Transfer laminate, manufacturing method of negative electrode for lithium secondary battery, negative electrode for lithium secondary battery and lithium secondary battery comprising negative electrode
A transfer laminate with a lithium carbonate-protected lithium metal layer, defined by color difference criteria, addresses the challenges of silicon-based anode pre-lithiation in lithium-ion batteries, enhancing stability and efficiency in lithium transfer.
Patent Information
- Application Number
- KR1020220182508
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-12-23
AI Technical Summary
Conventional pre-lithiation methods for silicon-based anode active materials in lithium-ion batteries face challenges such as increased initial irreversible capacity, volume changes, surface side reactions, and risks of heat generation and ignition during lithium transfer, with no effective quantitative measurement for surface treatment stability.
A transfer laminate with a substrate layer and a lithium metal layer protected by a lithium carbonate surface film, defined by specific color difference criteria, is used to facilitate controlled lithium transfer, reducing ignition and side reactions.
The laminate enables efficient and stable lithium transfer by quantifying surface treatment, minimizing quality and stability issues, and ensuring complete lithiation of the negative electrode.
Smart Images

Figure 112022138859271-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present application relates to a transfer laminate, a method for manufacturing a negative electrode for a lithium secondary battery, a negative electrode for a lithium secondary battery, and a lithium secondary battery comprising a negative electrode. Background Technology
[0002] Due to the rapid increase in the use of fossil fuels, there is a growing demand for alternative or clean energy. As part of this effort, the fields of power generation and energy storage utilizing electrochemical reactions are the most actively researched.
[0003] Currently, a representative example of an electrochemical device utilizing such electrochemical energy is the secondary battery, and its scope of application is steadily expanding.
[0004] With the increasing technological development and demand for mobile devices, the demand for secondary batteries as an energy source is rapidly rising. Among these secondary batteries, lithium-ion batteries, which possess high energy density and voltage, long cycle life, and low self-discharge rates, have been commercialized and are widely used. Furthermore, active research is being conducted on methods to manufacture high-density electrodes with higher energy density per unit volume for use in such high-capacity lithium-ion batteries.
[0005] Generally, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode includes a negative electrode active material that inserts and extracts lithium ions from the positive electrode, and silicon-based particles with a large discharge capacity may be used as the negative electrode active material.
[0006] Generally, carbon materials such as graphite are used as the negative electrode of lithium-ion batteries, but the theoretical capacity density of carbon is 372 mAh / g (833 mAh / cm³). 3Therefore, to improve the energy density of the cathode, silicon (Si), tin (Sn) alloyed with lithium, or their oxides and alloys are considered as cathode materials. Among them, silicon-based materials have attracted attention due to their low cost and high capacity (4200 mAh / g).
[0007] However, when using silicon-based anode active materials, a significant problem arises due to the large initial irreversible capacity. Specifically, in the charge-discharge reaction of a lithium secondary battery, lithium released from the anode is inserted into the anode during charging and detached from the anode to return to the anode during discharging. However, silicon-based anode active materials exhibit severe volume changes and surface side reactions, preventing a large amount of the lithium inserted into the anode during initial charging from returning to the anode. Consequently, this leads to a problem of increased initial irreversible capacity. A large initial irreversible capacity results in a rapid decrease in battery capacity and cycle life.
[0008] To solve the above problems, a method for pre-lithiating a silicon anode containing a silicon-based anode active material is known. Pre-lithiation methods include manufacturing an electrode after lithiation by physical / chemical methods such as electroplating, lithium metal transfer, and lithium metal deposition, and electrochemically pre-lithiating the anode.
[0009] To utilize conventional electrochemical methods, a wet process must be carried out within the electrolyte; since this entails risks such as fire and explosion, it was necessary to carefully control the inert environment. Specifically, creating such an environment requires complex control of conditions, such as moisture regulation, using inert gas within the room where the electrochemical process is conducted. Furthermore, uniform control of the initial irreversible capacity is achievable only by slowing down the rate of pre-lithiation using electrochemical methods, which resulted in increased production costs when applying these methods.
[0010] In addition, there was a problem where heat generation occurred during the pressurization process of the pre-lithiation process, specifically when lithium was inserted into the electrode. In particular, if the electrode's heating temperature exceeds 30°C, the lithium undergoes an oxidation reaction, which not only promotes side reactions but also poses a risk of electrode ignition during the lithium transfer process. These risk factors are critical elements that require management when performing the lithium transfer process.
[0011] To improve the aforementioned heat generation phenomenon, appropriate surface treatment is performed on the transfer laminate; however, there is no measurement method to quantitatively verify the extent to which transfer is facilitated while ignition stability and the suppression of lithium oxidation reactions are efficiently improved. Consequently, problems arise such as heat generation due to improper surface treatment, the inability to avoid side reactions caused by lithium oxidation, or the inability to avoid the risk of electrode ignition during the lithium transfer process.
[0012] Therefore, research is needed on criteria that can quantify surface treatment. Prior art literature
[0013] Japanese Published Patent Application No. 2009-080971 The problem to be solved
[0014] To solve the aforementioned problem, the inventors confirmed that the degree of oxidation reaction of surface lithium can be quantified by defining the color difference of the lithium metal surface, and thus found that the above problem can be solved.
[0015] Accordingly, the present application relates to a transfer laminate, a method for manufacturing a negative electrode for a lithium secondary battery, a negative electrode for a lithium secondary battery, and a lithium secondary battery comprising a negative electrode. means of solving the problem
[0016] One embodiment of the present specification provides a transfer laminate comprising a substrate layer and a lithium metal layer on one surface of the substrate layer, wherein the lithium metal layer comprises a surface protective film on its surface, the surface protective film comprises lithium carbonate (Li2CO3), and the surface color difference with respect to the surface of the lithium metal layer comprising the surface protective film satisfies the following formula (1).
[0017] L SCE ≥ 40 - Equation (1)
[0018] In the above equation (1), L SCE represents the brightness index measured in SCE (Specular component excluded) mode.
[0019] In another embodiment, a method for manufacturing a negative electrode for a lithium secondary battery is provided, comprising the steps of: forming a negative electrode for a lithium secondary battery by forming a negative electrode current collector layer and a negative active material layer on one or both sides of the negative electrode current collector layer; and laminating the transfer laminate on the opposite side of the negative active material layer that contacts the negative electrode current collector layer to transfer a lithium metal layer.
[0020] In addition, in one embodiment of the present specification, a negative electrode for a lithium secondary battery manufactured according to the method for manufacturing a negative electrode for a lithium secondary battery is provided.
