Method for manufacturing lithium secondary battery

By optimizing the electrolyte injection and pre-charge/discharge cycles in the manufacturing process, the frictional force between the battery case and electrode assembly is enhanced, addressing the vulnerability of pouch-type lithium secondary batteries to external impacts and preventing electrolyte leakage.

KR103047156B1Active Publication Date: 2026-11-11LG ENERGY SOLUTION LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020230188479
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-12-23
Filing Date
2023-12-21
Publication Date
2026-11-11
Estimated Expiration
2043-12-21

AI Technical Summary

Technical Problem

Pouch-type lithium secondary batteries are vulnerable to external impact due to low frictional force between the battery case and the electrode assembly, leading to potential electrolyte leakage and damage during harsh conditions.

Method used

A manufacturing method that ensures a specific relationship between the amount of electrolyte injected per unit capacity (a) and the number of pre-charge/discharge cycles (b) is established, adhering to the formula 15 ≤ 486.77 - 373.09 × e^(-0.006b) × a^0.29 ≤ 30, enhancing the frictional force between the battery case and the electrode assembly.

Benefits of technology

The method significantly increases the frictional force to 15 kgf or more, preventing electrolyte leakage and detachment of the electrode assembly during external impacts, thereby improving the impact resistance of the lithium secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023143936016-PAT00001_ABST
    Figure 112023143936016-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a lithium secondary battery, wherein the method for manufacturing a lithium secondary battery of the present invention comprises: a first step of preparing a battery case; a second step of assembling a battery cell by placing an electrode assembly in the battery case and injecting an electrolyte such that the mass of the electrolyte per unit capacity is a (g / Ah); a third step of activating the battery cell; and a fourth step of pre-charging and discharging the activated battery cell b times, and satisfies the following equation (1). Equation (1): 15 ≤ 486.77 - 373.09 × e(-0.006b)× a0.29≤ 30 In the above formula (1), a is an integer from 2.0 to 3.0 and b is an integer from 0 to 3.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a lithium secondary battery, and more specifically, to a method for manufacturing a lithium secondary battery with excellent impact resistance. Background Technology

[0003] A lithium secondary battery is generally manufactured by applying an electrode active material slurry to a positive electrode current collector and a negative electrode current collector to produce a positive electrode and a negative electrode, and then stacking them on both sides of a separator to form an electrode assembly of a predetermined shape, after which the electrode assembly is housed in a pouch and an electrolyte is injected.

[0004] Secondary batteries are classified into pouch type and can type depending on the material of the case housing the electrode assembly. Among these, pouch-type secondary batteries are manufactured by forming a cup portion through press processing on a flexible pouch film laminate, housing the electrode assembly in the cup portion, injecting an electrolyte, and then sealing the sealing portion; meanwhile, can-type secondary batteries are manufactured by housing the electrode assembly in a metal can, injecting an electrolyte, and then sealing the can by assembling a top cap on the top.

[0005] Pouch-type rechargeable batteries offer advantages such as lightweight design, excellent space efficiency, and the ability to achieve high energy density using stacked electrode assemblies; however, they have the drawback of being vulnerable to external impact compared to can-type rechargeable batteries. As the usage environments for rechargeable batteries have recently become more diverse, there is a growing demand for them to possess excellent safety even in harsh conditions; consequently, improvements in the impact resistance of pouch-type rechargeable batteries are required. The problem to be solved

[0007] The present invention is intended to solve the above-mentioned problems and relates to a method for manufacturing a lithium secondary battery in which the frictional force between the battery case and the electrode assembly is increased by ensuring that the amount of electrolyte injected and the number of pre-charge / discharge cycles satisfy a specific relationship during battery manufacturing. means of solving the problem

[0009] In one aspect, the present invention provides a method for manufacturing a lithium secondary battery satisfying the following formula (1), comprising: a first step of preparing a battery case; a second step of assembling a battery cell by placing an electrode assembly in the battery case and injecting an electrolyte such that the mass of the electrolyte per unit capacity is a (g / Ah); a third step of activating the battery cell; and a fourth step of pre-charging and discharging the activated battery cell b times.

[0010] Equation (1): 15 ≤ 486.77 - 373.09 × e (-0.006b) × a 0.29 ≤ 30

[0011] In the above formula (1), a is an integer of 2.0 to 3.0, preferably 2.0 to 2.5, and b is an integer of 0 to 3.

[0012] Preferably, the method for manufacturing the lithium secondary battery may satisfy the following formula (1-1).

[0013] Equation (1-1): 15 ≤ 486.77 - 373.09 × e (-0.006b) × a 0.29 ≤ 27

[0014] In the above equation (1-1), a and b are the same as in equation (1).

[0016] Meanwhile, in the fourth step above, the pre-charge / discharge can be performed in the SOC 0 to 99 range with a C-rate of 0.1C to 1C.

[0017] Preferably, the pre-charge / discharge can be performed in a voltage range of 2.50V to 4.35V.

[0019] Meanwhile, the third step of activating the battery cell may include a step of charging and discharging the battery cell.

