more; forming a transition metal-containing solution containing the recycled liquid raw material; and introducing the transition metal-containing solution, an ammonia solution, and a caustic soda solution into a reactor to form a reaction solution, and co-precipitating the reaction solution to form a positive electrode active material precursor for a lithium secondary battery, wherein the ratio of the number of moles of ammonia contained in the ammonia solution to the number of moles of transition metal elements contained in the transition metal-containing solution is 1.0 to 1.6.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a positive electrode active material precursor for a lithium secondary battery, a positive electrode active material precursor for a lithium secondary battery, a positive electrode active material, and a lithium secondary battery including the same. More specifically, the invention relates to a method for manufacturing a positive electrode active material precursor for a lithium secondary battery using liquid recycled raw materials extracted from waste lithium secondary batteries, a positive electrode active material precursor for a lithium secondary battery, a positive electrode active material, and a lithium secondary battery including the same. Background Technology

[0003] With the recent increase in demand for electric vehicles and medium-to-large energy storage devices, as well as for small electronic devices such as smartphones, laptops, and tablet PCs, the demand for secondary batteries capable of storing electrical energy is rapidly increasing.

[0004] In particular, the use of LiNiCoMnO2 (NCM), a ternary cathode active material, is expected to increase significantly in high-capacity lithium-ion batteries for electric vehicles. As the production and usage of lithium-ion batteries increase, so will the amount of waste, thus highlighting the need for reprocessing and recycling technologies for spent lithium-ion batteries. Furthermore, the secondary battery and materials industries are not only making efforts to lower costs through raw materials, low-cost processes, and yield improvements, but are also increasingly attempting to recycle spent batteries, defective products generated during the manufacturing process, and electrodes as the demand for secondary batteries grows.

[0005] However, battery raw materials obtained through recycling processes have a problem of high impurity content compared to conventional battery materials such as nickel sulfate, cobalt sulfate, and manganese sulfate. Furthermore, when manufacturing cathode materials using these raw materials, the presence of impurities within the structure inhibits the movement of lithium, consequently suppressing the movement of lithium ions within the electrode. This leads to a significant degradation in the electrochemical performance of lithium secondary batteries, including capacity, diffusion coefficient, resistance, and output characteristics. The problem to be solved

[0007] In order to solve the aforementioned problems, one objective of the present invention is to provide a method for manufacturing a cathode active material precursor for a lithium secondary battery, which can obtain a cathode active material precursor with excellent electrochemical performance even when manufactured using liquid nickel, cobalt, and manganese raw materials containing a large amount of impurities extracted from spent lithium secondary batteries.

[0008] Another objective of the present invention is to provide a positive electrode active material precursor for a lithium secondary battery manufactured through the above-described manufacturing method.

[0009] Another objective of the present invention is to provide a positive electrode active material for a lithium secondary battery formed using the positive electrode active material precursor for a lithium secondary battery, and a lithium secondary battery including the same. means of solving the problem

[0011] To achieve the aforementioned objective, one embodiment of the present invention provides a method for manufacturing a positive electrode active material precursor for a lithium secondary battery from a spent lithium secondary battery, comprising the steps of: preparing a recycled liquid raw material containing a liquid nickel raw material, a cobalt raw material, and a manganese raw material extracted from a spent lithium secondary battery, wherein the impurity content of each of the nickel raw material, the cobalt raw material, and the manganese raw material is 100 ppm or more; dissolving the recycled liquid raw material in a solvent to form a transition metal-containing solution; and introducing the transition metal-containing solution, an ammonia solution, and a caustic soda solution into a reactor to form a reaction solution, and co-precipitating the reaction solution to form a positive electrode active material precursor for a lithium secondary battery, wherein the ratio of the number of moles of ammonia contained in the ammonia solution to the number of moles of transition metal elements contained in the transition metal-containing solution is 1.0 to 1.6.

[0012] In the step of preparing the above-mentioned recycled liquid raw material, the impurity content of each of the nickel raw material, cobalt raw material and manganese raw material may be 100 to 500 ppm.

[0013] The concentration of the transition metal element in the above transition metal-containing solution may be 2.3 to 2.6 M.

[0014] The pH of the above reaction solution may be 11.1 to 11.3. Effects of the invention

[0016] A method for manufacturing a cathode active material precursor for a lithium secondary battery according to one embodiment of the present invention can produce a cathode active material precursor having excellent electrochemical performance and a cathode active material formed therefrom by controlling the co-precipitation reaction conditions, even when using liquid nickel raw material, cobalt raw material, and manganese raw material containing a large amount of impurities extracted from a spent lithium secondary battery. Brief explanation of the drawing

[0018] Figure 1 shows the results of component analysis (ICP analysis results) of the normal raw material of the battery grade used in the manufacture of the positive electrode active material and the recycled raw material obtained through the battery recycling process. Specific details for implementing the invention

[0019] Hereinafter, embodiments of the present invention will be described clearly and in detail with reference to the attached drawings so that those skilled in the art can easily implement the present invention. However, this is presented as an example and is not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0020] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0021] In this specification, expressions such as "comprising" should be understood as open-ended terms implying the possibility of including other embodiments.

[0022] In this specification, "preferred" or "preferably" refers to an embodiment of the invention that can provide a certain advantage under a certain environment. However, other embodiments may also be preferred under the same or different environments. Additionally, the mention of one or more preferred embodiments does not imply that other embodiments are not useful, nor is it intended to exclude other embodiments from the scope of the invention.

[0023] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.

[0024] In this specification, the description "A and / or B" means A or B or both.

[0026] 1. Method for manufacturing a cathode active material precursor for a lithium secondary battery

[0027] Conventional methods for synthesizing NCM cathode materials using recycled raw materials are manufactured using general cathode material synthesis methods, but applying general synthesis methods leads to performance degradation. When applying conventional general precursor manufacturing technology, a large amount of nucleation occurs due to impurities during the co-precipitation process, resulting in a reduction in particle size and the production of non-oriented precursors, which causes a significant decrease in performance when manufacturing cathode active materials.

[0028] Figure 1 shows the results of component analysis (ICP analysis results) of the normal raw material of the battery grade used in the manufacture of the positive electrode active material and the recycled raw material obtained through the battery recycling process.

[0029] The solid recycled raw material shown in Fig. 1 represents the final product that has gone through all stages of the recycling process, and the liquid recycled raw material refers to a raw material that does not include the final crystallization stage. As shown in Fig. 1, it can be confirmed that the impurity content of the recycled raw material is high at the level of several hundred ppm compared to the normal raw material, and it can be anticipated that such impurity content may be significantly related to performance degradation during the manufacture of cathode materials.

[0030] The present invention aims to provide a method to significantly enhance the performance of existing recycled materials by changing the structure of a precursor to overcome their problems.

[0031] More specifically, cathode materials generally possess a layered structure, and layered precursors are calcined to realize this structure. The unit cell structure of a layered precursor can be represented by the lengths in the horizontal and vertical directions as 'a' and the height as 'c'; the physical properties of the material change significantly depending on variations in the values ​​of 'a' and 'c' that characterize this crystal structure. It is generally known that Li mobility increases as the length of the c-axis increases. However, when cathode materials are manufactured using recycled raw materials via generally known methods, it has been observed that the length of the precursor's c-axis decreases due to impurities, which is considered a major factor in performance degradation.

[0032] The present invention relates to a method for dramatically improving the performance of a cathode material obtained using a liquid regenerated raw material, and aims to achieve this objective by controlling the c-axis length of a co-precipitated precursor without applying doping or calcination optimization to increase the c-axis length of the cathode material.

