Adhesive film for metal terminal, method for producing adhesive film for metal terminal, metal terminal with adhesive film for metal terminal attached thereto, power storage device using said adhesive film for metal terminal, and method for producing power storage device
The laminate adhesive film with specific polyolefin layers addresses the adhesion and conformability issues in capacitor devices, ensuring improved sealing and preventing electrolyte leakage by optimizing the Martens hardness and indentation modulus.
Patent Information
- Application Number
- KR1020257014812
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-08
- Filing Date
- 2020-11-09
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2040-11-09
AI Technical Summary
Conventional adhesive films for metal terminals in capacitor devices suffer from inadequate adhesion and conformability, leading to potential electrolyte leakage and reduced sealing performance due to the dissimilar materials involved.
An adhesive film composed of a laminate structure with a first polyolefin layer on the metal terminal side and a second polyolefin layer on the outer casing side, with specific Martens hardness and indentation modulus conditions, ensuring excellent adhesion and conformability to the metal terminal.
The adhesive film provides enhanced adhesion and conformability to the metal terminal, improving sealing performance and preventing electrolyte leakage, thereby enhancing the reliability of capacitor devices.
Smart Images

Figure 112025050186821-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to an adhesive film for a metal terminal, a method for manufacturing an adhesive film for a metal terminal, a metal terminal with an adhesive film attached thereto, a capacitor using an adhesive film for a metal terminal, and a method for manufacturing a capacitor. Background Technology
[0002] Although various types of capacitor devices have been developed, capacitor casings are indispensable components for encapsulating capacitor elements such as electrodes and electrolytes in all of them. Traditionally, metal capacitor casings have been widely used; however, with the recent increase in performance of electric vehicles, hybrid electric vehicles, PCs, cameras, and mobile phones, capacitors are required to have diverse shapes, as well as thinness and weight reduction. Conversely, conventional metal capacitor casings have drawbacks, such as difficulty in keeping up with the diversification of shapes and limitations in weight reduction.
[0003] Accordingly, a laminated sheet comprising a substrate layer, an adhesive layer, a barrier layer, and a heat-fusible resin layer sequentially laminated has recently been proposed as an outer casing for capacitor devices that is easy to process into various shapes and enables thinning and weight reduction. When using such a film-type outer casing for capacitor devices, the capacitor device element is encapsulated by the outer casing by heat-sealing the periphery of the outer casing with the heat-fusible resin layers located at the innermost layer facing each other.
[0004] A metal terminal protrudes from the heat-sealed portion of the casing for the capacitor device, and the capacitor device element enclosed by the casing is electrically connected to the outside by the metal terminal, which is electrically connected to the electrode of the capacitor device element. That is, among the heat-sealed portions of the casing for the capacitor device, the portion where the metal terminal is present is heat-sealed in a state where the metal terminal is clamped in a heat-fusible resin layer. Since the metal terminal and the heat-fusible resin layer are composed of dissimilar materials, adhesion at the interface between the metal terminal and the heat-fusible resin layer is prone to deterioration.
[0005] For this reason, an adhesive film may be placed between the metal terminal and the heat-fusible resin layer for purposes such as increasing their adhesion. An example of such an adhesive film is the one described in Patent Document 1. Prior art literature
[0006] Japanese Patent Publication No. 2015-79638 The problem to be solved
[0007] As mentioned above, the adhesive film disposed between the heat-fusible resin layer and the metal terminal of the outer casing for the capacitor device requires adhesion to the heat-fusible resin layer and the metal terminal through heat sealing.
[0008] In addition, if a gap is formed between the adhesive film and the metal terminal, the electrolyte, which is the content of the capacitor device, leaks out of the capacitor device. Therefore, the adhesive film is also required to have excellent conformability, such that the adhesive film follows the shape of the metal terminal through heat sealing to the metal terminal, and no gap is formed between the adhesive film and the metal terminal.
[0009] However, conventional adhesive films are not necessarily sufficient for achieving the same balance of adhesion and followability, and the inventors of the present disclosure have sought further improvement of adhesion and followability.
[0010] Under such circumstances, the present disclosure aims primarily to provide an adhesive film for a metal terminal having excellent adhesion to the metal terminal and also excellent following properties. Furthermore, the present disclosure also aims to provide a method for manufacturing the adhesive film for the metal terminal, a metal terminal attached with the adhesive film for the metal terminal using the adhesive film for the metal terminal, a capacitor device using the adhesive film for the metal terminal, and a method for manufacturing the capacitor device. means of solving the problem
[0011] The inventors of the present disclosure have conducted diligent investigations to solve the above-mentioned problem. As a result, they discovered that an adhesive film for a metal terminal, comprising a laminate having a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer casing side for a capacitor device in this order, can exhibit excellent adhesion and followability to the metal terminal through heat sealing to the metal terminal by setting the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer under a predetermined measurement condition to a value or less. The present disclosure was completed by conducting further investigations based on this finding.
[0012] That is, the present disclosure provides the invention of the sun exemplified below.
[0013] An adhesive film for a metal terminal interposed between a metal terminal electrically connected to an electrode of a capacitor device element and an outer casing for a capacitor device that encapsulates the capacitor device element, wherein
[0014] The adhesive film for the metal terminal above is composed of a laminate having, in this order, a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer casing side for the capacitor device.
[0015] Under the following measurement conditions, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 30 N / mm 2 Adhesive film for metal terminals.
[0016] <Measurement Conditions for Martens Hardness>
[0017] The load is 10 mN.
[0018] And, the load is the test load, and it is also the maximum load.
[0019] The load application speed is 1 mN / 10 seconds.
[0020] The duration is 10 seconds.
[0021] The unloading speed is 1 mN / 10 seconds.
[0022] The indenter is a Vickers indenter with a face angle of 136° at the tip of a square pyramid.
[0023] The measured temperature is 25℃.
[0024] The measurement value is the average of a total of 8 measurements, excluding 1 maximum value and 1 minimum value, taken 10 times by changing the measurement location. Effects of the invention
[0025] According to the present disclosure, an adhesive film for a metal terminal can be provided having excellent adhesion to the metal terminal and also excellent following properties. Furthermore, the present disclosure also aims to provide a method for manufacturing the adhesive film for the metal terminal, a metal terminal attached with the adhesive film for the metal terminal using the adhesive film for the metal terminal, a capacitor device using the adhesive film for the metal terminal, and a method for manufacturing the capacitor device. Brief explanation of the drawing
[0026] FIG. 1 is a schematic plan view of a capacitor device of the present disclosure. Figure 2 is a schematic cross-sectional view along line A-A' of Figure 1. Figure 3 is a schematic cross-sectional view along line B-B' of Figure 1. FIG. 4 is a schematic cross-sectional view of an adhesive film for metal terminals according to the present disclosure. FIG. 5 is a schematic cross-sectional view of an adhesive film for metal terminals according to the present disclosure. FIG. 6 is a schematic cross-sectional view of an outer casing for a capacitor device according to the present disclosure. FIG. 7 is a schematic cross-sectional view of an adhesive film / metal terminal / adhesive film laminate (metal terminal with adhesive film attached for metal terminal) obtained by clamping a metal terminal between two adhesive films and heat-fusing them in an embodiment. Figure 8 shows the Martens hardness, indentation modulus, and indentation depth h max This is an image of a graph showing the relationship between the indentation depth (㎛) and the load (mN) obtained by measurement. FIG. 9 is a schematic diagram illustrating a method for measuring martens hardness by pressing an indenter perpendicularly into a cross-section of the first polyolefin layer in the thickness direction of an adhesive film for metal terminals. Specific details for implementing the invention
[0027] The adhesive film for a metal terminal of the present disclosure is an adhesive film for a metal terminal interposed between a metal terminal electrically connected to an electrode of a capacitor device element and an outer casing for a capacitor device that encapsulates the capacitor device element, wherein the adhesive film for the metal terminal is composed of a laminate having, in this order, a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer casing for a capacitor device side.
[0028] Under the following measurement conditions, the Martens hardness measured in the direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 30 N / mm 2 It is characterized by the following.
[0029] <Measurement Conditions for Martens Hardness>
[0030] The load is 10 mN.
[0031] The load application speed is 1 mN / 10 seconds.
[0032] The duration is 10 seconds.
[0033] The unloading speed is 1 mN / 10 seconds.
[0034] The indenter is a Vickers indenter with a face angle of 136° at the tip of a square pyramid.
[0035] The measured temperature is 25℃.
[0036] The measurement value is the average of a total of 8 measurements, excluding 1 maximum value and 1 minimum value, taken 10 times by changing the measurement location.
[0037] As shown in the schematic diagram of FIG. 9, the Martens hardness is measured by pressing an indenter in the direction (x) perpendicular to the thickness direction (y) of the first polyolefin layer of the adhesive film for metal terminals (i.e., the cross-section obtained by cutting the adhesive film for metal terminals in the thickness direction) (arrow in FIG. 9).
[0038] The adhesive film for a metal terminal of the present disclosure has a first polyolefin layer disposed on the metal terminal side, wherein the martens hardness is 30 N / mm 2 Since it is set below, it exhibits excellent adhesion and excellent tracking performance to metal terminals through heat sealing.
[0039] In addition, the capacitor device of the present disclosure comprises, at least, a capacitor device element having a positive electrode, a negative electrode, and an electrolyte, an outer casing for a capacitor device encapsulating the capacitor device element, and a metal terminal electrically connected to each of the positive electrode and the negative electrode and protruding outward from the outer casing for a capacitor device, wherein an adhesive film for a metal terminal of the present disclosure is interposed between the metal terminal and the outer casing for a capacitor device. Hereinafter, the adhesive film for a metal terminal of the present disclosure and a method for manufacturing the same, and a capacitor device using the adhesive film for a metal terminal and a method for manufacturing the same will be described in detail.
[0040] Also, regarding numerical ranges in this specification, a numerical range indicated by “∼” means “greater than or equal to” or “less than or equal to”. For example, the notation 2 to 15 mm means 2 mm or more and 15 mm or less.
[0041] In addition, as a method for confirming the MD of an adhesive film for metal terminals, there is a method of confirming the island structure by observing a cross-section of the adhesive film for metal terminals (e.g., a cross-section of a first polyolefin layer, a substrate, or a second polyolefin layer) with an electron microscope. In the above method, the direction parallel to the cross-section where the average diameter of the island shape in the direction perpendicular to the thickness direction of the adhesive film for metal terminals is maximum can be determined as the MD. Specifically, the island structure is confirmed by observing each cross-section (a total of 10 cross-sections)—which changes the angle by 10 degrees from the direction parallel to the longitudinal cross-section and extends to the direction perpendicular to the longitudinal cross-section—with electron microscope images. Next, the shape of each drawing is observed for each cross-section. For each shape of the drawing, the straight-line distance connecting the leftmost end in the direction perpendicular to the thickness direction of the adhesive film for metal terminals and the rightmost end in the said vertical direction is defined as the diameter (y). For each cross-section, the average of the top 20 diameters (y) of the island shape is calculated in order of largest to smallest. The direction parallel to the cross-section with the largest average diameter (y) of the island shape is determined to be MD.
[0042] 1. Adhesive film for metal terminals
[0043] The adhesive film for metal terminals of the present disclosure is interposed between a metal terminal electrically connected to an electrode of a capacitor device element and an outer casing for a capacitor device that encapsulates the capacitor device element. Specifically, for example, as shown in FIGS. 1 to 3, the adhesive film (1) for metal terminals of the present disclosure is interposed between a metal terminal (2) electrically connected to an electrode of a capacitor device element (4) and an outer casing for a capacitor device (3) that encapsulates the capacitor device element (4). In addition, the metal terminal (2) protrudes outward from the outer casing for a capacitor device (3) and is clamped to the outer casing for a capacitor device (3) through the adhesive film (1) for metal terminals at the periphery (3a) of the heat-sealed outer casing for a capacitor device (3). In addition, in the present disclosure, the heating temperature when heat-sealing the outer casing for a capacitor device is typically in the range of 160 to 190°C, and the pressure is typically in the range of 1.0 to 2.0 MPa. In the process of bonding the metal terminal and the outer casing for a capacitor device through an adhesive film, it is common to perform multiple heating and pressurizing steps, such as a temporary bonding process to the metal terminal and a main bonding process. The temporary bonding process is a process of temporarily fixing the adhesive film to the metal terminal or removing bubbles, and the main bonding process is a process of bonding the adhesive film to the metal terminal by performing one or multiple heating and pressurizing steps under higher temperature conditions than the temporary bonding process. The process of pre-adhering the adhesive film for metal terminals to the metal terminals is carried out, for example, under conditions of a temperature of about 140 to 160°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a frequency of about 3 to 6 times, and the process of main adhesion is carried out, for example, under conditions of a temperature of about 160 to 240°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a frequency of about 1 to 3 times.