[0020] Meanwhile, in the present invention, the battery case may be a pouch comprising a barrier layer, a substrate layer formed on one side of the barrier layer, and a sealant layer formed on the other side of the barrier layer, and at least one cup portion indented in one direction.

[0021] In addition, the ratio of the length to the width of the electrode assembly may be 5 to 10, for example, the length may be 400 mm to 600 mm and the width may be 50 to 150 mm.

[0022] The lithium secondary battery of the present invention manufactured by the above method may have a frictional force between the inner surface of the battery case and the electrode assembly of 15 kgf or more, preferably 15 kgf to 30 kgf.

[0023] In addition, when the lithium secondary battery of the present invention manufactured by the method described above is subjected to a crash shock test under a collision condition of 133.7G × 15.8ms, no electrolyte leakage occurs. That is, the amount of electrolyte leakage is 0.

[0024] In addition, the above lithium secondary battery may have a rated capacity of 50Ah to 200Ah. Effects of the invention

[0026] As in the present invention, when a battery is manufactured such that the amount of electrolyte injected and the number of pre-charge / discharge cycles satisfy a specific relationship, the frictional force between the electrode assembly and the inner surface of the battery case increases significantly compared to conventional methods, and as a result, the detachment of the electrode assembly and / or electrolyte leakage during external impact is suppressed, thereby significantly improving the impact resistance of the lithium secondary battery.

[0027] The lithium secondary battery of the present invention manufactured according to the above method exhibits a high frictional force of 15 kgf or more between the electrode assembly and the battery case, and accordingly, when a crash shock test is performed under a collision condition of 133.7 G × 15.8 ms, no electrolyte leakage occurs due to damage to the battery case. Brief explanation of the drawing

[0029] FIG. 1 is a flowchart showing a method for manufacturing a lithium secondary battery according to the present invention. FIG. 2 is an exploded perspective view of a secondary battery according to one embodiment of the present invention. FIG. 3 is a cross-sectional view of a pouch according to one embodiment of the present invention. Figure 4 is a diagram showing the results of measuring the frictional force of secondary batteries manufactured according to the methods of Examples 1 to 4. Figure 5 is a diagram showing the results of measuring the frictional force of secondary batteries manufactured according to the methods of Comparative Examples 1 to 2 and Examples 5 to 6. Specific details for implementing the invention

[0030] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0032] The present invention will be explained in more detail below through specific embodiments.

[0033] Recently, as the demand for high-capacity batteries, such as those for electric vehicles, has increased, the rated capacity of secondary battery cells has been rising, leading to a trend of increasing electrode assembly weight. However, as the weight of the electrode assembly increases, the phenomenon of the assembly shifting upon external impact to damage or pierce the battery case is becoming more severe. If such pouch damage occurs, electrolyte leakage or deformation of the electrode assembly may result, causing serious problems with battery performance and safety.

[0035] As a result of repeated research to solve this problem, the inventors discovered that the amount of electrolyte injected (a) and the number of pre-charge / discharge cycles (b) are closely related to the frictional force between the battery case and the electrode assembly. Specifically, the inventors discovered that when a and b satisfy a specific relationship, the frictional force between the electrode assembly and the battery case increases significantly compared to conventional methods, thereby suppressing damage to the battery case caused by the detachment of the electrode assembly during external impact, and thus enabling excellent impact resistance, and completed the present invention.

[0037] Specifically, the method for manufacturing a lithium secondary battery according to the present invention comprises: a first step of preparing a battery case; a second step of assembling a battery cell by placing an electrode assembly in the battery case and injecting an electrolyte such that the mass of the electrolyte per unit capacity is a (g / Ah); a third step of activating the battery cell; and a fourth step of pre-charging and discharging the activated battery cell b times, wherein a and b satisfy the following formula (1), preferably the following formula (1-1).

[0038] Equation (1): 15 ≤ 486.77 - 373.09 × e (-0.006b) × a 0.29 ≤ 30

[0039] Equation (1-1): 15 ≤ 486.77 - 373.09 × e(-0.006b) × a 0.29 ≤ 27

[0040] In the above equations (1) and (1-1), a is an integer from 2.0 to 3.0 and b is an integer from 0 to 3.

[0041] When manufacturing a battery, if the amount of electrolyte injected per unit capacity a and the number of pre-charge / discharge cycles b satisfy the relationship of Equation (1) or Equation (1-1), the frictional force between the battery case and the electrode assembly increases significantly to 15 kgf or more, and accordingly, the impact resistance is greatly improved.

[0043] FIG. 1 illustrates a method for manufacturing a lithium secondary battery according to the present invention, FIG. 2 illustrates a perspective view of a secondary battery according to one embodiment of the present invention, and FIG. 3 illustrates a cross-sectional view of a battery case (pouch). The present invention will be described in more detail below with reference to FIG. 1 to FIG. 3.

[0045] Method for manufacturing a lithium secondary battery

[0046] First, a method for manufacturing a lithium secondary battery according to the present invention will be described.

[0048] Step 1: Battery Case Preparation Step

[0049] First, a battery case accommodating an electrode assembly and an electrolyte is prepared (S1). At this time, the battery case may preferably be a pouch, but is not limited thereto, and may be a prismatic or cylindrical battery case.

