Resin composition for a dicing film substrate, dicing film substrate, and dicing film
A resin composition combining ethylene-unsaturated carboxylic acid copolymers and styrene-based elastomers addresses the elongation and modulus strength issues of dicing films, enhancing chip handling and yield in semiconductor manufacturing.
Patent Information
- Application Number
- KR1020257007753
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-09
- Filing Date
- 2023-08-29
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-08-29
AI Technical Summary
Existing dicing films lack sufficient room temperature and low temperature elongation, leading to chip damage and decreased product yield during the pickup process, and conventional formulations are difficult to form into films due to high polyamide content.
A resin composition comprising an ethylene-unsaturated carboxylic acid copolymer, an ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, and a styrene-based elastomer, with specific ratios and degrees of neutralization, to achieve both modulus strength and elongation at room and low temperatures.
The composition results in a dicing film substrate with enhanced elongation and modulus strength at room and low temperatures, preventing chip damage and improving product yield.
Smart Images

Figure 112026054460135-PCT00002
Abstract
Description
Technology Field
[0001] The present invention relates to a resin composition for a dicing film substrate, a dicing film substrate, and a dicing film. Background Technology
[0002] In the manufacturing process of semiconductor devices such as ICs (integrated circuits), it is common practice to thin a semiconductor wafer with a circuit pattern formed thereon and then perform a dicing process to divide the semiconductor wafer into chip units. In the dicing process, a flexible wafer processing film (also referred to as a "dicing film" in this specification) is attached to the back side of the semiconductor wafer, and the semiconductor wafer is divided into chip units by means of a dicing blade or laser light. Then, through an expansion process, the dicing film is expanded to widen the spacing between chips and reduce the size of the chips. In the expansion process, for example, an expansion table placed beneath the dicing film is pushed up to expand the dicing film and divide the chips.
[0003] Afterwards, in the pickup process, only the desired chips are picked up from the dicing film and used for the desired purpose. In the pickup process, it is common to pick up only the desired chips from the dicing film side by poking them up with a fine pin.
[0004] Here, as a material constituting a dicing film, an ionomer in which an ethylene-(meth)acrylic acid copolymer is cross-linked with metal ions is known. For example, Patent Document 1 describes an antistatic resin containing a polyether component and a radiation-curable adhesive tape for wafer processing containing the ionomer. Patent Document 2 describes a resin composition for a dicing film substrate comprising the ionomer and a copolymer of ethylene, (meth)acrylic acid, and (meth)acrylic acid alkyl ester.
[0005] In addition, an ionomer / polyamide blend comprising an ionomer of a copolymer of ethylene and an α,β-ethylene unsaturated carboxylic acid and a polyamide is described in Patent Document 3 as a resin composition used for molded parts, etc. Prior art literature
[0006] Japanese Patent Publication No. JP2011-210887, Japanese Patent Publication No. JP2012-89732, Japanese Patent Publication No. JP2000-516984 The problem to be solved
[0007] Here, in the pickup process described above, in order to properly pick up only the desired chips, it is important that the dicing film surrounding the chips is sufficiently stretched (hereinafter also referred to as "room temperature elongation"). If the dicing film is not sufficiently stretched and multiple chips are pierced up by the micro-pins, a phenomenon may occur where chips that are not the target of pickup are peeled off from the dicing film. Furthermore, if the room temperature elongation of the dicing film is low, stress is applied to the chips during the pickup process, and damage may occur within the chips. If such problems occur, the product yield decreases or product defects increase.
[0008] However, Patent Document 1 does not contain a description focusing on the elongation of the adhesive tape for wafer processing itself. In addition, Patent Document 2 evaluates the heat resistance of the dicing film (e.g., elongation at 120°C), but does not focus on the elongation at room temperature. Furthermore, the ionomer / polyamide formulation of Patent Document 3 is difficult to form into a film because it contains a large amount of polyamide.
[0009] In addition, in addition to the room temperature elongation mentioned above, the resin composition for the dicing film substrate requires modulus strength of the dicing film at room temperature or low temperature, and in some cases, additional elongation at low temperature is also required. Specifically, in the case of a dicing-die bond integrated film, there is a process of separating and expanding the chip and die bond film at low temperature, and modulus strength required for separation and film elongation required for expansion are required. Furthermore, at room temperature, modulus strength to maintain a constant chip gap after separation and film elongation required during the pickup process as described above are required. However, conventionally, there has never been an attempt to achieve both modulus strength at room temperature or low temperature and elongation at room temperature and low temperature simultaneously.
[0010] The present invention has been made in consideration of the above problems. It aims to provide a resin composition for a dicing film substrate, a dicing film substrate, and a dicing film capable of realizing a dicing film substrate having excellent elongation at room temperature and low temperature, and furthermore, excellent modulus strength at room temperature and low temperature. means of solving the problem
[0011] That is, the present invention provides a resin composition for a dicing film substrate as follows.
[0012] [1] A resin composition for a dicing film substrate comprising an ionomer of an ethylene-unsaturated carboxylic acid copolymer (A), an ionomer of an ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer (B), and a styrene-based elastomer (C).
[0013] [2] A resin composition for a dicing film substrate described in [1], wherein the amount of a constituent unit derived from unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 1% or more and 30% or less of the total amount of constituent units of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer.
[0014] [3] A resin composition for a dicing film substrate described in [1] or [2], wherein the amount of a constituent unit derived from unsaturated carboxylic acid in the ionomer (B) of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is 1% or more and 30% or less with respect to the amount of a precursor unit of the ionomer (B) of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer.
[0015] [4] A resin composition for a dicing film substrate described in any one of [1] to [3], wherein the degree of neutralization of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 10% or more and 90% or less.
[0016] [5] A resin composition for a dicing film substrate described in any one of [1] to [4], wherein the degree of neutralization of the ionomer (B) of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is 10% or more and 90% or less.
[0017] [6] A resin composition for a dicing film substrate described in any one of [1] to [5], wherein the mass of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and the ionomer (B) of the ethylene-unsaturated carboxylic acid ester copolymer is 1, and the mass of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 0.10 or more and 0.95 or less.
[0018] [7] A resin composition for a dicing film substrate described in any one of [1] to [6], wherein the total mass of the ethylene-unsaturated carboxylic acid copolymer ionomer (A), the ethylene-unsaturated carboxylic acid ester copolymer ionomer (B), and the styrene-based elastomer (C) is 1, and the total mass of the ethylene-unsaturated carboxylic acid copolymer ionomer (A) and the ethylene-unsaturated carboxylic acid ester copolymer ionomer (B) is 0.60 or more and less than 1.00.
[0019] [8] A resin composition for a dicing film substrate described in any one of [1] to [7], wherein the total mass of the resin components included in the resin composition for a dicing film substrate is 100 mass%, and the ratio of the total mass of the ionomer of the ethylene-unsaturated carboxylic acid copolymer (A), the ionomer of the ethylene-unsaturated carboxylic acid ester copolymer (B), and the styrene-based elastomer (C) is 50 mass% or more and 100 mass% or less.
[0020] [9] A resin composition for a dicing film substrate as described in any one of [1] to [8], wherein the total mass of the resin components included in the resin composition for a dicing film substrate is 100 mass%, and the total content of the ionomer of the ethylene-unsaturated carboxylic acid copolymer (A), the ionomer of the ethylene-unsaturated carboxylic acid ester copolymer (B), and the styrene-based elastomer (C) is greater than 90 mass% and less than or equal to 100 mass%.
[0021]
[10] A resin composition for a dicing film substrate as described in any one of [1] to [9], having a melt flow rate of 0.1 g / 10 min or more and 30 g / 10 min or less when measured at 190°C and a load of 2160 g in accordance with JIS K 7210:1999.
[0022] The present invention provides the following dicing film substrate and dicing film.
[0023]
[11] A dicing film substrate having at least one layer comprising a resin composition for a dicing film substrate described in any one of [1] to
[10] above.