[0044] The adhesive film (1) for the metal terminal of the present disclosure is installed to increase the adhesion between the metal terminal (2) and the outer casing (3) for the capacitor device. By increasing the adhesion between the metal terminal (2) and the outer casing (3) for the capacitor device, the sealing performance of the capacitor device element (4) is improved. As described above, when heat-sealing the capacitor device element (4), the metal terminal (2), which is electrically connected to the electrode of the capacitor device element (4), is made to protrude to the outside of the outer casing (3) for the capacitor device, thereby encapsulating the capacitor device element. At this time, since the metal terminal (2) formed by metal and the heat-fusible resin layer (35) (a layer formed by a heat-fusible resin such as polyolefin) located in the innermost layer of the outer casing (3) for the capacitor device are formed by different materials, if such an adhesive film is not used, the sealing performance of the capacitor device element is likely to be lowered at the interface between the metal terminal (2) and the heat-fusible resin layer (35).
[0045] As shown in FIGS. 4 and 5, the adhesive film (1) for a metal terminal of the present disclosure comprises a configuration in which at least a first polyolefin layer (12a), a substrate (11), and a second polyolefin layer (12b) are laminated in this order. The first polyolefin layer (12a) is disposed on the metal terminal side. Additionally, the second polyolefin layer (12b) is disposed on the outer casing (3) side for a capacitor device. In the adhesive film (1) for a metal terminal of the present disclosure, the first polyolefin layer (12a) and the second polyolefin layer (12b) are respectively located on the surfaces of both sides.
[0046] In the adhesive film (1) for metal terminals of the present disclosure, the first polyolefin layer (12a) and the second polyolefin layer (12b) are each layers comprising a polyolefin-based resin. Examples of polyolefin-based resins include polyolefins and acid-modified polyolefins. The first polyolefin layer (12a) preferably comprises an acid-modified polyolefin among polyolefin-based resins, and more preferably is a layer formed by an acid-modified polyolefin. Furthermore, the second polyolefin layer (12b) preferably comprises a polyolefin or an acid-modified polyolefin among polyolefin-based resins, more preferably is a polyolefin, and even more preferably is a layer formed by a polyolefin. The resin forming the second polyolefin layer (12b) disposed on the side of the outer material (3) for the energy storage device is the same resin as the resin forming the heat-fusible resin layer (35) of the outer material (3) for the energy storage device, thereby increasing the adhesion between the adhesive film (1) for the metal terminal of the present disclosure and the outer material for the energy storage device.
[0047] In addition, the substrate (11) preferably comprises a polyolefin resin, preferably comprises a polyolefin, and more preferably is a layer formed by a polyolefin.
[0048] In the first polyolefin layer (12a), the second polyolefin layer (12b), and the substrate (11), the polyolefin resin is preferably a polypropylene resin, the polyolefin is preferably polypropylene, and the acid-modified polyolefin is preferably acid-modified polypropylene. In addition, the polyolefin resins, such as the polyolefin and acid-modified polyolefin, may contain known additives, fillers, pigments, etc., described later.
[0049] Specific examples of preferred laminated configurations of the adhesive film (1) for metal terminals of the present disclosure include a three-layer configuration in which a first polyolefin layer formed by acid-modified polypropylene, a substrate formed by polypropylene, and a second polyolefin layer formed by polypropylene are laminated in this order; and a three-layer configuration in which a first polyolefin layer formed by acid-modified polypropylene, a substrate formed by polypropylene, and a second polyolefin layer formed by acid-modified polypropylene are laminated in this order. Among these, a three-layer configuration in which a first polyolefin layer formed by acid-modified polypropylene, a substrate formed by polypropylene, and a second polyolefin layer formed by polypropylene are laminated in this order is particularly preferred.
[0050] Details regarding the materials constituting the first polyolefin layer (12a), the second polyolefin layer (12b), and the substrate (11) will be described later.
[0051] When the adhesive film (1) for a metal terminal of the present disclosure is placed between the metal terminal (2) of the capacitor device (10) and the outer casing (3) for the capacitor device, the surface of the metal terminal (2) made of metal and the heat-fusible resin layer (35) (a layer formed by a heat-fusible resin such as polyolefin) of the outer casing (3) for the capacitor device are bonded through the adhesive film (1) for the metal terminal. The first polyolefin layer (12a) of the adhesive film (1) for the metal terminal is placed on the side of the metal terminal (2), and the second polyolefin layer (12b) is placed on the side of the outer casing (3) for the capacitor device, and the first polyolefin layer (12a) is in close contact with the metal terminal (2), and the second polyolefin layer (12b) is in close contact with the heat-fusible resin layer (35) of the outer casing (3) for the capacitor device.
[0052] In the adhesive film (1) for metal terminals of the present disclosure, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer (12a) is 30 N / mm 2The following describes the adhesive film (1) for a metal terminal of the present disclosure. Since the first polyolefin layer (12a) disposed on the side of the metal terminal (2) has high flexibility, it is possible to exhibit excellent adhesion and conformability to the metal terminal (2). Although a limited interpretation is not desired, it is believed that excellent adhesion and conformability to the metal terminal (2) are exhibited because the first polyolefin layer (12a) has high flexibility, so the first polyolefin layer (12a) is easily embedded in the gap formed between the metal terminal and the outer casing for the capacitor device, and also because the first polyolefin layer (12a) is easily bent in the thickness direction of the metal terminal. The measurement conditions for the Martens hardness are as follows. Then, as a pretreatment of the sample to be measured, the adhesive film for the metal terminal is cut to MD 30 mm and TD 15 mm. Next, the sample is embedded in epoxy cold-filled resin and dried for about 1 day. Then, using a Tegrapol-35 mechanical polishing device manufactured by Marumoto Struers, the cross-section obtained by cutting in the TD direction is polished, and the cross-section of the sample is made to a surface roughness of about 1.0 μm. The Martens hardness is measured by the indentation method. The measurement by the indentation method can be performed, for example, using a picodenter HM-500 manufactured by Fischer Instruments.
[0053] <Measurement Conditions for Martens Hardness>
[0054] The load is 10 mN.
[0055] The load application speed is 1 mN / 10 seconds.
[0056] The duration is 10 seconds.
[0057] The unloading speed is 1 mN / 10 seconds.
[0058] The indenter is a Vickers indenter with a face angle of 136° at the tip of a square pyramid.
[0059] The measured temperature is 25℃.
[0060] The measurement value is the average of a total of 8 measurements, excluding 1 maximum value and 1 minimum value, taken 10 times by changing the measurement location.
[0061] The Martens hardness of the first polyolefin layer (12a) is 30 N / mm 2 It may be less than or equal to, but in terms of further preferably exhibiting excellent adhesion and excellent tracking ability to the metal terminal (2), it is preferably about 25 N / mm 2 Below, more preferably about 20 N / mm 2 Below, more preferably about 15 N / mm 2 Below, particularly preferably about 12 N / mm 2 The following applies. Additionally, the Martens hardness of the first polyolefin layer (12a) is preferably about 3 N / mm 2 Ideally, about 5 N / mm 2 Ideally, about 8 N / mm 2 That is all. A preferred range for the Martens hardness of the first polyolefin layer (12a) is 3 to 30 N / mm 2 Approximately 3–25 N / mm 2 Approximately 3–20 N / mm 2 Approximately 3–15 N / mm 2 Approximately 3–12 N / mm 2 Approximately 5–30 N / mm 2 Approximately 5–25 N / mm 2 Approximately 5–20 N / mm 2 Approximately 5–15 N / mm 2 Approximately 5–12 N / mm 2 Approximately 8–30 N / mm 2 Approximately 8–25 N / mm 2 Approximately 8–20 N / mm 2 Approximately 8–15 N / mm 2 Approximately 8–12 N / mm 2 Degrees can be cited as an example.
[0062] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), the indentation modulus measured perpendicularly to the cross-section in the thickness direction of the first polyolefin layer (12a) under the measurement conditions of the Martens hardness is preferably about 400 MPa or less, more preferably about 350 MPa or less, even more preferably about 300 MPa or less, even more preferably about 250 MPa or less, and particularly preferably about 200 MPa or less. In addition, the indentation modulus of the first polyolefin layer (12a) is preferably about 100 MPa or more, more preferably about 120 MPa or more, and even more preferably about 150 MPa or more. Preferred ranges for the indentation elasticity of the first polyolefin layer (12a) include approximately 100 to 400 MPa, approximately 100 to 350 MPa, approximately 100 to 300 MPa, approximately 100 to 250 MPa, approximately 100 to 200 MPa, approximately 120 to 400 MPa, approximately 120 to 350 MPa, approximately 120 to 300 MPa, approximately 120 to 250 MPa, approximately 120 to 200 MPa, approximately 150 to 400 MPa, approximately 150 to 350 MPa, approximately 150 to 300 MPa, approximately 150 to 250 MPa, and approximately 150 to 200 MPa.
[0063] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), in the measurement conditions of the Martens hardness, the indentation depth h at a load of 10 mN, which is measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer (12a), max The depth is preferably about 4.0 μm or more, more preferably about 4.5 μm or more, even more preferably about 4.8 μm or more, even more preferably about 5.0 μm or more, even more preferably about 5.5 μm or more, and particularly preferably about 6.0 μm or more. In addition, the indentation depth h of the first polyolefin layer (12a)max The indentation depth h of the first polyolefin layer (12a) is preferably about 10.0 μm or less, more preferably about 8.0 μm or less, and even more preferably about 7.0 μm or less. max Examples of desirable ranges include approximately 4.0 to 10.0 μm, approximately 4.0 to 8.0 μm, approximately 4.0 to 7.0 μm, approximately 4.5 to 10.0 μm, approximately 4.5 to 8.0 μm, approximately 4.5 to 7.0 μm, approximately 4.8 to 10.0 μm, approximately 4.8 to 8.0 μm, approximately 4.8 to 7.0 μm, approximately 5.0 to 10.0 μm, approximately 5.0 to 8.0 μm, approximately 5.0 to 7.0 μm, approximately 5.5 to 10.0 μm, approximately 5.5 to 8.0 μm, and approximately 5.5 to 7.0 μm.
[0064] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), regarding the measurement conditions for the Martens hardness, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the second polyolefin layer (12b) is preferably about 60 N / mm 2 Below, more preferably about 50 N / mm 2 Below, more preferably about 45 N / mm 2 The following applies. Additionally, the Martens hardness of the second polyolefin layer (12b) is preferably about 8 N / mm 2 Ideally, about 15 N / mm 2 Above, approximately 20 N / mm 2 Ideally, about 25 N / mm 2 Ideally, about 30 N / mm 2 That is all. A preferred range for the Martens hardness of the second polyolefin layer (12b) is 8 to 60 N / mm 2 Approximately 8–50 N / mm 2 Approximately 8–45 N / mm 2 Approximately 15–60 N / mm 2 Approximately 15–50 N / mm2 Approximately 15–45 N / mm 2 Approximately 20–60 N / mm 2 Approximately 20–50 N / mm 2 Approximately 20–45 N / mm 2 Approximately 25–60 N / mm 2 Approximately 25–50 N / mm 2 Approximately 25–45 N / mm 2 Approximately 30–60 N / mm 2 Approximately 30–50 N / mm 2 Approximately 30–45 N / mm 2 Degrees can be cited as an example.
