Method for Fabricating Silicone-Containing Copolymer Molded Article Having Hydrophilic Surface and Silicone Hydrogel Contact Lens Having Hydrophilic Surface
Patent Information
- Application Number
- LAP327
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2013-07-21
- Filing Date
- 2014-01-21
- Publication Date
- 2023-07-14
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
The present invention relates to a method for producing a silicone-containing copolymer molded article having a hydrophilic surface, and to a silicone hydrogel contact lens having a hydrophilic surface. When wearing contact lenses, the amount of oxygen supplied to the surface of the eye from the atmosphere decreases. Clinical results have indicated that this can lead to suppression of corneal epithelial cell division and corneal thickening. Therefore, in order to supply safer contact lenses, efforts are being made to improve the oxygen permeability of contact lens materials (hereinafter sometimes simply referred to as "materials"). Water-containing soft contact lenses are generally known for their comfortable fit due to their soft material. However, the oxygen permeability of conventional lenses depended on the lens's water content. Therefore, attempts were made to increase the water content of the material. However, simply increasing the water content of the material has limitations in improving oxygen permeability. Recently, however, silicone hydrogels obtained by polymerizing monomers including silicone monomers and siloxane macromonomers have been developed as a method to increase oxygen permeability without depending on water content, and these have been commercialized as lenses. Furthermore, the cast molding method is common for manufacturing soft contact lenses because it allows for the mass production of uniform products. Polypropylene is often used as the mold material for the cast molding method because it is inexpensive and easy to mold. However, polypropylene itself is hydrophobic. Therefore, when a silicone-containing copolymer is manufactured using a polypropylene mold, hydrophobic monomers become oriented in the area that comes into contact with the mold surface. As a result, the surface of the resulting polymer lens exhibits high hydrophobicity. When a lens surface exhibits hydrophobicity, lipid components from tears tend to adhere to it. This can lead to subjective symptoms such as the lens fogging up or blurred vision while wearing contact lenses. Alternatively, the adhesion of proteins and other substances on top of the lipid components may induce eye diseases. Therefore, in silicone-containing copolymers, it is known that hydrophilicity is imparted to the lens after polymerization by graft polymerization or plasma treatment. However, such post-treatment involves many complicated steps to impart hydrophilicity to the surface, making it unsuitable as a mass production method. On the other hand, as an alternative to imparting hydrophilicity through graft polymerization or plasma treatment, there is a method of incorporating a high molecular weight hydrophilic polymer as an internal wetting agent into the material. This method involves polymerizing a polymerization solution containing a high molecular weight hydrophilic polymer, such as polyvinylpyrrolidone, to obtain a material containing the high molecular weight hydrophilic polymer. The surface of the material obtained by this method exhibits hydrophilicity without the need for plasma treatment or graft polymerization. Incidentally, polymers obtained by polymerizing monomer mixtures generally retain unpolymerized monomers and oligomers. If these monomers and oligomers leach from the lens during wear, they can cause eye irritation. Therefore, it is common practice to extract monomers and oligomers from the polymer using alcohol or an aqueous alcohol solution after polymerization. The higher the concentration of alcohol used for extraction, the better the extraction efficiency, and the more unpolymerized monomers and oligomers can be removed in a short time. However, the high molecular weight hydrophilic polymers used to impart hydrophilicity are only physically entangled within the polymer's network structure. Therefore, if extraction is performed for a long time using alcohol or a high-concentration aqueous alcohol solution, the high molecular weight hydrophilic polymers are extracted from the polymer along with the unpolymerized monomers and oligomers. As a result, it becomes difficult to maintain good hydrophilicity after extraction. Furthermore, there is a method of manufacturing contact lenses using a mold made of a material other than polypropylene. For example, a resin mold for cast polymerization is used, which is molded using a resin having a water absorption rate in the range of 0.01 to 0.15% by mass and having a water contact angle on its surface in the range of 65 to 80 degrees. In this method, since the hydrophilic monomer is likely to be oriented in the portion in contact