Stripping agent for resin film for circuit boards and method for manufacturing a circuit board

The described stripping agent efficiently peels resin films on circuit boards with minimal residue and environmental burden by using a compound and aliphatic alcohol combination, addressing peelability and residue issues in existing technologies.

KR103046781B1Active Publication Date: 2026-11-10NOF CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
KR1020237044431
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-24
Filing Date
2022-06-10
Publication Date
2026-11-10
Estimated Expiration
2042-06-10

AI Technical Summary

Technical Problem

Existing stripping agents for resin films on circuit boards face challenges in achieving high peelability, leading to residue issues and environmental toxicity, with prolonged processing times affecting productivity.

Method used

A stripping agent comprising a compound represented by formula (1) and an aliphatic alcohol with specific carbon and molecular weight ranges, pH 13.0 to 14.0, and component ratios, enhancing penetration and subdivision of the resin film for efficient peeling.

Benefits of technology

The agent effectively peels resin films in a short time with reduced residue and low environmental impact, improving productivity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023144099994-PCT00017_ABST
    Figure 112023144099994-PCT00017_ABST
Patent Text Reader

Abstract

The present invention provides a resin film stripper for a circuit board that can strip a resin film formed on a circuit board in a short time, has high performance in separating the resin film, and has a low environmental load. One embodiment of the present invention relates to a resin film stripper for a circuit board containing a compound represented by formula (1) (component (A)), and an aliphatic alcohol (component (B)) having 1 to 6 carbon atoms and a molecular weight of 30 to 120, having a pH of 13.0 or higher and less than 14.0, wherein the content of component (A) is 0.1 mass% or higher and 5 mass% or lower, and the content of component (B) is 5 mass% or higher and 40 mass% or lower. (In formula (1), R1 represents a branched alkyl group having 6 to 10 carbon atoms, A1O represents an oxyalkylene group having 2 to 3 carbon atoms, and a, the average added mole of oxyalkylene groups, is a number between 2 and 15.)
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a release agent for a resin film for a circuit board and a method for manufacturing a circuit board. Background Technology

[0002] Recently, in the field of electronic information devices, technological evolution is progressing to enable the miniaturization and lightweighting of electronic devices, as well as to support high-capacity communication. To facilitate these technological advancements, high precision in electronic circuit components is being pursued. Electronic circuit components are formed by photolithography patterning using photosensitive resins. Furthermore, to meet the demands for high precision in electronic circuit components, the photosensitive resins require improved photoresponsiveness and strength after curing, such as enabling fine photolithography patterning. On the other hand, the photosensitive resins are also required to be easily peeled off and removed from the substrate after the photolithography patterning process. However, it is difficult to achieve both higher strength after curing and high peelability from the substrate after the photolithography patterning process.

[0003] In addition, conventionally, a release agent containing an amine compound, such as quaternary ammonium hydroxide, has been used for peeling off the above photosensitive resin from a substrate, but release agents containing amine compounds have the problem of being highly toxic and having a high burden on the environment. Therefore, there is a need to develop a method to improve the peelability of the photosensitive resin by using an alternative alkaline release agent.

[0004] For example, Patent Document 1 describes a water-based stripping solution for photoresist (photosensitive resin) that is a stripping agent for photoresist applied to a substrate having a conductive metal film including aluminum or silver, comprising a surfactant, an anti-corrosion agent, and a water-soluble organic solvent.

[0005] In addition, Patent Document 2 describes a water-based resin mask peeling detergent composition comprising an inorganic alkali, a polyhydric alcohol, and other organic solvents.

[0006] In addition, Patent Document 3 describes a cleaning agent composition for peeling resin masks comprising an inorganic alkali and a surfactant having an ethyleneoxy group. Prior art literature

[0007] [Patent Document 1] Japanese Published Patent Application No. 2008-58624 [Patent Document 2] Japanese Published Patent Application No. 2019-117331 [Patent Document 3] Japanese Published Patent Application No. 2019-105670 The problem to be solved

[0008] However, according to the inventors' knowledge, the above alternative stripping agent has a problem in that it is difficult to sufficiently remove residues of the resin film, such as photosensitive resin films, due to insufficient performance of the resin film segmentation, which is an advantage of amine compounds.