[0065] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), the indentation modulus measured perpendicularly to the cross-section in the thickness direction of the second polyolefin layer (12b) under the measurement conditions of the Martens hardness is preferably about 1500 MPa or less, more preferably about 1200 MPa or less, even more preferably about 1000 MPa or less, and even more preferably about 800 MPa or less. In addition, the indentation modulus of the second polyolefin layer (12b) is preferably about 400 MPa or more, more preferably about 500 MPa or more, even more preferably about 600 MPa or more, and even more preferably about 700 MPa or more. Preferred ranges for the indentation elasticity of the second polyolefin layer (12b) include approximately 400 to 1500 MPa, approximately 400 to 1200 MPa, approximately 400 to 1000 MPa, approximately 400 to 800 MPa, approximately 500 to 1500 MPa, approximately 500 to 1200 MPa, approximately 500 to 1000 MPa, approximately 500 to 800 MPa, approximately 600 to 1500 MPa, approximately 600 to 1200 MPa, approximately 600 to 1000 MPa, approximately 600 to 800 MPa, approximately 700 to 1500 MPa, approximately 700 to 1200 MPa, approximately 700 to 1000 MPa, and approximately 700 to 800 MPa.
[0066] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), in the measurement conditions of the Martens hardness, the indentation depth h at a load of 10 mN, which is measured in a direction perpendicular to the cross-section in the thickness direction of the second polyolefin layer (12b), max The depth is preferably about 2.5 μm or more, more preferably about 2.8 μm or more, and even more preferably about 3.0 μm or more. In addition, the indentation depth h of the second polyolefin layer (12b) max The indentation depth h of the second polyolefin layer (12b) is preferably about 5.0 μm or less, more preferably about 4.5 μm or less, and even more preferably about 4.0 μm or less. max Examples of desirable ranges include approximately 2.5 to 5.0 μm, approximately 2.5 to 4.5 μm, approximately 2.5 to 4.0 μm, approximately 2.8 to 5.0 μm, approximately 2.8 to 4.5 μm, approximately 2.8 to 4.0 μm, approximately 3.0 to 5.0 μm, approximately 3.0 to 4.5 μm, and approximately 3.0 to 4.0 μm.
[0067] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), in the measurement conditions for the Martens hardness, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the substrate (11) is preferably about 60 N / mm 2 Below, more preferably about 50 N / mm 2 Below, more preferably about 45 N / mm 2 The above Martens hardness of the substrate (11) is preferably about 10 N / mm 2 Ideally, about 15 N / mm 2 Above, approximately 20 N / mm 2 Ideally, about 25 N / mm 2 Ideally, about 30 N / mm 2That is all. A preferred range for the Martens hardness of the above-mentioned material (11) is 10 to 60 N / mm 2 Approximately 10–50 N / mm 2 Approximately 10–45 N / mm 2 Approximately 15–60 N / mm 2 Approximately 15–50 N / mm 2 Approximately 15–45 N / mm 2 Approximately 20–60 N / mm 2 Approximately 20–50 N / mm 2 Approximately 20–45 N / mm 2 Approximately 25–60 N / mm 2 Approximately 25–50 N / mm 2 Approximately 25–45 N / mm 2 Approximately 30–60 N / mm 2 Approximately 30–50 N / mm 2 Approximately 30–45 N / mm 2 Degrees can be cited as an example.
[0068] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), the indentation modulus measured in a direction perpendicular to the cross-section in the thickness direction of the substrate (11) under the measurement conditions of the Martens hardness is preferably about 1500 MPa or less, more preferably about 1200 MPa or less, even more preferably about 1000 MPa or less, and even more preferably about 800 MPa or less. In addition, the indentation modulus of the substrate (11) is preferably about 200 MPa or more, more preferably about 300 MPa or more, even more preferably about 500 MPa or more, and even more preferably about 700 MPa or more. Preferred ranges for the indentation elasticity modulus of the above-mentioned material (11) include approximately 200 to 1500 MPa, approximately 200 to 1200 MPa, approximately 200 to 1000 MPa, approximately 200 to 800 MPa, approximately 300 to 1500 MPa, approximately 300 to 1200 MPa, approximately 300 to 1000 MPa, approximately 300 to 800 MPa, approximately 500 to 1500 MPa, approximately 500 to 1200 MPa, approximately 500 to 1000 MPa, approximately 500 to 800 MPa, approximately 700 to 1500 MPa, approximately 700 to 1200 MPa, approximately 700 to 1000 MPa, and approximately 700 to 800 MPa.
[0069] In addition, in order to further preferably exhibit excellent adhesion and excellent following properties to the metal terminal (2), in the measurement conditions of the Martens hardness, the indentation depth h at a load of 10 mN, which is measured in a direction perpendicular to the cross-section in the thickness direction of the substrate (11), max The depth is preferably about 2.5 μm or more, more preferably about 2.8 μm or more, and even more preferably about 3.0 μm or more. In addition, the indentation depth h of the substrate (11) maxThe indentation depth h of the substrate (11) is preferably about 5.0 μm or less, more preferably about 4.5 μm or less, and even more preferably about 4.0 μm or less. max Examples of desirable ranges include approximately 2.5 to 5.0 μm, approximately 2.5 to 4.5 μm, approximately 2.5 to 4.0 μm, approximately 2.8 to 5.0 μm, approximately 2.8 to 4.5 μm, approximately 2.8 to 4.0 μm, approximately 3.0 to 5.0 μm, approximately 3.0 to 4.5 μm, and approximately 3.0 to 4.0 μm.
[0070] In the adhesive film (1) for metal terminals of the present disclosure, the Martens hardness, indentation modulus, and indentation depth h of the first polyolefin layer (12a), the second polyolefin layer (12b), and the substrate (11). max Each can be adjusted by the composition, framework, dispersibility, molecular weight, melting point, MFR of the resin constituting each layer, as well as conditions such as the T-die and inflation in the manufacture of the adhesive film (1) for metal terminals (e.g., extrusion width from the T-die, stretching ratio, stretching speed, heat treatment temperature, etc.). For example, the Martens hardness, indentation modulus, and indentation depth h of the first polyolefin layer of the adhesive film for metal terminals. max As a method for adjusting the composition of the first polyolefin layer (12a) to improve flexibility, examples include adding a predetermined amount of butene component, ethylene-propylene-butene copolymer, amorphous ethylene-propylene copolymer, propylene-α-olefin copolymer, etc.
[0071] The total thickness of the adhesive film (1) for a metal terminal according to the present disclosure is, for example, about 60 μm or more, preferably about 80 μm or more, preferably about 100 μm or more, more preferably about 120 μm or more, and even more preferably about 150 μm or more, in order to increase conformability to the shape of the metal terminal (2). In addition, the total thickness of the adhesive film (1) for a metal terminal according to the present disclosure is preferably about 200 μm or less, more preferably 180 μm or less. Preferred ranges for the total thickness of the adhesive film (1) for metal terminals of the present disclosure include approximately 60 to 200 μm, approximately 60 to 180 μm, approximately 80 to 200 μm, approximately 80 to 180 μm, approximately 100 to 200 μm, approximately 100 to 180 μm, approximately 120 to 200 μm, approximately 120 to 180 μm, approximately 150 to 200 μm, and approximately 150 to 180 μm. As a more specific example, for instance, when the adhesive film (1) for metal terminals of the present disclosure is used in a consumer energy storage device, it is preferable that the total thickness be approximately 60 to 100 μm, and when it is used in a vehicle-mounted energy storage device, it is preferable that the total thickness be approximately 100 to 200 μm.
[0072] Hereinafter, the first polyolefin layer (12a), the second polyolefin layer (12b), and the substrate (11) will be described in detail.
[0073] [First polyolefin layer (12a) and second polyolefin layer (12b)]
[0074] As shown in FIGS. 4 and 5, the adhesive film (1) for a metal terminal of the present disclosure has a first polyolefin layer (12a) on one side of a substrate (11) and a second polyolefin layer (12b) on the other side. The first polyolefin layer (12a) is positioned on the metal terminal (2) side. Additionally, the second polyolefin layer (12b) is positioned on the outer casing (3) side for a capacitor device. In the adhesive film (1) for a metal terminal of the present disclosure, the first polyolefin layer (12a) and the second polyolefin layer (12b) are positioned on the surfaces of both sides, respectively.
[0075] In the adhesive film (1) for metal terminals of the present disclosure, the first polyolefin layer (12a) and the second polyolefin layer (12b) are each layers comprising a polyolefin-based resin. Examples of polyolefin-based resins include polyolefins and acid-modified polyolefins. The first polyolefin layer (12a) preferably comprises an acid-modified polyolefin among polyolefin-based resins, and is more preferably a layer formed by an acid-modified polyolefin. Furthermore, the second polyolefin layer (12b) preferably comprises a polyolefin or an acid-modified polyolefin among polyolefin-based resins, is more preferably a polyolefin, and is even more preferably a layer formed by a polyolefin. Acid-modified polyolefins have high affinity for metals. Additionally, polyolefins have high affinity for heat-fusible resins such as polyolefins. Accordingly, in the adhesive film (1) for a metal terminal of the present disclosure, by placing a first polyolefin layer (12a) formed by an acid-modified polyolefin on the side of the metal terminal (2), further excellent adhesion can be achieved at the interface between the adhesive film (1) for the metal terminal and the metal terminal (2). Additionally, by placing a second polyolefin layer (12b) formed by a polyolefin on the side of the heat-sealable resin layer (35) of the outer material (3) for the capacitor device, further excellent adhesion can be achieved at the interface between the adhesive film (1) for the metal terminal and the heat-sealable resin layer (35).
[0076] Specific examples of preferred laminated configurations of the adhesive film (1) for metal terminals of the present disclosure include a three-layer configuration in which a first polyolefin layer formed by acid-modified polypropylene, a substrate formed by polypropylene, and a second polyolefin layer formed by polypropylene are laminated in this order; and a three-layer configuration in which a first polyolefin layer formed by acid-modified polypropylene, a substrate formed by polypropylene, and a second polyolefin layer formed by acid-modified polypropylene are laminated in this order. Among these, a three-layer configuration in which a first polyolefin layer formed by acid-modified polypropylene, a substrate formed by polypropylene, and a second polyolefin layer formed by polypropylene are laminated in this order is particularly preferred.
[0077] As for the acid-modified polyolefin, there are no particular limitations as long as it is an acid-modified polyolefin, but preferably, examples include polyolefins graft-modified with an unsaturated carboxylic acid or its anhydride.
[0078] Examples of polyolefins that undergo acid modification include, specifically, polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); and terpolymers of ethylene-butene-propylene. Among these polyolefins, polyethylene and polypropylene are preferably examples, and particularly preferably polypropylene.
[0079] In addition, the acid-modified polyolefin may also be a cyclic polyolefin. For example, a carboxylic acid-modified cyclic polyolefin is a polymer obtained by copolymerizing a portion of the monomers constituting the cyclic polyolefin with an α,β-unsaturated carboxylic acid or its anhydride, or by block polymerization or graft polymerization of an α,β-unsaturated carboxylic acid or its anhydride with respect to the cyclic polyolefin.
[0080] Acid-modified cyclic polyolefins are copolymers of olefins and cyclic monomers, and examples of olefins that are constituent monomers of the cyclic polyolefins include ethylene, propylene, 4-methyl-1-pentene, butadiene, isoprene, etc. In addition, examples of cyclic monomers that are constituent monomers of the cyclic polyolefins include cyclic alkenes such as norbornene; specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornene. Among these polyolefins, cyclic alkenes, more preferably norbornene, can be cited as examples. Styrene can also be cited as an example of a constituent monomer.
