Composite separator, method for manufacturing the same, and lithium-sulfur battery containing the same

A composite separator with a cobalt-doped molecular sieve and conductive carbon material addresses the shuttle effect in lithium-sulfur batteries, enhancing battery performance by restricting Li2Sx diffusion and improving conductivity and lithium ion transport.

KR103047528B1Active Publication Date: 2026-11-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020257003066
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-06-28
Filing Date
2022-09-28
Publication Date
2026-11-11
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Lithium-sulfur batteries face challenges such as the shuttle effect, leading to poor battery rate capability, low capacity, and poor circulation performance, which hinder their application in high-energy density batteries for new energy electric vehicles and large-capacity energy storage systems.

Method used

A composite separator is developed comprising a polymer substrate with a composite layer containing a cobalt-doped molecular sieve and conductive carbon material, manufactured by mixing the molecular sieve with cobalt and optionally lithium, dispersing in a solvent, and applying the mixture to a polymer substrate film.

Benefits of technology

The composite separator effectively restricts the movement and diffusion of Li2Sx, reduces side reactions, enhances conductivity, and improves lithium ion transport, resulting in improved rate capability and circulation stability of lithium-sulfur batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025010564197-PCT00004_ABST
    Figure 112025010564197-PCT00004_ABST
Patent Text Reader

Abstract

The present invention relates to a composite separator and a method for manufacturing the same and applications, and to a lithium-sulfur battery comprising the composite separator. The composite separator comprises a polymer substrate and a composite layer distributed on the surface of the polymer substrate, wherein the composite layer comprises a molecular sieve and a conductive carbon material, and the molecular sieve comprises cobalt and optionally selected lithium. Compared to conventional separators, the surface of the composite separator of the present invention has a composite layer comprising a molecular sieve containing cobalt and optionally selected lithium, thereby significantly improving the rate capability and circulation stability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to the field of battery separators, and specifically to a composite separator, a method for manufacturing the same, and a lithium-sulfur battery containing the same. Background Technology

[0002] As science and technology advance rapidly, lithium-ion batteries are finding it difficult to meet the demand for higher energy density batteries in new energy electric vehicles and large-capacity energy storage systems due to the low specific capacity of their cathode materials. Lithium-sulfur batteries possess a relatively high specific capacity (1675 mAh / g) and a theoretical energy density (2600 Wh / kg), making them a promising alternative to lithium-ion batteries and a focal point of research for next-generation high-specific-energy rechargeable batteries. Furthermore, sulfur, an active material for the cathode, has the advantages of being abundant in natural resources, inexpensive, and environmentally friendly.

[0003] However, at the current stage, the practical application of lithium-sulfur batteries still faces many challenges, among which the "shuttle effect," a side reaction within the battery, is the biggest obstacle limiting its application. Specifically, the shuttle effect is a phenomenon in which lithium-sulfur batteries can generate a series of sulfur-containing intermediate products during the charging and discharging process, among which long-chain polysulfides (Li2S2) x , 2 <x≤8)는 전해액에 쉽게 용해되며, 농도 구배 및 전기장의 작용에 의해, 분리막을 통과하여 리튬 음극과 화학적 부반응이 발생함으로써, 활성 물질이 손실되고 전지 내부 저항이 커져, 전지 용량 감소 및 순환 성능 저하를 초래한다. 또한, 리튬-황 전지는 전기 화학적 반응 과정이 다단계 고액 전환과 관련되고, 황 및 방전 최종 생성물인 황화 리튬 전자의 도전성이 떨어지므로, 폴리설파이드 전환 반응의 동력학이 느리게 작용하고, 전지 율속 성능이 좋지 않다.

[0004] Currently, conventional technology modifies a conventional separator using molecular sieves such as CN107546356A and CN103490027A to suppress the shuttle effect of lithium-sulfur batteries. These improve battery performance by utilizing the physical blocking action of molecular sieves such as ZSM-5, SAPO-34, 3A, and 13X to limit the movement and diffusion of Li2Sx in the electrolyte to some extent.

[0005] In order for (lithium-sulfur) batteries to meet the demand for higher energy density batteries in new energy electric vehicles and large-capacity energy storage systems, it is still necessary to develop battery separators that realize further improvements in current performance. The problem to be solved

[0006] The objective of the present invention is to overcome the problems of poor battery rate capability, low battery capacity, and poor circulation performance present in the prior art. The inventors of the present invention have discovered that by using a molecular sieve containing cobalt and optionally selected lithium in a lithium-sulfur battery separator, the performance of the battery can be further improved, thereby satisfying the aforementioned requirements of the prior art. Accordingly, a composite separator comprising a composite layer of a molecular sieve containing cobalt and optionally selected lithium is provided. The composite separator of the present invention can improve the rate capability and circulation stability of the battery. The present invention also provides a method for manufacturing the composite separator and a lithium-sulfur battery comprising the composite separator. means of solving the problem

[0007] A first aspect of the present invention provides a composite separation membrane, wherein the composite separation membrane comprises a polymer substrate; and a composite layer distributed on the surface of the polymer substrate, wherein the composite layer comprises a molecular sieve and a conductive carbon material, and the molecular sieve contains cobalt.

[0008] A second aspect of the present invention provides a method for manufacturing the composite separation membrane, and the method comprises:

[0009] (1) A step of mixing a molecular sieve and a conductive carbon material to obtain a mixture, wherein the molecular sieve contains cobalt;

[0010] (2) A step of dispersing the above mixture and binder in a solvent to obtain a coating slurry;

[0011] (3) A step of applying the coating slurry above to the surface of a polymer substrate film, and then removing the solvent to obtain a composite separation film; is included.