[0009] For example, the stripper described in Patent Document 1 had insufficient peelability of the resin film, and there were cases where residue of the resin film remained on the circuit board. Also, the cleaning agent composition described in Patent Document 2 showed insufficient peelability due to insufficient penetration of the active ingredient into the resin film and insufficient performance of separating the resin film, and there were also cases where residue of the resin film remained on the circuit board. Furthermore, the cleaning agent composition described in Patent Document 3 had improved penetration of the active ingredient into the resin film, but the peelability of the resin film was still insufficient, and there was a problem that a long processing time was required to sufficiently peel off the resin film, causing a decrease in productivity.

[0010] The present invention is made in consideration of the above circumstances and aims to provide a release agent for a resin film for a circuit board, a method for manufacturing a circuit board, and a method for manufacturing a circuit board using said release agent, which can peel off a resin film formed on a circuit board in a short time and has high performance in reducing residue on the circuit board by subdividing the resin film and also has a low environmental burden. means of solving the problem

[0011] In one embodiment of the present invention for solving the above problem, a stripper for a resin film for a circuit board contains a compound represented by formula (1) (component (A)) and an aliphatic alcohol (component (B)) having a carbon number of 1 or more and 6 or less and a molecular weight of 30 or more and 120 or less, the pH of the stripper is 13.0 or more and less than 14.0, and the content of the component (A) is 0.1 mass% or more and 5 mass% or less relative to the total mass of the stripper, and the content of the component (B) is 5 mass% or more and 40 mass% or less relative to the total mass of the stripper.

[0012]

[0013] (In Equation (1), R 1 A is a branched alkyl group having 6 to 10 carbon atoms, 1 O represents an oxyalkylene group having 2 to 3 carbon atoms, and a, the average added mole of the oxyalkylene group, is a number between 2 and 15.

[0014] A method for manufacturing a circuit board in another embodiment of the present invention for solving the above problem comprises a step of preparing a circuit board having a resin film formed on at least one surface, and a step of contacting the release agent with the resin film. Effects of the invention

[0015] According to the present invention, a resin film stripper for a circuit board and a method for manufacturing a circuit board are provided, which can strip a resin film formed on a circuit board in a short time and has high performance in reducing residue on the circuit board by subdividing the resin film and also has a low environmental load. Specific details for implementing the invention

[0016] Hereinafter, embodiments of the present invention will be described.

[0017] A stripping agent for a resin film for a circuit board according to one embodiment of the present invention (hereinafter also simply referred to as "stripping agent") contains a compound represented by formula (1) (component (A)), and an aliphatic alcohol (component (B)) having 1 to 6 carbon atoms and a molecular weight of 30 to 120, and has a pH of 13.0 or higher and less than 14.0.

[0018]

[0019] (In Equation (1), R 1 A is a branched alkyl group having 6 to 10 carbon atoms, 1 O represents an oxyalkylene group having 2 to 3 carbon atoms, and a, the average added mole of the oxyalkylene group, is a number between 2 and 15.

[0020] Below, each component included in the peeling agent is described.

[0021] Component (A) is a compound (polyalkylene glycol) represented by formula (1). Component (A) can sufficiently subdivide the resin film for circuit boards (hereinafter also simply referred to as "resin film") to make it easy to peel off, thereby reducing residue on the circuit board.

[0022]

[0023] In Equation (1), R 1 Silver represents a branched alkyl group having 6 to 10 carbon atoms. R 1It is preferable that the silver be a branched alkyl group having 8 or more and 9 or fewer carbon atoms. R 1 If this is a branched alkyl group with 6 or more carbon atoms and 10 or fewer carbon atoms, component (A) becomes easier to penetrate into the resin film, making it easier to sufficiently subdivide and peel off the resin film, thereby reducing residue on the circuit board, and it is also difficult to generate foam in the release agent, and the stability of the release agent during storage is higher.

[0024] In particular, component (A) is R 1 By being a branched alkyl group, the peeling performance of the resin film can be further enhanced. In the above regard, R 1 The branch chain included in the is preferably an alkyl group having 1 to 3 carbon atoms, and preferably a methyl branch or an ethyl branch.