[0081] Examples of carboxylic acids or their anhydrides used for acid modification include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, etc. When the first polyolefin layer (12a) is analyzed by infrared spectroscopy, it is preferable that a peak originating from maleic anhydride is detected. For example, when the maleic anhydride modified polyolefin is measured by infrared spectroscopy, the wavenumber is 1760 cm⁻¹ -1 Nearby and Watchtower 1780cm -1 A peak derived from maleic anhydride is detected in the vicinity. When the first polyolefin layer (12a) or the second polyolefin layer (12b) is a layer composed of maleic anhydride-modified polyolefin, a peak derived from maleic anhydride is detected when measured by infrared spectroscopy. However, if the degree of acid modification is low, the peak may become small and not be detected. In that case, analysis is possible using nuclear magnetic resonance spectroscopy.
[0082] The first polyolefin layer (12a) and the second polyolefin layer (12b) may each be formed by a single resin component alone, or by a blend polymer combining two or more resin components. Additionally, the first polyolefin layer (12a) and the second polyolefin layer (12b) may each be formed as a single layer, or by two or more layers formed by the same or different resin components. From the perspective of the film-forming properties of the first polyolefin layer (12a) and the second polyolefin layer (12b), it is preferable that these layers each be formed by a blend polymer combining two or more resin components. When using a blend polymer, for the first polyolefin layer (12a), it is preferable to use acid-modified polypropylene as the main component (component of 50 mass% or more) and 50 mass% or less as another resin (preferably polyethylene from the perspective of improving flexibility). In addition, for the second polyolefin layer (12b), it is preferable to have polypropylene as the main component (component of 50 mass% or more) and 50 mass% or less as another resin (preferably polyethylene from the perspective of improving flexibility). Meanwhile, from the perspective of the electrolyte resistance of the first polyolefin layer (12a) and the second polyolefin layer (12b), it is preferable that the first polyolefin layer (12a) contains acid-modified polypropylene alone as the resin, and the second polyolefin layer (12b) contains polypropylene alone as the resin.
[0083] Additionally, the first polyolefin layer (12a) and the second polyolefin layer (12b) may each include a filler as needed. Since the first polyolefin layer (12a) and the second polyolefin layer (12b) include a filler, the filler functions as a spacer, making it possible to effectively suppress a short circuit between the metal terminal (2) and the barrier layer (33) of the outer material (3) for the capacitor device. As for the particle size of the filler, an example range may be 0.1 to 35 μm, preferably 5.0 to 30 μm, and more preferably 10 to 25 μm. In addition, regarding the content of the filler, for every 100 parts by mass of the resin component forming the first polyolefin layer (12a) and the second polyolefin layer (12b), examples can be given of about 5 to 30 parts by mass, more preferably about 10 to 20 parts by mass.
[0084] Both inorganic and organic fillers can be used. Examples of inorganic fillers include carbon (carbon, graphite), silica, aluminum oxide, barium titanate, iron oxide, silicon carbide, zirconium oxide, zirconium silicate, magnesium oxide, titanium oxide, calcium aluminumate, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, calcium carbonate, etc. In addition, examples of organic fillers include fluoropolymer resin, phenolic resin, urea resin, epoxy resin, acrylic resin, benzoguanamine-formaldehyde condensate, melamine-formaldehyde condensate, polymethyl methacrylate crosslinker, polyethylene crosslinker, etc. Aluminum oxide, silica, fluoropolymer, acrylic resin, and benzoguanamine-formaldehyde condensate are preferred in terms of shape stability, rigidity, and resistance to contents, and among these, spherical aluminum oxide and silica are more preferred. As a method for mixing the filler into the resin components forming the first polyolefin layer (12a) and the second polyolefin layer (12b), a method of melt-blending both in advance with a Banbury mixer or the like to form a masterbatch and mixing it in a predetermined ratio, or a method of direct mixing with the resin components may be adopted.
[0085] Additionally, the first polyolefin layer (12a) and the second polyolefin layer (12b) may each include a pigment as needed. Various inorganic pigments may be used as pigments. As a specific example of a pigment, carbon (carbon, graphite) as exemplified in the filler above may be preferably exemplified. Carbon (carbon, graphite) is a material generally used inside capacitor devices and there is no concern about leaching into the electrolyte. Furthermore, a sufficient coloring effect can be obtained with an amount of additive that is large enough to prevent adhesion, and the melt viscosity of the added resin can be increased without melting by heat. In addition, it prevents the pressure portion from becoming thin during heat sealing, thereby providing excellent sealing performance between the capacitor device outer material and the metal terminal.
[0086] When pigment is added to the first polyolefin layer (12a) and the second polyolefin layer (12b), the amount added can be, for example, about 0.05 to 0.3 parts by mass, preferably about 0.1 to 0.2 parts by mass, with respect to 100 parts by mass of the resin component forming the first polyolefin layer (12a) and the second polyolefin layer (12b). By adding pigment to the first polyolefin layer (12a) and the second polyolefin layer (12b), the presence or absence of the adhesive film (1) for the metal terminal can be detected by a sensor or inspected by visual inspection. It is particularly preferable that the first polyolefin layer (12a) contains pigment. And, when adding a filler and a pigment to the first polyolefin layer (12a) and the second polyolefin layer (12b), the filler and the pigment may be added to the same first polyolefin layer (12a) and the second polyolefin layer (12b), but from the perspective of not impairing the heat fusion properties of the adhesive film (1) for metal terminals, it is preferable to add the filler and the pigment separately to the first polyolefin layer (12a) and the second polyolefin layer (12b).
[0087] The melt mass flow rate (MFR) of the first polyolefin layer (12a) and the second polyolefin layer (12b) at 230°C is preferably about 5 g / 10 min or more, more preferably about 7 g / 10 min or more, and even more preferably about 8 g / 10 min or more, in order to satisfy the aforementioned martens hardness and to further preferably exhibit excellent adhesion and excellent following ability of the adhesive film (1) for metal terminals (2). It is also preferably about 11 g / 10 min or less, and even more preferably about 10 g / 10 min or less. Examples of preferred ranges include about 5 to 11 g / 10 min, about 5 to 10 g / 10 min, about 7 to 11 g / 10 min, about 7 to 10 g / 10 min, about 8 to 11 g / 10 min, and about 8 to 10 g / 10 min. In addition, the melt mass flow rate (MFR) of the first polyolefin layer (12a) and the second polyolefin layer (12b) is a value (g / 10 min) at 230°C measured in accordance with the specifications of JIS K7210-1: 2014 (ISO 1133-1: 2011), respectively. When the first polyolefin layer (12a) is an acid-modified polyolefin layer, it is particularly desirable that the MFR value of the acid-modified polyolefin layer satisfies the above value.
[0088] In addition, the melting point of the first polyolefin layer (12a) is preferably about 120°C or higher, more preferably about 130°C or higher, in order to satisfy the aforementioned Martens hardness, etc., and to further preferably exhibit excellent adhesion and excellent following properties of the adhesive film (1) for metal terminals to the metal terminal (2), and is also preferably about 160°C or lower, more preferably about 150°C or lower, and as a preferred range, it is about 120 to 160°C, about 120 to 150°C, about 130 to 160°C, or about 130 to 150°C. In addition, the melting point of the second polyolefin layer (12b) is preferably about 120°C or higher, more preferably about 130°C or higher, in order to satisfy the aforementioned Martens hardness, etc., and to further preferably exhibit excellent adhesion and excellent following properties of the adhesive film (1) for metal terminals to the metal terminal (2), and is also preferably about 160°C or lower, more preferably about 150°C or lower, and as a preferred range, it is about 120 to 160°C, about 120 to 150°C, about 130 to 160°C, or about 130 to 150°C. The melting point is an endothermic peak measured by a differential scanning calorimeter (DSC).
[0089] The thickness of the first polyolefin layer (12a) and the second polyolefin layer (12b) is, in order to satisfy the aforementioned Martens hardness and to further preferably exhibit excellent adhesion and excellent following properties of the adhesive film (1) for metal terminals to the metal terminal (2), each preferably about 10 μm or more, more preferably about 15 μm or more, even more preferably about 20 μm or more, even more preferably about 30 μm or more, and also, for example, about 80 μm or less, preferably about 60 μm or less, more preferably about 50 μm or less. Preferred thickness ranges for the first polyolefin layer (12a) and the second polyolefin layer (12b) include, respectively, about 10 to 80 μm, about 10 to 60 μm, about 10 to 50 μm, about 15 to 80 μm, about 15 to 60 μm, about 15 to 50 μm, about 20 to 80 μm, about 20 to 60 μm, about 20 to 50 μm, about 30 to 80 μm, about 30 to 60 μm, and about 30 to 50 μm. As a more specific example, for instance, when the adhesive film (1) for metal terminals of the present disclosure is used in a consumer energy storage device, the thickness of the first polyolefin layer (12a) and the second polyolefin layer (12b) is preferably about 10 to 30 μm each, and when used in a vehicle-mounted energy storage device, the thickness is preferably about 30 to 80 μm each.
[0090] As a comparison of the thickness of the substrate (11) with respect to the total thickness of the first polyolefin layer (12a) and the second polyolefin layer (12b), in order to satisfy the aforementioned Martens hardness, etc. and to further preferably exhibit excellent adhesion and excellent following properties of the adhesive film (1) for metal terminals to the metal terminal (2), the thickness is preferably about 0.3 or more, more preferably about 0.4 or more, even more preferably 0.5 or more, and also preferably about 1.0 or less, more preferably about 0.8 or less. Examples of preferred ranges include about 0.3 to 1.0, about 0.3 to 0.8, about 0.4 to 1.0, about 0.4 to 0.8, about 0.5 to 1.0, and about 0.5 to 0.8.
[0091] In addition, the total thickness of the adhesive film (1) for the metal terminal is set to 100%, and the ratio of the total thickness of the first polyolefin layer (12a) and the second polyolefin layer (12b) is preferably about 30 to 80%, more preferably about 50 to 70%.
[0092] [Recording (11)]
[0093] In the adhesive film (1) for metal terminals, the substrate (11) is a layer that functions as a support for the adhesive film (1) for metal terminals.
[0094] The material forming the substrate (11) is not particularly limited. Examples of materials forming the substrate (11) include polyolefin resins, polyamide resins, polyester resins, epoxy resins, acrylic resins, fluoropolymers, silicone resins, phenolic resins, polyetherimide, polyimide, polycarbonates, and mixtures or copolymers thereof, and among these, polyolefin resins are particularly preferred. That is, the material forming the substrate (11) is preferably a resin containing a polyolefin backbone, such as a polyolefin or an acid-modified polyolefin. Whether the resin constituting the substrate (11) contains a polyolefin backbone can be analyzed, for example, by infrared spectroscopy, gas chromatography, mass spectrometry, etc.
[0095] As described above, the substrate (11) preferably comprises a polyolefin-based resin, preferably comprises a polyolefin, and more preferably is a layer formed by a polyolefin. Specifically, polyolefins may include polyethylene such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene; crystalline or amorphous polypropylene such as homopolypropylene, block copolymer of polypropylene (e.g., block copolymer of propylene and ethylene), or random copolymer of polypropylene (e.g., random copolymer of propylene and ethylene); or terpolymer of ethylene-butene-propylene. Among these polyolefins, polyethylene and polypropylene may be examples, and more preferably polypropylene may be examples. Furthermore, since the electrolyte resistance is excellent, the substrate (11) preferably comprises homopolypropylene, and is particularly preferably formed by homopolypropylene.
[0096] As polyamides, specifically, aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; aromatic polyamides such as hexamethylenediamine-isophthalic acid-terephthalic acid copolymer polyamides such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (where I represents isophthalic acid and T represents terephthalic acid) comprising constituent units derived from terephthalic acid and / or isophthalic acid, and polyamides such as polymethoxylylene adipamide (MXD6); and alicyclic polyamides such as polyaminomethylcyclohexyl adipamide (PACM6). In addition, examples include polyamides copolymerized with lactam components or isocyanate components such as 4,4'-diphenylmethane-diisocyanate, polyesteramide copolymers or polyetheresteramide copolymers which are copolymers of copolymerized polyamides and polyesters or polyalkylene ether glycols; and copolymers thereof. These polyamides may be used as a single type or in combination of two or more types.
