Polyester nonwoven fabric with suppressed deterioration of physical properties during tufting process, method for fabricating the same and primary backing substrate for carpet

A polyester-based nonwoven fabric with specific melting point and composition filaments addresses filament damage during tufting, maintaining mechanical properties and reducing manufacturing costs, suitable for carpet backing.

KR103047786B1Active Publication Date: 2026-11-11KOLON INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020210183999
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-21
Publication Date
2026-11-11
Estimated Expiration
2041-12-21

AI Technical Summary

Technical Problem

Conventional polyester nonwoven fabrics suffer from filament damage during the tufting process, which causes filament damage during the tufting process, causing filament damage during the tufting process, resulting in the filament, leading to the physical properties of the nonwoven fabric, such as tensile strength and tear strength, to deteriorate, making them unsuitable for use as carpet backing due to complex manufacturing processes and high costs.

Method used

A polyester-based nonwoven fabric is developed with a first component filament having a melting point of 250°C to 300°C and a second component filament with a melting point of 160°C to 220°C, combined in a specific weight ratio and processed through heat-bonding, to maintain mechanical properties before and after tufting.

Benefits of technology

The nonwoven fabric maintains excellent tensile and tear strength, reducing filament damage and manufacturing costs, while ensuring dimensional stability and flexibility, suitable for carpet backing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112021148133333-PAT00002
    Figure 112021148133333-PAT00002
  • Figure 112021148133333-PAT00003
    Figure 112021148133333-PAT00003
  • Figure 112021148133333-PAT00007
    Figure 112021148133333-PAT00007
Patent Text Reader

Abstract

The present invention relates to a polyester nonwoven fabric in which the reduction of physical properties caused by a tufting process is suppressed, a method for manufacturing the same, and a foamed paper for carpets containing the same. Specifically, the invention relates to a polyester nonwoven fabric capable of producing a foamed paper for carpets with excellent mechanical properties by controlling the fiber properties of a first component filament and a second filament to significantly suppress the reduction of physical properties before and after the tufting process, a method for manufacturing the same, and a foamed paper for carpets produced by the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a polyester nonwoven fabric in which the reduction of physical properties caused by a tufting process is suppressed, a method for manufacturing the same, and a foamed paper for carpets containing the same. Specifically, the invention relates to a polyester nonwoven fabric capable of producing a foamed paper for carpets with excellent mechanical properties by controlling the fiber properties of a first component filament and a second filament to significantly suppress the reduction of physical properties before and after the tufting process, a method for manufacturing the same, and a foamed paper for carpets produced by the same. Background Technology

[0003] Generally, polyester-based nonwoven fabrics composed of polyester filament fibers are widely used as carpet backings. When manufacturing carpets using these backings, a tufting process is essential, in which carpet yarns are implanted into the backing using needles.

[0005] In the above tufting process, there is a problem in that the filament fibers forming the polyester nonwoven fabric are damaged by the needle, causing the physical properties of the nonwoven fabric, such as tensile strength and tear strength, to deteriorate. As one of the methods to solve this disadvantage, Korean Patent Publication No. 1998-0061102 describes a method of manufacturing a spunbond nonwoven fabric for carpet backing paper by forming filament fibers and a web using two types of polyester polymers, performing needle punching, and passing it through a calender roll.

[0007] However, this method not only has a complex overall manufacturing process, but also causes damage to the filament fibers during the process of binding them by needle punching, resulting in more severe damage after the tufting process of embedding carpet yarns. Therefore, nonwoven fabrics manufactured by this method still exhibit the disadvantage of significantly degrading physical properties after tufting, making it difficult to apply them as carpet backing paper.

[0009] In addition, Korean Patent Publication No. 2001-0053138 discloses a method for manufacturing carpet backing paper through processes such as producing irregular cross-section yarns by spinning polyester and polylactic acid (PLA) using a composite spinning method. However, because this method has poor spinnability, spinning defects are prone to occur, and the manufacturing cost is high due to the high price of polylactic acid.

[0011] Therefore, there is a continuous demand for a nonwoven fabric and a method for manufacturing the same that can be manufactured with a simpler process and lower manufacturing costs, and that can be preferably used as a carpet backing sheet as it retains good physical properties even after the tufting process. Prior art literature

[0013] Korean Published Patent Application No. 1998-0061102 (October 7, 1998) Korean Published Patent Application No. 2001-0053138 (June 25, 2001) The problem to be solved

[0014] The present invention has been devised to solve the aforementioned problems, and the objective of the present invention is to provide a polyester-based nonwoven fabric capable of significantly suppressing the deterioration of physical properties before and after the tufting process by controlling the components and physical properties of the first component filament and the second component filament, a method for manufacturing the same, and a foam sheet for carpets containing the same. means of solving the problem

[0016] To solve the above-mentioned problem, the present invention comprises a first component filament comprising a first polyester having a melting point of 250°C to 300°C; and

[0017] A second component filament comprising a second polyester having a melting point of 160°C to 220°C; comprising,

[0018] A polyester-based nonwoven fabric is provided, characterized by having a stiffness before the tufting process, measured by the measurement method specified in ASTM D 6125-97, of 100 mg to 300 mg in both the machine direction (MD) and the vertical direction (CD).

