Manufacturing method of cathode active material for lithium secondary battery

A two-stage calcination process for lithium secondary batteries using tungsten and fluorine-doped lithium transition metal oxide particles addresses the structural and reaction issues of high-nickel NCM cathode materials, enhancing energy density and output characteristics while maintaining stability.

KR103047443B1Active Publication Date: 2026-11-11POSCO FUTURE M CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020240086472
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2026-11-11
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

Conventional high-nickel NCM cathode materials for lithium secondary batteries face issues such as increased gas generation due to large specific surface area, weak particle strength leading to structural collapse, and rapid degradation under high temperature and voltage conditions, along with side reactions during doping or coating processes.

Method used

A positive electrode active material for lithium secondary batteries is developed, comprising lithium transition metal oxide particles with controlled doping of tungsten and fluorine components, manufactured through a two-stage calcination process to suppress side reactions and enhance particle uniformity and c-axis expansion, resulting in improved energy density and output characteristics.

Benefits of technology

The method produces a positive electrode active material with enhanced press density, energy density, and lifespan characteristics by ensuring uniform particle growth and suppressing side reactions, leading to improved battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024071352840-PAT00001_ABST
    Figure 112024071352840-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a positive electrode active material for a lithium secondary battery, comprising the steps of: forming a mixture comprising a metal hydroxide precursor, a first doping raw material comprising fluorine, and a lithium raw material; calcining the mixture first; dissolving the first calcined product; and second calcining a mixture comprising the first calcined and dissolving product and a second doping raw material comprising tungsten, wherein the first calcination temperature is higher than the second calcination temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a positive electrode active material for a lithium secondary battery and a method for manufacturing a lithium secondary battery using the same. Background Technology

[0002] Driven by the recent explosive demand for electric vehicles and the need for increased driving range, the development of high-capacity, high-energy-density secondary batteries to meet these demands is actively underway worldwide.

[0003] As a measure to satisfy these requirements, a technology using high-nickel NCM (nickel-cobalt-manganese) cathode materials with a high Ni content has been proposed.

[0004] However, conventional high-nickel NCM cathode materials are composed of secondary particles formed by the aggregation of primary particles, and the large specific surface area of ​​the powder causes a somewhat larger contact area with the electrolyte, which leads to an increase in gas generation.

[0005] In addition, since secondary particles exist in an aggregated form of primary particles, the strength of the secondary particles is weak, and during the rolling process of the electrode, the secondary particles break into the form of primary particles, which causes a problem of deterioration in lifespan characteristics.

[0006] Accordingly, a single-crystal cathode material has been developed that can suppress the problem of lifespan degradation in high-nickel NCM cathode materials by increasing the size of primary particles to reduce the specific surface area and increasing the strength of the particles.

[0007] However, when manufacturing a single-crystal cathode material using conventional methods, the disintegration process is not easy, so there is a problem in that secondary particles formed by the aggregation of primary particles remain.

[0008] Meanwhile, in lithium secondary batteries using high-nickel NCM cathode materials, as charging and discharging are repeated, an increase in interfacial resistance between the electrode containing the active material and the electrolyte, degradation of the surface structure of the active material, and exothermic reactions accompanied by rapid structural collapse may occur.

[0009] As a result, problems may arise where the stability and lifespan characteristics of the battery deteriorate rapidly, and these problems become more severe, especially under high temperature and high voltage conditions.

[0010] Recently, to address these issues, methods have been proposed to improve the structural and surface stability of the active material itself and enhance interfacial stability between the electrolyte and the active material by doping or coating the cathode active material.

[0011] However, when the above-mentioned doping or coating treatment is performed, a problem arises in which the state of the cathode material and the structure or characteristics of the lithium secondary battery change significantly depending on the process sequence or conditions, and the added doping or coating components.

[0012] In particular, when doping a cathode active material with two or more multi-components rather than a single component, there is a problem in that the unique effects that each component is supposed to exhibit are not realized due to side reactions between the components.

[0013] Therefore, there is a need for a method to manufacture cathode active materials for lithium secondary batteries that can secure high energy density and high power output through a doping process that improves the uniformity of cathode material particles while simultaneously suppressing side reactions. The problem to be solved

[0014] The present invention aims to provide a positive electrode active material for a lithium secondary battery with excellent press density characteristics due to improved particle uniformity, and a method for manufacturing the same.

[0015] In addition, the present invention aims to provide a positive electrode active material for a lithium secondary battery with improved output characteristics due to c-axis expansion within the lattice, and a method for manufacturing the same.

[0016] The objects of the present invention are not limited to those mentioned above, and other unmentioned objects and advantages of the present invention may be understood from the following description and will be more clearly understood by the embodiments of the present invention. Furthermore, it will be readily apparent that the objects and advantages of the present invention can be realized by the means and combinations thereof set forth in the claims. means of solving the problem

[0017] To achieve the above objectives, one embodiment of the present invention provides a positive electrode active material for a lithium secondary battery comprising lithium transition metal oxide particles containing lithium, nickel, cobalt, manganese, and a doping element, wherein the doping element includes tungsten and fluorine components, and the side reaction between the tungsten and fluorine components of the doping element is suppressed.

[0019] To achieve the above objectives, another embodiment of the present invention provides a method for manufacturing a positive electrode active material for a lithium secondary battery, comprising the steps of: forming a mixture comprising a metal hydroxide precursor, a first doping raw material comprising fluorine, and a lithium raw material; calcining the mixture first; dissolving the first calcined product; and second calcining a mixture comprising the first calcined and dissolving product and a second doping raw material comprising tungsten, wherein the first calcination temperature is higher than the second calcination temperature.

[0021] In addition, the present invention provides a lithium secondary battery comprising a positive electrode including the aforementioned positive electrode active material for a lithium secondary battery; a negative electrode; and an electrolyte. Effects of the invention

[0022] The positive electrode active material for a lithium secondary battery according to the present invention has the effect of including two or more multi-components while not causing side reactions between each component.

[0023] As a result, the positive electrode active material for a lithium secondary battery according to the present invention has the effect of increasing energy density when applied to a lithium secondary battery by increasing the surface area of ​​the particles after the first calcination, thereby increasing the surface area receiving heat during the subsequent second calcination, sufficiently inducing lithium rearrangement, removal of residual lithium, and particle growth reactions within the positive electrode active material particles, improving the particle uniformity of the final calcined product, and improving the composite density of the positive electrode.