[0033] To achieve this objective, a specific co-precipitation region was discovered where the c-axis length increases by utilizing a precursor solution with high impurity content. Furthermore, when co-precipitation was performed using recycled raw materials, a region was identified that enhances the crystallization growth mechanism and minimizes agglomeration. It was confirmed that under these process conditions, the c-axis length of the precursor using the recycled solution increased significantly, and the performance of the cathode material improved. In particular, a phenomenon was observed where the c-axis structure of the precursor expanded significantly within a specific range of the input ammonia amount, a specific concentration of the transition metal-containing solution, and a specific pH range of the co-precipitation reaction solution. When cathode active materials were manufactured using precursors produced under these specific conditions, the lithium diffusion coefficient increased, resistance characteristics decreased, and electrochemical performance improved. Under these novel co-precipitation conditions, impurities are incorporated into the precursor, and the interaction between ammonia and metals is optimized, leading to an increase in the c-axis. Consequently, cathode materials utilizing precursors produced through this process exhibit increased Li mobility. In the case of products using recycled liquid raw materials, optimized performance of the cathode active material precursor and cathode active material can be achieved by applying the co-precipitation reaction conditions according to the present invention, particularly using a recycled liquid solution with an impurity content of 100 to 500 ppm. In particular, when this technology is applied, it was confirmed that the performance was actually improved compared to products using conventional raw materials.

[0035] Accordingly, one embodiment of the present invention provides a method for manufacturing a positive electrode active material precursor for a lithium secondary battery from a spent lithium secondary battery, comprising the steps of: preparing a recycled liquid raw material containing a liquid nickel raw material, a cobalt raw material, and a manganese raw material extracted from a spent lithium secondary battery, wherein the impurity content of each of the nickel raw material, the cobalt raw material, and the manganese raw material is 100 ppm or more; forming a transition metal-containing solution containing the recycled liquid raw material; and introducing the transition metal-containing solution, an ammonia solution, and a caustic soda solution into a reactor to form a reaction solution, and co-precipitating the reaction solution to form a positive electrode active material precursor for a lithium secondary battery, wherein the ratio of the number of moles of ammonia contained in the ammonia solution to the number of moles of transition metal elements contained in the transition metal-containing solution is 1.0 to 1.6.

[0037] A method for manufacturing a positive electrode active material precursor for a lithium secondary battery according to one embodiment of the present invention will be described in detail step by step below.

[0039] First, a recycled liquid raw material is prepared that includes liquid nickel raw material, cobalt raw material, and manganese raw material extracted from waste lithium secondary batteries, wherein the impurity content of each of the nickel raw material, cobalt raw material, and manganese raw material is 100 ppm or more.

[0040] More specifically, in the step of preparing the recycled liquid raw material, the impurity content of each of the nickel raw material, cobalt raw material and manganese raw material may be 100 to 500 ppm, 200 to 500 ppm, 300 to 500 ppm, 400 to 500 ppm, or 450 to 500 ppm.

[0041] The above nickel raw material is not particularly limited as long as it is used in the industry for manufacturing a cathode active material precursor. For example, the above nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, it may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, nickel fatty acid salt, nickel halide, or a combination thereof, but is not limited thereto.

[0042] The above-mentioned cobalt raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors. For example, the above-mentioned cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, CoSO₄ 4, It may be CoSO4·7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or a combination thereof, but is not limited thereto.

[0043] The above manganese raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors. For example, the above manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof. Specifically, it may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.

[0045] Next, a transition metal-containing solution containing the above-mentioned recycled liquid raw material is formed.

[0046] The above transition metal-containing solution may be prepared by adding nickel raw material, cobalt raw material, and manganese raw material contained in recycled liquid raw material to a solvent, specifically water or a mixed solvent of an organic solvent that can be uniformly mixed with water (e.g., alcohol, etc.), or by mixing an aqueous solution of nickel raw material, an aqueous solution of cobalt raw material, and manganese raw material.

[0047] Meanwhile, the above transition metal-containing solution may contain nickel in an amount of 60 to 99 atm%, 70 to 99 atm%, 80 to 99 atm%, 85 to 99 atm%, 90 to 99 atm%, or 90 to 95 atm% among the total transition metals.

[0048] In addition, the transition metal-containing solution may contain cobalt in an amount of 0 to 30 atm%, 1 to 20 atm%, 1 to 10 atm%, 2 to 8 atm%, or 2 to 6 atm% among the total transition metals.

[0049] In addition, the transition metal-containing solution may contain manganese among the total transition metals in an amount greater than 0 and less than or equal to 30 atm%, 1 to 20 atm%, 1 to 10 atm%, 2 to 8 atm%, or 2 to 6 atm%.

[0051] Next, the transition metal-containing solution, ammonia solution, and caustic soda solution are introduced into a reactor to form a reaction solution, and the reaction solution is subjected to a co-precipitation reaction to form a positive electrode active material precursor for a lithium secondary battery.

[0052] The above ammonia solution may include, for example, NH3, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3, or a combination thereof as a complex-forming agent, but is not limited thereto. Meanwhile, the above ammonia solution may be used in the form of an aqueous solution, in which case water or a mixture of water and an organic solvent that is uniformly miscible with water (specifically, alcohol, etc.) may be used as the solvent.

[0053] The above caustic soda solution may include alkali compounds such as hydroxides of alkali metals or alkaline earth metals like NaOH, KOH, or Ca(OH)2, their hydrates, or combinations thereof, as a precipitating agent or pH adjuster. The above caustic soda solution may also be used in the form of an aqueous solution, in which case water or a mixture of water and an organic solvent that is uniformly miscible with water (specifically, alcohol, etc.) may be used as the solvent.

[0054] The above co-precipitation reaction can be carried out under an inert atmosphere such as nitrogen or argon.

[0055] The above co-precipitation reaction can be carried out at a temperature inside the reactor of 30 to 70°C, specifically 40 to 60°C, and more specifically 45 to 55°C.

[0057] In particular, the ratio of the number of moles of ammonia contained in the ammonia solution to the number of moles of transition metal elements contained in the transition metal-containing solution is 1.0 to 1.6, and more specifically, it may be 1.4 to 1.6.

[0058] If the ratio of the number of moles of ammonia in the ammonia solution to the number of moles of transition metal elements in the transition metal-containing solution is too small or too large, the C-axis length of the active material precursor may be short, and the growth of the (001) crystal plane may occur excessively. Specifically, if the C-axis length is short, a problem may arise in which the mobility of Li is reduced. Also specifically, the (001) crystal plane corresponds to the (003) crystal plane of the positive electrode active material manufactured using it, and the (003) crystal plane of the positive electrode active material does not function as a path for the movement of lithium ions due to its thermodynamically stable and electrochemically inert characteristics. Therefore, as the ratio of the number of moles of ammonia is controlled within the above range, the mobility of lithium ions is improved, and the capacity, resistance characteristics, and output characteristics of the lithium secondary battery can be further improved.

[0060] In addition, the concentration of the transition metal element in the above transition metal-containing solution may be 2.3 to 2.6 M, and more specifically, 2.5 to 2.6 M.

[0061] If the concentration of transition metal elements is too low or too high, the C-axis length of the active material precursor may be short, and the growth of the (001) crystal plane may occur excessively. Therefore, as the concentration of transition metal elements is controlled within the above range, the lithium ion mobility is improved, and the capacity, resistance characteristics, and output characteristics of the lithium secondary battery can be further improved.

[0063] In addition, the pH of the reaction solution may be 11.1 to 11.3.

[0064] If the pH of the reaction solution is too low or too high, the C-axis length of the active material precursor may be short, and the growth of the (001) crystal plane may occur excessively. Therefore, as the concentration of the transition metal element is controlled within the above range, the lithium ion mobility is improved, and the capacity, resistance characteristics, and output characteristics of the lithium secondary battery can be further improved.

[0066] 2. Cathode active material precursor for lithium secondary batteries

[0067] Another embodiment of the present invention comprises nickel and manganese, wherein the C-axis length (Lc) is 4.6261 Å or greater, and the grain size C in the (001) plane (001) Grain size C in the (100) plane for (100) C of non-human (100) / C (001) A positive electrode active material precursor for a lithium secondary battery is provided, wherein the value is 0.301 to 0.35.