[0020] In a preferred embodiment of the present invention, the machine direction stiffness (S) of the polyester nonwoven fabric before the tufting process MD ) and vertical stiffness (S CD ) can satisfy the following condition 1).

[0021] 1) .

[0023] In a preferred embodiment of the present invention, the first polyester may have an intrinsic viscosity of 0.65 dl / g to 0.80 dl / g.

[0025] In a preferred embodiment of the present invention, the polyester nonwoven fabric may be formed by fusing the second component filament.

[0027] In a preferred embodiment of the present invention, the second polyester may be a copolyester formed by copolymerizing one or more acid components selected from terephthalic acid, dimethyl terephthalate, isophthalic acid, and dimethyl isophthalate, and one or more diol components selected from 1,4-butanediol (BD), ethylene glycol (EG), and neopentyl glycol (NPG).

[0029] In a preferred embodiment of the present invention, the polyester nonwoven fabric has a machine direction (MD) tensile strength (T) before the tufting process. MD,0 ) and vertical (CD) tensile strength (T CD,0 The deviation between ) is T CD,0 ×0.05 or less,

[0030] The reduction rate of tensile strength after the tufting process may be 60% or less in both the machine direction and the vertical direction.

[0032] In a preferred embodiment of the present invention, the polyester nonwoven fabric is T before the tufting process MD,0 and T CD,0 All of them may be 25kgf / 5cm to 35kgf / 5cm.

[0034] In a preferred embodiment of the present invention, the polyester nonwoven fabric may comprise the first component filament and the second component filament in a weight ratio of 85:15 to 90:10.

[0036] In a preferred embodiment of the present invention, the polyester nonwoven fabric may have a mechanical direction heat shrinkage rate of 1.5% or less and a vertical direction heat shrinkage rate of 1.0% or less, as measured according to the following measurement method.

[0037] [measurement method]

[0038] A pattern of 20cm × 20cm is drawn on a nonwoven fabric specimen of 25cm × 25cm in the machine direction and perpendicular direction, respectively. After preheating the specimen on a preheating plate at 180℃ for 3 minutes using a Mathis oven, the specimen is removed and the shrunk length is measured to calculate the shrinkage rate.

[0040] In a preferred embodiment of the present invention, the polyester nonwoven fabric may have a tear strength of 7 kgf to 13 kgf in both the machine direction and the vertical direction before the tufting process.

[0042] In a preferred embodiment of the present invention, the polyester nonwoven fabric may satisfy the following condition formulas 2) and 3).

[0043] 2)

[0044] 3)

[0045] In the above condition expressions 2) and 3), the above and Each represents the intrinsic viscosity of the first polyester and the intrinsic viscosity of the second polyester.

[0047] In a preferred embodiment of the present invention, the first component filament has a fineness of 7 to 10 denier, and the second component filament has a fineness of 2 to 4 denier, respectively.

[0048] The number of filaments of the first component filament may be included in a multiple of 2 to 5 of the number of filaments of the second component filament.

[0050] The present invention also provides a foam sheet for carpets comprising the polyester nonwoven fabric.

[0052] The present invention also comprises: 1) a step of forming a blended web by blending a first polyester having a melting point of 250°C to 300°C and a second polyester having a melting point of 160°C to 220°C and laminating the two fibers; and

[0053] 2) A step of heat-bonding the blended web with hot air having a temperature of 0°C to 10°C or higher than the melting point of the second polyester;

[0054] The present invention provides a method for manufacturing a polyester-based nonwoven fabric characterized by manufacturing a nonwoven fabric having both machine direction bending strength and vertical direction stiffness of 100 mg to 300 mg before the tufting process, including

[0056] In a preferred embodiment of the present invention, in step 1), the first polyester and the second polyester can be stretched at a speed of 4,500 m / min to 5,200 m / min to form the first component filament and the second component filament, respectively. Effects of the invention

[0058] The polyester-based nonwoven fabric according to the present invention can provide a polyester-based nonwoven fabric that maintains excellent tensile strength, tear strength, etc., even after a tufting process. Therefore, the polyester-based nonwoven fabric of the present invention can be usefully used as a carpet backing and can realize excellent mechanical properties. Specific details for implementing the invention

[0060] The detailed structure and effects of the present invention will be described below.

[0062] As mentioned above, conventional nonwoven fabrics for carpet backings had disadvantages such as filament damage during the tufting process in carpet manufacturing, resulting in degraded physical properties, poor fiber spinnability, and high manufacturing costs.

[0064] To solve these problems, the present invention comprises a first component filament comprising a first polyester having a melting point of 250°C to 300°C; and

[0065] A second component filament comprising a second polyester having a melting point of 160°C to 220°C; comprising,

[0066] A polyester-based nonwoven fabric is provided, characterized by having a stiffness before the tufting process, measured by the measurement method specified in ASTM D 6125-97, of 100 mg to 300 mg in both the machine direction (MD) and the vertical direction (CD).