[0025] R 1 Specific examples include isooctyl groups, 2-ethylhexyl groups, isononyl groups, 3,5,5-trimethylhexyl groups, and isodecyl groups.

[0026] In Equation (1), A 1 O represents an oxyalkylene group having 2 to 3 carbon atoms. Also, A 1 O may be only oxyethylene, only oxypropylene, or may include both oxyethylene and oxypropylene groups. A 1 It is preferable that O be only oxyethylene groups, or include both oxyethylene and oxypropylene groups.

[0027] A 1 When O includes both oxyethylene groups and oxypropylene groups, the oxyethylene group (EO group) forming alone or a block and the oxypropylene group (PO group) forming alone or a block are R 1 It is desirable that they be added in the order of -O-EO group-PO group-H. R 1A component (A) having such a structure as O has particularly high penetration into the resin film, further subdivides the resin film into finer segments, and also peels it off, thereby reducing the residue on the circuit board.

[0028] In formula (1), a is an oxyalkylene group (A 1 O) is the average additional forfeiture, and is a number between 2 and 15. It is preferable that a is a number between 4 and 7. Also, A 1 When O is composed solely of oxyethylene groups, it is preferable that a is a number between 2 and 10, and A 1 When O is composed solely of oxypropylene groups, it is preferable that a is a number between 2 and 6, and A 1 When O includes both oxyethylene and oxypropylene groups, it is preferable that a is a number of 5 or more and 10 or less.

[0029] A 1 When O contains both oxyethylene groups and oxypropylene groups, if the average number of moles added to the oxyethylene group is denoted as a' and the average number of moles added to the oxypropylene group is denoted as a", it is preferable that a' / a" be 0.5 or more and 1.5 or less. A component (A) in which a' / a" is within the above range has higher penetration into the resin film and can reduce the residue on the circuit board. In addition, a component (A) in which a' / a" is within the above range is less likely to cause foaming in the release agent, so the load on the surrounding environment caused by the release agent can be reduced, and the load on the device being used can be reduced, thereby increasing productivity.

[0030] The peeling agent may include only one type of compound represented by formula (1) as component (A), or may include multiple types, but it is more preferable to include multiple types from the perspective of peeling performance.

[0031] In cases involving multiple species, R 1 This is a branched alkyl group having 6 to 8 carbon atoms (a1), and R 1It is more preferable to combine the branched alkyl group (a2) having 9 or 10 carbon atoms, and it is more preferable to combine the branched alkyl group having 8 carbon atoms with the branched alkyl group having 9 carbon atoms.

[0032] When combining (a1) and (a2), regarding the ratio of (a1) and (a2), a mass ratio of (a1) / (a2)=99 / 1 to 40 / 60 is preferred, 98 / 2 to 50 / 50 is more preferred, 98 / 2 to 75 / 25 is more preferred, and 97 / 3 to 80 / 20 is particularly preferred.

[0033] The HLB value of component (A) is not specifically limited and, for example, can be 5 or more and 13 or less.

[0034] The content of component (A) relative to the total mass of the stripper is 0.1 mass% or more and 5 mass% or less, preferably 0.5 mass% or more and 5 mass% or less, and more preferably 1 mass% or more and 2 mass% or less. If the content of component (A) is 0.1 mass% or more, the penetration of the stripper into the resin film is increased, and the residue on the circuit board can be reduced. If the content of component (A) is 10 mass% or less, the stability of the stripper during storage is higher.

[0035] [Ingredient (B)]

[0036] Component (B) is an aliphatic alcohol having 1 to 6 carbon atoms and a molecular weight of 30 to 120. Component (B) can increase the peelability of the resin film from the circuit board, while making it difficult to generate foam in the release agent and also increasing the stability of the release agent during storage.

[0037] The stripping agent may include only one type of aliphatic alcohol as component (B) or multiple types, but it is more preferable to include multiple types from the perspective of fine-graining performance.

[0038] In the case of including multiple types, it is more preferable to combine (b1), which has one hydroxyl group in the molecule, and (b2), which has two or more hydroxyl groups in the molecule, and it is more preferable to combine one with one hydroxyl group and three with three hydroxyl groups.