[0068] The above-described positive active material precursor for a lithium secondary battery may be manufactured according to the method for manufacturing the aforementioned positive active material precursor.

[0070] The cathode active material precursor according to the present invention has a C-axis length (Lc) of 4.6261 Å or more, and more specifically, 4.6291 or 4.6294 Å or more, and 4.64 or 4.63 Å or less. As the C-axis length (Lc) increases, the lithium ion mobility is improved, and the capacity, resistance characteristics, and output characteristics of the lithium secondary battery can be further improved.

[0072] The positive active material precursor according to the present invention has a crystal grain size C in the (001) plane. (001) Grain size C in the (100) plane for (100) C of non-human (100) / C (001) α is 0.301 to 0.35, and more specifically, it may be 0.320 to 0.35 or 0.323 to 0.35. C (100) / C (001) If α is too small, it means that the growth of the (001) crystal plane occurs excessively, which reduces lithium ion mobility and may degrade the capacity, resistance, and output characteristics of the lithium secondary battery. C (100) / C (001)If α is too large, the movement distance of Li within the particle crystal becomes too long, which can lead to a problem where resistance increases rapidly.

[0074] The above-mentioned positive electrode active material precursor for a lithium secondary battery has a crystal grain size C in the (001) plane. (001) Grain size C in the (101) plane for (101) C of non-human (101) / C (001) α may be 1.033 to 1.05, and more specifically, may be 1.039 to 1.05 or 1.040 to 1.05. C (101) / C (001) If α is too small, it means that the growth of the (001) crystal plane occurs excessively, which reduces lithium ion mobility and may degrade the capacity, resistance, and output characteristics of the lithium secondary battery. C (101) / C (001) If α is too large, the movement distance of Li within the particle crystal becomes too long, which can lead to a problem where resistance increases rapidly.

[0076] The above-mentioned positive electrode active material precursor for a lithium secondary battery has a crystal grain size C in the (001) plane. (001) Grain size C in the (102) plane for (102) C of non-human (102) / C (001) ga may be 0.43 to 0.48, and more specifically, may be 0.447 to 0.48 or 0.449 to 0.48. C (102) / C (001) If α is too small, it means that the growth of the (001) crystal plane occurs excessively, which reduces lithium ion mobility and may degrade the capacity, resistance, and output characteristics of the lithium secondary battery. C (102) / C (001) If is too large, the displacement distance of Li in the ab plane (xy plane) direction within the particle crystal becomes too long, which can lead to a problem where resistance increases rapidly.

[0078] The above-mentioned positive electrode active material precursor for a lithium secondary battery can be represented by the following chemical formula 1.

[0079] [Chemical Formula 1]

[0080] Ni x1 Co y1 Mn z1 (OH)2

[0081] In the above chemical formula 1,

[0082] 0.6≤x1≤0.99, 0≤y1≤0.3, 0 <z1≤0.3 이다.

[0083] The above x1 represents the molar ratio of nickel among all metal elements in the transition metal hydroxide, and may be 0.6≤x1≤0.99, 0.7≤x1≤0.99, 0.80≤x1≤0.99, 0.85≤x1≤0.99, 0.90≤x1≤0.99, or 0.90≤x1≤0.95. When the nickel content in the transition metal hydroxide satisfies the above range, a positive electrode active material and a lithium secondary battery having high capacity characteristics can be manufactured.

[0084] The above y1 represents the molar ratio of cobalt among all metal elements in the transition metal hydroxide, and may be 0≤y1≤0.3, 0.01≤y1≤0.2, 0.01≤y1≤0.1, 0.02≤y1≤0.08, or 0.02≤y1≤0.06.

[0085] The above z1 represents the molar ratio of manganese among all metal elements in the transition metal hydroxide, where 0 <z1≤0.3, 0.01≤z1≤0.2, 0.01≤z1≤0.1, 0.02≤z1≤0.08 또는 0.02≤z1≤0.06일 수 있다.

[0087] 3. Cathode active material for lithium secondary batteries

[0088] Next, a positive electrode active material and a method for manufacturing the same according to another embodiment of the present invention will be described.

[0089] A positive electrode active material according to another embodiment of the present invention can be manufactured by the steps of: mixing the aforementioned positive electrode active material precursor and a lithium raw material to form a mixture; and calcining the mixture to form a lithium transition metal oxide.

[0090] The above lithium raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it is soluble in water. Specifically, the above lithium raw material may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a combination thereof, but is not limited thereto.

[0091] At this time, in the step of forming the above mixture, additional doping raw materials may be mixed.

[0092] The above doping raw material may be a doping raw material comprising Nb, Zr, Ti, Mg, Al, W, Mo, B, Ta, or a combination thereof.

[0093] The above firing can be performed at 600 to 900°C, and more specifically, at 600 to 800°C, 700 to 800°C, or 720 to 760°C.

[0094] The above firing can be performed for 5 to 20 hours, and more specifically, for 5 to 15 hours or 8 to 12 hours.

[0095] The above firing can be performed by dividing it into a first firing and a second firing as needed.

[0097] A positive electrode active material for a lithium secondary battery according to another embodiment of the present invention manufactured in this manner comprises a lithium transition metal oxide comprising nickel, cobalt, and manganese, has a c-axis length (Lc) of 14.1977 Å or more, and Lc / La, which is the ratio of the c-axis length (Lc) to the a-axis length (La), is 4.938 to 4.970.

[0098] The positive electrode active material for a lithium secondary battery according to the present invention has a c-axis length (Lc) of 14.1977 Å or more, and more specifically, may be 14.1980 Å or more, 14.1982 Å or more, or 14.1983 Å or more, and may be 15 Å or less, 14.6 Å or less, 14.4 Å or less, or 14.2 Å or less. If the c-axis length (Lc) of the positive electrode active material is too short, the lithium ion mobility is reduced, which may degrade the capacity, resistance characteristics, and output characteristics of the lithium secondary battery. If the c-axis length (Lc) of the positive electrode active material is too long, the resistance is high and the electrode capacity is low when Li is inserted into the electrode due to reduced interaction with the transition metal.

[0100] In addition, the positive electrode active material for a lithium secondary battery according to the present invention has a ratio of the c-axis length (Lc) to the a-axis length (La), Lc / La, which is 4.938 to 4.970, and more specifically, may be 4.94 to 4.970, 4.941 to 4.970, or 4.944 to 4.970. If Lc / La is too small, it means that the Lc value is small, which may lead to a decrease in lithium ion mobility and deterioration of the capacity, resistance characteristics, and output characteristics of the lithium secondary battery. If Lc / La is too large, the resistance becomes high and the electrode capacity becomes low when Li is inserted into the electrode due to a decrease in interaction with the transition metal.

[0103] Meanwhile, the cation mixing index ratio of nickel cations in the lithium layer within the structure of the lithium transition metal oxide may be 1.195 to 1.4, and more specifically, 1.20 to 1.4 or 1.21 to 1.3. If the cation mixing index ratio is too high, the layer of Li may easily collapse during charging and discharging, which significantly reduces battery cycle characteristics. If the cation mixing index ratio is too low, the irreversible sites in the bulk portion of the positive electrode active material may increase, which may lower lithium ion mobility and cause problems such as reduced resistance and output characteristics.

[0105] In addition, the Li slab distance of the lithium transition metal oxide may be 2.6093 to 2.6120 Å, and more specifically, 2.6100 to 2.6120 Å, 2.6111 to 2.6120 Å, or 2.6112 to 2.6120 Å. If the Li slab distance of the lithium transition metal oxide is too short, the mobility of Li may decrease, leading to a decrease in capacity and an increase in resistance. If it is too long, when inserted into the electrode, the interaction with the transition metal may decrease, resulting in high resistance and low capacity.

