composition

A water-soluble adhesive composition with controlled epoxy resin and isocyanate groups enables stable, rapid bonding of sheet metals, addressing toxicity and inefficiency issues in existing technologies, enhancing storage and process efficiency.

KR103047173B1Active Publication Date: 2026-11-10KANSAI HELIOS AUSTRIA GMBH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
KR1020237027438
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-15
Filing Date
2022-01-14
Publication Date
2026-11-10
Estimated Expiration
2042-01-14

AI Technical Summary

Technical Problem

Existing adhesive compositions for bonding sheet metals are difficult to handle due to toxicity, rapid curing times that are hard to control, leading to brittleness and inefficiency, and require precise temperature control, which increases energy consumption and reduces durability.

Method used

A water-soluble composition comprising specific ratios of linear and non-linear epoxy resins, a base curing agent with amine-bonded hydrogen atoms, and a crosslinker with blocked isocyanate groups, allowing for pre-crosslinking at lower temperatures and extended storage stability, enabling rapid bonding without the need for toxic catalysts.

Benefits of technology

The composition provides high storage stability for at least 6 months, allows for rapid bonding within minutes, reduces energy consumption, and avoids the use of harmful chemicals, resulting in cost-effective and efficient industrial processes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a composition for joining metal sheets together, preferably comprising the following: a. 1 part by mole of at least one linear epoxy resin having an average epoxy equivalent weight of 600 to 5,000 g / mol and an epoxy functionality of 2, b. 0.4 to 0.8 parts per mole of at least one non-linear epoxy resin having an average epoxy equivalent weight of 180 to 350 g / mol and an average epoxy functionality of at least 3, c. 0.8 to 1.3 parts per mole of at least one base curing agent comprising at least two free amine-bonded hydrogen atoms, d. 0.9 to 1.2 parts per mole of at least one crosslinker comprising at least two blocked isocyanate groups.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates particularly to a composition suitable for joining sheet metals together. Background Technology

[0002] Metal parts bonded together, such as sheet metal parts, are applied in various technical fields. In particular, in the manufacture of generators, electric motors, transformers, and other electrical machinery, stacks of bonded electric sheet metal parts are used as starting materials for magnetic cores. Bonded sheet metal parts are generally provided with a special adhesive layer on one or both sides, and it is preferable to use a so-called "bonding varnish," which is a crosslinkable hot-melt adhesive. A coating made of bonding varnish has the advantage that no adhesive effect occurs after it is applied to the surface of metal, particularly sheet metal (e.g., sheet metal strip). The adhesive layer is activated only during the bonding process, such as when thermal energy is supplied. As a result of this activation, the coating acquires adhesive properties, allowing the metals in contact to bond together. At the same time, the adhesive layer hardens and becomes a heat-resistant thermosetting plastic.

[0003] Producing sheet metal parts or sheet metal lamellas that are bonded together with bonding varnish, respectively, offers the following advantages:

[0004] a) Maintaining magnetic properties by preserving the microstructure of the steel structure through the application of appropriate bonding temperature and pressure;

[0005] b) Compact lamination packs with strict manufacturing tolerances improve the release of waste heat generated during operation. Therefore, the cooling assembly can be minimized;

[0006] c) The viscoelastic connecting layer between individual lamellae exhibits pronounced damping behavior in relation to sound transmission;

[0007] d) A thin and stable adhesive layer that does not leak at the outer edge allows for a high degree of design freedom while using the tightest possible tolerances;

[0008] e) preventing corrosion problems (inter-lamellar corrosion) through a very stable, heat-resistant, hydrolysis-resistant full-surface connection; and

[0009] f) Excellent insulation effect for electric short circuits, which can, for example, increase the efficiency of a transformer.

[0010] Crosslinkable hot-melt adhesives are appropriately described in the prior art. For example, WO 2006 / 049935 discloses an adhesive composition comprising a selection of curing agents such as epoxy resin, exothermic silicon dioxide particles and phenolic resins, carboxylic acids, anhydrides, isocyanates, and, among others, dicyandiamide, which is used as the sole curing agent in all examples of use. This self-adhesive coating is applied to an electrical sheet and dried at a temperature of 230°C to 260°C. Punched lamellae on the coated electrical sheet are placed overlapping each other and bonded together for 60 to 120 minutes at a temperature between 100°C and 300°C and high pressure.