[0024] In addition, the positive electrode active material for a lithium secondary battery according to the present invention has the effect of improving output characteristics when applied to a lithium secondary battery by expanding the c-axis within the positive electrode active material lattice due to the expansion of the Li slab.

[0025] In addition, the method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention has the effect of easily manufacturing a positive electrode active material for a lithium secondary battery with improved particle uniformity and output characteristics by suppressing side reactions between doping elements through a simplified process by controlling the process steps and doping sequence in the manufacturing process of the positive electrode active material for a lithium secondary battery.

[0026] In addition, the lithium secondary battery according to the present invention has the advantage of excellent capacity and lifespan characteristics. Brief explanation of the drawing

[0027] Figure 1 is a graph showing the rate characteristics of a lithium secondary battery using the positive active materials of Examples 1 to 3 and Comparative Examples 1 and 2 of the present invention. Figure 2 is a Scanning Electron Image (SEM) of the positive electrode active material of Example 1 of the present invention. Figure 3 is an enlarged SEM image of Figure 2. Specific details for implementing the invention

[0028] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings so that those skilled in the art can easily implement the invention. The present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0029] To clearly explain the present invention, parts unrelated to the description have been omitted, and the same reference numerals are assigned to identical or similar components throughout the specification. Furthermore, some embodiments of the present invention are described in detail with reference to the exemplary drawings. In assigning reference numerals to the components of each drawing, identical components may have the same reference numeral whenever possible, even if they are shown in different drawings. Additionally, in describing the present invention, if it is determined that a detailed description of related known components or functions could obscure the essence of the present invention, such detailed description may be omitted.

[0030] In describing the components of the present invention, terms such as first, second, A, B, (a), (b), etc., may be used. These terms are intended only to distinguish the components from other components, and the nature, order, sequence, or number of the components are not limited by these terms. Where it is stated that a component is "connected," "combined," or "connected" to another component, it should be understood that the component may be directly connected or connected to the other component, but that other components may be "interposed" between each component, or that each component may be "connected," "combined," or "connected" through other components.

[0032] Cathode active material for lithium secondary batteries

[0033] One aspect of the present invention relates to a positive electrode active material for a lithium secondary battery, comprising lithium transition metal oxide particles containing lithium, nickel, cobalt, manganese, and a doping element, wherein the doping element includes tungsten and fluorine, is in the form of a single particle, and the cation mixing ratio of nickel cations in the lithium layer within the crystal structure of the lithium transition metal oxide particles is 1.0 to 1.8%.

[0034] The above mixing ratio can be quantitatively measured through XRD (X-Ray Diffraction) analysis using the WPPF (Whole Powder Pattern Fitting) analysis method.

[0035] The lithium transition metal oxide according to the present invention may have a layered crystal structure.

[0037] Conventional positive electrode active materials for lithium secondary batteries have generally used positive electrode active material particles in the form of secondary particles formed by the aggregation of tens to hundreds of primary particles.

[0038] In the present invention, “primary particle” refers to a minimum particle unit that is distinguished as a single mass when the cross-section of the positive active material is observed through a scanning electron microscope (SEM), and may consist of a single crystal grain or a plurality of crystal grains.

[0039] Here, “grain” refers to a region in which atoms within a primary particle form a lattice structure in a specific direction.

[0040] In addition, “secondary particles” refers to aggregates formed by the aggregation of tens to hundreds of primary particles through physical or chemical bonding between primary particles without any intentional aggregation or assembly process of the primary particles, i.e., secondary structures.

[0041] In the present invention, the term “single particle” refers to a form in which various raw materials constituting the cathode active material, such as nickel, cobalt, and manganese, are combined into a single particle structure.

[0042] However, as derived from the dictionary definition of the term "single particle" above, the single particle in the present invention does not refer only to a single crystal consisting of a single grain.

[0043] The single particle in the present invention is a term used to distinguish it from the conventional positive active material particle, and refers to a particle that contains one primary particle or grain within a single particle, or contains an aggregate of 20 to 30 or fewer primary particles.

[0044] Therefore, single-crystal particles are also included in the single-particle concept of the present invention.

[0046] The positive electrode active material for a lithium secondary battery according to the present invention contains fluorine and tungsten as doping elements.

[0047] At this time, the above fluorine can be doped in the form of a fluorine compound.

[0048] As a specific and non-limiting example, the above fluorine compound may be LiF or NH4F.

[0049] The above fluorine compound can be doped in an amount of 0.003 to 0.005 mol% of the Li equivalent or 0.001 to 0.002 weight % relative to the total weight of the cathode active material.

[0050] When the amount of the above-mentioned fluorine compound added is less than 0.003 mol%, the effect of adding the fluorine compound is not clearly observed.

[0051] On the other hand, if the amount of fluorine compound added exceeds 0.005 mol%, it is undesirable because the battery performance decreases due to an increase in cation mixing (Li / Ni disordering).

[0052] When the above fluorine compound is added, Lia[NixCoyMnzMw]O with the chemical formula 2-x F x (Here, Mw is W, 0.8≤a≤1.3, 0.8≤x<1, 0 <y<0.08, 0<z<0.08, 0<w≤0.04이며, x+y+z+w=1이다.)와 같이 불소가 산소를 치환한다.

[0053] However, the bonding force between transition metals (Ni, Co, Mn) and fluorine is stronger than the bonding force between transition metals and oxygen.

[0054] Therefore, the strong bonding force of the substituted fluorine can suppress oxygen release within the lithium transition metal oxide structure.

[0055] In addition, because the bond length between the transition metal and fluorine is shorter than the bond length between the transition metal and oxygen, the Li slab (c-axis) within the layered crystal structure of the lithium transition metal oxide expands, facilitating the deintercalation of Li.

[0056] On the other hand, when fluorine compounds such as LiF, NH4F, ZrF4, and AlF3 are coated on the surface of the cathode active material rather than being doped, side reactions between the electrolyte and the cathode active material are suppressed. Therefore, it is difficult to expect the ease of Li deintercalation and the effect of suppressing oxygen generation obtained through oxygen substitution via doping with fluorine compounds as in the present invention.

[0058] Furthermore, when tungsten is doped with fluorine as an anion, the diffusion of lithium within the crystal of the positive electrode active material is facilitated, and as a result, the output characteristics of the battery can be further improved.

[0059] At this time, the tungsten mentioned above may be doped in the form of tungsten oxide as a specific example, although this is not limited to specific examples.

