Polyamide reverse osmosis membrane containing pollution resistance layer and method for manufacturing the same

The polyamide reverse osmosis membrane with an anti-fouling layer of heterocyclic amines or aliphatic diamines addresses fouling issues, maintaining high flow and salt removal rates even after contamination, enhancing membrane efficiency.

KR103046953B1Active Publication Date: 2026-11-10TORAY ADVANCED MATERIALS KOREA INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020240011063
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2026-11-10
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

Conventional reverse osmosis membranes suffer from reduced performance due to fouling, leading to decreased flow rates and salt removal efficiency, despite improvements in anti-fouling properties.

Method used

A polyamide reverse osmosis membrane is developed with an anti-fouling layer comprising heterocyclic amines or aliphatic diamines, which are integrated into the membrane structure to enhance permeation flow rate and salt removal rate while maintaining resistance to fouling.

Benefits of technology

The membrane maintains a flow rate of 26 gfd or more and a salt removal rate of 99.4% or more under standard conditions, with a less than 10% decrease in flow rate after fouling, demonstrating improved performance compared to conventional membranes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a polyamide reverse osmosis membrane comprising a non-fouling layer and a method for manufacturing the same. More specifically, the present invention relates to a polyamide reverse osmosis membrane comprising a non-fouling layer and a method for manufacturing the same, wherein the non-fouling layer comprises a porous support, a porous polymer support layer formed on at least one surface of the porous support, a polyamide layer formed on the polymer support layer, and a non-fouling layer formed on the polyamide layer, wherein the non-fouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof. The polyamide reverse osmosis membrane according to the present invention can have excellent permeation flow rate while improving salt removal rate and non-fouling properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a polyamide reverse osmosis membrane comprising a non-fouling layer and a method for manufacturing the same. More specifically, the present invention relates to a polyamide reverse osmosis membrane comprising a non-fouling layer and a method for manufacturing the same, wherein the non-fouling layer comprises a porous support, a porous polymer support layer formed on at least one surface of the porous support, a polyamide layer formed on the polymer support layer, and a non-fouling layer formed on the polyamide layer, wherein the non-fouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof. The polyamide reverse osmosis membrane according to the present invention can have excellent permeation flow rate while improving salt removal rate and non-fouling properties. Background Technology

[0003] Osmosis refers to the phenomenon in which a solvent moves through a semipermeable membrane between two solutions separated by the membrane, from a solution with a lower solute concentration to a solution with a higher solute concentration. The pressure exerted on the side of the solution with the higher solute concentration due to this movement of the solvent is called osmotic pressure. Conversely, if an external pressure higher than the osmotic pressure is applied, the solvent moves toward the solution with the lower solute concentration; this phenomenon is called reverse osmosis.

[0004] Conventional applications of reverse osmosis membranes are desalination processes for brackish water or seawater, and such desalination processes provide large quantities of fresh or pure water that is relatively suitable for industrial, agricultural, or domestic use. The desalination process of brackish water or seawater using reverse osmosis membranes is a process that literally filters out salts and other dissolved ions or molecules from brine. By passing brine through a reverse osmosis membrane and pressurizing it, purified water passes through the membrane, while salts and other dissolved ions or molecules do not pass through the membrane.

[0005] Since the performance of separation membranes used in membrane filtration processes continuously decreases due to phenomena such as organic fouling, inorganic fouling, particular fouling, and biofouling occurring depending on their use, there is a need for research on reverse osmosis membranes that possess excellent flow rate and salt removal rates as well as superior fouling resistance.

[0006] For example, Korean Registered Patent No. 10-1230843 describes an invention relating to a reverse osmosis membrane, characterized by a porous support layer, a polyamide layer, and a coating layer formed additionally on the polyamide layer to improve anti-fouling performance. However, while the anti-fouling performance was improved, the invention had a problem of reduced flow rate.

[0008] Prior art literature

[0009] Republic of Korea Registered Patent No. 10-1230843 (February 1, 2013) The problem to be solved

[0011] The present invention was devised to solve the above-mentioned problems. After confirming that a reverse osmosis membrane with improved salt removal rate and anti-fouling properties can be manufactured by forming an anti-fouling layer containing a heterocyclic amine, an aliphatic diamine, or a combination thereof on a polyamide layer, while increasing the permeation flow rate, the present invention was completed.

[0013] Accordingly, the present invention aims to provide a polyamide reverse osmosis separation membrane comprising an anti-fouling layer.