[0068] By providing a combination of fibers having the above-mentioned physical properties and a nonwoven fabric having the above-mentioned physical properties, the present invention can provide a polyester-based nonwoven fabric that can significantly suppress the reduction of physical properties such as tear strength and tensile strength of the nonwoven fabric despite the tufting process for carpet manufacturing.

[0070] The first component filament is manufactured by spinning high-melting-point polyester and serves as a matrix fiber (filament) in the nonwoven fabric manufacturing process. Additionally, the second component filament is manufactured by spinning low-melting-point polyester and serves as a binder fiber (filament) in the nonwoven fabric manufacturing process.

[0072] If the melting point of the first polyester of the first component filament is less than 250°C, the difference in melting point with the second polyester acting as a binder is reduced, and the usable temperature range for spinning may be reduced. Conversely, if the melting point exceeds 300°C, thermal decomposition of the second polyester may occur at the spinning temperature.

[0074] In addition, if the melting point of the second polyester of the second component filament is less than 160°C, thermal shrinkage may occur during the post-processing of the carpet base sheet containing the polyester-based nonwoven fabric, which may result in reduced dimensional stability. Conversely, if the melting point exceeds 220°C, the thermal shrinkage rate of the nonwoven fabric is stable, and deformation of the sheet may not occur during the carpet manufacturing process; however, during the high-temperature coating, heat treatment, and drying processes of the carpet, the flexibility of the nonwoven fabric decreases, resulting in a slight difference in elongation rate between the nonwoven fabric and the coating liquid applied to the bottom of the nonwoven fabric. While this slight difference is not a problem for the product immediately after manufacturing, as the carpet's usage period increases, latent stress caused by the difference in elongation rate between the coating material and the nonwoven fabric may cause deformation of the carpet.

[0076] In addition, if the stiffness of the nonwoven fabric is less than 100 mg, it has characteristics that are too soft for use as a carpet, so it does not maintain its shape well and is unsuitable for use as a carpet; if it exceeds 300 mg, it is excessively stiff, resulting in a problem where the physical properties of the nonwoven fabric deteriorate due to fiber damage, shedding, or lint generation during the tufting process. Furthermore, if the stiffness exceeds 300 mg, the nonwoven fabric becomes stiff and lacks flexibility, making it prone to wrinkling and potentially leading to reduced workability.

[0078] In a preferred embodiment of the present invention, the machine direction stiffness (S) of the polyester nonwoven fabric before the tufting process MD ) and vertical stiffness (S CD ) can satisfy the following condition 1).

[0079] 1) .

[0081] That is, the polyester-based nonwoven fabric according to the present invention exhibits a degree of stiffness in the machine direction and the perpendicular direction that is nearly similar, and if the above condition Equation 1 is not satisfied, i.e., S MD Ga S CD If it exceeds 1.05 times or is less than 0.95 times, significant degradation of the physical properties of the polyester-based nonwoven fabric during the tufting process may occur. Preferably, S MD and S CD ...can satisfy the following condition 1-1).

[0082] 1-1)

[0084] In a preferred embodiment of the present invention, the first polyester may have an intrinsic viscosity of 0.65 dl / g to 0.80 dl / g. If the intrinsic viscosity exceeds 0.80 dl / g, the tensile strength of the first component filament and the tear strength of the polyester-based nonwoven fabric increase, but the stiffness of the nonwoven fabric increases excessively, or the pressure of the spinneret increases rapidly, which may cause problems such as leakage of the molten first polyester polymer. However, conversely, if the intrinsic viscosity is 0.65 dl / g or less, the tensile strength of the filament and the tear strength of the nonwoven fabric decrease, and there may be a problem in that the tensile strength decreases significantly after the tufting process.

[0086] In a preferred embodiment of the present invention, the polyester-based nonwoven fabric may be formed by fusing the second component filament. Since the second polyester has a relatively lower melting point compared to the first polyester, the second component filament formed therefrom can easily fuse with the first component filament when heat is applied. Accordingly, according to the present invention, in which the second component filaments are uniformly distributed within the nonwoven fabric together with the first component filaments, the first and second component filaments can be easily bonded to each other to manufacture the nonwoven fabric without the need for a separate process such as needle punching.

[0088] Therefore, the nonwoven fabric manufacturing process can be simplified by the present invention, and the first and second component filaments included in the finally produced nonwoven fabric of the present invention may not have any damage caused by the needle punching process.

[0090] In a preferred embodiment of the present invention, the second polyester may be a copolyester formed by copolymerizing one or more acid components selected from terephthalic acid, dimethyl terephthalate, isophthalic acid, and dimethyl isophthalate, and one or more diol components selected from 1,4-butanediol (BD), ethylene glycol (EG), and neopentyl glycol (NPG).