[0011] Essentially, adhesive compositions as described in WO 2006 / 049935 (but without any indication of equivalents, functionality, etc.) comprising bisphenol-A or bisphenol-F epoxy resins and mixtures thereof, and curing agents such as exothermic silicon dioxide, e.g. Lewis acids as fillers and reinforcing agents, are difficult to handle, particularly because Lewis acids are mostly very harmful to health and toxic.

[0012] A heat-activable adhesive composition comprising an epoxy resin, an activating curing agent, and an activating accelerator is also described in WO 2017 / 050892. This adhesive composition is cured on a sheet metal surface at a temperature of 100°C or higher. Subsequently, sheet metal lamellas are punched, stacked one by one on top of them, and then the adhesive located on the surface is activated at a temperature of about 200°C to bond them together. The activation time of this adhesive is 0.5 to 1 second, and the maximum curing time is 5 seconds.

[0013] Rapid curing of the adhesive layer, specifically the catalytically accelerated reaction between the curing agent dicyandiamide and the epoxy resin, can be achieved in WO 2017 / 050892 by adding specific accelerators, particularly Lewis acids; however, this is generally harmful to health and toxic, and due to non-specific and rapid chemical reactions, the crosslinking density becomes very high, causing brittleness and reduced durability of the adhesive layer. Additionally, there is a risk of premature partial crosslinking in liquid delivery conditions, which manifests noticeably as a sharp increase in viscosity and a decrease in shelf life.

[0014] WO 2020 / 233840 teaches that temperature control of punched and already coated lamellae is required, in particular, to minimize electrical loss of the finished product (of a machine including a laminated pack bonded together). Due to this additional energy-intensive process step, the laminated core production process becomes inefficient.

[0015] All three papers discussed here share the commonality of fundamentally shortening the curing of dicyanate diamide using epoxy resin by employing so-called catalyst accelerators. Related problems have been acknowledged, including precise temperature control, excessively short crosslinking times that are difficult to control during production, over-crosslinking and associated brittleness, and the toxicity of the accelerators.

[0016] The object of the present invention is to provide a water-soluble composition capable of bonding metal parts, such as sheet metal, in the shortest possible time. Significant cost savings are possible by reducing the time required for the bonding process. In addition, the composition must not have the disadvantages of the prior art, in particular WO 2006 / 049935, WO 2017 / 050892, and WO 2020 / 233840.

[0017] Another objective of the present invention is to provide a composition having storage stability for at least 6 months. A metal coated with such a composition should also be able to bond without limitation even after being stored for more than 6 months. The problem to be solved

[0018] The present invention relates to a composition for joining metal sheets together, preferably comprising the following:

[0019] a. 1 part by mole of at least one linear epoxy resin having an average epoxy equivalent weight of 600 to 5,000 g / mol and an epoxy functionality of 2,

[0020] b. 0.4 to 0.8 parts per mole of at least one non-linear epoxy resin having an average epoxy equivalent weight of 180 to 350 g / mol and an average epoxy functionality of at least 3,

[0021] c. 0.8 to 1.3 parts per mole of at least one base curing agent comprising at least two free amine-bonded hydrogen atoms,

[0022] d. 0.9 to 1.2 parts per mole of at least one crosslinker comprising at least two blocked isocyanate groups.

[0023] The composition according to the present invention can be used as a one-component material for coating and subsequent bonding of metals, particularly sheet metal, sheet metal parts, or sheet metal lamellas. Surprisingly, it has been found that the composition according to the present invention exhibits high storage stability at room temperature, preferably, so that it can be used for coating and subsequent bonding of metals, particularly sheet metal, without loss of quality even after several months, i.e., at least 6 months, preferably at least 8 months, more preferably at least 12 months.

[0024] When a metal, particularly a sheet metal or a sheet metal part, is coated with a composition according to the present invention, it can be optionally bonded with a second coated metal even after a period of at least 6 months. As a result, the coated metal can be stored for a long period and, if necessary, processing and bonding are possible.

[0025] The composition according to the present invention has the advantage of being able to dry rapidly on a metal surface using a lower temperature than comparable compositions in the industry, while simultaneously enabling pre-crosslinking (within 2 minutes). In this way, the coating process can be optimized and shortened. In particular, for sheet metal coatings that are typically stored in a rolled-up state, the coating process is significantly simplified and optimized because the sheet metal can be rolled up again in a very short time immediately after the rolling and coating processes.

