Materials for melt processing and melted products

A polyimide structure derived from a bis(4-hydroxyphenyl)sulfone anhydrous trimellitic acid ester and a specific diamine addresses the challenge of poor melt fluidity in high heat resistance polyimides, enabling efficient melt processing of complex shapes.

KR103046961B1Active Publication Date: 2026-11-10HONSHU CHEM INDAL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020237040963
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-21
Filing Date
2022-04-19
Publication Date
2026-11-10
Estimated Expiration
2042-04-19

AI Technical Summary

Technical Problem

Polyimides with high heat resistance suffer from poor melt fluidity, making them difficult to process into complex shapes using conventional methods, and thermoplastic polyimides face challenges in achieving both high heat resistance and melt processability.

Method used

A polyimide structure derived from a bis(4-hydroxyphenyl)sulfone anhydrous trimellitic acid ester and a specific diamine, which exhibits thermoplasticity and high heat resistance, enabling melt processing.

Benefits of technology

The polyimide material achieves high heat resistance and excellent melt fluidity, allowing for the production of complex melt-processed products such as films, lenses, tapes, laminates, and flexible printed circuit boards with improved processing capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023132856251-PCT00014_ABST
    Figure 112023132856251-PCT00014_ABST
Patent Text Reader

Abstract

The present invention aims to provide a polyimide having high heat resistance and excellent melt fluidity, and a melt processing material having high heat resistance and excellent melt processability comprising said polyimide. As a means of solving the above problem, a melt processing material comprising a polyimide having repeating units represented by the following chemical formula 1 is provided. [Chemical Formula 1] (In the formula, R1 independently represents a straight-chain or branched-chain alkyl group having 1 to 6 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms, or a halogen atom; m independently represents 0, 1, or 2; and X represents a divalent chemical group represented by Chemical Formula 2 below.) [Chemical Formula 2]
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a melt processing material comprising a polyimide having a structure derived from a bis(4-hydroxyphenyl)sulfone anhydrous trimellitic acid ester and a specific diamine, and to a melt processing product such as a film, lens, tape, laminate, flexible printed circuit board (FPC), various electronic materials, and three-dimensional molded products obtained by melt processing using the material. Background Technology

[0002] While polyimide generally has the characteristic of excellent heat resistance, it is an insoluble and infusible material. Therefore, when used as a molding material, it is necessary to use special methods such as sintering molding. Furthermore, to obtain a processed product with a complex shape using the sintering molding method, complex and cumbersome processing steps are required, such as using a cutting machine like an NC lathe to cut the desired shape from a block of polyimide, which results in the processed product becoming expensive.

[0003] Among polyimides, there are some that are thermoplastic (e.g., Patent Document 1). When using a polyimide resin having a high glass transition temperature for the purpose of obtaining a polyimide film with high heat resistance, the higher the heat resistance, the worse the fluidity becomes, which causes processing problems. Prior art literature

[0004] Japanese Patent Publication No. Hei 09-048851 The problem to be solved

[0005] The present invention aims to provide a polyimide having high heat resistance and excellent melt fluidity, and a melt processing material having high heat resistance and excellent melt processability comprising said polyimide. means of solving the problem

[0006] As a result of careful consideration to solve the aforementioned problem, the inventors confirmed that a polyimide having a structure derived from a bis(4-hydroxyphenyl)sulfone anhydrous trimellitic acid ester and a specific diamine possesses thermoplasticity and discovered that it is useful as a material capable of melt processing, thereby completing the present invention. Furthermore, they discovered that the polyimide has high heat resistance and also excellent melt fluidity, which is in a trade-off relationship with that high heat resistance, and thus can be used as a material that combines high heat resistance and excellent melt processability.

[0007] The present invention is as follows.

[0008] 1. A melt processing material comprising a polyimide having repeating units represented by the chemical formula 1 below.

[0009]

[0010] (In the formula, R1 independently represents a straight-chain or branched-chain alkyl group having 1 to 6 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms, or a halogen atom; m independently represents 0, 1, or 2; and X represents a divalent chemical group represented by Chemical Formula 2 below.)

[0011]

[0012] (In the formula, R2 and R3 each independently represent a straight-chain or branched-chain alkyl group having 1 to 6 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms, or a halogen atom; Y represents a direct bond, an oxygen atom, a sulfur atom, a sulfonyl group (-SO2-), a carbonyl group (-CO-), an amide group (-NHCO-), an ester group (-OCO-), an alkylidene group having 1 to 15 carbon atoms, a fluorine-containing alkylidene group having 2 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a phenylmethylidene group, a phenylethylidene group, a phenylene group, or a fluorenylidene group; j represents 0 or 1; h and i each independently represent 0, 1, or 2; k represents 0, 1, or 2; and * represents each chemical formula 1 indicates the bonding position with the nitrogen atom.

