Polyamide-based resin expanded beads
By setting the crystallite size of polyamide resin foam particles to exceed 8 nm and optimizing other properties, the moldability and heat resistance of polyamide resin foam particles are significantly improved, enabling stable molding and lightweight, heat-resistant molded bodies.
Patent Information
- Application Number
- KR1020210021364
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-18
- Filing Date
- 2021-02-17
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-02-17
AI Technical Summary
Existing polyamide-based resin foam particles have a narrow moldable range, particularly when the thickness of the molded article is thick, leading to insufficient moldability.
The polyamide resin foam particles are designed with a crystallite size exceeding 8 nm, measured by X-ray diffraction, and possess specific melting characteristics, apparent density, closed-cell ratio, average bubble diameter, and surface film thickness, which enhance moldability and heat resistance.
The enhanced crystallite size and properties result in polyamide resin foam particles with improved moldability, allowing stable molding under various conditions, including thick sections, and provide lightweight molded bodies with excellent heat resistance.
Smart Images

Figure 112021019371323-PAT00001 
Figure 112021019371323-PAT00002 
Figure 112021019371323-PAT00003
Abstract
Description
Technology Field
[0001] The present invention relates to polyamide resin foam particles. Background Technology
[0002] Polyamide resins are known to be resins with high heat resistance, as well as excellent wear resistance and chemical resistance. Foamed molded articles produced by foaming this polyamide resin are expected to be developed for automotive parts and other applications because they can achieve lightweighting while maintaining these excellent properties. For this reason, various studies have been conducted on foamed molded articles of polyamide resins to facilitate their practical application in various fields. For example, Patent Document 1 discloses a polyamide resin foamed particle molded article characterized by having a crystallite size of 10 nm or more and a degree of crystallinity of 10 to 50%, which is obtained by filling polyamide resin pre-foamed particles into a mold cavity and performing a process of increasing the temperature in multiple stages using steam for the purpose of improving heat resistance and sound insulation. Prior art literature
[0003] Patent Document 1: International Publication No. 2016 / 147582 The problem to be solved
[0004] Patent Document 1 discloses a molded article of a polyamide-based resin foamed particle with excellent heat resistance. However, the foamed particle of Patent Document 1 has a narrow range of moldable range, and depending on the shape of the molded article, such as when the thickness is thick, the moldability is insufficient.
[0005] Therefore, the problem that the present invention aims to solve is to provide polyamide-based resin foam particles with excellent moldability. means of solving the problem
[0006] The inventors have discovered, through repeated close examination, that the above problem can be solved by setting the crystallite size of the polyamide resin foam particles to a specific value.
[0007] That is, the present invention provides the following [1] to [8].
[0008] [1] Polyamide resin foam particles with a crystallite size exceeding 8 nm as measured by X-ray diffraction.
[0009] [2] Polyamide resin foam particles described in [1] above, which are used as test specimens based on the differential scanning calorimetry method of JIS K7122-1987 and have a total melting heat of 40 to 140 J / g of the DSC curve measured when heated from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min.
[0010] [3] Polyamide resin foam particles described in [1] or [2] above, having an apparent density of 10 to 300 kg / m³.
[0011] [4] Polyamide resin foam particles described in [1] or [2], wherein the peak temperature of the melting peak of the DSC curve of the second heating obtained under condition 1 below is 185 to 285°C.
[0012] Condition 1
[0013] Based on the differential scanning calorimetry method of JIS K7121-1987, a polyamide resin foam particle is used as a test specimen, and the DSC curve measured when heating from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min, maintaining the temperature for 10 minutes, cooling to 30°C at a cooling rate of 10°C / min, and then heating again to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min is used as the DSC curve of the second heating.
[0014] [5] Polyamide resin foam particles described in [1] or [2], wherein the crystallite size of the polyamide resin foam particles measured by X-ray diffraction is 10 nm or larger.
[0015] [6] Polyamide resin foam particles described in [1] or [2] above, having an independent cell ratio of more than 90%.
[0016] [7] Polyamide resin foam particles described in [1] or [2], having an average bubble diameter of 20 to 200 μm.
[0017] [8] Polyamide resin foam particles described in [1] or [2], having a surface film thickness of 5 to 50 μm. Effects of the invention
[0018] According to the present invention, polyamide-based resin foam particles with excellent moldability can be provided. Specific details for implementing the invention
[0019] The present invention is a polyamide-based resin foam particle having a crystallite size exceeding 8 nm as measured by X-ray diffraction.
[0020] [Polyamide resin foam particles]
[0021] <Crystallinity of Polyamide Resin Foam Particles>
[0022] The polyamide-based resin foam particles of the present invention have a crystallite size exceeding 8 nm as measured by X-ray diffraction. Since the crystallite size exceeds 8 nm, the pressure range for molding is wide, resulting in excellent moldability. The crystallite size measured by X-ray diffraction is 9 nm or larger, 10 nm or larger is more preferable, 11 nm or larger is more preferable, and 12 nm or larger is more preferable. Additionally, although there is no upper limit, 30 nm or smaller is preferred, and 20 nm or smaller is more preferable. Although the reason why the moldability of the polyamide-based resin foam particles is excellent when the crystallite size is within the above range is not entirely clear, it is believed that the large crystallite size improves the heat resistance of the foam particles, allowing for stable molding under various conditions, such as when the thickness of the target molded body is thick, even at high temperatures during molding. The crystallite size is measured by X-ray diffraction, specifically by the method described below. X-ray diffraction (XRD) measurement of polyamide resin foam particles is performed by transmission using an X-ray scattering device. The X-ray diffraction profile obtained by the X-ray diffraction measurement is separated into crystalline diffraction peaks and amorphous diffraction peaks by assuming a Gaussian function as the peak shape. The full width at half maximum (β(rad)) of the peak having the narrowest peak width among the peaks obtained by peak separation is calculated, and the crystallite size (D) of the foam particles is calculated according to the following equation (2) using this full width at half maximum (β).
[0023]
[0024] β is the full width at half maximum of the crystal-derived diffraction peak, b is the full width at half maximum of the X-ray diffusion, λ is the wavelength of the X-ray (nm), and θ is the Bragg angle at the peak position (half of the diffraction angle (2θ)).
[0025] In addition, it is preferable that the crystallites of the polyamide-based resin foam particles, whose crystallite size exceeds 8 nm, consist of α-crystals. The crystals of the polyamide-based resin foam particles consist of α-crystals and γ-crystals; since α-crystals are more stable and tend to have higher mechanical properties and heat resistance compared to γ-crystals, it is preferable that the crystallites mainly consist of α-crystals, and it is even more preferable that the crystallite size of the α-crystals exceeds 8 nm. Whether the crystals are α-crystals or γ-crystals can be determined from the diffraction angle (2θ) at the peak position of the X-ray diffraction profile. In wide-angle X-ray diffraction measurements in the range of 5 to 35 degrees, the α-crystals appear around 20 degrees and 24 degrees, and the γ-crystals appear around 21 degrees.
[0026] Melting Characteristics of Polyamide Resin Foam Particles
[0027] It is preferable that the polyamide-based resin foam particles of the present invention have melting characteristics as described below. For the polyamide-based resin foam particles of the present invention, based on the differential scanning calorimetry method of heat flux of JIS K7122-1987, it is preferable that the total heat of melting of the DSC curve measured when the polyamide-based resin foam particles are used as a test specimen and heated from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min is 40 to 140 J / g, more preferable that it is 45 J / g or higher, and even more preferable that it is 50 J / g or higher. Furthermore, it is more preferable that it is 120 J / g or lower, and even more preferable that it is 100 J / g or lower. Since the DSC curve is obtained from the first heating using the polyamide-based resin foam particles as a test specimen, the above DSC curve is designated as the DSC curve of the first heating. It means that the larger the total heat of fusion of the DSC curve of the first heating, the more advanced the crystallization of the foamed particles is. Foamed particles that have undergone crystallization have superior heat resistance. It is desirable that the total heat of fusion of the DSC curve of the first heating falls within the above range, as this results in foamed particles with superior heat resistance.
[0028] The total heat of fusion is calculated as follows. A straight line is drawn connecting the point at 150°C on the obtained DSC curve and the point on the DSC curve representing the temperature at the end of the melting peak. Using this straight line as the baseline, the area enclosed by the baseline and the DSC curve located on the endothermic side relative to the baseline corresponds to the endothermic energy of the melting peak, and the heat calculated from this is the total heat of fusion. If the DSC curve has multiple melting peaks, the sum of all heat amounts is used as the total heat of fusion. Also, the point on the DSC curve representing the temperature at the end of the melting peak refers to the temperature at the end of the melting peak of the melting peak on the highest temperature side. In this specification, for the measurement of the DSC curve, a test specimen that has been set still for at least 24 hours under an environment of 23°C and 50% relative humidity is used.
[0029] The polyamide resin foam particles of the present invention preferably have a peak temperature of the melting peak of the DSC curve of the second heating obtained under condition 1 below of 185 to 285°C. The peak temperature of the melting peak of the DSC curve of the second heating obtained here (hereinafter also referred to as the melting point of the polyamide resin foam particles; also denoted as Tm1) corresponds to the melting point of the polyamide resin derived from the inherent crystal structure of the polyamide resin.
[0030] Condition 1
[0031] Based on the differential scanning calorimetry method of JIS K7121-1987, a polyamide resin foam particle is used as a test specimen, and the DSC curve measured when heating from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min, maintaining the temperature for 10 minutes, cooling to 30°C at a cooling rate of 10°C / min, and then heating again to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min is used as the DSC curve of the second heating.
[0032] The peak temperature of the melting peak of the DSC curve of the second heating step is preferably 185 to 285°C, more preferably 188°C or higher, and even more preferably 190°C or higher. Meanwhile, from the perspective of facilitating temperature control during foaming, the peak temperature of the melting peak of the second DSC curve is more preferably 280°C or lower, more preferably 260°C or lower, even more preferably 230°C or lower, and even more preferably 225°C or lower. It is desirable that the melting point of the polyamide resin foam particles satisfies the above range, as this makes it easier to obtain polyamide resin foam particles with low apparent density and also makes it easier to obtain polyamide resin foam particles with excellent heat resistance.
[0033] <Other Characteristics of Polyamide Resin Foam Particles>
[0034] In addition to the melting characteristics mentioned above, the polyamide resin foam particles of the present invention preferably have characteristics as described below.