[0014] In addition, the present invention aims to provide a method for manufacturing a polyamide reverse osmosis separation membrane comprising an anti-fouling layer. means of solving the problem

[0016] Accordingly, the present invention discloses a polyamide reverse osmosis separation membrane comprising an anti-fouling layer and a method for manufacturing the same.

[0018] According to the first embodiment,

[0019] porous support;

[0020] A porous polymer support layer formed on at least one surface of the above-mentioned porous support;

[0021] A polyamide layer formed on the above polymer support layer; and

[0022] It includes a stain-resistant layer formed on the above polyamide layer, and

[0023] A polyamide reverse osmosis separation membrane comprising a non-fouling layer, wherein the non-fouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof, is disclosed.

[0024] In the present invention, the heterocyclic amine may be selected from one or more of the group consisting of imidazole, pyridine, morpholine, and bipyridine.

[0025] In the present invention, the heterocyclic amine may be included in an amount of 0.02 to 0.2 weight% with respect to the total weight of the anti-contamination layer.

[0026] In the present invention, the aliphatic diamine may be selected from one or more of the group consisting of 1,2-bis(2-aminoethoxy)ethane and 1,3-bis(2-aminopropoxy)propane.

[0027] In the present invention, the aliphatic diamine may be included in an amount of 0.001 to 0.1 weight% with respect to the total weight of the anti-contamination layer.

[0028] In the present invention, when the polyamide reverse osmosis membrane is operated for 1 hour at a temperature of 25°C and a pressure of 225 psi under conditions of an aqueous solution containing 2,000 ppm of sodium chloride (NaCl), the flow rate may be 26 gfd or more and the removal rate may be 99.4% or more.

[0029] In the present invention, the polyamide reverse osmosis membrane may have a flow rate that decreases by less than 10% compared to the initial flow rate when the flow rate is measured after fouling the membrane by adding 50 ppm of dry milk, an organic contaminant, to raw water containing 2,000 ppm of sodium chloride (NaCl) and circulating the raw water for 2 hours under a pressure of 225 psi.

[0031] According to the second embodiment,

[0032] Step 1: Forming a porous polymer support layer by applying and drying a polymer solution on the surface of a porous support;

[0033] Step 2: forming a polyamide layer on the surface of the polymer support layer; and

[0034] It includes the third step of forming an anti-contamination layer on the surface of the polyamide layer, and

[0035] A method for manufacturing a polyamide reverse osmosis membrane is disclosed, wherein the anti-fouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof.

[0036] In the present invention, the heterocyclic amine may be selected from one or more of the group consisting of imidazole, pyridine, morpholine, and bipyridine, and may be included in an amount of 0.02 to 0.2 weight% with respect to the total weight of the anti-contamination layer.

[0037] In the present invention, the aliphatic diamine may be selected from one or more of the group consisting of 1,2-bis(2-aminoethoxy)ethane and 1,3-bis(2-aminopropoxy)propane, and may be included in an amount of 0.001 to 0.1 weight% with respect to the total weight of the anti-contamination layer.

[0038] In the present invention, the amine group in the anti-contamination layer can combine with the unreacted -COCl of the polyamide layer.

[0039] In the present invention, when the polyamide reverse osmosis membrane is operated for 1 hour at a temperature of 25°C and a pressure of 225 psi under conditions of an aqueous solution containing 2,000 ppm of sodium chloride (NaCl), the flow rate is 26 gfd or more and the removal rate is 99.4% or more, and when the flow rate is measured after adding 50 ppm of dry milk, an organic contaminant, to raw water containing 2,000 ppm of sodium chloride (NaCl) and circulating the raw water for 2 hours under a pressure of 225 psi to foul the membrane, the ratio of the flow rate decreasing compared to the initial flow rate may be less than 10%. Effects of the invention

[0041] The polyamide reverse osmosis membrane according to the present invention forms an anti-fouling layer comprising a heterocyclic amine, an aliphatic diamine, or a combination thereof on a polyamide layer, and when operated for 1 hour at a temperature of 25°C and a pressure of 225 psi under conditions of an aqueous solution containing 2,000 ppm of sodium chloride (NaCl), the flow rate is 26 gfd or more and the removal rate is 99.4% or more. Additionally, when 50 ppm of dry milk, an organic contaminant, is added to raw water containing 2,000 ppm of sodium chloride (NaCl) and the raw water is circulated for 2 hours at a pressure of 225 psi to foul the membrane, and the flow rate is measured, it was confirmed that the ratio of the decrease in flow rate compared to the initial flow rate is less than 10% (see Experimental Example 1). Accordingly, it has been proven that the polyamide reverse osmosis membrane according to the present invention can have excellent permeation flow rate while significantly improving salt removal rate and anti-fouling properties by including an anti-fouling layer comprising a heterocyclic amine, an aliphatic diamine, or a combination thereof on a polyamide layer. Specific details for implementing the invention

[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by a skilled expert in the art to which this invention pertains. In general, the nomenclature used herein is well known and commonly used in the art.