[0021] Finally, in one embodiment of the present specification, a lithium secondary battery is provided comprising: a first electrode; a second electrode; a separator provided between the first electrode and the second electrode; and an electrolyte, wherein either of the first electrode and the second electrode comprises a negative electrode for the lithium secondary battery. Effects of the invention
[0022] A transfer laminate according to one embodiment of the present invention quantifies the degree of surface treatment as a color difference, thereby defining characteristics that enable the efficient execution of the transfer process and making it easy to identify the progress of the surface treatment process. By utilizing such indicators of the surface treatment process, quality and stability issues occurring during the transfer process can be effectively reduced. Brief explanation of the drawing
[0023] FIG. 1 is a diagram showing a process of transferring lithium metal to a negative electrode for a lithium secondary battery according to one embodiment of the present specification. FIG. 2 is a drawing showing a stacked structure of a lithium secondary battery according to one embodiment of the present specification. Specific details for implementing the invention
[0024] Before describing the present invention, some terms are defined first.
[0025] In this specification, when a part is described as "comprising" a certain component, it means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0026] In this specification, 'p to q' means a range of 'p or more and q or less'.
[0027] In this specification, "specific surface area" is measured by the BET method, specifically calculated from the amount of nitrogen gas adsorbed at a liquid nitrogen temperature (77K) using BELSORP-mino II of BEL Japan. That is, in this application, the BET specific surface area may refer to the specific surface area measured by the above measurement method.
[0028] In this specification, "Dn" refers to the average particle size and represents the particle size at the n% point of the cumulative distribution of the number of particles according to particle size. That is, D50 is the particle size at the 50% point of the cumulative distribution of the number of particles according to particle size, D90 is the particle size at the 90% point of the cumulative distribution of the number of particles according to particle size, and D10 is the particle size at the 10% point of the cumulative distribution of the number of particles according to particle size. Meanwhile, the average particle size can be measured using the laser diffraction method. Specifically, after dispersing the powder to be measured in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the difference in diffraction patterns according to particle size is measured as the particles pass through the laser beam to calculate the particle size distribution.
[0030] Hereinafter, the present invention will be described in detail with reference to the drawings so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in various different forms and is not limited to the description below.
[0032] Transfer laminate
[0033] One embodiment of the present specification provides a transfer laminate comprising a substrate layer and a lithium metal layer on one surface of the substrate layer, wherein the lithium metal layer comprises a surface protective film on its surface, the surface protective film comprises lithium carbonate (Li2CO3), and the surface color difference with respect to the surface of the lithium metal layer comprising the surface protective film satisfies the following formula (1).
[0034] L SCE ≥ 40 - Equation (1)
[0035] In the above equation (1), L SCE represents the brightness index measured in SCE (Specular component excluded) mode.
[0036] In another embodiment of the present specification, regarding the surface color difference with respect to the surface of the lithium metal layer including the surface protective film, L SCE It may have a value of about 40 or more, preferably about 41 or more, or more preferably about 42 or more, or a value of about 100 or less, about 95 or less, about 90 or less, preferably 85 or less, or more preferably 83 or less.
[0037] In this specification, the surface color difference can be measured with equipment known in the industry, but specifically, Konica Minolta's CM-2600d can be used.
[0038] According to the above embodiment, the surface color difference can be determined by defining the brightness of reflected light (mainly scattered light) excluding specular reflection light using a brightness index measured in an SCE mode, thereby determining the hardness of the surface of a lithium metal layer including a surface protective film.
[0039] The transfer laminate according to the above embodiment can suppress ignition phenomena or side reactions caused by heat generation by having a surface color difference within a specific range.
[0040] In this specification, the measurement conditions for the surface color difference of the lithium metal layer may be based on using a standard light source D65, a 10° field of view, and 100% UV usage conditions.
[0041] In this specification, surface treatment may be performed using carbon dioxide (CO2), but is not limited thereto. For example, the surface treatment may be performed using a single gas of carbon dioxide (CO2) or a mixture of carbon dioxide and an inert gas (e.g., nitrogen (N2), argon (Ar), etc.).
[0042] In this specification, a mixture of an inert gas (e.g., argon) and carbon dioxide may be used, and the mixing ratio of argon and carbon dioxide may be 8:2, but is not limited thereto.
[0043] In the present specification, when surface treatment is performed with a single gas of carbon dioxide (CO2), the surface of the lithium metal layer may include lithium carbonate (Li2CO3), which is a lithium oxide, as a main component.
[0044] In the transfer laminate according to the above embodiment, by defining a color difference on the surface of the lithium metal layer containing the lithium carbonate, which is the lithium oxide, a surface treatment state capable of improving stability in the future lithium transfer process can be numerically identified.
[0045] In one embodiment of the present specification, the surface of the lithium metal layer may further include one or more components selected from LiOH, Li3N, Li2O, Li2O2, and combinations thereof.
[0046] In the present specification, when the lithium metal layer is surface-treated by being exposed to oxygen, nitrogen, moisture, etc. in the atmosphere during the surface treatment process, lithium oxide (e.g., Li2O, Li2O2), lithium nitride (Li3N), lithium hydroxide (LiOH), etc. may be further included as additional components on the surface of the lithium metal layer.
[0047] In one embodiment of the present specification, a transfer laminate is provided in which the surface color difference with respect to the surface of the lithium metal layer including the surface protective film satisfies the following formula (2).
[0048] L SCI L ≥ 90 measured in (Specular component included) mode - Equation (2)
[0049] In the above equation (2), L SCIrepresents the brightness index measured in SCI (Specular component included) mode.
[0050] In another embodiment of the present specification, regarding the surface color difference with respect to the surface of the lithium metal layer including the surface protective film, L SCI It may have a value of about 80 or more, preferably about 85 or more, or more preferably about 90 or more, or a value of about 100 or less, preferably about 98 or less, or more preferably 96 or less.
[0051] In the transfer laminate according to the above embodiment, by defining a color difference on the surface of the lithium metal layer containing the lithium carbonate, which is the lithium oxide, a surface treatment state capable of improving stability in the future lithium transfer process can be numerically identified.
[0052] In another embodiment of the present specification, the surface color difference of the surface of the lithium metal layer including the surface protective film may satisfy both Equation (1) and Equation (2).
[0053] In the transfer laminate according to the above embodiment, by defining a color difference on the surface of the lithium metal layer containing the lithium carbonate, which is the lithium oxide, a surface treatment state capable of improving stability in the future lithium transfer process can be numerically identified.
[0054] In this specification, the surface color difference of the lithium metal layer can be measured using equipment known in the industry, but specifically, the CM-2600d of Konica Minolta can be used.
[0055] In one embodiment of the present specification, the thickness of the substrate layer may be 5 μm or more and 300 μm or less, preferably 10 μm or more and 100 μm or less. If the substrate thickness is less than 5 μm, process issues such as creasing or tearing may occur during the process, and if it exceeds 300 μm, it is difficult to effectively remove heat during lithium deposition, making it difficult to increase the deposition rate, which may lead to problems such as increased costs.