[0097] Specifically, examples of polyesters include copolymer polyesters based on repeating units of polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, and ethylene terephthalate, and copolymer polyesters based on repeating units of butylene terephthalate. In addition, examples of copolymer polyesters having ethylene terephthalate as the main repeating unit include, specifically, copolymer polyesters polymerized with ethylene isophthalate having ethylene terephthalate as the main repeating unit (hereinafter abbreviated as polyethylene(terephthalate / isophthalate)), polyethylene(terephthalate / isophthalate), polyethylene(terephthalate / adipate), polyethylene(terephthalate / sodium sulfoisophthalate), polyethylene(terephthalate / sodium isophthalate), polyethylene(terephthalate / phenyl-dicarboxylate), and polyethylene(terephthalate / decanedicarboxylate). In addition, examples of copolymer polyesters based on butylene terephthalate as the repeating unit include, specifically, copolymer polyesters polymerized with butylene isophthalate based on butylene terephthalate as the repeating unit (hereinafter abbreviated as polybutylene(terephthalate / isophthalate)), polybutylene(terephthalate / adipate), polybutylene(terephthalate / sebacate), polybutylene(terephthalate / decandicarboxylate), polybutylene naphthalate, etc. These polyesters may be used individually or in combination of two or more types.
[0098] Additionally, the substrate (11) may be formed from a nonwoven fabric formed from the resin described above. When the substrate (11) is a nonwoven fabric, it is preferable that the substrate (11) be composed of the aforementioned polyolefin resin, polyamide resin, etc.
[0099] In addition, by incorporating a coloring agent into the substrate (11), the substrate (11) may be made into a layer containing a coloring agent. Additionally, light transmittance may be adjusted by selecting a resin with low transparency. If the substrate (11) is a film, a colored film or a film with low transparency may be used. In addition, if the substrate (11) is a nonwoven fabric, a nonwoven fabric using fibers or binders containing a coloring agent or a nonwoven fabric with low transparency may be used.
[0100] The melt mass flow rate (MFR) of the substrate (11) at 230°C is preferably 8 g / 10 min or less, more preferably 4 g / 10 min or less, in order to satisfy the aforementioned martens hardness, etc., and to further preferably exhibit excellent adhesion and excellent following properties of the metal terminal adhesive film (1) for metal terminals to the metal terminal (2); more preferably 1 g / 10 min or more, more preferably 2 g / 10 min or more, in order to make the metal terminal adhesive film (1) excellent in flexibility (good evaluation of following properties and adhesion properties described later); and as a preferred range, examples include about 1 to 8 g / 10 min, about 1 to 4 g / 10 min, about 2 to 8 g / 10 min, and about 2 to 4 g / 10 min. When the substrate (11) is a polyolefin layer (a layer formed by polyolefin), it is particularly preferable that the MFR value of the polyolefin layer satisfies the above value. Also, the melt mass flow rate (MFR) of the material (11) is a value (g / 10 min) at 230°C measured in accordance with the standards of JIS K7210-1: 2014 (ISO 1133-1: 2011).
[0101] In addition, the melting point of the substrate (11) is preferably 130°C or higher, more preferably 150°C or higher, in order to satisfy the aforementioned Martens hardness, etc., and to further preferably exhibit excellent adhesion and excellent following properties of the adhesive film (1) for metal terminals to the metal terminal (2), and is also preferably 190°C or lower, more preferably 170°C or lower, and as a preferred range, is approximately 130 to 190°C, approximately 130 to 170°C, approximately 150 to 190°C, and approximately 150 to 170°C. The melting point is an endothermic peak measured by a differential scanning calorimeter (DSC).
[0102] When the substrate (11) is composed of a resin film, the surface of the substrate (11) may be equipped with known easy-adhesion means, such as corona discharge treatment, ozone treatment, or plasma treatment, as needed.
[0103] The thickness of the substrate (11) is, for example, about 100 μm or less, preferably about 60 μm or less, more preferably about 55 μm or less, in order to further preferably exhibit excellent adhesion and excellent following properties of the adhesive film (1) for the metal terminal to the metal terminal (2). In addition, the thickness of the substrate (11) is preferably about 20 μm or more, more preferably about 30 μm or more, and even more preferably about 40 μm or more. Examples of preferred ranges for the thickness of the substrate (11) include about 20 to 100 μm, about 20 to 60 μm, about 20 to 55 μm, about 30 to 100 μm, about 30 to 60 μm, about 30 to 55 μm, about 40 to 100 μm, about 40 to 60 μm, and about 40 to 55 μm. As a more specific example, for instance, when the adhesive film (1) for metal terminals of the present disclosure is used in a consumer energy storage device, the thickness of the substrate (11) is preferably about 30 to 55 μm, and when used in a vehicle-mounted energy storage device, it is preferably about 40 to 100 μm.
[0104] [Adhesion promoter layer (13)]
[0105] The adhesion promoter layer (13) is a layer installed as needed for the purpose of firmly bonding the substrate (11) and the first polyolefin layer (12a) and the second polyolefin layer (12b) (see FIG. 5). The adhesion promoter layer (13) may be installed only on one side between the substrate (11) and the first polyolefin layer (12a) and the second polyolefin layer (12b), or it may be installed on both sides.
[0106] The adhesion promoter layer (13) can be formed using known adhesion promoters such as isocyanate-based, polyethyleneimine-based, polyester-based, polyurethane-based, and polybutadiene-based materials. From the perspective of further improving resistance to electrolytes, it is preferable that it be formed using an isocyanate-based adhesion promoter. As for the isocyanate-based adhesion promoter, it is composed of an isocyanate component selected from triisocyanate monomers and polymeric MDI, which provides excellent laminate strength and also causes less decrease in laminate strength after immersion in the electrolyte. In particular, it is especially preferable to form it using an adhesion promoter composed of a triisocyanate monomer, such as triphenylmethane-4,4',4"-triisocyanate, or a polymeric MDI, such as polymethylenepolyphenylpolyisocyanate (NCO content of about 30%, viscosity of 200 to 700 mPa·s). In addition, it is also preferable to form it using a two-component curing type adhesion promoter composed of a triisocyanate monomer, such as tris(p-isocyanatephenyl)thiophosphate, or a polyethyleneimine-based base and polycarbodiimide as a crosslinking agent.
[0107] The adhesion promoter layer (13) can be formed by applying and drying using known coating methods such as bar coating, roll coating, or gravure coating. As for the amount of adhesion promoter applied, in the case of an adhesion promoter composed of triisocyanate, 20 to 100 mg / m² 2Approximately, preferably 40 to 60 mg / m² 2 It is approximately that amount, and in the case of adhesion promoters composed of polymeric MDI, 40–150 mg / m² 2 Approximately, preferably 60 to 100 mg / m² 2 It is approximately, and in the case of a two-component curing type adhesion promoter based on a polyethyleneimine-based material and polycarbodiimide as a crosslinking agent, 5 to 50 mg / m² 2 The amount, preferably 10 to 30 mg / m² 2 It is to that extent. Also, the triisocyanate monomer is a monomer having three isocyanate groups in one molecule, and the polymeric MDI is a mixture of MDI and an MDI oligomer polymerized from MDI, and is represented by the following formula.
[0108]
[0109] The adhesive film (1) for metal terminals of the present disclosure can be manufactured, for example, by laminating a first polyolefin layer (12a) and a second polyolefin layer (12b) respectively on both surfaces of a substrate (11). The lamination of the substrate (11) and the first polyolefin layer (12a) and the second polyolefin layer (12b) can be performed by known methods such as extrusion lamination, T-die lamination, inflation lamination, and thermal lamination. In addition, when laminating the substrate (11), the first polyolefin layer (12a), and the second polyolefin layer (12b) through the adhesion promoter layer (13), for example, the adhesion promoter constituting the adhesion promoter layer (13) is applied and dried on the substrate (11) in the manner described above, and the first polyolefin layer (12a) and the second polyolefin layer (12b) are laminated respectively from the adhesion promoter layer (13).
[0110] The method of interposing the adhesive film (1) for the metal terminal between the metal terminal (2) and the outer casing (3) for the capacitor device is not particularly limited. For example, as shown in FIGS. 1 to 3, the adhesive film (1) for the metal terminal may be wound onto the metal terminal (2) in the portion where the metal terminal (2) is clamped by the outer casing (3) for the capacitor device. Additionally, although not shown in the illustration, the adhesive film (1) for the metal terminal may be placed on both sides of the metal terminal (2) so as to cross two metal terminals (2) in the portion where the metal terminal (2) is clamped by the outer casing (3) for the capacitor device.
[0111] [Metal terminal (2)]
[0112] The adhesive film (1) for metal terminals of the present disclosure is used by being interposed between a metal terminal (2) and an outer casing (3) for a capacitor device. The metal terminal (2) (tap) is a conductive member that is electrically connected to an electrode (positive or negative electrode) of a capacitor device element (4) and is composed of a metal material. The metal material constituting the metal terminal (2) is not particularly limited and, for example, may include aluminum, nickel, copper, etc. For example, the metal terminal (2) connected to the positive electrode of a lithium-ion capacitor device is typically composed of aluminum, etc. In addition, the metal terminal (2) connected to the negative electrode of a lithium-ion capacitor device is typically composed of copper, nickel, etc.
[0113] It is preferable that the surface of the metal terminal (2) undergoes a chemical treatment to increase its resistance to electrolytes. For example, when the metal terminal (2) is formed of aluminum, specific examples of the chemical treatment may include known methods for forming a corrosion-resistant film such as phosphates, chromates, fluorides, and triazinethiol compounds. Among the methods for forming a corrosion-resistant film, a phosphate chromate treatment using a three-component composition of phenol resin, chromium(III) fluoride, and phosphoric acid is preferred.
[0114] The size of the metal terminal (2) can be appropriately set according to the size of the capacitor device used. As for the thickness of the metal terminal (2), preferably, about 50 to 1000 μm, and more preferably, about 70 to 800 μm can be exemplified. Also, as for the length of the metal terminal (2), preferably, about 1 to 200 mm, and more preferably, about 3 to 150 mm can be exemplified. Also, as for the width of the metal terminal (2), preferably, about 1 to 200 mm, and more preferably, about 3 to 150 mm can be exemplified.
[0115] [Exterior material for capacitor device (3)]
[0116] As an example of an exterior material (3) for a storage device, it may have a laminated structure having at least a base layer (31), a barrier layer (33), and a heat-fusible resin layer (35) in this order. FIG. 6 shows an example of a cross-sectional structure of an exterior material (3) for a storage device in which a base layer (31), an adhesive layer (32) installed as needed, a barrier layer (33), an adhesive layer (34) installed as needed, and a heat-fusible resin layer (35) are laminated in this order. In the exterior material (3) for a storage device, the base layer (31) is on the outer side, and the heat-fusible resin layer (35) is on the innermost side. When assembling the capacitor device, the capacitor device element (4) is sealed by bringing the heat-fusible resin layers (35) located around the capacitor device element (4) into surface contact and heat-fusing them. In FIGS. 1 to 3, a capacitor device (10) is shown using an embossed type outer casing (3) for the capacitor device formed by embossing molding, etc., but the outer casing (3) for the capacitor device may be a pouch type that is not molded. In addition, among pouch types, there are three-way sealing, four-way sealing, pillow type, etc., but any type is acceptable.