[0024]
[12] A dicing film substrate described in
[11] , wherein the average value of the 30% modulus in the MD direction and the 30% modulus in the TD direction measured at 23°C in accordance with JIS K 7127:1999 is 8 MPa or more and 17 MPa or less.
[0025]
[13] A dicing film substrate described in
[11] or
[12] , wherein the average value of the 10% modulus in the MD direction and the 10% modulus in the TD direction measured at -15°C in accordance with JIS K 7127:1999 is 20 MPa or more, comprising the resin composition for the dicing film substrate above.
[0026]
[14] A dicing film having a dicing film substrate described in
[11] above and an adhesive layer laminated on at least one side of the dicing film substrate. Effects of the invention
[0027] According to the resin composition for a dicing film substrate of the present invention, a dicing film substrate having excellent elongation at room temperature and low temperature, and furthermore, excellent modulus strength at room temperature and low temperature is realized. Specific details for implementing the invention
[0028] In this specification, a numerical range expressed using "~" refers to a range that includes the values listed before and after "~" as lower and upper limits. Additionally, "(meth)acrylic acid" is a notation used to include both "acrylic acid" and "methacrylic acid," and "(meth)acrylate" is a notation used to include both "acrylate" and "methacrylate."
[0029] 1. Regarding the resin composition for the dicing film substrate
[0030] The resin composition for a dicing film substrate of the present invention (hereinafter also simply referred to as the “resin composition”) is mainly used as a substrate for a dicing film, but the use of the resin composition is not limited to a substrate for a dicing film.
[0031] As explained above, substrates for dicing films require not only modulus strength at room and low temperatures but also elongation at room and low temperatures. However, conventionally, no attempt has been made to achieve both.
[0032] In this regard, the inventors have carefully examined the present invention and found that a resin composition comprising an ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer, an ionomer (B) of an ethylene-unsaturated carboxylic acid ester copolymer, and a styrene-based elastomer (C) results in a dicing film substrate that combines modulus strength at room temperature and low temperature with elongation at room temperature and low temperature. The reason for this is not clear, but it is presumed as follows. For example, if the resin composition includes an ionomer (A) of an ethylene-unsaturated carboxylic acid copolymer (hereinafter also simply referred to as "binary ionomer (A)"), the cohesive strength (rigidity) of the resin composition is improved, and thus the low-temperature modulus of the dicing film obtained from the resin composition is improved. In addition, if the resin composition includes an ionomer (B) of an ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer (hereinafter also simply referred to as "ternary ionomer (B)"), the room temperature modulus and room temperature elongation obtained from the resin composition are improved because unsaturated carboxylic acid esters are included. In addition, if the resin composition includes a styrene-based elastomer (C), the compatibility between the binary ionomer (A) and the ternary ionomer (B) is improved, so the room temperature modulus and room temperature elongation obtained from the resin composition are improved. On the other hand, if these are included alone, it is difficult to achieve good low-temperature elongation of the dicing film. However, when these are combined, the binary ionomer (A), the ternary ionomer (B), and the styrene-based elastomer (C) are uniformly mixed, and as compatibility is improved, low-temperature elongation is also improved, so a dicing film substrate is obtained that combines modulus strength at room temperature and low temperature and elongation at room temperature and low temperature.
[0033] Below, each component included in the resin composition is described, and then the physical properties of the resin composition are described.
[0034] <Ionomer of ethylene-unsaturated carboxylic acid copolymer (A)>
[0035] The binary ionomer (A) is a copolymer of ethylene and an unsaturated carboxylic acid, that is, an ethylene-unsaturated carboxylic acid copolymer in which some or all of the acid is neutralized by metal ions, and has a structure in which multiple ethylene-unsaturated carboxylic acid copolymers are cross-linked. The resin composition may contain only one type of the binary ionomer (A) or may contain two or more types.
[0036] The ethylene-unsaturated carboxylic acid copolymer that forms the main framework of the binary ionomer (A) mainly comprises ethylene and unsaturated carboxylic acid. Within a range that does not impair the purpose and effect of the present invention, it may include a structure derived from a monomer other than ethylene and unsaturated carboxylic acid in part, for example, with respect to the amount of precursor units of the ethylene-unsaturated carboxylic acid copolymer, it may include a structure derived from another monomer in an amount of 20 mass% or less. However, in this specification, the ethylene-unsaturated carboxylic acid polymer does not include a structure derived from an unsaturated carboxylic acid ester.
[0037] In the ethylene-unsaturated carboxylic acid copolymer, the amount of ethylene-derived constituent units is not limited, but the amount of ethylene-derived constituent units is preferably 70 mass% or more and 99 mass% or less relative to the amount of precursor units of the ethylene-unsaturated carboxylic acid copolymer, more preferably 75 mass% or more and 95 mass% or less, and even more preferably 78 mass% or more and 90 mass% or less. If the amount of ethylene-derived constituent units is 70 mass% or more, it becomes difficult for blocking or the like to occur in the resulting dicing film. On the other hand, if the amount of ethylene-derived constituent units is 99 mass% or less, the amount of unsaturated carboxylic acid becomes relatively sufficiently large, making it easy for modulus strength and elongation to be good.
[0038] Meanwhile, the amount of constituent units derived from unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer is not limited. The amount of constituent units derived from unsaturated carboxylic acid is preferably 1 mass% or more and 30 mass% or less relative to the amount of precursor units of the ethylene-unsaturated carboxylic acid copolymer, more preferably 5 mass% or more and 25 mass% or less, and even more preferably 10 mass% or more and 22 mass% or less. If the amount of constituent units derived from unsaturated carboxylic acid is 1 mass% or more, the modulus strength and elongation rate tend to be good. On the other hand, if the amount of constituent units derived from unsaturated carboxylic acid is 30 mass% or less, blocking or the like becomes less likely to occur in the resulting dicing film.
[0039] Examples of unsaturated carboxylic acids include unsaturated carboxylic acids having 4 to 8 carbon atoms, such as acrylic acid, methacrylic acid, ethacrylic acid, itaconic acid, itaconic anhydride, fumaric acid, crotonic acid, maleic acid, and maleic anhydride; among these, acrylic acid or methacrylic acid is preferred from the perspective of reactivity and availability. The ethylene-unsaturated carboxylic acid copolymer may contain only one type of constituent unit derived from these, or may contain two or more types.
[0040] As described above, the ethylene-unsaturated carboxylic acid copolymer may have one or more constituent units derived from monomers other than ethylene and unsaturated carboxylic acid. Examples of monomers other than ethylene and unsaturated carboxylic acid include unsaturated hydrocarbons such as propylene, butene, 1,3-butadiene, pentene, 1,3-pentadiene, and 1-hexene; vinyl esters derived from vinyl acetate, vinyl propionate, etc.; oxides such as vinyl sulfuric acid or vinyl nitric acid; halogen compounds such as vinyl chloride and vinyl fluoride; primary amine compounds containing vinyl groups; secondary amine compounds containing vinyl groups; carbon monoxide; sulfur dioxide; etc.
[0041] The above ethylene-unsaturated carboxylic acid copolymer may be a block copolymer or a random copolymer. In addition, the ethylene-unsaturated carboxylic acid copolymer may be a graft copolymer in which a known compound is additionally graft polymerized to a random polymer or a block polymer, provided that the purpose and effects of the present invention are not impaired.
[0042] In addition, in the binary ionomer (A), the metal ion that neutralizes the acid of the ethylene-unsaturated carboxylic acid copolymer is not particularly limited, but examples include lithium ions, sodium ions, potassium ions, rubidium ions, cesium ions, zinc ions, magnesium ions, manganese ions, etc. Among these, magnesium ions, sodium ions, or zinc ions are preferred from the standpoint of ease of availability, sodium ions or zinc ions are more preferred, and zinc ions are even more preferred.