[0056] In one embodiment of the present specification, the substrate layer may be one or more selected from the group consisting of polyethylene terephthalate (PET), polyethylenenaphthalate (PEN), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate.
[0057] In one embodiment of the present specification, the thickness of the lithium metal layer may be 1 μm or more and 10 μm or less.
[0058] In another embodiment of the present application, the thickness of the lithium metal layer may be about 1 μm or more, about 2 μm or more, or 3 μm or more, or about 10 μm or less, about 9 μm or less, or about 8 μm or less.
[0059] As the thickness of the lithium metal layer satisfies the above range, the transfer of lithium metal to the negative electrode active material layer can occur efficiently, reverse transfer can be prevented, and the negative electrode active material layer can be fully lithiated to a desired degree.
[0060] In one embodiment of the present specification, a release layer may be further included between the substrate layer and the lithium metal layer.
[0061] The transfer laminate according to the above embodiment is laminated in the order of a substrate layer, a release layer (hereinafter referred to as a first release layer or a peel layer), and a lithium metal layer, wherein the release layer functions as a peel layer for transferring lithium. Due to the release layer, the problem of reverse peeling in which lithium metal is transferred onto the substrate layer during the winding process for transferring the deposited lithium metal layer to the negative electrode can be prevented, and furthermore, the substrate layer can be easily separated after transferring the lithium metal onto the negative electrode active material layer.
[0062] In another embodiment of the present application, a release layer may be formed on both sides of the substrate layer.
[0063] The transfer laminate according to the above embodiment may additionally include a second release layer (or may be referred to as a non-release layer) on the opposite side of the surface where the substrate layer and the first release layer contact each other, in addition to the first release layer interposed between the substrate layer and the lithium metal layer.
[0064] The above-mentioned second release layer is an auxiliary component used to reduce friction with the roll during the roll-to-roll process.
[0065] In the present specification, the release layer may comprise one or more selected from the group consisting of a silicone-modified polyester in which a silicone chain is grafted to a polyester main chain, an acrylic resin, Si, melamine, and fluorine.
[0066] In one embodiment of the present specification, the release layer may be formed by a coating method, for example, the coating method may be selected from the group consisting of dip coating, spray coating, spin coating, die coating, gravure coating, micro-gravure coating, comma coating, ink-jet coating, bar coating, wire-bar coating, and roll coating, but is not limited thereto, and various coating methods that can be used in the art to form a coating layer may be used.
[0067] In one embodiment of the present specification, the thickness of the release layer may be 0.1 μm or more and 10 μm or less.
[0068] Preferably, the thickness of the release layer may be about 0.1 μm or more, about 0.2 μm or more, about 0.3 μm or more, about 0.4 μm or more, or about 0.5 μm or more, or about 10 μm or less, about 9.9 μm or less, about 9.8 μm or less, about 9.7 μm or less, or about 9.6 μm or less.
[0069] The above release layer is transferred onto the upper surface of the negative electrode active material layer in the lithium metal transfer process described later, together with the lithium metal layer; if the thickness of the release layer satisfies the above range, the coating uniformity of the release layer can be increased. Furthermore, if the release layer satisfies the above thickness range, it has the characteristic of not causing the problem of increased battery resistance.
[0071] Method for manufacturing a negative electrode for a lithium secondary battery
[0072] In one embodiment of the present specification, a method for manufacturing a negative electrode for a lithium secondary battery is provided, comprising the steps of: preparing a negative electrode for a lithium secondary battery by forming a negative current collector layer and a negative active material layer on one or both sides of the negative current collector layer; and transferring a lithium metal layer by laminating the transfer laminate described above onto the opposite side of the negative active material layer that contacts the negative current collector layer.
[0073] In the present specification, the step of forming a negative active material layer on one or both sides of the negative current collector layer includes the step of coating a negative slurry comprising a negative active material layer composition on one or both sides of the negative current collector layer, wherein the negative active material layer composition may comprise one or more selected from the group consisting of a silicon-based active material; a negative conductive material; and a negative binder.
[0074] In one embodiment of the present specification, the cathode slurry may comprise a cathode active material layer composition; and a slurry solvent.
[0075] In one embodiment of the present specification, the solid content of the cathode slurry may satisfy 5% or more and 40% or less.
[0076] In another embodiment, the solid content of the cathode slurry may satisfy a range of 5% or more and 40% or less, preferably 7% or more and 35% or less, and more preferably 10% or more and 30% or less.
[0077] The solid content of the above-mentioned cathode slurry may refer to the content of the cathode active material layer composition included in the above-mentioned cathode slurry, and may refer to the content of the cathode active material composition based on 100 parts by weight of the cathode slurry.
[0078] When the solid content of the above cathode slurry satisfies the above range, the viscosity is suitable when forming the cathode active material layer, thereby minimizing particle aggregation of the cathode active material layer composition and enabling the cathode active material layer to be formed efficiently.
[0079] In one embodiment of the present specification, the slurry solvent is not limited thereto as long as it can dissolve the cathode active material layer composition, but specifically, acetone; distilled water; or NMP may be used.
[0080] A cathode according to one embodiment of the present specification can be formed by coating and drying the cathode slurry on a cathode current collector layer.
[0081] Through the above drying step, the slurry solvent in the cathode slurry can be dried, and subsequently, an electrode rolling step may be further included.
[0082] In one embodiment of the present specification, the negative current collector layer generally has a thickness of 1 μm to 100 μm. Such a negative current collector layer is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy may be used. In addition, fine irregularities may be formed on the surface to strengthen the bonding strength of the negative active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0083] In one embodiment of the present specification, the negative active material layer comprises a negative active material layer composition formed on one or both sides of the negative current collector layer.
[0084] In one embodiment of the present specification, the cathode active material layer composition may include a silicon-based active material; a cathode conductive material; and a cathode binder.
[0085] In one embodiment of the present specification, the silicon-based active material is SiOx (x=0), SiOx (0 <x<2), SiC, 금속 불순물 및 Si 합금으로 이루어진 군에서 선택되는 1 이상을 포함할 수 있다.
[0086] In one embodiment of the present specification, the silicon-based active material is SiOx (x=0) and SiOx (0 <x<2)로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 70 중량부 이상 포함할 수 있다.
[0087] In another embodiment, based on 100 parts by weight of the silicon-based active material, the SiOx (x=0) may be included in an amount of 70 parts by weight or more, preferably 80 parts by weight or more, more preferably 90 parts by weight or more, and 100 parts by weight or less, preferably 99 parts by weight or less, more preferably 95 parts by weight or less.