with the mold, it is possible to manufacture a contact lens having excellent surface water wettability. However, this method is not a preferable method. This is because the resin mold has a high water absorption rate of the constituent resin, resulting in poor shape stability after molding or difficulty in obtaining molding conditions and resin accuracy. In view of such a situation, various methods using hydrophilic monomers having a vinyl group, such as N-vinyl-2-pyrrolidone and N-methyl-N-vinylacetamide, which are widely used as raw materials for contact lenses, have been proposed for the purpose of easily improving the hydrophobicity of the surface of soft contact lenses using a silicone-containing copolymer. WO93 / 09154 (Japanese Patent Publication No. Hei 7-505169) (Patent Document 1) discloses a silicone-containing hydrogel obtained by curing a monomer mixture obtained by combining at least one vinyl-containing monomer, at least one acrylic-containing monomer, and at least one silicone-containing prepolymer. Here, examples of at least one vinyl-containing monomer include N-vinyl-2-pyrrolidone and N-methyl-N-vinylacetamide. Japanese Patent Application Laid-Open No. 2011-219512 (Patent Document 2) discloses a polymerizable composition containing [A] a polymerizable compound having an acryloyloxy group, not having a silicon atom, and having a glass transition temperature of 10°C or lower as its homopolymer, [B] a silicone compound having a polymerizable group, and [C] N-vinylpyrrolidinone as a monomer component. WO2008 / 061992 (Japanese Patent Publication No. 2010-510550) (Patent Document 3) discloses a silicone-containing copolymer obtained by polymerizing a polymerization solution comprising (A) a silicone-containing monomer represented by general formula I, (B) 3-methacryloyloxypropyltris(trimethylsiloxy)silane, (C) N-vinylpyrrolidone, and (D) at least one other nonionic hydrophilic monomer. WO2012 / 118680 (Patent Document 4) discloses a silicone-containing copolymer obtained by polymerizing a solution containing (a) a silicone monomer having polyethylene glycol groups represented by general formula (I), (b) at least one hydrophilic monomer having vinyl groups, and (c) a crosslinking agent having vinyl groups. US2013 / 0031873 A1 (Patent Document 5) discloses a method for producing a silicone-containing copolymer using a mold made of a nonpolar resin. The materials for lens preparation are polymerizable silicone monomers and non-silicone monomers, and the non-silicone monomers are described as monomers having a vinyl group, such as N-vinylpyrrolidone or N-vinyl-N-methylacetamide. Patent Document 1 uses N,N-dimethylacrylamide, a widely used amphiphilic monomer possessing both hydrophilic and lipophilic properties, in addition to N-vinyl-2-pyrrolidone and N-methyl-N-vinylacetamide. N,N-dimethylacrylamide exhibits excellent solubility in silicone monomers, allowing for the preparation of a homogeneous monomer mixture, and is therefore widely used as a component of silicone-containing copolymers. However, on the copolymer surface after polymerization, N,N-dimethylacrylamide imparts lipophilicity. This results in poor water wettability of the lens after water absorption and exhibits surface water repellency, which is undesirable (see the reproduction experiment results shown in Comparative Example 9 of this application). In the method described in Patent Document 2, component [A] plays a role in enhancing the compatibility between the silicone compound of component [B] and N-vinylpyrrolidinone of component [C]. However, because component [A] has poor hydrophilicity, and because TRIS (tris(trimethylsiloxy)silylpropyl methacrylate), which is used as the silicone compound of component [B] in the examples, does not contain hydroxyl groups or polyethylene glycol groups in its molecular structure, the resulting lens surface exhibits high water repellency. As a result, the obtained polymer is difficult to use as a contact lens without post-treatment such as plasma treatment or grafting (see the reproduction experiment results shown in Comparative Example 10 of this application). The monomers (A) and (B) used in the method described in Patent Document 3 are silicone monomers that do not contain hydroxyl groups or polyethylene glycol in their molecular structure. Because these silicone monomers exhibit high hydrophobicity, it is not possible to obtain a homogeneous monomer mixture with N-vinylpyrrolidone. Therefore, a homogeneous monomer mixture is prepared by adding a solvent. However, when a solvent is added to the monomer mixture, it becomes necessary to remove not only the unpolymerized monomers but also the solvent used after polymerization. As a result, this not only complicates the manufacturing process but is also not a preferable method considering the impact on the environment. Patent Document 4 discloses a silicone monomer having polyethylene glycol groups as general formula (I). However, the monomer used in the