Method for eliminating hydrogen in aluminium melt

By optimizing rotor diameter, rotation speed, and gas injection amount in the GBF process, the method efficiently removes hydrogen gas from molten aluminum, addressing inefficiencies in existing technologies and reducing costs.

KR103046748B1Active Publication Date: 2026-11-10RES INST OF IND SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020230182329
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2026-11-10
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

Existing methods for removing hydrogen gas from molten aluminum, such as the Gas Bubbling Filtration (GBF) method, are inefficient and costly due to the inability to optimize conditions related to hydrogen gas removal, leading to significant time and resource consumption.

Method used

A method that optimizes conditions such as rotor rotation speed, inert gas injection amount, and rotor diameter in the GBF process to efficiently remove hydrogen gas from molten aluminum, using a degassing step, condition setting, and verification steps to ensure compliance with desired hydrogen gas content standards.

Benefits of technology

Hydrogen gas is effectively removed from molten aluminum at minimal cost and in the shortest possible time by optimizing rotor diameter, rotation speed, and gas injection amount, achieving a hydrogen gas content of 1.0% or less within 30 minutes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023140583369-PAT00001_ABST
    Figure 112023140583369-PAT00001_ABST
Patent Text Reader

Abstract

A method for removing hydrogen gas from molten aluminum is provided. The method for removing hydrogen gas from molten aluminum according to the present invention includes a degassing step for removing hydrogen gas contained in the molten aluminum, a condition setting step for setting at least one of three elements of rotor rotation speed, inert gas input amount, and rotor diameter, and a condition application step for applying the condition to the element of the degassing step.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for removing hydrogen from molten aluminum. Background Technology

[0002] Generally, one of the factors that significantly affects the quality of aluminum alloy products is the content of hydrogen gas dissolved in the molten aluminum during melting.

[0003] Molten aluminum reacts with moisture in the atmosphere, combustion gases, refractories, and raw materials, resulting in the inclusion of a large amount of hydrogen within the molten metal.

[0004] In particular, the hydrogen generated by combining with atmospheric moisture is unavoidable even with prior preparation during atmospheric melting, so most of the hydrogen contained within the molten aluminum is produced through reactions with atmospheric moisture.

[0005] The solubility of hydrogen ions or hydrogen atoms contained within molten aluminum is lower at lower temperatures and has a greater dependence on higher temperatures, resulting in significant changes depending on temperature.

[0006] In addition, during the solidification process of manufacturing castings, the solubility decreases rapidly, causing hydrogen gas to be discharged from the solid-liquid interface and remain as defects in the form of pores or pinholes after solidification is complete.

[0007] When a large amount of hydrogen gas is discharged during the solidification process without proper pretreatment, such pores or pinholes are distributed in large numbers with significant sizes within the solidified structure, which inevitably causes a significant deterioration in the mechanical properties and surface quality of the product.

[0008] Various measures have been introduced to remove hydrogen from the molten aluminum or to prevent its formation in advance.

[0009] Currently, most industrial sites utilize a mechanism in which inert gas is introduced through a rotating shaft and an impeller or rotor coupled thereto, and the rotational force generated by the shaft and impeller or rotor evenly distributes the introduced inert gas within the molten aluminum, causing hydrogen ions or atoms to penetrate into and be removed by inert gas bubbles, after which the inert gas bubbles naturally float to the surface and separate due to buoyancy.

[0010] This method is collectively referred to as the Gas Bubbling Filtration (GBF) method.

[0011] Meanwhile, the hydrogen gas removal efficiency of the GBF method for molten aluminum is directly related to numerous factors, such as the quality of the inert gas, the stability of the molten metal during stirring, the temperature of the molten metal, the shape of the crucible, the size and shape of the rotor, the amount and bubble size of the input gas, and the temperature of the input gas.

[0012] Therefore, many practitioners try to find the optimal solution by changing various factors to improve the hydrogen gas removal efficiency of the GBF method, but this is inevitably a very difficult task because the direction and magnitude of the influence of each factor are different.

[0013] Conventionally, the conditions of factors directly related to hydrogen gas removal could not be optimized, resulting in significant costs and time consumption, and making it impossible to efficiently remove hydrogen gas from molten aluminum. The problem to be solved

[0014] The present invention aims to provide a method for removing hydrogen gas from molten aluminum that can efficiently remove hydrogen gas from molten aluminum at the minimum cost and in the shortest possible time by optimizing the conditions of elements directly related to hydrogen gas removal in the degassing step of the GBF method for removing hydrogen gas from molten aluminum. means of solving the problem

[0015] A method for removing hydrogen gas from a molten aluminum bath according to one embodiment of the present invention comprises a degassing step of removing hydrogen gas contained in the molten aluminum bath by introducing an inert gas into the molten aluminum bath contained in a melting furnace and rotating a rotor.