[0035] Preferably, the apparent density of the polyamide-based resin foam particles of the present invention is 10 to 300 kg / m³. The apparent density of the polyamide-based resin foam particles of the present invention is preferably 10 kg / m³ or more, more preferably 30 kg / m³ or more, even more preferably 50 kg / m³ or more, and even more preferably 100 kg / m³ or more. Furthermore, the apparent density of the polyamide-based resin foam particles is preferably 300 kg / m³ or less, more preferably 250 kg / m³ or less, even more preferably 200 kg / m³ or less, and even more preferably 150 kg / m³ or less. If the apparent density of the foam particles is within the above range, the foam particles or the molded body made of foam particles are less likely to shrink, making it easier to obtain a good foam particle molded body. In addition, the apparent density of the polyamide-based resin foam particles is measured by the following method.
[0036] Prepare a graduated cylinder containing water at a temperature of 23°C, and measure the mass (W1) of expanded particles with a volume of approximately 500 cm³ that have been left in the graduated cylinder for more than 24 hours under conditions of 50% relative humidity, 23°C, and 1 atm, and then sink them using a wire mesh. Measure the volume (V1 [cm³]) of the expanded particles read from the rise in water level, taking into account the volume of the wire mesh, and divide the mass (W1 [g]) of the expanded particles by the volume (V1) (W1 / V1) and convert the unit to [kg / m³] to obtain the apparent density of the expanded particles.
[0037] The closed-cell ratio of the polyamide resin foam particles of the present invention is preferably 85% or higher, more preferably 88% or higher, and even more preferably exceeds 90%. When the closed-cell ratio of the foam particles satisfies the above range, it is easy to obtain foam particles with low apparent density. In addition, the moldability of the foam particles is good, and the foam particle molded body produced by molding the foam particles in a mold has excellent surface properties and fusion properties. Thus, by using foam particles with large crystallite sizes and a closed-cell ratio within the above range, it is possible to obtain a molded body with excellent moldability and lighter weight. Furthermore, the closed-cell ratio is the ratio of the volume of closed cells to the volume of all cells in the foam particles, and can be obtained using an air-comparison specific gravity meter based on ASTM-D2856-70.
[0038] The average pore size of the polyamide-based resin foam particles of the present invention is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more. Meanwhile, the average pore size of the polyamide-based resin foam particles is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 140 μm or less. In addition, the average pore size of the polyamide-based resin foam particles is measured by the following method.
[0039] First, the foam particle is divided into approximately two sections passing through the center of the foam particle, and the cross-section is photographed using a scanning electron microscope. Next, from the obtained cross-sectional photograph, straight lines are drawn at equal intervals in eight directions from near the center of the cross-section of the foam particle to the outermost surface of the foam particle, changing the angle by 45°, and the number of bubbles intersecting these lines is counted. The value obtained by dividing the sum of the lengths of these lines by the counted number of bubbles is taken as the bubble diameter of the foam particle. This operation is performed in the same way for 10 or more foam particles, and the arithmetic mean value of the bubble diameters of each foam particle is taken as the average bubble diameter of the foam particle.
[0040] The surface film thickness of the polyamide resin foam particles of the present invention is preferably 5 μm or more, and more preferably 10 μm or more. Meanwhile, the surface film thickness of the polyamide resin foam particles is more preferably 50 μm or less, and even more preferably 30 μm or less. If the surface film thickness of the polyamide resin foam particles is within the above range, internal pressure is applied within the bubbles when the foam particles are pressurized, thereby making the foam particles excellent in terms of surface properties during mold molding. Furthermore, it is difficult for the foam particles to break when mold molding, making it easy to obtain a high-magnification foam particle molded body. Moreover, the excellent fusion between the foam particles during mold molding makes it possible to mold without excessively increasing the molding steam pressure. In particular, since the crystallite size of the foam particles is large, the heat resistance of the foam particles is excellent, allowing for the provision of foam particles with excellent mold moldability, and a molded body that is lightweight and has excellent heat resistance can be obtained.
[0041] The surface film thickness of a polyamide resin foam particle can be measured as follows. The length (surface film thickness) from the outermost surface of the foam particle to the outermost bubble of the foam particle is measured along eight straight lines from the vicinity of the center of the cross-section of the foam particle obtained from the average bubble diameter of the foam particle to the outermost surface of the foam particle, and the average surface film thickness of the foam particle is obtained by arithmetically averaging these values.
[0042] It is preferable that the polyamide resin foam particles of the present invention have a ratio [(Tm1-20℃ compressive stress) / (23℃ compressive stress)] of 5% compressive stress at a temperature 20℃ lower than the melting point (Tm1) of the polyamide resin foam particles (Tm1-20℃ compressive stress) to 5% compressive stress at 23℃ (23℃ compressive stress) [(Tm1-20℃ compressive stress) / (23℃ compressive stress)] of 0.1 or more.
[0043] The above ratio [(Tm1-20℃ compressive stress) / (23℃ compressive stress)] is more preferably 0.15 or higher, and even more preferably 0.2 or higher. Additionally, the upper limit is approximately 1. Foamed particles with a high above ratio [(Tm1-20℃ compressive stress) / (23℃ compressive stress)] indicate that the decrease in compressive stress at high temperatures relative to the compressive stress at room temperature is small, and that they maintain high compressive stress even at high temperatures and have excellent heat resistance. Polyamide resin foamed particles with a large value of the above ratio [(Tm1-20℃ compressive stress) / (23℃ compressive stress)] can be suitably used for applications such as fillers for composite molding. Furthermore, the reason for setting the temperature (Tm1-20℃) to be 20℃ lower than the melting point of the polyamide resin foamed particles is to evaluate the compressive properties at a temperature where the crystals of the foamed particles do not melt.
[0044] The 5% compressive stress at a temperature 20°C lower than the melting point of the polyamide resin foam particles (Tm1-20°C) can be obtained by measuring the foam particles in compression mode using a thermal analyzer (TMA; e.g., Hitachi High-Tech Science Corp. product “TMA7100”). Specifically, one foam particle is randomly selected, and a load of 10 mN is applied to the short diameter direction of the foam particle using a compression probe, and then the temperature is raised to a temperature 20°C lower than the melting point of the polyamide resin foam particles (Tm1-20°C). Subsequently, while maintaining an isothermal temperature 20°C lower than the melting point of the polyamide resin foam particles (Tm1-20°C), the particle is pushed in at a speed of 1 mm / min, and the load of the probe is monitored. The stress at the point where the thickness of the foam particle becomes 5% of the thickness of the foam particle before compression is defined as the 5% compressive stress of the foam particle at Tm1-20°C.
[0045] The 5% compressive stress at 23°C can similarly be obtained by measuring the foam particles in compression mode using a thermal analyzer (TMA; for example, Hitachi High-Tech Science Corp. product “TMA7100”). Specifically, one foam particle is randomly selected, and a load of 10 mN is applied to the short diameter direction of the foam particle using a compression probe. Then, it is pushed in at a speed of 1 mm / min at 23°C, and the load of the probe is monitored. The stress at the point where the thickness of the foam particle becomes 5% of the thickness of the foam particle before compression is defined as the 5% compressive stress at 23°C.
[0046] <Polyamide resin and thermoplastic resin included in polyamide-based resin foam particles>
[0047] Polyamide resin foam particles are obtained by foaming polyamide resin particles. Accordingly, polyamide resin foam particles contain the polyamide resin described in the [Polyamide Resin] section below. In addition, they may contain a thermoplastic resin or a thermoplastic elastomer other than the polyamide resin described in the (Polyamide Resin Particles) section below.
[0048] It is explained in detail below.
[0049] Examples of polyamide resins included in the polyamide resin foam particles include polyamide and polyamide copolymer, and polyamide copolymer is preferred.
[0050] As polyamides, for example, poly(6-aminohexanoic acid) (polycaproamide, Nylon 6), also known as poly(caprolactam); poly(laurolactam) (Nylon 12); poly(hexamethylene adipamide) (Nylon 66); poly(7-aminoheptanoic acid) (Nylon 7); poly(8-aminooctanoic acid) (Nylon 8); poly(9-aminononanoic acid) (Nylon 9); poly(10-aminodecanoic acid) (Nylon 10); poly(11-aminoundecanoic acid) (Nylon 11); poly(hexamethylene sebacaramide) (Nylon 610); poly(decamethylene sebacaramide) (Nylon 1010); poly(hexamethylene azelamide) (Nylon 69); poly(tetramethylene adipamide) (Nylon 46); and poly(tetramethylene Examples of homopolymers include poly(pentamethylene adipamide) (Nylon 410), poly(pentamethylene adipamide) (Nylon 56), and poly(pentamethylene sebacamide) (Nylon 510). A polyamide copolymer is defined as having two or more repeating units and having amide bonds in at least a portion of each repeating unit. Examples of polyamide copolymers include caprolactam / hexamethylene diaminoadipic acid (Nylon 6 / 66), caprolactam / hexamethylene diaminoadipic acid / laurylactam (Nylon 6 / 66 / 12), and caprolactam / laurylactam copolymer (Nylon 6 / 12). Polyamide resins may use one of these polyamides and polyamide copolymers alone, or may use a combination of two or more. From the perspective that it is easy to obtain polyamide resin foam particles with high water absorption and large crystallite size, it is preferable to use a polyamide resin that is a combination of one or more types selected from nylon 6, nylon 66, and nylon 6 / 66 among the above polyamide resins, and it is more preferable to use nylon 6 / 66.
[0051] The polyamide copolymer may be a block copolymer in which a certain amount of the same repeating unit amide is followed by a certain amount of another type of amide, or a random copolymer in which different types of amide are repeated randomly, but it is preferable to be a random copolymer. If the polyamide copolymer is a random copolymer, it becomes possible to mold polyamide-based resin foam particles with a relatively low molding steam pressure when molding them in a mold.