[0013] 2. A molten product obtained by melting using the melting material described in 1. Effects of the invention

[0014] The polyimide having a structure derived from a specific diamine and an anhydrous trimellitic acid ester of a bis(4-hydroxyphenyl)sulfone according to the present invention has thermoplasticity, so it is possible to perform melt processing, and thus it can be used as a material for melt processing. Furthermore, compared to a polyimide having a structure derived from an anhydrous trimellitic acid ester of a bis(4-hydroxyphenyl)sulfone known to have thermoplasticity, the polyimide has high heat resistance and excellent melt fluidity in a trade-off relationship with that high heat resistance. Therefore, a material containing the polyimide exhibits a remarkable effect of high heat resistance and excellent melt processing ability. The melt processing material of the present invention can be preferably used as a material for melt processed products containing polyimide, such as films, lenses, tapes, laminates (e.g., copper-clad laminates) or flexible printed circuit boards (FPCs), various electrical and electronic components, encapsulators for electronic components, automotive parts, laminates, adhesives, prepregs, and three-dimensional molded products. Brief explanation of the drawing

[0015] Figure 1 is a graph showing the storage modulus curve of the polyimide obtained in Example 1. Figure 2 is a graph showing the loss modulus curve of the polyimide obtained in Example 1. Figure 3 is a graph showing the TMA curve of the polyimide obtained in Example 1. Figure 4 is a graph showing the storage modulus curve of the polyimide obtained in Comparative Example 1. Figure 5 is a graph showing the loss modulus curve of the polyimide obtained in Comparative Example 1. Figure 6 is a graph showing the TMA curve of the polyimide obtained in Comparative Example 1. Figure 7 is a graph showing the TMA curve of the polyimide obtained in Example 2. Figure 8 is a graph showing the TMA curve of the polyimide obtained in Example 3. Figure 9 is a graph showing the TMA curve of the polyimide obtained in Example 4. Figure 10 is a graph showing the TMA curve of the polyimide obtained in Example 5. Figure 11 is a graph showing the storage modulus curve of the polyimide obtained in Comparative Example 2. Figure 12 is a graph showing the loss modulus curve of the polyimide obtained in Comparative Example 2. Figure 13 is a graph showing the TMA curve of the polyimide obtained in Comparative Example 2. Figure 14 is a graph showing the TMA curve of the polyimide obtained in Comparative Example 3. Specific details for implementing the invention

[0016] The melt processing material of the present invention comprises a polyimide having repeating units represented by the above chemical formula 1.

[0017] [Chemical Formula 1]

[0018]

[0019] (In the formula, R1 independently represents a straight-chain or branched-chain alkyl group having 1 to 6 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms, or a halogen atom; m independently represents 0, 1, or 2; and X represents a divalent chemical group represented by Chemical Formula 2 below.)

[0020] [Chemical Formula 2]

[0021]

[0022] (In the formula, R2 and R3 each independently represent a straight-chain or branched-chain alkyl group having 1 to 6 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms, or a halogen atom; Y represents a direct bond, an oxygen atom, a sulfur atom, a sulfonyl group (-SO2-), a carbonyl group (-CO-), an amide group (-NHCO-), an ester group (-OCO-), an alkylidene group having 1 to 15 carbon atoms, a fluorine-containing alkylidene group having 2 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a phenylmethylidene group, a phenylethylidene group, a phenylene group, or a fluorenylidene group; j represents 0 or 1; h and i each independently represent 0, 1, or 2; k represents 0, 1, or 2; and * represents each chemical formula 1 indicates the bonding position with the nitrogen atom.

[0023] In the above chemical formula 1, R1 each independently represents a straight-chain or branched-chain alkyl group having 1 to 6 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms, or a halogen atom. Among these, a straight-chain or branched-chain alkyl group having 1 to 4 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 4 carbon atoms, or a halogen atom is preferred, a straight-chain or branched-chain alkyl halide group having 1 to 4 carbon atoms, or a halogen atom is more preferred, and a trifluoromethyl group or a fluorine atom is particularly preferred.

[0024] It is preferable that the substitution position of this R1 be an ortho position with respect to the oxygen atom.

[0025] In the above chemical formula 1, m represents 0, 1, or 2 independently. Among these, 0 or 1 is preferred independently, and 0 is particularly preferred.

[0026] In the above chemical formula 2, R2 and R3 each independently represent a straight-chain or branched-chain alkyl group having 1 to 6 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms, or a halogen atom. Among these, a straight-chain or branched-chain alkyl group having 1 to 4 carbon atoms, a straight-chain or branched-chain alkyl halide group having 1 to 4 carbon atoms, or a halogen atom is preferred, a straight-chain or branched-chain alkyl halide group having 1 to 4 carbon atoms, or a halogen atom is more preferred, and a trifluoromethyl group or a fluorine atom is particularly preferred.