examples is only one with 4 repeating siloxane groups (m) and 1 repeating ethylene glycol group (n) (Si-1). Because this monomer has only one repeating ethylene glycol group, it has few hydrophilic sites in the silicone monomer structure, resulting in insufficient solubility with monomers having vinyl groups. Therefore, it is not possible to use the silicone component in a high blending ratio, and it is difficult to achieve high oxygen permeability. Patent Document 5 discloses a composition in an example in which a silicone monomer having a hydroxyl group in its molecular structure (SIGMA) and N-vinylpyrrolidone (NVP) are included as lens components (Examples 25, 26, 27, 28, 33, 48, 53, 55, 56). However, all of these compositions include the addition of solvents such as propanol, decanol, and hexanol. Therefore, after polymerization, it becomes necessary to remove not only the unpolymerized monomer but also the solvent used, which not only complicates the manufacturing process but is also not a preferable method considering the impact on the environment. The present invention aims to provide a method for producing a silicone-containing copolymer molded article having a hydrophilic surface by a cast molding method, without using a high molecular weight hydrophilic polymer and without requiring post-treatment to improve the water wettability of the polymer surface in the lens shape after polymerization, even when using a polypropylene mold. Furthermore, the invention aims to provide a silicone hydrogel contact lens having a hydrophilic surface, which can be obtained without using a high molecular weight hydrophilic polymer and without requiring post-treatment to improve the water wettability of the polymer surface in the lens shape after polymerization, even when using a polypropylene mold. [1] A method for producing a silicone-containing copolymer molded article having a hydrophilic surface and containing silicone monomer units, hydrophilic monomer units and crosslinkable monomer units, wherein the polymerization initiator has a half-life temperature of 10 hours (hereinafter abbreviated as T10) of 70°C or higher and 100°C or lower, and the polymerization is carried out in a P1 step of maintaining the temperature of the polymerization initiator contained in the monomer solution within a range from T10 to 35°C lower than T10 for 1 hour or more, and in a P2 step of maintaining the temperature of the polymerization initiator contained in the monomer solution at a temperature higher than T10 for 1 hour or more. [2] The method according to [1], wherein the maintenance temperature in step P1 is in the range of 10°C lower than T10 to 35°C lower than T10. [3] The method according to [1] or [2], wherein the maintenance temperature in step P2 is in the range of 5°C higher than T10 to 50°C higher than T10. [4] The method according to any one of [1] to [3], wherein the polymerization initiator is an azo polymerization initiator or an organic peroxide polymerization initiator. [5] The method according to any one of [1] to [4], wherein the content of the silicone monomer (a) units in the silicone-containing copolymer molded article is in the range of 20 to 56% by mass, the content of the hydrophilic monomer (b) units is in the range of 40 to 60% by mass, and the content of the crosslinkable monomer (c) units is in the range of 0.02 to 4% by mass. [6] The method according to any one of [1] to [5], wherein the silicone monomer (a) is at least one monomer selected from the group consisting of (a1) and (a2) below. (a1) One or more silicone monomers containing at least one hydroxyl group and one to four silicon atoms in one molecule; (a2) One or more silicone monomers containing at least one polyethylene glycol group and one to four silicon atoms in one molecule.[7] The method according to [6], wherein the silicone monomer (a1) is a monomer represented by the following general formula (a1-1) or (a1-2), [wherein R1, R2, R3 and R4 are methyl groups, R5 is a hydrogen atom or a methyl group, and a represents an integer from 1 to 3.], and the silicone monomer (a2) is a monomer represented by the following general formula (a2-1). [wherein R1, R2, R3 and R4 are methyl groups, a represents an integer from 1 to 3, and m is from 4 to 8. X in the formula is one selected from substituents represented by the following formula (Y1) or (Y2) (wherein R5 is a hydrogen atom or a methyl group). ] [8] The method according to any one of [1] to [7], wherein the hydrophilic monomer (b) is one or two selected from N-vinyl-2-pyrrolidone and N-vinyl-N-methylacetamide. [9] The method according to any one of [1] to [8], wherein the crosslinkable monomer (c) is at least one monomer selected from the group consisting of (c1), (c2), and (c3). (c1) One or more monomers containing two or more vinyl groups in one molecule, (c2) One or more monomers containing two or more allyl groups in one molecule, (c3) One or more monomers having two or more (meth)acrylate groups in one molecule.