[0052] The melting point (Tm) of the polyamide resin included in the polyamide resin foam particles is preferably 180°C or higher, more preferably 185°C or higher, even more preferably 188°C or higher, and even more preferably 190°C or higher. Meanwhile, the melting point (Tm) of the polyamide resin is preferably 280°C or lower, more preferably 260°C or lower, even more preferably 230°C or lower, and even more preferably 225°C or lower. A polyamide resin satisfying the above melting point range is desirable because it makes it easier to obtain polyamide resin foam particles with low apparent density and also makes it easier to obtain polyamide resin foam particles with excellent heat resistance. In addition, the term "melting point of the polyamide resin" refers to the melting point of the polyamide resin when a single type of polyamide resin is used alone. In cases where the polyamide resin is composed of a mixture of two or more types of polyamide resins or a mixture of a polyamide resin and another thermoplastic resin, it refers to the melting point of the mixture that has been kneaded in advance using an extruder or the like.
[0053] The melting point (Tm) of the polyamide resin included in the polyamide resin foam particles is a value obtained as the peak point temperature of the melting peak of the second DSC curve obtained under conditions identical to Condition 1 above, except that the polyamide resin of the raw material is used as a test specimen and left to stand for 24 hours in an environment of 23°C and 50% relative humidity, and then the test specimen is changed to a polyamide resin. In addition, if the DSC curve has multiple melting peaks, the peak point temperature of the melting peak having the largest area is adopted as the melting temperature.
[0054] The polyamide resin included in the polyamide resin foam particles has a bending modulus of preferably 1000 MPa or higher, more preferably 1200 MPa or higher, and even more preferably 1500 MPa or higher. It is desirable for the polyamide resin to have a bending modulus within the above range because, due to the high bending modulus, it is difficult to shrink even when exposed to room temperature after foaming, making it easier to obtain foamed particles with a high magnification. In addition, it is desirable because the high bending modulus results in excellent moldability. Furthermore, the upper limit of the polyamide resin's bending modulus is approximately 3000 MPa.
[0055] The flexural modulus of a polyamide resin can be obtained by measuring the test specimen in accordance with JIS K7171: 2016 after leaving it at a temperature of 23°C and a relative humidity of 50% for 24 hours.
[0056] The polyamide resin included in the polyamide resin foam particles has a density preferably of 1.05 g / cm³ or higher, and more preferably of 1.1 g / cm³ or higher. The density can be measured based on the method described in ISO 1183-3.
[0057] It is preferable that the polyamide resin included in the polyamide resin foam particles be a terminal-blocked polyamide resin in which the functional groups at the ends of the molecular chains are blocked. This allows for more reliable suppression of hydrolysis during the manufacturing process of the polyamide resin foam particles and makes it easier to obtain polyamide resin foam particles capable of withstanding in-mold molding.
[0058] Furthermore, the durability of the polyamide-based resin foamed particle molded body (hereinafter also referred to simply as "foamed particle molded body" or "molded body") obtained by in-mold molding is improved.
[0059] Examples of end-blocking agents for blocking the above molecular chain ends may include carbodiimide compounds, oxazoline compounds, isocyanate compounds, epoxy compounds, etc.
[0060] Among these, carbodiimide compounds are preferred. Specifically, examples include aromatic monocarbodiimides such as bis(dipropylphenyl)carbodiimide (e.g., "Stabaxol 1-LF" from Rhein Chemie), aromatic polycarbodiimides (e.g., "Stabaxol P", "Stabaxol P100", "Stabaxol P400" from Rhein Chemie), and aliphatic polycarbodiimides such as poly(4,4'-dicyclohexylmethanecarbodiimide) (e.g., "Carbodelite LA-1" from Nisshinbo Chemical Co., Ltd.). These terminal clotting agents may be used alone or in combination of two or more types.
[0061] In addition, the amount of terminal blocking agent is preferably 0.1 to 5 parts by mass per 100 parts by mass of polyamide resin, and more preferably 0.3 to 3 parts by mass.
[0062] As such, the polyamide resin used in the present invention is preferably a polyamide resin terminally blocked by one or more terminal blocking agents selected from carbodiimide compounds, epoxy compounds, and isocyanate compounds, and is more preferably a polyamide resin terminally blocked by a carbodiimide compound.
[0063] The polyamide resin included in the polyamide resin foam particles may be a single type, or a mixture of polyamide resins containing two or more types of the polyamide resin.
[0064] The polyamide-based resin foam particles of the present invention may contain other thermoplastic resins within a range that does not impede the purpose or effect of the present invention, and may contain a thermoplastic elastomer as the thermoplastic resin. Examples of other thermoplastic resins and thermoplastic elastomers include polyethylene-based resins, polypropylene-based resins, polystyrene-based resins, vinyl acetate resins, thermoplastic polyester resins, acrylic acid ester resins, methacrylic acid ester resins, ethylene-propylene-based rubbers, ethylene-1-butene rubbers, propylene-1-butene rubbers, ethylene-propylene-diene-based rubbers, isoprene rubbers, neoprene rubbers, nitrile rubbers, rubbers such as styrene-diene block copolymers or hydrogenated derivatives of styrene-diene block copolymers.
[0065] The content of other thermoplastic resins in the polyamide resin foam particles is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, with respect to heat resistance, wear resistance and chemical resistance, per 100 parts by mass of the polyamide resin, and even more preferably the polyamide resin foam particles are composed only of polyamide resin.
[0066] In addition to the polyamide resin, various additives such as commonly used antistatic agents, conductivity imparters, lubricants, antioxidants, UV absorbers, flame retardants, metal deactivators, colorants (pigments, dyes, etc.), crystal nucleating agents, and fillers can be appropriately incorporated into the polyamide resin foam particles as needed.
[0067] Method for manufacturing foamed polyamide resin particles
[0068] As long as the polyamide resin foam particles of the present invention have a crystallite size exceeding 8 nm as measured by X-ray diffraction, there are no restrictions on the manufacturing method, but it is preferable to manufacture them by the following method.
[0069] The polyamide-based resin foam particles of the present invention are preferably foam particles manufactured by a method having a process of heating the resin particles while they contain more moisture than the amount absorbed under normal environmental conditions to increase the crystallite size. Specifically, examples include a method of heating resin particles while they contain moisture to produce resin particles with grown crystallites, impregnating the resin particles with a foaming agent, and foaming them to produce foam particles with grown crystallites; a method of impregnating resin particles containing moisture with a foaming agent and heating them to foam them to produce foam particles with grown crystallites; and a method of incorporating water into foam particles and heating them to produce foam particles with grown crystallites.
[0070] Among the above, from the perspective of making it easy to increase the crystallite size, it is preferable that the polyamide resin foam particles of the present invention be obtained by foaming water-containing polyamide resin particles by adding a foaming agent and heating them.
[0071] Methods for incorporating moisture into polyamide resin particles or polyamide resin foam particles include immersing the resin particles or foam particles in water, leaving the resin particles or foam particles in an atmosphere of high humidity, such as 90% or more relative humidity, or spraying water onto the resin particles or foam particles. Among the above, the method of incorporating moisture by immersion in water is preferred in that it facilitates the incorporation of moisture.
[0072] In addition, when polyamide-based resin particles or polyamide-based resin foam particles are heated in water, they can be considered to satisfy the above moisture content because they are filled with water. The moisture content in the resin particles or foam particles can be determined by a Karl Fischer moisture measuring device, and specifically, by the following method.
[0073] After wiping off the water on the surface of the polyamide resin particles or polyamide resin foam particles with a dry cloth, the polyamide resin particles or polyamide resin foam particles are weighed. Next, the internal moisture is vaporized by heating the polyamide resin particles or polyamide resin foam particles using a heating moisture vaporization device, and the moisture content is measured by Karl Fischer titration (total titration method) using a Karl Fischer moisture measuring device.
[0074] The moisture content of the polyamide resin particles containing moisture or the polyamide resin particles is preferably 3% or more, more preferably 5% or more, even more preferably 7% or more, and particularly preferably 16% or more.
[0075] Methods for heating polyamide resin particles or polyamide resin foam particles include immersing the resin particles or foam particles in a medium such as water and heating the medium, or heating the resin particles or foam particles by blowing hot air. Among the above, heating in a medium such as water is preferred in that it heats uniformly.
[0076] When heating polyamide resin particles or polyamide resin foam particles, the heating temperature is preferably 90°C lower than the melting point (Tm) of the polyamide resin (Tm-90°C) or higher, more preferably 80°C or higher, and even more preferably 70°C or higher. Meanwhile, the heating temperature is preferably 20°C higher than the melting point (Tm) of the polyamide resin (Tm+20°C) or lower, more preferably 10°C or lower, and even more preferably lower than the melting point of the polyamide resin.
[0077] (Polyamide resin particles)
[0078] The polyamide resin particles used in the manufacture of polyamide resin foam particles contain polyamide resin. The polyamide resin may be a single type, or it may be a mixture of polyamide resins containing two or more types of polyamide resins.
[0079] The above-mentioned polyamide resin particles may contain other thermoplastic resins within a range that does not impede the purpose or effect of the present invention, and may contain a thermoplastic elastomer as the thermoplastic resin. Examples of other thermoplastic resins and thermoplastic elastomers include polyethylene resins, polypropylene resins, polystyrene resins, vinyl acetate resins, thermoplastic polyester resins, acrylic acid ester resins, methacrylic acid ester resins, ethylene-propylene rubbers, ethylene-1-butene rubbers, propylene-1-butene rubbers, ethylene-propylene-diene rubbers, isoprene rubbers, neoprene rubbers, nitrile rubbers, rubbers such as styrene-diene block copolymers or hydrogenated derivatives of styrene-diene block copolymers.
[0080] The content of other thermoplastic resins in the polyamide resin particles is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, with respect to obtaining polyamide resin foam particles with excellent heat resistance, wear resistance and chemical resistance, with respect to 100 parts by mass of polyamide resin.
[0081] In addition to the polyamide resin, various additives such as commonly used foaming agents, antistatic agents, conductivity imparters, lubricants, antioxidants, UV absorbers, flame retardants, metal deactivators, coloring agents (pigments, dyes, etc.), crystal nucleating agents, and fillers may be appropriately blended into the polyamide resin particles as needed. Examples of foaming agents include inorganic foaming agents such as talc, sodium chloride, calcium carbonate, silica, titanium oxide, gypsum, zeolite, borax, aluminum hydroxide, alum, and carbon, and organic foaming agents such as phosphate compounds, amine compounds, and polytetrafluoroethylene (PTFE). Although the amount of these various additives varies depending on the intended use of the molded article, it is preferable that the amount be 25 parts by weight or less per 100 parts by weight of the polymer component constituting the polyamide resin particles. More preferably, it is 15 parts by weight or less, even more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less.