[0016] Additionally, the hydrogen gas removal method may include a condition setting step for setting at least one of three elements—rotor rotation speed, inert gas injection amount, and rotor diameter—in a degassing step, and a condition application step for applying the hydrogen gas removal condition of the element set in the condition setting step to the element of the degassing step.

[0017] It may include a hydrogen gas content determination step for determining the hydrogen gas content contained in the molten aluminum, which is executed between the degassing step and the condition setting step.

[0018] In addition, after the execution of the condition application step, a standard content verification step may be included to check whether the hydrogen gas content contained in the molten aluminum has been reduced to within the standard content.

[0019] The standard content verification step may include a secondary hydrogen gas content determination step for determining the hydrogen gas content contained in the molten aluminum after the application of conditions in the condition application step.

[0020] The standard content verification step may include a hydrogen gas content comparison step that compares the hydrogen gas content after applying the conditions determined in the second hydrogen gas content judgment step with the standard content.

[0021] If the hydrogen gas content is not reduced to within the reference content during the hydrogen gas content comparison step, a condition reset step may be included to reset the hydrogen gas removal conditions by the difference between the hydrogen gas content after the application of the condition and the reference content.

[0022] In the hydrogen gas content determination step, the hydrogen gas content contained in the molten aluminum can be confirmed by comparing the DI index expressed by the following equation (1) through the vacuum solidification method (RPT).

[0023] DI exponent = (ρ atm -ρ 80mmHg ) / (ρ atm )[%] --- Equation(1)

[0024] In addition, the D1 index of the standard content may be 1% or less.

[0025] The shape of the rotor can be set to a wing type or a disc type.

[0026] The condition setting step may include a rotor diameter setting step that sets the diameter of the rotor to a first ratio range relative to the internal average diameter of the melting furnace.

[0027] In addition, in the rotor diameter setting step, the first ratio range can be set to a range of 29% to 43%.

[0028] The condition setting step may include a rotor rotation speed setting step that sets the rotation speed of the rotor to a second rotation speed range.

[0029] In the rotor rotation speed setting step, the second rotation speed range can be set to a range of 200 to 300 RPM.

[0030] In addition, the condition setting step may include a gas input amount setting step for setting the amount of inert gas introduced through the rotor to a third gas input amount range.

[0031] In addition, in the gas injection amount setting step, the third gas injection amount range can be set to a range of 20 to 25 LPM. Effects of the invention

[0032] According to an embodiment of the present invention, hydrogen gas in a molten aluminum can be efficiently removed at the minimum cost and in the shortest possible time by optimizing the conditions of elements that have a direct correlation with hydrogen gas removal in the degassing step of the GBF method for removing hydrogen gas in a molten aluminum.

[0033] By applying optimal conditions for rotor diameter, rotor rotation speed, and gas injection amount of the GBF method, molten aluminum containing a large amount of hydrogen gas can be treated to a value of 1.0% or less within 30 minutes, and by presenting lower and upper limits for each condition (variable), a standard can be provided to obtain an appropriate degassing effect with minimal cost and time. Brief explanation of the drawing

[0034] FIG. 1 is a schematic conceptual diagram of a GBF method used in a method for removing hydrogen gas from molten aluminum according to one embodiment of the present invention. FIG. 2 is a diagram showing the configuration of a method for removing hydrogen gas from molten aluminum according to one embodiment of the present invention. FIG. 3 is a drawing showing the shape of a rotor used in a method for removing hydrogen gas from molten aluminum according to one embodiment of the present invention, where (a) is a wing-type rotor and (b) is a disk-type rotor. FIG. 4 is a table for selecting the optimal range for diameter, rotational speed, and gas amount for a rotary rotor for degassing hydrogen gas from molten aluminum through a GBF process according to a method for removing hydrogen gas from molten aluminum according to one embodiment of the present invention. Specific details for implementing the invention

[0035] Hereinafter, embodiments of the present invention are described with reference to the attached drawings so that those skilled in the art can easily implement the present invention. As will be easily understood by those skilled in the art, the embodiments described below may be modified in various forms without departing from the concept and scope of the present invention. Where possible, identical or similar parts are indicated using the same reference numerals in the drawings.

[0036] The technical terms used below are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. The meaning of "comprising" as used in the specification specifies a particular characteristic, area, integer, step, action, element, and / or component, and does not exclude the presence or addition of other particular characteristic, area, integer, step, action, element, component, and / or group.

[0037] All terms used below, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms defined in advance are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.

[0038] FIG. 1 is a schematic conceptual diagram of a GBF method used in a method for removing hydrogen gas from a molten aluminum bath according to one embodiment of the present invention, and FIG. 2 is a configuration diagram of a method for removing hydrogen gas from a molten aluminum bath according to one embodiment of the present invention.

[0039] FIG. 3 is a drawing showing the shape of a rotor used in a method for removing hydrogen gas from molten aluminum according to one embodiment of the present invention, where (a) is a wing-type rotor and (b) is a disk-type rotor.