[0088] In one embodiment of the present specification, the silicon-based active material may particularly use pure silicon (Si) as the silicon-based active material. Using pure silicon (Si) as the silicon-based active material means that, when the silicon-based active material is based on 100 parts by weight of the total as described above, pure Si particles (SiOx (x=0)) that are not bonded with other particles or elements are included in the above range.
[0089] In the case of silicon-based active materials, there are increasing attempts to apply them because their capacity is significantly higher compared to conventionally used graphite-based active materials. However, due to their high volume expansion rate during the charge-discharge process, their use is limited to cases where they are mixed in trace amounts with graphite-based active materials. Furthermore, despite the above advantages, the high initial irreversible capacity leads to a decrease in lifespan, and to solve this, a pre-lithiation process is being carried out to pre-lithiate the anode.
[0090] Accordingly, the main objective of the present invention is to provide a transfer laminate capable of more smoothly transferring a lithium metal layer onto the upper surface of the negative electrode active material layer in order to resolve the aforementioned problems, while using only a high-content silicon-based active material as the negative electrode active material to improve capacity performance.
[0091] Meanwhile, the average particle size (D50) of the silicon-based active material of the present invention may be 5㎛ to 10㎛, specifically 5.5㎛ to 8㎛, and more specifically 6㎛ to 7㎛. When the average particle size falls within the above range, the specific surface area of the particles is within a suitable range, and the viscosity of the cathode slurry is formed within an appropriate range. Accordingly, the dispersion of particles constituting the cathode slurry becomes smooth. In addition, since the size of the silicon-based active material has a value greater than or equal to the lower limit range, the contact area between the silicon particles and the conductive material is excellent due to the composite composed of the conductive material and the binder within the cathode slurry, which increases the likelihood of the conductive network continuing and thus increases the capacity retention rate. Meanwhile, when the average particle size satisfies the above range, excessively large silicon particles are excluded, and the surface of the cathode is formed smoothly, thereby preventing current density non-uniformity during charging and discharging.
[0092] In one embodiment of this specification, the silicon-based active material generally has a characteristic BET surface area. The BET surface area of the silicon-based active material is preferably 0.01 to 150.0 m² 2 / g, more preferably 0.1 to 100.0 m 2 / g, particularly preferably 0.2 to 80.0 m 2 / g, most preferably 0.2 to 18.0 m 2 / g. The BET surface area is measured according to DIN 66131 (using nitrogen).
[0093] In one embodiment of this specification, the silicon-based active material may exist in, for example, a crystalline or amorphous form and is preferably not porous. The silicon particles are preferably spherical or fragmentary particles. Alternatively, but less preferably, the silicon particles may also have a fibrous structure or exist in the form of a silicon-containing film or coating.
[0094] In one embodiment of the present specification, the silicon-based active material may be 60 parts by weight or more based on 100 parts by weight of the negative electrode active material layer composition.
[0095] In another embodiment, the silicon-based active material may comprise at least 60 parts by weight, preferably at least 65 parts by weight, more preferably at least 70 parts by weight, based on 100 parts by weight of the negative electrode active material layer composition, and may comprise 95 parts by weight or less, preferably 90 parts by weight or less, more preferably 80 parts by weight or less.
[0096] The negative electrode active material layer composition according to the present application uses a conductive material and a binder capable of controlling the volume expansion rate during the charging and discharging process even when using a silicon-based active material with significantly high capacity within the above range, thereby not degrading the performance of the negative electrode even when including the above range and having excellent output characteristics during charging and discharging.
[0097] Conventionally, it was common practice to use only graphite-based compounds as negative electrode active materials; however, with the recent rise in demand for high-capacity batteries, there have been increasing attempts to mix in silicon-based compounds to increase capacity. Nevertheless, silicon-based compounds have a limitation in that their volume expands rapidly during the charging and discharging process, damaging the conductive pathways formed within the negative electrode active material layer and actually degrading battery performance.
[0098] Accordingly, in one embodiment of the present specification, the cathode conductive material may include one or more selected from the group consisting of a point-type conductive material; a linear conductive material; and a planar conductive material.
[0099] In one embodiment of the present specification, the point-shaped conductive material can be used to improve conductivity of the cathode and refers to a conductive material having conductivity without causing chemical changes. Specifically, the point-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, Farnes black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably may include carbon black in terms of achieving high conductivity and excellent dispersibility.
[0100] In one embodiment of this specification, the point-shaped conductive material has a BET specific surface area of 40 m² 2 / g or more 70m 2 It may be less than / g, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 It may be less than / g.
[0101] In one embodiment of the present specification, the particle size of the dot-shaped conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 20 nm to 60 nm.
[0102] In one embodiment of the present specification, the conductive material may include a planar conductive material.
[0103] The above-mentioned planar conductive material can be described as a plate-shaped conductive material or a bulk-shaped conductive material, as it can improve conductivity by increasing surface contact between silicon particles within the cathode and simultaneously suppress the interruption of conductive pathways due to volume expansion.
[0104] In one embodiment of the present specification, the planar conductive material may comprise at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and preferably may be plate-shaped graphite.
[0105] In one embodiment of the present specification, the average particle size (D50) of the planar conductive material may be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 4 μm to 5 μm. When the above range is satisfied, dispersion is easy without causing an excessive increase in the viscosity of the cathode slurry due to the sufficient particle size. Therefore, when dispersion is performed using the same equipment and time, the dispersion effect is excellent.
[0106] In one embodiment of the present specification, the planar conductive material provides a cathode composition in which D10 is 0.5 μm or more and 1.5 μm or less, D50 is 2.5 μm or more and 3.5 μm or less, and D90 is 7.0 μm or more and 15.0 μm or less.
[0107] In one embodiment of the present specification, the planar conductive material may be a planar conductive material with a high specific surface area and a high BET specific surface area; or a planar conductive material with a low specific surface area.
[0108] In one embodiment of the present specification, a planar conductive material with a high specific surface area or a planar conductive material with a low specific surface area may be used without limitation as the planar conductive material; however, since the planar conductive material according to the present application may be affected to some extent by dispersion in electrode performance, it may be particularly preferable to use a planar conductive material with a low specific surface area that does not cause problems with dispersion.
[0109] In one embodiment of this specification, the planar conductive material has a BET specific surface area of 5 m² 2 It can be more than / g.
[0110] In another embodiment, the planar conductive material has a BET specific surface area of 5m² 2 / g or more than 500m 2 It may be less than / g, preferably 5m 2 / g or more than 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2 It may be less than / g.
[0111] In another embodiment, the planar conductive material is a high specific surface area planar conductive material, and has a BET specific surface area of 50 m² 2 / g or more than 500m 2 / g or less, preferably 80m 2 / g or more than 300m 2 / g or less, more preferably 100m 2 / g or more than 300m 2 It can satisfy a range of / g or less.
