Method for preparing positive electrode active material for lithium secondary battery and lithium secondary battery comprising the positive electrode active material prepared by using the same
The described method using spray pyrolysis and controlled mixing for cathode active materials in lithium secondary batteries achieves uniform phase formation, enhancing electrochemical performance and structural stability, overcoming the inefficiencies of co-precipitation methods and single-crystal growth issues.
Patent Information
- Application Number
- KR1020250040682
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-03-28
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-03-28
AI Technical Summary
Existing methods for manufacturing cathode active materials for lithium secondary batteries, such as those using co-precipitation precursors, face challenges in achieving uniform phase formation, leading to increased costs and reduced efficiency, while single-crystal active materials suffer from overgrowth and non-uniform growth, compromising electrochemical performance and structural stability.
A method involving spray pyrolysis to prepare transition metal precursors, followed by mixing with lithium raw materials, calcination to form single-particles, and coating with a heat-treatment step to create a positive electrode active material, with specific density and molar ratio controls, ensuring uniform phase and structural stability.
The method results in a positive electrode active material with enhanced electrochemical properties, including improved charge capacity, discharge capacity, and efficiency, along with superior structural stability, addressing the limitations of previous manufacturing methods.
Smart Images

Figure 112025035579932-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present embodiments relate to a method for manufacturing a positive electrode active material for a lithium secondary battery and a lithium secondary battery comprising a positive electrode active material manufactured using the same. Background Technology
[0003] Driven by the recent explosive demand for electric vehicles and the need for increased driving range, the development of high-capacity, high-energy-density secondary batteries to meet these demands is actively underway worldwide.
[0004] As positive electrode active materials for such secondary batteries, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compound (LiFePO4), and lithium nickel cobalt manganese oxide (Li 1+a Ni x Co y Mn z O2) and others are being used. Among these, lithium nickel cobalt manganese oxide, or NCM material, is widely used due to its advantages of high operating voltage and excellent capacitance characteristics.
[0005] In the manufacturing of NCM-based cathode active materials, co-precipitation precursors have been used to ensure that each transition metal forms a uniform phase. In particular, oxide precursors have been utilized after undergoing processes such as precursor roasting to remove large amounts of moisture (H2O) and impurities from the co-precipitation precursors. However, manufacturing cathode active materials using the co-precipitation method involves co-precipitation and roasting processes, which leads to increased manufacturing costs and reduced overall process efficiency.
[0006] To address this, transition metal precursors produced through spray pyrolysis can be utilized; however, there are technical difficulties in controlling their properties to ensure the transition metal forms a uniform phase.
[0007] Therefore, there is a need for a method to manufacture a cathode active material that has excellent electrochemical performance and structural stability, while overcoming the limitations of single-crystal active materials that are inferior due to overgrowth and non-uniform growth. The problem to be solved
[0009] In this embodiment, we aim to provide a method for manufacturing a single-particle cathode active material for a lithium secondary battery that has excellent electrochemical properties and improved structural stability, and a lithium secondary battery comprising the cathode active material manufactured using the same. means of solving the problem
[0011] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment comprises: a step of preparing a transition metal precursor manufactured by spray pyrolysis; a step of mixing the transition metal precursor and a first lithium raw material to prepare a mixture; a step of calcining the mixture to obtain a calcined product in the form of a single particle; and a step of mixing the calcined product, a coating raw material, and a second lithium raw material, and then heat-treating the mixture to obtain a positive electrode active material having a coating layer formed thereon; wherein the tap density of the mixture is 1.465 g / cc or higher.
[0012] The step of preparing a mixture by mixing the above transition metal precursor and the first lithium raw material can satisfy Formula 1 below:
[0013] [Equation 1]
[0014] 1.45 < A / B < 1.63
[0015] (In the above Equation 1,
[0016] A is the tap density (g / cc) of the above mixture, and B represents the molar ratio (Li / Me) of lithium (Li) to the transition metal (Me) excluding lithium (Li) in the above mixture.
[0017] In the above mixture, the molar ratio of lithium (Li) to transition metal (Me) excluding lithium (Li) (Li / Me) may be greater than 0.90 and less than 1.00.
[0018] The first lithium raw material above may be Li2CO3.
[0019] The second lithium raw material may include at least one of LiOH, Li2CO3, LiNO3, LiNO2, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a combination thereof.
[0020] In the step of preparing a mixture by mixing the above transition metal precursor and the first lithium raw material, the average particle size (D50) of the first lithium raw material relative to the transition metal precursor may be 1.0 to 10.0 times.
[0021] The above calcination can be performed for 10 to 14 hours at a temperature of 900 to 960°C in a CO2-free air (CFA) atmosphere.
[0022] The above-mentioned sintered product may have an average crystallite size of 210 to 270 nm.
[0023] The ratio of the c-axis length to the a-axis length (c / a) obtained by X-ray diffraction analysis of the crystal of the above-mentioned sintered product may be 4.9440 to 4.9520.
[0024] The above heat treatment can be performed at a temperature of 730 to 770°C.
[0025] The above positive active material may have a molar ratio (Li / Me) of lithium (Li) to transition metal (Me) excluding lithium (Li) of 1.03 to 1.07.
[0026] The above positive active material can be represented by the following chemical formula 1:
[0027] [Chemical Formula 1]
[0028] Li a Ni x Co y Mn z M1 k O2
[0029] (In the above chemical formula 1,
[0030] 0.9 ≤ a ≤ 1.1, 0.3 ≤ x ≤ 0.73, 0.01 ≤ y ≤ 0.3, 0.01 ≤ z ≤ 0.4,
[0031] 0 ≤ k ≤ 0.2, x + y + z + k = 1, and
[0032] M1 is one or more elements selected from the group consisting of Al, Mg, Zr, Sn, Ca, Ge, Ti, Cr, Fe, Zn, Y, Ba, La, Ce, Sm, Gd, Yb, Sr, Cu, and Ga).
[0033] A lithium secondary battery according to another embodiment may include a positive electrode comprising a positive active material manufactured according to one embodiment; a negative electrode; and a non-aqueous electrolyte. Effects of the invention
[0035] According to the present embodiment, by adding Li in a divided manner during the mixing step and coating step before calcination, it is possible to realize a positive electrode active material for a lithium secondary battery with excellent electrochemical properties, such as charge capacity, discharge capacity, and efficiency, and improved structural stability. Brief explanation of the drawing
[0037] Figure 1 is an SEM image of the positive electrode active material according to Example 1, magnified 10,000 times. Figure 2 is an SEM image of the positive electrode active material according to Example 2, magnified 10,000 times. Figure 3 is an SEM image of the positive electrode active material according to Example 3, magnified 10,000 times. Figure 4 is an SEM image of the positive electrode active material according to Comparative Example 1, magnified 10,000 times. Figure 5 is an SEM image of the positive electrode active material according to Comparative Example 2, magnified 10,000 times. Figure 6 is an SEM image of the positive electrode active material according to Comparative Example 3, magnified 10,000 times. Figure 7 is an SEM image of the positive electrode active material according to Comparative Example 4, magnified 10,000 times. Figure 8 is an SEM image of the positive electrode active material according to Comparative Example 5, magnified 10,000 times. Specific details for implementing the invention
[0038] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used solely to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Accordingly, the first part, component, region, layer, or section described below may be referred to as the second part, component, region, layer, or section without departing from the scope of the present invention.
[0039] The technical terms used herein are for the reference of specific embodiments only and are not intended to limit the invention. The singular forms used herein include plural forms unless phrases clearly indicate otherwise. As used in the specification, the meaning of "comprising" specifies certain characteristics, areas, integers, steps, actions, elements, and / or components, and does not exclude the presence or addition of other characteristics, areas, integers, steps, actions, elements, and / or components.