[0040] Referring to FIGS. 1 to 3, a method for removing hydrogen gas from a molten aluminum bath according to one embodiment of the present invention may include a degassing step (S10) of the GBF method, a hydrogen gas content determination step (S20), a condition setting step (S30), a condition application step (S40), a reference content verification step (S50), and a termination step (S60).

[0041] The degassing step (S10) of the GBF (Gas Bubbling Filtration) method can remove hydrogen gas contained in the molten aluminum (20) by introducing an inert gas (30) into the molten aluminum (20) contained in the melting furnace (10) and rotating the rotor (40).

[0042] Additionally, the condition setting step (S30) can set conditions for the effective removal of hydrogen gas among at least one of three factors, such as rotor rotation speed, inert gas injection amount, and rotor diameter, which have a direct correlation with the hydrogen gas removal efficiency in the degassing step (S10).

[0043] The condition application step (S40) can apply the hydrogen gas removal condition of the element set in the condition setting step (S30) to the element of the degassing step (S10) by means of a control unit (not shown).

[0044] Additionally, the hydrogen gas content determination step (S20) is performed between the degassing step (S10) and the condition setting step (S30), and can determine the hydrogen gas content contained in the molten aluminum (20).

[0045] Additionally, the condition setting step (S30) can set optimization conditions for elements for effective removal of hydrogen gas based on the hydrogen gas content determined in the hydrogen gas content determination step (S20).

[0046] The standard content verification step (S50) can verify whether the hydrogen gas content contained in the molten aluminum (20) has been reduced to within the desired standard content after the execution of the condition application step (S40).

[0047] The standard content verification step (S50) may include a secondary hydrogen gas content determination step (S51) for determining the hydrogen gas content contained in the molten aluminum (20) after the application of the conditions of the condition application step (S40).

[0048] Additionally, the standard content verification step (S50) may include a hydrogen gas content comparison step (S52) that compares the hydrogen gas content after applying the hydrogen gas removal conditions determined in the second hydrogen gas content determination step (S51) with the desired standard content.

[0049] It may include a condition reset step (S300) that is placed between the gas content comparison step (S52) and the condition application step (S40), and if the hydrogen gas content is not reduced to within the reference content in the hydrogen gas content comparison step (S52), the hydrogen gas removal condition is reset by the difference between the hydrogen gas content after the condition application and the reference content.

[0050] Additionally, the termination step (S60) can terminate the degassing operation if the hydrogen gas content after applying the optimization condition determined in the second hydrogen gas content determination step (S51) of the reference content verification step (S50) is reduced to within the reference content.

[0051] In the degassing step (S10), an inert gas (30) is introduced through a rotor (30) rotating inside the molten aluminum (20), and the inert gas is evenly distributed within the molten aluminum (20) by the rotational force of the rotor (30), thereby separating the inert gas bubbles containing hydrogen gas that has penetrated into the molten aluminum (20) from the molten aluminum (20) by buoyancy.

[0052] In the hydrogen gas content determination step (S20), the hydrogen gas (31) content contained in the molten aluminum (20) can be indirectly confirmed by comparing the DI index expressed by the following equation (1) through the Reduced Pressure Test (RPT).

[0053] DI exponent = (ρ atm -ρ 80mmHg ) / (ρ atm )[%] --- Equation(1)

[0054] The DI index is basically the difference in density between a specimen solidified in the atmosphere and a specimen solidified under a pressure condition of -680 mmHg relative to atmospheric pressure (=80 mmHg), expressed as a percentage relative to the density of the specimen solidified in the atmosphere.

[0055] This DI index allows for an indirect assessment of the amount of hydrogen gas contained in the molten metal, and typically, a DI index (standard content) of 5% or less is required for low-quality aluminum products and 1% or less for high-quality aluminum products.

[0056] The shape of the rotor (40) used in the degassing step (S10) can be set to a wing type or a disc type, which has excellent stirring ability and degassing ability.

[0057] That is, the rotor (40) may include a wing-type rotor (41) as shown in FIG. 3(a), a disk-type rotor (42) as shown in FIG. 3(b), etc.

[0058] If the shape of the rotor (40) is inappropriate, even if the size of the rotor (40) is sufficient, the ability to properly stir the molten aluminum in the melting furnace (10) in the rotational direction or the up-and-down direction (Y direction in FIG. 1) is lost, or the surface of the molten aluminum (20) is excessively sloshed or disturbed, resulting in unnecessary loss of molten metal and the incorporation of impurities due to reoxidation.

[0059] In addition, if the shape of the rotor (40) is appropriate, the molten aluminum (20) in the melting furnace (10) can be stirred evenly in all areas, and the molten aluminum (20) surface is quiet, thereby preventing unnecessary loss of molten metal and reoxidation.

[0060] By applying the condition setting step (S30), effective removal of hydrogen gas from the molten aluminum (20) is possible in the shortest possible time, and unnecessary loss of molten metal and re-introduction of impurities can be prevented.