[0026] Another advantage of the present invention is that curing parameters can be set very precisely, so a wide application window (time and temperature gradient) can be omitted, and thus additional temperature control of the coated, punched, and optionally layered sheet metal before final bonding and curing is no longer required, which is a practice frequently performed according to the prior art (e.g., see WO 2020 / 233840). Therefore, using the composition according to the present invention results in additional energy savings and increased efficiency.

[0027] The "activation and final curing" of a coating pre-crosslinked to a metal and subsequent bonding with another metal can be achieved in a shorter time (within 2 minutes) compared to other compositions in the industry.

[0028] The composition according to the present invention is particularly advantageous because, as suggested in the literature, Lewis acids harmful to health can be omitted, for example, to crosslink the components. Additionally, the composition according to the present invention can be provided essentially as a water-based composition, and as a result, the use of organic solvents can be largely omitted. Using water as the basis of the composition has advantages related to safety on the one hand, and advantages in terms of health on the other, for example, because it can prevent and / or minimize the vapors / waste gases of organic solvents.

[0029] By providing a basic curing agent and a crosslinking agent to the composition according to the present invention, the (pre)crosslinking and final curing of the resin and the bonding to the metal surface can be controlled more advantageously than before by using an adhesive composition described in the art.

[0030] Therefore, the cross-linking of the composition according to the present invention and the resin occurs in two chemically different and easily controllable sub-steps.

[0031] In the first sub-step, the pre-crosslinking of the composition applied to the metal surface occurs at a temperature and time suitable for production through the reaction of secondary hydroxyl groups from a linear, difunctional (epoxy functional 2) and preferably long-chain epoxy resin with a multifunctional, preferably dual or triple functional isocyanate to form a wide-meshed elastic polyurethane matrix. In this first step, the epoxy groups are preserved for a while. The isocyanate present in the composition according to the present invention exists in an amine-blocked form on the carrier, and the blockage is released and polymerization is possible only under the appropriate influence of temperature. Surprisingly, the amine simultaneously generated in this process does not escape into the environment but is added to the oxirane groups of the epoxy resin to form a tertiary amine. This, in turn, accelerates the formation of polyurethane (the addition of isocyanate to the hydroxyl group), allowing the first sub-step of crosslinking to be completed very quickly and completely, and the resulting adhesive layer is still preserved in a thermoplastic state and is perfectly suitable as a hot-melt adhesive for the second sub-step.

[0032] By selecting the isocyanate, spacer length, blocking amine, and optimal crosslinking parameters, those skilled in the art can set the desired properties in a reproducible manner. Surprisingly, it has also been found that NCO equivalents (i.e., isocyanate equivalents) of 0.2 to 1.0, preferably 0.3 to 0.8, more preferably 0.3 to 0.6 per OH group produce particularly suitable pre-crosslinking.

[0033] In order to achieve heat-resistant full crosslinking with duroplastic in the second sub-step, a reaction is required to further add at least one basic curing agent having at least two amine-bonded hydrogen atoms per molecule and an abundance of heat-reactive epoxy groups in the composition. It has been proven that it is preferable to use, for example, a guanidine-based amine curing agent and at least trifunctional, non-linear epoxy resins that are free of hydroxyl groups, such as novolac epoxy resin (i.e., epoxy resins with an average epoxy function of 3 or higher).

[0034] In the composition according to the present invention, the average functionality of the epoxy resin mixture (i.e., the number of epoxy groups per resin molecule) is preferably in the range of 2.3 to 5.0, more preferably 2.4 to 3.5. Through this functionality, the best results can be obtained in terms of heat resistance, adhesion, and peel strength.

[0035] In addition, it has been found that the ratio of oxirane to NH groups in the composition according to the present invention should preferably be in the range of 0.8 to 1.3, and more preferably 0.9 to 1.1.

[0036] In summary, NCO and oxirane groups react in the graded order of the crosslinking steps mentioned above, but in each case, through additional reactions with OH and NH groups, they form a duroplastic, a sufficiently elastic material for connecting electrical sheets.

[0037] Another aspect of the present invention relates to a coated metal, preferably a coated sheet metal, which can be manufactured by applying a composition according to the present invention to a solid, preferably a sheet metal.

[0038] Another aspect of the present invention relates to a method for coating sheet metal and optionally joining it together, comprising the following steps.

