Method for producing silicon composites

The method addresses the inefficiencies of existing silicon composite production by controlling thermal decomposition parameters, ensuring uniform silicon deposition and reducing thick layer formation, enhancing electrochemical performance and stability in lithium-ion battery anodes.

KR103046745B1Active Publication Date: 2026-11-10WACKER CHEMIE AG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020237039434
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-20
Filing Date
2022-12-20
Publication Date
2026-11-10
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

Existing methods for producing silicon composites for lithium-ion battery anodes face challenges such as the formation of a thick silicon layer, which leads to mechanical stress and capacity loss due to volume changes, and require long reaction times and high inert gas consumption, making the process economically inefficient.

Method used

A method involving the thermal decomposition of Si precursors in the presence of porous particles, with controlled variations in temperature, precursor concentration, and flow rate, allowing for uniform deposition of silicon within and on the particles, reducing the formation of a thick silicon layer and enhancing cycle stability.

Benefits of technology

The method achieves a high conversion rate of Si precursors, resulting in a silicon composite with improved electrochemical performance and stability, while reducing process time and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023126543741-PCT00003
    Figure 112023126543741-PCT00003
  • Figure 112023126543741-PCT00004
    Figure 112023126543741-PCT00004
  • Figure 112023126543741-PCT00005
    Figure 112023126543741-PCT00005
Patent Text Reader

Abstract

The present invention relates to a method for producing a silicon composite by the pyrolysis of at least one silicon precursor in the presence of porous particles, wherein the silicon is deposited in pores and on the surface of the porous particles, and the silicon composite has a target Si content of 35 wt% to 60 wt%, wherein the method is performed at an average temperature T of 300°C to 500°C and a silicon precursor concentration C of 30 vol% to 100 vol% in a regular operation. The method comprises at least one step A in which a change Δ of at least one of parameters T and C is affected for the regular operation and optionally for an additional phase A, wherein ΔT = 10°C to 130°C and ΔC = 2 vol% to 70 vol%. Conditions apply such that 0.1% to 50% of the target silicon content mentioned is deposited during step A, or that up to 50% of the target silicon content mentioned is deposited overall over two or more steps A.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for producing a silicon composite by the thermal decomposition of at least one Si precursor in the presence of porous particles, wherein the silicon is deposited in the pores and on the surface of the porous particles, and the silicon composite has a target silicon content of 35% to 60% by weight. Background Technology

[0002] As an electrical storage medium, lithium-ion batteries (LIBs) are currently the most practical electrochemical energy storage devices with the highest energy density. LIBs are primarily used in portable electronics, tools, and electric-powered vehicles such as bicycles, scooters, or automobiles. Graphite carbon is currently widely used as the active material for the negative electrode (anode). A disadvantage is that the electrochemical capacity of this carbon is relatively low; theoretically, it is up to 372 mAh per gram of graphite, which corresponds to about one-tenth of the electrochemical capacity theoretically achievable with lithium metal. As described in EP 1730800 B1 or EP 3335262 B1, alternative active materials for the anode use silicon additives. Silicon forms an electrochemically active binary alloy with lithium, allowing for a very high electrochemically achievable lithium content of up to 3579 mAh per gram of silicon.

[0003] The intercalation and deintercalation of Li ions in silicon have the disadvantage of being accompanied by very high volume changes, which can reach up to 300% in the case of complete intercalation. These volume changes apply severe mechanical stress to the silicon-containing active material, which can eventually cause the active material to break down. This process, also known as electrochemical grinding, results in electrical contact loss in the active material and electrode structure, leading to an irreversible loss of electrode capacitance.

[0004] Furthermore, the surface of the silicon-containing active material can react with the components of the electrolyte to form a passivation protective layer (solid electrolyte interface; SEI). The formed components are no longer electrochemically active. Since the lithium bound within it can no longer be used in the system, the capacity of the LIB is significantly lost. Due to volume changes in silicon during the charging and discharging process of the LIB, the SEI regularly ruptures, exposing more of the empty surface of the Si-containing active material and forming additional SEIs. Because the amount of mobile lithium corresponding to the available capacity in the LIB is limited by the cathode material, it is increasingly consumed, and the capacity decreases after only a few cycles.

[0005] Active materials known for use in LIB anodes include Si-C composite particles in which silicon, in the form of gaseous or liquid precursors, is embedded within porous C particles. The advantage of Si-C composites is that silicon is finely distributed and embedded within a carbon framework that maintains electrical contact while allowing for volume variations of the silicon. These Si-C composites are produced, for example, by vapor deposition of one or more Si precursors into the pores of a porous carbon matrix. Introducing silicon into a porous structure is a chemical vapor penetration (CVI: chemical vapor infiltration It is also known as ).

[0006] When Si composites are produced by CVI, Si precursors are typically used at low absolute and partial pressures and low concentrations; consequently, long reaction times are required to achieve a high Si ratio in silicon-containing materials because a thick Si layer, also known as coarse silicon, forms on the exterior of the particles. This thick Si layer is detrimental in that it comes into contact with the electrolyte and leads to heavy structuring of the particle surface, along with the continuous reforming of SEI during cycling. Furthermore, the optimal tuning of process parameters requires precise knowledge of all reaction parameters, which must generally be determined empirically. Additionally, since the porous matrix used exhibits a specific range of variation regarding pore and particle size distribution, it is very difficult to prevent excessive infiltration leading to the thick Si layer. Even when infiltration is performed continuously at relatively high concentrations of silicon precursors (Si precursors) and / or relatively high temperatures for reasons of productivity, the thick Si layer is formed.

[0007] WO 2022 / 029422 A1 discloses a Si-C composite produced by CVI containing 25 to 65 wt% silicon. The composite consists of mesoporous and microporous C scaffolds containing various domains of nanoscale elemental silicon inside and on the pores. This can be produced from porous C particles and silane in a fluidized bed reactor at a temperature of 450°C and reduced pressure. To prevent the formation of a thick Si layer (rough bulk silicon), a total silane concentration of less than 20 volume% was used. Such high dilution inevitably leads to long reaction times and high inert gas consumption, which reduces the economics of the process.

[0008] Against this backdrop, the object of the present invention is to provide a method for producing a silicon-containing material that can be obtained more quickly and economically than known production methods while ensuring high cycle stability when used as an active material in the anode of a LIB. Accordingly, the formation of a thick silicon layer must be avoided.

[0009] The present invention relates to a method for producing a silicon composite by the thermal decomposition of at least one Si precursor in the presence of porous particles, wherein the silicon is deposited on the surface of the pores and porous particles, and the silicon composite has a target silicon content of 35% to 60% by weight, and in a regular operation, the method

[0010] - Average temperature T of 300℃ to 500℃, and

[0011] - Concentration of Si precursor C in the supplied gas stream of 30 to 100 volume%

[0012] It is performed in.

[0013] The above method comprises at least one stage A in which a change Δ of at least one of parameters T and C is affected for a regular operation and optionally for an additional stage A, and

[0014] ΔT = 10℃ to 130℃, and

[0015] ΔC = 2 volume% to 70 volume%, and

[0016] However, the condition applies that 0.1% to 50% of the stated target silicon content is deposited during Step A, or that up to 50% of the stated target content is deposited overall during two or more Step As.

[0017] Furthermore, the present invention provides an additional method substantially corresponding to the aforementioned method, and the additional method in a regular operation is

[0018] - Average temperature T of 300℃ to 500℃,

[0019] - Concentration C of Si precursor of 30 volume% to 100 volume%, and

[0020] - Volume flow of Si precursor at 0.01 to 20 NL / h based on 1 g of porous particle VS

[0021] It is performed in.

[0022] The additional method likewise includes at least one step A in which a change Δ of at least one of parameters T, C, and VS is affected for the regular operation and optionally for the additional step A, and

[0023] ΔT = 10℃ to 130℃, and

[0024] ΔC = 2 volume% to 7 volume%, and

[0025] ΔVS = 0.01 to 10 NL / h, and

[0026] However, the condition applies that 0.1% to 50% of the stated target silicon content is deposited during Step A, or that a total of up to 50% of the stated target content is deposited during two or more Step As.

[0027] One advantage of the method according to the present invention is that the conversion rate of the Si precursor exceeds 30% over the entire process period. This also results in high stability of the silicon composite produced when applied as an active material for an anode for LIBs, as silicon is deposited particularly uniformly on the porous particles, especially within the porous particles.

[0028] Dividing the penetration reaction into stages with different process parameters allows for a reduction in the overall process time while maintaining high product performance. Surprisingly, it was found that the conversion rate of the Si precursor supplied under static conditions does not remain constant but rather varies during the reaction period; consequently, the static process mode fails to achieve optimal utilization of the Si precursor. This is compensated for by an adapted process mode of the deposition reaction, which increases the conversion rate.

[0029] In addition, the method according to the present invention surprisingly overcomes the disadvantage of forming a thick Si layer, and as a result, the Si composite obtained by the process has high electrochemical performance.

[0030] In standard operation, the supplied volume flow VS of the Si precursor into the reactor may be 0.01 to 10 NL / h, preferably 0.01 to 5 NL / h, per gram of the porous particles used. The determination of the volume flow may be performed by commonly used methods such as a rotameter.

[0031] ΔVS may be 0.01 to 5 NL / h, preferably 0.01 to 2 NL / h, per gram of porous particles used.

[0032] The silicon composite may have a target content of silicon (obtained by deposition from a Si precursor) of 40% to 55% by weight, preferably 42% to 50% by weight, based on the total weight of the silicon composite.