[0061] The condition setting step (S30) may include a rotor diameter setting step (S31) for setting the diameter of the rotor (40) to a first ratio range relative to the internal average diameter of the melting furnace (10) so as to increase the degassing effect and prevent motor load on the rotor (40).

[0062] In the rotor diameter setting step (S31), the first ratio range can be set to a range of about 29% to 43%.

[0063] Thus, the reason for setting the first ratio range is that the degassing effect is minimal in the range of less than 29%, and in the range exceeding 43%, it entails an excessive motor load of the rotor (40).

[0064] For example, if the inner diameter of the melting furnace (10) is about 520 mm, the diameter ratio range of the appropriate rotor (40) is 150 to 225 mm.

[0065] That is, if the size of the rotor (40) is larger than the first ratio range, the shaft and motor of the rotor (40) must also be enlarged due to the weight, and if the size of the rotor (40) is smaller than the first ratio range, the entire area of ​​the melting furnace (10) cannot be stirred.

[0066] Additionally, the condition setting step (S30) may include a rotor rotation speed setting step (S32) for setting the rotation speed of the rotor (40) to a first rotation speed range so as to increase the degassing effect and stabilize the surface of the molten aluminum (20).

[0067] In the rotor rotation speed setting step (S32), the first rotation speed range can be set to a range of 200 to 300 RPM.

[0068] Thus, the reason for setting the first rotational speed range is that the degassing effect is minimal in the range of less than 200 RPM, and in the range exceeding 300 RPM, problems such as molten metal splashing, molten metal loss, and molten metal reoxidation occur due to excessive instability of the surface of the molten aluminum (20).

[0069] That is, if the rotational speed of the rotor (40) is slower than the first rotational speed range, it does not have sufficient stirring ability, and if the rotational speed of the rotor (40) is faster than the first rotational speed range, the surface of the molten aluminum (20) is excessively sloshed or disturbed, causing molten metal loss and reoxidation.

[0070] Additionally, the condition setting step (S30) may include a gas input amount setting step (S33) for setting the amount of inert gas injected through the rotor (40) to a third gas input amount range so as to increase the degassing effect and stabilize the surface of the molten aluminum (20).

[0071] In the gas injection amount setting step (S33), the first gas injection amount range can be set to a range of 20 to 25 LPM (Liters Per Minute).

[0072] Thus, the reason for setting the first gas injection range is that the degassing effect is reduced in the range of less than 20 LPM, and excessive instability of the surface of the molten aluminum (20) is caused in the range exceeding 25 LPM.

[0073] That is, if the amount of gas injected is smaller than the first amount of gas injected, hydrogen gas in the molten aluminum (20) cannot be removed within the required time, and if the amount of gas injected is larger than the first amount of gas injected, excessive unevenness of the molten surface is caused by the aggregation and floating of gas bubbles.

[0074] In addition, in the second hydrogen gas content determination step (S51), the content of hydrogen gas (31) contained in the molten aluminum (20) can be indirectly confirmed by comparing the DI index expressed by the following equation (1) through the reduced pressure solidification method (RPT), just like in the hydrogen gas content determination step (S20).

[0075] DI exponent = (ρ atm -ρ 80mmHg ) / (ρ atm )[%] --- Equation(1)

[0076] And, the condition reset step (S300) may include a rotor diameter reset step (S310) which resets the diameter of the rotor (40) to a second ratio range relative to the internal average diameter of the melting furnace (10) according to the difference between the hydrogen gas content and the reference content after the execution of the condition application step (S40).

[0077] In the rotor diameter reset step (S310), the second ratio range can be set to a range of about 30% to 42%.

[0078] The condition reset step (S300) may include a rotor rotation speed reset step (S320) that resets the rotation speed of the rotor (40) to a second rotation speed range according to the difference between the hydrogen gas content and the reference content after the execution of the condition application step (S40).

[0079] In the rotor rotation speed reset step (S320), the second rotation speed range can be set to a range of 210 to 290 RPM.

[0080] Additionally, the condition reset step (S300) may include a gas input amount reset step (S33) which resets the amount of inert gas input through the rotor (40) to a second gas input amount range according to the difference between the hydrogen gas content and the reference content after the execution of the condition application step (S40).

[0081] In the gas injection amount reset step (S330), the second gas injection amount range can be set to a range of 21 to 24 LPM.

[0082] Hereinafter, with reference to FIGS. 1 to 4, the process of a method for removing hydrogen gas from a molten aluminum bath according to one embodiment of the present invention will be described.

[0083] First, hydrogen gas (31) contained in the molten aluminum (20) is removed by introducing an inert gas (30) into the molten aluminum (20) contained in the melting furnace (10) and rotating the rotor (40) (S10).

[0084] That is, an inert gas (30) is introduced through a rotor (40) rotating inside the molten aluminum (20), and the inert gas (30) is evenly distributed within the molten aluminum (20) by the rotational force of the rotor (30), thereby separating the inert gas bubbles, into which hydrogen gas (31) contained in the molten aluminum (20) has penetrated, from the molten aluminum (20) by buoyancy.