[0039] - A step of applying a composition according to the present invention to a sheet metal surface,

[0040] - A step of drying the composition of the sheet metal surface at a temperature of 150 to 200°C, preferably 170 to 190°C, for 10 seconds to 2 minutes, preferably 20 to 30 seconds, and simultaneously pre-crosslinking,

[0041] - Optionally, a step of punching a sheet metal operation in the above sheet metal,

[0042] - Optionally, a step of stacking the above-mentioned punched sheet metal parts, and

[0043] - Optionally, a step of joining and reinforcing the punched sheet metal parts together at a temperature of 220 to 260°C for 5 seconds to 2 minutes, preferably 10 seconds to 30 seconds.

[0044] Another aspect of the present invention relates to a component part comprising a laminated core or a laminated core, in particular a component part for an electric machine and / or transformer, wherein the laminated core comprises at least two sheet metals joined together with a composition according to the present invention. means of solving the problem

[0045] The composition of the present invention is prepared by mixing the following.

[0046] a. 1 part by mole of at least one linear epoxy resin having an average epoxy equivalent weight of 600 to 5,000 g / mol and an epoxy functionality of 2,

[0047] b. 0.4 to 0.8 parts per mole of at least one non-linear epoxy resin having an average epoxy equivalent weight of 180 to 350 g / mol and an average epoxy functionality of at least 3,

[0048] c. 0.8 to 1.3 parts per mole of at least one base curing agent comprising at least two free amine-bonded hydrogen atoms,

[0049] d. 0.9 to 1.2 parts per mole of at least one crosslinker comprising at least two blocked isocyanate groups.

[0050] As used herein, “part by mole” refers to the mutual molar ratio of the components present in the composition. For example, the composition according to the present invention comprises 0.4 to 0.8 parts by mole of at least one non-linear epoxy resin per part by mole of at least one linear epoxy resin.

[0051] According to a preferred embodiment of the present invention, the composition comprises water and / or an organic solvent and is provided as a solution, emulsion, or dispersion.

[0052] The composition according to the present invention may preferably include water and / or an organic solvent, which is derived, for example, from a starting component dissolved or suspended in water or an organic solvent. Additionally, water and / or an organic solvent may be added to control the viscosity of the composition according to the present invention.

[0053] According to a more preferred embodiment of the present invention, at least one linear epoxy resin has an average epoxy equivalent weight of 1,500 to 2,500 g / mol.

[0054] Linear epoxy resins based on bisphenols, so-called bisphenol (di)glycidyl ethers, have been shown to have particularly advantageous properties. Accordingly, at least one linear epoxy resin is a bisphenol epoxy resin, preferably a bisphenol-A epoxy resin, a bisphenol-F epoxy resin, a bisphenol-S epoxy resin, or a bisphenol-Z epoxy resin, and a resin based on bisphenol A is particularly preferred.

[0055] According to a preferred embodiment of the present invention, at least one linear epoxy resin comprises at least three bisphenol units per molecule.

[0056] According to another preferred embodiment of the present invention, at least one linear epoxy resin is a bisphenol-A epoxy resin having 3 to 15, preferably 4, 7, or 9 bisphenol-A units per molecule.

[0057] The free hydroxyl groups of the linear epoxy resin are essential for the (pre)crosslinking of the resin. For this reason, it is desirable for at least one linear epoxy resin to contain hydroxyl groups, and it is desirable for the linear epoxy resin molecule to have at least one, preferably at least two, hydroxyl groups.

[0058] According to another preferred embodiment of the present invention, at least one linear epoxy resin comprises 2 to 14, preferably 3, 6, or 8 secondary hydroxyl groups per molecule.

[0059] According to a preferred embodiment of the present invention, at least one linear epoxy resin comprises a bisphenol-A epoxy resin having 2 to 14, preferably 3, 6, or 8 hydroxyl groups per molecule.

[0060] According to a particularly preferred embodiment of the present invention, at least one non-linear epoxy resin has an average epoxy equivalent weight of 190 to 280 g / mol.

[0061] Preferably, at least one non-linear epoxy resin is at least one novolac epoxy resin.

[0062] Novolac is a phenolic resin with a formaldehyde / phenol ratio of less than 1:1, obtained by the acidic condensation of vitreous educts. Novolac is particularly useful in the compositions of the present invention because it has a low oxirane equivalent weight and high functionality, and is therefore particularly suitable for controlled curing. Since it lacks hydroxyl groups, it participates in the processing cascade only during the final curing process (i.e., during bonding).

[0063] According to a preferred embodiment of the present invention, at least one novolac epoxy resin comprises phenol and / or cresol units, and at least one novolac epoxy resin comprises 3 to 8, preferably 3 to 6, epoxy groups per epoxy resin molecule.