[0117] The thickness of the laminate constituting the outer layer (3) for the energy storage device is not particularly limited, but regarding the upper limit, from the perspective of cost reduction and energy density improvement, preferably examples may be about 190 μm or less, about 180 μm or less, about 160 μm or less, about 155 μm or less, about 140 μm or less, about 130 μm or less, or about 120 μm or less; regarding the lower limit, from the perspective of maintaining the function of the outer layer (3) for the energy storage device of protecting the energy storage device element (4), preferably examples may be about 35 μm or more, about 45 μm or more, about 60 μm or more, or about 80 μm or more; regarding the preferred range, for example, about 35 to 190 μm, about 35 to 180 μm, about 35 to 160 μm, about 35 to 155 μm, about 35 to 140 μm, or 35 to 130 μm Examples include approximately 35–120 μm, approximately 45–190 μm, approximately 45–180 μm, approximately 45–160 μm, approximately 45–155 μm, approximately 45–140 μm, approximately 45–130 μm, approximately 45–120 μm, approximately 60–190 μm, approximately 60–180 μm, approximately 60–160 μm, approximately 60–155 μm, approximately 60–140 μm, approximately 60–130 μm, approximately 60–120 μm, approximately 80–190 μm, approximately 80–180 μm, approximately 80–160 μm, approximately 80–155 μm, approximately 80–140 μm, approximately 80–130 μm, and approximately 80–120 μm. It is possible.
[0118] (Insert layer (31))
[0119] In the outer casing (3) for a storage device, the substrate layer (31) is a layer that functions as a substrate for the outer casing of the storage device and is a layer that forms the outermost layer side.
[0120] The material forming the substrate layer (31) is limited to having insulating properties and is not particularly restricted. Examples of materials forming the substrate layer (31) include polyester, polyamide, epoxy, acrylic, fluoropolymer, polyurethane, silicone resin, phenol, polyetherimide, polyimide, and mixtures or copolymers thereof. Polyesters such as polyethylene terephthalate and polybutylene terephthalate have excellent resistance to electrolytes and have the advantage of not easily causing whitening when the electrolyte adheres, so they are preferably used as the material forming the substrate layer (31). In addition, polyamide film has excellent stretchability and can prevent the occurrence of whitening due to resin cracking of the substrate layer (31) during molding, so it is preferably used as the material forming the substrate layer (31).
[0121] The substrate layer (31) may be formed from a uniaxially or biaxially stretched resin film, or it may be formed from an unstretched resin film. Among these, the uniaxially or biaxially stretched resin film, particularly the biaxially stretched resin film, is preferably used as the substrate layer (31) because its heat resistance is improved by oriented crystallization.
[0122] Among these, as a resin film forming the substrate layer (31), preferably nylon, polyester, more preferably biaxially stretched nylon, biaxially stretched polyester can be cited as examples.
[0123] The substrate layer (31) may be laminated with resin films of other materials to improve pinhole resistance and insulation when used as a packaging body for a capacitor device. Specifically, examples include a multilayer structure in which a polyester film and a nylon film are laminated, or a multilayer structure in which biaxially stretched polyester and biaxially stretched nylon are laminated. When the substrate layer (31) is made into a multilayer structure, each resin film may be bonded using an adhesive, or may be laminated directly without using an adhesive. When bonding without using an adhesive, there are methods of bonding in a hot-melted state, such as co-extrusion, sand lamination, or thermal lamination.
[0124] Additionally, the substrate layer (31) may be made low-friction to improve moldability. When the substrate layer (31) is made low-friction, the coefficient of friction of its surface is not particularly limited, but for example, 1.0 or less. To make the substrate layer (31) low-friction, for example, mat treatment, formation of a thin film layer of a slip agent, or a combination thereof.
[0125] As for the thickness of the substrate layer (31), for example, about 10 to 50 μm, preferably about 15 to 30 μm can be given as an example.
[0126] (Adhesive layer (32))
[0127] In the outer material (3) for a capacitor device, the adhesive layer (32) is a layer disposed over the substrate layer (31) as needed to provide adhesion to the substrate layer (31). That is, the adhesive layer (32) is installed between the substrate layer (31) and the barrier layer (33).
[0128] The adhesive layer (32) is formed by an adhesive capable of bonding the substrate layer (31) and the barrier layer (33). The adhesive used to form the adhesive layer (32) may be a two-component curing adhesive or a one-component curing adhesive. Furthermore, the adhesive mechanism of the adhesive used to form the adhesive layer (32) is not particularly limited and may be any of the following: a chemical reaction type, a solvent volatilization type, a heat melting type, a heat pressing type, etc.
[0129] As for the resin component of the adhesive that can be used to form the adhesive layer (32), examples include a polyurethane-based two-component curing adhesive, which has excellent ductility, durability under high humidity conditions, yellowing inhibition, and heat degradation inhibition during heat sealing, and effectively inhibits delamination by inhibiting the decrease in laminate strength between the substrate layer (31) and the barrier layer (33); or a blending resin of polyamide, polyester, or modified polyolefin.
[0130] Additionally, the adhesive layer (32) may be multilayered with different adhesive components. When the adhesive layer (32) is multilayered with different adhesive components, in order to improve the laminate strength of the substrate layer (31) and the barrier layer (33), it is preferable to select a resin with excellent adhesion to the substrate layer (31) as the adhesive component disposed on the substrate layer (31) side, and to select an adhesive component with excellent adhesion to the barrier layer (33) as the adhesive component disposed on the barrier layer (33) side. When the adhesive layer (32) is multilayered with different adhesive components, specifically, as the adhesive component disposed on the barrier layer (33) side, examples may preferably include an acid-modified polyolefin, a metal-modified polyolefin, a mixed resin of polyester and acid-modified polyolefin, and a resin containing copolymerized polyester.
[0131] As for the thickness of the adhesive layer (32), for example, about 2 to 50 μm, preferably about 3 to 25 μm can be given as an example.
[0132] (Barrier layer (33))
[0133] In the outer casing for a capacitor device, the barrier layer (33) is a layer that, in addition to improving the strength of the outer casing for the capacitor device, has the function of preventing water vapor, oxygen, light, etc. from entering the capacitor device. The barrier layer (33) is preferably a metal layer, that is, a layer formed of metal. Specifically, examples of the metal constituting the barrier layer (33) include aluminum, stainless steel, titanium, etc., and preferably aluminum. The barrier layer (33) can be formed, for example, by a metal foil, a metal deposition film, an inorganic oxide deposition film, a carbon-containing inorganic oxide deposition film, or a film having these deposition films installed, and it is preferable to form it by a metal foil, and even more preferable to form it by an aluminum foil. In order to prevent wrinkles or pinholes from occurring in the barrier layer (33) when manufacturing an outer casing for a capacitor device, it is more preferable that the barrier layer be formed by a soft aluminum foil, such as annealed aluminum (JIS H4160: 1994 A8021H-O, JIS H4160: 1994 A8079H-O, JIS H4000: 2014 A8021P-O, JIS H4000: 2014 A8079P-O).
[0134] Regarding the thickness of the barrier layer (33), from the perspective of thinning the outer material for the capacitor device and allowing pinholes to easily occur even by molding, it is preferably about 10 to 200 μm, more preferably about 20 to 100 μm.
[0135] In addition, the barrier layer (33) is preferably phosphating at least one side, preferably both sides, to stabilize adhesion and prevent dissolution or corrosion. Here, phosphating refers to a treatment that forms a corrosion-resistant film on the surface of the barrier layer.
[0136] (Adhesive layer (34))
[0137] In the outer casing (3) for a storage device, the adhesive layer (34) is a layer installed between the barrier layer (33) and the heat-fusible resin layer (35) as needed to firmly bond the heat-fusible resin layer (35).
[0138] The adhesive layer (34) is formed by an adhesive capable of bonding the barrier layer (33) and the heat-fusible resin layer (35). The composition of the adhesive used to form the adhesive layer is not particularly limited, but, for example, a resin composition including an acid-modified polyolefin may be used. As for the acid-modified polyolefin, the same as those exemplified in the first polyolefin layer (12a) and the second polyolefin layer (12b) may be exemplified.
[0139] The thickness of the adhesive layer (34) is, for example, about 1 to 40 μm, preferably about 2 to 30 μm.
[0140] (Thermal fusion resin layer (35))
[0141] In the outer casing (3) for a capacitor device, the heat-fusible resin layer (35) corresponds to the innermost layer and is a layer that seals the capacitor device elements by heat-fusible resin layers together during assembly of the capacitor device.
[0142] Regarding the resin component used in the heat-fusible resin layer (35), it is limited to those that are heat-fusible and is not particularly limited, but examples include polyolefin and cyclic polyolefin.
[0143] Specifically, the above polyolefins may include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); and terpolymers of ethylene-butene-propylene. Among these polyolefins, polyethylene and polypropylene are preferably examples.
[0144] The above-mentioned cyclic polyolefin is a copolymer of an olefin and a cyclic monomer, and examples of olefins that are constituent monomers of the above-mentioned cyclic polyolefin include ethylene, propylene, 4-methyl-1-pentene, butadiene, isoprene, etc. In addition, examples of cyclic monomers that are constituent monomers of the above-mentioned cyclic polyolefin include cyclic alkenes such as norbornene; specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornene. Among these polyolefins, cyclic alkenes are preferably exemplified, and norbornene is more preferably exemplified. Styrene is also exemplified as a constituent monomer.
[0145] Among these resin components, preferably crystalline or amorphous polyolefins, cyclic polyolefins, and blend polymers thereof; more preferably polyethylene, polypropylene, copolymers of ethylene and norbornene, and blend polymers of two or more of these may be examples.
[0146] The heat-fusible resin layer (35) may be formed by a single resin component alone, or by a blend polymer combining two or more resin components. Additionally, the heat-fusible resin layer (35) may be formed as a single layer, but may also be formed as two or more layers using the same or different resin components. It is particularly desirable that the resins of the second polyolefin layer (12b) and the heat-fusible resin layer (35) are common, as this improves the adhesion between these layers.
[0147] In addition, the thickness of the heat-fusible resin layer (35) is not particularly limited, but can be 2 to 2000 μm, preferably 5 to 1000 μm, and more preferably 10 to 500 μm.
[0148] 2. Energy storage device
[0149] The energy storage device (10) of the present disclosure comprises, at least, an energy storage device element (4) having a positive electrode, a negative electrode, and an electrolyte, an outer casing (3) for the energy storage device that encloses the energy storage device element (4), and a metal terminal (2) that is electrically connected to each of the positive electrode and the negative electrode and protrudes outward from the outer casing (3) for the energy storage device. The energy storage device (10) of the present disclosure is characterized in that an adhesive film (1) for the metal terminal of the present disclosure is interposed between the metal terminal (2) and the outer casing (3) for the energy storage device. That is, the energy storage device (10) of the present disclosure can be manufactured by a method including a process in which an adhesive film (1) for the metal terminal of the present disclosure is interposed between the metal terminal (2) and the outer casing (3) for the energy storage device.
[0150] Specifically, a capacitor device element (4) having at least a positive electrode, a negative electrode, and an electrolyte is covered by interposing a metal terminal (2) connected to each of the positive electrode and the negative electrode in an outer casing (3) for a capacitor device between a metal terminal (2) and a heat-fusible resin layer (35) of the present disclosure, so as to form a flange portion (a region where the heat-fusible resin layers (35) come into contact with each other, and a periphery portion (3a)) of the outer casing for a capacitor device around the capacitor device element (4), and then heat-sealing the heat-fusible resin layers (35) of the flange portion to seal them together, thereby providing a capacitor device (10) using an outer casing (3) for a capacitor device. And, when the capacitor device element (4) is accommodated using the capacitor device outer casing (3), the heat-fusible resin layer (35) of the capacitor device outer casing (3) is used such that it becomes the inner side (the surface in contact with the capacitor device element (4)).
[0151] The casing material for a storage device disclosed in the present disclosure can preferably be used in a storage device such as a battery (including condensers, capacitors, etc.). In addition, the casing material for a storage device disclosed in the present disclosure may be used in either a primary battery or a secondary battery, but is preferably a secondary battery. The types of secondary batteries to which the casing material for a storage device disclosed in the present disclosure is applied are not particularly limited, and examples include lithium-ion batteries, lithium-ion polymer batteries, all-solid-state batteries, lead-acid batteries, nickel-hydrogen batteries, nickel-cadmium batteries, nickel-iron batteries, nickel-zinc batteries, silver oxide-zinc batteries, metal dry batteries, polyvalent cation batteries, condensers, capacitors, etc. Among these secondary batteries, lithium-ion batteries and lithium-ion polymer batteries can be cited as examples of preferred applications for the casing material for a storage device disclosed in the present disclosure.