[0085] At this time, in addition to the inert gas (30) and hydrogen gas (31) in the molten aluminum (20), inclusions (32) and oxides (33) are also floated up and separated by buoyancy.

[0086] In addition, the hydrogen gas content contained in the molten aluminum (20) during the degassing step (S10) is indirectly determined by the DI index calculated by the following formula (1) (S20).

[0087] DI exponent = (ρ atm -ρ 80mmHg ) / (ρ atm )[%] --- Equation(1)

[0088] Then, based on the hydrogen gas (31) content determined in the hydrogen gas content determination step (S20), conditions for elements for effective removal of hydrogen gas (31) are set (S30).

[0089] The condition setting step (S30) sets the conditions of the elements for the effective removal of hydrogen gas (31) according to the hydrogen gas content determination step (S20) determined in the hydrogen gas content determination step.

[0090] That is, the shape of the rotor (40) used in the degassing step (S10) is set to a wing type or a disc type with excellent stirring and degassing capabilities.

[0091] In addition, the diameter of the rotor (40) can be set to a first ratio range relative to the internal average diameter of the melting furnace (10), i.e., a range of about 29% to 43%, to increase the degassing effect and prevent motor load on the rotor (40) (S31).

[0092] For example, if the inner diameter of the melting furnace (10) is about 520 mm, the diameter ratio range of the appropriate rotor (40) is 150 to 225 mm.

[0093] And, the rotational speed of the rotor (40) can be set to a first rotational speed range, i.e., 200 to 300 RPM range to increase the degassing effect and stabilize the surface of the molten aluminum (20) (S32).

[0094] In addition, the amount of inert gas (30) introduced through the rotor (40) can be set to a first gas introduction range, i.e., a range of 20 to 25 LPM, to increase the degassing effect and stabilize the surface of the molten aluminum (20) (S33).

[0095] In this way, the conditions set in the condition setting step (S30) are applied in the optimization condition application step (S40).

[0096] Then, after the execution of the condition application step (S40), it is checked whether the content of hydrogen gas (31) contained in the molten aluminum (20) has been reduced to within the desired standard content (S50).

[0097] That is, the hydrogen gas content (31) contained in the molten aluminum (20) after the hydrogen gas removal condition of the condition application step (S40) is determined (S51), and the hydrogen gas content after the condition application determined in the second hydrogen gas content determination step (S51) is compared with the desired standard content (S52).

[0098] At this time, in the second hydrogen gas content determination step (S51), the content of hydrogen gas (31) contained in the molten aluminum (20) can be indirectly confirmed by comparing the DI index expressed by the following equation (1) through the reduced pressure solidification method (RPT), just like in the hydrogen gas content determination step (S20).

[0099] DI exponent = (ρ atm -ρ 80mmHg ) / (ρ atm )[%] --- Equation(1)

[0100] And, if the hydrogen gas (31) content is not reduced to within the reference content in the hydrogen gas content comparison step (S52), the condition is reset by the difference between the hydrogen gas content after applying the condition in the condition setting step (S30) and the reference content (S300).

[0101] That is, depending on the difference between the hydrogen gas content and the reference content after the execution of the condition application step (S40), the diameter of the rotor (40) is reset to a first ratio range relative to the internal average diameter of the melting furnace (10), for example, a range of about 30% to 42% (S310).

[0102] In addition, depending on the difference between the hydrogen gas content and the reference content after the execution of the condition application step (S40), the rotational speed of the rotor (40) is set to a first rotational speed range, for example, 210 to 290 RPM range (S320).

[0103] Depending on the difference between the hydrogen gas content and the reference content after the execution of the condition application step (S40), the amount of inert gas (30) introduced through the rotor (40) is set to a first gas introduction amount range, for example, a range of 21 to 24 LPM (S330).

[0104] In addition, if the hydrogen gas content after applying the optimization conditions determined in the second hydrogen gas content determination step (S51) is reduced to within the standard content, the degassing operation is terminated (S60).

[0105] In this way, the hydrogen gas removal condition reset in the condition reset step (S300) is applied to the condition application step (S40), and the subsequent steps are executed again.

[0106] Therefore, in the degassing step of the GBF method for removing hydrogen gas (31) in the molten aluminum (20), hydrogen gas in the molten aluminum can be efficiently removed at the minimum cost and in the shortest possible time by optimizing the conditions of the elements that have a direct relationship to hydrogen gas removal.

[0107] By applying optimal conditions for rotor diameter, rotor rotation speed, and gas injection amount of the GBF method, molten aluminum containing a large amount of hydrogen gas can be treated to a value of 1.0% or less within 30 minutes, and by presenting lower and upper limits for each condition (variable), a standard can be provided to obtain an appropriate degassing effect with minimal cost and time.

