Conductive metal film and its manufacturing method

A conductive metal film using copper nanoparticles and carboxylic acid prevents oxidation during heat treatment, ensuring high conductivity and flexibility in calcination conditions, addressing the oxidation issue in copper nanoparticles.

KR103047014B1Active Publication Date: 2026-11-10UNIVERSITY INDUSTRY COOPERATION GROUP OF KYUNG HEE UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020240115083
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2026-11-10
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Copper nanoparticles oxidize during heat treatment in air, leading to the formation of an oxide film that reduces conductivity, and existing methods struggle to prevent this oxidation effectively.

Method used

A conductive metal film is manufactured by mixing copper nanoparticles with a capping agent and an organic molecule containing a carboxylic acid, followed by heat treatment using light irradiation methods, which inhibits oxide film formation and enables high conductivity even in an air atmosphere.

Benefits of technology

The method ensures high electrical conductivity by preventing or removing oxide films, maintaining conductivity during and after heat treatment, even when stored in air for extended periods, and allows for flexible calcination conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024093688925-PAT00003_ABST
    Figure 112024093688925-PAT00003_ABST
Patent Text Reader

Abstract

The present invention relates to a conductive metal film and a method for manufacturing the same. According to an embodiment of the present invention, by surface treating a metal film with an organic molecule containing a carboxylic acid, an oxide film is hardly formed on the metal film even when a calcination reaction is carried out, and even if an oxide film is formed, it is reduced to provide a conductive metal nanoparticle film with excellent electrical conductivity and a method for manufacturing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a conductive metal film and a method for manufacturing the same. More specifically, the invention relates to a conductive metal film formed by light irradiation after manufacturing a metal nanoparticle film in which the formation of an oxide film is suppressed, and a method for manufacturing the same. Background Technology

[0003] Copper nanoparticles are a material that is gaining attention as they can be used as conductive inks capable of securing high conductivity while offering excellent cost competitiveness. However, unlike silver nanoparticles, copper nanoparticles undergo an oxidation reaction when a firing reaction is carried out through heat treatment in air, which is essential for securing conductivity. Accordingly, the present invention proposes an optimal process material technology to prevent oxidation from occurring even when a firing reaction is performed. Prior art literature

[0005] Korean Published Patent Application No. 10-2012-0132424, "Method for Photothermal Sintering of Conductive Copper Nanoink" The problem to be solved

[0006] One objective of the present invention is to provide a conductive metal film capable of inhibiting the formation of an oxide film and reducing the oxide film even if it is formed, by manufacturing a metal film adsorbed with an organic molecule containing a carboxylic acid.

[0007] Another objective of the present invention is to provide a metal film that maintains electrical conductivity by shortening the time required for an oxide film to be formed even when the metal film is fired in the atmosphere.

[0008] Another objective of the present invention is to provide a conductive metal film that can perform light irradiation under a wide range of conditions during a calcination reaction using a light irradiation method and exhibits high conductivity after light irradiation.

[0009] Another objective of the present invention is to provide a conductive metal film that exhibits electrical conductivity upon calcination even when metal nanoparticles are stored in air for a long period of time. means of solving the problem

[0011] A method for manufacturing a conductive metal film according to the present invention is characterized by comprising the steps of: preparing a metal nanoparticle ink by mixing an organic molecule containing a carboxylic acid having 1 to 17 carbon atoms into a solution in which metal nanoparticles are dispersed; preparing a metal nanoparticle film by applying the metal nanoparticle ink to a substrate; and heat-treating the metal nanoparticle film.

[0012] According to one embodiment, the metal nanoparticles are combined with a capping agent, and the metal nanoparticles may include any one selected from copper, nickel, tin, iron, aluminum, molybdenum, tungsten, gallium, indium, and alloy compositions thereof.

[0013] According to one embodiment, the capping agent may prevent contact between the metal nanoparticles and moisture or oxygen, and may play a role in improving the dispersibility of the metal nanoparticles when preparing a solution in which the metal nanoparticles are dispersed.

[0014] According to one embodiment, the capping agent may be a polymer or organic molecule comprising any one selected from the group consisting of pyridine, phosphine, phosphine oxide, amine, thiol, and hydroxyl functional groups.

[0015] According to one embodiment, the organic molecule containing the carboxylic acid comprises one to four carboxyl groups, and the organic molecule containing the carboxylic acid may be any one selected from the group consisting of fatty acid, hydrocarboxylic acid, amino acid, and aromatic acid.

[0016] According to one embodiment, the organic molecule containing the carboxylic acid may include formic acid, propionic acid, or butyric acid.

[0017] According to one embodiment, the step of heat-treating the metal nanoparticle film may be any one selected from the group consisting of high-temperature (furnace) heat treatment, laser irradiation heat treatment, white light irradiation heat treatment, plasma heat treatment, microwave heat treatment, and Joule heating.

[0018] According to one embodiment, in the heat treatment step, the laser irradiation heat treatment, white light irradiation heat treatment, plasma heat treatment, and microwave heat treatment may be performed in air.

[0019] According to one embodiment, the laser may be irradiated with a power of 0.5 W to 20 W.

[0020] According to one embodiment, the scanning speed of the laser may be 100 mm / sec to 2,000 mm / sec.

[0021] A conductive metal film according to the present invention is manufactured by a method for manufacturing a conductive metal film according to the present invention and comprises metal nanoparticles and an organic molecule comprising a carboxylic acid having 1 to 17 carbon atoms adsorbed on the metal nanoparticles, wherein the organic molecule comprising the carboxylic acid prevents the formation of an oxide film on the metal nanoparticles and can remove the formed oxide film even if the oxide film is formed.

[0022] According to one embodiment, the organic molecule containing the carboxylic acid may be adsorbed on the surface of the metal nanoparticle.

[0023] According to one embodiment, the electrical conductivity of the conductive metal film prepared using the metal nanoparticles stored in air for 1 to 60 days is 1.10 × 10⁻⁶ 4 S / cm to 9.07 × 10 4 It can be S / cm. Effects of the invention

[0025] The present invention provides a conductive metal film in which electrical conductivity is exhibited even when the metal nanoparticle film is calcined in the atmosphere. More specifically, the present invention provides a conductive metal film in which high electrical conductivity is exhibited even when a calcination reaction is carried out in the atmosphere using a light irradiation method and an organic molecule containing a carboxylic acid.