[0012] A third aspect of the present invention provides an application of the separator in a lithium-sulfur battery.

[0013] A fourth aspect of the present invention provides a lithium-sulfur battery comprising a positive electrode, a negative electrode, and a composite separator located between the positive electrode and the negative electrode.

[0014] The present invention may be implemented by each of the following claims.

[0015] 1. A molecular sieve modified separation membrane is characterized in that the separation membrane comprises a polymer substrate membrane and a cobalt-doped molecular sieve / conductive carbon material composite layer distributed on the surface of the polymer substrate membrane.

[0016] 2. In the separator according to claim 1, the thickness of the cobalt-doped molecular sieve / conductive carbon material composite layer is 5-50 μm, preferably 10-40 μm; and / or

[0017] In the above cobalt-doped molecular sieve / conductive carbon material composite layer, the mass ratio of the conductive carbon material to the cobalt-doped molecular sieve is 1:(1-9), preferably 1:(2-9).

[0018] 3. In the separation membrane according to claim 1 or 2, the cobalt-doped molecular sieve has a chemical composition represented by the formula “aCo·bM2O·ySiO2·zAl2O3”, preferably the cobalt-doped molecular sieve is selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR, and more preferably the cobalt-doped molecular sieve is at least one of MFI, MWW, and GIS.

[0019] 0.02≤a / y≤0.2, 0.01≤b / y≤0.2, 10≤y / z≤50; M is an alkali metal element of group IA, preferably selected from one or more of Na, K, and Li;

[0020] Preferably, the cobalt-doped molecular sieve is a cobalt-doped lithiated molecular sieve, and the cobalt-doped lithiated molecular sieve has a chemical composition represented by the formula “aCo·bLi2O·ySiO2·zAl2O3”, with 0.02≤a / y≤0.2, 0.01≤b / y≤0.2, and 10≤y / z≤50.

[0021] 4. In a separation membrane according to any one of paragraphs 1 to 3,

[0022] The material of the polymer substrate film is at least one of polyethylene, polypropylene, polyimide, polyacrylonitrile, polyethylene terephthalate, polytetrafluoroethylene, and polyvinylidene fluoride, preferably polyethylene and / or polypropylene; and / or

[0023] The conductive carbon material is at least one of graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, carbon nanofibers, acetylene black, Super P, and Ketjen black, and preferably at least one of graphene, graphene oxide, and reduced graphene oxide.

[0024] 5. A method for manufacturing a molecular sieve modified separation membrane according to any one of claims 1 to 4,

[0025] The above method is,

[0026] (1) A step of grinding and mixing a cobalt-doped molecular sieve and a conductive carbon material to obtain a mixture of a cobalt-doped molecular sieve and a conductive carbon material;

[0027] (2) A step of dispersing the mixture of the cobalt-doped molecular sieve, the conductive carbon material, and the binder in a solvent to obtain a coating slurry;

[0028] (3) A step of applying the coating slurry above to the surface of a polymer substrate film, and then removing the solvent to obtain a molecular sieve modified separation film; characterized by including the above step.

[0029] 6. In the manufacturing method pursuant to Paragraph 5,

[0030] A method for manufacturing a cobalt-doped molecular sieve comprises the step of adding a cobalt ion solution to a Na-type molecular sieve and drying and reducing it to obtain a cobalt-doped molecular sieve.

[0031] Preferably, the above cobalt-doped molecular sieve is a cobalt-doped lithiated molecular sieve, and the manufacturing method is,

[0032] S1: A step of obtaining a precursor (I) after exchanging, washing, and drying a Na-type molecular sieve and a lithium ion solution;

[0033] S2: A step of adding a cobalt ion solution to a precursor (I), drying and reducing to obtain a cobalt-doped lithiated molecular sieve; comprising,

[0034] Here, preferably,

[0035] The lithium ion solution of S1 above is at least one of a lithium chloride solution, a lithium sulfate solution, and a lithium nitrate solution, and

[0036] The exchange conditions of the above S1 include a temperature of 40-100℃ and a liquid-solid ratio of 10-50;

[0037] The above Na-type molecular sieve has a chemical composition represented by the formula “bNa2O·ySiO2·zAl2O3”, with 0.01≤b / y≤0.2 and 10≤y / z≤50; preferably, the topological structure of the above Na-type molecular sieve is selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR;

[0038] The above cobalt ion solution is at least one of cobalt chloride solution, cobalt nitrate solution, cobalt sulfate solution, and cobalt acetate solution;

[0039] The above reduction conditions include a reduction atmosphere being a hydrogen gas atmosphere, a reduction temperature of 600-750℃, and a reduction time of 1-4h.

[0040] 7. In the manufacturing method according to claim 5 or 6, the solvent of step (2) is at least one of deionized water, anhydrous ethanol, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide and N-methylpyrrolidone, and preferably N-methylpyrrolidone.

[0041] 8. In a manufacturing method according to any one of claims 5 to 7, the binder in step (2) is at least one of polyvinyl alcohol, carboxymethylcellulose, polyvinylidene fluoride, polytetrafluoroethylene, polyvinylpyrrolidone, styrene-butadiene rubber, and polyacrylate, and preferably polyvinylidene fluoride.

[0042] 9. In a manufacturing method according to any one of paragraphs 5 through 8,

[0043] The application method of step (3) is at least one of casting coating, blade coating, spray coating, and spin coating, and preferably blade coating.