[0044] Furthermore, throughout this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0046] 1. Polyamide reverse osmosis membrane including an anti-fouling layer

[0047] The present invention

[0048] porous support;

[0049] A porous polymer support layer formed on at least one surface of the above-mentioned porous support;

[0050] A polyamide layer formed on the above polymer support layer; and

[0051] It includes a stain-resistant layer formed on the above polyamide layer, and

[0052] The present invention aims to provide a polyamide reverse osmosis separation membrane comprising a non-fouling layer, wherein the non-fouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof.

[0053] According to the present invention, when the polyamide reverse osmosis membrane is operated for 1 hour under conditions of an aqueous solution containing 2,000 ppm sodium chloride (NaCl), at a temperature of 25°C and a pressure of 225 psi, the flow rate may be 26 gfd or more and the removal rate may be 99.4% or more.

[0054] According to the present invention, when the polyamide reverse osmosis membrane is fouled by adding 50 ppm of dry milk, an organic contaminant, to raw water containing 2,000 ppm of sodium chloride (NaCl) and circulating the raw water for 2 hours under a pressure of 225 psi, and then measuring the flow rate, the ratio of the decrease in flow rate compared to the initial flow rate may be less than 10%.

[0056] (1) Porous support

[0057] According to the present invention, the porous support is a typical microporous support, and although not particularly limited, the pore size must be large enough for permeable water to pass through, while not being large enough to hinder the formation of a thin film on the porous support.

[0058] According to the present invention, the pore size of the porous support may be 1 to 500 nm. If the pore size of the porous support exceeds 500 nm, the ultrathin film is sunken into the pores, so a desired flat sheet structure may not be formed.

[0059] According to the present invention, the average thickness of the porous support may be 30 to 300 μm, preferably 50 to 200 μm, but is not limited thereto.

[0060] According to the present invention, the porous support may comprise synthetic fibers or natural fibers. For example, the synthetic fibers may comprise one or more selected from polyester fibers, polypropylene fibers, nylon fibers, and polyethylene fibers, and the natural fibers may comprise cellulose-based fibers.

[0062] (2) Porous polymer support layer

[0063] According to the present invention, the porous polymer support layer may comprise one or more selected from polysulfone-based polymers, polyethersulfone-based polymers, polyamide-based polymers, polyimide-based polymers, polyester-based polymers, olefin-based polymers, polyvinylidene fluoride, and polyacrylonitrile.

[0065] (3) Polyamide layer

[0066] According to the present invention, the polyamide layer can be formed by interfacial polymerization of a polyfunctional amine and a polyfunctional acyl halide.

[0067] According to the present invention, the polyfunctional amine may include m-phenylenediamine, p-phenylenediamine, 1,3,6-benzenetriamine, 4-chloro-1,3-phenylenediamine, 6-chloro-1,3-phenylenediamine, 3-chloro-1,4-phenylenediamine, or a combination thereof, but is not limited thereto.

[0068] According to the present invention, the polyfunctional acyl halide may include trymeosoyl chloride (TMC), isophthaloyl chloride (IPC), terephthaloyl chloride (TPC), or a combination thereof, but is not limited thereto.

[0070] (4) Intense layer

[0071] According to the present invention, the anti-contamination layer may comprise a heterocyclic amine, an aliphatic diamine, or a combination thereof.

[0072] According to the present invention, the heterocyclic amine may be selected from one or more of the group consisting of imidazole, pyridine, morpholine, and bipyridine.

[0073] According to the present invention, the heterocyclic amine may be included in an amount of 0.02 to 0.2 weight% with respect to the total weight of the anti-contamination layer.

[0074] According to the present invention, the aliphatic diamine may be selected from one or more of the group consisting of 1,2-bis(2-aminoethoxy)ethane and 1,3-bis(2-aminopropoxy)propane.