[0060] The tungsten oxide can be doped in an amount of 0.002 to 0.0015 mol% of the Li equivalent or 0.06 to 0.15 weight % relative to the total weight of the cathode active material.

[0061] When the amount of the above-mentioned tungsten oxide added is less than 0.002 mol%, the effect of adding tungsten oxide is not clearly observed.

[0062] On the other hand, if the amount of tungsten oxide added exceeds 0.0016 mol%, it is undesirable because there is a concern that the structural stability of NMC oxide will decrease, leading to reduced high-temperature stability and increased gas generation.

[0064] Meanwhile, it is not desirable for the above-mentioned fluorine and tungsten to be simultaneously introduced and doped in any one of the steps or processes of manufacturing the cathode active material.

[0065] This is because if a fluorine compound and a tungsten oxide are mixed and calcined to simultaneously dope fluorine and tungsten, there is a possibility that fluorine, which is more reactive than oxygen, will inhibit the doping of tungsten and preferentially form a tungsten-fluorine compound.

[0066] The positive electrode active material for a lithium secondary battery according to the present invention has the advantage of being able to improve output characteristics when applied to a lithium secondary battery due to the composite doping of fluorine and tungsten and the characteristics of the manufacturing method described below.

[0068] In one embodiment of the present invention, the positive electrode active material for a lithium secondary battery has a specific surface area of ​​0.40 to 0.55 m² / g.

[0069] Specifically, the above specific surface area is the BET specific surface area, which can be measured using the BET method (Surface area and Porosity analyzer) (Micromeritics, ASAP2020).

[0070] The positive electrode active material for a lithium secondary battery according to the present invention can suppress the problem of lifespan characteristics deteriorating as particle strength increases by satisfying the above range of specific surface area.

[0072] In another embodiment of the present invention, the positive electrode active material for a lithium secondary battery may have a residual lithium content of 0.5 weight% or less, specifically 0.45 weight% or less, more specifically 0.4 weight% or less with respect to the total lithium transition metal oxide particles.

[0073] The above residual lithium amount can be measured using an automatic titrator.

[0075] In another embodiment of the present invention, based on 1 mole of the total of the nickel, cobalt, manganese, and doping elements, the content of the nickel may be 0.9 mole or more.

[0076] In other words, the positive electrode active material for a lithium secondary battery according to the present invention may be a high-nickel positive electrode active material.

[0077] Specifically, the positive electrode active material for a lithium secondary battery according to the present invention may be a high-nickel positive electrode active material containing nickel and manganese.

[0079] In another embodiment of the present invention, the positive electrode active material for a lithium secondary battery has an average particle size (D 50 ) can be 3.0 to 4.0 μm.

[0080] In the present invention, “average particle size (D 50 ")" refers to the particle size corresponding to 50% of the volume accumulation in the particle size distribution curve.

[0081] The above average particle size (D 50 ) can be measured, for example, using the laser diffraction method.

[0083] In another embodiment of the present invention, the positive electrode active material for a lithium secondary battery may have a Press Density (g / cc) of 2.0 or higher, more preferably 2.2 or higher.

[0084] The above-mentioned positive electrode active material for a lithium secondary battery can improve the composite density of the electrode as the Press Density increases, and as a result, the energy density of the electrode increases.

[0085] The “Press Density” in the present invention was measured using a Micromeritics Geopyc 1360 instrument.

[0086] Specifically, the above Press Density is achieved by placing 10g of the obtained sintered product into a mold with a diameter of 1.91 cm and then applying pressure with a force of 108 N.

[0087] The density of the compressed active material can be measured reproducibly by measuring the volume inside the mold after pressurization.

[0089] In another embodiment of the present invention, the ratio of particles having a diameter of 1 μm or less (equivalent diameter) after 9 ton pressing of the positive electrode active material for a lithium secondary battery may be 2.0% or less of the total particles (based on vol. %, and the same applies hereinafter), preferably 1.7% or less, and more preferably 1.0% or less.

[0090] In particular, when the positive electrode active material for a lithium secondary battery is a single crystal, the lower the “ratio of particles smaller than 1 μm after 9 ton press” of the positive electrode active material for the lithium secondary battery, the higher the degree of single crystallization of the single crystal due to the sintering process.

[0091] The method for measuring the “ratio of particles 1㎛ or less after 9 ton pressing” in the present invention is as follows.

[0092] First, 3.00 g of a positive active material sample was placed into a mold with a diameter of 1.3 cm, and then pressurized with a force of 67.8 kN / cm² (9 ton). The pressurized positive active material in the form of pellets was then placed in a mortar and pestle and ground to break up the clumped particles.

[0093] Afterwards, 0.01g of cathode active material was added to 61mL of 10wt% (NaPO3) as a dispersant, and ultrasonic treatment was performed for 1 minute.

[0094] Afterwards, particle size analysis was performed using Malvern (MS3000) equipment to obtain a particle size distribution curve, and the proportion of particles smaller than 1㎛ that increased after pressing compared to before pressing was measured in the particle size distribution results.

[0096] In another embodiment of the present invention, the positive electrode active material for a lithium secondary battery is a lithium transition metal oxide particle containing doping elements of tungsten and fluorine components, and is a lithium transition metal oxide particle in which side reactions between tungsten and fluorine components are suppressed, that is, in other words, doping of fluorine within the tungsten oxide is suppressed.

[0097] Fluorine and tungsten components are prone to causing side reactions during the doping process due to the strong chemical bonding characteristics of the fluorine component.

[0098] It is known that if a side reaction occurs when a fluorine component reacts with a tungsten component, a fluorine-doped tungsten peak (F-doped W peak) is observed in the 30–44 eV range of the XPS (X-ray Photo Electron Spectroscopy) spectrum, which particularly indicates the binding state of the 4f electrons of tungsten.

[0099] Therefore, by measuring the 4f peak of the tungsten in the 30–44 eV range of the XPS (X-ray Photo Electron Spectroscopy) spectrum as described above, the occurrence of side reactions between the fluorine component and the tungsten component can be easily measured.

[0100] The XPS observation in the present invention was performed using the K-ALPHA+ equipment of Thermo Fisher Scientific (UK).

[0101] First, the specimen can use an electrode made by mixing a positive active material with a conductive agent and a binder.

[0102] First, by repeating the process of performing XPS measurement on the surface of the specimen, etching, and then XPS measurement on the etched surface, the chemical bonding of the positive active material within a few μm in the depth direction of the specimen can be confirmed.