[0040] When it is stated that one part is "on" or "on" another part, it may be directly on or on the other part, or another part may be involved in between. In contrast, when it is stated that one part is "directly on" another part, no other part is interposed in between.
[0041] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as generally understood by those skilled in the art to which this invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with relevant technical literature and the present disclosure, and are not interpreted in an ideal or highly formal sense unless otherwise defined.
[0042] Also, unless otherwise specified, % means weight %, and 1 ppm is 0.0001 weight %.
[0043] In this specification, the term “combination(s) of these” described in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including any one or more selected from the group consisting of said components.
[0045] Method for manufacturing a positive electrode active material for a lithium secondary battery
[0046] A method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment comprises: a step of preparing a transition metal precursor; a step of mixing the transition metal precursor and a first lithium raw material to prepare a mixture; a step of calcining the mixture to obtain a calcined product in the form of a single particle; and a step of mixing the calcined product, a coating raw material, and a second lithium raw material, and then heat-treating the mixture to obtain a positive electrode active material having a coating layer formed thereon.
[0048] Hereinafter, a method for manufacturing a positive electrode active material for a lithium secondary battery according to one embodiment of the present invention will be described step by step.
[0050] 1. Step of preparing the transition metal precursor
[0051] First, a transition metal precursor is prepared. Specifically, a transition metal precursor containing nickel, cobalt, and manganese is prepared, and more specifically, a transition metal precursor containing 50 to 70 mol% of nickel based on the total molar amount of the transition metal is prepared.
[0052] In one embodiment, the transition metal precursor may have an average particle size (D50) of 0.50 to 2.50 μm, and more specifically, may be 0.55 μm or more, 0.60 μm or more, 0.65 μm or more, or 0.70 μm or more, or 2.40 μm or less, 2.30 μm or less, 2.20 μm or less, 2.10 μm or less, or 2.0 μm or less. According to one embodiment of the present invention, when the average particle size of the transition metal precursor satisfies the above range, the primary particles of the precursor receive heat uniformly during the calcination process, so crystallization and particle growth are sufficiently achieved, thereby effectively improving the degree of single crystallinity, and more preferably, the transition metal precursor D50 can be controlled to 0.70 to 1.0 μm.
[0053] In this specification, "average particle size (D50)" may be measured using a particle size analyzer or obtained from a cross-sectional image. Specifically, in this embodiment, "average particle size (D50)" may be measured using equipment from Microtrack or Malvern, utilizing a diffraction phenomenon based on the Fraunhofer diffraction theory.
[0054] Meanwhile, a transition metal precursor according to one embodiment of the present invention is prepared by a spray pyrolysis method. Specifically, the transition metal precursor can be prepared by spray pyrolysis of a metal salt solution including nickel salt, cobalt salt, and manganese salt, and a spray pyrolysis method conventionally used in the industry can be utilized.
[0055] For example, the transition metal precursor may be manufactured by obtaining particles formed by spraying a metal solution containing nickel, cobalt, and manganese raw materials in the form of fine droplets and then thermally decomposing it in a high-temperature atmosphere.
[0056] Conventional co-precipitation precursors are manufactured such that each transition metal forms a uniform phase. However, because they involve processes such as roasting or pre-calcination to remove large amounts of moisture (H2O) and impurities from the co-precipitation precursor, there are problems that increase manufacturing costs and reduce overall process efficiency.
[0057] On the other hand, transition metal precursors produced by spray pyrolysis can be used to produce single-crystal active materials by including a partial spinel phase resulting from changes in the Mn oxidation state. In particular, the spinel phase can induce uniform crystal growth by providing a stress-relieving effect within the crystal structure.
[0058] The above nickel raw material is not particularly limited as long as it is used in the industry for manufacturing a cathode active material precursor. For example, the above nickel raw material may be a nickel-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, it may be NiSO4, NiSO4·6H2O, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, nickel fatty acid salt, nickel halide, or a combination thereof, but is not limited thereto.
[0059] The above-mentioned cobalt raw material is not particularly limited as long as it is used in the industry for manufacturing a cathode active material precursor. For example, the above-mentioned cobalt raw material may be a cobalt-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically, may be CoSO4, CoSO4·7H2O, Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or a combination thereof, but is not limited thereto.
[0060] The above manganese raw material is not particularly limited as long as it is used in the industry for the manufacture of cathode active material precursors. For example, the above manganese raw material may be a manganese-containing sulfate, acetate, nitrate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof. Specifically, it may be a manganese salt such as MnSO4, MnCO3, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid, manganese oxide such as Mn2O3, MnO2, and Mn3O4, oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.
[0061] The above metal solution may be prepared by adding nickel raw material, cobalt raw material, and manganese raw material to a solvent, specifically water, or a mixture of water and an organic solvent that can be uniformly mixed with water (e.g., alcohol).
[0062] The above spray pyrolysis can be performed in a temperature range of 600 to 1000°C. Specifically, it can be performed in a temperature range of 650 to 900°C, more preferably in a temperature range of 700 to 850°C. When the spray pyrolysis temperature satisfies the above range, the crystallinity, particle size, etc., of a suitable precursor for manufacturing a single-crystal active material can be secured, and the conditions of the suitable precursor can be referenced from the above description.
[0063] The precursor produced by the above-described process preferably has a nickel (Ni) content of 50 mol% or more of the total metal content, specifically in the range of 50 mol% to 70 mol% or 58 mol% to 65 mol%.
[0064] When the nickel (Ni) content in the above precursor satisfies the above range, cell characteristics can be further improved when the positive electrode active material finally manufactured according to the embodiment of the present invention is applied to a battery. In the case of a positive electrode active material containing a nickel (Ni)-based metal oxide, the calcination temperature varies depending on the nickel (Ni) content during calcination; specifically, the higher the nickel (Ni) content, the lower the temperature required for calcination. More specifically, the lower the nickel (Ni) content, the higher the calcination temperature, and in this case, the surface portion of the active material may experience degradation due to high temperatures. In this case, it is common to reduce such degradation by coating the surface, and the heat treatment during coating also exhibits different coating element diffusion trends depending on the nickel (Ni) content. The heat treatment temperature of the embodiment can be controlled by the nickel (Ni) content of the above precursor according to the present invention, and thereby, the diffusion thickness of the coating element and the coating shape can be controlled.
[0066] 2. Step of preparing the mixture
[0067] Subsequently, a step is performed to prepare a mixture by mixing the above-mentioned transition metal precursor and the first lithium raw material.
[0068] In one embodiment, the first lithium raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it is soluble in water. Specifically, the first lithium raw material may be one or more selected from Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7. In this embodiment, the first lithium raw material may be, for example, Li2CO3.
[0069] Meanwhile, the tap density of the mixture according to one embodiment of the present invention is 1.465 g / cc or higher.
[0070] In one embodiment, the tap density of the mixture may be 1.466 g / cc or higher, 1.467 g / cc or higher, 1.468 g / cc or higher, 1.469 g / cc or higher, or 1.470 g / cc or higher. When the tap density of the mixture satisfies the above range, the amount of slag charged in the calcination process can be significantly increased, thereby greatly improving the calcination amount per unit time, i.e., the production yield. Furthermore, while increasing the production yield, the reactivity between the transition metal in the precursor and the lithium introduced during calcination can be sufficiently promoted to uniformly form a layered structure of the active material. Specifically, if the tap density of the mixture is lower than the above range, the manufacturing time required to produce a cathode active material of the desired quality under the same calcination conditions increases, thereby reducing productivity. Additionally, as the active material is exposed for a long time to the high calcination temperature range used to manufacture single-crystal active materials, structural degradation from the surface may increase. According to such structural degradation, there may be a problem in which the initial resistance increases and the electrochemical properties deteriorate.