[10] The method according to [9], wherein the monomer (c1) is one or more selected from 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, and triethylene glycol divinyl ether; the monomer (c2) is one or more selected from triallyl isocyanurate, trimethylolpropanediallyl ether, and pentaerythritol triallyl ether; and the monomer (c3) is one or more monomers selected from ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate.
[11] The method according to any one of [1] to
[10] , wherein the monomer solution further contains at least one auxiliary monomer selected from the group consisting of siloxane macromonomers, silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomers that do not contain silicon atoms in their molecular structure.
[12] The method according to any one of [1] to
[11] , wherein the hydrophilic surface of the silicone-containing copolymer molded article has a contact angle with pure water of 60° or less without any post-treatment to improve the surface wettability of the molded article surface after polymerization (however, the contact angle is the contact angle of a silicone hydrogel molded article in which the silicone-containing copolymer molded article has been hydrated.
[13] The method according to any one of [1] to
[12] , wherein the mold having a hydrophobic cavity surface is a double-sided cast mold for molding polyalkylene contact lenses, and the silicone-containing copolymer molded article is a precursor for silicone hydrogel soft contact lenses.
[14] A silicone-containing copolymer molded article prepared by any one of [1] to
[13] .
[15] A monomer unit consisting of at least one monomer unit selected from the group consisting of (a1) and (a2) below, the monomer unit of (b) below, and at least one monomer unit selected from the group consisting of (c1) to (c3) (however, (g) a monomer unit that does not contain a silicon atom in its molecular structure may be further included, and (g) the monomer that does not contain a silicon atom in its molecular structure is one selected from 2-hydroxyethyl (meth)acrylate, methacrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-methacryloyloxyethyl phosphorylcholine, etc. A silicone-containing copolymer molded article having a hydrophilic surface with a contact angle of 60° or less with respect to pure water (where the contact angle is the contact angle of a silicone hydrogel molded article made by impregnating a silicone-containing copolymer molded article with water), wherein the content of the silicone monomer (a1) to (a2) units is in the range of 20 to 56% by mass, the content of the monomer (b) unit is in the range of 40 to 60% by mass, the content of the monomer (c1) to (c3) units is in the range of 0.02 to 4% by mass, and the content of monomer units that do not contain silicon atoms in the molecular structure of (g) is in the range of less than 10% by mass. (a1) One or more units derived from a silicone monomer containing at least one hydroxyl group and one to four silicon atoms in one molecule and having a molecular weight of less than 900; (a2) One or more units derived from a silicone monomer containing at least one polyethylene glycol group and one to four silicon atoms in one molecule and having a molecular weight of less than 900; (b) One or more units derived from a hydrophilic monomer having a vinyl group; (c1) One or more monomer units containing two or more vinyl groups in one molecule; (c2) One or more monomer units containing two or more allyl groups in one molecule; (c3) One or more monomers having two or more (meth)acrylate groups in one molecule.