[0104] Method for manufacturing a positive electrode active material for a lithium secondary battery

[0105] Another aspect of the present invention relates to a method for manufacturing a positive electrode active material for a secondary battery, comprising the steps of: forming a mixture comprising a metal hydroxide precursor and a lithium raw material; mixing the mixture with a fluorine compound and performing a first calcination to obtain a calcined product; grinding and crushing the calcined product using a jet mill to obtain a metal oxide; and mixing the metal oxide with tungsten oxide and performing a second calcination to obtain lithium transition metal oxide particles in the form of single particles, wherein the metal hydroxide precursor contains nickel, cobalt, and manganese.

[0106] The method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention has the advantage of suppressing unwanted reactions and further increasing productivity compared to conventional single-particle manufacturing methods (e.g., multi-stage sintering) by separating the calcination process into a first calcination and a second calcination.

[0107] The above “multi-stage firing” may refer to a firing method in which only the temperature is changed within a single firing furnace, without including processes such as cooling, grinding, crushing, or mixing of doping materials between two or more firing stages with different firing temperatures.

[0108] Unlike the multi-stage firing described above, the first and second firing according to the present invention may be performed through one or two or more separate firing furnaces, including at least one process such as cooling, grinding, crushing, and mixing of doping materials between two or more firing stages with different firing temperatures.

[0109] In addition, the method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention has the advantage of suppressing unwanted side reactions compared to conventional single-particle manufacturing methods and further increasing productivity by separating the calcination process into a first calcination and a second calcination.

[0111] Mixture formation step

[0112] A method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention comprises the steps of forming a metal hydroxide precursor and forming a mixture comprising a lithium raw material and a first doping raw material.

[0113] The above metal hydroxide precursor contains one or more selected from the group consisting of Ni, Co, and Mn.

[0114] Specifically, the above metal hydroxide precursor may be purchased and used, or it may be manufactured directly using conventional methods practiced in the industry.

[0115] For example, the metal hydroxide precursor may be prepared by co-precipitating a metal-containing solution containing a complexing agent and a pH adjuster by adding them to a metal-containing solution containing a nickel raw material, a manganese raw material, or a cobalt raw material, but is not limited thereto.

[0117] The above nickel raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors.

[0118] For example, the nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, nickel fatty acid salts, nickel halides, or combinations thereof, but is not limited thereto.

[0120] The above-mentioned cobalt raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors.

[0121] For example, the above cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically may be CoSO4, CoSO4ㆍ7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2ㆍ4H2O, Co(NO3)2ㆍ6H2O or a combination thereof, but is not limited thereto.

[0123] The above manganese raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors.

[0124] For example, the above manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, and specifically, may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.

[0126] The above metal-containing solution may be prepared by adding a nickel raw material, a manganese raw material, or a cobalt raw material to a solvent, specifically water, or a mixture of water and an organic solvent that can be uniformly mixed with water (e.g., alcohol).

[0127] The above-mentioned complexing agent-containing solution performs the role of forming a complex, and may include, for example, NH3, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, NH4CO3, or a combination thereof as the complexing agent, but is not limited thereto.

[0128] Meanwhile, the above-mentioned complexing agent-containing solution may be used in the form of an aqueous solution, and in this case, water or a mixture of water and an organic solvent that is uniformly miscible with water (e.g., alcohol) may be used as the solvent.

[0129] The above pH-adjusting solution acts as a precipitating agent or pH regulator and may include alkali compounds such as hydroxides of alkali metals or alkaline earth metals like NaOH, KOH, or Ca(OH)2, hydrates thereof, or combinations thereof.

[0130] Meanwhile, the above-mentioned solution containing the pH adjuster can also be used in the form of an aqueous solution, and in this case, water or a mixture of water and an organic solvent that is uniformly miscible with water (e.g., alcohol) can be used as the solvent.

[0131] At this time, the solution containing the pH adjuster can be added in an amount such that the pH of the reaction solution becomes 10 to 13.

[0132] The above co-precipitation reaction can be carried out under an inert atmosphere such as nitrogen or argon, at a temperature of 30 to 70°C, and at a pH of 10 to 13.

[0133] By the above process, particles of nickel (or manganese-cobalt) hydroxide are generated and precipitated in the reaction solution. The precipitated precursor particles can be separated by conventional methods, washed, and dried to obtain the precursor.

[0134] At this time, the molar ratio of nickel, cobalt, or manganese in the precursor can be controlled by adjusting the concentration of the nickel raw material, cobalt raw material, or manganese raw material.

[0135] That is, the concentrations of nickel raw material, cobalt raw material, and manganese raw material can be controlled so that the molar ratio of nickel, cobalt, or manganese in the final product, lithium transition metal oxide, falls within the range according to the present invention.

[0137] The above-mentioned first doping raw material contains fluorine.

[0138] As a doping element, the aforementioned details can be applied to fluorine.

[0139] Specifically, the above fluorine can be added to satisfy the content included in the positive electrode active material for a lithium secondary battery according to the present invention.

[0141] The above lithium raw material may be lithium-containing sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or oxyhydroxides, and is not particularly limited as long as it is soluble in water.

[0142] Specifically, the above lithium raw material may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a combination thereof, but is not limited thereto.

[0143] The above lithium raw material can be introduced such that the molar ratio of lithium (Li / Me) to the total metal in the metal hydroxide precursor and the doping element is 1.02 to 1.08, preferably 1.02 to 1.05.

[0144] Although we do not wish to be limited by theory, the above lithium raw material may be partially lost during the oxidation process.

[0145] It is desirable that when the input amount of the above lithium raw material satisfies the above range, a positive electrode active material for a lithium secondary battery having a desired composition can be obtained.

[0147] First firing stage

[0148] The method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention includes the step of obtaining a calcined product by first calcining the mixture containing the first doping raw material containing a fluorine component at 840 to 890°C.

[0149] It is desirable that the above primary firing be performed within the above temperature range, as this can suppress the phenomenon of overgrowth particles or undergrowth particles being generated.

[0150] In addition, it is desirable to form an appropriate anion mixing ratio of fluoride anions in the lithium and transition metal layers within the crystal structure of the lithium transition metal oxide particles.

[0151] In another embodiment of the present invention, the first firing may be performed for 2 to 6 hours.