[0050] Referring to FIGS. 2 and 3, the battery case may be a pouch (100) comprising a barrier layer (20), a substrate layer (10) formed on one side of the barrier layer, and a sealant layer (30) formed on the other side of the barrier layer, and at least one cup portion (110) indented in one direction.

[0051] Specifically, the pouch (100) has flexibility and can be manufactured by inserting a pouch film laminate, in which a substrate layer (10), a barrier layer (20), and a sealant layer (30) are sequentially laminated, into a press forming device and applying pressure with a punch to a portion of the pouch film laminate to stretch it, thereby forming a cup portion with a shape indented in one direction.

[0052] The substrate layer (10) is placed on the outermost layer of the pouch to protect the electrode assembly from external shocks and to electrically insulate it.

[0053] The above substrate layer (10) may be made of a polymer material, for example, one or more polymer materials selected from the group consisting of polyethylene, polypropylene, polycarbonate, polyethylene terephthalate, polyvinyl chloride, acrylic polymer, polyacrylonitrile, polyimide, polyamide, cellulose, aramid, nylon, polyester, polyparaphenylenebenzobisoxazole, polyarylate, and Teflon.

[0054] The substrate layer (10) may be a single-layer structure, or a multi-layer structure in which different polymer films (12, 14) are laminated as shown in FIG. 3. If the substrate layer (10) is a multi-layer structure, an adhesive layer (16a) may be interposed between the polymer films.

[0055] Meanwhile, the substrate layer (10) may have an overall thickness of 10㎛ to 60㎛, preferably 20㎛ to 50㎛, and more preferably 30㎛ to 50㎛. If the substrate layer has a multilayer structure, the thickness includes the adhesive layer. When the substrate layer (10) satisfies the above range, excellent durability, insulation, and moldability are exhibited. If the substrate layer thickness is too thin, durability is reduced and damage to the substrate layer may occur during the molding process; if it is too thick, moldability may be reduced, the overall thickness of the pouch increases, and the battery receiving space decreases, which may result in a decrease in energy density.

[0056] According to one embodiment, the substrate layer (10) may be a laminated structure of a polyethylene terephthalate (PET) film and a nylon film. In this case, it is preferable that the nylon film is positioned toward the barrier layer (20), i.e., toward the inside, and the polyethylene terephthalate film is positioned toward the surface of the pouch.

[0057] Polyethylene terephthalate (PET) has excellent durability and electrical insulation properties, so when a PET film is placed on the surface side, excellent durability and insulation properties are exhibited. However, in the case of a PET film, the adhesion to the aluminum alloy thin film constituting the barrier layer (20) is weak and the stretching behavior is different; therefore, when a PET film is placed on the barrier layer side, delamination between the substrate layer and the barrier layer may occur during the molding process, and the barrier layer may not be stretched uniformly, resulting in a decrease in moldability. In contrast, since a nylon film has a stretching behavior similar to that of the aluminum alloy thin film constituting the barrier layer (20), an effect of improving moldability can be obtained when a nylon film is placed between the polyethylene terephthalate and the barrier layer.

[0058] The above polyethylene terephthalate film may have a thickness of 5㎛ to 20㎛, preferably 5㎛ to 15㎛, more preferably 7㎛ to 15㎛, and the above nylon film may have a thickness of 10㎛ to 40㎛, preferably 10㎛ to 35㎛, more preferably 15㎛ to 25㎛. When the thicknesses of the polyethylene terephthalate film and the nylon film satisfy the above ranges, excellent moldability and rigidity after molding are exhibited.

[0059] The barrier layer (20) is intended to secure the mechanical strength of the pouch (100), block the entry and exit of gases or moisture, etc., from outside the secondary battery, and prevent leakage of the electrolyte.

[0060] The above barrier layer (20) may have a thickness of 40㎛ to 100㎛, more preferably 50㎛ to 80㎛, and more preferably 60㎛ to 80㎛. When the thickness of the barrier layer satisfies the above range, moldability is improved, so the depth of molding of the cup portion is increased, and even when molding two cups, the occurrence of cracks and / or pinholes is reduced, thereby improving resistance to external stress after molding.

[0061] Meanwhile, the barrier layer (20) may be made of a metal material, specifically an aluminum alloy thin film.

[0062] The above aluminum alloy thin film may include aluminum and one or more metal elements other than aluminum, selected from the group consisting of iron (Fe), copper (Cu), chromium (Cr), manganese (Mn), nickel (Ni), magnesium (Mg), silicon (Si), and zinc (Zn).

[0063] Preferably, the aluminum alloy thin film may have an iron (Fe) content of 1.2 wt% to 1.7 wt%, preferably 1.3 wt% to 1.7 wt%, and more preferably 1.3 wt% to 1.45 wt%. When the iron (Fe) content in the aluminum alloy thin film satisfies the above range, the occurrence of cracks or pinholes can be minimized even when the cup portion is formed deeply.

[0064] The sealant layer (30) is bonded by heat pressing to seal the pouch and is located in the innermost layer of the pouch film laminate (1).