[0044] 10. Application of a molecular sieve-modified separator according to any one of claims 1 to 4 in a lithium-sulfur battery.

[0045] The present invention may also be implemented by each of the following claims.

[0046] 1. In a lithiated molecular sieve modified separator, the separator comprises a lithiated molecular sieve / conductive carbon material composite layer and a polymer substrate; the lithiated molecular sieve / conductive carbon material composite layer is distributed on the surface of the polymer substrate.

[0047] 2. In the lithiated molecular sieve modified separator according to claim 1, the lithiated molecular sieve is at least one of a lithiated MFI-type molecular sieve, a lithiated MWW-type molecular sieve, a lithiated GIS-type molecular sieve, a lithiated BEC-type molecular sieve, a lithiated FAU-type molecular sieve, and a lithiated MOR-type molecular sieve, and preferably at least one of a lithiated MFI-type molecular sieve, a lithiated MWW-type molecular sieve, and a lithiated GIS-type molecular sieve.

[0048] 3. In the lithiated molecular sieve modified separator according to claim 1 or 2, the material of the polymer substrate membrane is at least one of polyethylene, polypropylene, polyimide, polyacrylonitrile, polyethylene terephthalate, polytetrafluoroethylene, and polyvinylidene fluoride, and preferably polyethylene and / or polypropylene.

[0049] 4. In a lithiated molecular sieve modified separator according to any one of claims 1 to 3, the thickness of the lithiated molecular sieve / conductive carbon material composite layer is 2-40 μm, preferably 5-25 μm.

[0050] 5. In a lithiated molecular sieve modified separator according to any one of claims 1 to 4,

[0051] In the above lithiated molecular sieve / conductive carbon material composite layer, the mass ratio of the conductive carbon material to the lithiated molecular sieve is 1:(1-9), preferably 1:(2-9); and / or

[0052] The above lithiated molecular sieve has a chemical composition represented by the formula “xLi2O·ySiO2·zAl2O3”, with 0.01≤x / y≤0.2 and 10≤y / z≤50.

[0053] 6. In a lithiated molecular sieve modified separator according to any one of claims 1 to 5, the conductive carbon material is at least one of graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, carbon nanofibers, acetylene black, Super P, and Ketjenblack, and preferably at least one of graphene, graphene oxide, and reduced graphene oxide.

[0054] 7. A method for manufacturing a lithiated molecular sieve modified separator according to any one of claims 1 to 6, wherein the method comprises:

[0055] (1) A step of grinding and mixing a lithiated molecular sieve and a conductive carbon material to obtain a mixture of a lithiated molecular sieve and a conductive carbon material;

[0056] (2) A step of dispersing the mixture of the lithiated molecular sieve, the conductive carbon material, and the binder in a solvent to obtain a coating slurry;

[0057] (3) A step of applying the coating slurry above to the surface of a polymer substrate film, and then removing the solvent to obtain a molecular sieve modified separation film; characterized by including the above step.

[0058] 8. In the manufacturing method according to paragraph 7,

[0059] In step (2),

[0060] The above solvent is at least one of deionized water, anhydrous ethanol, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone, preferably N-methylpyrrolidone; and / or,

[0061] The binder is at least one of polyvinyl alcohol, polytetrafluoroethylene, polyvinylpyrrolidone, carboxymethylcellulose, styrene-butadiene rubber, polyvinylidene fluoride, and polyacrylate, preferably polyvinylidene fluoride; and / or,

[0062] The application method of step (3) is at least one of casting coating, blade coating, spray coating, and spin coating, and preferably is blade coating;

[0063] and / or

[0064] The above method for manufacturing a lithiated molecular sieve comprises the step of obtaining a Li-type molecular sieve after exchanging a Na-type molecular sieve with lithium ions, washing, and drying;

[0065] The above Na-type molecular sieve has a chemical composition represented by the formula “xNa2O·ySiO2·zAl2O3”, with 0.01≤x / y≤0.2 and 10≤y / z≤50; preferably, the above Na-type molecular sieve is selected from at least one of MFI molecular sieve, MWW molecular sieve, GIS molecular sieve, BEC molecular sieve, FAU molecular sieve, and MOR molecular sieve;

[0066] The above lithium ion solution is selected from at least one of a lithium chloride solution, a lithium sulfate solution, and a lithium nitrate solution;

[0067] The above exchange conditions include a temperature of 40-100℃ and a liquid-solid ratio of 10-50.

[0068] 9. Application of a lithiated molecular sieve modified separator according to any one of claims 1 to 8 in a lithium-sulfur battery.

[0069] 10. A lithium-sulfur battery comprises a positive electrode shell, a positive electrode sheet, a separator, a lithium sheet, a nickel foam, and a negative electrode shell, wherein the separator is a lithiated molecular sieve modified separator according to any one of claims 1 to 6.

[0070] The present invention has the following advantages:

[0071] The manufacturing process of the composite separator of the present invention is simple, and the impact on battery energy density is small.