[16] A silicone-containing copolymer molded article containing at least one monomer unit selected from the group consisting of (a1) and (a2) below, the monomer unit of (b) below, at least one monomer unit selected from the group consisting of (c1) to (c3) below, and the siloxane macromonomer unit of (e), having a hydrophilic surface with a contact angle to pure water of 60° or less, and having a water content of 35% or more and less than 60% (wherein the contact angle and water content are the contact angle and water content of a silicone hydrogel molded article obtained by impregnating a silicone-containing copolymer molded article with water, respectively). (a1) One or more units derived from a silicone monomer containing at least one hydroxyl group and 1 to 4 silicon atoms in one molecule and having a molecular weight of less than 900; (a2) One or more units derived from a silicone monomer containing at least one polyethylene glycol group and 1 to 4 silicon atoms in one molecule and having a molecular weight of less than 900; (b) One or more units derived from a hydrophilic monomer having a vinyl group; (c1) One or more monomer units containing two or more vinyl groups in one molecule; (c2) One or more monomer units containing two or more allyl groups in one molecule; (c3) One or more monomers having two or more (meth)acrylate groups in one molecule; (e) One or more macromonomers of general formulas (C1) and (C2) In formula (C1), R7 is a hydrogen atom or a methyl group, r is 0 to 10, and p is 8 to 60. In formula (C2), R8 is a hydrogen atom or a methyl group, q is 9 to 15, and t is 0 to 3.
[17] A silicone-containing copolymer molded article according to
[16] , wherein r is 0 to 8, p is 8 to 50, q is 9 to 13, and t is 0 to 2.
[18] A silicone-containing copolymer molded article according to
[16] , wherein the siloxane macromonomer unit of (e) is (E5) or (E6) below. Macromer A
[19] The silicone monomer (a1) is a monomer represented by the following general formula (a1-1) or (a1-2), [wherein R1, R2, R3 and R4 are methyl groups, R5 is a hydrogen atom or a methyl group, and a represents an integer from 1 to 3.], a silicone-containing copolymer molded article according to any one of
[15] to
[18] , wherein the silicone monomer (a2) is a monomer represented by the following general formula (a2-1). [In the formula, R1, R2, R3 and R4 are methyl groups, a represents an integer from 1 to 3, and m is from 4 to 8. In the formula, X is one selected from substituents represented by the following formula (Y1) or (Y2) (In the formula, R5 is a hydrogen atom or a methyl group).]
[20] A silicone-containing copolymer molded article according to any one of
[15] to
[19] , wherein the hydrophilic monomer (b) is one or two selected from N-vinyl-2-pyrrolidone and N-vinyl-N-methylacetamide.
[21] A silicone-containing copolymer molded article according to any one of
[15] to
[20] , wherein the monomer (c1) is one or more selected from 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, and triethylene glycol divinyl ether; the monomer (c2) is one or more selected from triallyl isocyanurate, trimethylolpropanediallyl ether, and pentaerythritol triallyl ether; and the monomer (c3) is one or more monomers selected from ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate.
[22] A silicone-containing copolymer molded article according to any one of the claims
[16] to
[21] , wherein the content of the silicone monomer (a1) and (a2) units is in the range of 20 to 56% by mass, the content of the monomer (b) unit is in the range of 40 to 60% by mass, and the content of the monomer (c1), (c2), and (c3) units is in the range of 0.02 to 4% by mass.
[23] A silicone-containing copolymer molded article according to any one of the claims
[16] to
[22] , wherein the content of the siloxane macromonomer unit of (e) is 25% by mass or less.
[24] The silicone-containing copolymer molded article according to any one of
[16] to
[23] , further comprising at least one additional monomer unit selected from the group consisting of silicone monomer units that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomer units that do not contain silicon atoms in their molecular structure.