[0112] In another embodiment, the planar conductive material is a low specific surface area planar conductive material, and the BET specific surface area is 5m² 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2It can satisfy a range of / g or less.
[0113] Other conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. The bundled carbon nanotubes may comprise a plurality of carbon nanotube units. Specifically, "bundle type" here refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged parallel or intertwined with the axes along the longitudinal direction of the carbon nanotube units having substantially the same orientation, unless otherwise noted. The carbon nanotube units have a graphite sheet having a cylindrical shape with a nano-sized diameter, and sp 2 It has a bonded structure. At this time, depending on the angle and structure in which the graphite plane is rolled, it may exhibit conductive or semiconductor characteristics. Compared to entangled type carbon nanotubes, the bundled carbon nanotubes can be uniformly dispersed during cathode manufacturing and smoothly form a conductive network within the cathode, thereby improving the conductivity of the cathode.
[0114] In one embodiment of the present specification, the cathode conductive material may be 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the cathode active material layer composition.
[0115] In another embodiment, the cathode conductive material may comprise 10 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, based on 100 parts by weight of the cathode active material layer composition, and more preferably 10 parts by weight or more and 20 parts by weight or less.
[0116] The cathode conductive material according to the present application has a completely separate composition from the conductive material applied to the anode. That is, the cathode conductive material according to the present application serves to hold the contact points between silicon-based active materials, which undergo significant volume expansion of the electrodes due to charging and discharging, whereas the anode conductive material serves as a buffer during rolling and provides partial conductivity; thus, their composition and roles are completely different from those of the cathode conductive material of the present invention.
[0117] Furthermore, the cathode conductive material according to the present application is applied to silicon-based active materials and has a completely different composition from that of a conductive material applied to graphite-based active materials. That is, a conductive material used in an electrode having a graphite-based active material simply has particles smaller than the active material, thereby providing improved output characteristics and some conductivity; thus, its composition and role are completely different from that of a cathode conductive material applied together with a silicon-based active material as in the present invention.
[0118] In one embodiment of this specification, the planar conductive material used as the aforementioned negative electrode conductive material has a structure and function different from that of the carbon-based active material generally used as the negative electrode active material. Specifically, the carbon-based active material used as the negative electrode active material may be artificial graphite or natural graphite, and refers to a material processed into a spherical or dot shape to facilitate the storage and release of lithium ions.
[0119] On the other hand, planar conductive materials used as cathode conductive materials are substances having a planar or plate-like form, which can be described as plate-like graphite. In other words, they refer to materials included to maintain conductive pathways within the cathode active material layer; they do not serve the role of lithium storage or release, but rather are materials intended to secure conductive pathways in a planar form within the cathode active material layer.
[0120] In other words, in the present application, the fact that plate-shaped graphite is used as a conductive material means that it is processed into a planar or plate-shaped form and used as a material that secures a conductive pathway rather than serving the role of storing or releasing lithium. At this time, the negative electrode active material included together has high capacity characteristics for lithium storage and release and plays a role in storing and releasing all lithium ions delivered from the positive electrode.
[0121] On the other hand, in the present application, the fact that a carbon-based active material is used as an active material means that it is processed into a point or spherical shape and used as a material that serves the role of storing or releasing lithium.
[0122] That is, in one embodiment of this specification, artificial graphite or natural graphite, which is a carbon-based active material, has a BET specific surface area of 0.1 m² 2 / g or more than 4.5m 2 It can satisfy a range of / g or less. In addition, plate-shaped graphite, a planar conductive material, has a planar form with a BET specific surface area of 5m² 2 It can be more than / g.
[0123] In one embodiment of the present specification, the cathode binder may comprise at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and materials in which hydrogens thereof are substituted with Li, Na, or Ca, etc., and may also comprise various copolymers thereof.
[0124] The cathode binder according to one embodiment of the present specification serves to hold the active material and the conductive material to prevent distortion and structural deformation of the cathode structure during volume expansion and relaxation of the silicon-based active material. Any general binder that satisfies the above role may be applied, specifically a water-based binder may be used, and more specifically, a PAM-based binder may be used.
[0125] In one embodiment of the present specification, the step of laminating the transfer laminate to transfer a lithium metal layer on the opposite side of the surface of the negative active material layer in contact with the negative current collector layer comprises: the step of laminating the transfer laminate so that the opposite side of the surface of the lithium metal layer in contact with the substrate layer in contact with the opposite side of the surface of the negative active material layer in contact with the negative current collector layer; and the step of removing the substrate layer, thereby providing a method for manufacturing a negative electrode for a lithium secondary battery.
[0126] FIG. 1 is a diagram illustrating a method for manufacturing a negative electrode for a lithium secondary battery according to one embodiment of the present specification. Specifically, the process involves preparing a transfer laminate (200) comprising a substrate layer (40), a release layer (30), and a lithium metal layer (35), stacking the negative electrode (200) for a lithium secondary battery in which a negative electrode active material layer (20) is formed on a negative electrode current collector layer (10) so that the negative electrode active material layer (20) and the lithium metal layer (35) are in contact, and then removing the substrate layer (40) to transfer only the lithium metal layer (35) onto the negative electrode active material layer (20).
[0127] In particular, the method includes the step of transferring a lithium metal layer through a transfer laminate including a specific substrate layer according to the present application as described above, thereby having the feature of being able to transfer the lithium metal layer more easily.
[0128] In one embodiment of the present specification, the laminating step is to perform lamination with a load of 200 kgf, thereby providing a method for manufacturing a negative electrode for a lithium secondary battery.
[0129] The above lamination can be performed through a transfer process via roll pressing. Subsequently, a process for removing the substrate layer is included. By including a release layer according to the present application during removal, direct contact between the lithium metal layer and the air can be prevented, thereby protecting the lithium metal layer. Furthermore, due to the presence of the release layer, the substrate layer can be easily removed with only weak linear pressure, allowing for easy control of the pre-lithiation rate. Additionally, removing the substrate layer facilitates the release of heat generated during pre-lithiation, thereby suppressing the formation of by-products.
[0130] In this specification, after the step of transferring the lithium metal layer, the method may further include a step of pre-lithiating the negative electrode active material layer. At this time, the process may be carried out simultaneously with the transfer of the lithium metal layer onto the negative electrode active material layer, and it can be confirmed that pre-lithiation is completed when the lithium metal layer is completely removed visually.
[0131] In one embodiment of the present specification, the method for manufacturing a negative electrode for a lithium secondary battery further comprises, after the step of transferring the lithium metal layer, the step of pre-lithiating the negative electrode active material layer, wherein the step of pre-lithiating the negative electrode active material layer is performed within 30 minutes to 48 hours after transferring the lithium metal.