[0072] The composite separator of the present invention comprises a molecular sieve containing cobalt and optionally selected lithium in a composite layer. When applied to a lithium-sulfur battery, the pore structure of the molecular sieve blocks Li2S through physical barrier. x The movement and diffusion of can be effectively restricted, and side reactions within the battery can be reduced. The molecular sieve of the present invention contains cobalt, and the introduced cobalt can improve the conductivity of the anode side of the separator and increase the conversion reaction kinetics of polysulfides as active sites. In a situation where the molecular sieve further contains lithium, the introduced lithium can provide many sites for adsorption and transport during battery circulation, thereby improving the lithium ion transport performance of the separator. More importantly, when the molecular sieve contains lithium and cobalt, a synergistic effect is realized in the obtained composite separator, thereby significantly improving the rate capability and circulation stability of the lithium-sulfur battery. Brief explanation of the drawing

[0073] Figure 1 is an electron microscope image of the composite membrane obtained in Example 2-1. Figure 2 is a charge-discharge curve at different current densities of the lithium-sulfur battery sample obtained in Example 2-1. Specific details for implementing the invention

[0074] The limit values ​​of the ranges and any values ​​disclosed in the text are not limited to the exact ranges or values, but should be understood to include values ​​close to such ranges or values. In the case of numerical ranges, the limits between each range, the limits between each range and individual point values, and the individual point values ​​may be combined to obtain one or more new numerical ranges. Such numerical ranges should be considered as specifically disclosed in the text. Except for the examples, all numerical values ​​of parameters in the text should be understood to be modified by the term "approximately" in all cases, regardless of whether "approximately" actually precedes the numerical value.

[0075] The present invention provides a composite separation membrane, wherein the composite separation membrane comprises a polymer substrate and a composite layer distributed on the surface of the polymer substrate, the composite layer comprises a molecular sieve and a conductive carbon material, and the molecular sieve contains cobalt. In one embodiment, based on the cobalt element, the amount of cobalt in the molecular sieve is 1-30% by weight, preferably 1-15% by weight, and more preferably 2-7% by weight, relative to the total weight of the cobalt and the molecular sieve.

[0076] In one embodiment, the molecular sieve further contains lithium, preferably, based on lithium ions, the amount of lithium in the molecular sieve is 0.1-5% by weight, preferably 0.2-3% by weight, and more preferably 0.5-2.5% by weight, relative to the total weight of the lithium and the molecular sieve.

[0077] In one embodiment, the molecular sieve has a topological structure selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR; preferably, it has a topological structure selected from at least one of MFI, MWW, and GIS.

[0078] The present invention does not limit the thickness of the composite layer. In one embodiment, the thickness of the composite layer is 5-50 μm, and preferably 10-40 μm.

[0079] The present invention does not limit the mass ratio of the conductive carbon material and the molecular sieve in the composite layer. According to one embodiment, in the composite layer, the mass ratio of the conductive carbon material and the molecular sieve is 1:(1-9), preferably 1:(2-9), and may be, for example, 1:1, 1:2, 1:4, 1:6, 1:8, 1:9.

[0080] The material of the polymer substrate film may be a material common in the field. According to one embodiment, the material of the polymer substrate film is at least one of polyethylene, polypropylene, polyimide, polyacrylonitrile, polyethylene terephthalate, polytetrafluoroethylene, and polyvinylidene fluoride, and preferably polyethylene and / or polypropylene.

[0081] The conductive carbon material may be a general material in the field. According to one embodiment, the conductive carbon material is at least one of graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, carbon nanofibers, acetylene black, Super P, and Ketjenblack, and preferably at least one of graphene, graphene oxide, and reduced graphene oxide.

[0082] A second aspect of the present invention provides a method for manufacturing a composite separation membrane, said method,

[0083] (1) A step of mixing a molecular sieve and a conductive carbon material to obtain a mixture, wherein the molecular sieve contains cobalt.

[0084] (2) A step of dispersing the above mixture and binder in a solvent to obtain a coating slurry;

[0085] (3) A step of applying the coating slurry above to the surface of a polymer substrate film, and then removing the solvent to obtain a composite separation film; is included.

[0086] In one embodiment, based on the cobalt element, the amount of cobalt in the molecular sieve with respect to the total weight of the cobalt and the molecular sieve is 1-30% by weight, preferably 1-15% by weight, and more preferably 2-7% by weight. In one embodiment, the method further comprises the step of obtaining the molecular sieve as follows: a cobalt ion solution is added to the raw molecular sieve, and then dried and reduced to obtain a cobalt-containing molecular sieve.

[0087] In one embodiment, the molecular sieve further contains lithium. Preferably, based on lithium ions, the amount of lithium in the molecular sieve is 0.1-5 wt% with respect to the total molar amount of lithium and the molecular sieve, preferably 0.2-3 wt%, and more preferably 0.5-2.5 wt%. In one embodiment, the method of the present invention further comprises the step of obtaining the molecular sieve as follows:

[0088] S1. After exchanging the raw material molecular sieve with the lithium ion solution, wash and dry to obtain a precursor (I);

[0089] S2. A cobalt ion solution is added to the precursor (I), and then dried and reduced to obtain the molecular sieve containing cobalt and lithium.

[0090] Preferably, the lithium ion solution is selected from at least one of lithium chloride, lithium sulfate, and lithium nitrate.

[0091] Preferably, the exchange is carried out under conditions including a temperature of 40-100°C and a liquid-to-solid ratio of 10-50. The exchange may be carried out one or more times, for example, 1-3 times.

[0092] Preferably, the cobalt ion solution is selected from at least one of cobalt chloride solution, cobalt nitrate solution, cobalt sulfate solution, and cobalt acetate solution.

[0093] Preferably, the reduction is carried out in a hydrogen gas atmosphere at a temperature of 600-750°C for 1-4 hours.