[0033] The target Si content can be determined empirically through repeated sampling during the process.

[0034] It is desirable to determine the target Si content during the process by analyzing the composition of the off-gas stream using one or more methods selected from the group consisting of gas chromatography, mass spectrometry, infrared spectroscopy, and thermal conductivity measurements.

[0035] The determination of the target Si content is particularly preferably performed by continuous analysis of the off-gas composition by gas chromatography or thermal conductivity measurement. The off-gas flow can be discharged directly from the reactor outlet for gas composition analysis. The determination of the deposited silicon may also be indirectly influenced by the quantification of hydrogen present in the off-gas when hydrogen is not used for silane dilution.

[0036] The average temperature T can be 315°C to 475°C during regular operation, preferably 330°C to 450°C.

[0037] Average temperature T during regular operation R is defined as the average of all temperatures during normal operation. Temperature should be understood as referring to the temperature of the process where the process is controlled. If the temperature of Step A changes by ΔT without interrupting the supply of the Si precursor, the heating or cooling step is considered part of Step A. Then, the average temperature of Step A (T A ) is used.

[0038] ΔT can be 20°C to 100°C, preferably 20°C to 50°C.

[0039] In regular operation, the concentration C can be 30 volume% to 100 volume%, preferably 50 volume% to 100 volume%.

[0040] The value for C is preferably related to the concentration of the Si precursor in the reaction gas, that is, generally the concentration in the supply conduit of the reaction gas to the reactor. The reaction gas generally contains the Si precursor and / or an inert gas such as nitrogen. The concentration of the Si precursor in the supplied reaction gas can be adjusted through a suitable metering device such as a rotameter.

[0041] ΔC can be 5 volume% to 60 volume%, preferably 10 volume% to 50 volume%.

[0042] It is preferable that at least one change Δ of parameters C, T, and VS be performed continuously from the beginning to the end of step A. In certain embodiments, the change may be performed in stages.

[0043] Depending on the determined target content of Si, the change Δ can be started or terminated. That is, step A can be started (deviated from regular operation) or terminated (returned to regular operation) depending on the amount of change Δ.

[0044] It is desirable to perform the process at a pressure of less than 0.7 MPa. In particular, the pressure is maintained substantially constant during the process. Here In reality This means that the pressure fluctuation range may be ±0.1MPa.

[0045] The production of Si composite particles according to the present invention can be carried out in any reactor commonly used for Si infiltration. For example, a reactor selected from a fluidized bed reactor, a retort oven, a tube reactor, a rotary kiln, and a fixed-bed reactor that can be operated as an open or closed system, such as a pressure reactor, which can be oriented in any arrangement from horizontal to vertical, is preferred. A reactor that enables a homogeneous mixing of the porous particles and the silicon-containing material formed during infiltration (only the finished final product is described as a silicon composite) with the Si precursor is particularly preferred. This is advantageous for depositing silicon most uniformly on the pores and the surface of the porous particles. The most preferred reactors are fluidized bed reactors, rotary kilns, pressure reactors, and bed reactors.

[0046] The method according to the present invention is preferably carried out in a reactor equipped with a close-clearance stirrer.

[0047] The above method may be further performed in a cascade reactor system comprising two or more reactors.

[0048] Performing a process in a cascade reactor system can offer advantages over performing the process in a single reactor, as it reduces the need for long cooling and heating phases. This can lead to economic benefits. Cascade reactor systems can also provide the additional advantage of allowing individual reactors to be configured precisely for specific purposes. Cascade reactor systems generally offer higher scalability, as reactors of varying sizes can be combined to form individual phases. Adjustments to temperature, volumetric flow, and concentration can also be achieved by performing Phase A and regular operations across multiple reactors in the reactor cascade.

[0049] The method according to the present invention may include at least three steps:

[0050] Step 1: Filling reactor A with porous particles and pre-treating the particles, then transferring the pre-treated particles to reactor B or a storage vessel, or retaining the material in reactor A.

[0051] Step 2: A step of passing a gas containing a Si precursor through reactor B using a gas, generally an inert gas. A Si-free precursor may also be present; a step of temperature-controlling the reactor to a temperature at which thermal decomposition of the Si precursor occurs on the surface and pores of the porous particles. A method profile is established comprising at least one step A in which at least one of parameters T, C, and VS is varied in addition to the regular operation. The reaction may be carried out under both negative and positive pressure. After introducing silicon into and onto the pores of the porous particles, the Si composite is transferred to reactor C, transferred to a storage vessel for intermediate storage, or the material remains in reactor B.

[0052] Step 3: Post-treatment of the Si composite for functionalization and / or coating of the silicon-containing particle surface. Cool the particles to a defined temperature and recover the Si composite from reactor C, preferably transferring it directly to a storage vessel or filling it directly into a suitable vessel.

[0053] In Step 1, the porous particles are charged into a heatable and / or vacuum-resistant and / or pressure-resistant reactor A. This charging can be performed manually or automatically.

[0054] Charging reactor A with porous particles can be carried out in an inert gas atmosphere or, preferably, in ambient air. Available inert gases include hydrogen, helium, neon, argon, krypton, xenon, nitrogen, carbon dioxide, or mixtures thereof, for example, forming gases. Argon or nitrogen is preferred.

[0055] Automatic filling can be performed through a weighing screw, rotary star valve, vibrating conveyor, plate-type weighing device, belt-type weighing device, vacuum weighing system, negative weighing, or any other weighing system, for example, a silo or other container system.

[0056] The purpose of pre-treating the particles in reactor A of step 1 is to remove air / oxygen, water or dispersants, such as surfactants or alcohols, and impurities from the particles. This can be achieved by inactivating with an inert gas (see previous step), raising the temperature up to 1000°C, lowering the pressure up to 1 Pa, or by combining individual process steps.

[0057] The purpose of the pretreatment in Step 1 may be to alter the chemical surface composition of the porous particles using additional components. Addition may be performed before or after drying, and an additional heating step may be performed before the material is transferred to reactor B. The components may be added to the reactor in gaseous, solid, or liquid form, or in solution form. Mixtures, emulsions, suspensions, aerosols, or foams are also possible. Possible components include carbon dioxide, water, sodium hydroxide solution, potassium hydroxide solution, hydrofluoric acid, phosphoric acid, nitric acid, hydrochloric acid, ammonia, ammonium hydrogen phosphate, lithium nitrate, sodium nitrate, potassium nitrate, lithium chloride, sodium chloride, potassium chloride, lithium bromide, sodium bromide, potassium bromide, and alkoxides.

[0058] Transferring porous particles to additional reactors or vessels can be performed via downpipes, continuous conveyors, flow conveyors / suction or pressure transfer devices (e.g., vacuum conveyors, conveying blowers); mechanical conveyors (e.g., electric roller conveyors, screw conveyors, hanging conveyors, over / under conveyors, bucket conveyors, rotary star valves, chain conveyors, scraper conveyors, conveyor belts, vibrating conveyors); and gravity conveyors (e.g., chutes, roller tracks, ball tracks, rail tracks).

[0059] The material pretreated in step 2 is heated in reactor B to an average temperature of 300°C to 500°C, particularly preferably 315°C to 475°C, particularly preferably 330°C to 450°C.

[0060] During temperature changes, when a temperature is reached, or during the progression of the temperature profile, Reactor B It may be alternately or simultaneously transversely passed by a gas composed of at least one reactive component consisting of at least one inert gas and / or at least one Si precursor and / or at least one Si-free precursor. Different compositions of the gas may be possible sequentially or may be changed within the parameters of the composition specified during step 2.

[0061] A preferred Si-free precursor (a precursor that does not contain a Si precursor) is one or more hydrocarbons. Carbon can generally be deposited in the pores and on the surface of porous particles through the thermal decomposition of hydrocarbons.

[0062] The Si-free precursor preferably does not contain additional components or one or more inert gases and / or one or more reactive components, such as hydrogen, and / or one or more dopants. The dopant may include a compound containing boron, nitrogen, phosphorus, arsenic, germanium, iron, or nickel. The dopant is preferably selected from the group comprising ammonia, diborane, phosphane, germane, arnic acid, and nickel tetracarbonyl.

[0063] The metered addition of reaction gas can be continuous or intermittent. The metered addition rate can vary during the reaction period.

[0064] The temperature, pressure, pressure change or differential pressure, and gas flow of Reactor B can be determined using commonly used measuring equipment and methods. After standard calibration, the same measurement results are generally obtained even when using various measuring instruments.

[0065] A certain amount of Si precursor can be passed through so that a sufficient amount of silicon is deposited for the target capacity of the Si composite to be produced in relation to the weighed amount of porous particles over the entire period of pyrolysis reactor B.

[0066] In step 2, heating of reactor B can be performed at a constant heating rate or at multiple different heating rates. The heating rate can be adjusted according to the process configuration, for example, the size of the reactor, the amount of porous particles in the reactor, the stirring technique, or the planned reaction time.

[0067] In step 2, heating of reactor B can be performed at a heating rate of 1°C to 100°C per minute, preferably 2°C to 50°C per minute.

[0068] The temperature at which the decomposition of the Si precursor begins may vary depending on the porous particles used, the Si precursor used, and other boundary conditions of decomposition, such as the partial pressure of the Si precursor at jucture and the presence of other reactive components, such as catalysts that affect the decomposition reaction.