[0027] Y in Chemical Formula 2 represents a direct bond, an oxygen atom, a sulfur atom, a sulfonyl group (-SO2-), a carbonyl group (-CO-), an amide group (-NHCO-), an ester group (-OCO-), an alkylidene group having 1 to 15 carbon atoms, a fluorine-containing alkylidene group having 2 to 15 carbon atoms, a cycloalkylidene group having 5 to 15 carbon atoms, a phenylmethylidene group, a phenylethylidene group, a phenylene group, or a fluorenylidene group. Among these, a direct bond, an oxygen atom, a sulfur atom, a sulfonyl group (-SO2-), a carbonyl group (-CO-), an amide group (-NHCO-), an ester group (-OCO-), an alkylidene group having 1 to 12 carbon atoms, a fluorine-containing alkylidene group having 2 to 12 carbon atoms, a cycloalkylidene group having 5 to 12 carbon atoms, a phenylethylidene group, or a fluorenylidene group is preferred, and a direct bond, an oxygen atom, a sulfur atom, a sulfonyl group (-SO2-), a carbonyl group (-CO-), an amide group (-NHCO-), an ester group (-OCO-), an alkylidene group having 1 to 8 carbon atoms, a fluorine-containing alkylidene group having 2 to 8 carbon atoms, a cycloalkylidene group having 6 to 12 carbon atoms, a phenylethylidene group, or a fluorenylidene group is more preferred, and a direct bond, an oxygen atom, Sulfur atoms, sulfonyl groups (-SO2-), amide groups (-NHCO-), ester groups (-OCO-), alkylidene groups having 1 to 4 carbon atoms, fluorine-containing alkylidene groups having 2 to 4 carbon atoms, cycloalkylidene groups having 6 to 9 carbon atoms, or fluorenylidene groups are particularly preferred.

[0028] The above cycloalkylidene group having 5 to 15 carbon atoms may include an alkyl group as a branched chain. Specifically, examples of cycloalkylidene groups include, for instance, a cyclopentylidene group (5 carbon atoms), a cyclohexylidene group (6 carbon atoms), a 3-methylcyclohexylidene group (7 carbon atoms), a 4-methylcyclohexylidene group (7 carbon atoms), a 3,3,5-trimethylcyclohexylidene group (9 carbon atoms), a cycloheptylidene group (7 carbon atoms), a cyclododecanylidene group (12 carbon atoms), etc.

[0029] In Chemical Formula 2, j represents 0 or 1, and 1 is preferred. h and i each independently represent 0, 1, or 2, and 0 or 1 is preferred. k represents 0, 1, or 2, and 0 or 1 is preferred, and 0 is more preferred.

[0030] Preferred examples of the divalent chemical group represented by Chemical Formula 2 in the present invention include Formulas (i) to (x) shown below.

[0031]

[0032] Among these, the chemical groups of formulas (i) to (iii), (ix), and (x) are preferred, the chemical groups of formulas (i), (ii), and (ix) are more preferred, and the chemical groups of formulas (ii) and (ix) are particularly preferred.

[0033] As a diamine compound having the structure of a divalent chemical group represented by the preferred chemical formula 2 above, specifically, for example, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenylsulfide, 3,4'-diaminodiphenylsulfide, 3,3'-diaminodiphenylsulfide, 1,5-diaminonaphthalene, 2,6-diaminonaphthalene, 2,7-diaminonaphthalene, 2,6-diaminoanthracene, 2,7-diaminoanthracene, 1,8-diaminoanthracene, 1,5-diaminoanthracene, 4,4'-diaminobenzanilide, Examples include 3-amino-N-(4-aminophenyl)-benzamide, 4-amino-N-(3-aminophenyl)-benzamide, 4-aminophenyl-4-aminobenzoate, 3-aminophenyl-4-aminobenzoate, 4-aminophenyl-3-aminobenzoate, 2,2'-bis(trifluoromethyl)benzidine, and 2,2'-dimethylbenzidine.

[0034] Among these, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 2,6-diaminonaphthalene, 2,7-diaminonaphthalene, 4,4'-diaminobenzanilide, 4-aminophenyl-4-aminobenzoate, 2,2'-bis(trifluoromethyl)benzidine, and 2,2'-dimethylbenzidine are preferred, and m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 2,2'-bis(trifluoromethyl)benzidine, and 2,2'-dimethylbenzidine are more preferred, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 4,4'-diaminodiphenyl ether, and 2,2'-bis(trifluoromethyl)benzidine are even more preferred, and 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, and 2,2'-bis(trifluoromethyl)benzidine are particularly preferred.

[0035] The method for manufacturing the polyimide included in the melt processing material of the present invention is not particularly limited, but for example, it can be manufactured by reacting a tetracarboxylic acid dianhydride represented by the chemical formula 3 below with a diamine compound having the structure of the chemical formula 2 so that the amounts of the two compounds are equal in molarity, and by undergoing a process of obtaining a polyimide precursor (polyamic acid) and a process of imidizing the polyimide precursor.

[0036]

[0037] (In the formula, R1 and m are identical to Chemical Formula 1.)

[0038] As a specific example thereof, a method of preparation in which the tetracarboxylic acid dianhydride represented by the above chemical formula 3 is 4,4'-dihydroxydiphenylsulfone-bis(trimellitate anhydride)(a) and the divalent chemical group represented by the above chemical formula 2 is 4,4'-diaminodiphenylsulfone (b), which is the chemical group of the above formula (ii), is shown by the reaction scheme below. By polymerizing compound (a) and compound (b) to obtain a polyimide precursor (polyamic acid) (c) having the following repeating unit, and by imidizing this, the target product, a polyimide (d) having the following repeating unit, can be obtained.