[0065] The sealant layer (30) must have insulating and corrosion-resistant properties because it is the surface that comes into contact with the electrolyte and electrode assembly after the pouch is formed, and must have high sealing properties because it must completely seal the inside to block material movement between the inside and the outside.

[0066] The sealant layer (30) may be made of a polymer material, for example, one or more selected from the group consisting of polyethylene, polypropylene, polycarbonate, polyethylene terephthalate, polyvinyl chloride, acrylic polymer, polyacrylonitrile, polyimide, polyamide, cellulose, aramid, nylon, polyester, polyparaphenylenebenzobisoxazole, polyarylate, and Teflon, and among these, it is particularly preferable to include polypropylene (PP), which has excellent mechanical properties such as tensile strength, rigidity, surface hardness, wear resistance, and heat resistance, and chemical properties such as corrosion resistance.

[0067] More specifically, the sealant layer (30) may comprise polypropylene, cast polypropylene (CPP), acid modified polypropylene, polypropylene-butylene-ethylene copolymer, or a combination thereof.

[0068] The sealant layer (30) may be a single-layer structure or a multi-layer structure including two or more layers made of different polymer materials.

[0069] The sealant layer may have a total thickness of 60㎛ to 100㎛, preferably 60㎛ to 90㎛, and more preferably 70㎛ to 90㎛. If the thickness of the sealant layer is too thin, sealing durability and insulation may be reduced, and if it is too thick, flexibility may be reduced and the total thickness of the pouch film laminate may increase, which may lower the energy density relative to volume.

[0070] Meanwhile, the above pouch film laminate can be manufactured through a method for manufacturing a pouch film laminate known in the art. For example, the pouch film laminate can be manufactured by attaching a substrate layer (10) to the upper surface of a barrier layer (20) using an adhesive and forming a sealant layer (30) on the lower surface of the barrier layer (20) using co-extrusion or an adhesive, but is not limited thereto.

[0071] A pouch film laminate as described above is inserted into a molding device, and a pouch (100) is manufactured by applying pressure with a punch to a portion of the pouch film laminate to form a cup portion. At this time, the pressure may be 0.3 MPa to 1 MPa, preferably 0.3 MPa to 0.8 MPa, and more preferably 0.4 MPa to 0.6 MPa. When molding the cup portion, if the pressure is too low, excessive drawing may occur and wrinkles may form, and if the pressure is too high, drawing may not occur properly and the molding depth may be reduced.

[0072] Meanwhile, the moving speed of the punch may be 20 mm / min to 80 mm / min, preferably 30 mm / min to 70 mm / min, and more preferably 40 mm / min to 60 mm / min. If the pressure during forming is too low or the moving speed of the punch is too fast, wrinkling may occur due to buckling, and if the pressure during forming is too high or the moving speed of the punch is too slow, the stress concentrated at the corner of the cup portion during forming increases, which may increase the occurrence of pinholes or cracks.

[0074] A pouch (100) manufactured by the above method comprises a lower case (101), an upper case (102), and a folding portion (130) connecting the lower case and the lower case, wherein the upper case and / or the lower case comprises a cup portion (110) having a shape indented in one direction.

[0075] Specifically, the pouch (100) may be in a 1-cup form in which a cup portion (110) is formed only in the lower case (101) as shown in FIG. 2, but is not limited thereto, and may be in a 2-cup form in which a cup portion is formed in both the upper case and the lower case. In the case of a 2-cup pouch, after accommodating the electrode assembly and the electrolyte, the upper case is folded so that the cup portion of the upper case and the cup portion of the lower case face each other, so that an electrode assembly with a thicker thickness than a 1-cup pouch can be accommodated, and thus there is an advantage in that it is advantageous for realizing high energy density.

[0076] The above-mentioned cup portion (110) has a receiving space for accommodating an electrode assembly (200). Meanwhile, the above-mentioned pouch (100) may include a terrace (120) around the periphery of the cup portion (110). The terrace (120) refers to an unformed portion of the pouch film laminate, that is, the remaining area excluding the cup portion (110). The terrace (129) is a portion that is sealed by heat bonding during the process of accommodating the electrode assembly (200) in the cup portion (110), injecting an electrolyte, and then sealing.

[0077] The above cup portion (110) may include a bottom surface and a perimeter surface. The perimeter surface may connect the bottom surface and the terrace (120). Multiple perimeter surfaces may be provided, more specifically, four. The bottom surface may cover one side of the electrode assembly (200), and the perimeter surface may surround the perimeter of the electrode assembly (200).

[0078] Meanwhile, the folding part (130) connects the lower case (101) and the upper case (102), accommodates the electrode assembly (200) in the cup part (110), and folds after injecting the electrolyte so that the upper case (102) can seal the cup part (110) of the lower case (101). When the folding part (130) is included, the lower case (101) and the upper case (102) are connected as a single unit, so when performing a sealing process later, the number of sides to be sealed is reduced, thereby improving processability.