[25] The silicone-containing copolymer article according to any one of
[15] to
[24] , wherein the hydrophilic surface having a contact angle to pure water of 60° or less is obtained without any post-treatment to improve the surface wettability of the lens-shaped material after polymerization (however, the contact angle is the contact angle of a silicone hydrogel molded article in which the silicone-containing copolymer molded article has been hydrated.
[26] A silicone hydrogel soft contact lens precursor, which is a silicone-containing copolymer molded article according to any one of
[14] to
[25] , and has a contact lens shape.
[27] A silicone hydrogel soft contact lens obtained by hydrating the silicone hydrogel soft contact lens precursor according to
[26] with physiological saline or a soft contact lens storage solution.
[28] The soft contact lens according to
[27] , wherein the silicone hydrogel soft contact lens in a hydrated state has a water content of 35% or more and less than 60%.
[29] The soft contact lens according to
[27] or
[28] , wherein the silicone hydrogel soft contact lens in a hydrated state is a soft contact lens with a replacement frequency of up to one month.
[30] The soft contact lens according to
[29] , wherein the silicone hydrogel soft contact lens in a hydrated state is of the type with a replacement frequency of one day or two weeks.
[31] A packaged soft contact lens product comprising the soft contact lens according to any one of
[27] to
[30] and physiological saline or soft contact lens storage solution stored in a sealed container.
[015] A silicone-containing copolymer molded article containing at least one monomer unit selected from the group consisting of (a1) and (a2) below, the monomer unit of (b) below, and at least one monomer unit selected from the group consisting of (c1) to (c3), and having a hydrophilic surface with a contact angle to pure water of 60° or less (wherein the contact angle is the contact angle of a silicone hydrogel molded article in which a silicone-containing copolymer molded article has been impregnated with water). (a1) One or more units derived from a silicone monomer containing at least one hydroxyl group and one to four silicon atoms in one molecule; (a2) One or more units derived from a silicone monomer containing at least one polyethylene glycol group and one to four silicon atoms in one molecule; (b) One or more units derived from a hydrophilic monomer having a vinyl group; (c1) One or more monomer units containing two or more vinyl groups in one molecule; (c2) One or more monomer units containing two or more allyl groups in one molecule; (c3) One or more monomers having two or more (meth)acrylate groups in one molecule.
[016] The silicone-containing copolymer molded article according to
[015] , wherein the silicone monomer (a1) is a monomer represented by the following general formula (a1-1) or (a1-2), [wherein R1, R2, R3 and R4 are methyl groups, R5 is a hydrogen atom or a methyl group, and a represents an integer from 1 to 3.], and the silicone monomer (a2) is a monomer represented by the following general formula (a2-1). [wherein R1, R2, R3 and R4 are methyl groups, a represents an integer from 1 to 3, and m is from 4 to 8. X in the formula is one selected from substituents represented by the following formula (Y1) or (Y2) (wherein R5 is a hydrogen atom or a methyl group). ]
[017] The silicone-containing copolymer molded article according to
[015] or
[016] , wherein the hydrophilic monomer (b) is one or two selected from N-vinyl-2-pyrrolidone and N-vinyl-N-methylacetamide.
[018] A silicone-containing copolymer molded article according to any one of
[015] to
[017] , wherein the monomer (c1) is one or more selected from 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, and triethylene glycol divinyl ether; the monomer (c2) is one or more selected from triallyl isocyanurate, trimethylolpropanediallyl ether, and pentaerythritol triallyl ether; and the monomer (c3) is one or more monomers selected from ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate.
[019] A silicone-containing copolymer molded article according to any one of the claims
[015] to
[018] , wherein the content of the silicone monomer (a1) and (a2) units is in the range of 20 to 56% by mass, the content of the hydrophilic monomer (b) unit is in the range of 40 to 60% by mass, and the content of the monomer (c1), (c2), and (c3) units is in the range of 0.02 to 4% by mass.