[0075] According to the present invention, the aliphatic diamine may be included in an amount of 0.001 to 0.1 weight% with respect to the total weight of the anti-contamination layer.

[0077] 2. Method for manufacturing a polyamide reverse osmosis membrane including an anti-fouling layer

[0078] The present invention

[0079] Step 1: Forming a porous polymer support layer by applying and drying a polymer solution on the surface of a porous support;

[0080] Step 2: forming a polyamide layer on the surface of the polymer support layer; and

[0081] It includes the third step of forming an anti-contamination layer on the surface of the polyamide layer, and

[0082] The present invention aims to provide a method for manufacturing a polyamide reverse osmosis membrane, wherein the above-mentioned antifouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof.

[0084] (1) Step 1

[0085] According to the present invention, the porous support may include synthetic fibers or natural fibers. For example, the synthetic fibers may include one or more selected from polyester fibers, polypropylene fibers, nylon fibers, and polyethylene fibers, and the natural fibers may include cellulose-based fibers. The average thickness of the porous support may be 30 to 300 μm, preferably 50 to 200 μm, but is not limited thereto.

[0086] According to the present invention, the polymer solution may comprise a polymer compound and a remainder of solvent, and the polymer compound may be included in an amount of 5 to 40 weight% of the total weight of the polymer solution, preferably in an amount of 7 to 35 weight%. The polymer compound may comprise one or more selected from polysulfone-based polymers, polyethersulfone-based polymers, polyamide-based polymers, polyimide-based polymers, polyester-based polymers, olefin-based polymers, polyvinylidene fluoride, and polyacrylonitrile. The solvent included in the polymer solution may be used without particular limitation as long as it can uniformly and completely dissolve the polymer without precipitation, and may include, for example, one or more selected from N-methyl-2-pyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and dimethylacetamide (DMAc).

[0087] According to the present invention, the coating can be performed such that the thickness of the polymer support layer is 30 to 300 μm. If the thickness of the polymer support layer is less than 30 μm, there may be problems with reduced flow rate and durability due to compaction, and if it exceeds 300 μm, problems with reduced flow rate may occur as the flow path becomes longer.

[0089] (2) Step 2

[0090] According to the present invention, a polyamide layer can be formed by sequentially coating a polyfunctional amine solution and a polyfunctional acyl halide solution onto the porous support. The coating of the polyfunctional amine solution can be performed by spraying or immersing the polyfunctional amine solution onto the porous support on which the polymer support layer is formed, and can be performed for 0.1 to 10 minutes. The polyfunctional amine may include, but is not limited to, m-phenylenediamine, p-phenylenediamine, 1,3,6-benzenetriamine, 4-chloro-1,3-phenylenediamine, 6-chloro-1,3-phenylenediamine, 3-chloro-1,4-phenylenediamine, or a combination thereof. The polyfunctional acyl halide solution can be applied dry for 5 seconds to 3 minutes. The above-mentioned polyfunctional acyl halide may include trymeosoyl chloride (TMC), isophthaloyl chloride (IPC), terephthaloyl chloride (TPC), or a combination thereof, but is not limited thereto.

[0091] According to the present invention, the polyamide layer may have a thickness of 0.1 to 1.0 μm. If the thickness of the polyamide layer exceeds 1.0 μm, the thickness of the selected layer may become excessively thick, which may cause a problem of reduced flow rate.

[0092] (3) Step 3

[0093] According to the present invention, the anti-contamination layer may comprise a heterocyclic amine, an aliphatic diamine, or a combination thereof. The heterocyclic amine may be selected from one or more of the group consisting of imidazole, pyridine, morpholine, and bipyridine, and may be included in an amount of 0.02 to 0.2 weight% relative to the total weight of the anti-contamination layer. The aliphatic diamine may be selected from one or more of the group consisting of 1,2-bis(2-aminoethoxy)ethane and 1,3-bis(2-aminopropoxy)propane, and may be included in an amount of 0.001 to 0.1 weight% relative to the total weight of the anti-contamination layer.

[0094] According to the present invention, the amine group in the anti-contamination layer can be combined with the unreacted -COCl of the polyamide layer.

[0096] The present invention will be described in detail below through examples, but the following examples and experimental examples are merely illustrative of one form of the present invention and the scope of the present invention is not limited by the following examples and experimental examples.