[0026] In the present invention, the formation of an oxide film can be suppressed due to an organic molecule containing a carboxylic acid included in a conductive metal film, and even if an oxide film is formed, electrical conductivity can be restored because the organic molecule containing the carboxylic acid reduces the oxide film.

[0027] In the present invention, even if a sufficient calcination reaction does not proceed due to low power conditions or fast scan speed conditions (low transmitted light energy) during a calcination reaction via a light irradiation method, additional calcination reaction can proceed due to organic molecules containing carboxylic acids, thereby exhibiting high conductivity.

[0028] In the present invention, even if an additional oxide film is formed due to high power conditions or slow scan speed conditions (high transmitted light energy) during the calcination reaction using a light irradiation method, the oxide film can be removed by causing a reduction reaction of the oxide film due to organic molecules containing carboxylic acids, thereby enabling high conductivity.

[0029] The present invention provides a conductive metal film capable of exhibiting electrical conductivity, wherein the oxide film formed during long-term storage due to organic molecules containing carboxylic acids is removed during the heat treatment step, even when metal nanoparticles are stored in air for a long period. Brief explanation of the drawing

[0031] Figure 1a is a graph showing the results of analyzing Preparation Example 1 using XPS (X-ray Photoelectron Spectroscopy). Figure 1b shows the results of calculating the ratio of each composition through the results of X-ray Photoelectron Spectroscopy (XPS) analysis of Preparation Example 1. Figure 2 is a graph showing the electrical conductivity according to the laser conditions of Comparative Example 1-2. Figures 3a and 3b are graphs showing the results of analyzing Comparative Example 1-2 by XPS (X-ray Photoelectron Spectroscopy). Figure 3c shows the results of calculating the ratio of each composition through the results of X-ray Photoelectron Spectroscopy (XPS) analysis of Comparative Examples 1-2. Figure 4 is an image of Comparative Example 1-2 taken with a scanning electron microscope (SEM). Figure 5 is a graph showing the electrical conductivity according to the laser conditions of Example 1-2. Figure 6 is an image of Example 1-2 taken with a scanning electron microscope (SEM). Figure 7 is a graph showing the electrical conductivity according to the laser conditions of Example 2-2. Figures 8a and 8b are graphs showing the results of analyzing Example 2-2 by XPS (X-ray Photoelectron Spectroscopy). Figure 8c shows the results of calculating the ratio of each composition through the X-ray Photoelectron Spectroscopy (XPS) analysis of Example 2-2. Figure 9 is an image of Example 2-2 taken with a scanning electron microscope (SEM). Figure 10 is a graph showing the electrical conductivity according to the laser conditions of Example 3-2. Figure 11 is an image of Example 3-2 taken with a scanning electron microscope (SEM). Figure 12 is a graph showing the electrical conductivity according to the laser conditions of Comparative Example 2-2. Figure 13 is an image of Comparative Example 2-2 taken with a scanning electron microscope (SEM). Specific details for implementing the invention

[0032] Embodiments of the present invention will be described in detail below with reference to the attached drawings and the contents described therein, but the present invention is not limited or restricted by the embodiments.

[0033] The terms used herein are for describing the embodiments and are not intended to limit the invention. In this specification, the singular form includes the plural form unless specifically stated otherwise in the text. As used herein, "comprises" and / or "comprising" do not exclude the presence or addition of one or more other components, steps, actions, and / or elements to the mentioned components, steps, actions, and / or elements.

[0034] As used herein, terms such as “examples,” “examples,” “aspects,” “examples,” etc., are not to be interpreted as implying that any described aspect or design is superior or more advantageous than other aspects or designs.

[0035] Furthermore, the term 'or' refers to an inclusive or rather an exclusive or. That is, unless otherwise noted or is not evident from the context, the expression 'x uses a or b' refers to any one of the natural inclusive permutations.

[0036] Additionally, singular expressions (“a” or “an”) used in this specification and claims should generally be interpreted to mean “one or more” unless otherwise stated or it is clear from the context that they relate to the singular form.

[0037] In addition, when a part such as a membrane, layer, region, or configuration request is described as being "on" or "on" another part, it includes not only cases where it is directly on top of the other part, but also cases where another membrane, layer, region, or component is interposed in between.

[0039] A method for manufacturing a conductive metal film according to the present invention comprises the steps of: preparing a metal nanoparticle ink by mixing an organic molecule containing a carboxylic acid having 1 to 17 carbon atoms into a solution in which metal nanoparticles are dispersed; preparing a metal nanoparticle film by applying the metal nanoparticle ink to a substrate; and heat-treating the metal nanoparticle film.

[0040] In a method for manufacturing a conductive metal film, a step of manufacturing metal nanoparticles may be further included prior to the step of manufacturing a metal nanoparticle ink. The size of the manufactured metal nanoparticles may be 10 nm to 200 nm, and the mixture may include metal micron particles with a size of 0.2 μm to 50 μm.

[0041] In the step of manufacturing metal nanoparticles, the metal nanoparticles may include any one selected from copper, nickel, tin, iron, aluminum, molybdenum, tungsten, gallium, indium, and alloy compositions thereof, and in the step of manufacturing metal nanoparticles, the metal nanoparticles may be combined with a capping agent.

[0042] Capping agents can play a role in suppressing particle overgrowth caused by collisions due to Brownian motion during synthesis at high temperatures, and can also inhibit oxidation of metal nanoparticles by acting as a surface protective layer that prevents direct contact with moisture and oxygen.

[0043] In addition, the dispersibility of metal nanoparticles in a solvent can be improved as the capping agent is bound to the metal nanoparticles.

[0044] The capping agent may be a polymer or organic molecule comprising a functional group capable of bonding with a metal, more specifically, any one selected from the group consisting of pyridine, phosphine, phosphine oxide, amine, thiol, and hydroxyl functional groups.

[0045] Non-limiting examples of capping agents containing a pyridine functional group may be any one selected from the group consisting of polyvinylpyrrolidone, poly(N-vinyl-2-pyrrolidone), and 4-dimethylaminopyridine, and non-limiting examples of capping agents containing a phosphine functional group may be any one selected from the group consisting of trioctylphosphine, triphenylphosphine, tri(p-tolyl)phosphine, 1,2-bis(diphenylphosphino)ethane, and 1,2-bis(diphenylphosphino)propane.