[0082] The average mass per polyamide resin particle is appropriately set according to the size, apparent density, etc., of the desired polyamide resin foamed particles, but is preferably 0.5 to 15.0 mg. Within the above range, the apparent density can be reduced. In this regard, the lower limit of the mass of the polyamide resin particles is more preferably 1.0 mg, and even more preferably 1.5 mg. Meanwhile, the upper limit is more preferably 10.0 mg, even more preferably 7.0 mg, and even more preferably 5.0 mg.
[0083] The method for manufacturing polyamide-based resin particles is not particularly limited and can be obtained by known methods. For example, polyamide-based resin particles can be obtained by a strand cutting method in which a polyamide-based resin and additives such as a foaming agent and a coloring agent are fed into an extruder as needed and mixed to form a molten mixture, the molten mixture is extruded in a strand shape from a small hole of a die installed at the end of the extruder, and the extruded strand is cut to a predetermined mass using a pelletizer; a hot cutting method in which the molten mixture is cut immediately after being extruded in the gas phase; and an underwater cutting method (UWC method) in which the molten mixture is cut immediately after being extruded in water.
[0084] [Polyamide resin]
[0085] Examples of polyamide resins in this specification include polyamide and polyamide copolymer, and polyamide copolymer is preferred.
[0086] As polyamides, for example, poly(6-aminohexanoic acid) (polycaproamide, Nylon 6), also known as poly(caprolactam); poly(laurolactam) (Nylon 12); poly(hexamethylene adipamide) (Nylon 66); poly(7-aminoheptanoic acid) (Nylon 7); poly(8-aminooctanoic acid) (Nylon 8); poly(9-aminononanoic acid) (Nylon 9); poly(10-aminodecanoic acid) (Nylon 10); poly(11-aminoundecanoic acid) (Nylon 11); poly(hexamethylene sebacaramide) (Nylon 610); poly(decamethylene sebacaramide) (Nylon 1010); poly(hexamethylene azelamide) (Nylon 69); poly(tetramethylene adipamide) (Nylon 46); and poly(tetramethylene Examples of homopolymers include poly(pentamethylene adipamide) (Nylon 410), poly(pentamethylene adipamide) (Nylon 56), and poly(pentamethylene sebacamide) (Nylon 510). A polyamide copolymer is defined as having two or more repeating units and having amide bonds in at least a portion of each repeating unit. Examples of polyamide copolymers include caprolactam / hexamethylene diaminoadipic acid (Nylon 6 / 66), caprolactam / hexamethylene diaminoadipic acid / laurylactam (Nylon 6 / 66 / 12), and caprolactam / laurylactam copolymer (Nylon 6 / 12). Polyamide resins may use one of these polyamides and polyamide copolymers alone, or may use a combination of two or more. From the perspective that it is easy to obtain polyamide resin foam particles with high water absorption and large crystallite size, it is preferable to use a polyamide resin that is a combination of one or more types selected from nylon 6, nylon 66, and nylon 6 / 66 among the above polyamide resins, and it is more preferable to use nylon 6 / 66.
[0087] The polyamide copolymer may be a block copolymer in which a certain amount of the same repeating unit amide is followed by a certain amount of another type of amide, or a random copolymer in which different types of amide are repeated randomly, but it is preferable to be a random copolymer. If the polyamide copolymer is a random copolymer, it becomes possible to mold polyamide-based resin foam particles with a relatively low molding steam pressure when molding them in a mold.
[0088] The melting point (Tm) of the polyamide resin is preferably 180°C or higher, more preferably 185°C or higher, even more preferably 188°C or higher, and even more preferably 190°C or higher. Meanwhile, the melting point (Tm) of the polyamide resin is preferably 280°C or lower, more preferably 260°C or lower, even more preferably 230°C or lower, and even more preferably 225°C or lower. A polyamide resin satisfying the above melting point range is desirable because it makes it easier to obtain polyamide resin foam particles with low apparent density and also makes it easier to obtain polyamide resin foam particles with excellent heat resistance. Furthermore, the term "melting point of the polyamide resin" refers to the melting point of the polyamide resin when a single type of polyamide resin is used alone. When the polyamide resin consists of a mixture of two or more types of polyamide resins or a mixture of a polyamide resin and another thermoplastic resin, it refers to the melting point of the mixture that has been kneaded in advance using an extruder or the like.
[0089] The melting point (Tm) of a polyamide resin is a value obtained as the peak point temperature of the melting peak of the second DSC curve obtained under conditions identical to Condition 1 above, except that the test specimen is set as a test specimen of the raw polyamide resin and left to stand for 24 hours in an environment of 23°C and 50% relative humidity, and then the test specimen is changed to a polyamide resin. In addition, if the DSC curve has multiple melting peaks, the peak point temperature of the melting peak having the largest area is adopted as the melting temperature.
[0090] In this specification, the flexural modulus of the polyamide resin is preferably 1000 MPa or higher, more preferably 1200 MPa or higher, and even more preferably 1500 MPa or higher. It is desirable that the flexural modulus of the polyamide resin be within the above range, as this makes it difficult to shrink even when exposed to room temperature after foaming due to the high flexural modulus, making it easier to obtain foamed particles of high magnification. In addition, it is desirable because the high flexural modulus results in excellent moldability. Furthermore, the upper limit of the flexural modulus of the polyamide resin is approximately 3000 MPa.
[0091] The flexural modulus of a polyamide resin can be obtained by measuring the test specimen in accordance with JIS K7171: 2016 after leaving it at a temperature of 23°C and a relative humidity of 50% for 24 hours.
[0092] In this specification, the polyamide resin preferably has a density of 1.05 g / cm³ or higher, and more preferably 1.1 g / cm³ or higher. The density can be measured based on the method described in ISO 1183-3.
[0093] The polyamide resin used in the present invention is preferably a terminal-blocked polyamide resin in which the functional groups at the ends of the molecular chains are blocked. This allows for more reliable suppression of hydrolysis during the manufacturing process of the polyamide resin foam particles and makes it easier to obtain polyamide resin foam particles capable of withstanding in-mold molding.
[0094] Furthermore, the durability of the polyamide-based resin foamed particle molded body (hereinafter also referred to simply as "foamed particle molded body" or "molded body") obtained by in-mold molding is improved.
[0095] Examples of end-blocking agents for blocking the above molecular chain ends may include carbodiimide compounds, oxazoline compounds, isocyanate compounds, epoxy compounds, etc.
[0096] Among these, carbodiimide compounds are preferred. Specifically, examples include aromatic monocarbodiimides such as bis(dipropylphenyl)carbodiimide (e.g., "Stabaxol 1-LF" from Rhein Chemie), aromatic polycarbodiimides (e.g., "Stabaxol P", "Stabaxol P100", "Stabaxol P400" from Rhein Chemie), and aliphatic polycarbodiimides such as poly(4,4'-dicyclohexylmethanecarbodiimide) (e.g., "Carbodelite LA-1" from Nisshinbo Chemical Co., Ltd.). These terminal clotting agents may be used alone or in combination of two or more types.
[0097] In addition, the amount of terminal blocking agent is preferably 0.1 to 5 parts by mass per 100 parts by mass of polyamide resin, and more preferably 0.3 to 3 parts by mass.
[0098] As such, the polyamide resin used in the present invention is preferably a polyamide resin terminally blocked by one or more terminal blocking agents selected from carbodiimide compounds, epoxy compounds, and isocyanate compounds, and is more preferably a polyamide resin terminally blocked by a carbodiimide compound.
[0099] The polyamide resin foam particles of the present invention are preferably obtained by a method of heating and foaming polyamide resin particles containing moisture as described above, but are preferably manufactured by the methods of Method 1 and Method 2 below.
[0100] Method 1 is a process of obtaining a dispersion by dispersing polyamide-based resin particles in water within a sealed container;
[0101] A process of impregnating the polyamide-based resin particles in the above dispersion with a foaming agent;
[0102] A process of maintaining the above dispersion at a temperature lower than the melting point of the polyamide resin; and
[0103] The method comprises a process of setting the temperature of the dispersion immediately before foaming to a temperature lower than the melting point of the polyamide resin, and foaming the polyamide resin particles containing a foaming agent by releasing them from a sealed container together with water under a pressure lower than the pressure inside the sealed container.
[0104] Method 2 is a process of obtaining water-containing resin particles by absorbing moisture into polyamide-based resin particles;
[0105] A process of impregnating the water-containing resin particles with a foaming agent within a sealed container; and
[0106] The method includes a process of heating and foaming water-containing resin particles containing a foaming agent.
[0107] Each method is explained below.
[0108] (Method for manufacturing foamed polyamide resin particles (Method 1))
[0109] Method 1 is a process of obtaining a dispersion by dispersing polyamide-based resin particles in water within a sealed container;
[0110] A process of impregnating the polyamide-based resin particles in the above dispersion with a foaming agent;
[0111] A process of maintaining the above dispersion at a temperature lower than the melting point of the polyamide resin; and
[0112] The method includes a process of foaming polyamide-based resin particles impregnated with a foaming agent.
[0113] Each process is explained below.
[0114] [Process for obtaining a dispersion]
[0115] The process for obtaining a dispersion is a process of dispersing polyamide-based resin particles in water within a sealed container to obtain a dispersion.
[0116] The method for dispersing polyamide resin particles in water is not particularly limited, and known methods may be used. For example, a dispersion can be obtained by adding polyamide resin particles to water while stirring with a stirrer and stirring further.
[0117] In addition, if necessary, it is desirable to add to the dispersion a dispersant such as inorganic materials such as aluminum oxide, tricalcium phosphate, magnesium pyrophosphate, zinc oxide, kaolin, mica, talc, and smectite, and a dispersion aid such as anionic surfactants such as sodium dodecylbenzenesulfonate and sodium alkanesulfonate. The mass ratio of polyamide resin particles to the dispersant (resin particles / dispersant) is preferably 20 to 2000, and more preferably 30 to 1000. In addition, the mass ratio of the dispersant to the dispersion aid (dispersant / dispersion aid) is preferably 1 to 500, and more preferably 1 to 100.