[0071] In this specification, tap density refers to a measurement using a GEOPYC 1365 (Micromeritics) tap density meter. Specifically, 10g of the prepared mixture was placed into a cylinder with a diameter of 19.1mm, and a horizontal force of 108N was applied, and this was repeated twice to measure the density.
[0072] In one embodiment, the molar ratio (Li / Me) of lithium (Li) to the transition metal (Me) excluding lithium (Li) in the mixture may be greater than 0.90 and less than 1.00. More specifically, it may be 0.92 to 0.98, or 0.95 to 0.98.
[0073] In one embodiment of the present invention, when Li / Me in the mixture is designed to be within the above range and Li is dividedly added by subsequently adding a second lithium raw material in the coating step described below, it is desirable to be able to control the physical properties of the spray pyrolysis precursor that does not form a uniform phase depending on the change in Mn oxidation state, and to effectively control the lithium content remaining on the surface of the final obtained cathode active material.
[0074] When the Li / Me ratio is designed to exceed 1.00 when mixing the first lithium raw material and the precursor, problems may arise in which the electrochemical performance and structural stability of the single-crystal active material are degraded due to overgrowth and non-uniform growth caused by Li.
[0075] In one embodiment, the step of preparing a mixture by mixing the transition metal precursor and the first lithium raw material may satisfy Formula 1 below:
[0076] [Equation 1]
[0077] 1.45 < A / B < 1.63
[0078] (In the above Equation 1,
[0079] A is the tap density (g / cc) of the above mixture, and B represents the molar ratio (Li / Me) of lithium (Li) to the transition metal (Me) excluding lithium (Li) in the above mixture).
[0080] More specifically, the above A / B may be 1.46 or higher, 1.47 or higher, 1.48 or higher, 1.49 or higher, or 1.50 or higher, or 1.62 or lower, or 1.61 or lower. In this embodiment, the above A / B may satisfy 1.50 ≤ A / B ≤ 1.60.
[0081] As the above mixture satisfies Equation 1, a positive electrode active material for a lithium secondary battery can be realized that has excellent electrochemical properties, such as charge capacity, discharge capacity, and efficiency, and improved structural stability. More specifically, when referring to the embodiments or comparative examples of the present invention, if the value of Equation 1 of the mixture is lower than the above range, for example, if the Li / Me molar ratio is excessively high, local necking between particles is excessively promoted during calcination, which may result in some large-sized grain growth. This may lead to a problem where the reaction within the electrode is not uniform due to non-uniform grain growth, resulting in inferior performance. Furthermore, if the excess residual lithium remaining after the reaction is not controlled, it may affect electrode manufacturing, which may adversely affect battery performance by accelerating side reactions with the electrolyte during charging and discharging. On the other hand, if the value of Equation 1 of the above mixture is higher than the above range, for example, if the Li / Me molar ratio is excessively low, it may be difficult to manufacture a cathode active material with structural stability under the same sintering conditions. Furthermore, as more heat is required for grain growth when manufacturing a single-crystal active material, the active material may be exposed to the high-temperature sintering range for a long time, which may lead to increased structural degradation from the surface. According to such structural degradation, there may be a problem in which the initial resistance increases and electrochemical properties deteriorate. According to one embodiment of the present invention, when a mixture is manufactured by designing Li / Me to be 0.92 to 0.98, it can be confirmed that the tap density of the mixture is high, at least 1.472 g / cc. Through this, it can be seen that even when charging a mixture of the same raw materials, the packing density can be increased when controlling Li / Me to the above range.
[0082] In one embodiment, to control the tap density to A / B within the range described above, the average particle size (D50) of the first lithium raw material relative to the transition metal precursor may be 1.0 to 10.0 times, and more preferably 2.0 times or more, 3.0 times or more, or 4.0 times or more, or 9.0 times or less, 8.0 times or less, or 7.0 times or less. For example, when the average particle size of the transition metal precursor is 0.70 to 1.0 μm, the average particle size of the first lithium raw material may be 0.70 to 10.0 μm. More specifically, the average particle size of the first lithium raw material may be 0.80 μm or more, 1.0 μm or more, 1.5 μm or more, 2.0 μm or more, 2.5 μm or more, 3.0 μm or more, 3.5 μm or more, or 4.0 μm or more, or 9.0 μm or less, 8.0 μm or less, 7.0 μm or less, or 6.0 μm or less. According to one embodiment of the present invention, when the average particle size of the first lithium raw material satisfies the above range, it is easy to control the tap density to A / B range when mixed with the transition metal precursor, and accordingly, an effect of improving productivity can be achieved. Furthermore, since heat is uniformly transferred during the calcination stage of the mixture, crystallization and grain growth are sufficiently achieved, and the degree of single crystallinity can be effectively improved.
[0083] Optionally, a doping raw material may be added during the preparation of the above mixture. Based on the total metal in the precursor, the doping element in the doping raw material may be 0.10 to 1.00 mol%, and specifically, may be 0.11 mol% or more, 0.12 mol% or more, 0.13 mol% or more, or 0.14 mol% or more, or 0.90 mol% or less, 0.80 mol% or less, 0.70 mol% or less, 0.60 mol% or less, or 0.50 mol% or less. More specifically, when two or more types of doping raw materials are mixed, each doping raw material may be mixed so that the content of each is individually 0.10 to 0.50 mol%.
[0084] Adding the above-mentioned doping raw material within the above range is desirable as it can improve the discharge capacity and charge / discharge efficiency performance of a lithium secondary battery using the finally manufactured cathode active material.
[0085] The above doping raw material may include one or more elements selected from Zr, V, Co, Mg, Ti, Y, Sr, Nb, Ba, Ca, B, W, Sc, Si, Fe, Mo, Ce, Hf, Ta, and La, and more specifically, the above doping raw material may include a Y raw material and a Zr raw material, and in a preferred embodiment, each doping raw material may be independently introduced in an amount of 500 to 5000 ppm.
[0086] The above doping raw material may include sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or oxyhydroxides containing doping elements, and the present invention is not particularly limited thereto.
[0088] 3. Step of obtaining the calcined product
[0089] Subsequently, the above mixture is calcined to obtain a calcined product in the form of single particles.
[0090] In this specification, a single particle may include at least one of a single crystal structure consisting of a single particle and a structure in which 2 to 20 or 2 to 10 particles are clustered together and distinguished as a single mass when the cross-section of the powder is observed through a scanning electron microscope (SEM). Here, a single particle refers to a single grain or crystallite.
[0091] As in this embodiment, the single-particle sintered material has a smaller specific surface area compared to the secondary particle form formed by the aggregation of tens to hundreds of primary particles in the past, which reduces the amount of gas generated due to side reactions with the electrolyte. Additionally, the particle strength is high, which can suppress particle breakage during rolling and reduce the occurrence of cracks due to repeated charging and discharging. Accordingly, it has the advantage of superior lifespan and safety compared to secondary particles, and enables the realization of high energy density of the electrode.