[0069] During the decomposition of the Si precursor in Step 2, the temperature may be kept constant or varied. The goal is to produce a Si composite suitable for application by largely completely converting the Si precursor during the contact time between the gas and the stirred bed.

[0070] The target temperature of SiH4 may be 300°C to 500°C, preferably 315°C to 475°C, and particularly preferably 330°C to 450°C. The target temperature of HSiCl3 may be 380°C to 1000°C, preferably 420°C to 600°C. The target temperature of H2SiCl2 may be 350°C to 800°C, preferably 380°C to 500°C.

[0071] Si-free precursors, such as C precursors, can be used in step 2 in addition to Si precursors. This can be performed continuously or alternately with a mixture of Si precursors. The goal is targeted functionalization of the newly formed silicon surface.

[0072] The gas phase of step 2 may consist of an inert gas and / or at least one reactive component containing Si and / or potentially at least one Si-free precursor of various compositions. One or more Si precursors may generally be introduced into reactor B in a mixed form, separately, as a mixture with the inert gas component, or as a pure component.

[0073] In step 2, the bed composed of porous particles is preferably continuously recirculated. Recirculation may be achieved through one or more stirring means, or by rotational movement of the reactor itself (e.g., the concentrated mixer of Maschinenfabrik Gustav Eirich), or a combination thereof. The moving state of the bed is characterized by a Froude number of 1 to 10. The Froude number is preferably 1 to 6, particularly preferably 1 to 4.

[0074] The thermal decomposition of the Si precursor in the presence of porous particles is preferably carried out at 0.05 MPa to 5 MPa, particularly preferably at 0.08 to 0.7 MPa.

[0075] The reaction progress of Step 2 is preferably monitored analytically to detect the end of the reaction and thereby keep the reactor occupancy time as short as possible. The process for observing the reaction progress includes additional methods, such as temperature measurements to determine exothermic or endothermic reactions and monitoring the changing composition of the gas space during the reaction, to determine the reaction progress through changes in the ratio of solid to gaseous components of the reactor contents, for example. In a preferred variation of the process, the composition of the gas phase is determined by a gas chromatograph and / or a thermal conductivity detector and / or an infrared spectrometer and / or a Raman spectrometer and / or a mass spectrometer. In a preferred embodiment, the moisture content is determined using a thermal conductivity detector and / or, optionally, the presence of any chlorosilane is determined using a gas chromatograph or a gas infrared spectrometer.

[0076] In a more preferred variation of the method, a technical solution for removing any condensable or re-sublimable byproduct generated at the reactor B / gas outlet location is installed. In a particularly preferred variation, silicon tetrachloride is condensed and removed separately from the Si complex.

[0077] In step 3 of the method, the Si-containing particles in reactor C are post-treated and / or deactivated and / or coated. To this end, reactor C is purged with oxygen, preferably, in particular, a mixture of oxygen and an inert gas. This allows the surface of the Si composite to be modified and / or functionalized and / or deactivated. For example, it is possible to induce a reaction of any reactive groups present on the surface of the Si composite. To this end, it is preferable to use a mixture of nitrogen, oxygen, and optionally alcohol and / or water containing oxygen, preferably up to 20 volume%, particularly preferably up to 10 volume%, particularly preferably up to 5 volume%, and water, preferably up to 100 volume%, particularly preferably up to 10 volume%, particularly preferably up to 1 volume%. This step is preferably performed at a temperature of up to 250°C, particularly preferably up to 100°C, and particularly preferably up to 50°C. Deactivation of the particle surface may also be performed using a gas mixture containing an inert gas and an alcohol. Here, it is preferable to use nitrogen and isopropanol. However, it is also possible to use methanol, ethanol, butanol, pentanol, or long-chain and branched alcohols and diols.

[0078] Inactivation of the particles can also be performed by dispersing them in a liquid solvent or solvent mixture. This may contain isopropanol or an aqueous solution. In step 3, inactivation of the particles can also be performed by coating with C-containing, Al-containing, and B-containing precursors at a temperature of 200°C to 800°C and optionally by subsequent treatment in an oxygen-containing atmosphere.

[0079] Available aluminum-containing precursors are trimethylaluminum ((CH3)3Al), aluminum 2,2,6,6-tetramethyl-3,5-heptanedione (Al(OCC(CH3)3CHCOC(CH3)3)3), tris(dimethylamido)aluminum (Al(N(CH3)2)3) and aluminum triisopropanoleate (C9H 21It includes AlO3.

[0080] Available boron-containing precursors include boran (BH3), triisopropyl borate ([(CH3)2CHO]3B), triphenylborane ((C6H5)3B) and tris(pentafluorophenyl)borane (C6F5)3B.

[0081] In step 3, post-coating of the particles using a solid-state electrolyte may be introduced, for example, by the thermal decomposition of tert-butyllithium and trimethyl phosphate.

[0082] In Step 3, the Si-composite can be recovered from Reactor C in principle while optionally maintaining an inert gas atmosphere present in Reactor C. This can be accomplished via the following discharge methods: pneumatic (via high or low atmospheric pressure); mechanical (rotary star valve, plate discharge device, discharge screw / stirring means within the reactor, belt discharge device); and gravimetric (double-flap valve / ball valve, optionally vibration-assisted).

[0083] When a hydrocarbon is used in Step 3 and / or an additional Si-free precursor is used in addition to Si infiltration in Step 2, the target temperature used is the temperature at which the decomposition of the hydrocarbon begins and carbon is deposited on the surface of the pores and porous particles. In this embodiment, the target temperature selected is preferably in the range of 250°C to 1000°C, particularly preferably 350°C to 850°C, and most preferably 400°C to 650°C.

[0084] Technical requirements for the reactor and optional details regarding specific variations of the invention:

[0085] Reactor A:

[0086] - The reactor is at least temperature-controllable.

[0087] - The reactor may be vacuum-resistant.

[0088] - System for preheating, drying, and inactivating porous particles.

[0089] - A system for target addition / metering addition of porous particles can be connected.

[0090] - Impurities in porous particles can be dried / removed by connecting a system capable of removing condensation or resublimation components.

[0091] - A system connection capable of transferring porous particles to reactor B is possible.

[0092] Reactor B:

[0093] - The reactor is at least temperature-controllable.

[0094] - Includes a stirrer means according to the present invention.

[0095] - Reaction gas metering and addition system

[0096] - Reaction gas discharge system

[0097] - A hydrogen separator can be connected to simplify the process.

[0098] - A vessel capable of removing condensation or resublimation byproducts can be connected to remove condensation or resublimation byproducts generated from gas reaction products.

[0099] - It is possible to connect a system capable of transferring material to reactor C or a storage vessel.

[0100] Reactor C:

[0101] - The reactor is at least temperature-controllable.

[0102] - Condensation or resublimation byproduct removal system.

[0103] - It is possible to connect a container capable of removing by-products by condensation or re-sublimation.

[0104] - Metering and Addition System for Reaction Gases for Functionalization

[0105] - Reaction gas discharge system

[0106] - It is possible to connect a system capable of transferring materials to a storage container.

[0107] The reactor may be simultaneously temperature-controlled, pressure-resistant, and vacuum-resistant; all combinations are possible. However, it is also possible for each reactor to satisfy only one of the aforementioned characteristics.

[0108] A temperature-controllable reactor is generally a reactor that can be operated so that the internal temperature can be adjusted in the range of -40°C to 1000°C. Smaller temperature ranges are also possible.

[0109] It is preferable that reactors A, B, and C are in the same vessel; in other words, the process may be carried out in only one reactor. In principle, the case where reactors A, B, and C are in the same vessel is not excluded.

[0110] It may be provided that the process in normal operation and at least one step A are performed in a single reactor. In certain embodiments, the normal operation and step A may be performed in separate reactors.

[0111] The porous particles and the resulting Si composite may generally be in the form of a fixed bed or a moving bed through mixing during the process. It is preferable to mix to provide a moving bed of porous particles / the resulting Si composite in reactors A, B, and C. However, the particles must generally be mixed while the Si precursor is pyrolyzed in Step 2. This enables ensuring homogeneous contact between all porous particles and the reaction gas or a homogeneous temperature distribution of the bed. Recirculation of the particles can be achieved through stirring inside the reactor or movement of the entire reactor around a stirrer.

[0112] An additional preferred configuration for reactors A, B, and C is a stationary reactor equipped with a moving stirring means for recirculation. The purpose of recirculation is to bring the porous solid into contact with the reaction gas as uniformly as possible. Preferred geometries for this are cylindrical reactors, conical reactors, spherical or polyhedral rotationally symmetric reactors, or combinations thereof. The movement of the stirring means is preferably rotational. For reactors A, B, and C that operate vertically, a configuration in which one stirring means or two or more stirring means mix the bed material through rotational movement, for example, via a main stirring shaft is preferred. An additional configuration for reactors A, B, or C that operate vertically is characterized by the use of a conveying screw. For reactors A, B, or C that operate horizontally, a configuration in which one stirring means or two or more stirring means mix the bed material through rotational movement, for example, via a main stirring shaft is preferred. For vertically operated reactors A, B, or C, a stirring means selected from the group comprising a spiral stirrer, a spiral stirrer, an anchor stirrer, or a stirring means that generally conveys bed material axially or radially or both axially and radially is preferred. Adding a scraper to the stirring means can reduce wall clearance. In addition to the moving stirring means, reactors A, B, or C may also have rigid internal devices such as baffles.