[0107] The above lithium transition metal oxide can be represented by the following chemical formula 2.

[0108] [Chemical Formula 2]

[0109] Li a [Ni x2 Co y2 Mn z2 ] (1-b) M b O2

[0110] In the above chemical formula 2, 0.8≤a≤1.2, 0.6≤x2≤0.99, 0≤y2≤0.3, 0 <z2≤0.3, 0≤b≤0.1 이고, 도핑 원소인 M은 Nb, Zr, Ti, Mg, Al, W, Mo, B, Ta,P,Mo 또는 이들의 조합이다.

[0111] The above a represents the molar ratio of lithium in the lithium transition metal oxide, and may be 0.8≤a≤1.2, 0.85≤a≤1.15, or 0.9≤a≤1.1.

[0112] The above x2 represents the molar ratio of nickel to the total moles of transition metal in the lithium transition metal oxide, and may be 0.60≤x2≤0.99, 0.70≤x2≤0.99, 0.80≤x2≤0.99, 0.85≤x2≤0.99, 0.90≤x1≤0.99, or 0.90≤x2≤0.95. When the nickel content in the lithium transition metal oxide satisfies the above range, a positive electrode active material and a lithium secondary battery having high capacity characteristics can be manufactured.

[0113] The above y2 represents the molar ratio of cobalt to the total moles of transition metal in the lithium transition metal oxide, and may be 0≤y2≤0.3, 0.01≤y2≤0.2, 0.01≤y2≤0.1, 0.02≤y2≤0.08, or 0.02≤y2≤0.06.

[0114] The above z2 represents the molar ratio of manganese to the total moles of transition metals in the lithium transition metal oxide, where 0 <z2≤0.3, 0.01≤z2≤0.2, 0.01≤z2≤0.1, 0.02≤z2≤0.08 또는 0.02≤z2≤0.06일 수 있다.

[0115] The above b represents the molar ratio of M, a doping element in the lithium transition metal oxide, and may be 0≤b≤0.1 or 0≤b≤0.06.

[0117] 4. Cathode for lithium secondary batteries and lithium secondary batteries

[0118] Meanwhile, another embodiment of the present invention provides a positive electrode for a lithium secondary battery comprising the aforementioned positive electrode active material for a lithium secondary battery, and a lithium secondary battery comprising said positive electrode.

[0120] Specifically, the anode may include an anode current collector and an anode active material layer formed on the anode current collector and comprising the anode active material.

[0121] In the above-mentioned positive electrode, the positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the above-mentioned positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the above-mentioned positive current collector to increase the adhesion of the positive active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0122] The above positive active material layer may include a conductive material and a binder along with the positive active material described above.

[0123] At this time, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that possesses electronic conductivity without causing chemical changes can be used without special limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The conductive material may typically be included in an amount of 1 to 30 weight percent relative to the total weight of the positive electrode active material layer.

[0124] In addition, the binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.

[0125] The above-mentioned anode can be manufactured according to a conventional anode manufacturing method, except for using the above-mentioned anode active material.

[0126] Specifically, a composition for forming an anode active material layer, comprising the above-described anode active material and optionally a binder, a conductive material, and a solvent, can be manufactured by applying the composition onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the anode active material, binder, and conductive material are as previously described.

[0127] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that allows for the dissolution or dispersion of the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.

[0128] Alternatively, the anode may be manufactured by casting the composition for forming the anode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.

[0130] Another embodiment of the present invention provides a lithium secondary battery comprising the aforementioned positive electrode.

[0131] The above lithium secondary battery may specifically include a positive electrode, a negative electrode positioned opposite to the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. Additionally, the lithium secondary battery may optionally further include a battery container housing an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member sealing the battery container.

[0133] In the above lithium secondary battery, the negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0134] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0135] The above-mentioned cathode active material layer may optionally include a binder and a conductive material together with the cathode active material. The above-mentioned cathode active material layer may be manufactured, as an example, by applying a composition for forming a cathode active material layer, comprising a cathode active material and optionally a binder and a conductive material, onto a cathode current collector and drying it, or by casting the composition for forming a cathode onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.

[0136] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; metal oxides capable of doping and dedoping lithium, such as SiOβ (0 < β < 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the above-mentioned metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the above-mentioned negative electrode active material. Furthermore, the carbon material may include both low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.

[0137] The binder and conductive material mentioned above may be the same as those previously described in the anode.

[0139] Meanwhile, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. Any separator typically used in lithium secondary batteries may be used without special limitations, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.

[0141] In addition, regarding the above lithium secondary battery, the electrolyte may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which are usable when manufacturing a lithium secondary battery, but is not limited to these.

[0142] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0143] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.

[0144] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.

[0145] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, haloalkylene carbonate-based compounds like difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexamethylphosphate triamide, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the additive may be included in an amount of 0.1 to 5 weight% based on the total weight of the electrolyte.

[0146] As described above, since the lithium secondary battery containing the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, it is useful in portable devices such as mobile phones, laptop computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).

[0147] Accordingly, another embodiment of the present invention provides a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the same.

[0148] The above battery module or battery pack can be used as a power source for one or more medium-to-large devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0150] The embodiments of the present invention will be described in more detail below through examples. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited by the following examples.

[0152] Examples 1-1 to 1-4

[0153] To evaluate the structural changes of the precursor and active material and the performance of the lithium secondary battery according to the molar ratio of ammonia in precursors prepared using recycled liquid raw materials, the following was conducted.

[0154] (1) Preparation of a positive electrode active material precursor

[0155] A transition metal-containing solution was prepared by mixing recycled liquid raw materials nickel sulfate (impurity content 450 ppm), cobalt sulfate (impurity content 465 ppm), and manganese sulfate (impurity content 485 ppm) in a molar ratio of 92:4:4. At this time, the concentration of the transition metal element in the transition metal-containing solution was set to 2.5 M. Then, an ammonia solution was prepared by adjusting the ratio of the molar amount of ammonia to the total molar amount of the transition metal to 1 (Example 1-1), 1.2 (Example 1-2), 1.4 (Example 1-3), and 1.6 (Example 1-4), respectively.

[0156] Then, the above transition metal-containing solution, ammonia solution, and distilled water were added to a co-precipitation reactor, and dissolved oxygen was removed by supplying nitrogen gas to the reactor. A co-precipitation reaction was performed while maintaining the reactor temperature at 50°C and stirring at 550 rpm to produce a cathode active material precursor. At this time, the pH of the reaction solution during the co-precipitation reaction was set to 11.3.

[0157] (2) Preparation of positive electrode active material

[0158] A lithium transition metal oxide cathode active material was prepared by mixing the cathode active material precursor prepared above with LiOH, a lithium raw material, in a molar ratio of 1:1.10 and then calcining it at a temperature of 740°C for 10 hours in an oxygen atmosphere.

[0159] (3) Lithium secondary battery manufacturing

[0160] SuperC was used as the positive active material and the conductive material and PVDF as the binder prepared above, and a positive active material slurry was prepared by mixing the positive active material, the conductive material, and the binder in a weight ratio of 96.5:1.5:2. The slurry was uniformly coated onto an aluminum foil 20 μm thick and vacuum dried at 130°C to prepare a positive electrode.

[0161] A coin cell was manufactured using a manufactured positive electrode as the working electrode, a lithium foil as the counter electrode, a polypropylene film as the separator, and an electrolyte in which 1.0 M LiPF-6 lithium salt was dissolved in an EC / EMC / DMC solvent.

[0163] Comparative Examples 1-1 to 1-3

[0164] A transition metal-containing solution was prepared using nickel sulfate (impurity content 2.8 ppm), cobalt sulfate (impurity content 3.8 ppm), and manganese sulfate (impurity content 2.9 ppm) as normal raw materials, rather than recycled raw materials with high impurity content, and an ammonia solution was prepared by adjusting the ratio of ammonia to the total moles of transition metal to the conventionally used appropriate ratios of 0.4 (Comparative Example 1-1), 0.6 (Comparative Example 1-2), and 0.8 (Comparative Example 1-3), and the same procedure as in Example 1-1 was performed to manufacture a positive electrode active material precursor, a positive electrode active material, and a lithium secondary battery.