[0092] In one embodiment, the calcination may be performed for 10 to 14 hours at a temperature of 900 to 960°C in a CO2-free air (CFA) atmosphere. More specifically, it may be performed for 10.5 to 13.5 hours, or 11 to 13 hours, at a temperature of 910 to 950°C or 920 to 940°C. When the temperature and time during calcination satisfy the above ranges, a single-particle cathode active material for a lithium secondary battery can be provided, ensuring stability while maximizing electrochemical performance. In particular, if the temperature and time during calcination are lower than the above ranges, the reaction does not proceed sufficiently, making particle growth difficult and potentially leading to the formation of secondary particles. This results in a higher residual lithium content, which may adversely affect battery performance. Conversely, if the temperature and time during calcination are higher than the above ranges, particle aggregation may become severe, leading to the formation of excessively large particles, and prolonged exposure to high temperatures may induce surface degradation. This can cause problems with battery performance.
[0093] In this specification, the term "sintering time" may mean the "sintering holding time." Specifically, the firing holding time may mean only the time of maintaining the temperature at the firing temperature, excluding the time for raising the temperature to the firing temperature and the time for lowering the temperature during cooling.
[0094] Generally, oxygen conditions are considered favorable for controlling residual lithium during the calcination of cathode active materials. This is because if oxygen is insufficient, lithium may revert to a form such as lithium carbonate, and there may be problems such as the failure to smoothly form a layered structure.
[0095] The inventors have discovered that oxygen conditions are not essential during the coating step following the manufacture of lithium metal oxides, and that general atmospheric conditions are actually more advantageous in some aspects. More specifically, regarding the aforementioned nickel (Ni) content range, a higher temperature than that in an atmospheric atmosphere is required for grain growth and subsequent single crystallization during calcination in an oxygen-rich, stable atmosphere. In this case, since the required reaction temperature under atmospheric conditions is actually lower than under oxygen conditions, favorable results can be expected, such as the suppression of various side reactions (e.g., changes in crystal structure) that may occur at high temperatures and economic benefits. These characteristics can be similarly realized through heat treatment during coating; more specifically, under atmospheric conditions, the diffusion of coating elements into the core is further promoted, and the structural stability of the core's surface can be significantly improved.
[0096] However, even in such cases, atmospheric conditions free of carbon dioxide may be desirable to prevent the loss of lithium raw materials due to carbon dioxide.
[0097] In this embodiment, if necessary, a step of disintegrating the sintered product may be further included after the step of obtaining the sintered product. That is, a disintegration process may be included after obtaining the sintered product and before the coating process.
[0098] The above-mentioned crushing step can be performed after cooling the calcined product to 50°C to 200°C.
[0099] The above-mentioned disintegration may be performed by methods conventionally practiced in the industry. The above-mentioned disintegration may be performed using, for example, rotor mills, ball mills, fin mills, jet mills, bead mills, and roll mills, but is not limited thereto.
[0100] A positive electrode active material for a lithium secondary battery manufactured according to one embodiment may include a single-particle calcined material, i.e., a lithium metal oxide.
[0101] Specifically, the positive active material for a lithium secondary battery manufactured according to one embodiment is a positive active material for a lithium secondary battery in the form of a single particle, and the positive active material may include a form in which 1 to 20 primary particles are aggregated.
[0102] In one embodiment, the sintered product may have an average grain size of 210 to 270 nm, and more specifically, 215 to 265 nm, or 220 to 260 nm.
[0103] In the present invention, "crystal grain" refers to a distinct region in which atoms within a primary particle form a lattice structure in a certain direction.
[0104] The above grain size can be estimated using peak broadening of XRD data and can be quantitatively calculated through the Scherrer equation.
[0105] The sintered product according to the present invention has the advantage of having excellent particle strength as the average grain size satisfies the above range, and can improve the lifespan characteristics and stability of the battery when applied to a lithium secondary battery.
[0106] In one embodiment, the ratio of the c-axis length to the a-axis length (c / a) obtained by X-ray diffraction analysis of the crystal of the sintered product may be 4.9440 to 4.9520, and more specifically 4.9450 to 4.9515, or 4.9460 to 4.9510.
[0107] Specifically, the a-axis length obtained by X-ray diffraction analysis of the crystal of the sintered material may be in the range of 2.8800 to 2.8850 Å, and the c-axis length may be in the range of 14.2610 to 14.2700 Å. When the ratio of the c-axis length to the a-axis length (c / a), the a-axis length, and the c-axis length obtained by X-ray diffraction analysis of the crystal of the sintered material satisfy the above ranges, the crystal structure of the sintered material is stabilized, thereby enabling the realization of a positive electrode active material with excellent electrochemical properties while including a sintered material in the form of a single particle, as in the present embodiment.
[0108] In addition, the cation mixing ratio of nickel cations in the lithium layer within the crystal structure of the above-mentioned calcined product may be 4% or more, more specifically 4.2% or more, 4.5% or more, or in the range of 4.7% to 7%.
[0109] In this embodiment, the electrochemical characteristics of a lithium secondary battery can be significantly improved by controlling the cation mixing ratio to be within the above range. Specifically, in this specification, the cation mixing ratio refers to the amount of nickel substituted at lithium sites in the lithium layer.
[0111] 4. A step of obtaining an anode active material with a coating layer formed thereon.
[0112] Subsequently, a step is performed to obtain an anode active material with a coating layer formed thereon by mixing the above-mentioned calcined material, the coating raw material, and the second lithium raw material, followed by heat treatment.
[0113] The above coating raw material may include one or more selected from Co(OH)2, CoCl2, CoO, CoF3, CoSO4·xH2O, CoSO4·7H2O, (CH3COO)2Co·4H2O, Co(NO3)2·6H2O, (CH3CO2)2Co, CoCO3·xH2O, and Co3(PO4)2.
[0114] The above coating raw material can be introduced in a content range of 1 mol% to 4 mol%, specifically 2.0 mol% to 3.0 mol%, based on the total metal excluding lithium in the above-mentioned product.
[0115] In one embodiment, the second lithium raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it is soluble in water. Specifically, the first lithium raw material may be one or more selected from Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7. In this embodiment, the second lithium raw material is, for example, LiOH·H2O It could be.
[0116] In the above heat treatment process, reactive lithium within the lithium remaining on the surface of the lithium metal oxide, additionally introduced lithium raw material; and cobalt contained in the coating raw material; react to form one or more coating materials selected from metal hydroxide, metal oxide, lithium metal hydroxide, and lithium metal oxide lithium cobalt compounds.
[0117] Specifically, cobalt oxide or lithium cobalt oxide can be produced alone or simultaneously.
[0118] In one embodiment, the heat treatment may more preferably be performed in an atmospheric (air atmosphere) at a temperature of 730°C to 770°C, more specifically 740°C to 760°C, or 750°C for 3 to 16 hours, more specifically 3.5 to 14 hours, 4 to 12 hours, 4.5 to 10 hours, or 5 to 8 hours. The heat treatment time is controlled so that the amount of lithium subsequently added according to the present invention can sufficiently react with the single-particle calcined material, and as the amount subsequently added increases, the heat treatment time required for the reaction may increase.
[0119] If the heat treatment process satisfies the above conditions, the deterioration of the layered manganese oxide present on the surface of the positive electrode active material into a spinel structure can be effectively prevented by stabilizing the surface structure during the charging and discharging process.
[0120] In one embodiment of the present invention, when heat treatment is performed under the above conditions, a coating layer is formed on the surface of the sintered product, i.e., the lithium metal oxide, and at the same time, a lithiation reaction occurs efficiently at the surface and / or particle boundaries of the lithium metal oxide, thereby forming coating particles in the coating layer within a range that allows for the recovery of the oxygen-deficient (O2 vacancy) region generated during the high-temperature manufacturing process of the lithium metal oxide, while also stabilizing the structure up to the depth range of the surface portion of the internal core. This is desirable because it can improve the electrochemical performance of the cathode active material finally produced.