[0113] In principle, materials suitable for the construction of reactors A, B, or C include all materials that exhibit the mechanical strength and resistance required under each process condition. In terms of chemical resistance, reactors A, B, or C may be composed of both suitable solid materials and chemically non-resistant (pressure-resistant) materials with specially coated or plated media-contact parts.

[0114] A cascade reactor system is a system in which at least two reactors are connected. There is no upper limit to the number of reactors. The relative number of reactors A, B, and C, as well as their size, shape, material, and composition, may differ. The reactors may be directly connected to each other or spatially separated from each other through a mobile storage vessel. It is also possible to consider two or more reactors B being connected to each other and each reaction step being performed in a separate reactor B.

[0115] The Si precursor and the Si-free precursor are preferably gaseous, liquid, or solid (e.g., sublimable), or optionally compositions of materials consisting of components in different states of matter. In one variation of the process, the Si precursor is fed directly into the bulk of porous particles in the reactor, for example, from below, from the side, or through a specific stirrer.

[0116] The Si precursor is preferably a silicon-hydrogen compound, such as monosilane (SiH4), disilane (Si2H6), and higher linear, branched, or cyclic homologues, neopentasilan (Si5H4). 12 ), cyclohexasilane (Si6H 12), chlorine-containing silanes, e.g., trichlorosilane (HSiCl3), dichlorosilane (H2SiCl2), chlorosilane (H3SiCl), tetrachlorosilane (SiCl4), hexachlorodisilane (Si2Cl6) and higher linear, branched or cyclic homologues, e.g., 1,1,2,2-tetrachlorodisilane (Cl2HSi-SiHCl2), chlorinated and partially chlorinated oligosilanes and polysilanes, methylchlorosilanes, e.g., trichloromethylsilane (MeSiCl3), dichlorodimethylsilane (Me2SiCl2), chlorotrimethylsilane (Me3SiCl), tetramethylsilane (Me4Si), dichloromethylsilane (MeHSiCl2), chloromethylsilane (MeH2SiCl), methylsilane (MeH3Si), chlorodimethylsilane (Me2HSiCl), dimethylsilane (Me2H2Si), It is selected from the group comprising a mixture of trimethylsilane (Me3SiH) and the described silicon compound.

[0117] In particular, the Si precursor is selected from the group comprising monosilane, disilane, trichlorosilane, dichlorosilane, methylsilane, and mixtures thereof.

[0118] Additional reactive components that may be present in the reaction gas are hydrogen, or even aliphatic hydrocarbons having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, such as methane, ethane, propane, butane, pentane, isobutane, hexane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane; Unsaturated hydrocarbons having 1 to 10 carbon atoms, e.g., ethene, acetylene, propene, methylacetylene butylene, butylene (1-butylene, 2-butylene), isoprene, butadiene, divinylbenzene, vinylacetylene, cyclohexadiene, cyclooctadiene, cyclic unsaturated hydrocarbons, e.g., cyclopropene, cyclobutene, cyclopentene, cyclohexene, cyclohexadiene, cyclopentadiene, dicyclopentadiene or norbornadiene; Aromatic hydrocarbons, e.g., benzene, toluene, p-, m-, o-xylene, styrene (vinylbenzene), ethylbenzene, diphenylmethane or naphthalene, other aromatic hydrocarbons, e.g., phenol, o-, m-, p-cresol, cymene, nitrobenzene, chlorobenzene, pyridine, anthracene and phenanthrene, myrcene, geraniol, thioterpineol, norbornan, borneol, isoborneol, bornein, camphor, limonene, terpinene, pinene, pinan, phylamine, charene, phenol, aniline, anisole, furan, furfural, furfuryl alcohol, hydroxymethylfurfural, bishydroxymethylfuran, and these compounds, e.g., natural gas condensates, petroleum distillates, coke oven condensates, fluid catalytic crackers (FCC), steam crackers or It may be charged with one or more hydrocarbons selected from the group comprising a mixed fraction of the product stream of a Fischer-Tropsch synthesis plant, or more generally, a stream of hydrocarbon-containing material from the processing of wood, natural gas, oil, and coal.

[0119] The porous particles for the method according to the present invention are preferably hard carbon, soft carbon, mesocarbon, microbeads, natural graphite or synthetic graphite, single-walled and multi-walled carbon nanotubes. and selected from the group comprising amorphous carbon in the form of graphene, oxides such as silicon dioxide, aluminum oxide, silicon-aluminum mixed oxide, magnesium oxide, lead oxide and zirconium oxide, carbides such as silicon carbide and boron carbide, nitrides such as silicon nitride and boron nitride, and other ceramic materials, and may be described by the following component chemical formula:

[0120] Al a B b C c Mg d N e O f Si g , where 0 ≤ a, b, c, d, e, f, g ≤ 1. At least two coefficients a, g > 0, and a*3 + b*3 + c*4 + d*2 + g*4 ≥ e*3 + f*2.

[0121] The ceramic material may be, for example, a two-component, three-component, four-component, five-component, three-component, or seven-component compound. A ceramic material having the following component formula is preferred:

[0122] - Non-stoichiometric boron nitride BN with z = 0.2 to 1 z ,

[0123] - Non-stoichiometric carbon nitride CN with z = 0.1 to 4 / 3 z ,

[0124] - Boron carbonitride B where x = 0.1 to 20 and z = 0.1 to 20, and x*3 + 4 ≥ z*3 x CN z ,

[0125] - Boron nitride oxide BN where z = 0.1 to 1 and r = 0.1 to 1, and 3 ≥ r*2 + z*3 z O r ,

[0126] - Boron carbonitride oxide B where x = 0.1 to 2, z = 0.1 to 1, r = 0.1 to 1, and x*3 + 4 ≥ r*2 + z*3 x CN z O r ,

[0127] - Silicon carbon oxide Si where x = 0.1 to 2 and z = 0.1 to 2, and x*4 + 4 ≥ z*2 x CO z ,

[0128] - Silicon carbonitride Si where x = 0.1 to 3 and z = 0.1 to 4, and x*4 + 4 ≥ z*3 x CN z ,

[0129] - Silicon boron carbonitride Si where w = 0.1 to 3, x = 0.1 to 2, and z = 0.1 to 4, and w*4 + x*3 + 4 ≥ z*3 w B x CN z ,

[0130] - Silicon boron carbon oxide Si where w = 0.10 to 3, x = 0.1 to 2, and z = 0.1 to 4, and w*4 + x*3 + 4 ≥ z*2 w B x CO z ,

[0131] - Silicon boron carbonitride oxide Si where v = 0.1 to 3, w = 0.1 to 2, x = 0.1 to 4, and z = 0.1 to 3, and v*4 + w*3 + 4 ≥ x*3 + z*2 v B w CN x O z , and

[0132] - u = 0.1 to 2 and Aluminum boron silicon carbonitride oxide Al, where v = 0.1 to 2, w = 0.1 to 4, x = 0.1 to 2, and z = 0.1 to 3, and u*3 + v*3 + x*4 + 4 ≥ w*3 + z*2. u B v Si x CN w O z .

[0133] The porous particles are preferably amorphous carbon selected from the group comprising hard carbon, soft carbon, mesocarbon, micro beads, natural or synthetic graphite, single-walled and multi-walled carbon nanotubes, graphene, and mixtures thereof.

[0134] Porous particles preferably have a density of 0.1 to 7 g / cm³ as measured by helium pycnometry. 3 , particularly preferably 0.3 to 3 g / cm² 3 This is the volumetric capacity (mAh / cm²) of a lithium-ion battery. 3 It is advantageous for increasing ).

[0135] The porous particles preferably have a diameter percentile d of ≥ 0.5 μm, particularly preferably ≥ 1.5 μm, and most preferably ≥ 2 μm. 50 It has a volume-weighted particle size distribution with diameter percentile d 50 It is preferably ≤ 20 μm, more preferably ≤ 12 μm, and most preferably ≤ 8 μm.

[0136] The volume-weighted particle size distribution of porous particles is preferably such that the diameter percentile is d 10 ≥ 0.2 μm to d 90 ≤ 20.0 μm, particularly preferably d 10 ≥ 0.4 μm to d 90 ≤ 15.0 μm, most preferably d 10 ≥ 0.6 μm to d 90 It is ≤ 12.0 μm.

[0137] The porous particles preferably have a diameter percentile d of ≤ 10 μm, particularly preferably ≤ 5 μm, particularly preferably ≤ 3 μm, and most preferably ≤ 2 μm. 10 It has a volume-weighted particle size distribution with diameter percentile d 10 It is preferably ≥ 0.2 μm, particularly preferably ≥ 0.5 μm, and most preferably ≥ 1 μm.

[0138] The porous particles preferably have a diameter percentile d of ≥ 4 μm, particularly preferably ≥ 8 μm. 90 It has a volume-weighted particle size distribution with diameter percentile d 90 It is preferably ≤ 18 μm, more preferably ≤ 15 μm, and most preferably ≤ 13 μm.

[0139] The volume-weighted particle size distribution of the porous particles preferably has a width d of ≤ 15.0 μm, more preferably ≤ 12.0 μm, particularly preferably ≤ 10.0 μm, particularly preferably ≤ 8.0 μm, and most preferably ≤ 4.0 μm. 90 -d 10 has

[0140] The volume-weighted particle size distribution of the Si composite that can be produced by the method according to the present invention preferably has a width d of ≥ 0.6 μm, particularly preferably ≥ 0.8 μm, and most preferably ≥ 1.0 μm. 90 -d 10 has

[0141] The volume-weighted particle size distribution of porous particles can be determined according to ISO 13320 by static laser scattering using the Mie model with a Horiba LA 950 measuring device using ethanol as the dispersion medium for porous particles.