[0094] Preferably, the raw molecular sieve has a chemical composition represented as “xM2O·ySiO2·zAl2O3”, 0.01≤x / y≤0.2, 10≤y / z≤50, and M is one or two types selected from Na and K. Preferably, the raw molecular sieve is a Na-type molecular sieve, i.e., M is Na.

[0095] Preferably, the raw molecular sieve is selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR; preferably, it is at least one of MFI, MWW, and GIS.

[0096] In one embodiment, the molecular sieve of step (1) has a topology structure selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR, and preferably has a topology structure selected from at least one of MFI, MWW, and GIS.

[0097] The solvent in step (2) above may be a general material in the field. According to one embodiment, the solvent in step (2) is selected from at least one of deionized water, anhydrous ethanol, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone, and preferably N-methylpyrrolidone.

[0098] The binder in step (2) may be a general material in the field. According to an embodiment of the present invention, the binder in step (2) is at least one of polyvinyl alcohol, carboxymethylcellulose, polyvinylidene fluoride, polytetrafluoroethylene, polyvinylpyrrolidone, styrene-butadiene rubber, and polyacrylate, and preferably polyvinylidene fluoride.

[0099] The coating of step (3) may be a general method in the field. According to the embodiment, the coating of step (3) is at least one of casting coating, blade coating, spray coating, and spin coating, and preferably blade coating.

[0100] A third aspect of the present invention provides an application of the composite separator in a lithium-sulfur battery.

[0101] A fourth aspect of the present invention provides a lithium-sulfur battery comprising a positive electrode, a negative electrode, and a composite separator located between the positive electrode and the negative electrode. The lithium-sulfur battery further comprises an electrolyte. The positive electrode, the negative electrode, and the electrolyte may each be selected from various positive electrodes, negative electrodes, and electrolytes used in lithium-sulfur batteries that are well known to those skilled in the art.

[0102] The composite separator of the present invention comprises a molecular sieve containing cobalt and optionally selected lithium in a composite layer. When applied to a lithium-sulfur battery, the pore structure of the molecular sieve blocks Li2S through physical barrier. x The movement and diffusion of can be effectively restricted, and side reactions within the battery can be reduced. The molecular sieve of the present invention contains cobalt, and the introduced cobalt can improve the conductivity of the anode side of the separator and increase the conversion reaction kinetics of polysulfides as active sites. In a situation where the molecular sieve further contains lithium, the introduced lithium can provide many sites for adsorption and transport during battery circulation, thereby improving the lithium ion transport performance of the separator. More importantly, when the molecular sieve contains lithium and cobalt, a synergistic effect is realized in the obtained composite separator, thereby significantly improving the rate capability and circulation stability of the lithium-sulfur battery.

[0103] The present invention will be described in detail below through examples.

[0104] Ingredient List:

[0105] MFI-type molecular sieves, GIS-type molecular sieves, MWW-type molecular sieves, BEC-type molecular sieves: Purchase from Sigma-Aldrich

[0106] Graphene, Graphene Oxide: Purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0107] PVDF, NMP, CMC, DMF, Cobalt Chloride: Purchased from Sinopharm Chemical Reagent Co., Ltd.

[0108] Test method:

[0109] Assembly of Lithium-Sulfur Battery Sample:

[0110] First, the cathode is prepared: sublimated sulfur as an active material, Ketjenblack as a conductive agent, and polyvinylidene fluoride as a binder are mixed in a mass ratio of 6:3:1, and N-methylpyrrolidone is added to form a cathode slurry; the cathode slurry is coated onto aluminum foil and dried to obtain a cathode. Subsequently, a 2025 button-type battery is assembled in an argon glove box with moisture and oxygen content lower than 0.1 ppm, in the order of a cathode shell, cathode, separator, lithium anode, nickel foam, and anode shell, and 100 μL of electrolyte is added. The electrolyte used is a 1,3-dioxolane / ethylene glycol dimethyl ether (DOL / DME, volume ratio 1:1) mixed solution containing 1 mol / L of bis(trifluoromethanesulfonyl)imide dilithium and 0.2 mol / L of lithium nitrate.

[0111] The rate capability and cycling performance of the lithium-sulfur battery sample manufactured as described above are measured through a constant current charge / discharge test.

[0112] Rate Cap Performance Test:

[0113] A lithium-sulfur battery sample is subjected to 5 cycles of charge-discharge cycling at a voltage range of 1.7-2.7 V and 1C (1C = 1675 mA / g). The discharge capacity of the corresponding charge-discharge cycle is recorded, and the average discharge capacity of the 5 cycles is calculated.

[0114] Average discharge capacity of 5 cycles at 1C = Sum of discharge capacities from the 1st to the 5th cycle / 5

[0115] Similarly, 5 cycles of charge-discharge are repeated at 2C and 3C, and the average discharge capacity of the 5 cycles at 2C and 3C is measured.

[0116] Cyclic Performance Test:

[0117] After performing two charge-discharge cycles at 0.1 and 0.2C, respectively, within a voltage range of 1.7-2.7 V, the lithium-sulfur battery sample is subsequently cycled for 100 and 150 cycles at 0.5C. The discharge capacity after the first cycle, the 100th cycle, and the 150th cycle at different current densities (i.e., the aforementioned 0.1C, 0.2C, and 0.5C) is recorded. The capacity retention rate after 100 or 150 cycles at 0.5C is calculated according to the following formula to indicate the cycling performance.

[0118] Capacity retention rate after 100 cycles = Discharge specific capacity of the 100th cycle / Discharge specific capacity of the 1st cycle * 100%.