[0121] In addition, by performing the calcination and heat treatment steps under the above conditions in the present invention, a separate washing process is not required to remove lithium remaining on the surface of the final-produced positive electrode active material.
[0122] In one embodiment, the total residual lithium content of the positive electrode active material may be 0.25 wt% or less, and more specifically, 0.245 wt% or less, 0.240 wt% or less, 0.235 wt% or less, or 0.230 wt% or less.
[0123] At this time, the residual lithium content of the positive electrode active material is distinct from the residual lithium content of the active material before coating. The residual lithium content of the single-particle calcined material before coating is significant in that it allows for controlling the amount of lithium added during coating according to the amount, thereby satisfying the Li / Me molar ratio of the final positive electrode active material within a predetermined range. For example, if the Li / Me molar ratio is controlled to be less than 1.00 during the mixing step to obtain a single-particle calcined material with a Li / Me molar ratio of less than 1.00 and containing residual lithium within a predetermined range, the Li / Me molar ratio of the final positive electrode active material can be satisfied by appropriately controlling the amount of lithium added during Co coating, taking into account the total residual lithium content of the calcined material.
[0124] Specifically, the total residual lithium content in the single-particle calcined product may be 0.25 wt% or less, and more preferably 0.24 wt% or less, 0.22 wt% or less, or 0.20 wt% or less. If the residual lithium content in the calcined product is too high, it may be that the reactivity during calcination is poor and the single-particle formation did not proceed sufficiently, which may have a negative effect on the physical properties and electrochemical performance of the final cathode active material after coating. On the other hand, if the total residual lithium content of the single-particle calcined product is controlled within the above range, the total residual lithium content of the final cathode active material can be controlled within a predetermined range while satisfying the Li / Me molar ratio of the final cathode active material by controlling the amount of lithium added after Co coating within an appropriate range.
[0125] Generally, residual lithium may exist on the surface of the cathode active material in the form of LiOH and / or Li2CO3 compounds as by-products that remain after failing to react. Such residual lithium can be a property directly related to the safety of the battery, as it promotes gelation of the slurry during the manufacture of the secondary inhibitor, thereby reducing process efficiency, or causes side reactions with the electrolyte during battery operation, generating a large amount of gas. According to the manufacturing method of the present invention, as the residual lithium content of the final cathode active material is controlled to the above range, the safety of the battery can be improved.
[0126] In one embodiment, the positive electrode active material having the coating layer formed thereon may have a molar ratio (Li / Me) of lithium (Li) to a transition metal (Me) excluding lithium (Li) of 1.03 to 1.07, and more specifically, may be 1.032 to 1.068 or 1.034 to 1.065.
[0127] In another embodiment of the present invention, the positive active material may be represented by the following chemical formula 1:
[0128] [Chemical Formula 1]
[0129] Li a Ni x Co y Mn z M1 k O2
[0130] (In the above chemical formula 1,
[0131] 0.9 ≤ a ≤ 1.1, 0.3 ≤ x ≤ 0.73, 0.01 ≤ y ≤ 0.3, 0.01 ≤ z ≤ 0.4, 0 ≤ k ≤ 0.2, x + y + z + k = 1,
[0132] M1 is one or more elements selected from the group consisting of Al, Mg, Zr, Sn, Ca, Ge, Ti, Cr, Fe, Zn, Y, Ba, La, Ce, Sm, Gd, Yb, Sr, Cu, and Ga).
[0133] Specifically, the above positive active material may have a Ni content of 70 mol% or less. More specifically, the above positive active material may have a Ni content of 60 to 70 mol%.
[0134] When the Ni content of the above-mentioned cathode active material satisfies the above range, there is an advantage in that the thermal propagation phenomenon occurring in high-nickel NCM-based cathode active materials with a nickel content exceeding 73 mol%, specifically 70 mol%, can be suppressed. In addition, it is desirable to suppress the problem of increased energy density costs due to rising prices of Ni and Co.
[0135] In another embodiment of the present invention, y may be 0.05 ≤ y ≤ 0.20. In short, the positive electrode active material may have a Co content of 5 to 20 mol%.
[0136] When the Co content of the above-mentioned cathode active material satisfies the above range, it is desirable as it offers the advantage of enabling sufficient efficiency characteristics and excellent reversible capacity while reducing the cost of raw materials.
[0137] The positive electrode active material manufactured according to the present invention has a high degree of crystallinity and excellent particle strength, and accordingly, has the advantage of suppressing the phenomenon of electrochemical performance degradation during the process of manufacturing a lithium secondary battery.
[0139] anode
[0140] In another embodiment of the present invention, a positive electrode is provided comprising a current collector and a positive electrode active material layer located on one surface of the current collector and comprising a positive electrode active material manufactured according to the above embodiment.
[0141] The characteristics of the positive active material constituting the above positive active material layer are the same as those previously described. Therefore, a detailed description of the positive active material will be omitted.
[0142] The above current collector may be, for example, made of stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treated with carbon, nickel, titanium, silver, etc.
[0143] Meanwhile, the above positive active material layer may include a binder and a conductive material.
[0144] At this time, the binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof. One of these alone or a mixture of two or more may be used, but is not limited thereto. The binder may be included in an amount of 1 to 30 weight% based on the total weight of the positive active material layer.
[0145] In addition, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special limitations as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used, but is not limited thereto. The conductive material may typically be included in an amount of 1 to 30 weight% relative to the total weight of the positive electrode active material layer.
[0146] Except for being manufactured to fall within the above range, the above anode may be manufactured according to a conventional anode manufacturing method.
[0147] Specifically, the anode may be manufactured by applying a composition for forming an anode active material layer, which optionally includes a binder, a conductive material, or a solvent as needed, onto an anode current collector, followed by drying and rolling. At this time, the types and contents of the anode active material, binder, and conductive material are as described above.
[0148] The above solvent may be a solvent commonly used in the relevant technical field, such as dimethylsulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it has a viscosity that allows for the dissolution or dispersion of the anode active material, conductive material, and binder, taking into account the coating thickness of the slurry and the manufacturing yield, and subsequently provides excellent thickness uniformity when coated for anode manufacturing.
[0149] Alternatively, the anode may be manufactured by casting a composition for forming an anode active material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.
[0151] lithium secondary battery
[0152] In another embodiment, a lithium secondary battery including the anode is provided.
[0153] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode positioned opposite to the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the positive electrode is as described above. Additionally, the lithium secondary battery may optionally further include a battery container housing an electrode assembly comprising the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.
[0154] In the above lithium secondary battery, the negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0155] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. In addition, the above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding strength of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0156] The above-mentioned cathode active material layer may optionally include a binder and a conductive material together with the cathode active material. The above-mentioned cathode active material layer may be manufactured, as an example, by applying a composition for forming a cathode active material layer, comprising a cathode active material and optionally a binder and a conductive material, onto a cathode current collector and drying it, or by casting the composition for forming a cathode onto a separate support and then laminating the film obtained by peeling it off from the support onto a cathode current collector.
[0157] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; metal oxides capable of doping and dedoping lithium, such as SiOβ (0 ≤ β ≤ 2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the above-mentioned metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the above-mentioned negative electrode active material. Furthermore, the carbon material may include both low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0158] The binder and conductive material mentioned above may be the same as those previously described in the anode.
[0159] Next, depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. As such a separator, polyethylene, polypropylene, polyvinylidene fluoride, or a multilayer film of two or more layers thereof may be used, and a mixed multilayer film such as a polyethylene / polypropylene two-layer separator, a polyethylene / polypropylene / polyethylene three-layer separator, or a polypropylene / polyethylene / polypropylene three-layer separator may also be used.