[0142] Porous particles are preferably in the form of individual particles. The particles may be separated or aggregated, for example. Porous particles are preferably not aggregated and are not aggregated. Aggregation generally means that during the production process of porous particles, primary particles are initially formed and grow together and / or, for example, connect with each other via covalent bonds to form aggregates in this manner. Primary particles are generally separated particles. Aggregates or separated particles may form aggregates. Aggregates are loose accumulations of aggregates or primary particles connected to each other via, for example, van der Waals interactions or hydrogen bonds. Aggregated aggregates can be easily broken back into aggregates by a typical kneading and dispersion process. Aggregates may be partially broken down into primary particles by this process. The presence of porous particles in the form of aggregates, aggregates, or separated particles can be visualized, for example, using a conventional scanning electron microscope (SEM). In contrast, static light scattering methods for determining the particle size distribution or particle diameter of matrix particles cannot distinguish between aggregates and aggregates.

[0143] Porous particles can have any shape, for example, split, fragmented, spherical, or needle-shaped, and split or spherical particles are preferred.

[0144] The shape can be characterized, for example, by sphericity ψ or sphericity S. According to Wadell's definition, sphericity ψ is the ratio of the surface area of ​​a sphere of the same volume to the actual surface area of ​​a volume. For a sphere, ψ is 1. According to this definition, the porous particles for the method according to the present invention preferably have a sphericity ψ of 0.3 to 1.0, particularly preferably 0.5 to 1.0, and most preferably 0.65 to 1.0.

[0145] Sphericity S is the ratio of the perimeter of an equivalent circle having the same area A as the projection of the particle onto the surface to the measured perimeter U of this projection: For ideal spherical particles, S will have a value of 1. For porous particles for the method according to the present invention, the sphericity S is the percentile S of the sphericity number distribution. 10 to S 90 Based on [the value], it is preferably in the range of 0.5 to 1.0, and particularly preferably in the range of 0.65 to 1.0. Measurement of sphericity (S) is performed by scanning electron microscopy, for example by referring to microscopic images of individual particles with an optical microscope, or, if the particles are less than 10 μm, by graphic evaluation using image analysis software such as ImageJ.

[0146] Porous particles are preferably ≥ 0.2 cm 3 / g, particularly preferably ≥ 0.6 cm 3 / g, most preferably ≥ 1.0 cm 3 It has a gas-accessible pore volume of / g. This is advantageous for obtaining high-capacity LIBs. The gas-accessible pore volume was determined by gas adsorption measurements using nitrogen according to DIN 66134.

[0147] Porous particles are preferably open pores. Open pores generally mean that the pores are connected to the surface of the particle, for example, through channels, and are preferably capable of exchanging materials, particularly gaseous materials, with the environment. This can be demonstrated by gas adsorption measurements (analysis according to Brunauer, Emmett, and Teller, "BET"), i.e., specific surface area. Porous particles are preferably ≥ 50 m² 2 / g, particularly preferably ≥ 500 m 2 / g, most preferably ≥ 1000 m 2 It has a specific surface area of ​​ / g. The BET surface area is determined according to DIN 66131 (including nitrogen).

[0148] The pores of the porous particles may have any diameter, namely, generally macropores (greater than 50 nm), mesopores (2 to 50 nm), and micropores (less than 2 nm). The porous particles may be used as any mixture of different pore types. It is desirable to use porous particles having 30% or less of macropores based on the total pore volume, very particularly preferably porous particles without macropores, and particularly preferably porous particles having at least 50% of pores with an average pore diameter of less than 5 nm. It is particularly desirable for porous particles to have only pores with a pore diameter of less than 2 nm (determination method: pore size distribution according to BJH (gas adsorption) and Horvath-Kawazoe (gas adsorption) in the intermediate pore range according to DIN 66134, according to DIN 66135 in the micropore range, and pore size distribution in the macropore range evaluated by mercury porosity according to DIN ISO 15901-1).

[0149] 0.3 cm 3 Less than / g, particularly preferably 0.15 cm 3 Porous particles having a gas-inaccessible pore volume of less than / g are preferred. This can also be used to increase the capacity of the LIB. The gas-inaccessible pore volume can be determined using the following formula:

[0150] Gas-inaccessible pore volume = 1 / density of pure matter - 1 / skeletal density.

[0151] Pure-material density is the theoretical density of porous particles based on phase composition or the density of the pure material (the density of a material without closed pores). Pure-material density data can be found by those skilled in the art, for example, at the National Institute of Standards and Technology's Ceramic Data Portal (NIST, https: / / srdata.nist.gov / CeramicDataPortal / scd). For example, the pure-material density of silicon oxide is 2.203 g / cm³. 3 The pure material density of boron nitride is 2.25 g / cm³ 3 The pure material density of silicon nitride is 3.44 g / cm³ 3 The pure material density of silicon carbide is 3.21 g / cm³ 3 The skeletal density is the actual density of porous particles (gas-accessible) determined by helium densitography.

[0152] Porous particles generally function as starting materials for producing silicon composites. It is desirable to be silicon-free, that is, in particular, to be silicon-free, specifically in the pores of the porous particles and in the presence of silicon obtained by the deposition of a Si precursor on the surface of the porous particles.

[0153] A silicon composite obtainable by the method according to the present invention by depositing silicon on the surface of pores and porous particles has a diameter percentile d in the range of 0.5 to 20 μm. 50 It can have a volume-weighted particle size distribution having d 50 The value is preferably 1.5 μm or more, particularly preferably 2 μm or more. Diameter percentile d 50 It is preferably 13 μm or less, particularly preferably 8 μm or less.

[0154] The volume-weighted particle size distribution of the silicon composite is preferably the diameter percentile d 10 ≥ 0.2 μm to d 90 ≤ 20.0 μm, particularly preferably d 10 ≥ 0.4 μm to d90 ≤ 15.0 μm, especially d 10 ≥ 0.6 μm to d 90 It is ≤ 12.0 μm.

[0155] The silicone composite preferably has a diameter percentile d of ≤ 10 μm, particularly preferably ≤ 5 μm, particularly preferably ≤ 3 μm, and most preferably ≤ 1 μm. 10 It has a volume-weighted particle size distribution with diameter percentile d 10 It is preferably ≥ 0.2 μm, particularly preferably ≥ 0.4 μm, and particularly ≥ 0.6 μm.

[0156] The silicone composite preferably has a diameter percentile d of ≥ 5 μm, particularly preferably ≥ 10 μm. 90 It has a volume-weighted particle size distribution with diameter percentile d 90 It is preferably ≤ 20.0 μm, particularly preferably ≤ 15.0 μm, and particularly ≤ 12.0 μm.

[0157] The volume-weighted particle size distribution of the silicon composite has a width d of ≤ 15.0 μm, preferably ≤ 12.0 μm, particularly preferably ≤ 10.0 μm, particularly ≤ 8.0 μm, and particularly preferably ≤ 4.0 μm. 90 -d 10 It may have. The volume-weighted particle size distribution of the silicon composite preferably has a width d such that ≥ 0.6 μm, particularly preferably ≥ 0.8 μm, and particularly ≥ 1.0 μm. 90 -d 10 has

[0158] The particles of the silicon composite are preferably in the form of particles. The particles may be separated or aggregated. It is preferable that the silicon composite is not aggregated, and it is desirable that it is not aggregated. The terms isolation, aggregation, and non-aggregation have already been defined above in relation to porous particles. The presence of the silicon composite in the form of aggregates or aggregates can be visualized, for example, using a conventional scanning electron microscope (SEM).

[0159] Si composites can have any shape, for example, split, flaked, spherical, or needle-shaped, and split or spherical particles are preferred.

[0160] According to Wadell's definition, sphericity ψ is the ratio of the surface area of ​​a sphere of equal volume to the actual surface area of ​​an object. For a sphere, ψ is 1. According to this definition, the Si composite obtained by the method according to the present invention preferably has a sphericity ψ of 0.3 to 1.0, particularly preferably 0.5 to 1.0, and most preferably 0.65 to 1.0.

[0161] Sphericity S is the ratio of the perimeter of an equivalent circle having the same area A as the projection of the particle onto the surface to the measured perimeter U of this projection: For ideal spherical particles, S will have a value of 1. For a silicon composite obtainable by the method according to the present invention, the sphericity S is preferably in the range of 0.5 to 1.0, particularly preferably 0.65 to 1.0, which corresponds to the percentile S of the sphericity number distribution. 10 to S 90 The measurement of sphericity (S) is based on [this]. For example, the measurement is performed by referring to microscopic images of individual particles with an optical microscope, or, if the particles are less than 10 μm, by a scanning electron microscope (SEM) preferably by a graphical evaluation using image analysis software such as ImageJ.

[0162] The cycling stability of LIBs can be further increased through morphology, material composition, and especially the internal porosity or specific surface area of ​​silicon composites.

[0163] In the case where the porous particles contain, for example, a Si compound in the form of silicon dioxide, the data expressed in weight% can be determined for the silicon obtained through deposition from the Si precursor by subtracting the Si mass of the porous particles determined by elemental analysis from the Si mass of the silicon composite determined by elemental analysis, and then dividing the result by the mass of the silicon composite.