[0079] The folding portion (130) is formed spaced apart from the cup portion (110), and the distance between the folding portion (130) and the cup portion (110) may be 0.5 mm to 3 mm, preferably 0.5 mm to 2 mm. If the folding portion (130) is formed too close to the cup portion (110), folding is not performed smoothly, and if the folding portion (130) is formed too far from the cup portion (110), the total volume of the secondary battery increases, and the energy density relative to volume may decrease. In the case of a two-cup case, the folding portion may be formed to satisfy the distance between each cup portion.

[0081] Phase 2: Battery Cell Assembly Phase

[0082] Next, when the battery case is prepared, the electrode assembly is placed in the battery case, and the electrolyte is injected to assemble the battery cell (S2).

[0083] In the case where the battery case is a pouch, an electrode assembly (200) can be placed in the cup portion (110) of the pouch and an electrolyte (not shown) can be injected to manufacture a battery cell. Specifically, an electrode assembly can be placed in the pouch cup portion, an electrolyte can be injected, the pouch can be folded to bring the upper case and the lower case into contact, and then heat can be applied to seal the sealant layer to manufacture a battery cell. At this time, a separate gas pocket space may be formed in the terrace (120).

[0084] The electrode assembly (200) may include a plurality of electrodes and a plurality of separators that are alternately stacked. The plurality of electrodes may include a positive electrode and a negative electrode having opposite polarities, which are alternately stacked with a separator in between.

[0085] Referring to FIG. 2, the electrode assembly (200) may be provided with a plurality of electrode tabs (230) welded together. The plurality of electrode tabs (230) may be connected to a plurality of electrodes (210) and may protrude outward from the electrode assembly (200) to serve as a passage through which electrons can move between the inside and outside of the electrode assembly (200). The plurality of electrode tabs (230) may be located inside the pouch (100).

[0086] The electrode tab (230) connected to the positive electrode and the electrode tab (230) connected to the negative electrode may protrude in different directions relative to the electrode assembly (200). However, this is not limited thereto, and it is also possible for the electrode tab (230) connected to the positive electrode and the electrode tab (230) connected to the negative electrode to protrude in the same direction parallel to each other.

[0087] A lead (240) that supplies electricity to the outside of the secondary battery can be connected to a plurality of electrode tabs (230) by spot welding or the like. One end of the lead (240) is connected to the plurality of electrode tabs (230), and the other end can protrude to the outside of the pouch (100).

[0088] A portion of the lead (240) may be surrounded by an insulating portion (250). For example, the insulating portion (250) may include insulating tape. The insulating portion (250) may be located between the terrace (120) of the first case (101) and the second case (102), and in this state, the terrace (120) and the second case (102) may be heat-fused to each other. In this case, a portion of the terrace (120) and the second case (102) may be heat-fused to the insulating portion (250). Thus, the insulating portion (250) prevents electricity generated from the electrode assembly (200) from flowing through the lead (240) to the pouch (100) and can maintain the sealing of the pouch (100).

[0089] Meanwhile, in the present invention, the ratio of the length of the electrode assembly (200) to the width of the electrode (W2) may be 5 to 10, preferably 5 to 8. When the ratio of the length of the electrode to the width satisfies the above range, the effect of achieving high energy density in a limited space can be obtained.

[0090] For example, the electrode assembly may have an overall length of 400 mm to 600 mm and an overall width of 50 to 150 mm, preferably an overall length of 500 mm to 600 mm and an overall width of 50 to 100 mm.

[0091] Next, the above electrolyte is intended to move lithium ions generated by the electrochemical reaction of the electrode during the charging and discharging of the secondary battery, and may include an organic solvent and a lithium salt.

[0092] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.

[0093] The above lithium salt can be used without special limitations as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 5.0 M, more preferably 0.1 to 3.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.

[0094] In addition to the above electrolyte components, the above electrolyte may additionally include additives for the purpose of improving the lifespan characteristics of the battery, suppressing the reduction of battery capacity, and improving the discharge capacity of the battery.

[0096] Meanwhile, in the present invention, the electrolyte is injected such that the amount of electrolyte per unit capacity of the secondary battery is a (g / Ah), wherein a may be 2.0 to 3.0, preferably 2.0 to 2.5, and more preferably 2.1 to 2.4. The amount of electrolyte per unit capacity refers to the ratio of the amount of secondary electrolyte injected (unit: g) to the rated capacity (unit: Ah) of the secondary battery. When the amount of electrolyte per unit capacity satisfies the above range, excellent impact resistance can be achieved without degrading the electrochemical properties of the secondary battery. If the amount of electrolyte is too small, the electrolyte may not be sufficient during battery operation, leading to a decrease in battery performance, and if it is too large, the effect of improving impact resistance is negligible.

[0098] Phase 3: Activation Phase

[0099] After assembling the battery cell, an activation process is performed (S3).

[0100] The activation process can be performed through general activation methods well known in the art to activate the assembled battery cell to impart electrical characteristics and stabilize the electrodes and electrolyte. For example, the activation process can be performed by charging and discharging the battery cell, and, if necessary, may include an aging process and / or a degassing process.