[0160] In addition, regarding the lithium secondary battery, the electrolyte may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., which are usable when manufacturing a lithium secondary battery, but is not limited to these.
[0161] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0162] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the above organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having C2 to C20 structures and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.In this case, using a mixture of cyclic carbonate and chain carbonate in a volume ratio of about 1:1 to about 1:9 can result in excellent performance of the electrolyte.
[0163] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.
[0164] As described above, since the lithium secondary battery including the positive electrode according to the present invention has excellent electrochemical characteristics such as charging capacity, discharging capacity, and efficiency, it is useful in portable devices such as mobile phones, laptop computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0166] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0168] Example 1
[0169] (Mixed) Ni 0.62 Co 0.07 Mn 0.31 O xA mixture was prepared by mixing Li2CO3 with an average particle size (D50) of 4.6 μm as a first lithium raw material with a transition metal precursor having an average particle size (D50) of 0.75 μm and a composition (x is 1.0 to 1.3, approximately 1.22 in this embodiment). At this time, the mixture was designed so that the molar ratio (Li / Me) of lithium (Li) to the transition metal (Me) excluding lithium was 0.98. In addition, the transition metal precursor used was prepared by spray pyrolysis.
[0170] After (calcination and disintegration), the mixture was calcined for 12 hours at a temperature of 930°C and under CO2-free atmospheric conditions (CO2-free air, CFA) to obtain a calcined product. Subsequently, the calcined product was naturally cooled to form a lithium metal oxide. Subsequently, the lithium metal oxide was disintegrated using an air jet mill to obtain a single-particle cathode active material.
[0171] (Coating) A positive electrode active material with a coating layer formed thereon was prepared by mixing the coating raw material Co(OH)2 and the second lithium raw material Li2CO3 with the above-mentioned single-particle positive electrode active material and then heat-treating it. At this time, 3 mol% of Co(OH)2 and Li2CO3 based on the above-mentioned calcined material was used, and the heat treatment temperature during coating was 750℃ and the heat treatment time was 6 hours.
[0172] The composition of the final manufactured cathode active material is Li 1.03~1.07 Ni 0.6 Co 0.1 Mn 0.3 It was designed to satisfy O2.
[0174] Examples 2-3 and Comparative Examples 1-5
[0175] The cathode active materials of Examples 2-3 and Comparative Examples 1-5 were prepared in the same manner as Example 1, except that the Li / Me design conditions and calcination temperature were changed during mixing as shown in Table 1 below.
[0176] division Design conditions for mixing firing conditions Li / Me ratio Firing temperature (°C) Firing time (hr) Example 1 0.98 930 12 Example 2 0.95 930 Example 3 0.92 950 Comparative Example 1 0.90 970 Comparative Example 2 1.01 930 Comparative Example 3 1.04 930 Comparative Example 4 1.07 930 Comparative Example 5 0.98 780
[0177] Experimental Example 1: Li 2 CO 3 and evaluation of physical properties of transition metal precursor mixtures
[0178] (1) Tap density analysis
[0179] The tap density of the Li2CO3 and transition metal precursor mixture was measured using a GEOPYC 1365 (Micromeritics) tap density meter. Specifically, 10 g of the prepared mixture was placed into a cylinder with a diameter of 19.1 mm, and a horizontal force of 108 N was applied. This was repeated twice to measure the density, and the results are shown in Table 2 below.
[0180] (2) Evaluation of Equation 1
[0181] For a mixture of Li2CO3 and transition metal precursors, Formula 1 below was evaluated, and the results are shown in Table 2 below.
[0182] [Equation 1]
[0183] 1.45 < A / B < 1.63
[0184] (In the above Equation 1,
[0185] A is the tap density (g / cc) of the above mixture, and B represents the molar ratio (Li / Me) of lithium (Li) to the transition metal (Me) excluding lithium (Li) in the above mixture.
[0186] division Tap density (g / cc) of Li2CO3 and transition metal precursor mixture A / B Example 1 1.498 1.53 Example 2 1.485 1.56 Example 3 1.472 1.60 Comparative Example 1 1.463 1.63 Comparative Example 2 1.461 1.45 Comparative Example 3 1.457 1.40 Comparative Example 4 1.452 1.36 Comparative Example 5 1.498 1.53
[0187] As confirmed in Table 2 above, in the case of Examples 1 to 3, which were prepared by designing the Li / Me ratio to be 0.92 to 0.98 when mixing Li2CO3 and transition metal precursors, it can be seen that the tap density of the mixture is higher compared to Comparative Examples 1 to 4. Through this, it can be seen that even when charging a mixture of the same raw materials, the packing density can be increased when controlling the Li / Me ratio to 0.92 to 0.98.
[0189] Experimental Example 2: SEM Image Evaluation
[0190] SEM images of the single-particle cathode active material prepared in the examples and comparative examples were obtained using a Scanning Electron Microscopy (SEM) analysis device at 10,000x magnification and under 10 keV conditions, and are shown in FIGS. 1 to 8.
[0191] Referring to FIGS. 1 to 8, it can be seen that the positive active materials of the examples and comparative examples are all in the form of single particles consisting of 1 to 5 primary particles.
[0192] In particular, referring to FIG. 8, in the case of Comparative Example 5, where Li2CO3 and transition metal precursors were mixed with Li / Me designed to be 0.98, the same as in Example 1, but the calcination temperature range is lower than that of the present invention, it is possible to manufacture a single-particle cathode active material, but as described below, it can be confirmed that the crystal grain size is small.
[0194] Experimental Example 3: Evaluation of Residual Lithium Content
[0195] The residual lithium in the positive electrode active material before and after coating prepared in the examples and comparative examples was confirmed using a neutralization titration method. By measuring the residual lithium content, it is possible to predict or prevent gas generation or explosion of the battery, or gallation occurring during electrode fabrication.
[0196] Specifically, distilled water was added to the cathode active material prepared according to the examples and comparative examples, and residual lithium was extracted using a stirrer, and the cathode active material powder and extract were separated using a filtering device. Then, the residual lithium content in the cathode active material was measured by neutralizing the extract using a Mettler Toledo potentiometric titrator, and the results are shown in Tables 3 and 4 below.
[0198] Experimental Example 4: XRD Evaluation
[0199] (1) Grain size measurement
[0200] The crystal size of the single-particle cathode active material prepared in the examples and comparative examples before coating was confirmed using X-ray diffraction (XRD).
[0201] After placing the pre-coating cathode active material powder prepared in the examples and comparative examples onto an XRD sample loader with a flat surface, XRD measurements were performed using a Bruker instrument.
[0202] Specifically, the cathode active material was uniformly loaded into a sample holder in powder form, and XRD analysis was performed in the 2θ region between 10 and 80° at a speed of 10.7° / min, with the X-ray tube set to 40kV and 40mA. The crystal size of the cathode active material before coating was calculated using the Smart Lab Studio program based on the extracted X-ray diffraction patterns, and the results are shown in Table 3 below. In Table 3, X-size represents the grain size.
[0203] (2) Measurement of Cation Mixing Ratio
[0204] The cation mixing ratio of the single-particle cathode active material prepared in the examples and comparative examples before coating was confirmed using X-ray diffraction (XRD).
[0205] Specifically, the cation mixing value was calculated using the Ni1(3b) occupancy value calculated in the Crystal structure tab of Edit parameter, and the result is shown in Table 3 below.
[0206] (3) Measurement of lattice parameters
[0207] The lattice parameters a and c of the single-particle cathode active materials prepared in the examples and comparative examples before coating were confirmed using X-ray diffraction (XRD). These can be derived using lattice parameters a and c, which represent one side of the unit cell within the crystal structure derived from XRD measurements.