[0043] The degree of neutralization of the ethylene-unsaturated carboxylic acid copolymer in the binary ionomer (A) is preferably 10% or more and 90% or less, more preferably 10% or more and 85% or less, and more preferably 15% or more and 82% or less. If the degree of neutralization of the ethylene-unsaturated carboxylic acid copolymer is 10% or more, the hardness of the substrate surface increases when the resin composition is used as a substrate for a dicing film. On the other hand, if the degree of neutralization is 90% or less, the processability and moldability of the resin composition improve. The degree of neutralization is the ratio of the mixing ratio of metal ions to the number of moles of acid groups (e.g., carboxyl groups) in the binary ionomer (A) (ethylene-unsaturated carboxylic acid copolymer). The unit is mol%. The degree of neutralization can be measured by infrared absorption spectrum (IR). By measuring the C=O stretching absorption peak of the resin using an infrared absorption spectrum, the non-ionized carboxyl groups can be quantified, and by measuring the C=O stretching absorption peak of the binary ionomer (A) treated with hydrochloric acid, the carboxyl groups of the entire resin can be quantified. By measuring both, the degree of neutralization can be determined and, specifically, calculated using the following formula.
[0044] Degree of neutralization (%) = (1 - P a1 / P a2 )×100
[0045] P a1 : C=O stretching absorption peak height of binary ionomer (A)
[0046] P a2 : Height of the C=O stretching absorption peak of hydrochloric acid-treated ethylene-unsaturated carboxylic acid copolymer
[0047] In addition, in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997) of the binary ionomer (A), the melt flow rate (MFR) measured at 190°C and a load of 2160g is preferably 0.2g / 10 min or more and 20.0g / 10 min or less, more preferably 0.5g / 10 min or more and 20.0g / 10 min or less, and more preferably 0.5g / 10 min or more and 18.0g / 10 min or less. If the melt flow rate of the binary ionomer (A) is within the above range, it becomes easier to mold the resin composition.
[0048] <Ionomer of ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer (B)>
[0049] The ternary ionomer (B) is a copolymer of ethylene, an unsaturated carboxylic acid, and an unsaturated carboxylic acid ester, i.e., an ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer in which some or all of the acids are neutralized by metal ions, and has a structure in which multiple ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymers are cross-linked. The resin composition may contain only one type of the ternary ionomer (B) or may contain two or more types.
[0050] The ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, which forms the main framework of the ternary ionomer (B), mainly comprises ethylene, unsaturated carboxylic acid, and unsaturated carboxylic acid ester. In a range that does not impair the purpose and effect of the present invention, it may include a structure derived from a monomer other than these in part, for example, with respect to the amount of precursor units of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, it may include a structure derived from another monomer in an amount of 20 mass% or less.
[0051] In the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, the amount of ethylene-derived constituent units is not limited, but the amount of ethylene-derived constituent units is preferably 60 mass% or more and 94 mass% or less with respect to the amount of precursor units of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, and more preferably 75 mass% or more and 90 mass% or less. If the amount of ethylene-derived constituent units is 60 mass% or more, it becomes difficult for blocking or the like to occur in the resulting dicing film. On the other hand, if the amount of ethylene-derived constituent units is 94 mass% or less, the amount of unsaturated carboxylic acid or unsaturated carboxylic acid ester becomes relatively sufficiently large, making it easy for modulus strength and elongation to be good.
[0052] Meanwhile, the amount of constituent units derived from unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is not limited. The amount of constituent units derived from unsaturated carboxylic acid is preferably 1 mass% or more and 30 mass% or less with respect to the amount of precursor units of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, and more preferably 5 mass% or more and 20 mass% or less. If the amount of constituent units derived from unsaturated carboxylic acid is 1 mass% or more, the modulus strength and elongation rate tend to be good. On the other hand, if the amount of constituent units derived from unsaturated carboxylic acid is 30 mass% or less, constituent units derived from ethylene or unsaturated carboxylic acid ester are relatively easily sufficiently included, and blocking or the like becomes difficult to occur in the dicing film.
[0053] Here, the type of unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is not particularly limited and is the same as the unsaturated carboxylic acid of the binary monomer ethylene-unsaturated carboxylic acid copolymer described above. The ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer may contain only one type of constituent unit derived from unsaturated carboxylic acid, or it may contain two or more types.
[0054] The amount of constituent units derived from unsaturated carboxylic acid esters in the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is not limited. The amount of constituent units derived from unsaturated carboxylic acid esters is preferably 1 mass% or more and 20 mass% or less with respect to the amount of precursor units of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, and more preferably 1 mass% or more and 15 mass% or less. If the amount of constituent units derived from unsaturated carboxylic acid is 1 mass% or more, the low-temperature elongation and room-temperature elongation of the substrate for the dicing film tend to be good. On the other hand, if the amount of constituent units derived from unsaturated carboxylic acid esters is 20 mass% or less, the composition derived from ethylene or unsaturated carboxylic acid tends to be sufficiently included relatively, making it difficult for blocking to occur in the dicing film.
[0055] In the above ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer, the unsaturated carboxylic acid ester includes a compound in which the carboxylic acid of the unsaturated carboxylic acid described above becomes a carboxylate. Examples of unsaturated carboxylic acid esters include alkyl group unsaturated carboxylic acid alkyl esters having 1 to 12 carbon atoms. The number of carbon atoms in the alkyl group is more preferably 1 to 8, and more preferably 1 to 4. Examples of alkyl groups include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, secondary butyl group, 2-ethylhexyl group, isooctyl group, etc.
[0056] Specific examples of the above unsaturated carboxylic acid alkyl esters include (meth)acrylic acid methyl ester, (meth)acrylic acid ethyl ester, (meth)acrylic acid isobutyl ester, acrylic acid n-butyl ester, acrylic acid isooctyl ester, maleic acid dimethyl ester, maleic acid diethyl ester, etc. The ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer may contain only one type of constituent unit derived from the unsaturated carboxylic acid ester, or may contain two or more types.
[0057] In addition, the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer may have one or more constituent units derived from monomers other than ethylene, unsaturated carboxylic acid, and unsaturated carboxylic acid ester. These are the same as other monomer-derived constituent units that the ethylene-unsaturated carboxylic acid copolymer may include.
[0058] The above ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer may be a block copolymer or a random copolymer. In addition, the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer may be a graft copolymer in which a known compound is additionally graft polymerized onto a random polymer or a block polymer, provided that the purpose and effects of the present invention are not impaired.
[0059] In addition, regarding the ternary ionomer (B), the metal ion that neutralizes the acid of the ethylene-unsaturated carboxylic acid copolymer is not particularly limited, but examples include lithium ions, sodium ions, potassium ions, rubidium ions, cesium ions, zinc ions, magnesium ions, manganese ions, etc. Among these, magnesium ions, sodium ions, or zinc ions are preferred from the perspective of ease of availability, sodium ions or zinc ions are more preferred, and zinc ions are even more preferred.
[0060] The degree of neutralization of the ethylene-unsaturated carboxylic acid copolymer in the ternary ionomer (B) is preferably 10% or more and 90% or less, more preferably 10% or more and 85% or less, and more preferably 15% or more and 82% or less. If the degree of neutralization of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is 10% or more, the hardness of the substrate surface increases when the resin composition is used as a substrate for a dicing film. On the other hand, if the degree of neutralization is 90% or less, the processability and moldability of the resin composition improve. The degree of neutralization is the ratio of the mixing ratio of metal ions to the number of moles of acid groups (e.g., carboxyl groups) in the ternary ionomer (B) (ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid copolymer). The unit is mol%. The degree of neutralization can be measured by infrared absorption spectrum (IR). By measuring the C=O stretching absorption peak of the resin using an infrared absorption spectrum, the non-ionized carboxyl groups can be quantified, and by measuring the C=O stretching absorption peak of the ternary ionomer (B) treated with hydrochloric acid, the carboxyl groups of the entire resin can be quantified. By measuring both, the degree of neutralization can be determined and, specifically, calculated using the following formula.