[0119] Capacity retention rate after 150 cycles = Discharge specific capacity of the 150th cycle / Discharge specific capacity of the 1st cycle * 100%.

[0120] Regarding the case where the molecular sieve contains lithium and cobalt

[0121] Example 2-1

[0122] Manufacturing of composite membranes

[0123] (1) 5g of raw material molecular sieve (MFI type molecular sieve with a composition of Na2O·20SiO2·Al2O3) and 0.5 mol / L LiCl solution (liquid-solid ratio 20) were subjected to ion exchange at 80°C for 2 hours, after which they were centrifuged and washed. The above ion exchange was repeated twice. The obtained sample was dried overnight at 100°C to obtain a precursor (1-I).

[0124] 2g of the prepared precursor (1-I) is immersed in a 0.1 mol / L cobalt chloride solution with a concentration of 18mL, dried for 8h under air conditions at 80°C, and then heat-treated for 2h under a hydrogen gas atmosphere at 700°C to obtain an MIF-type molecular sieve containing lithium and cobalt.

[0125] (2) 0.35g of MFI-type molecular sieve containing lithium and cobalt and 0.1g of graphene are ground and mixed in mortar to obtain a mixture;

[0126] (3) The above mixture and 0.05 g of polyvinylidene fluoride are dispersed in N-methylpyrrolidone, stirred, and uniformly mixed to obtain a coating slurry;

[0127] (4) The above coating slurry is uniformly applied to one side of a polyethylene / polypropylene substrate film using blade coating, and then dried to remove the solvent, thereby obtaining a composite separation film in which a composite layer is uniformly distributed on one side of a polymer substrate film, wherein the thickness of the composite layer is 15 μm.

[0128] Performance test of composite membranes:

[0129] In accordance with the description of the test method described above, a lithium-sulfur battery sample is assembled using the manufactured composite separator and its performance is tested. Refer to Table 2-1 for specific test results.

[0130] Figure 1 is an electron microscope image of the composite separator of Example 2-1. As shown, the composite layer is uniformly coated on the surface of the PP / PE membrane to form an excellent barrier layer.

[0131] Figure 2 is a charge-discharge curve at different current densities of a lithium-sulfur battery sample containing the composite separator of Example 2-1.

[0132] Example 2-2

[0133] Example 2-1 was repeated, with the following difference: an MFI-type molecular sieve was replaced with a GIS-type molecular sieve to produce a GIS-type molecular sieve containing lithium and cobalt of the same composition. Specifically, 5 g of raw molecular sieve (a GIS-type molecular sieve with a composition of Na2O·20SiO2·Al2O3) and a 0.5 mol / L LiCl solution (liquid-solid ratio 20) were subjected to ion exchange at 80°C for 2 hours, followed by centrifugation and washing. The above ion exchange was repeated twice. The obtained sample was dried overnight at 100°C to obtain a precursor (2-I). 2 g of the prepared precursor (2-I) was immersed in a 0.1 mol / L cobalt chloride solution with a concentration of 18 mL, dried for 8 hours under air conditions at 80°C, and then heat-treated for 2 hours in a hydrogen gas atmosphere at 700°C to obtain a GIS-type molecular sieve containing lithium and cobalt.

[0134] In addition, a composite separator is manufactured by adjusting the capacity of a GIS-type molecular sieve containing lithium and cobalt to 0.6g and the thickness of the composite layer to 30㎛.

[0135] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0136] Examples 2-3

[0137] Example 2-1 was repeated, with the following difference: an MFI-type molecular sieve was replaced with an MWW-type molecular sieve to prepare an MWW-type molecular sieve containing lithium and cobalt of the same composition. Specifically, 5 g of raw molecular sieve (an MWW-type molecular sieve with a composition of Na2O·20SiO2·Al2O3-) and a 0.5 mol / L LiCl solution (liquid-to-solid ratio 20) were subjected to ion exchange at 80°C for 2 hours, followed by centrifugation and washing. The above ion exchange was repeated twice. The obtained sample was dried overnight at 100°C to obtain a precursor (3-I). 2g of the prepared precursor (3-I) is immersed in a 0.1 mol / L cobalt chloride solution with a concentration of 18 mL, dried for 8 hours under air conditions at 80°C, and then heat-treated for 2 hours in a hydrogen gas atmosphere at 700°C to obtain a MWW type molecular sieve containing lithium and cobalt.

[0138] In addition, the capacity of the MWW-type molecular sieve containing the above lithium and cobalt is adjusted to 0.9g, and the thickness of the composite layer is adjusted to 40㎛ to manufacture a composite separator.

[0139] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0140] Examples 2-5

[0141] Repeat Example 2-1, with the difference being: the weight of the MFI-type molecular sieve containing lithium and cobalt is adjusted to 1 g.

[0142] Example 2-1 was repeated, and a lithium-sulfur sample was assembled using the prepared composite separator and a performance test was performed. Refer to Table 2-1 for the test results.

[0143] Examples 2-6

[0144] Repeat Example 2-1, with the difference being: the thickness of the composite layer is adjusted to 50 μm.

[0145] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0146] Examples 2-7

[0147] Example 2-1 is repeated, with the difference being as follows: an MFI-type molecular sieve having a composition of Na2O·20SiO2·Al2O3 is replaced with an MFI-type molecular sieve having a composition of 2Na2O·5SiO2·Al2O3 to produce an MFI-type molecular sieve containing lithium and cobalt.