[0064] According to another preferred embodiment of the present invention, a mixture of at least one linear epoxy resin and at least one non-linear epoxy resin comprises, on average, 2.3 to 5.0, preferably 2.4 to 3.5 epoxy groups per epoxy resin molecule.

[0065] According to a preferred embodiment of the present invention, at least one basic curing agent comprising at least two free amine-bonded hydrogen atoms is a guanidine derivative, preferably dicyandiamide, dicyandiamidine, aminoguanidine, creatine, creatinine, arginine, aliphatic biguanide, aromatic biguanide, 2-aminopyridimine, 3-amino-1,2,4-triazole, 5-amino-1H-tetrazole, 1,3-di-o-tolylguanidine, and It is selected from the group consisting of 2-cyanimino-1H,5-alkyl-1,3,5-triazine.

[0066] As described above, the ratio of oxirane to NH groups in the composition according to the present invention is preferably in the range of 0.8 to 1.3, more preferably 0.9 to 1.1. In cases where some of the guanidine derivatives described herein have two or more free amine-bonded hydrogen atoms that generally react in different ways, only the minimum two in each case are considered in the calculations and correlations related to the present invention.

[0067] In order to facilitate additional cross-connection in the pre-crosslinked polyurethane matrix during the final curing process, a basic curing agent containing free amino groups is added to the composition according to the present invention. Thus, the basic curing agent plays a role in causing the composition according to the present invention to solidify during the bonding process to form a high-strength, thermally stable duromer.

[0068] According to a more preferred embodiment of the present invention, at least one (pre-)crosslinking agent is an aliphatic or alicyclic diisocyanate or triisocyanate, and the isocyanate group of the aliphatic or alicyclic diisocyanate or triisocyanate is C4 to C4 as a spacer 10 It is separated by alkyl radicals.

[0069] According to a preferred embodiment of the present invention, at least one crosslinking agent comprising at least two isocyanate groups is a diisocyanate, preferably hexamethylene diisocyanate, 2-methyl-hexamethylene diisocyanate, 2,2,4(2,4,4)-trimethyl-hexamethylene diisocyanate (TMDI), 1,12-dodecane diisocyanate, omega,omega-diisocyanatodipropyl ether, 1,4-cyclohexane diisocyanate. It is selected from the group consisting of 1,4-diisocyanatomethylcyclohexane, isophorone diisocyanate and / or isocyanurate trimers thereof.

[0070] According to a particularly preferred embodiment of the present invention, at least one crosslinking agent comprising at least two isocyanate groups is hexamethylene diisocyanate, isophorone diisocyanate and / or its isocyanurate trimer.

[0071] According to a further preferred embodiment of the present invention, the isocyanate group is blocked by an amine, preferably a heterocyclic amine comprising at least two nitrogen heteroatoms.

[0072] The (pre-)crosslinking agent added to the composition according to the present invention is blocked to enable a long shelf life of the aqueous formulation and related compositions, because free isocyanates can only exist in an anhydrous system due to their reactivity. In the aqueous composition, free isocyanates can react (pre-crosslink) with the hydroxyl groups of the linear epoxy resin, which is undesirable at this point when the material has already been transferred. Therefore, this solution may become an impractical two-component solution with a short pot life upon mixing. While the final result is certainly comparable to the result according to the present invention, the objective of the present invention is to provide an aqueous-based, storable one-component formulation. During the coating process in which the metal is heated along with the coating, the blocking group is removed to enable crosslinking of the linear epoxy resin, thereby forming a matrix that remains thermoplastic.

[0073] According to a preferred embodiment of the present invention, the amine is a pyrazole, imidazole, benzimidazole, 1,2,3-triazole, preferably a benzotriazole, 1,2,4-triazole, triazabicyclodecene, or N-monosubstituted piperazine.

[0074] According to another preferred embodiment of the present invention, the amine is a pyrazole, preferably 3,4-dimethylpyrazole or 3,5-dimethylpyrazole.

[0075] According to a preferred embodiment of the present invention, the at least one organic solvent is a water-miscible solvent and is selected from the group consisting of C3-C6 ketones, C2-C4 alcohols, monoalkyl-(C2-C4)-ethers of C1-C4 glycols, di- and / or triethylene and / or propylene glycol, dioxane, tetrahydrofuran, and C4 to C8 lactones.

[0076] Another aspect of the present invention relates to a coated metal that can be manufactured by applying a composition according to the present invention to a solid, preferably a sheet metal.