[0152] It is desirable that the above first firing is performed within the above time range, as this allows the crystal grain size to grow sufficiently and an anode active material with a high degree of single-particle size to be easily obtained.

[0154] The stage of disintegration

[0155] A method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention comprises the step of obtaining a metal oxide by grinding and / or disintegrating the calcined material using a jet mill.

[0156] Although disintegration is generally performed after the calcination is completed, the method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention undergoes a disintegration step, specifically grinding and disintegration, between the first calcination and the second calcination.

[0157] In another embodiment of the present invention, the grinding and / or disintegration may be performed by cooling the calcined material to a temperature of 50 to 200°C, preferably 50 to 100°C.

[0158] Cooling to the above cooling temperature can be carried out at room temperature, and cooling to the above cooling temperature is desirable as it can suppress the reaction between external moisture and the calcined product and suppress the increase in residual lithium.

[0160] The above grinding and / or crushing can be performed using a jet mill at a pressure of 2.0 to 5.0 bar, preferably 3.0 to 4.5 bar, and more preferably 3.5 to 4.0 bar.

[0161] When the above grinding and / or disintegration is performed at a pressure within the above range, the single-particle cathode active material grown through the secondary calcination described later has an appropriate particle size and can provide excellent lifespan characteristics when applied to a lithium secondary battery, which is desirable.

[0162] Compared to rotary mills, ball mills, fin mills, bead mills, and roll mills, the above-mentioned jet mill has the advantage of being able to grind various materials and perform dry grinding and crushing of materials without contamination.

[0163] In particular, it is desirable because it offers the advantage of enabling quality control with consistent particle sizes during repetitive production, as various particle sizes can be controlled.

[0164] Prior to the step of obtaining a metal oxide by grinding and / or disintegrating the above-mentioned calcined product using a jet mill at a pressure of 2.0 to 5.0 bar, the method may further include, but is not limited to, a step of disintegrating the above-mentioned calcined product using a rotor mill, ball mill, fin mill, bead mill, roll mill equipment, etc.

[0165] The disintegration conditions of the disintegration step using the above-mentioned rotor mill, ball mill, pin mill, bead mill, roll mill equipment, etc., can be appropriately performed within a range that does not impede the purpose of the present invention, and are not specifically limited thereto in the present invention.

[0167] Second firing stage

[0168] The method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention includes the step of mixing a second doping raw material containing a tungsten component with the metal oxide that has been first calcined and broken down, and then secondarily calcining the mixture at 750 to 850°C to obtain lithium transition metal oxide particles in the form of single particles.

[0170] The above second doping raw material contains tungsten.

[0171] As a doping element, tungsten can be applied to the aforementioned content.

[0172] Specifically, the tungsten can be added to satisfy the content included in the positive electrode active material for a lithium secondary battery according to the present invention.

[0174] The method for manufacturing a positive electrode active material for a lithium secondary battery according to the present invention involves crushing and disintegrating a fluorine-doped primary calcined product to mix the ungrown metal oxide with tungsten oxide and then regrowing it through secondary calcination, thereby allowing the first doping element and the second doping element to be doped at oxygen and transition metal positions, respectively, without side reactions, so as to obtain a positive electrode active material for a secondary battery with improved particle size distribution and structural stability.

[0175] The above secondary firing can preferably be performed at 750 to 850°C, more preferably at 780 to 820°C.

[0176] Therefore, in the calcination process for manufacturing a single-particle cathode active material, since it is advantageous for single particles to be formed when primary particles or crystal grains grow significantly, it is desirable that the secondary calcination temperature be lower than the previous primary calcination temperature.

[0177] It is desirable that the crystal structure of the lithium transition metal oxide particles obtained is stabilized when the above secondary calcination is performed particularly within the above temperature range.

[0178] Specifically, by doping the transition metal position of the lithium transition metal oxide particle with tungsten, a second doping element, and doping the oxygen position with fluorine, a first doping element, through the previous first calcination, it becomes possible to manufacture an anode active material in which the composite density and single crystallinity of the anode active material particle increase and the lithium slab (Li slab) is expanded.

[0179] Accordingly, the energy density of the positive electrode active material can be increased, and a high-output lithium secondary battery can be obtained.

[0181] The above secondary firing may be performed for 8 to 12 hours, but is not limited thereto.

[0182] When the above secondary calcination is performed within the above time range, it is desirable that the lithium byproducts remaining on the surface of the lithium transition metal oxide particles are sufficiently decomposed by heat and diffused into the interior of the lithium transition metal oxide particles.

[0184] In another embodiment of the present invention, based on 1 mole of the total of the nickel, manganese, and doping elements, the content of the nickel may be 0.9 mole or more.

[0185] The lithium metal oxide particles after the above secondary calcination is completed may additionally undergo a step of disintegration, but are not limited thereto.

[0186] At this time, crushing can be performed using rotary mill, ball mill, pin mill, bead mill, roll mill equipment, etc., and the crushing conditions are not particularly limited as long as they are within a range that does not impede the purpose of the present invention.

[0188] Lithium secondary battery

[0189] Another aspect of the present invention relates to a lithium secondary battery comprising a positive electrode comprising the aforementioned positive electrode active material for a lithium secondary battery; a negative electrode; and an electrolyte.

[0190] In summary, another aspect of the present invention relates to a lithium secondary battery comprising: a positive electrode; a negative electrode; and an electrolyte; wherein the positive electrode active material for a lithium secondary battery comprises lithium metal oxide particles containing lithium, nickel, cobalt, manganese, and a doping element, wherein the doping element comprises fluorine and tungsten and is in the form of a single particle.

[0191] Specifically, the above-mentioned positive electrode may include a positive electrode active material layer containing the aforementioned positive electrode active material for a lithium secondary battery.

[0192] The positive active material layer for the lithium secondary battery described above may include a binder and a conductive material.

[0193] The above binder can perform the role of effectively attaching the positive active material particles for the lithium secondary battery to each other, and also effectively attaching the positive active material for the lithium secondary battery to the current collector.

[0194] The above conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any electronically conductive material that does not cause chemical changes can be used.

[0195] The above-mentioned cathode includes a current collector and a cathode active material layer formed on the current collector, and the cathode active material layer may include a cathode active material.

[0196] The above negative electrode active material may include a material capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a material capable of doping and dedoping lithium, or a transition metal oxide.