[0039]

[0040] For the tetracarboxylic acid dianhydride represented by the above chemical formula 3, R1 and m are the same as in chemical formula 1, and the preferred embodiment is also the same. As a tetracarboxylic acid dianhydride represented by Chemical Formula 3, specifically, for example, 4,4'-dihydroxydiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-dimethyldiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3',5,5'-tetramethyldiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-bis(trifluoromethyl)diphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3',5,5'-tetrakis(trifluoromethyl)diphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-difluorodiphenylsulfone-bis(trimellitate anhydride), Examples include 4,4'-dihydroxy-3,3',5,5'-tetrafluorodiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-dichlorodiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3',5,5'-tetrachlorodiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-dibromodiphenylsulfone-bis(trimellitate anhydride), and 4,4'-dihydroxy-3,3',5,5'-tetrabromodiphenylsulfone-bis(trimellitate anhydride). Among these, 4,4'-dihydroxydiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-dimethyldiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3',5,5'-tetramethyldiphenylsulfone-bis(trimellitate anhydride), 4,4'-dihydroxy-3,3'-bis(trifluoromethyl)diphenylsulfone-bis(trimellitate anhydride), and 4,4'-dihydroxy-3,3',5,5'-tetrakis(trifluoromethyl)diphenylsulfone-bis(trimellitate anhydride) are preferred, and 4,4'-dihydroxydiphenylsulfone-bis(trimellitate anhydride) is particularly preferred.

[0041] The polyimide included in the melt processing material of the present invention may have other skeletons as long as they do not impair the effects of the present invention, provided that they contain repeating units represented by Formula 1. For example, tetracarboxylic acid dianhydrides and diamines other than the skeleton represented by Formula 1 may be used. In such cases, it is preferable that the repeating units of the polyimide of the present invention represented by Formula 1 be present in an amount of 50 mol% or more of the total polyimide, more preferable that they be present in an amount of 60 mol% or more, even more preferable that they be present in an amount of 70 mol% or more, and particularly preferable that they be present in an amount of 90 mol% or more. Furthermore, the repeating units of Formula 1 may be arranged regularly or may exist randomly within the polyimide.

[0042] The method for manufacturing the polyimide included in the melt processing material of the present invention is not particularly limited, and known methods may be appropriately applied. Specifically, for example, it can be synthesized by the following method.

[0043] First, a diamine compound is dissolved in a polymerization solvent, and powders of a tetracarboxylic acid dianhydride in substantially equimolar amounts to the diamine compound are slowly added to the solution. The mixture is then stirred using a mechanical stirrer or the like at a temperature range of 0 to 100°C, preferably 20 to 60°C, for 0.5 to 150 hours, preferably 1 to 72 hours. At this time, the monomer concentration is typically in the range of 5 to 50 weight%, preferably 10 to 40 weight%. By performing polymerization within this monomer concentration range, a uniform polyimide precursor (polyamic acid) with a high degree of polymerization can be obtained. If the degree of polymerization of the polyimide precursor (polyamic acid) increases excessively and the polymerization solution becomes difficult to stir, it is also possible to dilute it appropriately with the same solvent. By performing polymerization within the above monomer concentration range, the degree of polymerization of the polymer is sufficiently high, and sufficient solubility of the monomer and polymer can be ensured. If polymerization is performed at a concentration lower than the above range, the degree of polymerization of the polyimide precursor (polyamic acid) may not be sufficiently high, and if polymerization is performed at a concentration higher than the above monomer concentration range, the dissolution of the monomer or the resulting polymer may be insufficient.

[0044] As a solvent used for the polymerization of a polyimide precursor (polyamic acid), aprotic solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and dimethyl sulfoxide are preferred; however, any solvent can be used without any problems as long as the raw monomer, the resulting polyimide precursor (polyamic acid), and the imidized polyimide are dissolved, and the structure or type of the solvent is not particularly limited. Specifically, for example, amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, ester solvents such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, α-methyl-γ-butyrolactone, butyl acetate, ethyl acetate, isobutyl acetate, etc., carbonate solvents such as ethylene carbonate, propylene carbonate, glycol-based solvents such as diethylene glycol dimethyl ether, triethylene glycol, triethylene glycol dimethyl ether, phenol-based solvents such as phenol, m-cresol, p-cresol, o-cresol, 3-chlorophenol, 4-chlorophenol, etc., ketone-based solvents such as cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone, methyl isobutyl ketone, etc. Examples of ether-based solvents include tetrahydrofuran, 1,4-dioxane, dimethoxyethane, diethoxyethane, and dibutyl ether. Other general-purpose solvents that may be used include acetophenone, 1,3-dimethyl-2-imidazolidinone, sulfolane, dimethyl sulfoxide, propylene glycol methyl acetate, ethyl cellosolve, butyl cellosolve, 2-methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, butanol, ethanol, xylene, toluene, chlorobenzene, turpentine, mineral spirits, and petroleum naphtha-based solvents. Two or more of these solvents may be used in combination.

[0045] The method for imidizing the obtained polyimide precursor (polyamic acid) is described.

[0046] For imidation, known imidation methods can be applied, for example, the "thermoimidation method" which thermally closes a polyimide precursor (polyamic acid) membrane, the "solution thermoimidation method" which closes a polyimide precursor (polyamic acid) solution at high temperature, and the "chemical imidation method" which uses a dehydrating agent can be appropriately used.