[0061] Degree of neutralization (%) = (1 - P b1 / P b2 )×100
[0062] P b1 : C=O stretching absorption peak height of ternary ionomer (B)
[0063] P b2 : Height of the C=O stretching absorption peak of hydrochloric acid-treated ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer
[0064] In addition, in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997) of the ternary ionomer (B), the melt flow rate (MFR) measured at 190°C and a load of 2160g is preferably 0.2g / 10 min or more and 20.0g / 10 min or less, more preferably 0.5g / 10 min or more and 20.0g / 10 min or less, and more preferably 0.5g / 10 min or more and 18.0g / 10 min or less. If the melt flow rate of the ternary ionomer (B) is within the above range, it becomes easier to mold the resin composition.
[0065] <Styrene-based elastomer (C)>
[0066] A styrene-based elastomer refers to a styrene-based polymer that is a rubber elastomer at room temperature. Examples of styrene-based elastomers include block copolymers comprising a hard segment made of a styrene block (styrene polymer) and a soft segment made of an alkylene block, or hydrogenated derivatives thereof; random copolymers of styrene and alkylene, or hydrogenated derivatives thereof; or acid-modified styrene-based elastomers obtained by acid-modifying the styrene-based elastomer.
[0067] In the above block copolymer, the styrene block may be a region formed by the polymerization of two or more styrenes, and the alkylene block may be a region formed by the polymerization of two or more alkenes. The alkylene block may be a homopolymer of one type of alkene or a copolymer of two or more types of alkenes.
[0068] Examples of the above block copolymers include styrene-butadiene block copolymer (SB), styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene block copolymer (SI), and styrene-isoprene-styrene block copolymer (SIS).
[0069] As explained above, the styrene-based elastomer may be a hydrogenated additive of the block copolymer. In the hydrogenated additive, both the styrene block and the alkylene block may be hydrogenated, only one of the styrene block or the alkylene block may be hydrogenated, and only a part of the styrene block and the alkylene block may be hydrogenated.
[0070] Specific examples of hydrogenated compounds of the above block copolymers include a styrene-ethylene-butylene block copolymer (SEB) which is a hydrogenated compound of a styrene-butadiene block copolymer (SB), a styrene-ethylene-butylene-styrene block copolymer (SEBS) which is a hydrogenated compound of a styrene-butadiene-styrene block copolymer (SBS), and a styrene-ethylene-propylene-styrene block copolymer (SEPS) which is a hydrogenated compound of a styrene-isoprene-styrene block copolymer (SIS).
[0071] As explained above, examples of styrene-based elastomers include random copolymers of styrene and alkylene. Examples include styrene-butadiene random copolymer, styrene-isoprene random copolymer, styrene-ethylene-butylene random copolymer, styrene-ethylene-propylene random copolymer, styrene-isobutylene random copolymer, styrene-ethylene-isoprene random copolymer, etc.
[0072] As explained above, the styrene-based elastomer may be a hydrogenated derivative of the random copolymer. Examples include a hydrogenated derivative of a styrene-butadiene random copolymer (HSBR).
[0073] In the styrene-based elastomer that has not undergone acid modification as described below, among the above, a hydrogenated material is preferred, and styrene-ethylene-butylene-styrene block copolymer (SEBS) and styrene-ethylene-propylene-styrene block copolymer (SEPS) are more preferred, and styrene-ethylene-butylene-styrene block copolymer (SEBS) is particularly preferred from the view that it can improve the low-temperature elongation and room-temperature elongation of a substrate for a dicing film obtained from a resin composition.
[0074] Meanwhile, the styrene-based elastomer may be an acid-modified styrene-based elastomer in which the elastomer consisting of the block copolymer or random polymer, or hydrogenated derivative thereof, as described above, is graft-modified by an unsaturated carboxylic acid or its derivative. The acid-modified styrene-based elastomer may be one in which the block copolymer or random polymer, or hydrogenated derivative thereof, is graft-modified by one unsaturated carboxylic acid or its derivative, or may be graft-modified by two or more unsaturated carboxylic acids or their derivatives.
[0075] Examples of unsaturated carboxylic acids grafted onto the above-mentioned block copolymer or random copolymer include (meth)acrylic acid, 2-ethylacrylic acid, crotonic acid, maleic acid, fumaric acid, itaconic acid, etc. Meanwhile, examples of unsaturated carboxylic acid derivatives grafted onto styrene-based elastomers include acid anhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride; acid esters such as monomethyl maleic acid and monoethyl maleic acid; acid amides; acid halides; etc. Among these, maleic acid or maleic anhydride is preferred from the perspective of reactivity with styrene-based elastomers, etc.
[0076] The above acid-modified styrene-based elastomer is obtained by graft polymerizing an unsaturated carboxylic acid or its derivative onto the above block copolymer or random copolymer, etc., in the presence of a radical initiator. The radical initiator may be any compound used in the graft reaction of a polyolefin, and any known compound may be used.
[0077] The acid value of the above acid-modified styrene-based elastomer is preferably greater than 0 mgCH3ONa / g and less than 20 mgCH3ONa / g, more preferably greater than 0 mgCH3ONa / g and less than 11 mgCH3ONa / g, and more preferably 0.5 mgCH3ONa / g or higher and 11 mgCH3ONa / g or lower. If the acid value of the acid-modified styrene-based elastomer is within this range, the elongation at low and room temperatures is likely to be good.
[0078] The melt flow rate of the styrene-based elastomer (C) is preferably 0.1 g / 10 min to 100 g / 10 min, more preferably 0.5 g / 10 min to 90 g / 10 min, more preferably 1.0 g / 10 min to 80 g / 10 min, and more preferably 2.0 g / 10 min to 75 g / 10 min. The melt flow rate is a value measured at 230°C and a load of 2160 g in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997).
[0079] The Tanδ peak temperature of the styrene-based elastomer (C) is preferably -60°C or higher, more preferably -55°C or higher, and more preferably -50°C or higher from the view that it can improve the low-temperature elongation or room-temperature elongation of the substrate for the obtained dicing film. The above Tanδ peak temperature is the temperature that shows a peak value in a dynamic viscoelasticity test (temperature-dependent measurement 10 Hz) in accordance with JIS K 6394 (equivalent to ISO 4664-1: 2005).
[0080] Other Polymers and Additives
[0081] The resin composition may include various additives, antistatic agents, ultraviolet absorbers, fillers, other polymers, etc., as needed, to the extent that it does not impair the effects of the present invention.
[0082] Examples of various additives include antioxidants, heat stabilizers, light stabilizers, pigments, dyes, lubricants, anti-blocking agents, antifungal agents, antibacterial agents, flame retardants, flame retardant aids, crosslinking agents, crosslinking aids, foaming agents, foaming aids, fiber reinforcing materials, etc. The content of the additive is preferably 20 parts by mass or less, and more preferably 18 parts by mass or less, when the total mass of the resin component included in the resin composition is 100 parts by mass.
[0083] In addition, examples of antistatic agents include low-molecular-weight antistatic agents and high-molecular-weight antistatic agents, with high-molecular-weight antistatic agents being preferred. In this specification, a high-molecular-weight antistatic agent is a copolymer comprising a conductive portion (e.g., a structural portion derived from polyether, a quaternary ammonium base portion, etc.) and a non-conductive portion (e.g., a structural portion derived from polyamide, a structural portion derived from polyolefin such as polyethylene, a structural portion derived from acrylate, a structural portion derived from methacrylate, a structural portion derived from styrene, etc.), and having a molecular weight of 300 or more (preferably 1,000 to 10,000). The molecular weight is the weight-average molecular weight of polystyrene equivalent measured by GPC. Furthermore, conductivity is defined as a surface resistivity of 10 as measured according to ASTM D257. 10 It refers to those having Ω / □ or less. Examples of the polymeric antistatic agent include vinyl copolymers having sulfonate groups within the molecule, alkylsulfonates, alkylbenzenesulfonates, betaine, etc. Other examples of polymeric antistatic agents include polyetheramide, polyetheresteramide, salts of inorganic protonate of polyetheramide, or salts of inorganic protonate of polyetheresteramide. Examples of salts of inorganic protonate include alkali metal salts, alkaline earth metal salts, zinc salts, or ammonium salts.