[0046] In addition, non-limiting examples of capping agents containing a phosphine oxide functional group may be trioctylphosphine oxide or triphenylphosphine oxide, and non-limiting examples of capping agents containing an amine functional group may be any one selected from the group consisting of oleylamine, hexylamine, dodecylamine, octadecylamine, and dimethylethanolamine.

[0047] In addition, non-limiting examples of capping agents containing a thiol functional group may be any one selected from the group comprising 1-octanethiol, 1-dodecanethiol, 1,9-nonaneedithiol, 4-toluenethiol, Benzene-1,4-dithiol, Poly(ethylene glycol)methyl ether thiol, and 5-methyl-1,3,4-thiadiazole-2-thiol, and non-limiting examples of capping agents containing a hydroxyl functional group may be polyethylene glycol or polypropylene glycol.

[0049] In the step of manufacturing metal nanoparticle ink, an organic molecule containing a carboxylic acid can be added to a polar solvent in which metal nanoparticles are dispersed and stirred.

[0050] In the step of manufacturing metal nanoparticle ink, the polar solvent may be any one selected from the group consisting of acetone, methyl ethyl ketone, methyl alcohol, ethyl alcohol, isopropyl alcohol, butyl alcohol, ethylene glycol, polyethylene glycol, tetrahydrofuran, dimethylformamide, dimethylacetamide, and N-methyl-2-pyrrolidone, and an organic molecule containing a carboxylic acid may be adsorbed on the surface of the metal nanoparticles to perform the role of inhibiting the oxidation reaction of the metal nanoparticles and reducing the surface oxide film.

[0051] The number of carbon atoms in an organic molecule containing a carboxylic acid can be 1 to 17.

[0052] If the number of carbon atoms in an organic molecule containing a carboxylic acid exceeds 17, the adsorption reaction between the organic molecule containing the carboxylic acid and the metal nanoparticle may be limited due to steric resistance with the capping agent bound to the surface of the metal nanoparticle. In other words, organic molecules containing carboxylic acids with more than 17 carbon atoms are blocked by the capping agent, making it difficult for them to approach the surface of the metal nanoparticle. When using organic molecules containing carboxylic acids with more than 17 carbon atoms, the carboxylic acid functional groups of the organic molecules are adsorbed to the reactive groups of the capping agent, and upon heat treatment, the organic molecules containing carboxylic acids carbonize and become unable to perform the function of inhibiting oxide film formation. Therefore, when manufacturing a metal nanoparticle film using organic molecules containing carboxylic acids with more than 17 carbon atoms, the inhibition of oxide film formation and the reduction reaction cannot be initiated upon heat treatment, and the film cannot function as a conductive film.

[0054] The organic molecule containing the carboxylic acid may be any one selected from the group consisting of fatty acids, hydrocarboxylic acids, amino acids, and aromatic acids containing one carboxyl group, and may be an organic molecule containing two to four carboxyl groups. Preferably, the organic molecule containing the carboxylic acid may be formic acid, propionic acid, or butyric acid.

[0055] Non-limiting examples of fatty acids containing one carboxyl group may be any one selected from the group consisting of formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, decanoic acid, and lauric acid, and non-limiting examples of hydrocarboxylic acids containing one carboxyl group may be glycolic acid or lactic acid.

[0056] Non-limiting examples of amino acids containing one carboxyl group may be any one selected from the group consisting of glycine, alanine, serine, and threonine, and non-limiting examples of aromatic acids containing one carboxyl group may be 2-furoic acid or niacin.

[0057] Non-limiting examples of organic molecules containing two to four carboxyl groups may be any one selected from the group consisting of oxalic acid, maleic acid, malonic acid, fumaric acid, malic acid, ascorbic acid, succinic acid, adipic acid, glutaric acid, tartaric acid, citric acid, aconic acid, propane-1,2,3-tricarboxylic acid, trimesic acid, and ethylene-diamine-tetraacetic acid.

[0059] The organic molecule containing the carboxylic acid may be any one selected from the group consisting of monomers having a carboxylic acid functional group having 1 to 17 carbon atoms.

[0060] According to one embodiment, the organic molecule containing the carboxylic acid may be any one selected from the group consisting of monomers having a carboxylic acid functional group having one to three carbon atoms. Non-limiting examples may be any one selected from the group consisting of formic acid, acetic acid, propionic acid, glycolic acid, lactic acid, glycine, alanine, serine, threonine, 2-furoic acid, niacin, oxalic acid, and malonic acid.

[0061] According to one embodiment, the organic molecule containing the carboxylic acid may be any one selected from the group consisting of monomers having a carboxylic acid functional group having 4 to 17 carbon atoms. Non-limiting examples may be any one selected from the group consisting of butyric acid, valeric acid, caproic acid, caprylic acid, decanoic acid, lauric acid, maleic acid, fumaric acid, malic acid, ascorbic acid, succinic acid, adipic acid, glutaric acid, tartaric acid, citric acid, aconic acid, propane-1,2,3-tricarboxylic acid, trimesic acid, and ethylene-diamine-tetraacetic acid.

[0063] Organic molecules containing carboxylic acids can be used in an amount of 1% to 15% by weight relative to the total weight of metal nanoparticles.

[0064] When using organic molecules containing carboxylic acids in an amount of less than 1 mass%, they cannot perform the role of inhibiting oxide film formation and reducing oxide films, and when using more than 15 mass%, problems may arise in which conductivity is reduced due to excessive adsorption of organic molecules.

[0066] In the step of manufacturing a metal nanoparticle film, metal nano ink can be applied to the upper surface of a glass substrate or a polymer substrate and dried at room temperature, and can be applied by any one of spin coating, bar coating, slot-die coating, tape casting, inkjet printing, dispensing printing, and screen printing.

[0067] The thickness of the manufactured metal nanoparticle film can be 0.1 μm to 30 μm.

[0068] When the film thickness is less than 0.1 μm, the three-dimensional connectivity of the metal nanoparticles is not secured, so conductivity is not exhibited, and when the film thickness exceeds 30 μm, there is a possibility that cracks may occur due to shrinkage after firing, and delamination from the substrate may occur.

[0070] A calcination process is required for metal nanoparticle films to exhibit electrical conductivity. Therefore, after the step of manufacturing the metal nanoparticle film, a heat treatment step can be performed to enable electrical conductivity.