[0092] However, the compounds of the acid component and the diol component are not limited to the compounds listed above, and may be selected from among the compounds of the acid component and the diol component for polyester polymerization generally used in the industry, depending on the purpose of the invention.

[0094] In a preferred embodiment of the present invention, the polyester nonwoven fabric has a machine direction (MD) tensile strength (T) before the tufting process. MD,0 ) and vertical (CD) tensile strength (T CD,0 The deviation between ) is T CD,0 ×0.05 or less,

[0095] The reduction rate of tensile strength after the tufting process may be 60% or less in both the machine direction and the vertical direction.

[0097] The present invention relates to a tensile strength magnitude in the machine direction and the vertical direction before the tufting process, wherein the vertical tensile strength (T CD,0 Since it has a uniform tensile strength of 5% or less, there is almost no difference in material properties depending on the direction, and the defect rate during the tufting process can be significantly reduced, and after the tufting process, the reduction rate of tensile strength in both the machine direction and the vertical direction is 60% or less, so the deterioration of material properties can be significantly suppressed.

[0099] If the reduction rate of tensile strength exceeds 60%, the tensile strength of the nonwoven fabric is significantly lowered after the tufting process, so it may not be suitable for use as a carpet backing.

[0101] In a preferred embodiment of the present invention, the polyester nonwoven fabric is T before the tufting process MD,0 and T CD,0 All of them may be between 25 kgf / 5 cm and 35 kgf / 5 cm. If either or more of the tensile strength in the machine direction or the vertical direction before the tufting process is 25 kgf / 5 cm or less, the tensile strength decreases after the tufting process, and the nonwoven fabric may not be suitable for use as a carpet backing. Conversely, if the tensile strength before the tufting process exceeds 35 kgf / 5 cm in either the machine direction or the vertical direction, the stiffness of the nonwoven fabric becomes excessively high, which may result in problems such as vulnerability to wrinkles, reduced workability, or a significant decrease in physical properties before and after the tufting process.

[0103] In a preferred embodiment of the present invention, the polyester-based nonwoven fabric may contain the first component filament and the second component filament in a weight ratio of 85:15 to 90:10. If the content ratio of the second component filament is less than 10 weight%, the physical properties become similar to those of a nonwoven fabric made only of the first component filament with a high melting point, so a nonwoven fabric satisfying the required strength cannot be manufactured by heat bonding alone, and a separate process such as needle punching, which causes filament breakage, will be required to manufacture the nonwoven fabric.

[0105] On the other hand, if the content ratio of the second component filament exceeds 15 weight%, the adhesive component in the nonwoven fabric becomes too high, so if the nonwoven fabric is used as a base for carpets, filament breakage will occur during the tufting process, and as a result, the deterioration of the physical properties of the base fabric due to the tufting process will be severe.

[0107] In a preferred embodiment of the present invention, the polyester nonwoven fabric may have a mechanical direction heat shrinkage rate of 1.5% or less and a vertical direction heat shrinkage rate of 1.0% or less, as measured according to the following measurement method.

[0108] [measurement method]

[0109] A pattern of 20cm × 20cm is drawn on a nonwoven fabric specimen of 25cm × 25cm in the machine direction and perpendicular direction, respectively. After preheating the specimen on a preheating plate at 180℃ for 3 minutes using a Mathis oven, the specimen is removed and the shrunk length is measured to calculate the shrinkage rate.

[0111] If the heat shrinkage rate in the machine direction exceeds 1.5% or the heat shrinkage rate in the vertical direction exceeds 1.0%, the dimensional stability of the manufactured nonwoven fabric is reduced, and it may not be suitable for use as a carpet backing.

[0113] In a preferred embodiment of the present invention, the polyester nonwoven fabric may have a tear strength of 7 kgf to 13 kgf in both the machine direction and the vertical direction before the tufting process.

[0114] If the tear strength is less than 7 kgf in the machine direction or vertical direction, damage to the nonwoven fabric may occur, such as the nonwoven fabric tearing during the tufting process, or the nonwoven fabric may not be suitable for use as a foam sheet for carpets due to a decrease in tear strength after the tufting process, and if it exceeds 13 kgf, problems such as an excessive increase in stiffness or a decrease in tensile strength may occur.

[0116] In a preferred embodiment of the present invention, the polyester nonwoven fabric may satisfy the following condition formulas 2) and 3).

[0117] 2)

[0118] 3)

[0119] In the above condition expressions 2) and 3), the above and Each represents the intrinsic viscosity of the first polyester and the intrinsic viscosity of the second polyester.

[0121] By satisfying the above conditions 2) and 3), the bending strength, tensile strength, and tear strength of the nonwoven fabric prior to the tufting process for achieving the objective of the present invention can be satisfied.