[0084] Examples of ultraviolet absorbers include benzophenone-based, benzoate-based, benzotriazole-based, cyanoacrylate-based, hindered amine-based, etc.
[0085] Examples of fillers include silica, clay, calcium carbonate, barium sulfate, glass beads, talc, etc.
[0086] The amounts of additives, antistatic agents, UV absorbers, and fillers are appropriately selected according to their type.
[0087] Examples of other polymers include polyolefins such as polyethylene and polypropylene, and polyamides. However, the amount of polyamide is preferably less than 5 parts by mass when the total mass of the resin components included in the resin composition is 100 parts by mass. It is preferable that the resin composition does not include polyamide as an other polymer.
[0088] Desirable composition
[0089] In the resin composition of the present invention, the amount of the binary ionomer (A) is preferably 10 mass% or more and 80 mass% or less with respect to the total amount of the resin composition, and more preferably 15 mass% or more and 75 mass% or less. In addition, the amount of the ternary ionomer (B) is preferably 10 mass% or more and 80 mass% or less with respect to the total amount of the resin composition, and more preferably 12 mass% or more and 75 mass% or less. In addition, the amount of the styrene-based elastomer (C) is preferably 5 mass% or more and 35 mass% or less with respect to the total amount of the resin composition, and more preferably 7 mass% or more and 32 mass% or less.
[0090] In addition, in the resin composition, when the total amount of binary ionomer (A) and ternary ionomer (B) is set to 1, the mass of binary ionomer (A) is preferably 0.10 or more and 0.95 or less, more preferably 0.15 or more and 0.90 or less, and more preferably 0.20 or more and 0.85 or less. Also, when the total mass of binary ionomer (A), ternary ionomer (B), and styrene-based elastomer (C) is set to 1, the total mass of binary ionomer (A) and ternary ionomer (B) is preferably 0.60 or more and less than 1.00, and more preferably 0.65 or more and 0.95 or less. In addition, when the total mass of the resin components included in the resin composition is 100 mass%, the total content of the binary ionomer (A), the ternary ionomer (B), and the styrene-based elastomer (C) is preferably 50 mass% or more and 100 mass% or less, more preferably 60 mass% or more and 100 mass% or less, more preferably 70 mass% or more and 100 mass% or less, more preferably 80 mass% or more and 100 mass% or less, more preferably exceeding 90 mass% and 100 mass% or less, more preferably exceeding 95 mass% and 100 mass% or less, more preferably exceeding 95 mass% and 100 mass% or less, more preferably 98 mass% or more and 100 mass% or less, and 99 mass% or more and 100 mass% It is more desirable to be less than this.
[0091] If these conditions are met, as explained, the film formability, modulus strength at room and low temperatures, and elongation at room and low temperatures are all improved.
[0092] In addition, when the total mass of the resin components included in the resin composition is 100 mass%, it is preferable to adjust the amount of each component so that the ratio of the “sum of the amount (mass) of the constituent unit derived from unsaturated carboxylic acid in the binary ionomer (A) and the amount (mass) of the constituent unit derived from unsaturated carboxylic acid in the ternary ionomer (B)” to the total mass of the resin components is 5 mass% or more and 20 mass% or less, it is more preferable to adjust the amount of each component so that it is 7 mass% or more and 15 mass% or less, and even more preferable to adjust the amount of each component so that it is 9 mass% or more and 13 mass% or less. If the amount of the constituent unit derived from unsaturated carboxylic acid in the resin composition is within the above range, the low-temperature modulus property is likely to be good.
[0093] In addition, when the total mass of the resin component included in the resin composition is 100 mass%, it is preferable to adjust the amount of each component so that the ratio of the “amount (mass) of constituent units derived from unsaturated carboxylic acid esters in the ternary ionomer (B)” to the total mass of the resin component is 0.5 mass% or more and 10 mass% or less, and it is more preferable to adjust the amount of each component so that it is 1 mass% or more and 8 mass% or less. If the amount of constituent units derived from unsaturated carboxylic acid esters in the resin composition is within the above range, the elongation at room temperature and low temperature is likely to be good.
[0094] In addition, the degree of neutralization of the carboxylic acid in the resin composition, that is, the degree of neutralization of the “unsaturated carboxylic acid in the binary ionomer (A) and the unsaturated carboxylic acid in the ternary ionomer (B)”, is preferably 40% or more and 90% or less, more preferably 45% or more and 85% or less, more preferably 50% or more and 80% or less, more preferably 55% or more and 75% or less, and more preferably 60% or more and 70% or less. The above degree of neutralization can be determined by calculating "a, the ratio of the mass of binary ionomer (A) to the total mass of binary ionomer (A) and ternary ionomer (B)" and "b, the ratio of the mass of ternary ionomer (B) to the total mass of binary ionomer (A) and ternary ionomer (B)" respectively, and by "degree of neutralization of binary ionomer (A) × a + degree of neutralization of ternary ionomer (B) × b". If the degree of neutralization of the unsaturated carboxylic acid in the entire resin composition is 40% or more, when the resin composition is used as a substrate for a dicing film, the modulus strength of the substrate film at room temperature and low temperature increases. On the other hand, if the degree of neutralization is 90% or less, the processability and moldability of the resin composition improve.
[0095] <Method for manufacturing resin composition and physical properties of resin composition>
[0096] The method for manufacturing the resin composition of the present invention is not particularly limited, and is not particularly limited as long as it is a method capable of mixing binary ionomers (A), ternary ionomers (B), and styrene-based elastomers (C), and additionally other polymers or additives as needed. For example, all components may be dry blended and then melt-kneaded, or some components may be kneaded first and then the next components added.
[0097] The shape of the resin composition after mixing is not particularly limited and, for example, may be in the form of pellets, or may be processed into a long sheet or a single-leaf sheet.
[0098] In accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997), the melt flow rate of the above resin composition, measured at 190°C and a load of 2160g, is preferably 0.1g / 10 min or more and 30g / 10 min or less, more preferably 0.2g / 10 min or more and 20g / 10 min or less, more preferably 0.3g / 10 min or more and 10g / 10 min or less, more preferably 0.4g / 10 min or more and 5g / 10 min or less, and more preferably 0.5g / 10 min or more and 3g / 10 min or less. If the melt flow rate of the resin composition falls within this range, the modulus strength at room temperature and low temperature and the elongation at room temperature of the substrate obtained from the resin composition are likely to be good.
[0099] 2. Dicing film substrate
[0100] The dicing substrate may be a substrate having at least one layer containing the resin composition described above. Since the dicing film substrate has a layer containing the resin composition described above, it exhibits excellent modulus strength and elongation at room temperature and low temperature. The dicing film substrate is preferably used as a substrate for a dicing film, but is not limited to such use.
[0101] The composition of the dicing film substrate is not particularly limited, and it may have only one layer containing the resin composition described above, or it may have two or more layers containing the resin composition described above. In addition, other resin layers may be laminated as needed.
[0102] Examples of dicing film substrates include: a laminate having a single-layer structure consisting only of a layer containing the resin composition described above; a laminate having a two-layer structure consisting of a layer containing the resin composition described above and another resin layer; a laminate having a three-layer structure consisting of a layer containing the resin composition described above, another resin layer, and a layer containing the resin composition described above. In addition, the dicing film substrate may additionally include a layer containing an adhesive or an adhesive sheet, etc.