[0039] When combining (b1) and (b2), regarding the ratio of (b1) and (b2), a mass ratio of (b1) / (b2)=99 / 1 to 80 / 20 is preferred, 98 / 2 to 85 / 15 is more preferred, and 97 / 3 to 90 / 10 is particularly preferred.

[0040] Component (B) is preferably a water-soluble alcohol. Additionally, component (B) may have an alicyclic structure or an alicyclic (straight or branched) structure. Additionally, component (B) may have an ether structure within the molecule. Component (B) may have one or more hydroxyl groups within the molecule. The number of hydroxyl groups within the molecule of component (B) is not limited, but it is preferably between one and three.

[0041] Examples of component (B) include methanol, ethanol, isopropyl alcohol, ethylene glycol, diethylene glycol, glycerin, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, 3-methoxy-1-butanol, 3-methoxy-3-methyl-1-butanol, tetrahydrofurfuryl alcohol, etc.

[0042] Among these, 3-methoxy-3-methyl-1-butanol, tetrahydrofurfuryl alcohol, glycerin, diethylene glycol, and methanol are preferred, and 3-methoxy-3-methyl-1-butanol and glycerin are more preferred.

[0043] The content of component (B) relative to the total mass of the release agent is 5 mass% or more and 40 mass% or less, preferably 5 mass% or more and 35 mass% or less, and more preferably 5 mass% or more and 30 mass% or less. If the above content of component (B) is 5 mass% or more, the resin film can be sufficiently subdivided. If the above content of component (B) is 40 mass% or less, the releaseability and subdivision performance of the resin film are increased, and the stability of the release agent during storage is also higher.

[0044] [Ingredient (C)]

[0045] In addition to the components described above, the stripping agent may also include a rust inhibitor (component (C)). Component (C) can further enhance the effects of the present invention.

[0046] As a component (C), the stripping agent may include only one type of the above-mentioned rust inhibitor or may include multiple types.

[0047] The type of rust inhibitor is not particularly limited, and known rust inhibitors having imidazole, pyrazol, oxazole, thiazole, triazole, and tetrazole rings can be used.

[0048] In terms of increasing the peelability of the resin film, component (C) is preferably a compound having a triazole ring, more preferably a compound having a benzotriazole structure, and even more preferably a compound represented by formula (2).

[0049]

[0050] In Equation (2), R 2 represents a hydrogen atom, a methyl group, or a carboxyl group. Among these, in terms of further enhancing the water solubility of component (C) and the peelability of the resin film, R 2 It is preferable that it be a hydrogen atom or a carboxyl group, and more preferable that it be a hydrogen atom.

[0051] The content of component (C) relative to the total mass of the stripper is not particularly limited, but it is preferable that it be 0.5 mass% or more and 2 mass% or less, more preferable that it be 0.5 mass% or more and 1.5 mass% or less, and more preferable that it be 1.0 mass% or more and 1.5 mass% or less. If the above content of component (C) is 0.5 mass% or more, the stability of the stripper during storage can be increased. Also, if the above content of component (C) is 0.5 mass% or more, the resin film can be sufficiently subdivided to make it easy to peel off, thereby reducing residue on the circuit board. If the above content of component (C) is 2 mass% or less, it is difficult to generate foam in the stripper. Also, if the above content of component (C) is 2 mass% or less, the stability of the stripper during storage is higher. Also, if the above content of component (C) is 2 mass% or less, the resin film can be sufficiently subdivided to make it easy to peel off, thereby reducing residue on the circuit board.

[0052] [pH·Alkaline Components]

[0053] The pH of the peeling agent is preferably 13.0 or higher and 14.0 or lower, preferably 13.2 or higher and 13.8 or lower, and more preferably 13.4 or higher and 13.6 or lower. When the pH is within the above range, the peelability of the resin film is sufficiently high. The pH of the peeling agent can be adjusted to the above range by adding a known alkali component.

[0054] The above alkali component is a compound that is water-soluble and makes the aqueous solution alkaline when dissolved in water. The above alkali component may be an organic alkali component containing carbon atoms in its molecules, or an inorganic alkali component that does not contain carbon atoms in its molecules.

[0055] The peeling agent may include only one type of alkaline component for adjusting the pH, or it may include multiple types.