[0164] The volume of silicon deposited on porous particles is the mass fraction of silicon obtained through deposition from the Si precursor to the total mass of the silicon composite, relative to the density of silicon (2.336 g / cm³). 3 It can be derived by dividing into ).

[0165] Pore ​​volume of silicone composite P It can be derived from the sum of the gas-accessible pore volume and the gas-inaccessible pore volume. The Gurvich gas-accessible pore volume of the silicon composite can be determined by gas adsorption measurements using nitrogen according to DIN 66134.

[0166] The gas-inaccessible pore volume of a silicon composite can be determined as described above: Gas-inaccessible pore volume = 1 / framework density - 1 / pure material density.

[0167] Pore ​​volume of Si composites P Based on the volume of silicon present in the Si composite and obtained by the deposition of the Si precursor, it is preferably in the range of 0 volume% to 400 volume%, particularly preferably in the range of 100 volume% to 350 volume%, and particularly preferably in the range of 200 volume% to 350 volume%.

[0168] The porosity of the silicon composite may be gas-accessible or gas-inaccessible. The volume ratio of gas-accessible porosity to gas-inaccessible porosity of the silicon composite may generally be in the range of 0 (no gas-accessible pores) to 1 (all gas-accessible). The volume ratio of gas-accessible porosity to gas-inaccessible porosity of the silicon composite is preferably in the range of 0 to 0.8, particularly preferably in the range of 0 to 0.3, and particularly preferably in the range of 0 to 0.1.

[0169] The pores of the silicon composite may have any diameter range, for example, macropores (> 50 nm), mesopores (2 to 50 nm), and micropores (< 2 nm). The Si composite may also contain any mixture of different pore types. It is preferable that it contain up to 30% macropores based on the total pore volume. A Si composite without macropores is particularly preferred, and a Si composite having more than 50% pores based on the total pore volume and an average pore diameter of less than 5 mm is very particularly preferred. The Si composite particularly preferably contains only pores with a diameter of up to 2 nm.

[0170] The Si composite comprises a silicon structure having a structural size of preferably up to 1000 nm in at least one dimension, particularly preferably less than 100 nm, particularly less than 5 nm (determination method: SEM and / or high-resolution transmission electron microscopy (HR-TEM)).

[0171] The Si composite preferably contains a Si layer having a layer thickness of less than 1000 nm, particularly preferably less than 100 nm, and particularly less than 5 nm (Decision: SEM and / or HR-TEM). The Si composite may also contain silicon in particulate form. The Si particles preferably have a diameter of up to 1000 nm, particularly preferably less than 100 nm, and particularly less than 5 nm (Decision: SEM and / or HR-TEM). Here, the figure for the Si particles preferably relates to the particle circumferential diameter in the micrograph.

[0172] It is preferable that the amount of coarse silicon in the deposited silicon be less than 3 weight%, particularly preferably less than 1 weight%, and particularly preferably less than 0.1 weight%.

[0173] The Si composite is preferably up to 100 m 2 / g, particularly preferably 30 m 2 Less than / g, particularly preferably 10 m 2 It has a specific surface area of ​​less than / g. The BET surface area is determined according to DIN 66131 (using nitrogen). This allows for reduced SEI formation and increased initial Coulomb efficiency when using Si composites as active materials for LIB anodes.

[0174] Additionally, silicon deposited from a Si precursor of a Si composite may contain a dopant selected from the group comprising, for example, Li, Fe, Al, Cu, Ca, K, Na, S, Cl, Zr, Ti, Pt, Ni, Cr, Sn, Mg, Ag, Co, Zn, B, P, Sb, Pb, Ge, Bi, rare earth elements, and combinations thereof. Li and / or Sn are preferred. The content of the dopant in the Si composite is preferably up to 1 wt%, particularly preferably up to 100 ppm, based on the total weight of the Si composite that can be determined by ICP-OES.

[0175] Si composites exhibit remarkably high stability under compressive and / or shear stresses. This compressive and shear stability is evident from the fact that the porous structure of the Si composite changes only slightly under compressive loads (e.g., during electrode compression) and shear stress (e.g., during electrode compression) and shear stress (e.g., during electrode preparation).

[0176] The Si composite may optionally contain additional elements such as carbon. Carbon is preferably present in the form of a thin layer having a thickness of up to 1 μm, preferably less than 100 nm, particularly preferably less than 5 nm, and particularly preferably less than 1 nm (Decision: SEM and HR-TEM). The C layer may be present in both the pores and the surface of the Si composite. Additionally, it is possible to freely select the order of different layers in the Si composite through the alternating metering of different precursors and appropriate repetition thereof. Thus, a layer of additional material distinct from the porous particles, for example, made of carbon, may first be present on the porous particles, and a Si layer or a layer of Si particles may be present thereon. Furthermore, on the Si layer or the layer of Si particles, a layer of additional material that may be distinct from or identical to the material of the porous particles may be present, regardless of whether an additional layer of material distinct from the material of the porous particles exists between the porous particles and the layer composed of Si or Si particles.

[0177] The Si composite may contain 50 weight% or less of additional elements, preferably 40 weight% or less, and particularly preferably 20 weight% or less. The silicon composite may contain 1 weight% or more, particularly preferably 2 weight% or more of additional elements. The figures indicated in weight% represent the total weight of the Si composite. It is also possible for the Si composite not to contain additional elements.

[0178] The Si composite obtained by the method according to the present invention is suitable as an active material for an anode material for a LIB, and the use of such an anode is suitable for the production of LIBs. All components and materials required for production are generally known. The production of these battery components and their assembly are carried out by processes familiar in the field of battery production.

[0179] The Si composite obtained by the method according to the present invention is characterized by significantly improved electrochemical behavior and results in a LIB having high volumetric capacity and excellent performance characteristics. The Si composite is permeable to Li ions and electrons, enabling charge transport. The SEI of the LIB can be significantly reduced by using the obtained Si composite. Furthermore, due to the design of the Si composite, the SEI is separated from the surface of the active material or at least separated to a much smaller extent. All of this leads to high cyclic stability of the LIB containing the Si composite obtained by the method according to the present invention in the anode. Specific details for implementing the invention

[0180] The following examples serve to further clarify the invention described herein.

[0181] The following analysis methods and tools were used for characterization:

[0182] Weapon Analysis / Elemental Analysis:

[0183] The carbon content reported in the examples was determined using a Leco CS 230 analyzer, and the O and optionally N or H content were determined using a Leco TCH-600 analyzer. The qualitative and quantitative analysis of other specified elements was performed by inductively coupled plasma (ICP) emission spectroscopy (Optima 7300 DV, Perkin Elmer). For this purpose, samples were acid-digested (HF / HNO3) in a microwave (Microwave 3000, Anton Paar). ICP-OES determinations were based on the analysis of acidic aqueous solutions (e.g., acidified drinking water, wastewater and other water samples, aqua regia extracts from soil and sediments) according to ISO 11885 "Water quality - Determination of selected elements by inductively coupled plasma optical emission spectrometry (ICP-OES) (ISO 11885:2007); German version of EN ISO 11885:2009". The Si determination method used was generally accurate to ±1 wt%.

[0184] Particle Size Determination:

[0185] Particle size distribution was determined according to ISO 13320 via static laser scattering using a Horiba LA 950. During sample preparation, special care must be taken to disperse the particles in the measurement solution to ensure that the size of individual particles, rather than aggregates, is measured. The particles were dispersed in ethanol for measurement. If necessary, the dispersion was sonicated at 250 W for 4 minutes in a Hielscher UIS250v ultrasonic laboratory device equipped with an LS24d5 sonotrode prior to measurement.

[0186] BET surface area measurement:

[0187] The specific surface area of ​​the material was measured by the BET method (determined according to DIN ISO 9277:2003-05 using nitrogen) through nitrogen gas adsorption using a Sorptomatic 199090 instrument (Porotec) or a SA-9603MP instrument (Horiba).

[0188] Skeletal density:

[0189] The skeletal density, that is, the density of a porous solid based on the volume of the external gas-inaccessible pore space alone, was determined by the He specific gravity method according to DIN 66137-2.

[0190] Gas-accessible pore volume:

[0191] The Gurvich gas-accessible pore volume was determined by gas adsorption measurements using nitrogen according to DIN 66134.

[0192] Thermogravimetric Analysis (TGA) and Coarse Silicon Crystals:

[0193] The reactivity of the powder to oxygen was determined by TGA measurements of pure oxygen in a temperature window of 25°C to 1000°C using a heating rate of 5 K / min.

[0194] conversion:

[0195] Conversion is calculated as the quotient of the amount of a component within the converted starting material (reactant) relative to the amount of a component of the used starting material (reactant) in moles. Conversion indicates how many of the used SiH4 molecules are converted to Si at a specific time. Conversion is variable and may vary depending on the process duration.

[0196]

[0197] Total conversion indicates how much silicon was deposited compared to the silicon measured over the entire process.

[0198] Throughput:

[0199] Throughput represents the weight% of Si measured over one hour. This is calculated from the deposition time across all steps and the Si content of the recovered product in weight% per hour (target content of Si).

[0200]

[0201] Examples

[0202] In the example, a Si composite with a silicon ratio of 47 wt% to 49 wt% was produced.

[0203] The SiH4 used, quality 4.0, was purchased from Linde GmbH.

[0204] In all examples, amorphous carbon was used as the porous starting material:

[0205] - Specific surface area = 1636 m² 2 / g

[0206] - Stomatal volume = 0.76 cm 2 / g

[0207] - Average volume-weighted particle size D50 = 6.4 μm

[0208] Ratio of deposited silicon based on target content:

[0209] 0.1% to 50% of the target content is deposited during step A, or up to 50% of the total target content is deposited during two or more steps A.