[0123] If the intrinsic viscosity of the second polyester is lower than that of the first polyester, it has a significantly lower melt viscosity compared to the first polyester at the spinning temperature, so there may be spinnability problems due to the difference in viscosity, and the deviation may be 5% to 12% relative to the intrinsic viscosity of the first polyester. If the intrinsic viscosity of the second polyester is greater than 12% of the intrinsic viscosity of the first polyester, it may increase the internal pressure of the extruder and clog the nozzle during the melt spinning of the second component filament, causing process problems, and may cause the fiber properties to deteriorate and the tear strength of the nonwoven fabric to decrease due to fragmentation of the manufactured yarn. In addition, if the deviation between the intrinsic viscosity of the second polyester and the intrinsic viscosity of the first polyester is less than 5%, the effect of improving the strength of the yarn due to the manufacture of high-viscosity fibers may be negligible.

[0125] In a preferred embodiment of the present invention, the first component filament has a fineness of 7 to 10 denier, and the second component filament has a fineness of 2 to 4 denier, and the number of filaments of the first component filament may be included in a multiple of 2 to 5 of the number of filaments of the second component filament.

[0127] If the fineness of the first component filament is less than 7 denier, the number of first component filaments per unit area increases, so when the nonwoven fabric is used as a base material for carpets and undergoes a tufting process, significant damage to the filaments caused by the needle will occur, and as a result, the physical properties of the base material will deteriorate severely due to the tufting process. On the other hand, if the fineness of the first filament exceeds 10 denier, the uniformity of the nonwoven fabric manufactured using it will be severely impaired, and its commercial utility will be lost.

[0129] In addition, if the fineness of the second component filament is less than 2 denier, cutting of the second component filament may occur during the cooling process. On the other hand, if the fineness of the second component filament exceeds 4 denier, the cooling of the second component filament is not properly performed during the cooling process (e.g., a cooling process performed immediately after web formation), so adhesion between the second component filaments is caused, which reduces the uniformity of the nonwoven fabric and, as a result, the commercial utility of the nonwoven fabric is lost.

[0131] The present invention also provides a foam sheet for carpets comprising the polyester nonwoven fabric.

[0133] By having the composition described above, the polyester-based nonwoven fabric of the present invention can appropriately suppress filament breakage during the tufting process for carpet yarn transplantation, thereby exhibiting excellent physical properties even after the tufting process and providing a carpet base fabric with excellent physical properties. Furthermore, since the polyester-based nonwoven fabric can be easily manufactured by heat-bonding the filaments constituting it, the manufacturing process is easy and simple, and the manufacturing cost can also be significantly reduced.

[0135] Below, the method for manufacturing the above-mentioned polyester-based nonwoven fabric will be described in detail.

[0137] The present invention comprises: 1) a step of forming a blended web by blending a first polyester having a melting point of 250°C to 300°C and a second polyester having a melting point of 160°C to 220°C and laminating the two fibers; and

[0138] 2) A step of heat-bonding the blended web with hot air having a temperature of 0°C to 10°C or higher than the melting point of the second polyester;

[0139] The present invention provides a method for manufacturing a polyester-based nonwoven fabric characterized by manufacturing a nonwoven fabric having both machine direction bending strength and vertical direction stiffness of 100 mg to 300 mg before the tufting process, including

[0141] The temperature of the hot air may preferably be 0°C to 5°C or higher than the melting point of the second polyester.

[0143] In a preferred embodiment of the present invention, in step 1), the first polyester and the second polyester can be stretched at a speed of 4,500 m / min to 5,200 m / min to form the first component filament and the second component filament, respectively.

[0145] By stretching at such a speed, a first component filament and a second component filament having a fineness within the range described above can be obtained.

[0147] As the composition and physical properties of each first component filament, second component filament, and the first and second polyesters are identical to those described for the polyester-based nonwoven fabric, they will be omitted.

[0149] Other steps of the nonwoven fabric manufacturing process can be performed through general nonwoven fabric manufacturing process methods, and these are within the range that a person of ordinary skill can easily select and implement.

[0151] In the following, the specific effects of the present invention will be explained through specific embodiments. However, it should be understood that the scope of the present invention is not limited to the following embodiments, and that the following embodiments are merely exemplary embodiments provided to aid in understanding the present invention.

[0153] <Example>

[0154] Example 1

[0155] Polyester for matrix filaments having a melting point of 255°C and an intrinsic viscosity (IV) of 0.65 dl / g (manufactured by Kolon Industries Co., Ltd., polymerization of terephthalic acid (TPA) and ethylene glycol (EG)) and low-melting point copolyester for binder filaments having a melting point of 212°C and an intrinsic viscosity of 0.82 dl / g (manufactured by Kolon Industries Co., Ltd., copolymerization of terephthalic acid (TPA), isophthalic acid (IPA), adipic acid (AA) and ethylene glycol (EG)) were melted using a continuous extruder, then extruded through the spinning nozzle at the bottom of the continuous extruder and blended to produce a blended yarn for the first row of webs. The blended yarn was made such that the weight ratio of the matrix filament and the binder filament was 90:10, and the fineness of the matrix filament and the binder filament was 8.5 denier and 3.5 denier, respectively.

[0157] In addition, the continuous filament emitted from the above-mentioned spinning nozzle was solidified with cooling air, and then stretched using a high-pressure air stretching device to a spinning speed of 5,000 m / min.