[0148] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0149] Comparative Example 2-1

[0150] Compared to a repetition of Example 2-1, the difference is as follows: the MFI-type molecular sieve containing lithium and cobalt is replaced with a raw material MFI-type molecular sieve.

[0151] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0152] Comparative Example 2-2

[0153] Compared to a repetition of Example 2-1, the difference is as follows: a 13X type molecular sieve containing lithium and cobalt of the same composition is prepared by replacing the MFI type molecular sieve with a 13X type molecular sieve.

[0154] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0155] Comparative Example 2-3

[0156] Compared to a repetition of Example 2-1, the difference is as follows: an MFI-type molecular sieve is replaced with a SAPO-34-type molecular sieve to produce a SAPO-34-type molecular sieve containing lithium and cobalt of the same composition.

[0157] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0158] Comparative Example 2-4

[0159] Compared to a repetition of Example 2-1, the difference is as follows: a composite separator is prepared by replacing the MFI-type molecular sieve containing lithium and cobalt with the precursor (I).

[0160] Example 2-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 2-1 for the test results.

[0161] Table 2-1 Performance test results of the above lithium-sulfur battery samples tested

[0162]

[0163] Regarding the case where the molecular sieve contains cobalt

[0164] Example 3-1

[0165] (1) 2g of raw molecular sieve (MFI molecular sieve with a composition of Na2O·20SiO2·Al2O3) is immersed in a 0.1 mol / L cobalt chloride solution with a concentration of 18mL, dried for 8h under air conditions at 80℃, and then heat-treated for 2h under a hydrogen gas atmosphere at 700℃ to obtain a cobalt-containing MFI type molecular sieve.

[0166] (2) A mixture is obtained by grinding and mixing 0.35 g of cobalt-containing MFI-type molecular sieve and 0.1 g of graphene in mortar;

[0167] (3) The above mixture and 0.05 g of polyvinylidene fluoride are dispersed in N-methylpyrrolidone, stirred, and uniformly mixed to obtain a coating slurry;

[0168] (4) The above coating slurry is uniformly applied to one side of a polyethylene / polypropylene substrate film using blade coating, and then dried to remove the solvent, thereby obtaining a composite separation film in which a composite layer is uniformly distributed on one side of a polymer substrate film, wherein the thickness of the composite layer is 15 μm.

[0169] In accordance with the description of the test method described above, a lithium-sulfur battery sample is assembled using the manufactured composite separator and its performance is tested. Refer to Table 1 for specific test results.

[0170] Example 3-2

[0171] Example 3-1 was repeated, with the difference being as follows: an MFI-type molecular sieve was replaced with a GIS-type molecular sieve to produce a GIS-type molecular sieve containing cobalt of the same composition. Specifically, 2 g of raw material molecular sieve (a GIS-type molecular sieve with a composition of Na2O·20SiO2·Al2O3-) was immersed in a 0.1 mol / L cobalt chloride solution with a concentration of 18 mL, dried for 8 hours under air conditions at 80°C, and then heat-treated for 2 hours in a hydrogen gas atmosphere at 700°C to obtain a GIS-type molecular sieve containing cobalt.

[0172] In addition, a composite separation membrane is manufactured by adjusting the volume of the GIS-type molecular sieve containing cobalt to 0.6g and the thickness of the composite layer to 30㎛.

[0173] Example 3-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 3-1 for the test results.

[0174] Example 3-3

[0175] Example 2-1 is repeated, with the difference being as follows: an MFI-type molecular sieve is replaced with an MWW-type molecular sieve to produce a MWW-type molecular sieve containing cobalt of the same composition. Specifically, 2 g of raw molecular sieve (an MWW-type molecular sieve with a composition of Na2O·20SiO2·Al2O3-) is immersed in a 0.1 mol / L cobalt chloride solution with a concentration of 18 mL, dried for 8 hours under air conditions at 80°C, and then heat-treated for 2 hours in a hydrogen gas atmosphere at 700°C to obtain a MWW-type molecular sieve containing cobalt.

[0176] In addition, the capacity of the MWW-type molecular sieve containing the above cobalt is adjusted to 0.9g, and the thickness of the composite layer is adjusted to 40㎛ to manufacture a composite separation membrane.

[0177] Example 3-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 3-1 for the test results.

[0178] Examples 3-4

[0179] Repeat Example 3-1, with the difference being: the amount of the cobalt-containing MFI type molecular sieve is adjusted to 1 g.

[0180] Example 3-1 was repeated, and a lithium-sulfur sample was assembled using the prepared composite separator and a performance test was performed. Refer to Table 3-1 for the test results.

[0181] Examples 3-5

[0182] Repeat Example 3-1, with the difference being: the thickness of the composite layer is adjusted to 50 μm.

[0183] Example 3-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 3-1 for the test results.

[0184] Examples 3-6

[0185] Example 3-1 is repeated, with the difference being as follows: an MFI-type molecular sieve having a composition of Na2O·20SiO2·Al2O3 is replaced with an MFI-type molecular sieve having a composition of 2Na2O·5SiO2·Al2O3 to produce a cobalt-containing MFI-type molecular sieve.

[0186] Example 3-1 is repeated, and a lithium-sulfur battery sample is assembled using the prepared composite separator and its performance is tested. Refer to Table 3-1 for the test results.