[0108] [Example]

[0109] In one embodiment of the present invention, the GBF rotor (40) used two types of rotors selected based on excellent stirring ability and degassing ability, namely a wing-type rotor (41) (Fig. 3a) and a disc-type rotor (42) (Fig. 3b).

[0110] FIG. 4 is a table for selecting the optimal range for diameter, rotational speed, and gas amount for a rotary rotor for degassing hydrogen gas from molten aluminum through a GBF process according to a method for removing hydrogen gas from molten aluminum according to one embodiment of the present invention.

[0111] First, the rotational speed of the rotor (40) was optimized.

[0112] For example, a degassing step of the GBF method was performed on a molten aluminum (20) containing hydrogen gas (31) under conditions of a rotational speed of 150 RPM and an input gas amount of 15 LPM using a disc-shaped rotor (42) with a diameter of 150 mm.

[0113] The inner diameter of the melting furnace (10) containing the molten aluminum (20) was about 520 mm, and the depth was about 680 mm.

[0114] The molten aluminum (20), which had a DI value of 8.89% before degassing treatment, showed a DI value of 4.75% when treated for 15 minutes, 3.61% when treated for 18 minutes, and 1.76% when treated for 28 minutes under the above conditions (see Fig. 4).

[0115] These results show that it was difficult to achieve the target DI value of 1.0% through a processing time of nearly 30 minutes, and that the rotational speed of 150 RPM in the disc rotor (42) is insufficient to show sufficient degassing performance.

[0116] However, when using a disc-type rotor (42) with a diameter of 150 mm, a rotational speed of 150 RPM, and an input gas volume of 15 LPM, the DI is slightly insufficient at 1.76%, but considering the time required is 28 minutes, it can be recognized as a performance that can secure almost 1.5% DI.

[0117] In addition, it was confirmed that when using a disc-type rotor (42) with a diameter of 125 mm, under conditions of a rotational speed of 125 RPM and an input gas volume of 15 LPM, the DI was 4.0% and the degassing performance was significantly reduced at a critical diameter (150 mm) or lower.

[0118] At this time, it was confirmed that the degassing performance dropped significantly at critical diameters (150 mm) or less with a DI of 4.0%.

[0119] Also, if the DI is 1.5% or higher, it is insufficient in terms of ensuring quality.

[0120] In addition, to improve degassing performance, the rotational speed of the same disc-shaped rotor (42) was increased to 200 RPM, and then the GBF process was performed on the molten aluminum (20) containing hydrogen gas (31).

[0121] The molten aluminum (20), which had a DI value of 10.2% before treatment, showed a DI value of 3.1% when treated for 15 minutes under the above conditions, 1.5% when treated for 20 minutes, and 1.0% when treated for 30 minutes (see FIG. 4).

[0122] These results showed that a target DI value of 1.0% could be achieved with a processing time of 30 minutes, and that a rotational speed of 200 RPM on the disc rotor (42) showed sufficient degassing performance.

[0123] In addition, the same experiment was repeated by increasing the rotation speed of the rotor (40) to 350 RPM, but the surface of the molten aluminum (20) was severely sloshing and the splashing and loss of the molten metal increased rapidly, so the GBF process could not be carried out normally.

[0124] As a result of lowering the rotational speed in that state, it was confirmed that the GBF process could be carried out normally at about 300 RPM, and the degassing results under the above conditions could not be measured.

[0125] In order to examine the effect on degassing performance when the diameter of the rotor (40) is increased, a wing-type rotor (41) with a diameter of 225 mm was prepared instead of a disc-type rotor (42) with a diameter of 150 mm.

[0126] It was confirmed that when using a wing-type rotor (41) with a diameter of 225 mm, under conditions of a rotation speed of 100 RPM and an input gas volume of 20 LPM, the diameter of the wing-type rotor (41) was greatly increased, but the mixing force was insufficient due to the low rotation speed, so the injected inert gas was not mixed evenly, and the DI remained high at 3.3% even after 30 minutes (see Fig. 4).

[0127] In addition, it was confirmed that when the conditions were a rotation speed of 150 RPM and an input gas volume of 10 LPM with a wing-type rotor (41) having a diameter of 225 mm, degassing was not properly carried out because there was insufficient inert gas to react with the hydrogen gas in the molten metal, even though the diameter of the wing-type rotor (41) was large and the rotation speed was sufficient.

[0128] In the case of this wing-type rotor (41) with a diameter increased by about 50%, it was expected to show sufficient stirring and degassing capabilities compared to the disc-type rotor (42), and accordingly, the rotational speed was prepared at 150 RPM, which showed insufficient degassing capabilities in the 150 mm diameter wing-type rotor (41), and the gas injection amount was prepared at 20 LPM, which was increased by 5 LPM as the diameter increased.

[0129] As a result of GBF treatment of the aluminum molten metal (20) containing hydrogen gas (31) under the above conditions, the molten metal (20), which had a DI value of 8.3% before treatment, showed a DI value of 4.3% after 10 minutes of treatment, 1.5% after 20 minutes of treatment, and 1.2% after 30 minutes of treatment (see FIG. 4).