[0132] As described above, the substrate layer can be removed immediately after the lithium metal layer transfer, and since the removal of the substrate layer proceeds easily, heat dissipation is facilitated during pre-lithiation in which the lithium metal layer reacts with the negative electrode active material layer, resulting in less byproduct generation and, consequently, the negative electrode active material layer can be uniformly pre-lithiated.
[0133] The above pre-lithiation completion time can be calculated by measuring the time from the time of lithium metal transfer until the transferred lithium metal is not observed on the surface of the negative electrode active material layer.
[0135] <Cathode for Lithium Secondary Batteries>
[0136] In one embodiment of the present specification, a negative electrode for a lithium secondary battery is provided according to the method for manufacturing a negative electrode for a lithium secondary battery. The negative electrode according to the present embodiment may be subject to the above-described details.
[0138] Lithium secondary battery
[0139] In one embodiment of the present specification, a lithium secondary battery is provided comprising: a first electrode; a second electrode; a separator provided between the first electrode and the second electrode; and an electrolyte, wherein either of the first electrode and the second electrode comprises a negative electrode for the lithium secondary battery.
[0140] In the present specification, the first electrode may be an anode and the second electrode may be a cathode, or the first electrode may be a cathode and the second electrode may be an anode.
[0141] In the present specification, the positive electrode may include a positive electrode current collector layer and a positive electrode active material layer formed on the positive electrode current collector layer and comprising the positive electrode active material.
[0142] In the above-mentioned positive electrode, the positive electrode current collector layer is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector layer may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the positive electrode current collector layer to increase the adhesion of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0143] The above-mentioned positive electrode active material may be a commonly used positive electrode active material. Specifically, the above-mentioned positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+c 1Mn 2-c1Lithium manganese oxides such as O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7, etc.; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3 Examples include lithium manganese composite oxides represented by O2 (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, satisfying 0.01≤c3≤0.1) or Li2Mn3MO8 (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); and LiMn2O4 in which a portion of the Li in the chemical formula is substituted with alkaline earth metal ions, but are not limited thereto. The anode may also be Li-metal.
[0144] The above-described positive active material layer may include a positive conductive material and a positive binder together with the positive active material described above.
[0145] At this time, the above-mentioned positive conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that has electronic conductivity without causing chemical changes can be used without special limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive whiskey such as zinc oxide or potassium titanate; conductive metal oxide such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used.
[0146] In addition, the anode binder serves to improve adhesion between anode active material particles and adhesion between the anode active material and the anode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.
[0147] As a separator, it separates the negative and positive electrodes and provides a pathway for the movement of lithium ions. Any separator typically used in secondary batteries may be used without special restrictions, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity. Specifically, a porous polymer film, such as a porous polymer film made from a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.
[0148] FIG. 2 is a diagram showing a stacked structure of a lithium secondary battery according to one embodiment of the present specification. Specifically, a negative electrode (100) for a lithium secondary battery including a negative active material layer (20) on one surface of a negative current collector layer (10) can be seen, and a positive electrode (300) for a lithium secondary battery including a positive active material layer (70) on one surface of a positive current collector layer (60) can be seen, and the structure is formed such that the negative electrode (200) for a lithium secondary battery and the positive electrode (100) for a lithium secondary battery are stacked with a separator (50) in between.
[0149] At this time, the release layer transferred together during pre-lithiation may be partially removed depending on the electrolyte used, and thus a small amount is contained on the upper part of the cathode. The release layer is not shown in Fig. 2.
[0150] In one embodiment of the present specification, the electrolyte may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc., which can be used in the manufacture of a lithium secondary battery, but is not limited to these.
[0151] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0152] As the above-mentioned non-aqueous organic solvent, for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyl lactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolone, formamide, dimethylformamide, dioxolone, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolone derivative, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivative, tetrahydrofuran derivative, ether, methyl propionate, ethyl propionate, etc. may be used.
[0153] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts, so they can be used preferably. Furthermore, if low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed with these cyclic carbonates in appropriate proportions, an electrolyte with high electrical conductivity can be produced, making it even more preferable to use.
[0154] The metal salt mentioned above may be a lithium salt, and the lithium salt is a substance that dissolves well in the non-aqueous electrolyte; for example, as the anion of the lithium salt, F - , Cl - , I -, NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6-, (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more types selected from the group consisting of can be used.
[0155] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride.
[0156] One embodiment of the present invention provides a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the same. Since the battery module and the battery pack include the secondary battery having high capacity, high rate capability and cycle capability, they can be used as a power source for a medium-to-large device selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles and power storage systems.
[0157] Hereinafter, preferred embodiments are presented to aid in understanding the present invention; however, the above embodiments are merely illustrative of the description, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and spirit of the description, and that such variations and modifications fall within the scope of the appended claims.
[0159] Manufacturing Example. Manufacturing of a transfer laminate
[0160] Preparation Example 1
[0161] Polyethylene terephthalate was prepared as a substrate layer, and a film (manufacturer: I-One Film) coated with 1 μm of acrylic resin was prepared as a release layer on the substrate layer. A lithium metal layer was deposited on the release layer by a thermal evaporation method to form a lithium metal layer with the thickness listed in Table 1 below, thereby manufacturing a transfer laminate. At this time, the deposition machine was an EWK-060 from ULVAC, and the deposition process was carried out with the speed set to 2.5 m / min, the temperature of the lithium supply unit set to 500°C, and the temperature of the main roll set to -25°C.
[0163] Example. Surface treatment of a transfer laminate
[0164] Example 1
[0165] Each of the previously manufactured transfer laminates (Li Film, Li thickness 3μm) is placed inside the chamber, and 10 -3After creating a vacuum below torr, the vacuum valve was closed and the gas purge valve was opened, and argon (gas) and carbon dioxide (gas) were injected into the chamber at room temperature in a ratio of 8:2.
[0166] Each gas was purged until the vacuum level of the chamber reached atmospheric pressure, and after processing for 30 minutes, the surface color difference of the lithium metal layer (film) was analyzed using CM-2600d.
[0167] After attaching the above surface-treated transfer laminate (Li Film) to both sides of the silicon anode, lithium was transferred to the electrode portion using a rolling machine with a load of about 200 kgf.
[0169] Example 2
[0170] The procedure was carried out in the same manner as Example 1, except that the Li thickness (thickness of the lithium metal layer) of the transfer laminate used was 4 μm.
[0172] Example 3
[0173] The procedure was carried out in the same manner as Example 1, except that the Li thickness of the transfer laminate used was 5 μm.