[0047] Specifically, in the “thermoimidation method,” a polyimide precursor (polyamic acid) solution is spread on a substrate or the like, and a polyimide precursor (polyamic acid) film is formed by drying at 50 to 200°C, preferably 60 to 150°C, and then the imidation is completed by heating at 150°C to 400°C, preferably 200°C to 380°C, for 1 to 12 hours in an inert gas or under reduced pressure to thermally dehydrate and ring-closure, thereby obtaining the polyimide included in the melt processing material of the present invention. In addition, by doing so, the melt processing material of the present invention in the form of a film can be obtained.

[0048] In addition, in the "solution thermoimidation method," a polyimide precursor (polyamic acid) solution to which a basic catalyst or the like has been added is heated at 100 to 250°C, preferably 150 to 220°C, for 0.5 to 12 hours in the presence of an azeotropic agent such as xylene, thereby removing by-product water from the system and completing the imidation, so that a polyimide solution included in the melt processing material of the present invention can be obtained.

[0049] In the "chemical imidation method," a solution of a polyimide precursor (polyamic acid) adjusted to a suitable solution viscosity that is easy to stir is stirred using a mechanical stirrer or the like, and a dehydrating ring-closing agent (chemical imidation agent) consisting of an anhydride of an organic acid and an amine as a basic catalyst is added dropwise, and chemical imidation is completed by stirring at 0 to 100°C, preferably 10 to 50°C, for 1 to 72 hours. The organic acid anhydride that can be used at this time is not particularly limited, but examples include acetic anhydride and propionic anhydride. Acetic anhydride is preferably used due to the ease of handling and purification of the reagent. In addition, pyridine, triethylamine, quinoline, etc., can be used as the basic catalyst, and pyridine is preferably used due to the ease of handling and separation of the reagent, but is not limited to these. The amount of organic acid anhydride in the chemical imidizing agent is in the range of 1 to 10 moles relative to the theoretical dehydration amount of the polyimide precursor (polyamic acid), and more preferably in the range of 1 to 5 moles. In addition, the amount of basic catalyst is in the range of 0.1 to 2 moles relative to the amount of organic acid anhydride, and more preferably in the range of 0.1 to 1 mole.

[0050] In the "solution thermoimidation method" or "chemical imidation method," by-products such as catalysts, chemical imidizing agents, and carboxylic acids (hereinafter referred to as impurities) are incorporated into the reaction solution; therefore, purification may be performed by removing these. Purification may be carried out using known methods. For example, the simplest method involves dropping the imidized reaction solution dropwise into a large amount of empty solvent while stirring to precipitate the polyimide, recovering the polyimide powder, and repeatedly washing it until the impurities are removed. At this time, the solvents that can be used are preferably water, methanol, ethanol, isopropanol, and other alcohols, which can precipitate the polyimide, efficiently remove impurities, and dry easily; a mixture of these may also be used. If the concentration of the polyimide solution is excessively high when precipitating by dropwise addition into a solvent, the precipitated polyimide may form granules, potentially leaving impurities within the coarse particles or requiring a long time to dissolve the obtained polyimide powder in the solvent. On the other hand, if the concentration of the polyimide solution is excessively low, a large amount of solvent is required, which is undesirable as it increases the environmental burden from waste solvent treatment and raises manufacturing costs. Therefore, the concentration of the polyimide solution when dropwise addition into the solvent is 20% by weight or less, more preferably 10% by weight or less. The amount of solvent used should preferably be equal to or greater than the polyimide solution, and preferably 1.5 to 3 times that amount.

[0051] The obtained polyimide powder can be recovered, and the residual solvent can be removed by vacuum drying or hot air drying to obtain the polyimide included in the melt processing material of the present invention. In addition, by doing so, the resin material for melt processing of the present invention in powder form can be obtained. There are no limitations on the drying temperature and time as long as the temperature prevents the polyimide from deteriorating and the residual solvent from decomposing, and it is preferable to dry for 48 hours or less at a temperature range of 30 to 200°C.

[0052] The polyimide included in the melt processing material of the present invention has an intrinsic viscosity of the polyimide preferably in the range of 0.1 to 10.0 dL / g, and more preferably in the range of 0.2 to 5.0 dL / g.

[0053] The polyimide included in the melt processing material of the present invention can be made into a polyimide varnish as it is soluble in various organic solvents. The organic solvent can be selected according to the intended use or processing conditions of the varnish. For example, but not specifically limited, amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, ester solvents such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, α-methyl-γ-butyrolactone, carbonate solvents such as ethylene carbonate, propylene carbonate, glycol solvents such as diethylene glycol dimethyl ether, triethylene glycol, triethylene glycol dimethyl ether, phenol solvents such as phenol, m-cresol, p-cresol, o-cresol, 3-chlorophenol, 4-chlorophenol, ketone solvents such as cyclopentanone, cyclohexanone, acetone, methyl ethyl ketone, diisobutyl ketone, methyl isobutyl ketone, tetrahydrofuran, 1,4-dioxane, Ether-based solvents such as dimethoxyethane, diethoxyethane, and dibutyl ether, and other general-purpose solvents such as acetophenone, 1,3-dimethyl-2-imidazolidinone, sulfolane, dimethyl sulfoxide, butyl acetate, ethyl acetate, isobutyl acetate, propylene glycol methyl acetate, ethyl cellosolve, butyl cellosolve, 2-methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, chloroform, butanol, ethanol, xylene, toluene, chlorobenzene, turpentine oil, mineral spirits, and petroleum naphtha-based solvents may also be used. Among these, from the perspective of solubility, it is preferable to use amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, ester solvents such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, α-methyl-γ-butyrolactone, and carbonate solvents such as ethylene carbonate and propylene carbonate. Two or more of these solvents may also be used in combination.