[0101] The above charging and discharging process is intended to impart electrical characteristics to the battery cell and form a Solid Electrolyte Interphase (SEI) film on the electrode surface, and the charging and discharging conditions can be appropriately adjusted according to the composition of the positive electrode, negative electrode, and electrolyte of the battery cell. For example, in the case of a battery in which lithium nickel-cobalt-manganese oxide is applied as the positive electrode active material and graphite is applied as the negative electrode active material, charging and discharging can be performed at 20 to 60°C in a voltage range of 2.0V to 4.4V.

[0102] Meanwhile, the above aging process is intended to ensure that the injected electrolyte is evenly dispersed within the cell and permeates well into the positive and negative electrodes, and is performed by storing the battery cell for a certain period of time at a predetermined temperature and humidity. For example, the above aging process may be performed at 10°C to 70°C for 0 to 72 hours, but is not limited thereto.

[0103] Meanwhile, the order and number of times the above-mentioned charging / discharging process and aging process are not specifically limited and can be appropriately adjusted as needed. For example, the charging / discharging process and the aging process may each be performed independently one or more times, and the aging may be performed before and / or after the charging / discharging process.

[0104] The degassing process is intended to remove gas from inside the battery cell. Gas is generated as the electrolyte and electrodes chemically react during the aging and charge / discharge processes. Since the presence of residual gas inside the battery cell can cause a degradation in electrochemical performance, it is desirable to discharge the gas from inside the battery cell. The degassing process may utilize any general methods used in the industry without limitation and is not specifically restricted. For example, it may be performed by forming a gas outlet in a part of the pouch, discharging the gas in a depressurization chamber, and then sealing the gas outlet through thermal fusion, or by forming a gas pocket in a part of the pouch, moving the gas into the gas pocket through pressurization, and then cutting and removing the gas pocket.

[0106] Step 4: Pre-charge / discharge stage

[0107] Next, b pre-charge / discharge cycles are performed on the activated battery cell (S4). At this time, b is an integer from 0 to 3, preferably from 1 to 3. If b=0, it means that no pre-charge / discharge cycles are performed.

[0108] According to the inventors' research, when pre-charging and discharging are performed, additional electrolyte impregnation occurs during the pre-charging and discharging process, which reduces the amount of electrolyte at the interface between the electrode assembly and the battery case. Consequently, the frictional force between the battery case and the electrode assembly increases, thereby suppressing the flow of the electrode assembly caused by external impact. However, if the amount of electrolyte injected is too small or the number of pre-charging and discharging cycles is too high, the amount of residual electrolyte is too low, which may degrade the electrochemical properties of the battery. Therefore, the pre-charging and discharging cycles must be performed at an appropriate number of times, taking into account the amount of electrolyte injected. Specifically, the number of pre-charging and discharging cycles b must be performed to satisfy Equation (1) or (1-1), and it is preferable to perform them within three cycles. If the number of pre-charging and discharging cycles exceeds three, the time required for battery manufacturing increases, leading to reduced productivity, and manufacturing costs increase because multiple charging and discharging facilities must be provided. Additionally, if the number of pre-charging and discharging cycles increases, swelling occurs, which causes the battery thickness to increase.

[0109] The above pre-charge / discharge can be performed at a C-rate of 0.1C to 1C, preferably 0.1C to 0.5C, in the range of SOC 0 to 100, preferably SOC 0 to 99, more preferably SOC 0 to 98.5. If the current rate during pre-charge / discharge is too high, the degradation reaction of the battery may be accelerated, which may degrade battery performance, and if the SOC range is too small, the battery may not be able to breathe sufficiently, resulting in a negligible increase in frictional force.

[0110] Meanwhile, the above pre-charge / discharge may vary depending on the active material and electrolyte used, and, for example, may be performed within a voltage range of 2.50V to 4.35V. If the pre-charge / discharge voltage range falls outside the above range, battery performance degradation due to overcharging or over-discharging may occur.

[0112] When a lithium secondary battery is manufactured such that the amount of electrolyte injected per unit capacity a and the number of pre-charge / discharge cycles b satisfy the relationship of Equation (1) or Equation (1-1) as described above, the frictional force between the electrode assembly and the inner surface of the battery case in contact with the electrode assembly (e.g., the bottom surface of the cup portion of the pouch) increases significantly.

[0113] Specifically, a lithium secondary battery manufactured according to the method of the present invention may have a frictional force between the inner surface of the battery case and the electrode assembly of 15 kgf or more, preferably 15 kgf to 30 kgf, and more preferably 17 kgf to 30 kgf. At this time, the frictional force between the electrode assembly and the battery case was measured by the following method.

[0114] A portion of the battery case (pouch) of the secondary battery was cut, and the welded portion between the negative lead and the electrode assembly was cut. Then, the positive tab was connected to a universal testing machine (UTM), and the force applied while pulling at a speed of 100 mm / min was measured to evaluate the frictional force between the electrode assembly and the inner surface of the battery case.

[0116] As the frictional force between the electrode assembly and the battery case is high in the secondary battery according to the present invention as described above, the electrode assembly detaches less even upon external impact, thereby minimizing damage to the battery case and exhibiting excellent impact resistance. Specifically, when a crash shock test is performed on the lithium secondary battery according to the present invention under a collision condition of 133.7G × 15.8ms (acceleration × duration), no electrolyte leakage occurs.