[0166] Comparative Examples 1-4 to 1-6

[0167] A positive electrode active material precursor, a positive electrode active material, and a lithium secondary battery were prepared in the same manner as in Example 1-1, except that an ammonia solution was prepared by adjusting the ratio of ammonia to the total number of moles of transition metal to 0.8 (Comparative Example 1-4), 1.8 (Comparative Example 1-5), and 2 (Comparative Example 1-6), respectively.

[0169] Experimental Example 1-1: Evaluation of Cathode Active Material Precursor Structure According to Ammonia Molar Ratio

[0170] The c-axis length, C of the cathode active material precursor prepared according to Examples 1-1 to 1-4 and Comparative Examples 1-1 to 1-6 (100) / C (001), C (101) / C (001) and C (102) / C (001) An evaluation experiment was conducted, and the results are shown in Table 1 below. The specific experimental method is as follows.

[0171] (1) c-axis length measurement

[0172] To analyze the crystal structure of the precursor and the cathode active material, X-ray diffraction phenomena were measured using a powder XRD measuring device (X-ray diffractometer), and the measured diffraction pattern was analyzed for lattice constants, unit cell volume, etc. through Rietveld refinement.

[0173] (2) C (100) / C (001), C (101) / C (001) and C (102) / C (001) measurement

[0174] After obtaining the diffraction pattern results by performing XRD analysis, the (100), (101), (102), and (001) peaks were obtained, and the peak intensity ratios of (100) / (001), (101) / (001), and (102) / (001) were calculated, respectively.

[0175] Precursor Types of raw materials Ammonia rain Lc (Å) (100) / (001) (101) / (001) (102) / (001) Comparative Example 1-1 Normal product 0.4 4.6291 0.321 1.044 0.445 Comparative Example 1-2 Normal product 0.6 4.6297 0.325 1.047 0.449 Comparative Examples 1-3 Normal product 0.8 4.6294 0.329 1.045 0.451 Comparative Examples 1-4 Recycled liquid 0.8 4.6257 0.295 1.034 0.433 Example 1-1 Recycled liquid 1 4.6264 0.301 1.036 0.434 Examples 1-2 Recycled liquid 1.2 4.6272 0.304 1.033 0.43 Examples 1-3 Recycled liquid 1.4 4.6291 0.323 1.047 0.449 Examples 1-4 Recycled liquid 1.6 4.6295 0.329 1.045 0.45 Comparative Examples 1-5 Recycled liquid 1.8 4.6266 0.299 1.031 0.428 Comparative Examples 1-6 Recycled liquid 2 4.6258 0.296 1.03 0.427

[0176] From Table 1, in the case of Examples 1-1 to 1-4 where the ammonia ratio is 1 to 1.6, compared to Comparative Examples 1-4 to 1-6 which are outside the above range, the c-axis length, C (100) / C (001), C (101) / C (001) and C (102) / C (001) It was confirmed that was large. In particular, in the case of Examples 1-3 to 1-4 where the ammonia ratio was 1.4 to 1.6, the c-axis length, C (100) / C (001), C (101) / C (001) and C (102) / C (001) It was confirmed that it was at a level equivalent to or even superior to the active material precursor using a normal product.

[0178] Experimental Example 1-2: Evaluation of Cathode Active Material Structure According to Ammonia Molar Ratio

[0179] Experiments were conducted to evaluate the c-axis length (Lc), the ratio of the c-axis length (Lc) to the a-axis length (La) (Lc / La), the cation mixing ratio, and the Li slab distance of the cathode active materials prepared according to Examples 1-1 to 1-4 and Comparative Examples 1-1 to 1-6, and the results are shown in Table 2 below. The specific experimental method is as follows.

[0180] (1) c-axis length, Lc / La measurement

[0181] To analyze the crystal structure of the precursor and the cathode active material, X-ray diffraction phenomena were measured using an XRD measuring device (X-ray diffractometer), and the lattice constant values ​​were obtained through Rietveld refinement of the measured diffraction pattern. Lc / La was expressed as the ratio of the obtained lattice constant values ​​of c and a.

[0182] (2) Measurement of cation mixing ratio

[0183] After measuring the X-ray diffraction phenomenon using an XRD measuring device (X-ray diffractometer), the ratio of the (003) and (104) diffraction peak intensities was obtained from the diffraction pattern results to obtain the cation mixing index value.

[0184] (3) Li slab distance measurement

[0185] After measuring the X-ray diffraction phenomenon using an XRD measuring device (X-ray diffractometer) and obtaining the diffraction pattern result, the lattice constant was obtained through Rietveld refinement, and the value was calculated using the following equation.

[0186]

[0187] active material Types of raw materials Ammonia rain Lc (Å) Lc / La Cation mixing index (003) / (104) Li slab distance (Å) Comparative Example 1-1 Normal product 0.4 14.198 4.943 1.208 2.6107 Comparative Example 1-2 Normal product 0.6 14.1983 4.946 1.21 2.6109 Comparative Examples 1-3 Normal product 0.8 14.1984 4.945 1.213 2.611 Comparative Examples 1-4 Recycled liquid 0.8 14.1976 4.937 1.194 2.6092 Example 1-1 Recycled liquid 1 14.1978 4.939 1.195 2.6093 Examples 1-2 Recycled liquid 1.2 14.1977 4.943 1.198 2.6097 Examples 1-3 Recycled liquid 1.4 14.1984 4.944 1.213 2.611 Examples 1-4 Recycled liquid 1.6 14.1986 4.946 1.215 2.6112 Comparative Examples 1-5 Recycled liquid 1.8 14.1975 4.94 1.19 2.6095 Comparative Examples 1-6 Recycled liquid 2 14.1974 4.941 1.187 2.6089

[0188] From Table 2, it was confirmed that in the case of Examples 1-1 to 1-4, where the ammonia ratio was 1 to 1.6, the c-axis length and Lc / La were generally larger compared to Comparative Examples 1-4 to 1-6, which were outside the above range. In particular, in the case of Examples 1-3 to 1-4, where the ammonia ratio was 1.4 to 1.6, it was confirmed that the c-axis length and Lc / La were at a level equivalent to or even larger than that of the active material using a normal product.

[0190] Experimental Example 1-3: Evaluation of Electrochemical Characteristics of Lithium Secondary Battery According to Ammonia Molar Ratio

[0191] Experiments were conducted to evaluate the initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate of lithium secondary batteries prepared according to Examples 1-1 to 1-4 and Comparative Examples 1-1 to 1-6, and the results are shown in Table 3 below. The specific experimental methods are as follows.

[0192] (1) Initial discharge capacity measurement

[0193] The initial capacity was measured through a constant current charging and discharging method of 0.1C within a voltage range of 2.5 to 4.25 V.

[0194] (2) Measurement of diffusion coefficient

[0195] After 0.1C constant current charging and discharging within a voltage range of 2.5 to 4.25 V, the diffusion coefficient was expressed using the following equation via the GITT method (galvanostatic intermittent titration technique).

[0196]

[0198] m B : Molecular weight of electrode active material (g / mol)

[0199] M B : Weight of electrode active material (g)

[0200] V M : Molar volume of active material (m 3 / mol)

[0201] S : Surface area of ​​electrode material (m2 / g)

[0202] L : Electrode thickness (m)

[0203] υ : Characteristic time for diffusion (sec)

[0204] ΔE s : Voltage difference (V) due to surface polarization

[0205] ΔEυ: Voltage difference due to concentration polarization (V)

[0207] (3) Resistance measurement

[0208] DCIR resistance was measured using the DC voltage and DC current values ​​obtained through 0.1C constant current charging and discharging within a voltage range of 2.5 to 4.25 V at a discharge time of 60 seconds.