[0159] Subsequently, the manufactured filament is laminated in the form of a web on a conveyor net using a conventional fiber opening method, then subjected to a calendering process using heated smooth rolls to impart smoothness and an appropriate thickness, and heat-bonded using hot air at a temperature of +3°C (melting point of the low-melting-point copolyester for binder filaments) to obtain a weight of 100 g / m² per unit area. 2A spunbond nonwoven fabric for carpet foam was manufactured.

[0161] Example 2

[0162] A spunbond nonwoven fabric for carpet backing was manufactured using the same method as in Example 1, except that the matrix filament was spun using a polyester with an intrinsic viscosity of 0.78 dl / g.

[0164] Example 3

[0165] A spunbond nonwoven fabric for carpet backing was manufactured using the same method as in Example 1, except that the binder filament was a low-melting point copolyester with a melting point of 164°C (manufactured by Kolon Industries Co., Ltd., copolymer of terephthalic acid (TPA), isophthalic acid (IPA), adipic acid (AA), and ethylene glycol (EG)) and heat-bonded with hot air at 167°C.

[0167] Example 4

[0168] A spunbond nonwoven fabric for carpet base paper was manufactured using the same method as in Example 1, except that the weight ratio of the matrix filament and the binder filament was adjusted to 85:15.

[0170] Examples 5 to 7

[0171] A spunbond nonwoven fabric for carpet base paper was manufactured using the same method as in Example 1, except that the polyesters of the matrix filament and binder filament were different as shown in Table 1, and the copolyester for the binder filament was heat-bonded with hot air at a temperature of +3°C, the melting point of the binder filament.

[0173] Comparative Example 1

[0174] A spunbond nonwoven fabric for carpet backing was prepared using the same method as in Example 1, except that the matrix filament used was a polyester with an intrinsic viscosity of 0.57 dl / g.

[0176] Comparative Example 2

[0177] A spunbond nonwoven fabric for carpet backing was manufactured using the same method as in Example 1, except that the binder filament was changed to a copolyester with a melting point of 156°C (manufactured by Kolon Industries Co., Ltd., copolymer of terephthalic acid (TPA), isophthalic acid (IPA), adipic acid (AA), and ethylene glycol (EG)) and heat-bonded with hot air at 159°C.

[0179] Comparative Example 3

[0180] A spunbond nonwoven fabric for carpet base paper was manufactured using the same method as in Example 1, except that the melting point of the binder filament was adjusted to 226°C and heat-bonded with hot air at 229°C.

[0182] Comparative Example 4

[0183] A spunbond nonwoven fabric for carpet base paper was manufactured using the same method as in Example 1, except that the weight ratio of the matrix filament to the binder filament was changed to 94:6.

[0185] Comparative Example 5

[0186] A spunbond nonwoven fabric for carpet base paper was manufactured using the same method as in Example 1, except that the weight ratio of the matrix filament and the binder filament was changed to 80:20.

[0188] <Experimental Example>

[0189] Experimental Example 1: Measurement of Nonwoven Fabric Stiffness (mg)

[0190] The stiffness of the polyester nonwoven fabrics prepared according to the examples and comparative examples was measured using a Bending Resistance Tester manufactured by Gurley Precision Instruments (Troy, New York) in accordance with the method specified in ASTM D 6125-97.

[0192] Experimental Example 2: Measurement of Tear Strength (kgf)

[0193] According to the KS K 0536 (Single Tongue) method, a spunbond nonwoven fabric was cut into specimens measuring 7.6 cm × 20 cm, and the tear strength was measured using a universal tensile testing machine (Instron) at a tensile speed of 300 mm / min.

[0195] Experimental Example 3: Measurement of Tensile Strength (kgf / 5cm)

[0196] The tensile strength before the tufting process was measured using the measurement method specified in KS K 0521.

[0198] Specifically, a specimen measuring 5cm x 20cm was fixed to a jig 5 / 5cm above and below using measuring equipment from INSTRON (USA), and measured at a tensile speed of 200mm / min.

[0200] The tensile strength after tufting was measured using the KS K 0521 method as described above after tufting using a small tufting machine with a width of 1.0 m.

[0202] At this time, the operating conditions of the tufting machine were a pile height of 5.0 mm, a gauge of 1.10 inches, a stitch of 1 / 13 inch, and an operating speed of 600 rpm, and the carpet yarn (BCF) used at this time was a 1200 denier 96 filament triangular cross-section yarn made of nylon 6 material manufactured by Hyosung Corporation, and a single loop type carpet was manufactured.

[0204] Experimental Example 4: Measurement of Thermal Shrinkage Rate (%)

[0205] A pattern of 20 cm × 20 cm is drawn on a nonwoven fabric specimen measuring 25 cm × 25 cm. After preheating it on a preheating plate at 180°C for 3 minutes using a Mathis oven (Daelim Starlet), it is removed, and the shrinkage rate is calculated based on the shrunk length.