[0118] [Process of impregnating with foaming agent]
[0119] The process of impregnating with a foaming agent involves impregnating the foaming agent into polyamide resin particles within a dispersion. In this process, moisture may be absorbed into the polyamide resin particles in addition to impregnating with the foaming agent. Although the method of impregnating the polyamide resin particles with the foaming agent is not particularly limited, it is preferable to disperse the polyamide resin particles in water within a pressurized sealed container, such as an autoclave, and then impregnate the polyamide resin particles with the foaming agent. Furthermore, from the perspective of sufficiently impregnating the polyamide resin particles with the foaming agent in a short period of time, it is preferable to impregnate the polyamide resin particles with the foaming agent by heating in addition to applying pressure.
[0120] The temperature of the impregnation performed under heating is preferably 50°C or higher, more preferably 80°C or higher, from the perspective of sufficiently impregnating the foaming agent into the polyamide resin particles in a short time, and preferably below the melting point (Tm(°C)) of the polyamide resin particles, more preferably below (Tm-20(°C)).
[0121] In addition, regarding the pressure during impregnation performed under pressure (hereinafter also referred to as impregnation pressure), it is preferable to have the pressure inside the sealed container become 1.5 MPa (G) or higher by adding the foaming agent to the container containing the dispersion liquid, with the view that the foaming agent is sufficiently impregnated into the polyamide resin particles in a short time. It is more preferable to have the pressure become 2.5 MPa (G) or higher, and it is preferable to have it become 7.0 MPa (G) or lower, and more preferable to have it become 5.0 MPa (G) or lower.
[0122] Also, “1.5MPa(G)” means that the gauge pressure is 1.5MPa.
[0123] The period from the process of dispersing polyamide resin particles in water to obtain a dispersion, up to the maintenance process, also serves to allow the polyamide resin particles to absorb moisture.
[0124] From the perspective of sufficiently absorbing polyamide resin particles, the heating rate is preferably 10°C / min or less, and more preferably 7°C / min or less. Meanwhile, from the perspective of productivity of polyamide resin foam particles, the heating rate is preferably 1°C / min or more, and more preferably 2°C / min or more.
[0125] (blowing agent)
[0126] Physical blowing agents may be used as blowing agents. Examples of organic physical blowing agents include aliphatic hydrocarbons such as propane, butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; chlorofluoromethane, trifluoromethane, 1,1-difluoroethane, 1,1,1,2-tetrafluoroethane; halogenated hydrocarbons such as methyl chloride, ethyl chloride, and methylene chloride; and dialkyl ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether. In addition, examples of inorganic physical blowing agents include carbon dioxide, nitrogen, helium, argon, and air.
[0127] Among physical blowing agents, inorganic physical blowing agents are preferred from the perspective of having minimal environmental impact, being non-flammable, and having excellent safety, carbon dioxide or nitrogen are more preferred, and carbon dioxide is even more preferred.
[0128] [Maintaining Process]
[0129] The holding process is a process of holding the dispersion at a temperature lower than the melting point of the polyamide resin. The holding process is a process of heating the polyamide resin particles to a state containing moisture.
[0130] In the holding process, the holding temperature of the dispersion is preferably at least 90°C lower than the melting point (Tm) of the polyamide resin (Tm-90°C) from the perspective of increasing the crystallite size, more preferably at least 80°C lower (Tm-80°C), even more preferably at least 70°C lower (Tm-70°C), and even more preferably at least 65°C lower (Tm-65°C). In addition, in the holding process, the holding temperature of the dispersion is preferably less than 50°C lower than the melting point (Tm) of the polyamide resin (Tm-50°C), more preferably at least 55°C lower (Tm-55°C), even more preferably at least 57°C lower (Tm-57°C), and even more preferably at least 59°C lower (Tm-59°C).
[0131] It is believed that this is because it became possible to manufacture foamed particles with a desired crystallite size by plasticizing the polyamide resin particles with water used as a dispersion medium and maintaining them at a specific temperature range.
[0132] In the holding process, the holding time is preferably 5 minutes or more, more preferably 10 minutes or more, and even more preferably 20 minutes or more, from the perspective of making it easier to grow crystallites within a specific range. Additionally, the holding time in the holding process is preferably 60 minutes or less, and more preferably 40 minutes or less. By holding for the above time, it becomes possible to obtain polyamide-based resin foam particles with large crystallite sizes. Furthermore, it is easy to obtain foam particles with low apparent density and a high closed-cell ratio. The holding process may be set in multiple stages within the above temperature range, or it is also possible to raise the temperature slowly by requiring a sufficient amount of time within the above temperature range. From the perspective of making it easier to grow crystallites, it is preferable to set it to a single stage (constant holding temperature) within the above temperature range and hold for the above time.
[0133] The maintaining process is preferably carried out under pressure from the perspective of sufficiently absorbing moisture into the polyamide resin and uniformly impregnating the foaming agent into the polyamide resin, and it is preferable to maintain a pressure equal to the impregnation pressure. It is preferable that the pressure inside the container containing the dispersion be 1.5 MPa (G) or higher, and more preferable that it be 2.5 MPa (G) or higher. In addition, it is preferable that the pressure inside the container containing the dispersion be 7.0 MPa (G) or lower, and more preferable that it be 5.0 MPa (G) or lower.
[0134] [Foaming process]
[0135] The foaming process is a process of foaming polyamide-based resin particles impregnated with a foaming agent.
[0136] The method of foaming polyamide resin particles is not particularly limited, but a foaming method is preferred in which, following the above-mentioned holding process, polyamide resin particles impregnated with a foaming agent are released together with water under a pressure atmosphere lower than the pressure inside a sealed container (usually under atmospheric pressure) to foam them.
[0137] The temperature (Te) of the dispersion immediately before foaming (hereinafter also referred to as the foaming temperature) is preferably a temperature 90°C lower than the melting point (Tm) of the polyamide resin (Tm-90°C) or higher, more preferably a temperature 80°C lower than the melting point (Tm) of the polyamide resin (Tm-80°C) or higher, even more preferably a temperature 70°C lower than the melting point (Tm-70°C) or higher, and even more preferably a temperature 65°C lower than the melting point (Tm) of the polyamide resin (Tm-65°C) or higher. In addition, the foaming temperature is preferably less than a temperature 50°C lower than the melting point (Tm) of the polyamide resin (Tm-50°C), more preferably 55°C lower than the melting point (Tm) of the polyamide resin (Tm-55°C) or lower, even more preferably 57°C lower than the melting point (Tm-57°C) or lower, and even more preferably 59°C lower than the melting point (Tm-59°C) or lower.
[0138] In the foaming process, the pressure immediately before release (foaming pressure) is preferably 0.5 MPa (G) or higher, more preferably 1.5 MPa (G) or higher, and even more preferably 2.5 MPa (G) or higher. In addition, the foaming pressure is preferably 10.0 MPa (G) or lower, more preferably 7.0 MPa (G) or lower, and even more preferably 5.0 MPa (G) or lower.
[0139] In addition, during the foaming process, when releasing polyamide resin particles impregnated with a foaming agent together with water under a pressure lower than the pressure inside the sealed container, it is desirable to maintain a high ambient temperature during release.
[0140] That is, in the manufacturing method of Method 1, as a foaming process, the temperature of the dispersion immediately before foaming is set to a temperature lower than the melting point of the polyamide resin, and it is preferable to maintain a high ambient temperature when foaming polyamide resin particles containing a foaming agent by releasing them together with water from a sealed container under a pressure lower than the pressure inside the sealed container. Here, the ambient temperature refers to the temperature of the atmosphere that the dispersion comes into contact with immediately after releasing the dispersion from the sealed container. As a method for maintaining a high ambient temperature, it is preferable to raise the ambient temperature using steam, but it is also acceptable to raise the ambient temperature using high-temperature air. By maintaining a high ambient temperature during release, the growth of crystallites of the resin particles can be promoted, and the resulting polyamide resin foam particles can be foam particles with larger crystallite sizes. The ambient temperature is preferably 80 to 120°C. In addition, the pressure is preferably 0.05 to 0.3 MPa (G).
[0141] (Method for manufacturing foamed polyamide resin particles (Method 2))
[0142] Method 2 is a process of obtaining water-containing resin particles by absorbing moisture into polyamide-based resin particles;
[0143] A process of impregnating resin particles with a foaming agent within a sealed container; and
[0144] The method includes a process of heating and foaming water-containing resin particles containing a foaming agent.
[0145] Each process is described below. Furthermore, the order of the process for obtaining water-containing resin particles and the process for impregnating the resin particles with a foaming agent is not particularly limited. The process of impregnating the resin particles with a foaming agent may be performed after the process of obtaining water-containing resin particles, the process of obtaining water-containing resin particles may be performed after the process of impregnating the resin particles with a foaming agent, or the process of obtaining water-containing resin particles and the process of impregnating the resin particles with a foaming agent may be performed simultaneously.
[0146] [Process for obtaining water-containing resin particles]
[0147] The process of obtaining water-containing resin particles is a process of absorbing moisture into polyamide-based resin particles.
[0148] One method for absorbing moisture into polyamide resin particles is to immerse the polyamide resin particles in water.
[0149] The immersion conditions are not specifically limited as long as the polyamide resin particles sufficiently absorb moisture, but for example, it is preferable to place polyamide resin particles and an amount of water sufficient to completely immerse the polyamide resin particles into a container and perform the process at the following temperature and time.
[0150] The temperature during immersion is preferably 10°C or higher, more preferably 15°C or higher, from the perspective of sufficiently impregnating water into the polyamide resin particles in a short time, and preferably 100°C or lower, more preferably 80°C or lower.
[0151] The immersion time is preferably 20 minutes or more, and more preferably 40 minutes or more. From the perspective of shortening the manufacturing time, the upper limit of the immersion time is approximately 24 hours. In addition, the process of obtaining water-containing resin particles may be carried out under pressure.
[0152] [Process of impregnating with foaming agent]
[0153] In the process of impregnating the polyamide resin particles with a foaming agent, the method of impregnating the polyamide resin particles with the foaming agent is not particularly limited, but it is preferable to place the polyamide resin particles in a pressurizable sealed container, such as an autoclave, and impregnate the polyamide resin particles with the foaming agent. In addition, when transferring the water-containing resin particles from the container (container 1) of the process of obtaining the water-containing resin particles to the container (container 2) of the process of impregnating the foaming agent, the water-containing resin particles can be removed from container 1 and introduced into container 2 without removing the moisture on the surface of the resin particles.