[0130] These results showed that the target DI value of 1.0% could not be achieved through 30 minutes of treatment, and that despite the increase in diameter, a rotor rotation speed of 150 RPM did not provide sufficient degassing ability.

[0131] To compensate for the insufficient degassing ability of the wing-type rotor (41) with a diameter of 225 mm, the rotational speed was increased to 250 RPM and the gas volume to 25 LPM, and a GBF test for removing hydrogen gas from molten aluminum was conducted.

[0132] Although GBF could not be performed for a sufficient amount of time due to experimental conditions, it was confirmed that the molten metal, which initially had a DI value of 13.0%, was degassed to have a DI value of 1.3% in 20 minutes. Although the change in DI value after 30 minutes of treatment could not be confirmed, it was confirmed that the degassing performance was relatively improved.

[0133] In addition, to further improve the degassing ability of the wing-shaped rotor (41) with a diameter of 225 mm, the rotational speed was increased to 300 RPM and the gas volume was maintained at 25 LPM.

[0134] As a result of performing the GBF process on the molten aluminum (20) containing hydrogen gas (31), it initially had a DI value of 6.0%, then showed a very low DI value of 0.77% after 10 minutes, 0.80% after 15 minutes, and 0.52% after 20 minutes (see FIG. 4).

[0135] Through this, it was found that increasing the rotational speed to 300 RPM significantly contributes to the improvement of degassing ability.

[0136] In addition, to verify the change in degassing ability with respect to the shape change of the rotor (40) at the same diameter of 225 mm, an experiment was conducted using a disc-shaped rotor (42) with a diameter of 225 mm.

[0137] This disc-shaped rotor (42) has six slit-shaped blades on the bottom surface and six slit-shaped blades on the sides. For comparison, the rotational speed was maintained at 300 RPM and the gas volume at 25 LPM.

[0138] As a result of performing the GBF process on the molten aluminum (20) containing hydrogen gas (31), the initial DI value was 7.4%, then 0.97% after 10 minutes, 0.46% after 15 minutes, and 0.52% after 20 minutes.

[0139] And, when the conditions were a rotation speed of 350 RPM and an input gas volume of 25 LPM with a wing-type rotor (41) with a diameter of 225 mm, molten metal splashing occurred due to excessive stirring force and a vortex was generated around the rotation axis of the wing-type rotor (41), causing the degassing process to stop.

[0140] This is because severe vortex formation leads to adverse effects, such as the mixing of suspended foreign substances into the surface of the molten metal and an increase in hydrogen concentration due to the re-mixing of moisture from the air.

[0141] In addition, when using a wing-type rotor (41) with a diameter of 250 mm at a rotational speed of 300 RPM and an input gas volume of 25 LPM, the molten metal splashing occurred due to excessive stirring force, causing the degassing process to stop.

[0142] Compared to the results of a wing-shaped rotor (41) of the same diameter, the results showed a change in superiority over time, but regardless of the difference in the shape of the rotor (40), a very good DI value was shown within 20 minutes, and it was confirmed that excellent degassing ability was shown at a diameter of 225 mm, a rotation speed of 300 RPM, and a gas volume of 25 LPM (see FIG. 4).

[0143] When using a disc-shaped rotor (42) with a diameter of 225 mm at a rotational speed of 300 RPM and an input gas volume of 30 LPM, the same DI of 0.5% is achieved compared to when using a disc-shaped rotor (42) with the same diameter at a rotational speed of 300 RPM and an input gas volume of 25 LPM, so there is no difference.

[0144] Rather, when using a disc-shaped rotor (42) with a diameter of 225 mm at a rotational speed of 300 RPM and an input gas volume of 30 LPM, the instability caused by the escape of the input gas to the surface of the molten metal increases qualitatively, and the input gas is excessive and uneconomical.

[0145] For the rotary rotor (40) for degassing hydrogen gas (31) from the molten aluminum (20) through the GBF process, an optimal range for diameter, rotation speed, and gas volume was selected.

[0146] For example, in an aluminum melting furnace (10) with an inner diameter of 520 mm and a depth of 680 mm, the optimal diameter of the rotor (40) was 150 to 225 mm.

[0147] It was confirmed that a rotor (40) with a diameter of 150 mm could not reach the DI standard value of 1.0% within 30 minutes when the rotational speed was low, but could barely reach the standard value within 30 minutes when the rotational speed was high, and that such a diameter of the rotor (40) could be considered as the minimum value.

[0148] Meanwhile, in a rotor (40) with a diameter of 225 mm, the degassing ability was insufficient when the rotational speed was 150 RPM, but when the speed was 250 RPM or higher, a DI value of 1.0% could be obtained within 30 minutes.

[0149] And it was confirmed that for rotors (40) with a diameter of more than 225 mm, the load cannot be handled by motors typically used in the field, so expensive motors must be applied.