[0197] The material capable of reversibly intercalating / deintercalating the above lithium ions may be, for example, a carbon material, and any carbon-based negative electrode active material generally used in the above lithium secondary battery may be used.

[0198] For example, crystalline carbon, amorphous carbon, or a combination thereof can be used.

[0199] As the above lithium metal alloy, an alloy of a metal selected from the group consisting of lithium, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn may be used.

[0200] Examples of materials capable of doping and dedoping the above lithium include Si, SiOx (0 < x < 2), Si-Y alloy (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), Sn, SnO2, Sn-Y (wherein Y is an element selected from the group consisting of alkali metals, alkaline earth metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Sn).

[0201] Examples of the above transition metal oxides include vanadium oxide, lithium vanadium oxide, etc. The above negative electrode active material layer also includes a binder and may optionally further include a conductive material.

[0202] The above binder can serve to effectively attach the negative electrode active material particles to each other and also effectively attach the negative electrode active material to the current collector.

[0203] The above conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any electronically conductive material that does not cause chemical changes can be used.

[0204] For example, the above current collector may be selected from the group consisting of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0205] The above-mentioned cathode and anode may be manufactured by preparing an active material composition by mixing an active material, a conductive material, and a binder in a solvent, and applying the composition to a current collector, and the present invention does not limit the method of manufacturing the electrodes.

[0206] The above solvent may include N-methylpyrrolidone, but is not limited thereto.

[0207] The above electrolyte may be a non-aqueous electrolyte or a solid electrolyte, and may be used in which a lithium salt is dissolved.

[0208] The above-mentioned non-aqueous electrolyte may include an organic solvent, and the above-mentioned non-aqueous organic solvent may serve as a medium through which ions involved in the electrochemical reaction of the battery can move.

[0209] The above organic solvent may be, for example, cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate; chain carbonates such as dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate; esters such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone; ethers such as 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 1,2-dioxane, 2-methyltetrahydrofuran; nitriles such as acetonitrile; amides such as dimethylformamide. These may be used individually or in combination.

[0210] In particular, a mixed solvent of cyclic carbonates and chain carbonates can be preferably used.

[0211] In addition, as an electrolyte, a gel-type polymer electrolyte in which an electrolyte solution is impregnated into a polymer electrolyte such as polyethylene oxide or polyacrylonitrile, or an inorganic solid electrolyte such as LiI or Li3N, is possible.

[0212] The above lithium salt is a material that is dissolved in an organic solvent and acts as a source of lithium ions within the battery, enabling the operation of a basic lithium secondary battery and facilitating the movement of lithium ions between the positive and negative electrodes.

[0213] The above lithium salt may be any commonly used in the art without limitation, provided that it does not impede the purpose of the present invention.

[0214] For example, the lithium salt may be one selected from the group consisting of LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiSbF6, LiAlO4, LiAlCl4, LiCl, and LiI.

[0215] Depending on the type of the above lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof may be used, and of course, mixed multilayer films such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may be used.

[0216] Lithium secondary batteries can be classified into lithium-ion batteries, lithium-ion polymer batteries, and lithium polymer batteries depending on the type of separator and electrolyte used; they can be classified into cylindrical, prismatic, coin, and pouch types depending on their shape; and they can be divided into bulk and thin-film types depending on their size.

[0217] The present invention does not limit the structure and manufacturing method of the battery.

[0218] Preferred embodiments and comparative examples of the present invention are described below. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.

[0220] <Example>

[0222] Preparation of NCM precursors

[0223] The positive active material precursor was prepared by a general co-precipitation method.

[0224] NiSO4·6H2O was used as the nickel source material, CoSO4·7H2O as the cobalt source material, and MnSO4·H2O as the manganese source material. These raw materials were dissolved in distilled water to prepare aqueous metal salt solutions.

[0225] After preparing the co-precipitation reactor, N2 was purged to prevent oxidation of metal ions during the co-precipitation reaction.

[0226] The reactor temperature was maintained at 50℃.

[0227] NH4(OH) was added as a chelating agent to the co-precipitation reactor, and NaOH was used to adjust the pH. The precipitate obtained from the co-precipitation process was filtered, washed with distilled water, and dried in a 180°C cake dryer to prepare a cathode active material precursor.

[0228] The composition of the manufactured precursor is (Ni 0.90 Co 0.05 Mn 0.05 It was )(OH)2.

[0230] Manufacturing of cathode active material for lithium secondary batteries

[0231] Example 1

[0232] A metal hydroxide precursor prepared according to the preparation example, LiOH·H2O, and LiF as the first doping raw material were introduced into the mixer and mechanically mixed to form a mixture.

[0233] At this time, LiOH·H2O was added so that the molar ratio of lithium to the total metal in the metal precursor (Li / Me) was 1.02, and LiF was added at 0.003 mol. %.

[0234] Afterwards, first firing was performed for 4 hours at the firing temperature according to Table 1 below.

[0235] The above first calcined product was crushed using a jet mill.

[0236] The above first calcined and crushed calcined product and WO3 as the second doping raw material were fed into the mixer and mechanically mixed to form a mixture.

[0237] At this time, WO3 was added at a rate of 0.0002 mol. %.

[0238] Afterwards, a second firing was performed for 8 hours at the firing temperature according to Table 1 below.

[0240] Example 2

[0241] A positive electrode active material was prepared in the same manner as in Example 1, except that the amount of WO3 added was 0.0005 mol.%.

[0243] Example 3

[0244] A positive electrode active material was prepared in the same manner as in Example 1, except that the amount of WO3 added was 0.001 mol.%.

[0246] Example 4

[0247] A positive electrode active material was prepared in the same manner as in Example 1, except that the amount of LiF added was 0.006 mol. % and the amount of WO3 added was 0.0005 mol. %.

[0249] Example 5

[0250] A positive electrode active material was prepared in the same manner as in Example 1, except that the amount of LiF added was 0.006 mol.% and the amount of WO3 added was 0.001 mol.%.

[0252] Comparative Example 1

[0253] A metal hydroxide precursor prepared according to the preparation example, LiOH·H2O, and doping elements LiF and WO3 were fed into the above mixer and mechanically mixed to form a mixture.

[0254] At this time, LiOH·H2O was added so that the molar ratio of lithium to the total metal in the metal precursor (Li / Me) was 1.02, LiF was added at 0.003 mol. %, and WO3 was added at 0.0002 mol. %.

[0255] Afterwards, it was fired under firing conditions maintained at 870℃ for 4 hours, followed by maintaining at 800℃ for 8 hours.