[0077] The composition according to the present invention can be applied to a metal surface using known methods (e.g., dipping, spraying, rolling, doctoring, or spreading). After the composition is applied, the coating is pre-crosslinked by heating. The metal can then be stored for further processing and / or transport.

[0078] Another aspect of the present invention relates to a method for coating sheet metal and optionally bonding it together, comprising the following steps.

[0079] - A step of applying a composition according to the present invention to a sheet metal surface,

[0080] - A step of drying and pre-crosslinking the composition of the sheet metal surface at a temperature of 150 to 200°C, preferably 170 to 190°C, for 10 seconds to 2 minutes, preferably 20 to 30 seconds,

[0081] - Optionally, a step of punching a piece of sheet metal from the sheet metal,

[0082] - Optionally, a step of joining punched sheet metal parts together at a temperature of 220 to 260°C for 5 seconds to 2 minutes, preferably 10 to 30 seconds.

[0083] Surprisingly, it has been demonstrated that the composition according to the present invention can be cured and bonded within a particularly short, yet technically controllable and adjustable time. Furthermore, the temperature used for this purpose is lower than that of compositions known in the art. As a result, industrial processes can be designed and accelerated in a more cost-effective manner.

[0084] Another aspect of the present invention relates to a laminated core or a component comprising a laminated core, in particular a component for an electric machine and / or transformer, wherein the laminated core comprises at least two sheet metals joined together with a composition according to the present invention.

[0085] By using the method and composition according to the present invention, laminated cores can be produced simply and quickly. Laminated cores are applied in various fields, and their use in generators, transformers, and electric motors is the most important application area.

[0086] Another aspect of the present invention relates to a laminated core or a component part comprising a laminated core that can be obtained by the method according to the present invention, in particular a component part for an electric machine and / or transformer. Specific details for implementing the invention

[0087] Example 1: Water-based Composition I

[0088] The following components were mixed with water to form a dispersion with a total solid content of 53%:

[0089] 1 mole of linear epoxy resin (based on bisphenol A) having an epoxy functionality of 2 and an average epoxy equivalent weight of 1,750 g / mol was provided as a 53% dispersion in water / methoxypropanol (3:1), and

[0090] 0.8 moles of a non-linear epoxy resin (based on phenol novolak) having an epoxy functionality of 3.6 and an average equivalent weight of 194 g / mol were provided as a 58% dispersion in water, and

[0091] - 1.1 molar dicyandiamide (DCDA) is calculated as functional 2, equivalent weight 42 g / mole, and is provided as a 30% methoxypropanol solution, and

[0092] 1.12 molar hexamethylene diisocyanate (HMDI) is blocked by 3,5-dimethylpyrazole (DMP) and has function 2, and is provided as a 38% solution in water.

[0093] After mixing, the dispersion was heated to 60°C for 15 minutes and then cooled to room temperature. The viscosity of the dispersion was 60 to 80 seconds (flow time according to DIN EN ISO 2431:2011).

[0094] Composition I according to the present invention exhibited the following parameters:

[0095] ∑ Equiv. -OH: 6

[0096] ∑ Equiv. -NH: 4.45

[0097] ∑ Equiv. -NCO: 2.25

[0098] ∑ equiv. -oxirane: 4.9

[0099] ∑ OH +NH: 10.45

[0100] ∑ NCO +oxirane: 7.15

[0101] Composition I showed an average epoxy functionality of linear and non-linear epoxy resins of 2.71. The ratio of NCO to OH groups was 0.37, the ratio of oxirane to NH groups was 1.10, and the ratio of NCO and oxirane groups to OH and NH groups was 0.68.

[0102] Composition I can be stored at room temperature for more than 6 months without affecting beneficial properties. During this period, no components separated noticeably.

[0103] It was found that Composition I could be dried and pre-crosslinked in 20 seconds at 195°C after being applied to a sheet metal. One of two sheet metals coated with Composition I could be bonded together in 15 seconds at 210°C.

[0104] To rule out the possibility that this was not the pure catalytic action of the amine (DMP), the reaction promoter DCDA / OXIRAN was used instead of the capped amine, and equimolar amounts of DMP were used in additional experiments. After application to the sheet metal, the composition was highly reactive, and the reactive groups of the composition were almost perfectly cross-linked on the metal surface within a very short time. As a result of this quick cross-linking, the applied composition acquired duroplastic properties and could no longer be thermally bonded.

[0105] To demonstrate the necessity of the NCO specifications required according to the present invention, the simplest prototype of a blocked isocyanate, namely urea, was used instead of the HMDI compound. This reference composition solidified within 14 hours at room temperature, making further processing impossible and thus unable to be stored.