[0071] In the heat treatment step, the heat treatment can be performed by any one of the following methods: furnace heat treatment, Joule heating, laser irradiation heat treatment, white light irradiation heat treatment, plasma heat treatment, or microwave heat treatment, and can be carried out in an inert gas atmosphere or atmosphere.

[0072] Here, high temperature (Furnace) heat treatment refers to heat treatment in a furnace. In addition, Joule heating is a method of heating a metal object using electromagnetic induction; when current is supplied to a coil, eddy currents are generated in the metal to be heated, and the Joule heat generated by the resistance of the metal raises the temperature.

[0073] The heat treatment step can be carried out in an inert gas atmosphere or in the atmosphere.

[0074] More specifically, when heat treatment is performed using a high-temperature heat treatment method during the heat treatment step, it can be carried out in an inert gas atmosphere such as argon (Ar) or nitrogen (N2).

[0075] While performing the sintering process using high-temperature heat treatment offers the advantage of obtaining high conductivity, it requires a relatively long time. Since metal nanoparticles may oxidize and lose their metallic properties during the treatment, an inert gas atmosphere must be established during the heat treatment.

[0076] However, when performing high-temperature heat treatment, manufacturing costs may increase due to inert gas atmosphere control and long heat treatment times, and since selective firing of electrode patterns is impossible, it may be limited in terms of intensive processes due to substrate and chip damage.

[0077] In the heat treatment step, if light irradiation such as laser irradiation heat treatment or white light irradiation heat treatment is performed, it may be performed in air. "Air" means that the oxygen content is 21 v / v% and the pressure is 1 atm.

[0078] When light irradiation is performed, light energy is converted into thermal energy, producing an effect similar to heat treatment. However, since light irradiation produces an effect similar to heat treatment even when performed for a short period of about 1 msec, the process can be carried out without concern for metal oxidation in the atmosphere. In addition, since only the electrode pattern can be sintered, there is an advantage in that the sintering process can be carried out without degrading the characteristics of passive or active chips mounted on the substrate.

[0080] In the heat treatment step, light irradiation may be laser irradiation.

[0081] Metal nanoparticles possess plasmonic light absorption characteristics at specific wavelengths. Therefore, when using white light that covers all visible light wavelengths during the irradiation phase, the irradiation efficiency is poor and substrate damage is inevitable because most wavelengths remain unabsorbed. On the other hand, in the case of short-wavelength laser irradiation that matches the absorption wavelengths of the metal nanoparticles, irradiation efficiency can be maximized and substrate damage minimized through light absorption control.

[0083] According to one embodiment, the process range of light irradiation can be extended by adsorbing an organic molecule containing a carboxylic acid with metal nanoparticles.

[0084] Generally, when light irradiation is performed with high power or at a slow irradiation speed, a large amount of light energy reaches the metal nanoparticle film per unit time, so an oxidation reaction occurs at the laser-irradiated area and an oxide film may be formed.

[0085] According to one embodiment of the present invention, a reduction reaction of an oxide film formed by an excess amount of light energy occurs due to an organic molecule containing a carboxylic acid adsorbed on metal nanoparticles, and the oxide film can be removed. The reduction reaction and removal reaction of the oxide film caused by an organic molecule containing a carboxylic acid are as follows.

[0086] Organic molecules containing carboxylic acids adsorbed on the surface of metal nanoparticles by light irradiation can be separated into hydrogen ions and carboxylates. The separated hydrogen ions combine with oxygen atoms present in the oxide film generated by light irradiation to be converted into hydroxyl groups, while the separated carboxylates remain adsorbed on the surface of the oxide film.

[0087] Subsequently, the carboxylate is decomposed into carbon dioxide and alkyl radicals, and the highly reactive alkyl radicals combine with the hydroxyl group converted by hydrogen ions to volatilize as an alcohol gas byproduct, so the oxide film can be removed.

[0088] In other words, organic molecules containing carboxylic acids included in metal nanoparticle films enable the reduction of additional oxide films formed when light is irradiated using high power or when the irradiation speed of the light source is reduced, so high conductivity can be secured even when the transmitted light energy is high.

[0089] Generally, when light irradiation is performed at a low power or high irradiation rate, the amount of light energy reaching the metal nanoparticle film per unit time is small, so a sufficient calcination reaction does not proceed, making it difficult to develop electrical conductivity.

[0090] According to one embodiment of the present invention, even if the amount of light energy reaching the metal nanoparticle film per unit time is small and a sufficient calcination reaction does not proceed, sufficient electrical conductivity can be achieved because an additional calcination reaction proceeds due to the reduction and removal reaction of the oxide film caused by the organic molecule containing the aforementioned carboxylic acid.

[0091] In the light irradiation step, the laser may be irradiated with a power of 0.5 W to 20 W. Preferably, the laser may be irradiated with a power of 1.5 W to 4 W.

[0092] In addition, during the light irradiation step, the laser irradiation speed may be 100 mm / sec to 2,000 mm / sec, and a more preferable irradiation speed may be 500 mm / sec to 1,200 mm / sec. In this case, the laser irradiation speed may refer to the speed at which the laser irradiation unit moves (scans) on the metal nanoparticle film.

[0094] Organic molecules containing carboxylic acids may be adsorbed onto an oxide film formed on the surface of metal nanoparticles. The oxide film formed on the surface of the metal particles contains hydroxyl groups, and the organic molecules containing carboxylic acids possess highly polar functional groups. Therefore, surface adsorption of organic molecules containing carboxylic acids is possible through physical bonding (Keesum Force) acting on the highly polar functional groups.

[0096] The electrical conductivity of a conductive metal film prepared by storing metal nanoparticles prepared according to the method of the present invention in air for 1 to 60 days is 1.10 × 10⁻⁶. 4 S / cm to 9.07 × 10 4 It can be S / cm.

[0097] More specifically, the electrical conductivity of a conductive metal film prepared by storing in air for 1 to 60 days followed by photocalcination is 1.10 × 10⁻⁶ 4 S / cm to 1.42 × 10 4 It can be S / cm, and the electrical conductivity of the conductive film manufactured by heat treatment after storage is 4.32 × 10⁻⁶ 4 S / cm to 9.07 × 10 4 It can be S / cm.

[0098] The above-described electrical conductivity value may be a value corresponding to 85% to 94% of the electrical conductivity of a conductive metal film manufactured by using unstored metal nanoparticles and performing light irradiation or high-temperature heat treatment.