[0175] Example 4
[0176] The procedure was carried out in the same manner as Example 1, except that the Li thickness of the transfer laminate used was 6 μm.
[0178] Example 5
[0179] Each of the previously manufactured transfer laminates (Li Film, Li thickness 6μm) is placed inside the chamber, and 10 -3 After creating a vacuum below torr, the vacuum valve was closed and the gas purge valve was opened, and argon (gas) and carbon dioxide (gas) were injected into the chamber at room temperature in a ratio of 8:2.
[0180] After purging each gas until the vacuum level of the chamber reaches atmospheric pressure, the temperature of the chamber is 60 o It was maintained at C. After gas treatment for 5 hours, the surface color difference of the lithium metal layer was analyzed using CM-2600d.
[0181] After attaching the above surface-treated transfer laminate (Li Film) to both sides of the silicon anode, lithium was transferred to the electrode portion using a rolling machine with a load of about 200 kgf.
[0183] Example 6
[0184] The procedure was carried out in the same manner as Example 5, except that gas treatment was performed for approximately 24 hours.
[0186] Example 7
[0187] The procedure was carried out in the same manner as in Example 5, except that gas treatment was performed for about 12 hours.
[0189] Example 8
[0190] The procedure was carried out in the same manner as Example 1, except that the Li thickness of the transfer laminate used was 9 μm.
[0192] Comparative Example 1
[0193] The surface color difference of the lithium metal layer of the Li 6μm thick transfer laminate prepared in Preparation Example 1 was analyzed using CM-2600d without purging with additional gas.
[0194] After attaching the above surface-treated transfer laminate (Li Film-lithium metal layer) to both sides of the silicon anode, lithium was transferred to the Si electrode portion prepared in Preparation Example 2 using a rolling machine with a load of approximately 200 kgf. At this time, a 5 cm x 5 cm electrode was used for the transfer.
[0196] Comparative Example 2
[0197] Each of the previously manufactured transfer laminates (Li Film, Li thickness 6μm) is placed inside the chamber, and 10 -3 After creating a vacuum below torr, close the vacuum valve and open the gas purge valve, then 25 After purging each gas with CDA (Cleaned Dry Air, dew point -40 ℃) at ℃ until the vacuum level of the chamber reaches atmospheric pressure, the chamber temperature is 25 It was maintained at ℃. After gas treatment for 30 min, the surface color difference of the lithium metal layer was analyzed using CM-2600d.
[0198] After attaching the above surface-treated transfer laminate (Li Film-lithium metal layer) to both sides of the silicon anode, lithium was transferred to the Si electrode portion prepared in Preparation Example 2 using a rolling machine with a load of approximately 200 kgf. At this time, a 5 cm x 5 cm electrode was used for the transfer.
[0200] Comparative Example 3
[0201] Each of the previously manufactured transfer laminates (Li Film, Li thickness 6μm) is placed inside the chamber, and 10 -3 After creating a vacuum below torr, close the vacuum valve and open the gas purge valve, then 25 Argon (gas) and carbon dioxide (gas) were injected into the chamber at a ratio of 99:1 at ℃.
[0202] After purging each gas until the vacuum level of the chamber reaches atmospheric pressure, the temperature of the chamber is 25 It was maintained at ℃. After gas treatment for 30 min, the surface color difference of the lithium metal layer was analyzed using CM-2600d.
[0203] After attaching the surface-treated transfer laminate (Li Film) to both sides of the silicon anode, lithium was transferred to the Si electrode portion prepared in Preparation Example 2 using a rolling machine with a load of approximately 200 kgf. At this time, a 5 cm x 5 cm electrode was used for the transfer.
[0205] Comparative Example 4
[0206] Each of the previously manufactured transfer laminates (Li Film, Li thickness 6μm) is placed inside the chamber, and 10 -3 After creating a vacuum below torr, close the vacuum valve and open the gas purge valve, then 25 Argon (gas) and carbon dioxide (gas) were injected into the chamber at a ratio of 8:2 at ℃.
[0207] After purging each gas until the vacuum level of the chamber reaches atmospheric pressure, the temperature of the chamber is 10 It was maintained at ℃. After gas treatment for 30 min, the surface color difference of the lithium metal layer was analyzed using CM-2600d.
[0208] After attaching the surface-treated transfer laminate (Li Film) to both sides of the silicon anode, lithium was transferred to the Si electrode portion prepared in Preparation Example 2 using a rolling machine with a load of approximately 200 kgf. At this time, a 5 cm x 5 cm electrode was used for the transfer.
[0210] Comparative Example 5
[0211] Each of the previously manufactured transfer laminates (Li Film, Li thickness 6μm) is placed inside the chamber, and 10 -3 After creating a vacuum below torr, close the vacuum valve and open the gas purge valve, then 25 Argon (gas) and carbon dioxide (gas) were injected into the chamber at a ratio of 8:2 at ℃.
[0212] After purging each gas until the vacuum level of the chamber reaches atmospheric pressure, the temperature of the chamber is 25 It was maintained at ℃. After gas treatment for 3 min, the surface color difference of the lithium metal layer was analyzed using CM-2600d.
[0213] After attaching the surface-treated transfer laminate (Li Film) to both sides of the silicon anode, lithium was transferred to the Si electrode portion prepared in Preparation Example 2 using a rolling machine with a load of approximately 200 kgf. At this time, a 5 cm x 5 cm electrode was used for the transfer.
[0215] [Measurement of heating temperature]
[0216] The heating temperatures of the electrodes of Examples 1 to 8 and Comparative Examples 1 to 5 were measured in the following manner. Immediately after transferring Li to the electrode portion, the PET was removed, and a TC (Thermocouple) was attached to the center of the surface of the electrode on which Li was transferred, and the maximum value of the heating electrode surface temperature was measured.
[0218] The results of Examples 1 to 8 and Comparative Examples 1 to 5 above are shown in Table 1 below.