[0209] (4) Measurement of room temperature output characteristics

[0210] During a constant current discharge process within a voltage of 2.5 to 4.25 V, the C-rate was varied from 0.1C to 2C and measured (reference capacity: 200mAh / g), and the room temperature output was expressed as the 2C capacity value relative to the 0.1C capacity.

[0211] (5) Measurement of capacity retention rate

[0212] After a formation cycle of 0.2 C constant current charge / discharge within a voltage of 2.5 to 4.25 V, a constant current charge / discharge test was performed at 0.33 C, and the capacity retention rate was expressed through the capacity of the 30th cycle relative to the capacity of the first cycle.

[0213] secondary battery Types of raw materials Ammonia rain Initial discharge capacity (mAh / g) Diffusion coefficient (cm²) 2 / s) DCIR (Ω) Room temperature output (2C / 0.1C, %) Dose retention rate (%) Comparative Example 1-1 Normal product 0.4 210.5 5.30*10 -10 17.3 87.2 87.9 Comparative Example 1-2 Normal product 0.6 210.8 5.32*10 -10 17.1 88.3 88.1 Comparative Examples 1-3 Normal product 0.8 211 5.33*10 -10 17.4 88.9 88 Comparative Examples 1-4 Recycled liquid 0.8 206.3 4.97*10 -10 18.5 85.7 84.8 Example 1-1 Recycled liquid 1 209.1 5.15*10 -10 18.3 87.9 87 Examples 1-2 Recycled liquid 1.2 209.3 5.11*10 -10 18.3 88 87.9 Examples 1-3 Recycled liquid 1.4 210.9 5.34*10 -10 16.9 89.5 89.1 Examples 1-4 Recycled liquid 1.6 212.4 5.37*10 -10 17.1 90.1 89.7 Comparative Examples 1-5 Recycled liquid 1.8 206.6 4.97*10 -10 18.6 86.1 85.8 Comparative Examples 1-6 Recycled liquid 2 205.5 4.88*10 -10 19.1 84.8 84.5

[0214] From Table 3, it was confirmed that in the case of Examples 1-1 to 1-4, where the ammonia ratio was 1 to 1.6, the initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate were generally superior compared to Comparative Examples 1-4 to 1-6, which were outside the above range. In particular, in the case of Examples 1-3 to 1-4, where the ammonia ratio was 1.4 to 1.6, it was confirmed that the initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate were at a level equivalent to or even superior to that of a lithium secondary battery using a normal product.

[0216] Examples 2-1 to 2-3

[0217] (1) Preparation of a positive electrode active material precursor

[0218] A transition metal-containing solution was prepared by mixing recycled liquid raw materials nickel sulfate (impurity content 450 ppm), cobalt sulfate (impurity content 465 ppm), and manganese sulfate (impurity content 485 ppm) in a molar ratio of 92:4:4. At this time, the concentration of the transition metal elements in the transition metal-containing solution was set to 2.3 M (Example 2-1), 2.5 M (Example 2-2), and 2.6 M (Example 2-3), respectively. Then, an ammonia solution was prepared by adjusting the ratio of the molar amount of ammonia to the total molar amount of the transition metal to 1.4.

[0219] Then, the above transition metal-containing solution, ammonia solution, and distilled water were added to a co-precipitation reactor, and dissolved oxygen was removed by supplying nitrogen gas to the reactor. A co-precipitation reaction was performed while maintaining the reactor temperature at 50°C and stirring at 550 rpm to produce a cathode active material precursor. At this time, the pH of the reaction solution during the co-precipitation reaction was set to 11.3.

[0220] (2) Preparation of positive electrode active material

[0221] A lithium transition metal oxide cathode active material was prepared by mixing the cathode active material precursor prepared above with LiOH, a lithium raw material, in a molar ratio of 1:1.10 and then calcining it at a temperature of 740°C for 10 hours in an oxygen atmosphere.

[0222] (3) Lithium secondary battery manufacturing

[0223] SuperC was used as the positive active material and the conductive material and PVDF as the binder prepared above, and a positive active material slurry was prepared by mixing the positive active material, the conductive material, and the binder in a weight ratio of 96.5:1.5:2. The slurry was uniformly coated onto an aluminum foil 20 μm thick and vacuum dried at 130°C to prepare a positive electrode.

[0224] A coin cell was manufactured using a manufactured positive electrode as the working electrode, a lithium foil as the counter electrode, a polypropylene film as the separator, and an electrolyte in which 1.0 M LiPF6 lithium salt was dissolved in an EC / EMC / DMC solvent.

[0226] Comparative Examples 2-1 to 2-3

[0227] A transition metal-containing solution was prepared using nickel sulfate (impurity content 2.8 ppm), cobalt sulfate (impurity content 3.8 ppm), and manganese sulfate (impurity content 2.9 ppm) as normal raw materials, rather than recycled raw materials with high impurity content; the ratio of ammonia to the total moles of transition metals was set to 0.8, which is the conventionally used titration ratio, and the transition metal element concentration of the transition metal-containing solution was set to 1.5 M (Comparative Example 2-1), 2 M (Comparative Example 2-2), and 2.3 M (Comparative Example 2-3), which are the conventionally used titration concentrations. Except for these factors, the procedure was carried out in the same manner as in Example 2-1 to produce a positive electrode active material precursor, a positive electrode active material, and a lithium secondary battery.

[0229] Reference Examples 2-1 to 2-3

[0230] A positive electrode active material precursor, a positive electrode active material, and a lithium secondary battery were prepared in the same manner as in Example 2-1, except that the concentration of the transition metal element in the transition metal-containing solution was 1.5 M (Reference Example 2-1), 2 M (Reference Example 2-2), and 2.7 M (Reference Example 2-3), respectively.

[0232] Experimental Example 2-1: Evaluation of Cathode Active Material Precursor Structure According to Transition Metal Element Concentration

[0233] The c-axis length, C of the cathode active material precursor prepared according to Examples 2-1 to 2-3, Comparative Examples 2-1 to 2-3, and Reference Examples 2-4 to 2-6 (100) / C (001), C (101) / C (001) and C (102) / C (001) An evaluation experiment was conducted, and the results are shown in Table 4 below. The specific experimental method is the same as in Experimental Example 1-1.

[0234] Precursor Types of raw materials Concentration of transition metal elements (M) Lc (Å) (100) / (001) (101) / (001) (102) / (001) Comparative Example 2-1 Normal product 1.5 4.6296 0.329 1.043 0.45 Comparative Example 2-2 Normal product 2 4.6297 0.33 1.045 0.451 Comparative Example 2-3 Normal product 2.3 4.6295 0.327 1.041 0.448 Reference Example 2-1 Recycled liquid 1.5 1.5 4.626 0.3 1.029 Reference Example 2-2 Recycled liquid 2 2 4.6264 0.302 1.031 Example 2-1 Recycled liquid 2.3 2.3 4.6293 0.328 1.041 Example 2-2 Recycled liquid 2.5 2.5 4.6295 0.329 1.043 Examples 2-3 Recycled liquid 2.6 2.6 4.6294 0.325 1.039 Reference Example 2-3 Recycled liquid 2.7 2.7 4.627 0.31 1.03

[0235] From Table 4, in the case of Examples 2-1 to 2-3 where the transition metal element concentration is 2.3 to 2.6 M, compared to Reference Examples 2-1 to 2-3 which are outside the above range, the c-axis length, C (100) / C (001), C (101) / C (001) and C (102) / C (001) It was confirmed that was large. In particular, for Examples 2-2 and 2-3, where the transition metal element concentration was 2.5 to 2.6 M, the c-axis length, C (100) / C (001), C (101) / C (001) and C (102) / C (001) It was confirmed that it was at a level equivalent to or even superior to the active material precursor using a normal product.