[0099] In the case of copper nanoparticles stored in air for a long period, the surface oxide film can increase significantly. Therefore, when manufacturing a conductive metal film using metal nanoparticles stored for a long period, there is a limitation in that the electrical conductivity decreases significantly. However, in the present invention, the reduction reaction of the oxide film generated by organic molecules containing carboxylic acid is possible during the heat treatment step, thereby ensuring the long-term stability of the material.

[0100] In other words, metal nanoparticles manufactured according to the method of the present invention have the advantage of ensuring long-term stability of the material because, even when stored in air for a long period, the oxide film can be reduced through organic molecules containing carboxylic acids during the heat treatment step, thereby removing the increased oxide film during long-term storage and possessing high electrical conductivity.

[0102] The present invention will be described in more detail below through examples and drawings. These examples are intended to explain the invention more specifically, and the scope of the invention is not limited by these examples.

[0104] [Preparation Example 1] Copper nanoparticles

[0105] 56 g of polyvinylpyrrolidone (PVP) with a molecular weight of 58,000 was added to 280 ml of diethyleneglycol and dissolved by stirring at 90°C for 30 minutes. The stirred solution was cooled to room temperature, and 2.35 g of sodium phosphinate monohydrate (NaH2PO2·H2O) was added and heated to 130°C while stirring. 7 g of copper sulfate pentahydrate (CuSO4·5H2O) was dissolved in 21 ml of distilled water and injected at an injection rate of 1 ml / min, and the reaction was carried out by stirring for 1 hour. The stirred reaction solution was cooled to room temperature and centrifuged at 7,000 rpm for 15 minutes to obtain a precipitate. The obtained precipitate was purified by centrifugation twice using ethanol. As a result, copper nanoparticles without an oxide film (Preparation Example 1) were produced.

[0107] Figure 1a is a graph showing the results of analyzing Preparation Example 1 using XPS (X-ray Photoelectron Spectroscopy). Referring to Figure 1a, it can be seen that copper particles (Cu) with almost no oxide film formed were synthesized through Preparation Example 1.

[0108] Figure 1b shows the results of calculating the ratio of each composition through the X-ray Photoelectron Spectroscopy (XPS) analysis of Preparation Example 1. Referring to Figure 1b, the proportion of copper oxide (CuO, Cu2O) is 13.6 at%, confirming that most of the copper was not oxidized.

[0110] [Comparative Example 1-1] Preparation of Copper Nanoparticle Film

[0111] A coating ink was prepared by dispersing oxide-free copper nanoparticles prepared in Preparation Example 1 in an ethanol solvent at a concentration of 20 wt%. After UV Ozone Clean a 75 μm thick Kapton HN film for 30 minutes, copper nanoparticle ink was bar-coated twice with a thickness of 70 μm per pass and dried at room temperature to prepare Comparative Example 1-1.

[0113] [Comparative Example 1-2] Laser-irradiated copper nanoparticle film

[0114] Comparative Example 1-2 with a size of 1 mm x 0.1 mm was prepared by irradiating the copper nanoparticle film of Comparative Example 1-1 with a green laser of 532 nm wavelength at various irradiation speeds and powers.

[0116] [Comparative Examples 1-3] Copper nanoparticle film

[0117] Comparative Example 1-3 was prepared by coating copper nanoparticles with a size of 20 mm x 20 mm and drying at room temperature using the same method as Comparative Example 1-1, except that slide glass was used instead of a 75 μm thick Kapton HN film in the method of Comparative Example 1-1.

[0119] [Comparative Example 1-4] Heat-treated copper nanoparticle film

[0120] The copper nanoparticle films of Comparative Examples 1-3 were subjected to furnace heat treatment in an argon (Ar) atmosphere. The heat treatment was carried out for 1 hour at temperatures of 350°C, 400°C, and 450°C, respectively.

[0122] Figure 2 is a graph showing the electrical conductivity according to the laser conditions of Comparative Examples 1-2. Referring to Figure 2, only when the laser is irradiated at a low power intensity of 1.75 W or less and a high irradiation speed of 800 mm / sec or more (low transmitted light energy) is 10 4 Conductivity of S / cm or higher is possible, and when a laser is irradiated with higher power intensity and lower irradiation speed (higher transmitted light energy), 10 is achieved due to the formation of an additional oxide film. 4 Electrical conductivity was limited to S / cm or less.

[0123] For example, 0.45×10 after a laser process with an intensity of 2.35 W and an irradiation speed of 1000 mm / sec 4 Electrical conductivity was measured at S / cm, and 0.37×10⁻⁶ after laser processing at an intensity of 1.7 W and an irradiation speed of 600 mm / sec. 4 The electrical conductivity in S / cm was measured.

[0124] Copper nanoparticles that have not undergone surface treatment (adsorption of organic molecules containing carboxylic acids X, hereinafter referred to as surface treatment) exhibit 10 only in a very narrow intensity and irradiation rate range (conditions of low transmitted light energy). 4 It can be seen that it exhibits electrical conductivity greater than S / cm, and under conditions of high transmitted light energy, it becomes oxidized upon laser irradiation and fails to exhibit high electrical conductivity.

[0126] Figures 3a and 3b are graphs showing the results of analyzing Comparative Example 1-2 using XPS (X-ray Photoelectron Spectroscopy).

[0127] Referring to Fig. 3a, it can be seen that copper nanoparticles are oxidized when irradiated with a laser under high intensity conditions (2.35 W, 1000 mm / sec). Also, referring to Fig. 3b, it can be seen that copper nanoparticles are oxidized after laser sintering under low irradiation speed conditions (1.7 W, 600 mm / sec).

[0128] Figure 3c shows the results of calculating the ratio of each composition through the results of X-ray Photoelectron Spectroscopy (XPS) analysis of Comparative Examples 1-2.

[0129] Referring to Fig. 3c, it can be seen that a large amount of oxide film was formed under both conditions, with the specific gravity of copper oxide (CuO, Cu2O) after laser sintering being 50.1 at% under high intensity conditions (2.35 W, 1000 mm / sec) and the specific gravity of copper oxide (CuO, Cu2O) after laser sintering being 37.1 at% under low irradiation rate conditions (1.7 W, 600 mm / sec).