[0103] Here, the layer comprising the resin composition described above may be a layer consisting only of the resin composition described above, or a layer comprising the resin composition described above and other components within a range that does not impair the purpose and effect of the present invention, but it is preferable from the viewpoint of the elongation and modulus strength of the dicing film substrate that it is substantially a layer consisting of the resin composition described above.
[0104] The thickness of the layer containing the resin composition described above is not particularly limited, but from the perspective of improving the strength, modulus strength, elongation, etc. of the dicing film substrate, it is preferable to have a thickness of 50 μm or more and 200 μm or less, and more preferable to have a thickness of 60 μm or more and 180 μm or less.
[0105] In addition, the average value of the 30% modulus in the MD direction (Machine Direction) and the 30% modulus in the TD direction (Transverse Direction) measured at 23°C of the layer containing the resin composition is preferably 8 MPa or more and 17 MPa or less, and more preferably 10 MPa or more and 15 MPa or less. If the average value of the 30% modulus at 23°C is within this range, the elongation of the dicing film substrate at room temperature is likely to be good. The above 30% modulus is a value measured by a Shimadzu desktop precision universal tester AG-X, which is a measuring device, in accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), by preparing a film with a thickness of 100 μm, a TD direction length of 10 mm, and an MD direction length of 180 mm, having the same composition as the layer containing the resin composition. The spacing between rods is 100 mm, and the test speed is 300 mm / min.
[0106] Meanwhile, the average value of the 10% modulus in the MD direction and the 10% modulus in the TD direction measured at -15°C of the layer containing the resin composition is preferably 20 MPa or higher, and more preferably 24 MPa or higher. If the average value of the 10% modulus at -15°C is 20 MPa or higher, the cleavage and elongation properties of the dicing film substrate at low temperatures tend to be good. The above 10% modulus is a value measured by a Shimadzu desktop precision universal testing machine AG-X, which is a measuring device, in accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), by preparing a film having the same composition as the layer containing the resin composition, with a thickness of 100 μm, a TD direction length of 10 mm, and an MD direction length of 180 mm. The chuck distance is set to 100 mm, and the test speed is set to 1000 mm / min.
[0107] It is preferable that the layer containing the resin composition be capable of measuring both the 200% modulus in the MD direction and the 200% modulus in the TD direction at 23°C. If both the 200% modulus in the MD direction and the 200% modulus in the TD direction at 23°C are measurable, it is difficult to apply stress to the chip during the pickup process, and thus it is difficult for breakage to occur within the chip. The above 200% modulus is a value measured by a Shimadzu desktop precision universal testing machine AG-X, which is a measuring device, in accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), by preparing a film having the same composition as the layer containing the resin composition, with a thickness of 100 μm, a length of 10 mm in the TD direction, and a length of 180 mm in the MD direction. The test speed is set to 300 mm / min.
[0108] It is preferable that the layer containing the resin composition be capable of measuring both the 200% modulus in the MD direction and the 200% modulus in the TD direction at -15°C. If both the 200% modulus in the MD direction and the 200% modulus in the TD direction at -15°C are measurable, it is easy to perform the splitting and expansion of the chip and die bond film well in the process of splitting and expanding at low temperatures. The above 200% modulus is a value measured by a Shimadzu desktop precision universal tester AG-X, which is a measuring device, in accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), by preparing a film with a thickness of 100 μm, a TD direction length of 10 mm, and an MD direction length of 180 mm, having the same composition as the layer containing the resin composition. The test speed shall be 1000 mm / min.
[0109] Meanwhile, examples of other resin layers include a layer comprising linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), ethylene-α-olefin copolymer, polypropylene, ethylene-unsaturated carboxylic acid copolymer or its ionomer, ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid alkyl ester ternary copolymer or its ionomer, ethylene-unsaturated carboxylic acid alkyl ester copolymer, ethylene-vinyl ester copolymer, ethylene-unsaturated carboxylic acid alkyl ester-carbon monoxide copolymer, unsaturated carboxylic acid grafts thereof, polyvinyl chloride, etc. The other resin layer may include only one type of the above resin, or may include two or more types.
[0110] The thickness of the other resin layer is not particularly limited, but from the viewpoint of not impairing the modulus strength or elongation of the layer containing the resin composition, it is preferably 10 μm or more and 100 μm or less, and more preferably 15 μm or more and 80 μm or less.
[0111] Here, considering that it is used as a component of the dicing film, the total thickness of the dicing film substrate is preferably 50 μm or more from the perspective of frame retention during dicing and 200 μm or less from the perspective of expandability.
[0112] The surface of the above-mentioned dicing film substrate may be subjected to various treatments, for example, corona treatment, etc. Additionally, electron beam irradiation, etc., may be performed.
[0113] The method of manufacturing the above-described dicing film substrate is not particularly limited and can be manufactured by known molding methods. For example, when manufacturing a dicing film substrate consisting only of a layer containing the resin composition described above, the resin composition, etc. can be molded by conventionally known T-die casting molding method, T-die nip molding method, inflation molding method, extrusion lamination method, calendering method, etc.
[0114] Meanwhile, if the dicing film substrate is a laminate of a layer containing the resin composition described above and a different resin layer, the resin different from the resin composition described above may be molded by a co-extrusion lamination method or the like. In addition, the layer containing the resin composition described above and the different resin layer may be manufactured separately and joined together by an adhesive or an adhesive sheet. Examples of materials for adhesives or adhesive sheets include various ethylene copolymers or unsaturated carboxylic acid grafts thereof. In addition, if the dicing film substrate is a laminate of a layer containing the resin composition described above and a different resin layer, either the layer containing the resin composition described above or the other resin layer may be formed first, and the other layer may be formed and laminated on the said layer by means of a T-die film forming machine, an extrusion coating forming machine, etc.
[0115] 3. Dicing film
[0116] The dicing film of the present invention may comprise the dicing film substrate described above and an adhesive layer laminated on at least one surface thereof, and may include other compositions as needed. In addition, when the dicing film substrate described above is made of multiple layers, it is preferable that a layer containing a resin composition within the dicing film substrate and an adhesive layer are laminated.
[0117] The adhesive constituting the adhesive layer may be an adhesive used for the adhesive layer of a general dicing film. Examples of adhesives include rubber-based, acrylic-based, silicone-based, and polyvinyl ether-based adhesives; radiation-curable adhesives; and heat-foaming adhesives. Among these, considering the peelability of the dicing film from the semiconductor wafer, it is preferable for the adhesive layer to include a radiation-curable adhesive, and it is more preferable for it to include a UV-curable adhesive.
[0118] UV-curing adhesives typically comprise a radical polymerizable compound capable of radical polymerization (which may be any of a monomer, oligomer, or polymer) and a photopolymerization initiator, and optionally include additives such as crosslinking agents, tackifiers, fillers, anti-aging agents, and colorants.
[0119] Examples of radical polymerizable compounds include monomers or oligomers of (meth)acrylate alkyl esters such as (meth)acrylate methyl, (meth)acrylate ethyl, (meth)acrylate butyl, (meth)acrylate 2-ethylhexyl, (meth)acrylate octyl, (meth)acrylate isononyl, etc.; monomers or oligomers of (meth)acrylate hydroxyalkyl esters such as (meth)acrylate hydroxyethyl, (meth)acrylate hydroxybutyl, (meth)acrylate hydroxyhexyl, etc.; A copolymer monomer or oligomer of the above (meth)acrylic acid alkyl ester and / or (meth)acrylic acid hydroxyalkyl ester and other monomers (e.g., (meth)acrylic acid, itaconic acid, maleic anhydride, (meth)acrylic acid amide, (meth)acrylic acid N-hydroxymethylamide, (meth)acrylic acid alkylaminoalkyl ester, vinyl acetate, styrene, acrylonitrile, etc.); (Meth)acrylic acid glycidyl ester, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol (meth)acrylate, neopentyl glycol di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ester monomers of (meth)acrylic acid and polyhydric alcohols, and their oligomers; isocyanurates such as 2-propenyldi-3-butenylcyanurate, 2-hydroxyethylbis(2-acryloxyethyl)isocyanurate, tris(2-acryloxyethyl)isocyanurate, and tris(2-methacryloxyethyl)isocyanurate are included.