[0208] Specifically, the pre-coating positive electrode active material prepared in the examples and comparative examples has a crystal structure that is layered (R-3m), and in this structure, the side existing on the x and y axes can be represented as a, and the side existing on the z axis can be represented as c.
[0209] Specifically, the pre-coating cathode active material was placed in a holder and X-rays were irradiated onto the particles by measuring at 40 kV based on a Cu-Ka target, and the resulting diffraction grating was analyzed to measure the grating parameters a and c, and the results are shown in Table 3 below.
[0211] Experimental Example 5: Evaluation of Electrochemical Properties
[0212] (1) Manufacturing of coin-type half-cells
[0213] A CR2032 coin cell was manufactured using the positive electrode active material prepared in the examples and comparative examples in the following manner.
[0214] Specifically, a positive electrode active material, a conductive material (acetylene black FX35, Denka), and a polyvinylidene fluoride binder (product name: KF9709) were mixed in a weight ratio of 95:2:3, and this mixture was added to an N-methyl-2-pyrrolidone solvent so that the solid content was about 65-69% by weight to prepare a positive electrode active material slurry.
[0215] The above slurry was coated onto an anode current collection chain aluminum foil (Al foil, thickness: 20㎛) using a doctor blade, dried, and then rolled to manufacture an anode. The loading amount of the anode was approximately 14-15 mg / cm², and the rolling density was approximately 3.5 g / cm³.
[0216] A 2032 coin-type half-cell was manufactured by a conventional method using the above-mentioned positive electrode, lithium metal negative electrode (thickness 400 μm, NEBA), electrolyte, and polypropylene polyethylene separator. The above-mentioned electrolyte was prepared by dissolving 1M LiPF6 in a mixed solvent of ethylene carbonate, dimethyl carbonate, and diethyl carbonate (mixing ratio EC:DMC:DEC = 1:2:1 volume%) to prepare a mixed solution, and then adding 2 weight% of vinylene carbonate (VC) to it.
[0217] (2) Capacity and efficiency evaluation
[0218] After aging the coin-type half battery manufactured in (1) above at room temperature (25℃) for 10 hours, a charge / discharge test was performed.
[0219] The capacity evaluation was based on a reference capacity of 200 mAh / g, and the charge / discharge conditions applied were a constant current (CC) / constant voltage (CV) of 2.5 V to 4.45 V and a 1 / 20 C cut-off.
[0220] The initial capacity was measured by charging at 0.1C and discharging at 0.1C, and the discharge capacity was calculated. The results are shown in Table 5 below.
[0221] (3) Room temperature resistance measurement
[0222] The initial resistance at room temperature (Direct current internal resistance: DC-IR) was calculated by measuring the voltage value 60 seconds after applying the discharge current at 100% charge at 4.45V, while performing one cycle of 0.1C charging and 0.1C discharging with the battery at 25℃ under constant current-constant voltage conditions of 2.5V to 4.45V and 1 / 20C cut-off conditions, and the results are shown in Table 5 below.
[0224] Analysis results
[0225] (1) Residual lithium content and XRD evaluation of the positive electrode active material before coating
[0226] division Residual lithium content XRD LiOH(wt%) Li2CO3(wt%) Total Li(wt%) X-size(nm) Li / Ni (%) a(Å) c(Å) c / a Example 1 0.12 0.08 0.20 239 4.7 2.8807 14.2611 4.9506 Example 2 0.09 0.07 0.16 252 5.6 2.8828 14.2661 4.9487 Example 3 0.07 0.08 0.15 220 6.3 2.8846 14.2700 4.9470 Comparative Example 1 0.05 0.07 0.12 266 6.5 2.8860 14.2700 4.9446 Comparative Example 2 0.12 0.12 0.25 201 4.0 2.8776 14.2529 4.9531 Comparative Example 3 0.16 0.59 0.75 193 3.6 2.8773 14.2512 4.9530 Comparative Example 4 0.21 0.98 1.18 206 3.2 2.8764 14.2491 4.9538 Comparative Example 5 0.57 0.89 1.47 48 8.2 2.8816 14.2194 4.9346
[0227] Referring to FIGS. 1 to 8 and Table 3, compared to Examples 1 to 3, which were prepared by designing the Li / Me ratio to be 0.92 to 0.98 when mixing Li2CO3 and a transition metal precursor, Comparative Examples 2 to 5, which fall outside the above range, have a higher residual lithium content and smaller grain sizes.
[0228] Comparative Examples 2 to 4 show that while the crystal grain size is small, they exhibit an excessive primary particle shape in the SEM images. This indicates that while an excess amount of lithium hinders crystal growth, small crystals aggregate to form large particles, resulting in an uneven particle size distribution that can cause performance degradation. Additionally, the c / a value is large, exceeding 4.9530, which may lead to structural instability as the c-axis length increases excessively relative to the a-axis length.
[0229] Meanwhile, Comparative Example 5 was designed with a Li / Me ratio of 0.98, identical to Example 1, and mixed with Li2CO3 and a transition metal precursor; however, due to the low calcination temperature of 780°C, the lithium raw material did not react sufficiently. As a result, it was confirmed that the residual lithium content was the highest at 1.47 wt%, the grain size was significantly smaller at 48 nm, the Li / Ni ratio was the highest at 8.2%, and the c / a was the smallest.
[0230] In addition, Comparative Example 1 was designed with the lowest Li / Me ratio of 0.90, resulting in a very low residual lithium content of 0.12 wt%, but it was confirmed that the largest grain size of 266 nm was formed. However, since excessive lithium must be added during subsequent Co coating, the difficulty of the Co coating process may increase, and there is a possibility that productivity may decrease.
[0231] (2) Evaluation of residual lithium content and electrochemical properties of the positive electrode active material after coating
[0236] division Co 3 mol% coating Final active material Li / Me molar ratio Residual lithium content Lithium Post-add (Moll%) Coating temperature (°C) Coating time (hr) LiOH(wt%) Li2CO3(wt%) Total Li(wt%) Example 1 Example 1-1 3 750 6 1.036 0.09 0.13 0.22 Examples 1-2 4 750 6 1.048 0.09 0.12 0.21 Examples 1-3 5 750 6 1.057 0.08 0.14 0.22 Examples 1-4 6 750 6 1.066 0.08 0.13 0.21 Examples 1-5 8 750 6 1.091 0.09 0.20 0.28 Examples 1-6 10 750 6 1.107 0.10 0.49 0.59 Example 2 Example 2-1 2 750 6 0.99 0.08 0.10 0.18 Example 2-2 3 750 6 0.998 0.08 0.11 0.19 Examples 2-3 4 750 6 1.007 0.08 0.12 0.19 Examples 2-4 5 750 6 1.018 0.10 0.08 0.18 Examples 2-5 6 750 6 1.031 0.09 0.10 0.19 Examples 2-6 5 750 6 1.017 0.07 0.12 0.19 Examples 2-7 5 750 12 1.015 0.06 0.11 0.17 Examples 2-8 5 750 16 1.014 0.06 0.11 0.17 Example 3 8 750 6 1.013 0.09 0.18 0.27 Comparative Example 1 10 750 6 1.009 0.09 0.64 0.72 Comparative Example 2 3 750 6 1.076 0.09 0.12 0.22 Comparative Example 3 3 750 6 1.098 0.09 0.12 0.22 Comparative Example 4 3 750 6 1.152 0.10 0.13 0.23 Comparative Example 5 3 750 6 1.041 0.12 0.18 0.30
[0240] division 0.1C Charging Capacity (mAh / g) 0.1C discharge capacity (mAh / g) Efficiency (%) Room temperature resistance (Ω) Example 1 Example 1-1 219.8 198.4 90 23.8 Examples 1-2 219.1 200.0 91 22.7 Examples 1-3 219.0 200.5 92 23.1 Examples 1-4 219.4 201.3 92 22.0 Examples 1-5 218.3 198.8 91 22.9 Examples 1-6 216.6 197.7 91 28.6 Example 2 Example 2-1 221.2 195.3 88 25.6 Example 2-2 222.2 195.3 88 25.5 Examples 2-3 222.1 198.9 90 25.5 Examples 2-4 220.7 198.8 90 25.4 Examples 2-5 219.2 198.6 91 24.6 Examples 2-6 219.2 197.9 90 24.9 Examples 2-7 220.1 199.2 90 24.7 Examples 2-8 220.0 199.1 91 23.9 Example 3 218.9 196.7 90 25.9 Comparative Example 1 217.4 193.9 89 26.3 Comparative Example 2 220.5 198.9 90 25.3 Comparative Example 4 218.9 196.2 90 28.8
[0241] Referring to Tables 4 and 5 and Figures 1 to 8, in the case of Examples 1 to 3, in which calcination was performed with a Li / Me ratio of 0.92 to 0.98 when mixing Li2CO3 and a transition metal precursor, it can be seen that fine particles and coarse particles are reduced and the uniformity of the primary particles increases.