[0054] When the polyimide included in the melt processing material of the present invention is dissolved in a solvent to form a solution, the solid content concentration varies depending on the molecular weight of the polyimide, the manufacturing method, and the workpiece being manufactured, but it is preferable to have a solid content of 5% by weight or more. If the solid content concentration is excessively low, it becomes difficult to process with a sufficient film thickness, and conversely, if the solid content concentration is high, there is a risk that the solution viscosity will become excessively high, making processing difficult. As a method for dissolving the polyimide included in the melt processing material of the present invention in a solvent, for example, the polyimide powder included in the melt processing material of the present invention can be added while stirring the solvent, and dissolved over a period of 1 to 48 hours in air or an inert gas at a temperature range from room temperature to below the boiling point of the solvent to form a polyimide solution (varnish).

[0055] The obtained polyimide solution can be processed into various shapes of polyimide by known methods. For example, when processing into a film shape, which is one of the shapes of the melt processing material of the present invention, the polyimide solution can be processed by using a doctor blade or the like on a support such as a glass substrate, and by drying it using a hot air dryer, an infrared dryer, a vacuum dryer, an inert oven, etc., in a range of typically 40 to 350°C, preferably in a range of 50 to 250°C.

[0056] In the present invention, melt processing refers to a broad definition of processing involving thermal melting, including not only generally known melt molding methods such as injection molding, extrusion molding, blow molding, compression molding, rotational molding, blow molding, calendering, melt spinning, foam molding, etc., but also processing by methods such as thermal melt additive manufacturing and selective laser sintering, as well as welding or welding with different resin materials or metal materials.

[0057] The melt processing material of the present invention refers to a material that can be used to manufacture a melt processing product comprising the polyimide of the present invention by being provided for the aforementioned melt processing.

[0058] In one embodiment, the melt processing material of the present invention may comprise only a polyimide having repeating units represented by the above chemical formula 1 and may not comprise any other components. On the other hand, in another embodiment, the melt processing material of the present invention may comprise optional components (other known thermoplastic resin materials, additives, colorants, fillers, etc.) for various purposes. For example, high-density polyethylene, medium-density polyethylene, isotactic polypropylene, polycarbonate, polyarylate, aliphatic polyamide, aromatic polyamide, polyamideimide, polysulfone, polyethersulfone, polyetherketone, polyphenylene sulfide, polyetherimide, polyesterimide, modified polyphenylene oxide, hydrophilic agents, antioxidants, secondary antioxidants, lubricants, release agents, antifogging agents, weather stabilizers, light stabilizers, UV absorbers, antistatic agents, metal deactivators, dyes, pigments, various metal powders, silver nanowires, carbon fibers, glass fibers, carbon nanotubes, graphene, calcium carbonate, titanium oxide, silica, and ceramic materials may be included. These may be incorporated in appropriate amounts depending on the intended use.

[0059] The shape of the melt processing material of the present invention is not particularly limited as long as it is a shape preferred for manufacturing a melt processing product containing the polyimide of the present invention, and examples include a powder shape, particle shape, chip shape, fiber shape, pellet shape, film shape, tape shape, etc.

[0060] In addition, the melt-processed article containing polyimide in the present invention is not particularly limited as long as it is an article obtained by the aforementioned melt-processing method, but examples include various electrical and electronic components such as films, lenses, tapes, laminates (e.g. copper-clad laminates) or flexible printed circuit boards (FPCs), encapsulanters for electronic components, automotive parts, laminates, adhesives, prepregs, three-dimensional molded articles, etc.

[0061] Examples

[0062] The present invention is described in detail below by way of examples, but the present invention is not limited to these examples.

[0063] The analysis method in the present invention is as follows.

[0064] <Analysis Method>

[0065] (1) Glass transition temperature (Tg) and thermoplasticity

[0066] The obtained polyimide film was measured under the conditions below using the apparatus, and the glass transition temperature (Tg) was calculated as an extrapolation point from the TMA curve. In addition, thermoplasticity was evaluated based on the steepness of the displacement of the TMA curve.

[0067] Device: TMA 7100 manufactured by Hitachi High-Tech Science Corp.

[0068] Sample size: Width 5 mm, Length 15 mm

[0069] Conditions: Load 20 mN, temperature range 30℃∼350℃, heating rate 5℃ / min

[0070] Measurement Mode: Tension

[0071] (2) Dynamic viscoelasticity

[0072] The storage modulus and loss modulus of the obtained polyimide film were measured under the following conditions using device 1 or 2 below, and dynamic viscoelasticity was evaluated.

[0073] Device 1: DMA Q800 manufactured by T.A. Instrument Japan Co., Ltd.

[0074] Device 2: DMA 850 manufactured by T.A. Instrument Japan Co., Ltd.