[0056] Examples of the above organic alkali components include monoethanolamine, diethanolamine, and triethanolamine. Examples of the above inorganic alkali components include sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium hydroxide, sodium carbonate, potassium carbonate, sodium silicate, and potassium silicate.

[0057] The above organic alkali component is preferably sodium hydroxide, potassium hydroxide, sodium carbonate, or potassium carbonate in order to further increase the peelability of the resin film, and is more preferably sodium hydroxide or potassium hydroxide.

[0058] [Other ingredients]

[0059] In addition to the components described above, the release agent may include other components generally incorporated into release agents for resin films for circuit boards. Examples of the above other components may include preservatives, thickeners, colorants, etc.

[0060] [Preparation of the peeling agent]

[0061] The stripping agent can be prepared by a known method of diluting the above components with water to an appropriate concentration to form an aqueous solution. As the water for dilution, ion-exchanged water, distilled water, RO water, tap water, and industrial water may be used.

[0062] The water content relative to the total mass of the peeling agent is preferably 50 mass% or more, more preferably 60 mass% or more, and more preferably 70 mass% or more. The water content is not particularly limited, but is preferably 90 mass% or less.

[0063] [Use of stripping agents]

[0064] A stripping agent is used to remove a resin film temporarily formed on the surface of a circuit board after performing the necessary processing, in a known method of manufacturing a circuit board.

[0065] That is, the method for manufacturing the circuit board comprises a process of forming a resin film on the surface of the circuit board, a process of processing the circuit board on which the resin film is formed on at least one surface, and a process of removing the resin film from the circuit board after processing using a release agent.

[0066] The resin film formed on the surface of the circuit board may be a negative-type resin film that hardens by external stimuli such as light and heat, or a positive-type resin film that dissolves by said external stimuli, but a negative-type resin film is preferred. Examples of said negative-type resin films include negative-type dry film resists and negative-type liquid resists. By forming a fine pattern on the resin film by said external stimuli (specifically exposure and development), the circuit board can be micro-processed using the resin film with the formed pattern as a mask (protective film). The method of processing the circuit board is not particularly limited, and known methods such as laser irradiation and etching may be used.

[0067] Thereafter, the resin film after processing can be removed by bringing a stripping agent into contact with the resin film. The contact can be performed by known methods, such as immersing the circuit board in a stripping solution and spraying the stripping solution onto the circuit board.

[0068] It is believed that the release agent peels off the resin film by dissolving the resin film at the interface between the circuit board and the resin film, or by penetrating into the resin film and swelling the resin film, thereby reducing the adhesion at the interface between the circuit board and the resin film. In order to make these actions more fully manifest, it is desirable to sufficiently penetrate the release agent into the resin film so that a sufficient amount of release agent reaches the interface between the circuit board and the resin film. In addition, it is believed that the release agent breaks down the resin film through the above penetration, thereby making it easier to peel off the resin film.

[0069] When the release agent is brought into contact with the resin film, it is preferable to set the temperature of the release agent to about 20 to 60°C.

[0070] [Example]

[0071] The present invention will be explained below using examples and comparative examples, but the present invention is not limited to the following examples at all.

[0072] 1. Preparation of release agent

[0073] 1-1. Materials

[0074] 1-1-1. Alcohol having the structure represented by formula (1)

[0075] Compounds A1, A2, and A1' shown in Table 1 were prepared. Compounds A1 and A2 are compounds (component (A)) represented by formula (1), and compound A1' has the structure represented by formula (1), but R 1 Because this is different, it is a compound that is not component (A).

[0076]

[0077] In Table 1, R in Formula (1) of Compound A1, Compound A2 and Compound A1' 1 Structure of (sensory name), R 1 The number of carbon atoms of, A 1 It represents the composition of O, the number of EO groups and PO groups (average value), the value of a' / a" (number of EO groups (average value) / number of PO groups (average value)), and the number of a (average value).

[0078]

[0079] 1-1-2. Organic Solvents

[0080] Compounds B1 to B5 and compound B1' listed in Table 2 were prepared. Compounds B1 to B5 are aliphatic alcohols (component (B)) having 1 to 6 carbon atoms and a molecular weight of 30 to 120, and compound B1' is an organic solvent that is not component (B).

[0081] Table 2 shows the compound names, molecular weights, number of carbon atoms, and number of hydroxyl groups of compounds B1 to B5 and compound B1'.