[0242] In particular, referring to Examples 1-1 to 1-4 and Examples 2-1 to 2-8, it can be seen that when Co 3 mol% reacts sufficiently with a lithium post-additive amount of up to 6 mol% (Li:Co molar ratio = 2:1), the residual lithium content is low, and the initial capacity and initial efficiency are excellent, while the electrochemical properties are excellent with low room temperature resistance. Additionally, in the case of Examples 2-7 and 2-8, it was confirmed that the residual lithium content and electrochemical properties improved somewhat when the coating time was increased to 12 hours or 16 hours. However, increasing the coating time may be limited considering productivity and process costs.
[0243] Meanwhile, when the lithium post-additive amounts in Examples 1-5 and 1-6 are 8 mol% and 10 mol%, respectively, it can be seen that the residual lithium content is higher and the electrochemical properties are somewhat inferior compared to Examples 1-1 to 1-4 due to the excessive ratio of lithium to Co. However, as described above, there is room for improvement if the coating time is increased, but this is not recommended when considering productivity and process efficiency.
[0244] In the case of Example 3 and Comparative Example 1, where the second lithium raw material was added in relatively high amounts to match the lithium ratio of the active material with the coating layer formed, which is the final product, because the Li / Me design values were low at 0.92 and 0.90, it can be confirmed that the amount of lithium added after Co coating is 8 mol% and 10 mol%, respectively. At this time, it can be confirmed that Comparative Example 1 has an excessive amount of residual lithium that does not participate in the reaction, resulting in the highest residual lithium content and high room temperature resistance, which degrades the electrochemical properties.
[0245] Comparative Examples 2 to 4, in which the Li / Me design value exceeds 1.00, show non-uniform grain growth when referring to FIGS. 5 to 7. In particular, in Comparative Example 4, which has the highest Li / Me design value, the reaction is sufficient even with a lithium post-add amount of 3 mol% and Co of 3 mol% (Li:Co molar ratio = 1:1) when coating Co. However, when referring to FIG. 7, it was found that fine particles and excessive coarse particles were generated due to the non-uniformity of the primary particles after calcination, resulting in very high room temperature resistance and consequently very inferior electrochemical properties.
[0246] In the case of Comparative Example 5, where the Li / Me design values and Co coating conditions are the same as those in Example 1, referring to Figure 8, it can be seen that grain growth is very poor and single-particle formation is not sufficiently achieved, and as a result, crystallinity is also very low, and consequently, electrochemical performance is expected to be very poor.
[0248] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.
Claims
Claim 1 A step of preparing a transition metal precursor manufactured by spray pyrolysis; a step of mixing the transition metal precursor and a first lithium raw material to prepare a mixture; a step of calcining the mixture to obtain a calcined product in the form of single particles; A method for manufacturing a positive electrode active material for a lithium secondary battery, comprising the step of obtaining a positive electrode active material having a coating layer formed thereon by mixing the above-mentioned calcined material, a coating raw material, and a second lithium raw material, and then heat-treating the mixture; wherein the tap density of the mixture is 1.465 g / cc or higher, and the step of preparing a mixture by mixing the transition metal precursor and the first lithium raw material satisfies the following Equation 1, [Equation 1] 1.45 < A / B < 1.63 (wherein A is the tap density (g / cc) of the mixture and B is the molar ratio (Li / Me) of lithium (Li) to the transition metal (Me) excluding lithium (Li) in the mixture) and the molar ratio (Li / Me) of lithium (Li) to the transition metal (Me) excluding lithium (Li) in the mixture is greater than 0.90 and less than 1.
00. Claim 2 delete Claim 3 delete Claim 4 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the first lithium raw material is Li2CO3. Claim 5 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the second lithium raw material comprises at least one of LiOH, Li2CO3, LiNO3, LiNO2, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a combination thereof. Claim 6 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in the step of mixing the transition metal precursor and the first lithium raw material to prepare a mixture, the average particle size (D50) of the first lithium raw material relative to the transition metal precursor is 1.0 to 10.0 times. Claim 7 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the calcination is performed at a temperature of 900 to 960°C for 10 to 14 hours in a CO2-free air (CFA) atmosphere. Claim 8 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the calcined material has an average crystallite size of 210 to 270 nm. Claim 9 A method for manufacturing a positive electrode active material for a lithium secondary battery, wherein, in claim 1, the ratio of the c-axis length to the a-axis length (c / a) obtained by X-ray diffraction analysis of the crystal of the calcined product is 4.9440 to 4.9520. Claim 10 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the heat treatment is performed in the range of 730 to 770℃. Claim 11 A method for manufacturing a positive electrode active material for a lithium secondary battery according to claim 1, wherein the positive electrode active material has a molar ratio (Li / Me) of lithium (Li) to a transition metal (Me) excluding lithium (Li) of 1.03 to 1.
07. Claim 12 A method for manufacturing a positive active material for a lithium secondary battery according to claim 1, wherein the positive active material is represented by the following chemical formula 1: [Chemical Formula 1]Li a Ni x Co y Mn z M1 k O2 (in the above chemical formula 1, 0.9 ≤ a ≤ 1.1, 0.3 ≤ x ≤ 0.73, 0.01 ≤ y ≤ 0.3, 0.01 ≤ z ≤ 0.4, 0 ≤ k ≤ 0.2, x + y + z + k = 1, and M1 is one or more elements selected from the group consisting of Al, Mg, Zr, Sn, Ca, Ge, Ti, Cr, Fe, Zn, Y, Ba, La, Ce, Sm, Gd, Yb, Sr, Cu and Ga). Claim 13 A lithium secondary battery comprising a positive electrode containing a positive active material manufactured according to claim 1; a negative electrode; and a non-aqueous electrolyte.
Citation Information
Patent Citations
Solid phase synthesis method of positive electrode material of nikel-rich lithium composite transition metal oxide in a form of a single particle, positive electrode material of nikel-rich lithium composite transition metal oxide in a form of a single particle formed therefrom, positive electrode and secondary lithium battery containing the same
KR1020220041032A
Postive electrode active material, positve electrode and lithium secondary battery comprising the same
KR1020250030415A