[0154] The temperature during impregnation is preferably 0°C or higher, more preferably 5°C or higher, from the perspective of sufficiently impregnating the foaming agent into the polyamide resin particles in a short time. It is preferably 80°C or lower, more preferably 60°C or lower, from the perspective of suppressing mutual adhesion between water-containing resin particles.
[0155] In addition, regarding the pressure during impregnation under pressure (impregnation pressure), it is preferable to have the pressure inside the pressure vessel become 1.5 MPa (G) or higher by adding the foaming agent to the pressure vessel containing the particles, with the view that the foaming agent is sufficiently impregnated into the polyamide resin particles in a short time. It is more preferable to have the pressure become 2.5 MPa (G) or higher, and it is preferable to have it become 7.0 MPa (G) or lower, and more preferable to have it become 5.0 MPa (G) or lower.
[0156] The total time of the process for impregnating with a foaming agent is preferably 30 minutes or more, and more preferably 60 minutes or more. Meanwhile, from the perspective of the productivity of the polyamide resin foam particles, the above time is preferably 300 minutes or less, and more preferably 240 minutes or less.
[0157] By applying a foaming agent and then gradually lowering the pressure to atmospheric pressure, it is possible to form water-containing resin particles containing the foaming agent.
[0158] [Foaming process]
[0159] The foaming process is a process of heating water-containing resin particles containing a foaming agent to foam polyamide-based resin particles impregnated with the foaming agent. The foaming process is a process of heating the polyamide-based resin particles to a state containing moisture.
[0160] The method of foaming polyamide-based resin particles is not particularly limited, but it is preferable to foam water-containing polyamide-based resin particles impregnated with a foaming agent by heating them with a heat medium such as steam, high-temperature air, or oil, for example.
[0161] [Polyamide resin foamed particle molded body]
[0162] A polyamide-based resin foamed particle molded body (foamed molded body) can be obtained by molding the polyamide-based resin foamed particles of the present invention. That is, the foamed molded body obtained here is formed by molding the polyamide-based resin foamed particles of the present invention.
[0163] While conventional methods known for in-mold molding can be employed, it is preferable to use heating with steam. Since the polyamide resin within the foamed particles is plasticized by water absorption due to the steam, it becomes possible to lower the molding steam pressure. Furthermore, when the obtained molded body is dried, it returns to the original physical properties of the polyamide resin, resulting in a molded body with high heat resistance.
[0164] Since the polyamide-based resin foam particles of the present invention have large crystallite growth, they exhibit excellent moldability and can be formed into a good foamed particle molded body. Furthermore, because the foam particles also possess excellent heat resistance, a molded body that is lightweight and has excellent heat resistance can be obtained. Specifically, excellent moldability means that when molding to obtain a molded body, the surface properties are excellent, and the fusion and recovery properties are also excellent, resulting in a wide moldable pressure range. Additionally, because the polyamide-based resin foam particles of the present invention exhibit excellent moldability, a good molded body can be obtained even if the thickness is thick. A thick molded body is, for example, preferably 30 mm or more, more preferably 40 mm or more, and even more preferably 50 mm or more. That is, the thickness of the polyamide-based resin foamed particle molded body of the present invention is preferably 30 mm or more, more preferably 40 mm or more, and even more preferably 50 mm or more.
[0165] The density of the molded polyamide resin foamed particle molded article of the present invention is preferably 20 kg / m³ or more, more preferably 40 kg / m³ or more, and even more preferably 50 kg / m³ or more. In addition, the density of the molded article is preferably 300 kg / m³ or less, more preferably 250 kg / m³ or less, even more preferably 200 kg / m³ or less, and even more preferably 150 kg / m³ or less.
[0166] If the density of the molded body is within the above range, the balance between lightness and strength of the molded body is excellent.
[0167] In addition, the density of the molded body is measured by the following method.
[0168] First, a molded foam particle body that has been left for more than 24 hours in an environment with a temperature of 23℃ and a relative humidity of 50% is cut into rectangular samples of appropriate size (the molding skin is removed). Then, the apparent volume of each sample is determined from the external dimensions of each sample, and the sum of these is taken as the apparent volume (H) of the sample. In addition, the density [kg / ㎥] of the molded body is obtained by dividing the total weight (W) of each sample by the aforementioned apparent volume (H).
[0169] The closed-cell ratio of the polyamide resin foamed particle molded article of this specification is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. If the closed-cell ratio of the foamed particle molded article satisfies the above range, it is easy to obtain a foamed particle molded article with low apparent density. In addition, the closed-cell ratio of the foamed particle molded article refers to the ratio of the volume of closed cells to the volume of cells (the sum of the volume of closed cells and the volume of continuous cells) contained in the foamed particles constituting the foamed particle molded article, and can be obtained using an air-comparison specific gravity meter, etc., in accordance with procedure C described in ASTM-D2856-70.
[0170] In this way, by using polyamide resin foam particles with large crystallite sizes, a molded body with low apparent density and high closed-cell ratio can be obtained.
[0171] Examples
[0172] The present invention will be described in detail below by way of examples, but the present invention is not limited thereto.
[0173] Various physical properties of the polyamide resin and polyamide resin particles in each manufacturing example were measured by the following method.
[0174] [Measurement of Physical Properties of Polyamide Resins and Polyamide Resin Particles]
[0175] [Melting Point (Tm)]
[0176] Based on JIS K7121-1987, the melting point of polyamide resin particles was measured by differential scanning calorimetry (DSC) based on the heat flow rate. Under conditions of a nitrogen inflow rate of 30 mL / min, the sample was heated from 30°C to a temperature 30°C higher than the end of the melting peak (first heating step) at a heating rate of 10°C / min. Next, the sample was maintained at that temperature for 10 minutes, cooled to 30°C at a cooling rate of 10°C / min, and then heated again at a heating rate of 10°C / min to a temperature 30°C higher than the end of the melting peak. The peak temperature of the melting peak of the second DSC curve obtained was determined as the melting point (Tm). Additionally, a high-sensitivity differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII Nanotechnologies) was used as the measuring device. Furthermore, for the measurement of the DSC curve, polyamide resin particles that had been left standing for more than 24 hours in an environment of 23°C and 50% relative humidity were used.
[0177] 〔density〕
[0178] It is a catalog value obtained based on the method described in ISO 1183-3.
[0179] [Bending Modulus]
[0180] The bending modulus of the polyamide resin was determined by measuring in accordance with JIS K7171: 2016. A resin test specimen with a thickness of 4 mm, a width of 10 mm, and a length of 80 mm was prepared, and the specimen was left to stand for 72 hours at a room temperature of 23°C and a relative humidity of 50%. Afterward, the average value of the values (5 points) calculated by measuring with an Autograph AGS-10kNG (manufactured by Shimadzu Corporation) under conditions of a distance between points of 64 mm, a radius of the indenter of 15.0 mm, a radius of the support of 25.0 mm, a test speed of 2 mm / min, a room temperature of 23°C, and a relative humidity of 50% was adopted as the bending modulus.
[0181] In addition, the bending modulus of an amide-based elastomer (Arkema product, product name "PEBAX5533", melting point 159°C, density 1.01 g / cm³) was measured based on the above method and was 150 MPa.
[0182] [Manufacture of Polyamide Resin Particles]
[0183] Preparation Example 1
[0184] A polyamide resin (5033B, details shown in Table 1) was supplied to an extruder, and 0.8000 parts by mass of "Talcum Powder PK-S" (manufactured by Kasei Hayashi Co., Ltd.) was added as a foaming agent per 100 parts by mass of the polyamide resin. Additionally, an aromatic polycarbodiimide (Stabaxol P, manufactured by Rhein Chemie) was supplied as a terminal blocking agent at a ratio of 1 part by mass per 100 parts by mass of the polyamide resin, and the mixture was melt-kneaded. The melt-kneaded mixture was extruded in the shape of a strand with a circular cross-section through the pores of a cover mounted on the end of the extruder, and the extruded strand was water-cooled. Subsequently, the mixture was cut using a pelletizer to obtain polyamide resin particles with an average mass of 2 mg and dried.
[0185] Preparation Example 2
[0186] Polyamide resin particles were obtained in the same manner as in Preparation Example 1, except that the polyamide resin was changed from 5033B to 1030B (details are shown in Table 1).
[0187] Preparation Example 3
[0188] Polyamide resin particles were obtained as in Preparation Example 1, except that the polyamide resin was changed from 5033B to E2046 (details are shown in Table 1) and the terminal blocking agent was changed from Stabaxol P to aromatic polycarbodiimide (Stabaxol P100, manufactured by Rhein Chemie).
[0189] Preparation Example 4
[0190] Polyamide resin particles were obtained as in Preparation Example 1, except that a terminal blocking agent (Stabaxol P) was not used.
[0191]
[0192] Various physical properties of the polyamide resin foam particles in each example and comparative example were measured by the following method.
[0193] [Measurement of Physical Properties of Polyamide Resin Foam Particles]
[0194] Various physical properties of the polyamide resin foam particles, other than the moisture content, were measured after performing the following condition control. First, the obtained polyamide resin foam particles were placed in an environment at a temperature of 60°C for 24 hours, and then slowly cooled to room temperature (23°C). Next, the condition was controlled by leaving the particles in an environment at a temperature of 23°C, relative humidity of 50%, and 1 atm for 24 hours.
[0195] [Moisture Content]
[0196] Polyamide resin foam particles immediately after foaming were randomly selected, and moisture on the surface of the foam particles was wiped off with a dry cloth, after which about 0.2g of the foam particles were weighed. Next, the moisture inside the foam particles was vaporized by heating the foam particles to 160°C using a heating moisture vaporization device, and the moisture content was measured by Karl Fischer titration (total titration method) using a Karl Fischer moisture measuring device (AQ-2200A, manufactured by Hiranuma Industrial Co., Ltd.).