[0256] The continuously fired sintered product was crushed using a jet mill.

[0258] Comparative Example 2

[0259] A positive electrode active material was prepared in the same manner as in Example 1, except that the first doping raw material was not included in the first calcination and the second doping raw material was not included in the second calcination.

[0261] Table 1 below shows the manufacturing methods of Examples 1 to 5 and Comparative Examples 1 and 2.

[0263] Types of firing Temperature (°C) LiF content mol.% WO 3 Content mol.% Comparative Example 1 Multistage firing 870 (4h) - 800 (8h) 0.003 0.0002 Comparative Example 2 1st and 2nd firing 1st round 870 (4h) / 2nd round 800 (8h) X X Example 1 1st and 2nd firing 1st round 870 (4h) / 2nd round 800 (8h) 0.003 0.0002 Example 2 1st and 2nd firing 1st round 870 (4h) / 2nd round 800 (8h) 0.003 0.0005 Example 3 1st and 2nd firing 1st round 870 (4h) / 2nd round 800 (8h) 0.003 0.001 Example 4 1st and 2nd firing 1st round 870 (4h) / 2nd round 800 (8h) 0.006 0.0005 Example 5 1st and 2nd firing 1st round 870 (4h) / 2nd round 800 (8h) 0.006 0.001

[0265] The particle size of the positive active materials of Examples 1 to 5 and Comparative Examples 1 and 2 was measured, and the results are shown in Table 2 below.

[0266] At this time, the particle size was measured using the general method with laser diffraction.

[0268] D min D 5 D 10 D 50 D 90 D 95 D max Span Comparative Example 1 0.63 1.21 1.46 2.63 4.72 5.73 8.24 1.24 Comparative Example 2 1.78 2.48 2.78 4.13 6.40 7.33 9.66 0.88 Example 1 1.06 1.90 2.18 3.24 4.99 5.77 7.81 0.87 Example 2 1.26 2.11 2.38 3.45 5.20 5.97 7.93 0.82 Example 3 1.26 2.12 2.39 3.46 5.21 5.97 7.92 0.82 Example 4 1.50 2.26 2.53 3.67 5.54 6.34 8.31 0.82 Example 5 1.26 2.19 2.48 3.68 5.73 6.60 8.65 0.88

[0270] As shown in Table 2 above, Examples 1 to 5 were found to have a narrower particle size distribution, that is, a smaller span value, than Comparative Example 1, which was prepared using a multi-stage calcination process with the same doping raw material, as well as Comparative Example 2, which was prepared using a first and second calcination process without doping raw material.

[0271] In particular, Examples 2 to 4 showed that the span value was improved by approximately 8% more than Examples 1 and 5, as well as the comparative examples.

[0273] The press density (PD) and the ratio of particles smaller than 1 μm after pressing of the positive electrode active materials of Examples 1 to 5 and Comparative Examples 1 and 2 were measured and are shown in Table 3 below.

[0274] At this time, the particle size was measured using the general method with laser diffraction.

[0275] As explained above, the compressive density was determined by placing 10g of the positive active material into a mold and applying a pressure of 108N, after which the volume of the positive active material was measured.

[0276] As explained above, the ratio of particles smaller than 1 μm (volume %) after compression (press) was measured by placing 3 g of the positive active material into a mold using a Malvern MS3000 instrument, applying a force of 9 tons, obtaining the corresponding active material, and measuring the ratio of particles smaller than 1 μm (volume) to the total particles.

[0278] Press density (g / cc) Press 1 ㎛ Particle ratio (%) Comparative Example 1 2.01 7.26 Comparative Example 2 2.05 3.17 Example 1 2.21 1.63 Example 2 2.27 0.90 Example 3 2.28 0.95 Example 4 2.32 0.79 Example 5 2.29 1.00

[0280] As shown in Table 3 above, Examples 1 to 5 were found to have higher press density than Comparative Example 1, which was prepared using a multi-stage firing process with the same doping raw material, as well as Comparative Example 2, which was prepared using a first and second firing process without doping raw material.

[0281] Specifically, the Press Density values ​​of all of the above Examples 1 to 5 were measured to be improved by approximately 15% compared to Comparative Examples 1 and 2.

[0282] Furthermore, the ratio of particles smaller than 1 μm after pressing, in other words, the fine particle ratio, was measured to be reduced to nearly half or less in Examples 1 to 5 compared to Comparative Examples 1 and 2.

[0283] The results of Tables 2 and 3 above are in good agreement with the results of Table 2 above.

[0284] Specifically, as shown in Table 1, the positive electrode active materials of Examples 1 to 5 have improved particle uniformity compared to the positive electrode active materials of Comparative Examples 1 and 2 (particularly Comparative Example 1), and it is determined that this improvement in uniformity led to an increase in Press Density.

[0285] In addition, the fact that the above-mentioned fineness ratio in Table 3 is lower for the positive active materials of Examples 1 to 5 compared to the positive active materials of Comparative Examples 1 and 2 means that the positive active materials of Examples 1 to 5 have a higher degree of single crystallinity than the positive active materials of Comparative Examples 1 and 2.

[0287] Figures 2 and 3 are Scanning Electron Images (SEM) of the positive electrode active material of Example 1 of the present invention.

[0288] Figures 2 and 3 directly show that the positive active material of Example 1 of the present invention consists of only one or a few primary particles or crystal grains constituting each positive active material.

[0289] The results of Figures 2 and 3 above directly demonstrate that the anode active material of Example 1 of the present invention has a very high degree of single crystallinity.

[0290] Ultimately, it is determined that the high degree of single crystallinity of the cathode active materials of Examples 1 to 5 led to improvements in not only the particle size distribution but also the Press Density and fineness ratio.

[0292] Table 4 shows the crystallographic measurement results of the positive active materials of Examples 1 to 3 and Comparative Examples 1 and 2 above.

[0293] Table 4 above shows the results of XRD (X-Ray Diffraction) analysis using the WPPF (Whole Powder Pattern Fitting) analysis method.

[0295] WPPF XS(nm) WPPF Li / Ni(%) WPPF a(Å) WPPF c(Å) c / a Comparative Example 1 185 1.2 2.8769 14.1981 4.9352 Comparative Example 2 241 2.7 2.8792 14.1975 4.9311 Example 1 252 1.6 2.8766 14.1985 4.9359 Example 2 259 1.6 2.8768 14.1988 4.9356 Example 3 260 1.6 2.8769 14.1989 4.9355

[0297] As shown in Table 4 above, it was confirmed that Examples 1 to 3 not only increased the crystallite size compared to Comparative Examples 1 and 2, but also increased the size of the c-axis compared to Comparative Examples 1 and 2.