[0210] The ratio of Si deposited during Step A or during regular operation based on the target content represents the relative ratio of Si deposited in the corresponding step. For example, a target content of 48 wt% of Si for the composite corresponds to a relative ratio of 100% of the deposited Si. 50% of the Si deposited during Step A corresponds to a target Si content of 24 wt% in the composite.

[0211] The determination of fine and coarse silicon within a sample can be performed using TGA measurements, which involve the formation of SiO2 through the reaction of silicon and oxygen. The distinction between different Si chemical species can be attributed to the fact that thin silicon layers exhibit higher reactivity to oxygen than thick layers or Si particles. This results in TGA measurements showing that thin Si layers react (increase in mass) even at low temperatures (400°C to 655°C), while thick layer / coarse Si structures react only at temperatures above 700°C. Ideally, silicon-containing composites intended for use as anode active materials do not exhibit mass increase in TGA measurements under an oxygen-containing atmosphere at temperatures above 800°C. This method allows for the further determination of the elemental silicon content. Silicon that has previously been oxidized and passivated through contact with air is not considered in TGA measurements as it no longer participates in the reaction.

[0212] To calculate the existing rough silicon, the residual mass (m) of the TGA method 잔여 ) and mass difference due to oxidation of coarse silicon (m 차이 ) is required. Using the molar mass of O2 (32 g / mol) and the molar mass of SiO2 (60.08 g / mol), the ratio of coarse silicon in the deposited silicon can now be calculated using the following formula:

[0213]

[0214] Comparative Example 1 : Production of Si composites in a reactor suitable for the production of Si composites.

[0215] Porous carbon particles in a quartz glass boat in a tubular reactor (specific surface area = 1636 m²) 2 / g; Gurvich pore volume = 0.76 cm 3 / g, average volume-weighted particle size D 502.2 g (= 6.40 μm) was added. After inactivating with nitrogen, the reactor was heated to 410°C. Upon reaching this temperature, a Si precursor (50% SiH4 in N2, 10 NL / h) was passed through the reactor. The decomposition reaction of SiH4 to produce Si was monitored and quantified in the off-gas stream using a thermal conductivity detector. After 2.1 g of Si was deposited, the SiH4 gas stream was converted to a pure nitrogen stream, and heating was stopped. The reactor was cooled to room temperature with N2 purging, and the product was recovered.

[0216] Comparative Example 2: Production of silicon composites in a reactor suitable for the production of Si composites.

[0217] Porous carbon particles in a quartz glass boat in a tubular reactor (specific surface area = 1636 m²) 2 / g; Gurvich pore volume = 0.76 cm 3 / g, average volume-weighted particle size D 50 2.2 g (= 6.40 μm) was added. After inactivating with nitrogen, the reactor was heated to 380°C. Upon reaching this temperature, a Si precursor (50% SiH4 in N2, 10 NL / h) was passed through the reactor. The decomposition reaction of SiH4 to produce Si was monitored and quantified in the off-gas stream using a thermal conductivity detector. After 2.1 g of Si was deposited, the SiH4 gas stream was converted to a pure nitrogen stream, and heating was stopped. The reactor was cooled to room temperature with N2 purging, and the product was recovered.

[0218] Examples 1 to 2: Production of a Si composite by the method according to the present invention having step A (indices A represent parameters of step A).

[0219] Porous carbon particles in a quartz glass boat in a tubular reactor (specific surface area = 1636 m²) 2 / g; Gurvich pore volume = 0.76 cm 3 / g, average volume-weighted particle size D 50 = 6.40 μm) 2.2 g was filled. After inactivating with nitrogen, the reactor T A It was heated to (step (index) A). When the target temperature was reached, the monosilane was transferred to the reactor with N2 (concentration C A , volume of Si precursor fluid VS A It was passed as a mixture with ). The decomposition reaction of SiH4 generating Si in the off-gas stream was monitored and quantified using a thermal conductivity detector. Once Si M A When [g] is deposited, the plant operates normally (exponent R): temperature T R , monosilane concentration C R , Volume flow of Si precursors VS R Convert to, and additional Si amount M R It was deposited in a regular operation. The reactor was cooled to room temperature with N2 purging, and the silicon composite was recovered.

[0220] Table 1: Experimental parameters for Examples 1 and 2 of the present invention

[0221] Experimental parameters explanation Example number Example 1 Example 2 Si, [g] deposited in a regular operation M R 2.220 1.910 Si, [g] deposited in step A M A 0.006 0.004 Temperature during normal operation, [℃] T R 410 400 Temperature at Step A, [℃] T A 380 400 SiH4 concentration in regular operation, [Volume %] C R 50 50 SiH4 in Step A, [Volume %] C A 50 30 Volume flow of SiH4 per gram of carbon in normal operation [NL / h per gram of carbon in reactor] VS R 2.27 2.27 Volume flow of SiH4 per gram of carbon in Step A [NL / h per gram of carbon in reactor] VS A 2.27 1.36

[0222] Examples 3 to 4: Production of a Si composite by a method according to the present invention having two or more steps A.

[0223] Porous carbon particles in a quartz glass boat in a tubular reactor (specific surface area = 1636 m²) 2 / g; Gurvich pore volume = 0.76 cm 3 / g, average volume-weighted particle size D 50 = 6.40 μm) 2.2 g was filled. After inactivating with nitrogen, the reactor T A1 It was heated to (step (index) A1). When the target temperature was reached, the monosilane was transferred to the reactor with N2 (concentration C A1 , volume of Si precursor fluid VS A1 It was passed as a mixture with ). The decomposition reaction of SiH4 generating Si in the off-gas stream was monitored and quantified using a thermal conductivity detector. Once Si M A1 When [g] is deposited (step (exponent) A1), the plant operates normally: temperature T R , monosilane concentration C R , Volume flow of Si precursors VS R Convert to, and additional Si amount M R [g] was deposited in a regular operation. First M R [g] When silicon is deposited in a regular operation ( M A1 + M R Si target content up to a single moment), converts the plant anew, and new change △: temperature T A2 , monosilane concentration C A2 , Volume flow of Si precursors VS A2 Perform (step (exponent) A2), and additional Si amount M A2 [g] was deposited. Afterwards, the reactor was purged with N2, cooled to room temperature, and the product was recovered.

[0224] Table 2: Experimental parameters for Examples 1 and 2 of the present invention

[0225] Experimental parameters explanation Example number Example 3 Example 4 Si, [g] deposited in a regular operation M R 1.58 1.24 Si1, [g] deposited in step A M A1 0.20 0.42 Si2, [g] deposited in step A M A2 0.20 0.42 Temperature during normal operation, [℃] T R 410 400 Temperature 1 at Step A, [℃] T A1 380 400 Temperature 2 at Step A, [℃] T A2 380 400 SiH4 concentration in regular operation, [Volume %] C R 50 100 SiH4 in Step A1, [Volume %] C A1 50 50 SiH4 in step A2, [volume%] C A2 50 50 Volume flow of SiH4 in regular operation [NL / h per gram of carbon in reactor] VS R 2.27 4.55 Volume flow of SiH4 in step A1 [NL / h per gram of carbon in the reactor] VS A1 2.27 2.27 Volume flow of SiH4 in step A2 [NL / h per gram of carbon in the reactor] VS A2 2.27 2.27

[0226] The reaction conditions and material properties for the production of Si composites are summarized in Table 3 below.

[0227] Comparative Example 1* Comparative Example 2* Example 1 Example 2 Example 3 Example 4 Regular tasks: Ratio of target content in the product, [%Si] 100 100 99.72 99.8 80 60 Regular tasks: Temperature T R , [℃] 410 380 410 400 410 400 Regular tasks: Monosilane concentration C R , [Volume %] 50 50 50 50 50 100 Regular tasks: Monosilane volume flow vs. R [NL / h per gram of carbon in the reactor] 2.27 2.27 2.27 2.27 2.27 4.55 Step A: Ratio of target content in the product, [%Si] - - 0.27 0.21 20 40 Step A: Temperature T A , [℃] - - 380 400 380 400 Step A: Monosilane concentration C A , [Volume %] - - 50 30 50 50 Step A: Monosilane volume flow vs. A [NL / h per gram of carbon in the reactor] - - 2.27 1.36 2.27 2.27 △T , [℃] - - 20 0 30 0 △C , [Volume %] - - 0 20 0 50 △VS , [NL / h per gram of carbon in the reactor] - - 0 0.90 0 0 Total conversion rate, [%] 56.84 19.42 53.55 44.97 50.21 64.31 Throughput [weight% / h] 82.76 28.74 49.48 63.16 45.49 75.68 Amount of reactant, [g] 2.20 2.20 2.20 2.20 2.20 2.20 Amount of product, [g] 4.29 4.22 4.22 4.11 4.18 4.28 Si, [weight%] 48 48 48 48 48 48 O, [Weight %] 2.18 3.31 2.99 2.24 3.30 3.38 Rough Si, [%] 0.6 0.0 0.0 0.0 0.0 0.0 BET, [m² / g] 9.43 30.21 12.4 11.44 26.11 17.40

[0228] *Not the present invention

[0229] Selected parameter M R , M A , T R , T A , C R , C A , VS A and VS R Accordingly, it was possible to maximize material performance while significantly increasing the overall conversion rate and plant throughput of the Si precursor.