[0098] <Example>

[0099] Comparative Example 1. Preparation of a reverse osmosis membrane free of a fouling layer

[0100] A porous polysulfone support with a thickness of 140 μm, cast on a nonwoven fabric with an average thickness of 100 μm, was immersed for 40 seconds in an aqueous amine solution containing 2.0 wt% of metaphenylenediamine (MPD), a polyfunctional amine, and 0.2 wt% of ethylhexanediol as an additive, after which the excess aqueous solution was removed. The support coated with the amine aqueous solution on its surface was immersed for 1 minute in an organic solution containing 0.1 wt% of trimezoychloride (TMC), a polyfunctional acid halogen compound, and an isopar solvent as a solvent to carry out interfacial polymerization. Subsequently, the excess organic solution was removed by spraying air at 0.5 bar for 10 seconds, and a polyamide coating layer was formed on the surface of the support by drying at 25°C for 1.5 minutes, followed by thermal crosslinking at 60°C for 2 minutes.

[0102] Example 1. Preparation of an imidazole-resistant contaminant-containing reverse osmosis membrane

[0103] A final polyamide reverse osmosis membrane was prepared by spraying an aqueous solution containing 0.05 wt% imidazole onto the surface of the polyamide thin film prepared in Comparative Example 1 for 20 seconds, removing the excess solution, drying it at 50°C for 4 minutes, and storing it in air at room temperature for 1 day.

[0105] Example 2. Preparation of an imidazole and aliphatic diamine anti-fouling layer-containing reverse osmosis membrane

[0106] A polyamide reverse osmosis membrane was prepared using the same method as in Example 1, except that 0.05 wt% imidazole and 0.02 wt% aliphatic diamine (1,2-bis(2-aminoethoxy)ethane) were used instead of 0.05 wt% imidazole in Example 1.

[0108] Comparative Example 2. Preparation of a reverse osmosis membrane containing a methylamine-resistant layer

[0109] A polyamide reverse osmosis membrane was prepared using the same method as in Example 1, except that methylamine was used instead of imidazole in Example 1.

[0111] Comparative Example 3. Preparation of a reverse osmosis membrane containing a glycine anti-fouling layer

[0112] A polyamide reverse osmosis membrane was prepared using the same method as in Example 1, except that glycine was used instead of imidazole in Example 1.

[0114] Comparative Example 4. Preparation of a reverse osmosis membrane containing an ethanolamine anti-fouling layer

[0115] A polyamide reverse osmosis membrane was prepared using the same method as in Example 1, except that ethanolamine was used instead of imidazole in Example 1.

[0117] <Experimental Example>

[0118] Experimental Example 1. Evaluation of Flow Rate and Salt Removal Rate

[0119] The permeate flow rate and salt removal rate of the reverse osmosis membranes prepared according to the above examples and comparative examples were measured in a 2,000 ppm sodium chloride (NaCl) aqueous solution under conditions of 25°C and 225 psi. In addition, the flow rate reduction rate relative to the initial performance was measured after operating the reverse osmosis membranes prepared according to the above examples and comparative examples in raw water containing 50 ppm dry milk for 2 hours.

[0120] No. Flow rate (gfd) Removal rate (%) Flow rate reduction rate (%) Comparative Example 1 25.74 98.87 -15.7 Example 1 28.09 99.43 -8.64 Example 2 27.66 99.64 -8.29 Comparative Example 2 26.88 99.05 -13.95 Comparative Example 3 26.22 99.35 -15.08 Comparative Example 4 24.91 99.02 -9.96

[0121] As a result, as can be seen from Table 1 above, the flow rate, removal rate, and flow rate reduction rate of Examples 1 and 2 according to the present invention were found to be significantly improved compared to Comparative Examples 1 to 4. Specifically, the flow rates of the reverse osmosis membranes according to Comparative Example 1 (contamination-free), Comparative Example 2 (methylamine-contamination-free), Comparative Example 3 (glycine-contamination-free), and Comparative Example 3 (ethanolamine-contamination-free) were 25.74, 26.88, 26.22, and 24.91, respectively, whereas the flow rates of the reverse osmosis membranes according to Examples 1 and 2 were confirmed to be 28.09 and 27.66, which are increased compared to the Comparative Examples. In addition, the flow rate reduction rates of Comparative Examples 1 to 4 were -15.7%, -13.95%, -15.08%, and -9.96%, respectively, whereas the flow rate reduction rates of the reverse osmosis membranes according to Example 1 and Example 2 were -8.64 and -8.29, respectively, confirming that they have significantly improved antifouling properties compared to the Comparative Examples.