[0237] Experimental Example 2-2: Evaluation of Cathode Active Material Structure According to Transition Metal Element Concentration

[0238] Experiments were conducted to evaluate the c-axis length (Lc), the ratio of the c-axis length (Lc) to the a-axis length (La) (Lc / La), the cation mixing ratio, and the Li slab distance of the cathode active materials prepared according to Examples 2-1 to 2-3, Comparative Examples 2-1 to 2-3, and Reference Examples 2-1 to 2-3, and the results are shown in Table 5 below. The specific experimental method is the same as that in Experimental Example 1-2.

[0239] active material Types of raw materials Concentration of transition metal elements (M) Lc (Å) Lc / La Cation mixing index(003) / (104) Li slab distance (Å) Comparative Example 2-1 Normal product 1.5 14.1982 4.94 1.207 2.611 Comparative Example 2-2 Normal product 2 14.1984 4.943 1.209 2.6112 Comparative Example 2-3 Normal product 2.3 14.1982 4.941 1.205 2.6112 Reference Example 2-1 Recycled liquid 1.5 14.1968 4.93 1.19 2.6085 Reference Example 2-2 Recycled liquid 2 14.197 4.933 1.192 2.6093 Example 2-1 Recycled liquid 2.3 14.1982 4.941 1.209 2.611 Example 2-2 Recycled liquid 2.5 14.1985 4.944 1.211 2.6114 Examples 2-3 Recycled liquid 2.6 14.1984 4.941 1.204 2.611 Reference Example 2-3 Recycled liquid 2.7 14.1976 4.932 1.193 2.6097

[0240] From Table 5, it was confirmed that in the case of Examples 2-1 to 2-3, where the transition metal element concentration was 2.3 to 2.6 M, the c-axis length, Lc / La, and Li slab distance were larger compared to Reference Examples 2-1 to 2-3, which were outside the above range. In particular, in the case of Examples 2-2 to 2-3, where the transition metal element concentration was 2.5 to 2.6 M, it was confirmed that the c-axis length, Lc / La, and Li slab distance were at a level equivalent to or even larger than that of the active material using a normal product.

[0242] Experimental Example 2-3: Evaluation of Electrochemical Characteristics of Lithium Secondary Batteries According to Transition Metal Element Concentration

[0243] Experiments were conducted to evaluate the initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate of lithium secondary batteries prepared according to Examples 2-1 to 2-3, Comparative Examples 2-1 to 2-3, and Reference Examples 2-1 to 2-3, and the results are shown in Table 6 below. The specific experimental method is the same as that of Experimental Example 1-3.

[0244] secondary battery Types of raw materials Transition metal element concentration (M) Initial discharge capacity (mAh / g) Diffusion coefficient (cm²) 2 / s) DCIR(Ω) Room temperature output (2C / 0.1C, %) Dose retention rate (%) Comparative Example 2-1 Normal product 1.5 211.8 5.39*10 -10 17 88.7 88.1 Comparative Example 2-2 Normal product 2 212 5.40*10 -10 17 89.1 89 Comparative Example 2-3 Normal product 2.3 211.6 5.36*10 -10 17.2 88.5 88.7 Reference Example 2-1 Recycled liquid 1.5 203.5 4.93*10 -10 24.7 85.1 85.2 Reference Example 2-2 Recycled liquid 2 204.9 4.99*10 -10 21.2 87 87.1 Example 2-1 Recycled liquid 2.3 211.4 5.34*10 -10 17.2 88.4 88.2 Example 2-2 Recycled liquid 2.5 212.5 5.40*10 -10 17 89.5 89.8 Examples 2-3 Recycled liquid 2.6 212.2 5.37*10 -10 17.5 88.1 88.6 Reference Example 2-3 Recycled liquid 2.7 209.1 5.14*10 -10 19.5 86.6 87.3

[0245] From Table 6, it was confirmed that in the case of Examples 2-1 to 2-3, where the transition metal element concentration was 2.3 to 2.6 M, the initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate were superior compared to Reference Examples 2-1 to 2-3, which were outside the above range. In particular, in the case of Examples 2-2 to 2-3, where the transition metal element concentration was 2.5 to 2.6 M, it was confirmed that the initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate were almost equivalent to or even superior to those of a lithium secondary battery using a normal product.

[0247] Examples 3-1 to 3-2

[0248] (1) Preparation of a positive electrode active material precursor

[0249] A transition metal-containing solution was prepared by mixing recycled liquid raw materials nickel sulfate (impurity content 450 ppm):cobalt sulfate (impurity content 465 ppm):manganese sulfate (impurity content 485 ppm) in a molar ratio of 92:4:4. At this time, the transition metal element concentration of the transition metal-containing solution was set to 2.5 M. Then, an ammonia solution was prepared by adjusting the ratio of the molar amount of ammonia to the total molar amount of the transition metal to 1.0.

[0250] Then, the above transition metal-containing solution, ammonia solution, and distilled water were added to a co-precipitation reactor, and dissolved oxygen was removed by supplying nitrogen gas to the reactor. A co-precipitation reaction was performed while maintaining the reactor temperature at 50°C and stirring at 550 rpm to produce a cathode active material precursor. At this time, the pH of the reaction solution during the co-precipitation reaction was set to 11.1 (Example 3-1) and 11.3 (Example 3-2), respectively.

[0251] (2) Preparation of positive electrode active material

[0252] A lithium transition metal oxide cathode active material was prepared by mixing the cathode active material precursor prepared above with LiOH, a lithium raw material, in a molar ratio of 1:1.10 and then calcining it at a temperature of 740°C for 10 hours in an oxygen atmosphere.

[0253] (3) Lithium secondary battery manufacturing

[0254] The cathode active material prepared above, SueprC as a conductive material, and PVDF as a binder were used, and a cathode active material slurry was prepared by mixing the cathode active material, conductive material, and binder in a weight ratio of 96.5:1.5:2. The slurry was uniformly coated onto an aluminum foil with a thickness of 20 μm and vacuum dried at 130°C to produce a cathode.

[0255] A coin cell was manufactured using a manufactured positive electrode as the working electrode, a lithium foil as the counter electrode, a polypropylene film as the separator, and an electrolyte in which 1 M LiPF6 lithium salt was dissolved in an EC / DMC / EMC solvent.

[0257] Comparative Examples 3-1 to 3-3

[0258] A transition metal-containing solution was prepared using nickel sulfate (impurity content 2.8 ppm), cobalt sulfate (impurity content 3.8 ppm), and manganese sulfate (impurity content 2.9 ppm) as normal raw materials, rather than recycled raw materials with high impurity content; the ratio of the molar amount of ammonia to the total molar amount of transition metal was set to 0.8, which is the conventionally used titration ratio, and the transition metal-containing solution was prepared by setting the concentration of the transition metal element in the transition metal-containing solution to 2.3 M, which is the conventionally used titration concentration; and the pH of the reaction solution during the co-precipitation reaction was 11.5 (Comparative Example 3-1), 11.7 (Comparative Example 3-2), and 11.9 (Comparative Example 3-3), respectively, in the same manner as Example 3-1 to manufacture a positive active material precursor, a positive active material, and a lithium secondary battery.

[0260] Reference Examples 3-1 to 3-4

[0261] A positive electrode active material precursor, a positive electrode active material, and a lithium secondary battery were prepared in the same manner as in Example 3-1, except that the pH of the reaction solution during the co-precipitation reaction was set to 10.9 (Reference Example 3-1), 11.5 (Reference Example 3-2), 11.7 (Reference Example 3-3), and 11.9 (Reference Example 3-4), respectively.