[0187] Table 3-1 Performance test results of tested lithium-sulfur battery samples

[0188]

[0189] Although preferred embodiments of the present invention have been described in detail above, the present invention is not limited thereto. Within the scope of the technical spirit of the present invention, the technical methods of the present invention may be modified in various simple ways and include combining various technical features in any other suitable manner. Such simple modifications and combinations should likewise be considered as disclosed in the present invention and all fall within the scope of protection of the present invention.

Claims

Claim 1 A composite separation membrane, wherein the composite separation membrane comprises a polymer substrate and a composite layer distributed on the surface of the polymer substrate, wherein the composite layer comprises a molecular sieve and a conductive carbon material, wherein the molecular sieve contains cobalt, and the molecular sieve containing cobalt has a chemical composition represented as aCo·bM2O·ySiO2·zAl2O3, wherein 0.02≤a / y≤0.2, 0.01≤b / y≤0.2, 10≤y / z≤50, and wherein M is an alkali metal element of group IA. Claim 2 A composite separator according to claim 1, wherein the thickness of the composite layer is 5-50 μm or 10-40 μm; and / or, in the composite layer, the mass ratio of the conductive carbon material to the molecular sieve is 1:(1-9) or 1:(2-9). Claim 3 In claim 1, the molecular sieve is a composite separator containing lithium. Claim 4 A composite separator according to claim 3, wherein, based on lithium ions, the amount of lithium in the molecular sieve is 0.1-5 wt%, or 0.2-3 wt%, or 0.5-2.5 wt%; and / or based on cobalt element, the amount of cobalt in the molecular sieve is 1-30 wt%, or 1-15 wt%, or 2-7 wt%. Claim 5 In paragraph 3, the molecular sieve is a composite separation membrane having a topological structure selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR. Claim 6 A composite separator according to claim 1, wherein the material of the polymer substrate film is at least one of polyethylene, polypropylene, polyimide, polyacrylonitrile, polyethylene terephthalate, polytetrafluoroethylene, and polyvinylidene fluoride; and / or the conductive carbon material is at least one of graphene, graphene oxide, reduced graphene oxide, carbon nanotubes, carbon nanofibers, acetylene black, Super P, and Ketjenblack. Claim 7 A method for manufacturing a composite separation membrane according to claim 1, wherein the method comprises: (1) a step of mixing a molecular sieve and a conductive carbon material to obtain a mixture, wherein the molecular sieve contains cobalt and the molecular sieve containing cobalt has a chemical composition represented as aCo·bM2O·ySiO2·zAl2O3, wherein 0.02≤a / y≤0.2, 0.01≤b / y≤0.2, 10≤y / z≤50, and M is an alkali metal element of group IA; (2) a step of dispersing the mixture and a binder in a solvent to obtain a coating slurry; and (3) a step of coating the coating slurry onto the surface of a polymer substrate film and then removing the solvent to obtain a composite separation membrane. Claim 8 A method for manufacturing a composite separation membrane according to claim 7, wherein the manufacturing method further comprises the step of obtaining the molecular sieve, and the step comprises mixing a cobalt ion solution with a raw molecular sieve, and then drying and reducing it to obtain a molecular sieve containing cobalt. Claim 9 A method for manufacturing a composite separator according to claim 7, wherein the molecular sieve further contains lithium, and the manufacturing method further comprises the step of obtaining the molecular sieve as follows: S1. After exchanging a raw molecular sieve with a lithium ion solution, wash and dry to obtain a precursor (I); S2. After mixing a cobalt ion solution with the precursor (I), dry and reduce to obtain the molecular sieve containing cobalt and lithium. Claim 10 In claim 9, the lithium ion solution is selected from at least one of lithium chloride, lithium sulfate, and lithium nitrate; and / or the exchange condition is carried out under conditions including a temperature of 40-100°C and a liquid-solid ratio of 10-50; and / or the cobalt ion solution is selected from at least one of cobalt chloride solution, cobalt nitrate solution, cobalt sulfate solution, and cobalt acetate solution; and / or the reduction is carried out for 1-4 hours at a temperature of 600-750°C in a hydrogen gas atmosphere; and / or the raw molecular sieve has a chemical composition represented as "xM2O·ySiO2·zAl2O3", 0.01≤x / y≤0.2, 10≤y / z≤50, and M is one or two selected from Na and K; A method for manufacturing a composite separation membrane, wherein the raw molecular sieve is selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR. Claim 11 A method for manufacturing a composite separator according to claim 9, wherein the molecular sieve has a topological structure selected from at least one of MFI, MWW, GIS, BEC, FAU, and MOR; and / or, based on lithium ions, the amount of lithium in the molecular sieve is 0.1-5 wt%, or 0.2-3 wt%, or 0.5-2.5 wt%; and / or based on cobalt elements, the amount of cobalt in the molecular sieve is 1-30 wt%, or 1-15 wt%, or 2-7 wt%. Claim 12 A method for manufacturing a composite separator according to claim 7, wherein the solvent of step (2) is selected from at least one of deionized water, anhydrous ethanol, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, and N-methylpyrrolidone; and / or the binder of step (2) is at least one of polyvinyl alcohol, carboxymethylcellulose, polyvinylidene fluoride, polytetrafluoroethylene, polyvinylpyrrolidone, styrene-butadiene rubber, and polyacrylate; and / or the coating of step (3) is at least one of casting coating, blade coating, spray coating, and spin coating. Claim 13 A lithium-sulfur battery characterized by comprising a positive electrode, a negative electrode, and a composite separator according to claim 1 located between the positive electrode and the negative electrode.

Citation Information

Patent Citations

  • ACSAPPL

  • ELECTROCHIMICAACTA