[0106] In additional comparative tests, common crosslinking agents that replace DCDA, such as hexamethylene tetramine or hexamethylolmelamine, were also found to significantly reduce the batch's service life and cure after a few hours.

[0107] Example 2: Composition II Solvent-based Comparison

[0108] Composition II differs from Composition I (see Example 1) in that a linear epoxy resin is added as a 75% solution in methyl ethyl ketone (MEK) and a non-linear epoxy resin is added as a liquid resin. Additionally, blocked hexamethylene diisocyanate is added as a 50% solution in MEK / MP (methoxypropanol) (1:1). The total solid content is adjusted to 40% with MP.

[0109] After mixing, the composition was heated to 60°C for 15 minutes and then cooled to room temperature. The viscosity of the dispersion was 60 s (flow time according to DIN EN ISO 2431:2011).

[0110] The parameters and relationships were similar to those in Example 1.

[0111] When the above composition was stored at room temperature, gelation began after 10 weeks.

[0112] Shelf life: 10 weeks, onset of gelation.

[0113] However, it was found that solvent-based composition II enables pre-crosslinking at 195°C in just 20 seconds after application to sheet metal. Two sheet metals coated with composition II could be bonded together in 12 seconds at 215°C.

[0114] Example 3: Water-based Composition III

[0115] Composition III was composed of 1 mole of linear epoxy resin, similar to Composition I. Additionally, Composition III contained 0.6 moles of cresol-based novolak resin with an epoxy function of 5.5 and an average equivalent weight of 215 g / mol, and was provided as a 40% dispersion in water. As a curing agent, Composition III contained 1.1 moles of creatinine with a function of 2 and an equivalent weight of 56.5 g / mol, and was provided as a 30% solution in methoxypropanol. Composition III further contained 1 mole of trimer HMDI, which is blocked by DMP and has a function of 3, and was provided as a 40% solution in water.

[0116] After mixing, Composition III was heated to 60°C for 15 minutes and then cooled to room temperature. The viscosity of the dispersion was 60 to 80 s (flow time according to DIN EN ISO 2431:2011).

[0117] Composition III according to the present invention exhibited the following parameters:

[0118] ∑ Equivalents -OH: 6

[0119] ∑ Equivalents -NH: 5

[0120] ∑ Equivalents -NCO: 3

[0121] ∑ Equivalents oxirane: 5.3

[0122] ∑ OH + NH: 11

[0123] ∑ NCO + oxirane: 8.3

[0124] Composition III showed an average epoxy functionality of linear and non-linear epoxy resins of 2.97. The ratio of NCO to OH groups was 0.5, the ratio of oxirane to NH groups was 1.06, and the ratio of NCO and oxirane groups to OH and NH groups was 0.75.

[0125] Composition III was found to be able to dry at 180°C to 195°C in 20 to 30 seconds after being applied to a sheet metal. Two sheet metals coated with Composition III could be bonded at 230°C in 25 seconds.

[0126] After being stored at room temperature for one month, the viscosity of Composition III increased slightly, and after two months, the composition began to gel. However, as a result, the thixotropic properties remained in an acceptable state for three months.