[0123] Specific parts of the present invention have been described in detail above. It is evident to those skilled in the art that such specific descriptions are merely preferred embodiments and do not limit the scope of the invention. Accordingly, the actual scope of the invention is defined by the appended claims and their equivalents.

Claims

Claim 1 A polyamide reverse osmosis membrane comprising a non-fouling layer, wherein the non-fouling layer comprises: a porous support; a porous polymer support layer formed on at least one surface of the porous support; a polyamide layer formed on the polymer support layer; and a non-fouling layer formed on the polyamide layer, wherein the non-fouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof, wherein the heterocyclic amine is selected from one or more of the group consisting of imidazole, pyridine, morpholine, and bipyridine, and the aliphatic diamine is selected from one or more of the group consisting of 1,2-bis(2-aminoethoxy)ethane and 1,3-bis(2-aminopropoxy)propane. Claim 2 delete Claim 3 A polyamide reverse osmosis separation membrane including a non-fouling layer, characterized in that, in claim 1, the heterocyclic amine is included in an amount of 0.02 to 0.2 weight% with respect to the total weight of the non-fouling layer. Claim 4 delete Claim 5 A polyamide reverse osmosis separation membrane including a non-fouling layer, characterized in that, in claim 1, the aliphatic diamine is included in an amount of 0.001 to 0.1 weight% with respect to the total weight of the non-fouling layer. Claim 6 A polyamide reverse osmosis membrane including an anti-fouling layer according to claim 1, characterized in that when the polyamide reverse osmosis membrane is operated for 1 hour under conditions of an aqueous solution containing 2,000 ppm sodium chloride (NaCl), at a temperature of 25°C and a pressure of 225 psi, the flow rate is 26 gfd or more and the removal rate is 99.4% or more. Claim 7 A polyamide reverse osmosis membrane including a fouling-resistant layer according to claim 1, characterized in that when the flow rate is measured after fouling the membrane by adding 50 ppm of dry milk, an organic contaminant, to raw water containing 2,000 ppm of sodium chloride (NaCl) and circulating the raw water under a pressure of 225 psi for 2 hours, the ratio of the decrease in flow rate compared to the initial flow rate is less than 10%. Claim 8 A method for manufacturing a polyamide reverse osmosis membrane, comprising: a first step of forming a porous polymer support layer by applying and drying a polymer solution on the surface of a porous support; a second step of forming a polyamide layer on the surface of the polymer support layer; and a third step of forming an anti-fouling layer on the surface of the polyamide layer, wherein the anti-fouling layer comprises a heterocyclic amine, an aliphatic diamine, or a combination thereof, wherein the heterocyclic amine is selected from one or more of the group consisting of imidazole, pyridine, morpholine, and bipyridine, and the aliphatic diamine is selected from one or more of the group consisting of 1,2-bis(2-aminoethoxy)ethane and 1,3-bis(2-aminopropoxy)propane. Claim 9 A method for manufacturing a polyamide reverse osmosis membrane according to claim 8, characterized in that the heterocyclic amine is included in an amount of 0.02 to 0.2 weight% relative to the total weight of the anti-contamination layer. Claim 10 A method for manufacturing a polyamide reverse osmosis membrane, wherein, in claim 8, the aliphatic diamine is included in an amount of 0.001 to 0.1 weight% relative to the total weight of the anti-fouling layer. Claim 11 A method for manufacturing a polyamide reverse osmosis membrane according to claim 8, characterized in that the amine group in the anti-contamination layer combines with the unreacted -COCl in the polyamide layer. Claim 12 A method for manufacturing a polyamide reverse osmosis membrane according to claim 8, wherein the polyamide reverse osmosis membrane is operated for 1 hour at a temperature of 25°C and a pressure of 225 psi under conditions of an aqueous solution containing 2,000 ppm of sodium chloride (NaCl), the flow rate is 26 gfd or more and the removal rate is 99.4% or more, and when the flow rate is measured after membrane fouling by adding 50 ppm of dry milk, an organic contaminant, to raw water containing 2,000 ppm of sodium chloride (NaCl) and circulating the raw water under a pressure of 225 psi for 2 hours, the ratio of the decrease in flow rate compared to the initial flow rate is less than 10%.

Citation Information

Patent Citations

  • Method for modifying surface of polyamide composite film

    CN105148750A

  • Producing method of the polyamide reverse osmosis membrane having fouling resistence and improved durability

    KR100781625B1