[0152] Examples
[0153] Examples and comparative examples are presented below, and the present disclosure is described in detail. However, the present disclosure is not limited to the examples.
[0154] Manufacture of adhesive film for metal terminals
[0155] Example 1
[0156] Maleic anhydride-modified polypropylene (PPa) was prepared as the polyolefin forming the first polyolefin layer, polypropylene (PP) as the polyolefin forming the second polyolefin layer, and an unoriented polypropylene film (CPP, homopolypropylene, thickness 50 μm) as the substrate. As the material forming the first polyolefin layer, the Martens hardness, indentation modulus, and indentation depth h listed in Table 1 were prepared. max A material with particularly high flexibility, which is not used in conventional adhesive films for metal terminals, was used to provide the above. Maleic anhydride modified polypropylene (PPa) was extruded on one side of a substrate (CPP) using a T-die extruder to form a first polypropylene layer (thickness 50 μm), and polypropylene (PP) was extruded on the other side of the substrate (CPP) using a T-die extruder to form a second polypropylene layer (thickness 50 μm), and an adhesive film for metal terminals was obtained in which the first polyolefin layer (50 μm, PPa layer) / substrate (50 μm, CPP layer) / second polyolefin layer (50 μm, PP layer) were laminated in order.
[0157] Example 2
[0158] Maleic anhydride-modified polypropylene (PPa) colored black with carbon black was prepared as the polyolefin forming the first polyolefin layer, polypropylene (PP) was prepared as the polyolefin forming the second polyolefin layer, and an unoriented polypropylene film (CPP, homopolypropylene, thickness 50 μm) was prepared as the substrate. As the material forming the first polyolefin layer, the Martens hardness, indentation modulus, and indentation depth h listed in Table 1 were prepared. maxA highly flexible material, which is not used in conventional adhesive films for metal terminals, was used to provide the above. Maleic anhydride modified polypropylene (PPa), colored black with carbon black, was extruded on one side of a substrate (CPP) using a T-die extruder to form a first polypropylene layer (thickness 50 μm), and polypropylene (PP) was extruded on the other side of the substrate (CPP) using a T-die extruder to form a second polypropylene layer (thickness 50 μm), and an adhesive film for metal terminals was obtained in which the first polyolefin layer (50 μm, PPa layer) / substrate (50 μm, CPP layer) / second polyolefin layer (50 μm, PP layer) were laminated in order.
[0159] Example 3
[0160] Maleic anhydride-modified polypropylene (PPa) was prepared as the polyolefin forming the first polyolefin layer, polypropylene (PP) was prepared as the polyolefin forming the second polyolefin layer, and a polypropylene film (PP) colored black with carbon black was prepared as the substrate. As for the materials forming the first polyolefin layer and the substrate, each of these layers has the Martens hardness, indentation modulus, and indentation depth h listed in Table 1. max A highly flexible material, which is not used in conventional adhesive films for metal terminals, was used to provide the above. Polypropylene (PP) was extruded using a T-die extruder to form a substrate (thickness 30 μm), maleic anhydride modified polypropylene (PPa) was extruded using a T-die extruder on one side of the substrate (PP) to form a first polypropylene layer (thickness 50 μm), and polypropylene (PP) was extruded using a T-die extruder on the other side of the substrate (PP, thickness 30 μm) to form a second polypropylene layer (thickness 20 μm), and an adhesive film for metal terminals was obtained in which the first polyolefin layer (50 μm, PPa layer) / substrate (30 μm, PP layer) / second polyolefin layer (20 μm, PP layer) were laminated in order.
[0161] Comparative Example 1
[0162] Maleic anhydride modified polypropylene (PPa) was prepared as the polyolefin forming the first polyolefin layer, maleic anhydride modified polypropylene (PPa) was prepared as the polyolefin forming the second polyolefin layer, and polypropylene (PP, homopolypropylene) was prepared as the substrate. Using the resin of each layer, multilayer air-cooled inflation molding was performed, and an adhesive film for metal terminals was obtained in which the first polyolefin layer (50 μm, PPa layer) / substrate (50 μm, PP layer) / second polyolefin layer (50 μm, PPa layer) were laminated in order.
[0163] Comparative Example 2
[0164] Maleic anhydride modified polypropylene (PPa) was prepared as the polyolefin forming the first polyolefin layer, maleic anhydride modified polypropylene (PPa) was prepared as the polyolefin forming the second polyolefin layer, and polypropylene (PP, homopolypropylene) was prepared as the substrate. Using the resin of each layer, multilayer air-cooled inflation molding was performed, and an adhesive film for metal terminals was obtained in which the first polyolefin layer (35 μm, PPa layer) / substrate (80 μm, PP layer) / second polyolefin layer (35 μm, PPa layer) were laminated in order.
[0165] And, the Martens hardness, indentation modulus, and indentation depth h of each layer of the adhesive film for metal terminals listed in Table 1 max Each can be adjusted by the composition, framework, dispersibility, molecular weight, melting point, MFR of the resin constituting each layer, and further by conditions such as the T-die and inflation in the manufacture of the adhesive film (1) for metal terminals (e.g., extrusion width from the T-die, stretching ratio, stretching speed, heat treatment temperature, etc.). The Martens hardness, indentation modulus, and indentation depth h of the first polyolefin layer of the adhesive film for metal terminals described in Table 1. max Regarding this, flexibility was adjusted by adding butene components, ethylene-propylene-butene copolymer, amorphous ethylene-propylene copolymer, propylene-α-olefin copolymer, etc.
[0166] Martens hardness, indentation modulus, indentation depth h max Measurement of
[0167] For the first polyolefin layer, substrate, and second polyolefin layer of the adhesive film for metal terminals of the examples and comparative examples, respectively, Martens hardness, indentation modulus, and indentation depth h max ...was measured. For this measurement, as a pretreatment of the sample to be measured, an adhesive film for metal terminals was cut to an MD of 30 mm and a TD of 15 mm. Next, the sample was embedded in an epoxy cold-filled resin and dried for about one day. Afterward, using a Tegrapol-35 mechanical polishing device manufactured by Marumoto Struers, the cross-section obtained by cutting in the TD direction was polished, and the cross-section of the sample was made to a surface roughness of approximately 1.0 μm. As a measurement by the indentation method, the measurement was performed using a Picodenter HM-500 manufactured by Fisher Instruments, and the measurement was taken in a direction perpendicular to the cross-section in the thickness direction (the center part in the thickness direction) of the layer to be measured. The cross-section to be measured is the cross-section obtained by cutting the adhesive film for metal terminals in the TD direction and subjected to the above pretreatment. The measurement conditions are as follows.
[0168] (Measurement conditions)
[0169] The load is 10 mN.
[0170] The load application speed is 1 mN / 10 seconds.
[0171] The duration is 10 seconds.
[0172] The unloading speed is 1 mN / 10 seconds.
[0173] The indenter is a Vickers indenter in which the face angle of the tip of a square pyramid is 136°.
[0174] The measured temperature is 25℃.
[0175] The measurement value is the average of a total of 8 measurements, excluding 1 maximum value and 1 minimum value, taken 10 times by changing the measurement location.
[0176] And, for reference, the aforementioned Martens hardness, indentation modulus, and indentation depth h max Figure 8 shows an image of a graph representing the relationship between the indentation depth (μm) and the load (mN) obtained by measurement.
[0177] Martens hardness is calculated by the following formula.
[0178] HM (Martens Hardness) = Surface area of the indenter calculated from maximum load F (N) / indentation depth (mm²) 2 =Maximum load F(N) / 26.43h 2
[0179] F: Maximum load (N)
[0180] h: Indentation depth under test load = h max (Value of point E in Fig. 8 (the point where the perpendicular line drawn from point C to the Y-axis meets))
[0181] In addition, the indentation modulus is calculated from the slope of the tangent line of CD in Fig. 8. Also, the indentation depth h max is calculated from the value of point E in Fig. 8.
[0182] <Measurement of Adhesion Strength between Adhesive Film for Metal Terminals and Metal Terminals>
[0183] As a metal terminal, aluminum (JIS H4160: 1994 A8079H-O) with a length of 50 mm, a width of 22.5 mm, and a thickness of 200 μm was prepared. In addition, each adhesive film for the metal terminal obtained in the examples and comparative examples was cut to a length of 45 mm and a width of 15 mm. Next, the adhesive film for the metal terminal was placed on the metal terminal to obtain a laminate of the metal terminal and the adhesive film. At this time, the vertical and horizontal directions of the metal terminal were aligned with the length and width directions of the adhesive film for the metal terminal, respectively, and the centers of the metal terminal and the adhesive film for the metal terminal were aligned. Next, a tetrafluoroethylene-ethylene copolymer film (ETFE film, thickness 100 μm) was placed on the adhesive film for the metal terminal of the laminate (covering the surface of the adhesive film for the metal terminal with the ETFE film) and mounted on a hot plate heated to 190°C (with the metal terminal facing the hot plate). Additionally, a 500g weight with a sponge attached was placed on the plate and left standing for 12 seconds to heat-fuse the adhesive film to the metal terminal. After heat-fusion, the laminate was naturally cooled to 25°C. Next, in an environment of 25°C, the adhesive film for the metal terminal was peeled off from the metal terminal using a Tensilon universal testing machine (RTG-1210 manufactured by A&D). The maximum strength at the time of peeling was defined as the adhesion strength to the metal terminal (N / 15 mm). The peeling speed was set to 50 mm / min, the peeling angle to 180°, and the chuck distance to 30 mm, and the average value was obtained from three measurements. In addition, the treatment of standing for 12 seconds in a heated pressurized environment of a temperature of 190°C and a surface pressure of 0.016 MPa is a treatment simulating the heat and pressure applied in the aforementioned temporary bonding and main bonding processes. The results are shown in Table 1.
[0184] <Followability Evaluation (Adhesive Film / Metal Terminal)>
[0185] As a metal terminal, an aluminum foil (JIS H4160:1994 A8079H-O) with a length of 50 mm, a width of 22.5 mm, and a thickness of 400 μm was prepared. Additionally, adhesive films for each metal terminal obtained in the examples and comparative examples (with a length of 45 mm and a width of 15 mm) were prepared. Next, a metal terminal was placed between two adhesive films to obtain a laminate of adhesive film / metal terminal / adhesive film. At this time, the metal terminals were overlapped so that the longitudinal direction of the metal terminal and the width direction of the adhesive film for the metal terminal coincided, and the overlapped area was 22.5 mm × 15 mm. Next, the laminate was placed on a hot plate heated to 190°C with the laminate clamped with two tetrafluoroethylene-ethylene copolymer films (ETFE films, thickness 100 μm), and a 500g weight with a sponge attached was placed on it (pressure becomes 0.015 MPa), and the laminate was left standing for 12 seconds to heat-fuse the adhesive film to the metal terminal. At this time, as shown in the schematic diagram of FIG. 7, as the metal terminal was clamped by the adhesive film, the area around the metal terminal was covered with the adhesive film, and a portion was formed where the two adhesive films were heat-fused together. After heat-fusion, the laminate was naturally cooled to 25°C, and the cross-section in the thickness direction (refer to area M enclosed by the dashed circle in FIG. 7) was observed with a laser microscope to evaluate the conformability of the adhesive film for the metal terminal to the shape of the metal terminal according to the following criteria.
[0186] The results are shown in Table 1.
[0187] A: There are no air bubbles between the adhesive film for metal terminals and the metal terminals.
[0188] B: There are no bubbles at the interface between the adhesive film for metal terminals and the metal terminals, but there are bubbles in the adhesive film for metal terminals near the interface.
[0189] B-: There are bubbles at the interface between the adhesive film for metal terminals and the metal terminals, but there are no bubbles in the adhesive film for metal terminals near the interface.