[0131] Figure 4 is an image of Comparative Example 1-2 (laser conditions: 1.7 W, 600 mm / sec) taken with a scanning electron microscope (SEM). According to Figure 4, Comparative Example 1-2 contains copper nanoparticles that have not been surface-treated with an organic molecule containing a carboxylic acid, and it can be seen that the density is not high because a sufficient calcination reaction does not occur due to the oxide film formed upon laser irradiation.

[0133] [Example 1-1] Copper nanoparticle film surface-functionalized with formic acid

[0134] Preparation Example 1 was dispersed in an ethanol solvent at a concentration of 20 wt%, and formic acid (FA) corresponding to 3 wt% of the nanoparticles was added and stirred for 30 minutes to prepare a copper nanoparticle ink adsorbed with formic acid, and then Example 1-1 was prepared by the same process as Comparative Example 1-1.

[0136] [Examples 1-2] Laser irradiation of copper nanofilms surface-functionalized with formic acid

[0137] In Example 1-1, a 1 mm x 0.1 mm irradiated pattern was prepared by irradiating a laser at various intensities and irradiation speeds.

[0139] [Examples 1-3] General heat treatment of copper nanoparticle films surface-functionalized with formic acid

[0140] Example 1-3 was prepared by coating copper nanoparticles with a size of 20 mm x 20 mm and drying at room temperature using the same method as Example 1-1, except that a slide glass was used instead of a 75 μm thick Kapton HN film in the method of Example 1-1.

[0142] [Examples 1-4] General heat treatment of copper nanoparticle films surface-functionalized with formic acid

[0143] Furnace heat treatment was performed on the films of Examples 1-3 in an Ar atmosphere. The heat treatment temperatures were 350°C, 400°C, and 450°C, and heat sintering was performed for 1 hour.

[0145] FIG. 5 is a graph showing the electrical conductivity according to the laser conditions of Examples 1-2. Referring to FIG. 5, even when the laser is irradiated at a low intensity of 2.35 W or less and a high irradiation speed of 600 mm / sec or more, 10 4 Conductivity of S / cm or higher is achievable. It can be confirmed that the additional oxide film formed can be removed when irradiated with a high-intensity, low-velocity laser, and that high conductivity can be achieved even when irradiated with a low-intensity, high-velocity laser. For example, 1.17×10⁻⁶ after a laser process with an intensity of 2.35 W and an irradiation speed of 1000 mm / sec, where an additional oxide film may form. 4 Electrical conductivity was measured at S / cm, and 1.29×10⁻⁶ after laser processing at an intensity of 1.7 W and an irradiation speed of 600 mm / sec. 4 The electrical conductivity in S / cm was measured.

[0147] Figure 6 is an image of Example 1-2 (laser conditions: 1.7 W, 600 mm / sec) taken with a scanning electron microscope (SEM). According to Figure 6, it can be confirmed that the light irradiation reaction is sufficiently completed through the removal of the oxide film, and a microstructure with very high density is formed.

[0149] [Example 2-1] Copper nanofilm surface-functionalized with propionic acid

[0150] Copper nanoparticles from Preparation Example 1 were dispersed in an ethanol solvent at a concentration of 20 wt%, and propionic acid (PA) corresponding to 3 wt% of the nanoparticles was added and stirred for 30 minutes to prepare a copper nanoparticle functional ink adsorbed with propionic acid. Subsequently, Example 2-1 was prepared by the same process as Comparative Example 1-1.

[0152] [Example 2-2] Laser irradiation of copper nanofilm surface-functionalized with propionic acid

[0153] In Example 2-1, a 1 mm x 0.1 mm irradiated pattern was prepared by irradiating a laser at various power intensities and irradiation speeds.

[0155] Figure 7 is a graph showing the electrical conductivity according to the laser conditions of Example 2-2. Referring to Figure 7, even when the laser is irradiated at a low power intensity of 2.35 W or less and a high irradiation speed of 600 mm / sec or more, 10 4 Conductivity of S / cm or higher can be achieved. It can be confirmed that the additionally formed oxide film can be removed when irradiated with a laser of high power intensity and low irradiation speed, and that high conductivity can be achieved even when irradiated with a laser of low power intensity and high irradiation speed. For example, after a laser process at an intensity of 2.35 W and an irradiation speed of 1000 mm / sec, where an additional oxide film may form, 1.42 × 10⁻⁶ 4 Electrical conductivity was measured at S / cm, and 1.40×10⁻⁶ after laser processing at an intensity of 1.7 W and an irradiation speed of 600 mm / sec. 4 The electrical conductivity in S / cm was measured.

[0157] Figures 8a and 8b are graphs showing the results of analyzing Example 2-2 using XPS (X-ray Photoelectron Spectroscopy).

[0158] Referring to Fig. 8a, it was confirmed that almost no oxide film was formed on the copper nanoparticles after laser sintering under high power intensity conditions (2.35 W, 1000 mm / sec), and referring to Fig. 8b, it was confirmed that almost no oxide film was present on the copper nanoparticles even after laser sintering at a low irradiation speed (1.7 W, 600 mm / sec).

[0159] Figure 8c shows the results of calculating the ratio of each composition through the X-ray Photoelectron Spectroscopy (XPS) analysis of Example 2-2.

[0160] Referring to Fig. 8c, it was confirmed that the specific gravity of copper oxide (CuO, Cu2O) after laser sintering under high power intensity conditions (2.35 W, 1000 mm / sec) was 16.2 at%, and the specific gravity of copper oxide (CuO, Cu2O) after laser sintering under low irradiation speed conditions (1.7 W, 600 mm / sec) was 21.2 at%.

[0162] Figure 9 is a scanning electron microscope (SEM) image of Example 2-2 (laser conditions: 1.7 W, 600 mm / sec). According to Figure 9, it can be confirmed that a microstructure with very high density was formed after photocalcination was performed by irradiating with a laser at 1.7 W and 600 mm / sec. This means that the oxide film was efficiently removed by propionic acid, allowing a sufficient calcination reaction to occur, and as a result, the density was dramatically improved.

[0164] [Example 3-1] Copper nanofilm surface-functionalized with butyric acid

[0165] Copper nanoparticles from Preparation Example 1 were dispersed in an ethanol solvent at a concentration of 20 wt%, and butyric acid (BA) corresponding to 3 wt% of the nanoparticles was added and stirred for 30 minutes to prepare a copper nanoparticle functional ink adsorbed with butyric acid. Subsequently, a film was prepared by the same process as in Comparative Example 1-1.