[0150] In the above, the diameter of the 150mm rotor (40) is about 29% of the inner diameter of the melting furnace (10), and the diameter of the 225mm rotor (40) is about 43% of the inner diameter of the melting furnace (10).

[0151] In addition, the optimal rotational speed of the rotor (40) was 200 to 300 RPM. At a rotational speed of 150 RPM, it was not possible to obtain a DI value of 1.0% within 30 minutes even with a rotor of 225 mm in diameter, and at a rotational speed of 350 RPM, normal operation was impossible due to excessive molten metal surface sloshing and vortex phenomena.

[0152] Also, the optimal gas injection amount was 20 to 25 LPM. At a gas injection amount of 15 LPM, there were no cases where sufficient degassing capacity was secured, and at a gas injection amount of 20 LPM, there were cases where sufficient degassing capacity was secured only when the rotational speed was sufficient.

[0153] In addition, very sufficient degassing capability was secured at a rotation speed of 250 to 300 RPM with a gas injection amount of 25 LPM. However, it was confirmed that if more than 30 LPM of gas is injected, there is a safety issue due to the phenomenon of bubbles merging and rising, then bursting at the surface of the molten metal.

[0154] Finally, the appropriate rotor shape was a disc shape. When comparing the experimental results of a disc-shaped rotor (42) with the same diameter of 225 mm and the experimental results of a wing-shaped rotor (41), it was confirmed that the stability of the molten metal surface was superior in the experiment of the disc-shaped rotor (42), although it is not expressed in numerical DI values.

[0155] It can be estimated that such molten metal surface stability will have the effect of minimizing molten metal reoxidation and hydrogen gas (31) re-incorporation.

[0156] Although the present disclosure has been described through preferred embodiments as described above, those skilled in the art will readily understand that the present invention is not limited thereto and that various modifications and variations are possible without departing from the scope of the claims set forth below. Explanation of the symbols

[0157] 10: Melting furnace 20: Molten aluminum 30: Inert gas 31: Hydrogen gas 32: Inclusion 33: Oxide 40: Rotor 41: Winged rotor 42: Disc rotor S10: Degassing stage S20: Hydrogen gas content determination step S30: Condition setting step S31: Rotor diameter setting step S32: Rotor rotation speed setting step S33: Gas injection amount setting step S40: Condition application step S50: Standard content verification step S51: Secondary hydrogen gas content determination step S52: Hydrogen gas content comparison step S60: Termination phase S310: Rotor diameter reset step S320: Rotor rotation speed reset step S330: Gas injection amount reset step

Claims

Claim 1 A hydrogen gas content determination step for determining the hydrogen gas content contained in the molten aluminum contained in the melting furnace by comparing the DI index expressed by the following formula (1) through the vacuum solidification method (RPT); a condition setting step for setting hydrogen gas removal conditions for all three elements of rotor rotation speed, inert gas input amount, and rotor diameter in the degassing step after the hydrogen gas content determination step, wherein, based on a melting furnace with an inner diameter of 520 mm and a depth of 680 mm, the rotation speed of a rotor having a diameter in the range of 29% to 43% relative to the inner average diameter of the melting furnace is set to a range of 200 to 300 RPM, and the input amount of inert gas introduced through the rotor is set to a range of 20 to 25 LPM; a condition application step for applying the hydrogen gas removal conditions of the elements set in the condition setting step to the elements of the degassing step; a degassing step for removing hydrogen gas contained in the molten aluminum contained in the melting furnace by the introduction of inert gas and the rotation of the rotor; and the A method for removing hydrogen gas from molten aluminum, comprising: a second hydrogen gas content determination step in which, after a degassing step, the hydrogen gas content contained in the molten aluminum after applying the conditions of the condition application step is determined through the following formula (1); a hydrogen gas content comparison step in which the DI index of the hydrogen gas content after applying the conditions determined in the second hydrogen gas content determination step is compared with a reference content DI index of 1%; and a condition reset step in which, if the DI index of the hydrogen gas content is not reduced to 1% or less as a result of the comparison in the hydrogen gas content comparison step, the diameter of the rotor is reset to a range of 30% to 42% relative to the internal average diameter of the melting furnace, the rotation speed of the rotor is reset to a range of 210 to 290 RPM, and the amount of inert gas injected is reset to a range of 21 to 24 LPM, thereby re-executing the condition application step and the degassing step. DI Index = (ρ atm -ρ 80mmHg ) / (ρ atm )[%] --- Equation (1) Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 delete Claim 8 delete Claim 9 A method for removing hydrogen gas from molten aluminum, wherein, in claim 1, the shape of the rotor is set to be wing-shaped or disc-shaped. Claim 10 delete Claim 11 delete Claim 12 delete Claim 13 delete Claim 14 delete Claim 15 delete

Citation Information

Patent Citations

  • Rotary stirring device for processing molten metal

    JP2006511705A