[0120] Specific examples of photopolymerization initiators include benzoin alkyl ethers such as benzoin methyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; aromatic ketones such as α-hydroxycyclohexylphenyl ketone; aromatic ketales such as benzyl dimethyl ketal; and thioxantones such as polyvinylbenzophenone, chlorothioxantone, dodecylthioxantone, dimethylthioxantone, and diethylthioxantone.
[0121] Examples of crosslinking agents include polyisocyanate compounds, melamine resins, urea resins, polyamines, and carboxyl group-containing polymers.
[0122] The thickness of the adhesive layer is appropriately selected according to the type of adhesive, and is preferably 3 to 100 μm, and more preferably 3 to 50 μm.
[0123] Additionally, the adhesive layer of the dicing film may be protected by a separator. If the adhesive layer is protected by a separator, the surface of the adhesive layer can be kept smooth. Furthermore, while facilitating the handling and transportation of the dicing film, it also becomes possible to process labels on the separator. The separator peels off when the dicing film is used.
[0124] The separator may be paper, or a synthetic resin film such as polyethylene, polypropylene, or polyethylene terephthalate. Additionally, to improve peelability from the adhesive layer, the surface of the separator in contact with the adhesive layer may be subjected to release treatments such as silicone treatment or fluorine treatment as necessary. The thickness of the separator is typically 10 to 200 μm, preferably 25 to 100 μm.
[0125] The method of manufacturing the above dicing film is not particularly limited, and, for example, it may be manufactured by applying an adhesive to the dicing substrate described above using a known method. At this time, the application of the adhesive may be carried out by a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, etc. In addition, an adhesive layer may be formed by applying an adhesive to a release sheet and transferring the adhesive layer to the dicing film substrate, thereby laminating the dicing film substrate and the adhesive layer. In addition, the dicing film substrate and the adhesive layer may be formed simultaneously by co-extrusion, etc.
[0126] Examples
[0127] The present invention will be described below with reference to examples. The scope of the present invention is not to be interpreted as limited by the examples.
[0128] [Preparation of materials]
[0129] Each component used the following.
[0130] <Ionomer of ethylene-unsaturated carboxylic acid copolymer (A)>
[0131] IO1: Ionomer of ethylene-methacrylic acid copolymer (content of constituent units derived from ethylene: 85 mass%, content of constituent units derived from methacrylic acid: 15 mass%, degree of neutralization: 59% zinc, MFR measured at 190°C and 2160g load in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997): 8.9g / 10 min)
[0132] IO2: Ionomer of ethylene-methacrylic acid copolymer (content of constituent units derived from ethylene: 80 mass%, content of constituent units derived from methacrylic acid: 20 mass%, degree of neutralization: 40% zinc, MFR measured at 190°C and 2160g load in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997): 8.0g / 10 min)
[0133] <Ionomer of ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer (B)>
[0134] IO3: Ionomer of ethylene-methacrylic acid-acrylic acid butyl ester copolymer (content of constituent units derived from ethylene: 80 mass%, content of constituent units derived from methacrylic acid: 10 mass%, content of constituent units derived from acrylic acid butyl ester: 10 mass%, degree of neutralization: 70% zinc, MFR measured at 190°C and 2160g load in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997): 1g / 10 min)
[0135] <Styrene-based elastomer (C)>
[0136] · Styrene-based elastomer 1:SEBS (Styrene-ethylene-butylene-styrene block copolymer (SOES1611 (trademark), a product of Asahi Kasei Chemicals Co., Ltd., MFR measured at 230℃ and 2160g load: 12.0g / 10min, Tanδ peak temperature: 9℃ in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997))
[0137] ·Styrene-based Elastomer 2: SEBS (Styrene-ethylene-butylene-styrene block copolymer (Toughtec H1221 (trademark), a product of Asahi Kasei Chemicals, MFR measured at 230°C and 2160g load: 4.5g / 10 min, Tanδ peak temperature: -19°C in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997))
[0138] ·Styrene-based Elastomer 3: SEBS (Styrene-ethylene-butylene-styrene block copolymer (Toughtec H1062 (trademark), a product of Asahi Kasei Chemicals, MFR measured at 230°C and 2160g load in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997): 4.5g / 10min, Tanδ peak temperature: -47°C)
[0139] ·Styrene-based Elastomer 4: SEBS (Styrene-ethylene-butylene-styrene block copolymer (Toughtac H1041 (trademark), a product of Asahi Kasei Chemicals, MFR measured at 230°C and 2160g load in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997): 5.0g / 10min, Tanδ peak temperature: -45°C)
[0140] · Styrene-based Elastomer 5: HSBR (Hydrogenated styrene-butadiene random copolymer (Dynalon 1320P, a JSR product (trademark), MFR measured at 230°C and 2160g load in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997): 3.5g / 10 min, Tanδ peak temperature: -15°C)
[0141] ·Styrene-based elastomer 6: SEPS (Styrene-ethylene·propylene-styrene block copolymer (Curareau product, Septon 2002, in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997), MFR measured at 230℃ and 2160g load: 70.0g / 10min)
[0142] [Examples 1–11 and Comparative Examples 1–5]
[0143] An ionomer of an ethylene-unsaturated carboxylic acid copolymer (A), an ionomer of an ethylene-unsaturated carboxylic acid ester copolymer (B), and a styrene-based elastomer (C) were dry blended at the ratios (mass ratios) shown in Table 1. Next, the dry-blended mixture was fed into the resin inlet of a 30 mmφ twin-screw extruder and melt-kneaded at a die temperature of 230°C to obtain a resin composition for a dicing film substrate. For the obtained resin composition for a dicing film substrate, the MFR was measured at 190°C and a load of 2160 g in accordance with JIS K 7210:1999 (equivalent to ISO 1133:1997). The results are shown in Table 1.
[0144] [evaluation]
[0145] The obtained resin composition for the dicing film substrate was molded using a 40 mmφ T-die film molding machine at a processing temperature of 230°C to produce a T-die film with a thickness of 100 μm. The obtained T-die film was used as a dicing film substrate and evaluated by the following method.
[0146] In addition, the total amount of constituent units derived from unsaturated carboxylic acids was calculated from the sum of “content ratio of binary ionomer (A) × amount of constituent units derived from carboxylic acids in binary ionomer (A)” and “content ratio of ternary ionomer (B) × amount of constituent units derived from carboxylic acids in ternary ionomer (B)”.
[0147] The total amount of constituent units derived from unsaturated carboxylic acid esters was calculated from “content ratio of ternary ionomer (B) × amount of constituent units derived from carboxylic acid esters in ternary ionomer (B)”.
[0148] The degree of neutralization (mol%) was determined by “degree of neutralization of binary ionomer (A) × (ratio of the amount of binary ionomer (A) to the total amount of binary ionomer (A) and ternary ionomer (B))” + “degree of neutralization of ternary ionomer (B) × (ratio of the amount of ternary ionomer (B) to the total amount of binary ionomer (A) and ternary ionomer (B))”. In addition, “total amount of constituent units derived from unsaturated carboxylic acid × degree of neutralization / 100” was calculated. Each result is shown in Table 1.
[0149] (1) Room temperature modulus strength
[0150] The above dicing film substrate was cut into a short sheet with a width of 10 mm × a length of 180 mm. In accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), a Shimadzu desktop precision universal testing machine AG-X was used as a measuring device to measure the 30% modulus at 23°C for the MD direction (Machine Direction) and TD direction (Transverse Direction) of the sample (dicing film substrate), respectively. The chuck distance was 100 mm, and the test speed was 300 mm / min.
[0151] The 30% modulus in the MD direction and the 30% modulus in the TD direction obtained from the above test were averaged, and the room temperature modulus strength of the dicing film substrate was evaluated according to the following criteria.