[0167] [Example 3-2] Laser irradiation of copper nanofilms surface-functionalized with butyric acid

[0168] In Example 3-1, a 1 mm x 0.1 mm irradiated pattern was produced by irradiating a laser at various power intensities and irradiation speeds.

[0170] FIG. 10 is a graph showing the electrical conductivity according to the laser conditions of Example 3-2. Referring to FIG. 10, even when the laser is irradiated at a low power intensity of 1.7 W or less and a high irradiation speed of 600 mm / sec or more, 10 4 Conductivity of S / cm or higher is achievable. It can be confirmed that the removal of the additionally formed oxide film is limited when irradiated with a high-intensity, low-velocity laser, and that high conductivity is possible even when irradiated with a low-power, high-velocity laser. For example, 1.13×10⁻⁶ after a laser process at an intensity of 2.35 W and an irradiation speed of 1000 mm / sec, where an additional oxide film may form 4 Electrical conductivity was measured at S / cm, and 1.36×10⁻⁶ after laser processing at an intensity of 1.7 W and an irradiation speed of 600 mm / sec. 4 The electrical conductivity in S / cm was measured.

[0171] In other words, although copper nanoparticles surface-treated with butyric acid exhibit electrical conductivity under broad laser irradiation conditions and can be seen as removing the oxide film, copper nanoparticles surface-treated with formic acid or propionic acid exhibit higher electrical conductivity under broader laser irradiation conditions, indicating that they have a superior effect in inhibiting oxide film formation.

[0173] Figure 11 is an image of Example 3-2 (laser conditions: 1.7 W, 600 mm / sec) taken with a scanning electron microscope (SEM). According to Figure 11, it can be confirmed that a high-density microstructure was formed after photolithography.

[0175] [Comparative Example 2-1] Oleic acid-surface-functionalized copper nanofilms

[0176] Copper nanoparticles from Preparation Example 1 were dispersed in an ethanol solvent at a concentration of 20 wt%, and oleic acid (OA) corresponding to 3 wt% of the nanoparticles was added and stirred for 30 minutes to prepare a copper nanoparticle ink adsorbed with oleic acid. Subsequently, a film was prepared by the same process as in Comparative Example 1-1.

[0178] [Comparative Example 2-2] Laser irradiation of oleic acid-surface-functionalized copper nanofilms

[0179] In Comparative Example 2-1, a 1 mm x 0.1 mm irradiated pattern was prepared by irradiating a laser with various intensities and irradiation speeds.

[0181] FIG. 12 is a graph showing the electrical conductivity of Comparative Example 2-2 according to laser conditions. Referring to FIG. 12, Comparative Example 2-2 is 0.6×10⁻⁶ under all laser conditions. 4 It exhibited low conductivity of less than S / cm. This is because bulky oleic acid cannot be adsorbed onto the surface of copper nanoparticles due to steric resistance with polyvinylpyrrolidone (PVP) present on the surface. Consequently, oleic acid carbonizes while adsorbed onto the functional groups of PVP, preventing it from acting as a functional group that reduces the oxide film.

[0183] Figure 13 is an image of Comparative Example 2-2 (laser conditions: 1.7 W, 600 mm / sec) taken with a scanning electron microscope (SEM). According to Figure 13, the rough areas on the surface of the copper nanoparticle film are carbonized oleic acid adsorbed on PVP.

[0185] [Characterization] Comparison of Conductivity Between Heat-Treated Copper Nanofilms and Laser-Treated Copper Nanofilms

[0186] The copper nanoparticle films of Comparative Example 1 and Example 1 were sintered through laser heat treatment in air or high-temperature (furnace) heat treatment in an argon (Ar) atmosphere, and then their conductivity was measured.

[0188] Heat treatment conditions atmosphere Sample Evangelism (10 4 S / cm) 1.7 W, 600 mm / sec air Comparative Example 1-2 0.37 2.35 W, 1000 mm / sec air Comparative Example 1-2 0.45 350 ℃ inert gas (Ar) Comparative Examples 1-4 - 400 ℃ inert gas (Ar) Comparative Examples 1-4 1.45 450 ℃ inert gas (Ar) Comparative Examples 1-4 4.28

[0189] Referring to Table 1, when a film prepared using copper nanoparticles not surface-treated with organic molecules containing carboxylic acids was subjected to laser heat treatment in air, 0.45 x 10⁻⁶ was obtained under high power intensity conditions (2.35 W, 1000 mm / sec) and low irradiation rate conditions (1.7 W, 600 mm / sec) where an additional oxide film was formed. 4 Low conductivity of less than S / cm was measured. This implies that light irradiation is limited by the additional oxide film formed during the laser sintering process.

[0190] In addition, as a result of high-temperature heat treatment in an Ar atmosphere for 1 hour, no electrical conductivity was measured at 350 ℃, and 1.45 x 10⁻⁶ due to high-temperature heat treatment at 400 ℃ and 450 ℃ 4 S / cm, 4.28 x 10 4 An electrical conductivity of S / cm was measured. This implies that the PVP capping agent present on the surface of copper nanoparticles cannot burn through heat treatment for 1 hour at a temperature below 350 ℃, and that thermal decomposition can occur at high temperatures above 400 ℃.

[0192] Sintering conditions atmosphere Sample Evangelism (10 4 S / cm) 1.7 W, 600 mm / sec air Examples 1-2 1.29 2.35 W, 1000 mm / sec air Examples 1-2 1.17 350 ℃ inert gas (Ar) Examples 1-4 0.59 400 ℃ inert gas (Ar) Examples 1-4 5.08 450 ℃ inert gas (Ar) Examples 1-4 9.65

[0193] Referring to Table 2, when films prepared using formic acid-surface-functionalized copper nanoparticles were subjected to laser heat treatment in air, 1.29 x 10⁻⁶ were formed under high power intensity conditions (2.35 W, 1000 mm / sec) and low irradiation speed conditions (1.7 W, 600 mm / sec), respectively, where an additional oxide film was formed. 4 S / cm, 1.17 x 10 4 A high conductivity of S / cm was measured. This implies that the additional oxide film formed during the laser sintering process can be effectively reduced by formic acid.