[0075] Conditions: Frequency 0.1 Hz, Temperature range 30℃∼350℃, Heating rate 3℃ / min, Amplitude 0.1%

[0076] <Example 1>: Method for manufacturing a film-shaped melt processing material comprising a polyimide (d) having the following repeating unit

[0077]

[0078] 1.9862 g of 4,4'-diaminodiphenylsulfone (b) and 27.0957 g of dimethylacetamide were added to a 100 mL screw vial and dissolved at room temperature. Subsequently, 4.7885 g of 4,4'-dihydroxydiphenylsulfone-bis(trimellitate anhydride) (a) was added to the diamine solution that had been fully dissolved, and the mixture was stirred under a nitrogen atmosphere. When the viscosity of the solution was sufficiently high, stirring was stopped to obtain a polyamic acid solution (c) with a resin content of 20 wt% and a reduced viscosity of 0.48 dL / g (40°C, 0.5 wt%).

[0079] This polyamic acid (c) was cast onto a smooth glass plate as a support, and after removing the solvent over 2 hours at 60°C under a nitrogen stream, imidization was performed by gradually increasing the temperature to 320°C.

[0080] After immersing the film after imidization in water and peeling it off, drying it at 250°C and 0.1 kPa for 1 hour yielded a film-shaped melt processing material containing the polyimide (d) having the repeating unit. The glass transition temperature (Tg) of the obtained polyimide film was 298°C. In addition, it was confirmed that it is flexible and strong without breaking even when folded at 180°. Furthermore, from the steepness of the displacement of the TMA curve, it was confirmed for the first time that the polyimide represented by the above equation (d) has thermoplasticity.

[0081] The storage modulus curve and loss modulus curve of the obtained polyimide film are shown in Figures 1 and 2, and the TMA curve is shown in Figure 3.

[0082] <Comparative Example 1>: Method for manufacturing polyimide (e) having the following repeating unit

[0083]

[0084] 1.9867 g of 4,4'-diaminodiphenylsulfone (b) and 14.3639 g of dimethylacetamide were added to a 100 mL screw vial and dissolved at room temperature. Subsequently, 4.1639 g of 4,4'-(4,4'-isopropylidenediphenoxy)-bis(phthalic anhydride) was added to the diamine solution that had been fully dissolved, and the mixture was stirred under a nitrogen atmosphere. When the viscosity of the solution became sufficiently high, stirring was stopped to obtain a polyamic acid solution with a resin content of 30 wt% and a reduced viscosity of 0.53 dL / g (40°C, 0.5 wt%).

[0085] The obtained polyamic acid was cast onto a smooth glass plate as a support, and after removing the solvent over 2 hours at 60°C under a nitrogen stream, imidization was performed by gradually increasing the temperature to 320°C.

[0086] After immersing the film in water to remove it, it was dried at 250°C and 0.1 kPa for 1 hour. The glass transition temperature (Tg) of the obtained polyimide film was 253°C.

[0087] The storage modulus curve and loss modulus curve of the obtained polyimide film are shown in Figures 4 and 5, and the TMA curve is shown in Figure 6.

[0088] The polyimide of Example 1 was confirmed to be a high-heat-resistant thermoplastic resin because the softening of the film was observed around its glass transition temperature (Tg) of 300°C, and as shown in Figures 1 and 2, the slope of the decline of the storage modulus curve and the loss modulus curve was very steep.

[0089] Meanwhile, the polyimide of Comparative Example 1 was confirmed to have softened film at its glass transition temperature (Tg) of around 250°C, and as shown in Figures 4 and 5, it was confirmed to be a thermoplastic resin from the slope of the downward slope of the storage modulus curve and the loss modulus curve.

[0090] Looking at the storage modulus curve and the loss modulus curve from the perspective of melt processability, it was confirmed that the curves of the polyimide of Example 1 all continue to decline after the glass transition temperature (Tg) of 300°C. This indicates that during melt processing, even at around 300°C, which is slightly higher than the glass transition temperature (Tg), the elasticity and viscosity of the polymer properties decrease rapidly, resulting in a good flow state. In addition, as shown in Figure 3, it became clear from the TMA curve that it exhibits a steep displacement around the glass transition temperature (Tg) of 300°C. From the above, it became clear that the polyimide of Example 1 is a thermoplastic polyimide resin that has high heat resistance and excellent melt fluidity.

[0091] Meanwhile, in the polyimide of Comparative Example 1, relaxation phenomena were observed in both the storage modulus curve and the loss modulus curve after the glass transition temperature (Tg) of 250°C. This suggests that in order to sufficiently lower elasticity and viscosity during melt processing, a melt processing temperature even higher than the glass transition temperature (Tg) of 250°C is required. Furthermore, as shown in Fig. 6, displacement can be observed from the TMA curve around the glass transition temperature (Tg) of 250°C, but immediately thereafter, a decrease in the slope of the displacement curve's rise can be observed. This indicates that the melt processing performance is inferior because elasticity and viscosity were not sufficiently lowered, along with the relaxation phenomena observed in the storage modulus curve and the loss modulus curve shown in Figs. 4 and 5.

[0092] From the above results, it has become clear that the polyimide resin of Example 1, which is a specific example of the melt processing material of the present invention, is a polyimide resin that satisfies the trade-off relationship between high heat resistance and excellent melt fluidity, and can be used as a melt processing material having high heat resistance and excellent melt processing properties.