[0207] The above experimental results are each shown in Table 1 below.

[0209] division Component 1 Melting Point, IV, Content (°C, dl / g, wt%) Component 2 (melting point, IV, content) Leanness (mg) MD / CD Tear strength (kgf) MD / CD Tensile strength (kgf / 5cm) MD / CD Thermal shrinkage rate (%) MD / CD Before tufting After tufting Decrease rate (%) Example 1 255 0.65 90 212 0.82 10 229 / 234 9.4 / 9.9 31.7 / 33.7 14.0 / 18.1 56 / 46 0.5 / 0.0 Example 2 255 0.78 90 212 0.82 10 254 / 269 10.5 / 10.9 32.5 / 33.9 16.6 / 18.3 49 / 46 0.4 / 0.0 Example 3 255 0.65 90 164 0.82 10 197 / 204 11.2 / 11.5 30.4 / 31.1 16.7 / 18.0 45 / 42 0.9 / 0.2 Example 4 255 0.65 85 212 0.82 15 265 / 273 8.4 / 8.6 33.2 / 32.1 13.6 / 13.8 59 / 57 0.6 / 0.0 Example 5 267 0.69 90 201 0.79 10 248 / 260 8.1 / 8.3 31.6 / 33.0 16.4 / 16.2 48 / 51 0.7 / 0.0 Example 6 258 0.68 90 193 0.64 10 216 / 231 7.3 / 7.5 29.8 / 30.9 16.7 / 13.3 44 / 57 0.8 / 0.0 Example 7 252 0.66 90 218 0.74 10 257 / 284 8.6 / 9.1 28.4 / 29.2 9.4 / 11.1 67 / 62 0.6 / 0.1 Comparative Example 1 255 0.57 90 212 0.82 10 279 / 287 6.4 / 6.7 30.5 / 30.1 8.8 / 9.3 71 / 69 2.5 / 1.8 Comparative Example 2 255 0.65 90 156 0.82 10 185 / 193 11.5 / 11.7 29.9 / 32.2 16.7 / 19.6 44 / 39 3.1 / 2.9 Comparative Example 3 255 0.65 90 226 0.82 10 305 / 321 5.9 / 6.4 29.5 / 31.7 6.8 / 7.6 77 / 76 0.3 / 0.0 Comparative Example 4 255 0.65 94 212 0.82 6 213 / 222 10.3 / 9.8 15.8 / 17.2 8.7 / 8.9 45 / 48 0.6 / 0.0 Comparative Example 5 255 0.65 80 212 0.82 20 298 / 303 5.4 / 5.2 29.4 / 30.1 8.5 / 7.5 71 / 75 1.5 / 0.2

[0210] Referring to Table 1 above, it can be seen that Comparative Example 1 is not suitable for use as a polyester nonwoven fabric for carpet backing paper because the intrinsic viscosity of the first component filament is excessively low, the tear strength is low, and the rate of reduction in tensile strength of the nonwoven fabric is significantly high before and after tufting.

[0212] In addition, it can be seen that Comparative Example 2 has a problem in that the melting point of the second component filament is excessively low, resulting in a high thermal shrinkage rate and consequently reduced dimensional stability of the nonwoven fabric.

[0214] Comparative Example 3 shows that as a result of the melting point of the second component filament being excessively high, the stiffness of the nonwoven fabric is excessively high, the tear strength is low, and the rate of reduction in tensile strength after the tufting process is significantly high.

[0216] Comparative Example 4 shows that the content of the second component filament is excessively low, resulting in significantly low tensile strength of the nonwoven fabric and poor physical properties.

[0218] In Comparative Example 5, it was confirmed that the content of the second component filament was excessively high, resulting in high stiffness of the nonwoven fabric and low tear strength, and that the tensile strength was excessively reduced due to the tufting process.

[0220] In addition, it was found that the nonwoven fabrics according to the examples were suitable for use as carpet backing sheets because the rate of decrease in tensile strength before and after tufting was not significant and the rate of thermal shrinkage was low. However, in the case of Example 7, it was confirmed that there was a large difference in physical properties between the machine direction and the vertical direction, and a large rate of decrease in tensile strength before and after tufting, indicating that the physical properties were insufficient for use as a backing sheet nonwoven fabric compared to Example 1. However, the rate of thermal shrinkage is low and the tear strength is excellent. Therefore, it can be seen that the smaller the deviation in stiffness between the vertical direction and the machine direction, the better the physical properties.