[0117] The above crash shock test can be performed by mounting the battery to be measured onto a jig of a drop impact device, dropping the battery from a specific height, and then determining whether the battery is damaged. In this case, the free-fall height is set by considering the collision conditions to be measured (acceleration × duration time). Specifically, the impact energy under the collision conditions to be measured is converted into potential energy, and the free-fall height can be set by calculating the height at which the converted potential energy can be achieved, taking into account the weight of the battery to be measured. Meanwhile, battery damage can be evaluated based on the presence or absence of electrolyte leakage.

[0119] The present invention will be explained more specifically below through specific embodiments.

[0121] Example 1

[0122] A pouch was prepared in which nylon, polyethylene terephthalate, an Al alloy thin film, and polypropylene were sequentially laminated and a cup portion was formed. A stacked electrode assembly with a total length of 548 mm and a total width of 99 mm was placed in the cup portion, an electrolyte was injected such that the amount of electrolyte per unit capacity was 2.19 g / Ah, and then sealed to manufacture a battery cell. Then, the battery cell was charged and discharged at a temperature range of 10 to 70°C and a voltage range of 2.0 to 4.25 V, and then activated by performing a degassing process. Pre-charging and discharging were not performed.

[0124] Example 2

[0125] An activated battery cell was prepared in the same manner as in Example 1, and then a pre-charge / discharge process was performed once in which the battery cell was charged to 4.25V at 0.33C in the SOC range of 0 to 98.3, and then discharged to 2.5V at 0.33C.

[0127] Example 3

[0128] An activated battery cell was prepared in the same manner as in Example 1, and then a pre-charge / discharge process was performed twice in which the battery cell was charged to 4.25V at 0.33C in the SOC range of 0 to 98.3, and then discharged to 2.5V at 0.33C.

[0130] Example 4

[0131] An activated battery cell was prepared in the same manner as in Example 1, and then a pre-charge / discharge process was performed three times in which the battery cell was charged to 4.25V at 0.33C in the SOC range of 0 to 98.3, and then discharged to 2.5V at 0.33C.

[0133] Comparative Example 1

[0134] A pouch was prepared in which nylon, polyethylene terephthalate, an Al alloy thin film, and polypropylene were sequentially laminated and a cup portion was formed. A stacked electrode assembly with a total length of 548 mm and a total width of 99 mm was placed in the cup portion, an electrolyte was injected such that the amount of electrolyte per unit capacity was 2.30 g / Ah, and then sealed to manufacture a battery cell. Then, the battery cell was charged and discharged at a temperature range of 10 to 70°C and a voltage range of 2.0 to 4.25 V, and then activated by performing a degassing process. Pre-charging and discharging were not performed.

[0136] Comparative Example 2

[0137] An activated battery cell was manufactured in the same manner as in Comparative Example 1, and then a pre-charge / discharge process was performed once in which the battery cell was charged to 4.25V at 0.33C in the SOC range of 0 to 98.3, and then discharged to 2.5V at 0.33C.

[0139] Example 5

[0140] After manufacturing an activated battery cell in the same manner as Comparative Example 1, the battery cell was charged to 4.25V at 0.33C in the SOC range of 0 to 98.3, and then discharged to 2.5V at 0.33C, a pre-charge / discharge process was performed twice.

[0142] Example 6

[0143] After manufacturing an activated battery cell in the same manner as Comparative Example 1, the battery cell was charged to 4.25V at 0.33C in the SOC range of 0 to 98.3, and then discharged to 2.5V at 0.33C, a pre-charge / discharge process was performed three times.

[0145] Table 1 below shows the electrolyte injection amount (a), the number of pre-charge / discharge cycles (b), and the values ​​calculated by Equation 1 for Examples 1 to 6 and Comparative Examples 1 to 2.

[0146] Electrolyte injection amount (a) [g / Ah] Pre-charge / discharge cycles (b) 486.77 - 373.09 × e (-0.006b) × a 0.29 Example 1 2.19 0 18.45 Example 2 2.19 1 21.25 Example 3 2.19 2 24.03 Example 4 2.19 3 26.8 Comparative Example 1 2.3 0 11.74 Comparative Example 2 2.3 1 14.58 Example 5 2.3 2 17.41 Example 6 2.3 3 20.22

[0147] Experimental Example 1: Friction Force Test

[0148] A portion of the pouch of the lithium secondary battery prepared according to Examples 1 to 6 and Comparative Examples 1 to 2 was cut, and the welded portion between the negative lead and the electrode assembly was cut. Then, the positive tab was connected to a Universal Testing Machine (UTM), and the force applied while pulling at a speed of 100 mm / min was measured to evaluate the frictional force between the electrode assembly and the inner surface of the battery case (bottom surface of the cup portion). For accurate measurement, two or three secondary batteries were measured for each example and comparative example. The measurement results are shown in Figures 4 and 5.