[0093] <Example 2>

[0094] In the above Example 1, a polyimide film was obtained in the same way, except that 4,4'-diaminodiphenylsulfone was replaced with 4,4'-diaminodiphenyl ether.

[0095] The glass transition temperature (Tg) of the obtained polyimide film was 272°C. In addition, it was confirmed that it is flexible and strong without breaking even when folded 180°. Furthermore, from the steepness of the displacement of the TMA curve, it was confirmed that it has thermoplasticity and excellent melt fluidity.

[0096] The TMA curve of the obtained polyimide film is shown in Fig. 7.

[0097] <Example 3>

[0098] In the above Example 1, a polyimide film was obtained in the same way except that 4,4'-diaminodiphenylsulfone was replaced with 2,2'-bis(trifluoromethyl)benzidine.

[0099] The glass transition temperature (Tg) of the obtained polyimide film was 284°C. In addition, it was confirmed that it is flexible and strong without breaking even when folded 180°. Furthermore, from the steepness of the displacement of the TMA curve, it was confirmed that it has thermoplasticity and excellent melt fluidity.

[0100] The TMA curve of the obtained polyimide film is shown in Fig. 8.

[0101] <Example 4>

[0102] In the above Example 1, a polyimide film was obtained in the same way except that 4,4'-diaminodiphenylsulfone was replaced with m-phenylenediamine.

[0103] The glass transition temperature (Tg) of the obtained polyimide film was 273°C. In addition, it was confirmed that it is flexible and strong and does not break even when folded 180°. Furthermore, from the steepness of the displacement of the TMA curve, it was confirmed that it has thermoplasticity and excellent melt fluidity.

[0104] The TMA curve of the obtained polyimide film is shown in Fig. 9.

[0105] <Example 5>

[0106] In the above Example 1, a polyimide film was obtained in the same way, except that 4,4'-diaminodiphenylsulfone was replaced with a 1:1 mixture of p-phenylenediamine and m-phenylenediamine.

[0107] The glass transition temperature (Tg) of the obtained polyimide film was 286°C. In addition, it was confirmed that it is flexible and strong without breaking even when folded 180°. Furthermore, from the steepness of the displacement of the TMA curve, it was confirmed that it has thermoplasticity and excellent melt fluidity.

[0108] The TMA curve of the obtained polyimide film is shown in Fig. 10.

[0109] From the results of Examples 2 to 5, it has become clear that, just like the polyimide of Example 1, the polyimides of Examples 2 to 5 are polyimide resins having high heat resistance and excellent melt fluidity, and can be used as melt processing materials having high heat resistance and excellent melt processability.

[0110] <Comparative Example 2>

[0111] In the above Example 1, a polyimide film was obtained in the same way except that 4,4'-diaminodiphenylsulfone was replaced with 2,2'-bis[4-(4-aminophenoxy)phenyl)propane.

[0112] The glass transition temperature (Tg) of the obtained polyimide film was 241℃.

[0113] The storage modulus curve and loss modulus curve of the obtained polyimide film are shown in Figures 11 and 12, and the TMA curve is shown in Figure 13.

[0114] In the polyimide of Comparative Example 2, just like in Comparative Example 1, both the storage modulus curve and the loss modulus curve, which decreased after the glass transition temperature (Tg) of 240°C, showed a relaxation phenomenon. This indicates that in order to sufficiently lower elasticity and viscosity during melt processing, a melt processing temperature even higher than the glass transition temperature (Tg) of 240°C is required.

[0115] In addition, from the TMA curve shown in Fig. 13, displacement can be observed around the glass transition temperature (Tg) of 240°C, but the slope at the start of the rise in the displacement curve is small. This also indicates that the melt processability is inferior, just like in Comparative Example 1.

[0116] <Comparative Example 3>

[0117] In the above Example 1, a polyimide film was obtained in the same way except that 4,4'-diaminodiphenylsulfone was replaced with 1,3-bis(4-aminophenoxy)benzene.

[0118] The glass transition temperature (Tg) of the obtained polyimide film was 226℃.

[0119] The TMA curve of the obtained polyimide film is shown in Fig. 14. From the TMA curve shown in Fig. 14, displacement can be observed around the glass transition temperature (Tg) of 230°C, but it can be observed that the slope at the start of the rise in the displacement curve is small. This indicates that the melt processability is inferior, just like in Comparative Example 1.

Claims

Claim 1 A melt processing material comprising a polyimide having repeating units represented by the chemical formula 1 below. [Chemical Formula 1] (In the formula, m represents 0, and X represents a divalent chemical group represented by Chemical Formula 2 below.)[Chemical Formula 2] (In the formula, R2 and R3 each independently represent a straight-chain or branched-chain alkyl halide group having 1 to 6 carbon atoms; Y represents a direct bond, an oxygen atom, a sulfur atom, or a sulfonyl group (-SO2-); j represents 0 or 1; h and i each independently represent 0, 1, or 2; k represents 0; and * each represents the bonding position with the nitrogen atom of Chemical Formula 1.) Claim 2 A molten product obtained by melting using the melting processing material described in paragraph 1.

Citation Information

Patent Citations

  • Polyimides of a bis-(trimellitate) dianhydride and a diamine

    US3355427A

  • Process for producing polyimide resin

    WO2001025313A1