[0197] [Determinant Size]
[0198] The crystallite size of the polyamide resin foam particles was determined by the following method. X-ray diffraction (XRD) measurements of the obtained polyamide resin foam particles were performed by the reflection method using the X-ray scattering device “SmartLab SE” (manufactured by Rigaku Co., Ltd.). The semiconductor 1D detector D / teX Ultra 250 was used as the detector. For the sample, a test specimen was used in which randomly selected foam particles were packed as densely as possible into a 24 mm diameter sample holder without overlapping. Empty cell scattering correction was also performed. Using software (product name: SmartLab Studio II), the 1D X-ray diffraction profile obtained in this way was assumed to have a Gaussian function as the peak shape, and peak separation was performed into crystalline diffraction peaks and amorphous diffraction peaks. The full width at half maximum (β(rad)) of the peak having the narrowest peak width among the peaks obtained by peak separation was calculated, and the crystallite size (D) of the foam particles was calculated according to the following equation (2) using this full width at half maximum (β). The above measurements were performed on 10 test specimens, and their arithmetic mean value was taken as the crystallite size of the foam particles.
[0199]
[0200] [Total heat of fusion of the DSC curve of the first heating]
[0201] A high-sensitivity differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII Nanotechnologies) was used for the measurement.
[0202] A polyamide resin foam particle was used as a test specimen, and a DSC curve of the first heating was obtained by heating from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min by differential scanning calorimetry based on JIS K7122-1987.
[0203] A straight line was drawn connecting the point at 150°C on the obtained DSC curve and the point at the end of the melting peak on the DSC curve, and this straight line was used as the baseline. The heat amount calculated from the area of the portion enclosed by the baseline and the DSC curve located on the endothermic side of the baseline was taken as the total melting heat amount of the DSC curve for the first heating.
[0204] [Peak temperature of the melting peak of the DSC curve of the second heating]
[0205] A high-sensitivity differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII Nanotechnologies) was used for the measurement.
[0206] Polyamide resin foam particles were used as test specimens, and based on JIS K7121-1987, by differential scanning calorimetry of heat flow rate, they were heated from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min and maintained at that temperature for 10 minutes.
[0207] After that, the temperature was cooled to 30°C at a cooling rate of 10°C / min and then heated again from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min to obtain the DSC curve of the second heating.
[0208] The peak temperature of the maximum melting peak (endothermic peak) appearing on the DSC curve in the obtained DSC curve was set as the peak temperature of the melting peak of the DSC curve of the second heating.
[0209] [Apparent Density of Polyamide Resin Foam Particles]
[0210] A graduated cylinder containing water at a temperature of 23°C was prepared, and the mass (W1) of expanded particles with a volume of approximately 500 cm³ was measured and settled using a wire mesh. The volume (V1 [cm³]) of the expanded particles read from the rise in water level, taking into account the volume of the wire mesh, was measured, and the mass (W1 [g]) of the expanded particles was divided by the volume (V1) (W1 / V1) and the unit was converted to [kg / m³] to obtain the apparent density of the expanded particles.
[0211] [Average bubble size]
[0212] First, the foam particle was divided into approximately two sections passing through the center of the foam particle, and the cross-section was photographed using a scanning electron microscope. Next, from the obtained cross-sectional photographs, straight lines were drawn at equal intervals in eight directions from near the center of the cross-section of the foam particle to the surface of the foam particle, changing the angle by 45°, and the number of bubbles intersecting these lines was counted. The value obtained by dividing the sum of the lengths of these lines by the counted number of bubbles was taken as the bubble diameter of the foam particle. This operation was performed in the same way for 30 foam particles, and the arithmetic mean value of the bubble diameters of each foam particle was taken as the average bubble diameter of the foam particle.
[0213] [Surface film thickness]
[0214] The length (thickness of the outermost surface layer) from the outermost surface of the foamed particle to the outermost bubble of the foamed particle was measured along the eight straight line segments of the above average bubble diameter, and the average thickness of the outermost surface layer of each foamed particle was obtained by arithmetically averaging these values. Then, the average surface film thickness of the foamed particle was obtained by arithmetically averaging the values of 30 foamed particles.
[0215] [Independent cell ratio of polyamide resin foam particles]
[0216] The value (Vx) of the true volume of the foamed particles (the sum of the volume of the resin constituting the foamed particles and the volume of the independent bubble portions within the foamed particles) was measured in accordance with procedure C of ASTM-D2856-70. Toshiba-Beckmann Inc.'s air-comparison hydrometer "930" was used to measure this true volume (Vx). Next, the independent bubble ratio was calculated using the following equation (1), and the arithmetic mean of the results of five measurements was obtained.
[0217] Independent bubble ratio (%) = (Vx - W / ρ) × 100 / (Va - W / ρ) … (1)
[0218] Vx: Real volume (cm³) of the foamed particles measured by the above method
[0219] Va: Apparent volume of foam particles (cm³)
[0220] W: Mass (g) of the sample for measuring foam particles
[0221] ρ: Density of the resin constituting the foam particles (g / cm³)
[0222] [Evaluation of Polyamide Resin Foam Particles]
[0223] [Heat resistance evaluation (ratio of 5% compressive stress at a temperature 20°C lower than the melting point (Tm1-20°C) to 5% compressive stress at 23°C of polyamide resin foam particles)]
[0224] The foamed particles were measured in compression mode (diameter of the tip of the compression probe: 3.5 mm) using a thermal analyzer (TMA; "TMA7100" manufactured by Hitachi High-Tech Science Corp.). Specifically, one foamed particle was randomly selected, and a load of 10 mN was applied to the short diameter direction of the foamed particle using a compression probe, and the temperature was set to a predetermined level. Subsequently, while maintaining an isothermal position at this temperature, the particle was pushed in at a speed of 1 mm / min, and the load of the probe was monitored. The stress was recorded at the point when the thickness of the foamed particle reached 5% of the thickness of the foamed particle before compression. The above operation was performed three times, and the arithmetic mean value was taken as the 5% compression stress.
[0225] The above predetermined temperatures are 20°C lower than the melting point of the polyamide resin foam particles used in the polyamide resin foam particle molded body as described in Table 2 (Tm1-20°C) and 23°C.
[0226] Furthermore, using the measurement values obtained by the above measurement, the ratio of the 5% compressive stress at a temperature 20°C lower than the melting point (Tm1-20°C) to the 5% compressive stress at 23°C of the polyamide resin foam particles [(Tm1-20°C compressive stress) / (23°C compressive stress)] was calculated. The above operation was performed on three foam particles, and their arithmetic mean values were set as the ratio of the 5% compressive stress at a temperature 20°C lower than the melting point (Tm1-20°C) to the 5% compressive stress at 23°C of the polyamide resin foam particles [(Tm1-20°C compressive stress) / (23°C compressive stress)].
[0227] The higher the value of the above ratio, the better the heat resistance. These heat-resistant polyamide resin foam particles are suitable for applications requiring heat resistance, such as manufacturing composites by mixing or laminating them with uncured thermosetting resins to cure the thermosetting resins.
[0228] [Manufacture of Polyamide Resin Foam Particles]
[0229] Example 1
[0230] 1 kg of polyamide-based resin particles obtained in Preparation Example 1 and 3 liters of water as a dispersion medium were placed in a 5-liter autoclave equipped with a stirrer. Additionally, 0.3 parts by mass of kaolin as a dispersant and 0.004 parts by mass of sodium alkylbenzenesulfonate as a surfactant were added to the dispersion solution for every 100 parts by mass of polyamide-based resin particles. While stirring the contents in the autoclave, carbon dioxide as a foaming agent was injected into the autoclave from room temperature (23°C) until it reached 136°C (impregnation temperature), and the pressure inside the autoclave reached 4.0 MPa (G) (impregnation pressure). At this time, the heating time from room temperature (23°C) to reach the impregnation temperature was 40 minutes. Next, the temperature was maintained at 136°C (holding temperature) and 4 MPa (G) (holding pressure) for 30 minutes.
[0231] Thereafter, polyamide resin particles impregnated with a foaming agent were released together with a dispersion under atmospheric pressure (0.1 MPa). The foaming temperature (temperature of the dispersion immediately before foaming (Te)) was 136°C. The obtained polyamide resin foam particles were cured in an oven at 60°C for 24 hours, and then slowly cooled to obtain polyamide resin foam particles.
[0232] The physical properties of the obtained polyamide resin foam particles are shown in Table 2. In addition, the moisture content of the polyamide resin foam particles immediately after foaming in Example 1 was measured to be 18%. The moisture content of the polyamide resin foam particles is higher than the saturated absorption rate of the polyamide resin. This is thought to be because the polyamide resin foam particles are in a supersaturated absorption state, resulting in a value higher than the saturated absorption rate of the polyamide resin. Furthermore, although it is difficult to measure the moisture content of the polyamide resin foam particles inside an autoclave, it is thought to be at least higher than the moisture content of the polyamide resin foam particles immediately after foaming.
[0233] Example 2
[0234] Polyamide resin foam particles were obtained by the same method as in Example 1, except that polyamide resin particles obtained in Preparation Example 2 were used, and the impregnation temperature, holding temperature, and foaming temperature were set to 158°C.
[0235] Example 3
[0236] Polyamide resin foam particles were obtained by the same method as in Example 1, except that polyamide resin particles obtained in Preparation Example 3 were used, and the impregnation temperature, holding temperature, and foaming temperature were set to 175.5℃.
[0237] Example 4
[0238] Polyamide resin foam particles were obtained by the same method as in Example 1, except that polyamide resin particles obtained in Preparation Example 4 were used.
[0239] Example 5
[0240] In this embodiment, the polyamide resin particles impregnated with a foaming agent were released into atmospheric pressure while supplying steam at a pressure of 0.1 MPa (G) to the outlet of the valve when releasing them from the autoclave into atmospheric pressure, as in Example 1. In addition, the atmosphere temperature of the dispersion in the part where the steam contacts the dispersion containing the polyamide resin particles and water was 100°C.
[0241] Example 6
[0242] 3 kg of polyamide resin particles obtained in Preparation Example 1 were completely immersed in 6 liters of water and left to stand for 1 hour.
[0243] Next, the resin particles extracted from water were placed into an autoclave, and carbon dioxide was injected into the autoclave as a foaming agent until the pressure inside the autoclave reached 4 MPa (G) (impregnation pressure). Next, the temperature was maintained at 10°C (impregnation temperature) and 4 MPa (G) for 3 hours.