[0190] C: There are bubbles at the interface between the adhesive film for metal terminals and the metal terminals, and there are also bubbles in the adhesive film for metal terminals near the interface.
[0191] [Table 1]
[0192]
[0193] The adhesive film for metal terminals of Examples 1-3 has a Martens hardness of 30 N / mm², measured perpendicular to the cross-section in the thickness direction of the first polyolefin layer. 2 The following describes the adhesive film for metal terminals of Examples 1-3. The film has excellent adhesion to metal terminals and also has excellent following properties.
[0194] As described above, the present disclosure provides the invention of the following aspects.
[0195] Claim 1. An adhesive film for a metal terminal interposed between a metal terminal electrically connected to an electrode of a capacitor device element and an outer casing for a capacitor device that encapsulates the capacitor device element, wherein
[0196] The adhesive film for the metal terminal above is composed of a laminate having, in this order, a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer casing side for the capacitor device.
[0197] Under the following measurement conditions, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 30 N / mm 2 Adhesive film for metal terminals.
[0198] <Measurement Conditions for Martens Hardness>
[0199] The load is 10 mN.
[0200] The load application speed is 1 mN / 10 seconds.
[0201] The duration is 10 seconds.
[0203] The unloading speed is 1 mN / 10 seconds.
[0204] The indenter is a Vickers indenter with a face angle of 136° at the tip of a square pyramid.
[0205] The measured temperature is 25℃.
[0206] The measurement value is the average of a total of 8 measurements, excluding 1 maximum value and 1 minimum value, taken 10 times by changing the measurement location.
[0207] Claim 2. An adhesive film for metal terminals described in Claim 1, wherein, in the measurement conditions for the Martens hardness above, the indentation modulus measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 400 MPa or less.
[0208] Claim 3. In the measurement conditions for the Martens hardness above, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the substrate is 60 N / mm 2 An adhesive film for metal terminals described in claim 1 or 2, which is less than or equal to the following.
[0209] Claim 4. In the measurement conditions for the Martens hardness above, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the second polyolefin layer is 60 N / mm 2 An adhesive film for metal terminals described in any one of claims 1 to 3, wherein the following
[0210] Claim 5. An adhesive film for a metal terminal as described in any one of Claims 1 to 4, wherein the thickness of the first polyolefin layer is 60 μm or less.
[0211] Claim 6. An adhesive film for metal terminals described in any one of Claims 1 to 5, wherein the thickness of the above-described material is 60 μm or less.
[0212] Claim 7. An adhesive film for a metal terminal as described in any one of Claims 1 to 6, wherein the thickness of the second polyolefin layer is 60 μm or less.
[0213] Claim 8. An adhesive film for a metal terminal as described in any one of Claims 1 to 7, wherein the thickness of the adhesive film for the metal terminal is 180 μm or less.
[0214] Claim 9. In the measurement conditions for the Martens hardness above, the indentation depth h at a load of 10 mN, measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer. max A metal terminal adhesive film described in any one of claims 1 to 8, having a thickness of 4.0 μm or more.
[0215] Claim 10. An adhesive film for metal terminals described in any one of claims 1 to 9, wherein, in the measurement conditions for the Martens hardness above, the indentation modulus measured in a direction perpendicular to the cross-section in the thickness direction of the substrate is 1000 MPa or less.
[0216] Claim 11. The first polyolefin layer comprises a pigment, and is an adhesive film for a metal terminal as described in any one of claims 1 to 10.
[0217] Claim 12. The above description is an adhesive film for metal terminals described in any one of claims 1 to 11, comprising a polyolefin backbone.
[0218] Claim 13. A method for manufacturing an adhesive film for a metal terminal interposed between a metal terminal electrically connected to an electrode of a capacitor device element and an outer casing for a capacitor device that encapsulates the capacitor device element, wherein
[0219] The adhesive film for the metal terminal above is composed of a laminate having, in this order, a first polyolefin layer disposed on the metal terminal side, a substrate, and a second polyolefin layer disposed on the outer casing side for the capacitor device.
[0220] The method includes a process for obtaining a laminate having the first polyolefin layer, the substrate, and the second polyolefin layer in this order.
[0221] Under the following measurement conditions, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 30 N / mm 2 Method for manufacturing an adhesive film for metal terminals, with the following information.
[0222] <Measurement Conditions for Martens Hardness>
[0223] The load is 10 mN.
[0224] The load application speed is 1 mN / 10 seconds.
[0225] The duration is 10 seconds.
[0226] The unloading speed is 1 mN / 10 seconds.
[0227] The indenter is a Vickers indenter with a face angle of 136° at the tip of a square pyramid.
[0228] The measured temperature is 25℃.
[0229] The measurement value is the average of a total of 8 measurements, excluding 1 maximum value and 1 minimum value, taken 10 times by changing the measurement location.
[0230] Claim 14. A metal terminal with an adhesive film attached thereto, wherein the metal terminal is equipped with an adhesive film for a metal terminal as described in any one of Claims 1 to 12.
[0231] Claim 15. A capacitor device comprising, at least, a capacitor device element having a positive electrode, a negative electrode, and an electrolyte, an outer casing for the capacitor device that encapsulates the capacitor device element, and a metal terminal electrically connected to each of the positive electrode and the negative electrode and protruding to the outside of the outer casing for the capacitor device,
[0232] A capacitor device formed by interposing an adhesive film for a metal terminal described in any one of claims 1 to 12 between the metal terminal and the outer casing for the capacitor device.
[0233] Claim 16. A method for manufacturing a capacitor device comprising, at least, a capacitor device element having a positive electrode, a negative electrode, and an electrolyte, an outer casing for the capacitor device that encapsulates the capacitor device element, and a metal terminal electrically connected to each of the positive electrode and the negative electrode and protruding to the outside of the outer casing for the capacitor device, wherein
[0234] A method for manufacturing a capacitor, comprising the steps of interposing an adhesive film for a metal terminal described in any one of claims 1 to 12 between the metal terminal and the outer material for the capacitor device, and encapsulating the capacitor device element with the outer material for the capacitor device. Explanation of the symbols
[0235] 1: Adhesive film for metal terminals 2: Metal terminal 3: Exterior materials for capacitor devices 3a: Peripheral portion of the outer casing for a capacitor device 4: Capacitive device elements 10: Capacitor device 11: Entry 12a: First polyolefin layer 12b: Second polyolefin layer 13: Adhesion promoter layer 31: Base layer 32: Adhesive layer 33: Barrier layer 34: Adhesive layer 35: Heat-fusible resin layer
Claims
Claim 1 An adhesive film for a metal terminal interposed between a metal terminal electrically connected to an electrode of a capacitor device element and an outer casing for a capacitor device that encapsulates the capacitor device element, wherein the adhesive film for the metal terminal is composed of a laminate having, in this order, a first polyolefin layer disposed on the side of the metal terminal, a substrate, and a second polyolefin layer disposed on the side of the outer casing for the capacitor device, wherein the melting point of the substrate is 130°C or higher and 170°C or lower, and under the following Martens hardness measurement conditions, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 30 N / mm 2 An adhesive film for metal terminals having the following, wherein, under the following conditions for measuring Martens hardness, the indentation modulus measured in a direction perpendicular to the cross-section in the thickness direction of the above description is 1000 MPa or less: <Measurement conditions for Martens hardness> The load is 10 mN, the load application speed is 1 mN / 10 seconds, the holding time is 10 seconds, the load removal speed is 1 mN / 10 seconds, the indenter is a Vickers indenter with a face angle of 136° at the tip of a square pyramid, the measurement temperature is 25℃, and the measurement value is the average of a total of 8 measurement values excluding one maximum value and one minimum value, measured 10 times by changing the measurement location. Claim 2 An adhesive film for metal terminals according to claim 1, wherein, under the measurement conditions for the Martens hardness, the indentation modulus measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 400 MPa or less. Claim 3 In claim 1 or 2, regarding the measurement conditions for the Martens hardness, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the substrate is 60 N / mm 2 Adhesive film for metal terminals. Claim 4 In claim 1 or 2, regarding the measurement conditions for the Martens hardness, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the second polyolefin layer is 60 N / mm 2 Adhesive film for metal terminals. Claim 5 An adhesive film for a metal terminal according to claim 1 or 2, wherein the thickness of the first polyolefin layer is 60 μm or less. Claim 6 An adhesive film for metal terminals according to claim 1 or 2, wherein the thickness of the above-described material is 60 μm or less. Claim 7 An adhesive film for a metal terminal according to claim 1 or 2, wherein the thickness of the second polyolefin layer is 60 μm or less. Claim 8 An adhesive film for a metal terminal according to claim 1 or 2, wherein the thickness of the adhesive film for the metal terminal is 180 μm or less. Claim 9 In claim 1 or 2, regarding the measurement conditions for the Martens hardness, the indentation depth h at a load of 10 mN, measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer. max A, adhesive film for metal terminals having a thickness of 4.0 μm or more. Claim 10 In claim 1 or 2, the first polyolefin layer is an adhesive film for metal terminals comprising a pigment. Claim 11 In claim 1 or 2, the above description is an adhesive film for metal terminals comprising a polyolefin backbone. Claim 12 A method for manufacturing an adhesive film for a metal terminal interposed between a metal terminal electrically connected to an electrode of a capacitor device element and an outer casing for a capacitor device that encapsulates the capacitor device element, wherein the adhesive film for the metal terminal is composed of a laminate having, in this order, a first polyolefin layer disposed on the side of the metal terminal, a substrate, and a second polyolefin layer disposed on the side of the outer casing for the capacitor device, wherein the melting point of the substrate is 130°C or higher and 170°C or lower, and the method comprises a process of obtaining a laminate having, in this order, the first polyolefin layer, the substrate, and the second polyolefin layer, wherein, under the following conditions for measuring Martens hardness, the Martens hardness measured in a direction perpendicular to the cross-section in the thickness direction of the first polyolefin layer is 30 N / mm 2 A method for manufacturing an adhesive film for metal terminals, wherein, under the following conditions for measuring Martens hardness, the indentation modulus measured in a direction perpendicular to the cross-section in the thickness direction of the above description is 1000 MPa or less: <Measurement conditions for Martens hardness> The load is 10 mN, the load application speed is 1 mN / 10 seconds, the holding time is 10 seconds, the load removal speed is 1 mN / 10 seconds, the indenter is a Vickers indenter with a face angle of 136° at the tip of a square pyramid, the measurement temperature is 25℃, and the measurement value is the average of a total of 8 measurement values excluding one maximum value and one minimum value, measured 10 times by changing the measurement location. Claim 13 A metal terminal with an adhesive film attached thereto, wherein the metal terminal is equipped with an adhesive film for a metal terminal as described in claim 1 or 2. Claim 14 A capacitor device comprising, at least, a capacitor device element having a positive electrode, a negative electrode, and an electrolyte, an outer casing for a capacitor device that encapsulates the capacitor device element, and a metal terminal electrically connected to each of the positive electrode and the negative electrode and protruding outwardly from the outer casing for a capacitor device, wherein an adhesive film for the metal terminal described in claim 1 or 2 is interposed between the metal terminal and the outer casing for a capacitor device. Claim 15 A method for manufacturing a capacitor having at least a capacitor device element having a positive electrode, a negative electrode, and an electrolyte, an outer casing for a capacitor device that encapsulates the capacitor device element, and a metal terminal electrically connected to each of the positive electrode and the negative electrode and protruding outwardly from the outer casing for a capacitor device, the method comprising the steps of interposing an adhesive film for a metal terminal described in claim 1 or 2 between the metal terminal and the outer casing for a capacitor device, and encapsulating the capacitor device element with the outer casing for a capacitor device. Claim 16 delete
Citation Information
Patent Citations
Resin film for terminal, tab using the same, and power storage device
JP2017033820A
Adhesive film for tightly sealing metal terminal portion of electricity storage device
JP2017120790A
Battery, manufacturing method thereof, metal terminal with adhesive film for metal terminal, and winding body for the adhesive film for metal terminal
JP2019036540A