[0298] Furthermore, the results of Table 4 show that Examples 1 to 3 have excellent cation mixing at the 1.6% level (WPPF Li / Ni %) even though the c-axis is extended.

[0299] The results of Table 4 above are in good agreement with the results of Tables 1 to 3 above.

[0300] In other words, the cathode active materials of Examples 1 to 3 showed an increased degree of single crystallinity and a larger crystallite size compared to Comparative Examples 1 and 2, and it is determined that this increase in crystallite size improved not only the particle size distribution and structural stability but also the Press Density and fineness ratio.

[0302] Meanwhile, the results of Table 4 above are expected to improve the characteristics of lithium secondary batteries.

[0303] To verify this, a lithium secondary battery was manufactured using the positive electrode active material prepared according to the examples and comparative examples to investigate its electrochemical properties.

[0304] The slurry for manufacturing the electrode plate was prepared by mixing the above-prepared positive active material:conductive material (carbon black, Super C):binder (PVDF, KF1120) in a ratio of 96.5:1.5:2 wt%, and adding NMP (NMethyl-2-pyrrolidone) to adjust the viscosity so that the solid content was about 70%.

[0305] The manufactured slurry was coated onto a 20㎛ thick Al foil using a Doctor blade and then dry-rolled.

[0306] The electrode loading amount is 16.7 mg / cm²2 It was, and the rolled density (25℃) was 3.5 g / cm³ 3 It was.

[0307] A coin cell was manufactured using 1M LiPF6 in EC:DMC:EMC=3:4:3 (vol%) electrolyte with 3.0 wt% VC, 0.5 wt% PS, and 1.0 wt% ESA added relative to the total amount of electrolyte, and a PP separator and a lithium anode (200 μm, Welcos) were used.

[0309] Table 5 and Figure 1 show the results of measuring the rate capability of the positive electrode active materials of Examples 1 to 3 and Comparative Examples 1 and 2.

[0311] Specific capacity (mAh / g) CE (%) 0.1 / 0.2 0.2 / 0.5 0.5 / 1.0 1.0 / 2.0 Comparative Example 1 209.9 89.5 94.9 93.1 93.4 92.1 Comparative Example 2 198.2 86.3 95.0 93.8 94.0 92.5 Example 1 214.0 88.5 96.0 94.7 95.3 93.8 Example 2 211.9 88.2 95.6 94.2 94.8 93.0 Example 3 208.6 87.6 95.4 93.9 94.3 92.7

[0313] The rate capability in Table 5 above was measured using a GCD (galvanostatic charge-discharge, model name: PESC 05) under conditions of 45℃ after a 10 h rest.

[0314] The positive active materials of Examples 1 to 3 above exhibited higher rate characteristics than the positive active materials of Comparative Examples 1 and 2.

[0315] Table 5 above also shows the capacity retention rate when the C-rate changes.

[0316] For example, “0.1 / 0.2” in Table 5 above is the result of calculating the capacity at 0.2C based on the capacity at 0.1C when the C-rate changes from 0.1C to 0.2C.

[0317] Since capacity decreases when the C-rate increases, a large value in Table 5 above means that the capacity is maintained excellently even with changes in the C-rate.

[0318] The results of Table 5 above experimentally demonstrate that the cathode active materials of Examples 1 to 3 not only have superior specific capacity compared to Comparative Example 2, but also superior C-rate characteristics compared to Comparative Examples 1 and 2.

[0320] Generally, it is reported that positive electrode active materials for lithium secondary batteries having a layered crystal structure improve the output characteristics of the lithium secondary battery as the c-axis increases, thereby increasing the diffusion capacity of lithium.

[0321] On the other hand, if the c-axis increases excessively, cation mixing occurs, which causes anodic degradation.

[0322] Therefore, an increase in the c-axis represents a trade-off between the output characteristics of lithium secondary batteries and cathode degradation.

[0323] However, the results of Tables 4 and 5 in the embodiments of the present invention demonstrate that although the crystallite size and c-axis size of Examples 1 to 3 of the present invention increased compared to Comparative Examples 1 and 2, the cation mixing was excellent at the level of 1.6% (Table 4), and at the same time, the increase in c-axis size improved C-rate characteristics and suppressed irreversible capacity growth.

[0325] Although the present invention has been described above with reference to the illustrated drawings, the present invention is not limited by the embodiments and drawings disclosed in this specification, and it is obvious that various modifications can be made by a person skilled in the art within the scope of the technical concept of the present invention. Furthermore, even if the effects of the configuration of the present invention were not explicitly described while describing the embodiments of the present invention above, it is natural to acknowledge that the effects predictable by said configuration should also be recognized.

Claims

Claim 1 A method for manufacturing a positive electrode active material for a lithium secondary battery, comprising: (a) a step of forming a mixture comprising a metal hydroxide precursor, a first doping raw material comprising fluorine, and a lithium raw material; (b) a step of first calcining the mixture; and (c) a step of disintegrating the first calcined product; and (d) a step of second calcining a mixture comprising the first calcined and disintegrated product and a second doping raw material comprising tungsten; wherein the first calcination temperature is higher than the second calcination temperature. Claim 2 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the metal hydroxide precursor contains nickel, cobalt, and manganese. Claim 3 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 2, wherein the nickel content is 0.9 moles or more based on 1 mole of the total sum of the nickel, manganese, and doping elements. Claim 4 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the primary calcination is performed at 840 to 890°C. Claim 5 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 4, the first calcination is performed for 2 to 6 hours. Claim 6 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the first doping raw material containing fluorine is mixed in a ratio of 0.003 to 0.005 mol.% of the Li equivalent. Claim 7 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the disintegration is performed by cooling the primary calcined product to 50 to 200°C. Claim 8 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the secondary calcination is performed at 750 to 850°C. Claim 9 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 8, the secondary calcination is performed for 8 to 12 hours. Claim 10 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the second doping raw material containing tungsten is mixed in a ratio of 0.002 to 0.0015 mol.% of the Li equivalent.

Citation Information

Patent Citations

  • Manufacturing method of positive electrode active material

    KR1020210155367A