[0230] Evaluation of Si composite particles in an electrochemical cell

[0231] Example 5: Examples 1 to 4 and Comparative Example of the present invention Si composites were tested as the anode component of LIBs.

[0232] 29.71 g of polyacrylic acid (dried to constant weight at 85°C; Sigma-Aldrich, Mw approx. 450,000 g / mol) and 756.60 g of deionized water were stirred in a shaker (290 L / min) for 2.5 hours. The dissolution of the polyacrylic acid was completed. Lithium hydroxide monohydrate (Sigma-Aldrich) was added to the solution in small amounts until the pH reached 7.0 (measured with a WTW pH 340i pH meter and SenTix RJD probe). The solution was then mixed in a shaker for an additional 4 hours. 3.87 g of the neutralized polyacrylic acid solution and 0.96 g of graphite (Imerys, KS6L C) were initially filled into a 50 ml container and mixed in an oil mixer (SpeedMixer, DAC 150 SP) at 2000 rpm. In each case, 3.35 g of the silicon composite from Examples 1 to 5 and Comparative Examples 1 and 2 was then stirred at 2000 rpm for 1 minute. Subsequently, 1.21 g of 8% conductive carbon black dispersion and 0.8 g of deionized water were added and mixed in an oil mixer at 2000 rpm. Then, dispersion was performed in a dissolving chamber at 3000 rpm for 30 minutes at a constant temperature of 20°C. The ink was degassed again in an oil mixer at 2500 rpm under vacuum for 5 minutes. The completed dispersion was applied to a copper foil (Schlenk Metallfolien, SE-Cu58) with a thickness of 0.03 mm using a film drawing frame (Erichsen, Model 360) with a clearance of 0.06 mm. The resulting anode coating was dried at 50°C and 1 bar atm for 60 minutes. The average basis weight of the dry anode coating is 2.7 mg / cm² 2 The coating density is 0.8 g / cm³ 3 It was.

[0233] Electrochemical studies were performed in a 2-electrode array button cell (CR2032 type, Hohsen Corp.). The electrode coating was used as the counter electrode or cathode (Dm = 15 mm). Content 94.0% and average basis weight 15.9 mg / cm³ 2 A lithium-nickel-manganese-cobalt oxide 6:2:2-based coating (obtained from SEI) was used as the working electrode / anode (Dm = 15 mm). Glass fiber filter paper (Whatman, GD Type D) saturated with 60 μl of electrolyte was used as the separator (Dm = 16 mm). The electrolyte used consisted of a 1.0 molar solution of lithium hexafluorophosphate in a 1:4 (v / v) mixture of fluoroethylene carbonate and diethyl carbonate. The cell was assembled in a glove box (< 1 ppm H2O, O2). The moisture content of the dry matter of all components used was less than 20 ppm.

[0234] Electrochemical tests were performed at 20°C. The cell was charged by the cc / cv method (constant current / constant voltage) with a constant current of 5 mA / g (corresponding to C / 25) and 60 mA / g (corresponding to C / 2) in the first cycle. In subsequent cycles, and upon reaching a voltage limit of 4.2 V, the current was charged at a constant voltage until it dropped below 1.2 mA / g (corresponding to C / 100) or 15 mA / g (corresponding to C / 8). The cell was discharged by the cc method (constant current) with a constant current of 5 mA / g (corresponding to C / 25) in the first cycle until a voltage limit of 2.5 V was achieved, and with a constant current of 60 mA / g (corresponding to C / 2) in subsequent cycles. The selected specific current was based on the weight of the anode coating. The electrodes were established such that the capacitance ratio of cathode to anode was 1:1.2.

[0235] Electrochemical test results for complete cells of LIBs containing Si composites of Examples 1 to 4 and Comparative Examples 1 and 2 It is shown in Table 4.

[0236] Example number Reversible specific capacity of the cathode in the second cycle, [mAh / g] Number of cycles with a capacity retention of 80% or more Coulomb efficiency of formation [%][%] Comparative Example 1* 1034 391 86.5 Comparative Example 2* 1064 842 85.6 Example 1 1086 833 85.3 Example 2 1066 870 86.7 Example 3 1063 862 85.7 Example 4 1039 687 85.8

[0237] *Not the present invention

[0238] Comparative Example 1 showed high throughput combined with good conversion of the Si precursor but achieved only low cycling stability because it provided a coarse Si content of 0.6% (Table 3). Comparative Example 2 showed excellent electrochemical performance, but this was achievable only at low conversion rate and throughput (Table 4).

[0239] Examples 1 to 3 of the present invention exhibited higher throughput and higher conversion rates compared to Comparative Example 2 while maintaining very excellent electrochemical performance. In contrast to Comparative Example 1, Examples 1 to 3 should be considered advantageous as they do not provide coarse Si. By adjusting the temperature and silane concentration, Example 4 achieved better electrochemical performance and a higher conversion rate than Comparative Example 1.

Claims

Claim 1 A method for producing a silicon composite by a chemical vapor penetration method by the pyrolysis of at least one Si precursor in the presence of porous particles, wherein the silicon is deposited on the surface of the pores and porous particles, and the porous particles are amorphous carbon selected from the group comprising hard carbon, soft carbon, mesocarbon, natural graphite or synthetic graphite, single-walled and multi-walled carbon nanotubes, graphene, and mixtures thereof, and the silicon composite has a target Si content of 35 wt% to 60 wt%, wherein in a regular operation the method is performed at an average temperature T of -300°C to 500°C and a concentration C of -30 vol% to 100 vol% of a Si precursor, and wherein the method comprises at least one step A, wherein in step A a change Δ of at least one of parameters T and C occurs for the regular operation and optionally for an additional step A, -ΔT = 10°C to 130°C and -ΔC = 2 vol% to 70 vol%, provided that during step A the aforementioned target A method to which the condition is applied that 0.1% to 50% of the content is deposited, or that up to 50% of the overall target content mentioned is deposited during two or more steps A. Claim 2 A method for producing a silicon composite by a chemical vapor penetration method by the pyrolysis of at least one silicon precursor in the presence of porous particles, wherein the silicon is deposited on the surface of the pores and porous particles, the porous particles are amorphous carbon selected from the group comprising hard carbon, soft carbon, mesocarbon, natural graphite or synthetic graphite, single-walled and multi-walled carbon nanotubes, graphene and mixtures thereof, the silicon composite has a target Si content of 35 wt% to 60 wt%, wherein in a regular operation the method is performed at an average temperature T of -300°C to 500°C, a concentration C of silicon precursor of 30 vol% to 100 vol%, and a volume flow VS of silicon precursor of 0.01 to 20 NL / h based on 1 g of porous particles, wherein the method comprises at least one step A, wherein in step A a change Δ of at least one of the parameters T, C and VS occurs for the regular operation and optionally for an additional step A, A method in which ΔT = 10℃ to 130℃, - ΔC = 2 vol% to 70 vol%, - ΔVS = 0.01 to 10 NL / h, provided that 0.1% to 50% of the stated target content is deposited during step A, or up to 50% of the stated target content is deposited overall during two or more steps A. Claim 3 In paragraph 2, the method wherein VS in regular operation is 0.01 to 10 NL / h or 0.01 to 5 NL / h based on 1 g of porous particles. Claim 4 A method according to claim 2 or 3, wherein ΔVS is 0.01 to 5 NL / h or 0.01 to 2 NL / h based on 1 g of porous particles. Claim 5 A method according to any one of claims 1 to 3, wherein the silicon composite has a target Si content of 40% to 55% by weight, or 42% to 50% by weight. Claim 6 A method according to any one of claims 1 to 3, wherein the target content of Si is determined during the process by analyzing the composition of an off-gas stream by at least one method selected from the group comprising gas chromatography, mass spectrometry, infrared spectroscopy, and thermal conductivity measurement. Claim 7 A method according to any one of claims 1 to 3, wherein T in regular operation is 315°C to 475°C, or 330°C to 450°C. Claim 8 A method according to any one of claims 1 to 3, wherein C in the regular operation is 40 volume% to 100 volume%, or 50 volume% to 100 volume%. Claim 9 A method according to any one of claims 1 to 3, wherein ΔT is 20℃ to 100℃ or 20℃ to 50℃. Claim 10 A method according to any one of claims 1 to 3, wherein ΔC is 5 volume% to 60 volume%, or 10 volume% to 50 volume%. Claim 11 A method according to any one of paragraphs 1 to 3, wherein the change Δ is performed continuously from the start of step A until the end thereof. Claim 12 A method according to any one of paragraphs 1 to 3, performed at a pressure of less than 0.7 MPa. Claim 13 A method according to any one of claims 1 to 3, performed in a reactor equipped with a close-clearance stirrer. Claim 14 A method according to any one of claims 1 to 3, performed in a cascade reactor system comprising two or more reactors. Claim 15 A method according to any one of claims 1 to 3, wherein the silicon precursor is selected from the group comprising monosilane, disilane, trichlorosilane, dichlorosilane, methylsilane, and mixtures thereof. Claim 16 delete

Citation Information

Patent Citations

  • Process for producing silicon

    KR1020070001165A

  • Silicon-containing structure, preparing method thereof, carbon composite using the same, electrode including the same, lithium battery including the same, and device including the same

    KR1020190091411A

  • Method for preparing electroactive materials for metal-ion batteries

    KR1020210118087A

  • Process for preparing electroactive materials for metal-ion batteries

    US10508335B1