[0082]

[0083] 1-1-3. Rust Inhibitor

[0084] Benzotriazole was prepared. Benzotriazole is R in Equation (2). 2 is a compound of H (component (C)).

[0085]

[0086] 1-1-4. Alkaline Components

[0087] Compounds D1 to D3 listed in Table 3 were prepared. Compounds D1 to D3 are all alkaline components (component D).

[0088] Table 3 shows the names of compounds D1 to D3.

[0089]

[0090] 1-2. Preparation of Peeling Agents

[0091] Each of the above components was dissolved in water, and water was added so that the total amount was 100 mass% to prepare water-based stripping agents 1 to 14 for resin films for circuit boards and stripping agents 21 to 28 for resin films for circuit boards.

[0092] 1-3. Measurement of pH

[0093] The pH of stripping agents 1 to 14 and stripping agents 21 to 28 was measured using a pH meter ("LAQUA F-72": manufactured by Horiba Seisakusho Co., Ltd.). In addition, the measurement temperature was set to 25°C, and each stripping agent was measured while stirring in a constant temperature bath at 25°C.

[0094] 2. Evaluation of Release Agents

[0095] The above-prepared release agents 1 to 14 and release agents 21 to 28 were evaluated according to the following criteria.

[0096] 2-1. Peel-off Test

[0097] 2-1-1. Formation of a resin film for a circuit board

[0098] As a resin film for integrated circuits, a photosensitive PCB circuit film (manufactured by Guang Zhou TiYaLin Electronic Technology Co., Ltd.) was used. The above film is a negative-type dry film resist.

[0099] As an electronic circuit board, an oxygen-free copper plate ("Oxygen-free copper plate": manufactured by TP Giken Co., Ltd., length × width × thickness = 50 × 15 × 1 mm) was used. The negative-type dry film resist was coated on the electronic circuit board. Specifically, the negative-type dry film resist was processed to a predetermined size (height × width = 20 × 15 mm), and after peeling off the protective film on one side, the side from which the protective film was peeled off was adhered to the electronic circuit board. In this state, a hot plate was used to heat-press for 30 seconds under conditions of 100°C. After that, using a UV spot light source ("LIGHTNING CURE LC6": manufactured by Hamamatsu Photonics Co., Ltd.), UV light was irradiated onto the surface of the negative-type dry film resist that was heat-pressed on the electronic circuit board (irradiation time: 120 seconds, total light intensity: approximately 22 mW), and the negative-type dry film resist was cured to obtain a circuit board having a resin film (resin film for circuit boards) formed thereon.

[0100] 2-1-2. Peeling Test (Peeling Evaluation, Detailed Evaluation)

[0101] A circuit board coated with the above-described negative-type dry film resist was completely immersed in approximately 50g of one of the above-described stripping agents within a 50mL screw tube, and while stirring at 500rpm, the time until the complete removal of the resin film was visually confirmed was measured. In addition, several test specimens after stripping were randomly removed from the stripping agent, and the lengths of the four sides of the test specimens were measured, and the average values ​​were calculated. The liquid temperature during the stripping test was adjusted to 50℃, and the test was conducted. This series of stripping processes was repeated three times.

[0102] The average value of three tests performed on the time required until the resin film is completely removed visually after immersing a circuit board in a stripping solution was defined as the "strip time" by the stripping solution. In addition, the average value of three tests performed on the average length of the side of the test specimen measured by immersing a circuit board in a stripping solution was defined as the "side length of the stripped specimen" generated by the stripping solution.

[0103] Based on the above "peeling time" and "quadruple length of peeled piece," each peeling solution was evaluated according to the following criteria.

[0104] <(1-1) Detachment Evaluation>

[0105] ◎: The peeling time was within 90 seconds.

[0106] ○: The peeling time was more than 90 seconds and within 120 seconds.

[0107] ×: The peeling process exceeded 120 seconds.

[0108] <(1-2) Detailed Evaluation>

[0109] ◎: The average quadrant length of the peeled fragment was 2 mm or less.

[0110] ○: The average side length of the peel fragment was greater than 2 mm and less than or equal to 5 mm.