[0244] Subsequently, the polyamide resin particles impregnated with a foaming agent were removed from the autoclave and transferred to a foaming container filled with an oil medium heated to the temperature (foaming temperature) shown in Table 2. Foaming was then performed by immersing the polyamide resin particles impregnated with the foaming agent. The surface of the obtained polyamide resin foam particles was cleaned with normal hexane to remove the oil. Afterward, the polyamide resin foam particles were cured in an oven at 60°C for 24 hours, and then slowly cooled to obtain the polyamide resin foam particles.
[0245] The physical properties of the obtained polyamide resin foam particles are shown in Table 2. In addition, the moisture content of the polyamide resin particles immediately before foaming was measured to be 6.2%.
[0246] Example 7
[0247] In this embodiment, polyamide resin foam particles were obtained by the same method as in Example 1, except that the holding temperature was changed to 139°C and the foaming temperature to 135°C.
[0248] Comparative Example 1
[0249] 3 kg of polyamide resin particles obtained in Preparation Example 1 were placed in an autoclave, and carbon dioxide was injected into the autoclave as a blowing agent until the pressure inside the autoclave reached 4 MPa (G) (impregnation pressure). Next, the temperature was maintained at 10°C (impregnation temperature) and 4 MPa (G) for 3 hours.
[0250] Afterwards, polyamide resin particles impregnated with a foaming agent were transferred to a foaming device, and air at the temperature (foaming temperature) shown in Table 2 was blown in for 20 seconds to obtain polyamide resin foam particles. The obtained polyamide resin foam particles were cured in an oven at 60°C for 24 hours, and then slowly cooled to obtain polyamide resin foam particles.
[0251] The physical properties of the obtained polyamide resin foam particles are shown in Table 2. In addition, the moisture content of the polyamide resin particles immediately before foaming was measured to be 3.0%.
[0252] [Evaluation of Moldability of Polyamide Resin Foamed Particles and Molded Polyamide Resin Foamed Particles]
[0253] The moldability of the polyamide-based resin foam particles in each example and comparative example was evaluated by the following method, and the various physical properties of the obtained molded body were measured by the following method.
[0254] [Manufacture of Polyamide Resin Foamed Particle Molded Articles]
[0255] First, the polyamide-based resin foam particles obtained in Examples 1 to 7 and Comparative Example 1 were filled into a flat molding mold measuring 300 mm in length × 300 mm in width × 50 mm in thickness, and molding was performed by steam heating to obtain a plate-shaped foam particle molded body. The heating method involved preheating (exhaust process) by supplying steam for 5 seconds with the drain valves of the mold on both sides open, followed by heating one side at a pressure 0.04 MPa (G) lower than the molding steam pressure shown in Table 2, and then heating one side from the opposite direction at a pressure 0.02 MPa (G) lower than the molding steam pressure shown in Table 2, followed by main heating from both sides at the molding steam pressure shown in Table 2. After heating was finished, the pressure was released and water-cooled until the surface pressure due to the foaming force of the molded body dropped to 0.02 MPa (gauge pressure), after which the mold was opened and the molded body was removed from the mold. The obtained molded body was cured in an oven at 80°C for 12 hours and then slowly cooled to room temperature. In this way, a polyamide foamed particle molded body was obtained. The moldability of the foamed particles was evaluated for the molded body at each molding steam pressure, and the physical properties of the molded body were also measured. The results are shown in Table 2.
[0256] [Evaluation of Moldability of Polyamide Resin Foam Particles]
[0257] The moldability of the polyamide resin foamed particles was evaluated by measuring the recovery, surface properties, and fusion properties of the polyamide resin foamed particle molded body obtained by the above manufacturing method. The evaluation method is shown below.
[0258] (Recovery of foamed particle molded body)
[0259] The thickness of the end (10 mm inward from the end) and the center (the part dividing in both the vertical and horizontal directions) of the foamed particle molded body corresponding to the dimensions of the flat plate mold used in mold molding was measured. Next, the thickness ratio of the foamed particle molded body (thickness of the center of the molded body / thickness of the end of the molded body × 100 (%)) was calculated and evaluated as follows. The higher the thickness ratio, the better the recovery and the better the moldability.
[0260] A: Thickness ratio is 95% or higher.
[0261] B: Thickness ratio is less than 95%.
[0262] (Surface properties of foamed particle molded bodies)
[0263] The surface properties of the foamed particle molded body were evaluated as follows. The more the gaps between the foamed particles on the surface of the molded body are filled, the better the surface properties and the better the moldability of the foamed particle molded body.
[0264] A: The gaps between the foam particles on the surface of the molded body are filled.
[0265] B: The gaps between the foam particles on the surface of the molded body are not filled.
[0266] (Fusability of foamed particle molded body)
[0267] The fusion rate of the molded body was determined based on the ratio of the number of material-damaged foam particles among the foam particles exposed on the fracture surface when the molded body of foam particles was fractured. Specifically, first, a test specimen (length 100 mm × width 100 mm × thickness: thickness of the molded body) was cut from the molded body of foam particles, and a cut of about 5 mm was made in the thickness direction of each test specimen using a cutter knife, and then the test specimen was fractured from the cut portion. Next, the number of foam particles (n) present on the fracture surface of the molded body of foam particles and the number of material-damaged foam particles (b) were measured, and the ratio of (b) to (n) (material damage on the fracture surface, b / n) was expressed as a percentage. The higher the value of material damage on the fracture surface, the better the fusion ability of the foam particles and the better the moldability.
[0268] [Measurement of Physical Properties of Polyamide Resin Foamed Particle Molded Body]
[0269] The various physical properties of the polyamide resin foamed particle molded body shown below were measured after the polyamide resin foamed particle molded body, which had been slowly cooled to room temperature, was left standing for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%.
[0270] (Molded body density)
[0271] A sample (length 100 mm × width 100 mm × thickness 30 mm) excluding the skin surface was cut from the foamed particle molded body. Then, the apparent volume of the sample was determined from the external dimensions of the sample and set as the apparent volume (H) of the sample. The density of the molded body [kg / m³] was calculated by dividing the total weight (W) of the sample by the apparent volume (H) (W / H).
[0272] (Independent cell ratio of polyamide resin foamed particle molded body)
[0273] A sample (30 mm in length × 30 mm in width × 30 mm in thickness) excluding the skin surface was cut from the foamed particle molded body, and the value (Vx) of the true volume (the sum of the volume of the resin constituting the foamed particle molded body and the volume of the independent bubble portion within the foamed particle molded body) was measured in accordance with procedure C of ASTM-D2856-70. Toshiba-Beckmann Inc.'s air comparison hydrometer "930" was used to measure this true volume (Vx). Next, the independent bubble ratio was calculated using the following equation (3), and the arithmetic mean of the results of five measurements was obtained.
[0274] Independent bubble ratio (%) = (Vx - W / ρ) × 100 / (Va - W / ρ) … (3)
[0275] Vx: The actual volume (cm³) of the foamed particle molded body measured by the above method
[0276] Va: Apparent volume (cm³) of the foamed particle molded body
[0277] W: Mass (g) of a sample for measuring a foamed particle molded body
[0278] ρ: Density of the resin constituting the foamed particle molded body (g / cm³)
[0279]
[0280] From the results shown in Table 2, it can be seen that the polyamide resin foam particles of the example have excellent moldability. In addition, the polyamide resin foam particles of the example also had excellent heat resistance.
Claims
Claim 1 A polyamide resin foam particle obtained by incorporating a foaming agent into moisture-containing polyamide resin particles and foaming them by heating, wherein the crystallite size measured by X-ray diffraction exceeds 8 nm, the moisture content of the moisture-containing polyamide resin particles immediately after foaming is 3% or higher, which is a value higher than the saturation absorption rate of the polyamide resin, the flexural modulus of the polyamide resin constituting the polyamide resin particles is 1000 MPa or higher, the apparent density of the polyamide resin foam particles is 90 to 300 kg / m³, the surface film thickness of the polyamide resin foam particles is 5 to 50 μm, and the peak temperature of the melting peak of the DSC curve of the second heating obtained under Condition 1 below is 185 to 285°C. Condition 1: Based on the heat flux differential scanning calorimetry method of JIS K7121-1987, a polyamide resin foam particle is used as a test specimen and the heating rate The DSC curve measured when heating from 30°C to a temperature 30°C higher than the end of the melting peak at a rate of 10°C / min, maintaining that temperature for 10 minutes, cooling to 30°C at a rate of 10°C / min, and then heating again to a temperature 30°C higher than the end of the melting peak at a rate of 10°C / min is used as the DSC curve of the second heating. Claim 2 A polyamide resin foam particle according to claim 1, wherein the total heat of melting of the DSC curve measured when the polyamide resin foam particle is used as a test specimen based on the heat flux differential scanning calorimetry method of JIS K7122-1987 and heated from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min is 40 to 140 J / g. Claim 3 Polyamide resin foam particles according to claim 1 or claim 2, wherein the apparent density of the polyamide resin foam particles is 100 to 250 kg / m³. Claim 4 A polyamide resin foam particle according to claim 1 or claim 2, wherein the peak temperature of the melting peak of the DSC curve of the second heating obtained under condition 1 below is 188 to 280°C. Condition 1: A polyamide resin foam particle is used as a test specimen based on the differential scanning calorimetry method of JIS K7121-1987, heated from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min, maintained at that temperature for 10 minutes, cooled to 30°C at a cooling rate of 10°C / min, and then heated again to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min. The DSC curve measured at this time is used as the DSC curve of the second heating. Claim 5 A polyamide resin foam particle according to claim 1 or claim 2, wherein the crystallite size of the polyamide resin foam particle measured by X-ray diffraction is 10 nm or more. Claim 6 The polyamide resin foam particles of claim 1 or claim 2, wherein the closed-cell ratio of the polyamide resin foam particles exceeds 90%. Claim 7 The polyamide resin foam particles of claim 1 or claim 2, wherein the average pore size of the polyamide resin foam particles is 20 to 200 μm. Claim 8 The polyamide resin foam particles of claim 1 or claim 2, wherein the surface film thickness of the polyamide resin foam particles is 10 to 30 μm.
Citation Information
Patent Citations
Polyamide prefoamed beads and foam therefrom and its production
JP1986268737A
Polyamide resin foamed molding
JP2018044127A
Amide elastomer foam particles, method for producing same, foam molded body and method for producing foam molded body
KR1020170036090A
Method for producing foam particles comprising a thermoplastic elastomer having polyamide segments
KR1020190022727A