Claims

Claim 1 A first component filament comprising a first polyester having a melting point of 252℃ to 300℃; A polyester-based nonwoven fabric comprising: a second component filament comprising a second polyester having a melting point of 160°C to 220°C; wherein the weight ratio of the first component filament to the second component filament is 85:15 to 90:10, the intrinsic viscosity of the second polyester is 0.74 dl / g to 0.82 dl / g, the deviation between the intrinsic viscosity of the second polyester and the intrinsic viscosity of the first polyester is 5% to 12% with respect to the intrinsic viscosity of the first polyester, and the stiffness before the tufting process, measured by the measurement method specified in ASTM D 6125-97, is 100 mg to 300 mg in both the machine direction (MD) and the vertical direction (CD), and the machine direction stiffness (S) before the tufting process MD ) and vertical stiffness (S CD Polyester-based nonwoven fabric characterized by satisfying the following condition 1): 1) . Claim 2 In claim 1, the machine direction stiffness (S) of the polyester nonwoven fabric before the tufting process MD ) and vertical stiffness (S CD Polyester-based nonwoven fabric characterized by satisfying the following condition 1-1): 1-1) . Claim 3 A polyester-based nonwoven fabric according to claim 1, characterized in that the first polyester has an intrinsic viscosity of 0.65 dl / g to 0.80 dl / g. Claim 4 A polyester-based nonwoven fabric according to claim 1, characterized in that the second component filament is formed by fusing. Claim 5 A polyester-based nonwoven fabric according to claim 1, wherein the second polyester is a copolyester formed by copolymerizing one or more acid components selected from terephthalic acid, dimethyl terephthalate, isophthalic acid, and dimethyl isophthalate, and one or more diol components selected from 1,4-butanediol (BD), ethylene glycol (EG), and neopentyl glycol (NPG). Claim 6 In claim 1, the polyester nonwoven fabric has a machine direction (MD) tensile strength (T) before the tufting process. MD,0 ) and vertical (CD) tensile strength (T CD,0 The deviation between ) is T CD,0 A polyester-based nonwoven fabric characterized by having a tensile strength of ×0.05 or less and a reduction rate of 60% or less in both the machine direction and the vertical direction after the tufting process. Claim 7 In claim 6, the polyester-based nonwoven fabric is T before the tufting process MD,0 and T CD,0 Polyester-based nonwoven fabric characterized by having a thickness of 25 kgf / 5 cm to 35 kgf / 5 cm. Claim 8 delete Claim 9 A polyester nonwoven fabric according to claim 1, characterized in that the thermal shrinkage rate in the machine direction measured according to the following measurement method is 1.5% or less and the thermal shrinkage rate in the vertical direction is 1.0% or less: [Measurement method] A pattern of 20cm × 20cm is drawn on a nonwoven fabric specimen of 25cm × 25cm in the machine direction and vertical direction, respectively, and the specimen is preheated at 180℃ for 3 minutes on a preheating plate using a Mathis oven, then removed and the shrunk length is measured to calculate the shrinkage rate. Claim 10 The polyester nonwoven fabric according to claim 1, characterized in that the tear strength prior to the tufting process is 7 kgf to 13 kgf in both the machine direction and the vertical direction. Claim 11 In claim 1, the polyester-based nonwoven fabric is characterized by satisfying the following condition formulas 2) and 3): 2) 3) In the above condition expressions 2) and 3), the above and Each represents the intrinsic viscosity of the first polyester and the intrinsic viscosity of the second polyester. Claim 12 A polyester-based nonwoven fabric according to claim 1, wherein the first component filament has a fineness of 7 to 10 denier and the second component filament has a fineness of 2 to 4 denier, and the number of filaments of the first component filament is included in a multiple of 2 to 5 times the number of filaments of the second component filament. Claim 13 A foam sheet for carpets comprising a polyester-based nonwoven fabric according to any one of claims 1 to 7 and claims 9 to 12. Claim 14 1) A step of forming a blended web by blending a first polyester having a melting point of 252℃ to 300℃ and a second polyester having a melting point of 160℃ to 220℃ and laminating the resulting webs; and 2) a step of heat-bonding the blended web with hot air having a temperature of 0°C to 10°C or higher than the melting point of the second polyester; a method for manufacturing a polyester-based nonwoven fabric comprising: the weight ratio of the first component filament and the second component filament is 85:15 to 90:10, the intrinsic viscosity of the second polyester is 0.74 dl / g to 0.82 dl / g, and the machine direction bending strength and vertical direction stiffness measured by the measurement method specified in ASTM D 6125-97 before the tufting process are both 100 mg to 300 mg, and the machine direction stiffness (S) before the tufting process MD ) and vertical stiffness (S CD A method for manufacturing a polyester-based nonwoven fabric according to claim 1, characterized in that ) satisfies the following condition 1): 1) . Claim 15 A method for manufacturing a polyester-based nonwoven fabric according to claim 14, characterized in that, in step 1) above, the first polyester and the second polyester are each stretched at a speed of 4,500 m / min to 5,200 m / min to form the first component filament and the second component filament, respectively.

Citation Information

Patent Citations

  • Improved nonwovens and fibers

    JP2007535624A

  • Filter spun bond nonwoven and manufacturing method

    KR1020180097515A

  • Non-woven structure with fibers catalyzed by a metallocene catalyst

    US20200157716A1

  • Highly uniform spunbond nonwoven fabric

    JP2013544975A

  • Polyester Nonwoven Fabric, Method for Manufacturing The Same, and Primary Backing Substrae for Carpet Comprising The Same