[0152] A (Good): 10MPa or higher and 15MPa or lower
[0153] B (Slightly Good): 8MPa or higher but less than 10MPa, or greater than 15MPa but less than or equal to 17MPa
[0154] C (Defective): Less than 8MPa, or greater than 17MPa
[0155] (2) Low temperature modulus strength
[0156] The above dicing film substrate was cut into a single piece with a width of 10 mm × a length of 180 mm. In accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), a Shimadzu desktop precision universal testing machine AG-X was used as a measuring device, and the 10% modulus was measured for the MD direction and TD direction of the sample (dicing film substrate) at -15°C. The chuck distance was set to 100 mm, and the test speed was set to 1000 mm / min.
[0157] The 10% modulus in the MD direction and the 10% modulus in the TD direction obtained by the above test were averaged, and the low-temperature modulus strength of the dicing film substrate was evaluated according to the following criteria.
[0158] A (Good): 24 MPa or higher
[0159] B (Slightly Good): 20MPa or higher and less than 24MPa
[0160] C (Defective): Less than 20MPa
[0161] (3) Room temperature extensibility
[0162] The above dicing film substrate was cut into a single sheet with a width of 10 mm × a length of 180 mm. In accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), a Shimadzu desktop precision universal tester AG-X was used as a measuring device to measure the 200% modulus at 23°C for each of the MD direction and TD direction of the measurement target.
[0163] Based on the obtained measurement results, the room temperature elongation of the dicing film substrate was evaluated according to the following criteria.
[0164] A (Good): Measurable 200% modulus at 23℃
[0165] C (Defective): The dicing film substrate broke during measurement, making it impossible to measure the 200% modulus at 23℃.
[0166] (4) Low temperature elongation
[0167] The dicing film substrate was cut into a single sheet measuring 10 mm in width × 180 mm in length. In accordance with JIS K 7127:1999 (equivalent to ISO 527-3:1995), the Shimadzu desktop precision universal tester AG-X was used as a measuring device to measure the 200% modulus at -15°C for the MD direction and TD direction of the measurement target, respectively.
[0168] Based on the obtained measurement results, the low-temperature elongation of the dicing film substrate was evaluated according to the following criteria.
[0169] A (Good): Measurable 200% modulus at -15℃
[0170] C (Defective): The dicing film substrate broke during measurement, making it impossible to measure the 200% modulus at -15℃.
[0171] [Table 1]
[0172]
[0173] As shown in Table 1, in Comparative Example 1, which does not contain a ternary ionomer (B) and a styrene-based elastomer (C), the room temperature modulus strength, room temperature elongation, and low temperature elongation were low, and in Comparative Example 2, the room temperature modulus strength and room temperature elongation were low.
[0174] Meanwhile, in Comparative Example 3, which does not include binary ionomer (A) and styrene-based elastomer (C), low-temperature elongation was low. Also, in Comparative Example 4, which does not include styrene-based elastomer (C), low-temperature elongation was low. Also, in Comparative Example 5, which does not include ternary ionomer (B), low-temperature elongation was low.
[0175] In contrast, in the dicing film substrate using the resin composition of Examples 1 to 11, which includes a binary ionomer (A), a ternary ionomer (B), and a styrene-based elastomer (C), the room temperature modulus strength, low temperature modulus strength, room temperature elongation, and low temperature elongation were excellent (Examples 1 to 11). By combining the binary ionomer (A), the ternary ionomer (B), and the styrene-based elastomer (C), the binary ionomer (A), the ternary ionomer (B), and the styrene-based elastomer (C) are uniformly mixed, so that not only do the modulus strength and room temperature elongation at room temperature or low temperature complement each other, but the low temperature elongation is also very good.
[0176] From the above results, it was confirmed that according to the resin composition for a dicing film substrate of the present invention, a dicing film substrate with excellent room temperature modulus strength, low temperature modulus strength, room temperature elongation, and low temperature elongation can be realized.
[0177] This application claims priority based on Japanese Patent Application No. 2022-144100 filed on September 9, 2022. All contents described in the specification of said application are incorporated by reference into this specification. Industrial applicability
[0178] According to the resin composition for a dicing film substrate of the present invention, a dicing film substrate is realized that has excellent elongation at room temperature and low temperature, and furthermore, excellent modulus strength at room temperature and low temperature. Therefore, it is very useful in the field of manufacturing semiconductor devices.
Claims
Claim 1 A resin composition for a dicing film substrate comprising an ionomer of an ethylene-unsaturated carboxylic acid copolymer (A), an ionomer of an ethylene-unsaturated carboxylic acid ester copolymer (B), and a styrene-based elastomer (C), wherein when the total mass of the resin components included in the resin composition for a dicing film substrate is 100 mass%, the total content of the ionomer of the ethylene-unsaturated carboxylic acid copolymer (A), the ionomer of the ethylene-unsaturated carboxylic acid ester copolymer (B), and the styrene-based elastomer (C) is greater than 90 mass% and less than or equal to 100 mass%. Claim 2 A resin composition for a dicing film substrate according to claim 1, wherein the amount of a constituent unit derived from an unsaturated carboxylic acid in the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 1 mass% or more and 30 mass% or less with respect to the amount of a precursor unit of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer. Claim 3 A resin composition for a dicing film substrate according to claim 1, wherein the amount of a constituent unit derived from unsaturated carboxylic acid in the ionomer (B) of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is 1 mass% or more and 30 mass% or less with respect to the amount of a precursor unit of the ionomer (B) of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer. Claim 4 A resin composition for a dicing film substrate according to claim 1, wherein the degree of neutralization of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 10% or more and 90% or less. Claim 5 A resin composition for a dicing film substrate according to claim 1, wherein the degree of neutralization of the ionomer (B) of the ethylene-unsaturated carboxylic acid-unsaturated carboxylic acid ester copolymer is 10% or more and 90% or less. Claim 6 A resin composition for a dicing film substrate according to claim 1, wherein, when the total mass of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer and the ionomer (B) of the ethylene-unsaturated carboxylic acid ester copolymer is set to 1, the mass of the ionomer (A) of the ethylene-unsaturated carboxylic acid copolymer is 0.10 or more and 0.95 or less. Claim 7 A resin composition for a dicing film substrate according to claim 1, wherein, when the total mass of the ethylene-unsaturated carboxylic acid copolymer ionomer (A), the ethylene-unsaturated carboxylic acid ester copolymer ionomer (B), and the styrene-based elastomer (C) is set to 1, the total mass of the ethylene-unsaturated carboxylic acid copolymer ionomer (A) and the ethylene-unsaturated carboxylic acid ester copolymer ionomer (B) is 0.60 or more and less than 1.
00. Claim 8 A resin composition for a dicing film substrate according to claim 1, wherein, in accordance with JIS K 7210:1999, the melt flow rate measured at 190°C and a load of 2160g is 0.1g / 10 min or more and 30g / 10 min or less. Claim 9 A dicing film substrate having at least one layer comprising a resin composition for a dicing film substrate described in any one of claims 1 to 8. Claim 10 A dicing film substrate according to claim 9, wherein the average value of the 30% modulus in the MD direction and the 30% modulus in the TD direction, measured at 23°C in accordance with JIS K 7127:1999, is 8 MPa or more and 17 MPa or less. Claim 11 A dicing film substrate according to claim 9, wherein the average value of the 10% modulus in the MD direction and the 10% modulus in the TD direction measured at -15℃ in accordance with JIS K 7127:1999 is 20 MPa or more, of the layer comprising the resin composition for the dicing film substrate. Claim 12 A dicing film having a dicing film substrate described in claim 9 and an adhesive layer laminated on at least one surface of the dicing film substrate. Claim 13 delete Claim 14 delete
Citation Information
Patent Citations
Dicing sheet
JP2015109436A
Resin composition for dicing film base, dicing film base and dicing film
JP2017098369A