[0111] ×: The average quadrant length of the peeled fragments exceeded 5 mm.

[0112] 2-2. Low Foaming Test

[0113] 10g of the above peeling agent, before adding water, was weighed into each 100ml screw tube so that the total amount was 100% by mass. Then, the lid was covered and the mixture was shaken vigorously up and down for 10 seconds, after which it was left to stand. The height of the foam from the liquid surface was measured after 30 seconds of standing.

[0114] Based on the foam height measured above, each peeling solution was evaluated according to the following criteria.

[0115] <(2) Low-saturation>

[0116] ◎: The foam height was 5mm or less.

[0117] ○: The foam height was higher than 5mm and less than or equal to 10mm.

[0118] ×: The bubble height was higher than 10mm

[0119] 2-3. Stability Test

[0120] 50 ml of the above stripping agent was poured into each 100 ml screw tube, and each was left in a constant temperature bath at -10°C and 25°C for one week. The appearance of the stripping agent after leaving it was checked.

[0121] Based on the appearance of the peeling agent observed above, each peeling solution was evaluated according to the following criteria.

[0122] <(3) Stability>

[0123] ○: At either temperature, the release agent after settling was uniform and transparent.

[0124] ×: At least at one temperature, the release agent after settling was cloudy.

[0125] The content of each of the above components included in peeling agents 1 to 15 and peeling agents 21 to 28, the pH of each peeling solution, and the results of the above evaluation for each peeling solution are shown in Tables 4 to 8. In addition, the numerical values ​​for the components in Tables 4 to 8 represent the ratio (unit is mass%) to the total mass of the peeling agent.

[0126]

[0127]

[0128]

[0129]

[0130]

[0131] As can be seen from Tables 4 to 8, the release agent containing component (A) and component (B) can peel off the resin film formed on the circuit board in a short time, has high performance in breaking down the resin film, and has low environmental burden due to its low foaming properties.

[0132] This application claims priority based on Japanese application No. 2021-104677 filed on June 24, 2021, and the claims and contents of the specification of said application are incorporated into this application. Industrial applicability

[0133] According to the present invention, a release agent is provided that can peel off a resin film formed on a circuit board in a short time, has high performance in subdividing the resin film, and has a low environmental burden. The present invention is expected to contribute to shortening the manufacturing time and reducing the manufacturing load of electronic circuit components, thereby bringing about further development in various fields utilizing electronic circuit components.

Claims

Claim 1 A stripper for a resin film for a circuit board comprising a compound represented by formula (1) (component (A)), an aliphatic alcohol (component (B)) having 1 or more carbon atoms and a molecular weight of 30 or more and 120 or less, an alkali component, and water, wherein the pH of the stripper is 13.0 or more and less than 14.0, the content of component (A) is 0.1 mass% or more and 5 mass% or less relative to the total mass of the stripper, the content of component (B) is 5 mass% or more and 40 mass% or less, the content of the alkali component is 1 mass% or more and 5 mass% or less, and the content of water is 50 mass% or more and 90 mass% or less. (In Equation (1), R 1 A is a branched alkyl group having 6 to 10 carbon atoms, 1 O represents an oxyalkylene group having 2 to 3 carbon atoms, and a, the average added mole of the oxyalkylene group, is a number between 2 and 15. Claim 2 A stripper for a resin film for a circuit board according to claim 1, further containing a rust inhibitor (component (C)), wherein the content of the component (C) relative to the total mass of the stripper is 0.5 mass% or more and 2 mass% or less. Claim 3 In paragraph 2, the above rust inhibitor is a stripper for a resin film for a circuit board, which is a compound represented by formula (2). (In Equation (2), R 2 represents a hydrogen atom, a methyl group, or a carboxyl group. Claim 4 A method for manufacturing a circuit board, comprising: a process of preparing a circuit board having a resin film formed on at least one surface, and a process of contacting a release agent described in any one of claims 1 to 3 with said resin film.

Citation Information

Patent Citations

  • Photoresist remover and method for treatment of board using same

    JP2006085017A

  • Coating film peeling agent

    JP2017057369A

  • Resist stripping liquid and resist stripping method

    JP2018087958A

  • Polymer-stripping composition

    KR1020070019604A

  • Cleaning composition

    KR1020180029080A