[0220] No. Surface Treatment (Gas Type, Treatment Temperature and Time)_Thickness of Lithium Metal Layer SCI mode SCE mode Heat temperature (°C) immediately after transfer L* a* b* L* a* b* Comparative Example 1 Untreated_6μm 94.65 4.55 6.42 15.80 17.85 26.95 60 Comparative Example 2 CDA(Room temperature, 30 min)_6μm 94.12 3.85 6.99 19.84 14.17 30.81 50 Comparative Example 3 Ar:CO2=99:1(25℃, 30min)_6μm 93.95 3.75 7.07 20.73 12.51 30.55 50 Comparative Example 4 Ar:CO2=8:2(10℃, 30min)_6μm 94.25 -0.23 9.96 28.35 2.82 21.28 38 Comparative Example 5 Ar:CO2=8:2(25℃, 3min)_6μm 94.15 -0.47 9.22 32.19 0.26 5.17 42 Example 1 Ar:CO2=8:2(25℃, 30min)_3μm 95.01 -0.34 10.20 42.51 0.27 6.73 24 Example 2 Ar:CO2=8:2(25℃, 30min)_4μm 93.77 0.45 10.80 43.92 -0.56 2.62 24 Example 3 Ar:CO2=8:2 (25℃, 30min)_5μm 92.46 1.38 12.68 45.64 0.27 3.77 28 Example 4 Ar:CO2=8:2 (25℃, 30min)_6μm 91.85 0.95 12.48 42.24 0.58 4.71 28 Example 5 Ar:CO2=8:2 (60℃, 5hr)_6μm 91.98 0.92 9.65 62.81 -0.39 0.40 24 Example 6 Ar:CO2=8:2 (60℃, 24hr)_6μm 90.99 1.15 10.00 82.80 0.41 7.88 24 Example 7 Ar:CO2=8:2 (60℃, 12hr)_6μm 94.32 0.04 8.17 70.89 -1.14 3.46 24 Example 8 Ar:CO2=8:2 (25℃, 30min)_9μm 93.02 0.36 11.75 51.70 -0.72 2.64 30
[0222] However, in Table 1 above, CDA means the same as the components of the general atmosphere.
[0224] According to Table 1 above, in the case of Comparative Examples 1 to 5, even if the lightness (L) measured in SCI mode was 90 or higher, the lightness (L) measured in SCE mode was less than 40, and thus it can be confirmed that the heat generation temperature immediately after transfer was 38℃ or higher.
[0225] In contrast, in the case of Examples 1 to 8, the lightness (L) measured in SCI mode was 90 or higher, and the lightness (L) measured in SCE mode was 40 or higher, thereby confirming that the heat generation temperature immediately after transfer was low at 30℃ or lower.
[0226] In particular, as in Comparative Examples 2 and 3, the content of carbon dioxide in the surface treatment gas (where trace amounts of carbon dioxide are present in CDA, or in a ratio of Ar:CO2 = 99:1) is changed, respectively, or as in Comparative Example 4, the temperature of the chamber after purging the surface treatment gas is 10 When the temperature was lowered to ℃ or the surface treatment time was set to a short 3 min, as in Comparative Example 5, the brightness measured in SCE mode was less than 40 in all cases. According to these results, compared to the Comparative Example group, in the Example group, it is easy to predict whether lithium carbonate (Li2CO3) is formed within a short time even if the surface treatment conditions are slightly changed, so the degree of surface treatment can be precisely determined, and accordingly, the temperature of heat generation immediately after transfer can be easily predicted, thereby significantly reducing the risk of ignition during pre-lithiation. Explanation of the symbols
[0227] 10: Cathode current collector layer 20: Cathode active material layer 35: Lithium metal layer 30: Heterogeneous layer 40: Base layer 50: Separator 60: Positive current collector layer 70: Positive active material layer 100: Negative electrode for lithium secondary battery 200: Transfer laminate 300: Cathode for lithium secondary batteries
Claims
Claim 1 A transfer laminate comprising a substrate layer and a lithium metal layer on one surface of the substrate layer, wherein the lithium metal layer comprises a surface protective film on its surface, the surface protective film comprises lithium carbonate (Li2CO3), and the surface color difference with respect to the surface of the lithium metal layer comprising the surface protective film satisfies the following equation (1): L SCE ≥ 40 - Equation (1) In the above Equation (1), L SCE represents the brightness index measured in SCE (Specular component excluded) mode. Claim 2 A transfer laminate according to claim 1, wherein the surface color difference with respect to the surface of the lithium metal layer including the surface protective film satisfies the following formula (2): L SCI L ≥ 90 measured in (Specular component included) mode - Equation (2) In the above Equation (2), L SCI represents the lightness index measured in SCI (Specular component included) mode. Claim 3 A transfer laminate according to claim 1, wherein the surface of the lithium metal layer further comprises one or more components selected from LiOH, Li3N, Li2O, Li2O2, and combinations thereof. Claim 4 A transfer laminate according to claim 1, wherein the thickness of the substrate layer is 5 μm or more and 300 μm or less. Claim 5 A transfer laminate according to claim 1, wherein the substrate layer is one or more selected from the group consisting of polyethylene terephthalate (PET), polyethylenenaphthalate (PEN), polyimide (PI), poly(methylmethacrylate), PMMA, polypropylene, polyethylene, and polycarbonate. Claim 6 A transfer laminate according to claim 1, wherein the thickness of the lithium metal layer is 1 μm or more and 10 μm or less. Claim 7 A transfer laminate according to claim 1, further comprising a release layer between the substrate layer and the lithium metal layer. Claim 8 A transfer laminate according to claim 7, wherein the thickness of the release layer is 0.1 μm or more and 10 μm or less. Claim 9 A method for manufacturing a negative electrode for a lithium secondary battery, comprising: a step of preparing a negative electrode for a lithium secondary battery by forming a negative current collector layer and a negative active material layer on one or both sides of the negative current collector layer; and a step of transferring a lithium metal layer by laminating a transfer laminate of any one of claims 1 to 8 onto the opposite side of the negative active material layer that contacts the negative current collector layer. Claim 10 A method for manufacturing a negative electrode for a lithium secondary battery according to claim 9, wherein the step of laminating the transfer laminate on the opposite side of the surface of the negative active material layer in contact with the negative current collector layer to transfer a lithium metal layer comprises: the step of laminating the transfer laminate so that the opposite side of the surface of the lithium metal layer in contact with the substrate layer contacts the opposite side of the surface of the negative active material layer in contact with the negative current collector layer; and the step of removing the substrate layer. Claim 11 A method for manufacturing a negative electrode for a lithium secondary battery according to claim 9, wherein the lamination is performed with a load of 200 kgf. Claim 12 A method for manufacturing a negative electrode for a lithium secondary battery according to claim 9, further comprising the step of pre-lithiating the negative electrode active material layer after the step of transferring the lithium metal layer, wherein the step of pre-lithiating the negative electrode active material layer is performed within 30 minutes to 48 hours after transferring the lithium metal. Claim 13 A negative electrode for a lithium secondary battery manufactured according to the method for manufacturing a negative electrode for a lithium secondary battery according to claim 9. Claim 14 A lithium secondary battery comprising: a first electrode; a second electrode; a separator provided between the first electrode and the second electrode; and an electrolyte, wherein either of the first electrode and the second electrode comprises a negative electrode for a lithium secondary battery according to claim 13.
Citation Information
Patent Citations
Lithium Metal Electrode and Lithium Secondary Battery Comprising the Same
KR1020180137989A
Lithium thin film lamination technology on electrode to increase battery capacity
WO2001006578A2