[0149] As shown in FIGS. 4 and 5, the lithium secondary batteries of Examples 1 to 6, in which the electrolyte injection amount (a) and the number of pre-charge / discharge cycles (b) satisfy the conditions of Equation (1), were found to have a frictional force between the electrode assembly and the bottom surface of the cup that exceeds 15 kgf, whereas the lithium secondary batteries of Comparative Examples 1 to 2, in which the electrolyte injection amount (a) and the number of pre-charge / discharge cycles (b) do not satisfy the conditions of Equation (1), were found to have a frictional force between the electrode assembly and the bottom surface of the cup that is 15 kgf or less.

[0151] Experimental Example 2: Collision Shock Test

[0152] A crash shock test was performed on the pouch-type secondary batteries prepared in Examples 1 to 6 and Comparative Examples 1 to 2 under a crash condition of 133.7G × 15.8ms. The measurement results are shown in Table 2 below. After the test, if no electrolyte leakage or electrode assembly detachment occurred, it was marked as Pass, and if electrolyte leakage and / or electrode assembly detachment occurred, it was marked as Fail.

[0154] Crash Shock Test Results Example 1 Pass Example 2 Pass Example 3 Pass Example 4 Pass Comparative Example 1 Fail Comparative Example 2 Fail Example 5 Pass Example 6 Pass

[0155] As shown in [Table 1] above, the lithium secondary batteries of Examples 1 to 6, in which the electrolyte injection amount (a) and the number of pre-charge / discharge cycles (b) satisfy the conditions of Equation (1), showed high frictional force between the electrode assembly and the bottom surface of the cup portion, and as a result, the detachment of the electrode assembly due to external impact was suppressed, exhibiting excellent impact resistance. In contrast, the lithium secondary batteries of Comparative Examples 1 to 2, in which the electrolyte injection amount (a) and the number of pre-charge / discharge cycles (b) do not satisfy the conditions of Equation (1), showed low frictional force between the electrode assembly and the bottom surface of the cup portion compared to the batteries of the examples, and as a result, electrolyte leakage occurred during the collision shock test.

Claims

Claim 1 A method for manufacturing a lithium secondary battery comprising: a first step of preparing a battery case; a second step of assembling a battery cell by placing an electrode assembly in the battery case and injecting an electrolyte such that the mass of the electrolyte per unit capacity is a (g / Ah); a third step of activating the battery cell; and a fourth step of pre-charging and discharging the activated battery cell b times, satisfying the following formula (1). Formula (1): 15 ≤ 486.77 - 373.09 × e (-0.006b) × a 0.29 ≤ 30 In the above formula (1), a is an integer from 2.0 to 2.5 and b is an integer from 0 to 3. Claim 2 A method for manufacturing a lithium secondary battery according to claim 1, satisfying the following formula (1-1). Formula (1-1): 15 ≤ 486.77 - 373.09 × e (-0.006b) ×a 0.29 ≤ 27 In the above equation (1-1), a is an integer from 2.0 to 2.5 and b is an integer from 0 to 3. Claim 3 delete Claim 4 A method for manufacturing a lithium secondary battery according to claim 1, wherein in the fourth step, the pre-charge / discharge is performed in the SOC 0 to 99 range with a C-rate of 0.1C to 1C. Claim 5 A method for manufacturing a lithium secondary battery according to claim 1, wherein in the fourth step, the pre-charge / discharge is performed in a voltage range of 2.50V to 4.35V. Claim 6 A method for manufacturing a lithium secondary battery according to claim 1, wherein the third step comprises a step of charging and discharging a battery cell. Claim 7 In claim 1, the method for manufacturing a lithium secondary battery wherein the frictional force between the inner surface of the battery case and the electrode assembly is 15 kgf or more. Claim 8 In claim 1, the method for manufacturing a lithium secondary battery wherein the frictional force between the inner surface of the battery case and the electrode assembly is 15 kgf to 30 kgf. Claim 9 A method for manufacturing a lithium secondary battery in which the electrolyte leakage amount is 0 when the lithium secondary battery is subjected to a crash shock test under a collision condition of 133.7G × 15.8ms. Claim 10 A method for manufacturing a lithium secondary battery according to claim 1, wherein the battery case comprises a barrier layer, a substrate layer formed on one side of the barrier layer, and a sealant layer formed on the other side of the barrier layer, and is a pouch comprising at least one cup portion indented in one direction. Claim 11 In claim 1, the electrode assembly is a method for manufacturing a lithium secondary battery in which the ratio of the length to the width is 5 to 10. Claim 12 A method for manufacturing a lithium secondary battery according to claim 11, wherein the electrode assembly has an overall length of 400 mm to 600 mm and an overall width of 50 to 150 mm. Claim 13 In claim 1, the method for manufacturing a lithium secondary battery having a rated capacity of 50Ah to 200Ah.

Citation Information

Patent Citations

  • Method of manufacturing nonaqueous electrolyte secondary battery

    JP2010080105A

  • Prismatic lithium rechargeable battery including polymer anhydrous electrolytes, and thereof method

    KR100859628B1

  • Method of precise measurement for the level of electrolyte impregnation of electrode in the battery cell

    KR1020200018308A

  • Method for manufacturing secondary battery

    KR1020210034985A

  • Manufacturing method for the Secondary battery

    KR1020220141548A