Claims

Claim 1 A composition for bonding metal sheets together, comprising: a. 1 part by mole of at least one linear epoxy resin having an average epoxy equivalent weight of 600 to 5,000 g / mol and an epoxy functionality of 2; b. 0.4 to 0.8 parts by mole of at least one non-linear epoxy resin having an average epoxy equivalent weight of 180 to 350 g / mol and an average epoxy functionality of at least 3; c. 0.8 to 1.3 parts by mole of at least one base curing agent having at least two free amine-bonded hydrogen atoms; and d. 0.9 to 1.2 parts by mole of at least one crosslinker having at least two blocked isocyanate groups. Claim 2 A composition according to claim 1, characterized in that the composition comprises water and / or an organic solvent and is provided as a solution, emulsion, or dispersion. Claim 3 A composition according to claim 1, characterized in that at least one linear epoxy resin has an average epoxy equivalent of 1,500 to 2,500 g / mol. Claim 4 A composition according to claim 1, wherein at least one linear epoxy resin is a bisphenol-A epoxy resin, a bisphenol-F epoxy resin, a bisphenol-S epoxy resin, or a bisphenol-Z epoxy resin, and comprises at least three bisphenol units per molecule. Claim 5 A composition according to claim 1, characterized in that at least one linear epoxy resin is a bisphenol-A epoxy resin having 3 to 15 bisphenol-A units per molecule. Claim 6 A composition according to claim 1, characterized in that at least one linear epoxy resin comprises 2 to 14 secondary hydroxyl groups per molecule. Claim 7 A composition according to claim 1, characterized in that at least one non-linear epoxy resin has an average epoxy equivalent weight of 190 to 280 g / mol. Claim 8 A composition according to claim 1, wherein at least one non-linear epoxy resin is at least one novolak epoxy resin, said at least one novolak epoxy resin comprises phenol and / or cresol units, said at least one novolak epoxy resin comprises 3 to 8 epoxy groups per molecule of the epoxy resin. Claim 9 A composition according to claim 1, characterized in that at least one linear epoxy resin and at least one non-linear epoxy resin jointly comprise an average of 2.3 to 5.0 epoxy groups per molecule of the epoxy resin. Claim 10 A composition according to claim 1, characterized in that at least one basic curing agent comprising at least two free amine-bonded hydrogen atoms is a guanidine derivative. Claim 11 In claim 10, the guanidine derivative comprises dicyandiamide, dicyandiamidine, aminoguanidine, creatine, creatinine, arginine, aliphatic biguanide, aromatic biguanide, 2-aminopyridimine, 3-amino-1,2,4-triazole, 5-amino-1H-tetrazole, 1,3-di-o-tolylguanidine, and 2-cyanimino-1H,5-alkyl-1,3,5-triazine. A composition characterized by being selected from a group. Claim 12 In claim 1, at least one crosslinking agent is an aliphatic or cycloaliphatic diisocyanate or a triisocyanate, and the isocyanate group of the aliphatic or cycloaliphatic diisocyanate or triisocyanate is C4 to C 10 A composition characterized by being separated by an alkyl radical. Claim 13 In claim 12, the aliphatic or alicyclic diisocyanate or triisocyanate is hexamethylene diisocyanate, 2-methyl-hexamethylene diisocyanate, 2,2,4(2,4,4)-trimethyl-hexamethylene diisocyanate (TMDI), 1,12-dodecane diisocyanate, omega,omega-diisocyanatodipropyl ether, 1,4-cyclohexane diisocyanate, 1,4-diisocyanatomethylcyclohexane, A composition characterized by being selected from the group consisting of isophorone diisocyanate and isocyanurate trimers thereof. Claim 14 A composition according to claim 1, characterized in that the isocyanate group is blocked by an amine. Claim 15 A composition according to claim 14, characterized in that the amine is pyrazole, 3,4-dimethylpyrazole or 3,5-dimethylpyrazole, imidazole, benzimidazole, 1,2,3-triazole, benzotriazole, 1,2,4-triazole, triazabicyclodecene or N-monosubstituted piperazine. Claim 16 A composition according to claim 2, wherein the organic solvent is a water-miscible solvent and is selected from the group consisting of C3-C6 ketones, C2-C4 alcohols, monoalkyl-(C2-C4)-ethers of C1-C4 glycols, di- and / or triethylene and / or -propylene glycol, dioxane, tetrahydrofuran, and C4 to C8 lactones. Claim 17 A coated metal that can be manufactured by applying a composition according to any one of claims 1 to 16 to a solid. Claim 18 A method for coating a sheet metal and optionally bonding it together, comprising the steps of: applying a composition according to any one of claims 1 to 16 to the surface of the sheet metal; drying and pre-crosslinking the composition on the surface of the sheet metal at a temperature of 150 to 200°C for 10 seconds to 2 minutes; optionally punching a piece of sheet metal from the sheet metal; optionally stacking the punched sheet metal parts; and optionally bonding and curing the punched sheet metal parts together at a temperature of 220 to 260°C for 5 seconds to 2 minutes. Claim 19 A laminated core comprising at least two sheet metals combined with a composition according to any one of claims 1 to 16. Claim 20 A laminated core obtainable by the method according to paragraph 18.

Citation Information

Patent Citations

  • Single-component thermosetting epoxide adhesive with improved adhesion

    EP3460019A1

  • Flame-retardant resin composition, and prepreg and laminate using the same

    JP2000344861A

  • Surface-treated steel sheet superior in corrosion resistance, electroconductivity and abrasion resistance

    JP2008248356A

  • Adhesive coating composition

    JP2008518087A

  • Adhesive compositions and articles manufactured from said adhesives

    JP2018530660A