[0263] Experimental Example 3-1: Evaluation of the structure of cathode active material precursors according to pH during co-precipitation reaction

[0264] The c-axis length, C of the cathode active material precursor prepared according to Examples 3-1 to 3-2, Comparative Examples 3-1 to 3-3, and Reference Examples 3-1 to 3-4 (100) / C (001), C (101) / C (001) and C (102) / C (001) An evaluation experiment was conducted, and the results are shown in Table 7 below. The specific experimental method is the same as Experimental Example 1-1.

[0265] Precursor Types of raw materials pH Lc (Å) (100) / (001) (101) / (001) (102) / (001) Comparative Example 3-1 Normal product 11.5 4.6293 0.329 1.043 0.450 Comparative Example 3-2 Normal product 11.7 4.6296 0.332 1.044 0.453 Comparative Example 3-3 Normal product 11.9 4.6295 0.331 1.041 0.451 Reference Example 3-1 Recycled liquid 10.9 4.6283 0.328 1.039 0.447 Example 3-1 Recycled liquid 11.1 4.6296 0.332 1.044 0.451 Example 3-2 Recycled liquid 11.3 4.6294 0.33 1.042 0.45 Reference Example 3-2 Recycled liquid 11.5 4.6291 0.329 1.04 0.448 Reference Example 3-3 Recycled liquid 11.7 4.6284 0.326 1.035 0.441 Reference Example 3-4 Recycled liquid 11.9 4.6272 0.323 1.032 0.438

[0266] From Table 7, in the case of Examples 3-1 to 3-2, where the pH during the co-precipitation reaction is 11.1 to 11.3, compared to Reference Examples 3-1 to 3-4, which are outside the above range, the c-axis length, C (100) / C (001), C (101) / C (001) and C (102) / C (001) It was possible to confirm that it was large, and in particular, the above physical properties It was confirmed that the active material precursor was at a level equivalent to or even superior to that of a standard product.

[0268] Experimental Example 3-2: Evaluation of Cathode Active Material Structure According to pH During Co-precipitation Reaction

[0269] Experiments were conducted to evaluate the c-axis length (Lc), the ratio of the c-axis length (Lc) to the a-axis length (La) (Lc / La), the cation mixing ratio, and the Li slab distance of the cathode active materials prepared according to Examples 3-1 to 3-2, Comparative Examples 3-1 to 3-3, and Reference Examples 3-1 to 3-4, and the results are shown in Table 8 below. The specific experimental method is the same as that in Experimental Example 1-2.

[0270] active material Types of raw materials pH Lc (Å) Lc / La Cation mixing index (003) / (104) Li slab distance (Å) Comparative Example 3-1 Normal product 11.5 14.198 4.942 1.209 2.6112 Comparative Example 3-2 Normal product 11.7 14.1983 4.945 1.213 2.6115 Comparative Example 3-3 Normal product 11.9 14.1982 4.943 1.211 2.6114 Reference Example 3-1 Recycled liquid 10.9 14.1982 4.939 1.209 2.6109 Example 3-1 Recycled liquid 11.1 14.1985 4.943 1.212 2.6115 Example 3-2 Recycled liquid 11.3 14.1982 4.94 1.21 2.6113 Reference Example 3-2 Recycled liquid 11.5 14.198 4.936 1.208 2.6107 Reference Example 3-3 Recycled liquid 11.7 14.1974 4.932 1.203 2.6104 Reference Example 3-4 Recycled liquid 11.9 14.1971 4.926 1.193 2.6095

[0271] From Table 8, it was confirmed that in the case of Examples 3-1 to 3-2, where the pH during the co-precipitation reaction was 11.1 to 11.3, the c-axis length, Lc / La, and Li slab distance were larger compared to Reference Examples 3-1 to 3-4, which were outside the above range, and in particular, it was confirmed that the physical properties were at a level equivalent to or even greater than that of the active material using normal raw materials.

[0273] Experimental Example 3-3: Evaluation of Electrochemical Characteristics of Lithium Secondary Batteries According to pH During Co-precipitation Reaction

[0274] Experiments were conducted to evaluate the initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate of lithium secondary batteries prepared according to Examples 3-1 to 3-2, Comparative Examples 3-1 to 3-3, and Reference Examples 3-1 to 3-4, and the results are shown in Table 9 below. The specific experimental method is the same as that of Experimental Example 1-3.

[0275] secondary battery Types of raw materials pH Initial discharge capacity (mAh / g) Diffusion coefficient (cm²) 2 / s) DCIR(Ω) Room temperature output (2C / 0.1C, %) Capacity retention rate (%) Comparative Example 3-1 Normal product 11.5 211.7 5.36*10 -10 17.2 89 88.5 Comparative Example 3-2 Normal product 11.7 212 5.41*10 -10 17 89.7 88.9 Comparative Example 3-3 Normal product 11.9 211.9 5.38*10 -10 17.1 89.3 88.3 Reference Example 3-1 Recycled liquid 10.9 211.8 5.34*10 -10 17.8 88.5 88 Example 3-1 Recycled liquid 11.1 212.8 5.40*10 -10 16.8 89.5 89 Example 3-2 Recycled liquid 11.3 212 5.37*10 -10 17.2 89.2 88.4 Reference Example 3-2 Recycled liquid 11.5 211.4 5.29*10 -10 18 87.5 87.5 Reference Example 3-3 Recycled liquid 11.7 209.6 5.21*10 -10 18.4 87.1 86.9 Reference Example 3-4 Recycled liquid 11.9 208.2 5.14*10 -10 19 86.1 86.5

[0276] From Table 9, it was confirmed that Examples 3-1 to 3-2, in which the pH during the co-precipitation reaction was 11.1 to 11.3, exhibited superior initial discharge capacity, diffusion coefficient, resistance, room temperature output characteristics, and capacity retention rate compared to Reference Examples 3-1 to 3-4, which were outside the above range. In particular, it was confirmed that the electrochemical characteristics were nearly equivalent to or even superior to those of a lithium secondary battery using normal raw materials.

[0278] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented with various modifications within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is obvious that such modifications also fall within the scope of the present invention.

[0279] Therefore, the substantive scope of the present invention shall be defined by the appended claims and their equivalents.

Claims

Claim 1 A method for manufacturing a precursor of a positive electrode active material for a lithium secondary battery from a spent lithium secondary battery, comprising: a step of preparing a recycled liquid raw material containing a liquid nickel raw material, a cobalt raw material, and a manganese raw material extracted from a spent lithium secondary battery, wherein the impurity content of each of the nickel raw material, the cobalt raw material, and the manganese raw material is 100 ppm or more; a step of forming a transition metal-containing solution containing the recycled liquid raw material; and a step of introducing the transition metal-containing solution, an ammonia solution, and a caustic soda solution into a reactor to form a reaction solution, and co-precipitating the reaction solution to form a precursor of a positive electrode active material for a lithium secondary battery, wherein the ratio of the number of moles of ammonia contained in the ammonia solution to the number of moles of transition metal elements contained in the transition metal-containing solution is 1.0 to 1.

6. Claim 2 A method for manufacturing a positive electrode active material precursor for a lithium secondary battery, wherein, in the step of preparing the recycled liquid raw material, the impurity content of each of the nickel raw material, cobalt raw material, and manganese raw material is 100 to 500 ppm. Claim 3 A method for manufacturing a positive electrode active material precursor for a lithium secondary battery, wherein, in claim 1, the transition metal element concentration of the transition metal-containing solution is 2.3 to 2.6 M. Claim 4 A method for manufacturing a positive electrode active material precursor for a lithium secondary battery, wherein the pH of the reaction solution is 11.1 to 11.3, in accordance with claim 1.

Citation Information

Patent Citations

  • Ternary positive electrode material short-process recycling method, recycled material and application

    CN112467241A

  • Impurity ion doped regenerated ternary positive electrode material and preparation method and application thereof

    CN114314691A

  • Manufacturing method of positive electrode active material precursor, and positive electrode active material precursor

    KR1020210048434A