[0194] In addition, as a result of performing high-temperature heat treatment in an Ar atmosphere, 0.59 x 10⁻⁶ after high-temperature heat treatment at 350 ℃4 An electrical conductivity of S / cm is measured, and after high-temperature heat treatment at 400 ℃ and 450 ℃, 5.08 x 10 4 S / cm, 9.65 x 10 4 High electrical conductivity of S / cm is measured.

[0195] The results in Tables 1 and 2 show that at 350 ℃, PVP is not effectively thermally decomposed, but the oxide film is removed by formic acid, and the copper nanoparticle film is partially sintered, improving electrical conductivity. This implies that when heat treatment is performed at high temperatures of 400 ℃ and 450 ℃, the capping agent is thermally decomposed through the heat treatment, and at the same time, the oxide film is reduced by formic acid, allowing the copper nanoparticle film to be effectively thermally sintered.

[0197] [Characterization] Evaluation of Long-term Stability of Surface-Treated Copper Nanoparticles

[0198] Copper nanoparticles without oxide film formation from Preparation Example 1 and copper nanoparticles from Examples 1-1, 2-1, and 3-1 were stored in air for 30 days, and then a copper nanoparticle film was prepared using the same process as in Comparative Example 1-1. A laser was irradiated onto the copper nanoparticle film at an intensity of 1.5 W and an irradiation speed of 800 mm / sec to produce a light-irradiated pattern of 1 mm x 0.1 mm.

[0199] Sample Electrical conductivity (10 4 S / cm) Storage X1.5 W 800 mm / sec After 30 days 1.5 W, 800 mm / sec Preparation Example 1 1.17 0.53 (45.30%) Example 1-1 1.51 1.42 (94.0%) Example 2-1 1.41 1.31 (92.9%) Example 3-1 1.29 1.10 (85.2%)

[0200] Referring to Table 3, the copper nanoparticles of Preparation Example 1 oxidized during storage for 30 days and exhibited low conductivity after light irradiation. This suggests that the long-term storage stability of untreated copper nanoparticles is poor.

[0201] On the other hand, in the case of Examples 1-1, 2-1, and 3-1, which were surface-treated with formic acid, propionic acid, and butyric acid, even if oxidation occurred during storage, the organic molecules containing carboxylic acids (formic acid, propionic acid, and butyric acid) reduced the oxide film during the light irradiation process, so the film produced after light irradiation exhibited high conductivity similar to that of a film prepared using copper nanoparticles that were not stored for a long period. In other words, copper nanoparticles surface-treated with organic molecules containing carboxylic acids have excellent long-term storage stability.

[0203] As described above, although the present invention has been explained by limited embodiments and drawings, the present invention is not limited to the above embodiments, and various modifications and variations are possible from this description by those skilled in the art to which the present invention belongs. Therefore, the scope of the present invention should not be limited to the described embodiments, but should be defined by the claims set forth below as well as equivalents thereof.

Claims

Claim 1 A method for manufacturing a conductive metal film comprising: a step of preparing a metal nanoparticle ink by mixing an organic molecule containing a carboxylic acid having 1 to 17 carbon atoms into a solution in which metal nanoparticles are dispersed; a step of preparing a metal nanoparticle film by applying the metal nanoparticle ink to a substrate; and a step of heat-treating the metal nanoparticle film, wherein the metal nanoparticles are bonded to a capping agent, the capping agent is a polymer or organic molecule containing a pyridine functional group, the organic molecule containing the carboxylic acid includes formic acid, propionic acid, or butyric acid, and the organic molecule containing the carboxylic acid is adsorbed on the surface of the metal nanoparticles to perform the role of inhibiting the oxidation reaction of the metal nanoparticles and reducing the surface oxide film. Claim 2 A method for manufacturing a conductive metal film according to claim 1, characterized in that the metal nanoparticle comprises any one selected from copper, nickel, tin, iron, aluminum, molybdenum, tungsten, gallium, indium, and alloy compositions thereof. Claim 3 A method for manufacturing a conductive metal film according to claim 2, wherein the capping agent prevents the metal nanoparticles from coming into contact with moisture or oxygen and performs the role of improving the dispersibility of the metal nanoparticles. Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 A method for manufacturing a conductive metal film according to claim 1, wherein the step of heat-treating the metal nanoparticle film is selected from the group consisting of high temperature (furnace) heat treatment, laser irradiation heat treatment, white light irradiation heat treatment, plasma heat treatment, microwave heat treatment, and Joule heating. Claim 8 A method for manufacturing a conductive metal film according to claim 7, wherein in the heat treatment step, the laser irradiation heat treatment, white light irradiation heat treatment, plasma heat treatment, and microwave heat treatment are performed in air. Claim 9 A method for manufacturing a conductive metal film according to claim 8, characterized in that the laser is irradiated with a power of 0.5 W to 20 W. Claim 10 A method for manufacturing a conductive metal film according to claim 8, characterized in that the scanning speed of the laser is 100 mm / sec to 2,000 mm / sec. Claim 11 A conductive metal film prepared according to claim 1, comprising: metal nanoparticles; and an organic molecule comprising a carboxylic acid having 1 to 17 carbon atoms adsorbed on the metal nanoparticles, wherein the metal nanoparticles are bonded to a capping agent, the capping agent is a polymer or organic molecule comprising a pyridine functional group, the organic molecule comprising the carboxylic acid comprises formic acid, propionic acid, or butyric acid, the organic molecule comprising the carboxylic acid prevents the formation of an oxide film on the metal nanoparticles and removes the formed oxide film even if the oxide film is formed, and the organic molecule comprising the carboxylic acid is adsorbed on the surface of the metal nanoparticles and performs the role of inhibiting the oxidation reaction of the metal nanoparticles and reducing the surface oxide film. Claim 12 A conductive metal film according to claim 11, characterized in that the organic molecule containing the carboxylic acid is adsorbed on the surface of the metal nanoparticle. Claim 13 In claim 11, the electrical conductivity of the conductive metal film prepared using the metal nanoparticles stored in air for 1 to 60 days is 1.10 × 10⁻⁶ 4 S / cm to 9.07 × 10 4 A conductive metal film characterized by having S / cm.

Citation Information

Patent Citations

  • Fabrication Method of Conductive Metal Film with Light Sintering

    KR1020160010359A

  • Liquid metal-based electrode and manufacturing method thereof

    KR1020230171195A