[020] A silicone-containing copolymer molded article according to any one of the claims
[015] to
[019] , wherein the silicone-containing copolymer molded article further contains at least one additional monomer unit selected from the group consisting of siloxane macromonomer units, silicone monomer units that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomer units that do not contain silicon atoms in their molecular structure.
[021] A silicone-containing copolymer article according to any one of
[015] to
[020] , wherein the hydrophilic surface having a contact angle with pure water of 60° or less is obtained without any post-treatment to improve the surface wettability of the lens-shaped material after polymerization (however, the contact angle is the contact angle of a silicone hydrogel molded article in which a silicone-containing copolymer molded article has been hydrated).
[022] A silicone hydrogel soft contact lens precursor, which is a silicone-containing copolymer molded article according to any one of
[015] to
[021] , and has a contact lens shape.
[023] A silicone hydrogel soft contact lens obtained by hydrating the silicone hydrogel soft contact lens precursor described in
[022] with physiological saline or soft contact lens storage solution.
[024] The soft contact lens described in
[023] wherein the hydrated silicone hydrogel soft contact lens has a water content of 35% or more and less than 60%.
[025] The soft contact lens described in
[023] or
[024] wherein the hydrated silicone hydrogel soft contact lens is a soft contact lens with a replacement frequency of up to one month.
[026] The soft contact lens described in
[025] wherein the hydrated silicone hydrogel soft contact lens is of the type with a replacement frequency of one day or two weeks.
[027] A packaged soft contact lens product comprising the soft contact lens described in any one of
[023] to
[026] and physiological saline or soft contact lens storage solution stored in a sealed container. According to the present invention, even with silicone-containing copolymers obtained by curing using a double-sided cast mold of a hydrophobic material such as polypropylene, it is possible to provide a method for producing a silicone-containing copolymer molded article having a hydrophilic surface without post-treatment to improve the surface wettability of the lens-shaped material after polymerization, or without including a high molecular weight hydrophilic polymer to enhance the surface wettability. Furthermore, according to the present invention, it is possible to provide a silicone hydrogel contact lens having a hydrophilic surface. Figure 1 shows the ¹H-NMR spectrum of the compound obtained in Synthesis Example 1. Figure 2 shows the MALDI-TOF MS spectrum of the compound obtained in Synthesis Example 1. Figure 3 shows the ¹H-NMR spectrum of the compound obtained in Synthesis Example 2. Figure 4 shows the MALDI-TOF MS spectrum of the compound obtained in Synthesis Example 2. Figure 5 shows the results of contact angle measurement with pure water for the silicone-containing copolymer molded articles obtained in Examples 1 to 4 and Comparative Examples 1 and 2 (image). [Method for producing a silicone-containing copolymer molded article having a hydrophilic surface] The method for producing a silicone-containing copolymer molded article having a hydrophilic surface according to the present invention involves polymerizing a monomer solution containing (a) at least one silicone monomer, (b) at least one hydrophilic monomer having a vinyl group, (c) at least one crosslinkable monomer, and (d) at least one polymerization initiator in a mold cavity having a hydrophobic cavity surface, thereby producing a silicone-containing copolymer molded article having a hydrophilic surface and containing silicone monomer units, hydrophilic monomer units, and crosslinkable monomer units. Here, the polymerization initiator has a 10-hour half-life temperature (T10) of 70°C or higher and 100°C or lower. Furthermore, the polymerization includes a P1 step of maintaining the monomer solution at a temperature range from T10 to 35°C lower than T10 for at least 1 hour, and a P2 step of maintaining the monomer solution at a temperature higher than T10 for at least 1 hour. <Mold Type> The mold type used in the method of the present invention is a mold type having a hydrophobic cavity surface. The hydrophobicity of the hydrophobic cavity surface means, for example, that the contact angle with pure water is 90° or more. The hydrophobicity of the cavity surface refers to the hydrophobicity caused by the material of the cavity surface or the mold type, and it is not necessary to perform any special hydrophobic treatment. However, this does not mean to exclude molds that have undergone special hydrophobic treatment on the cavity surface, taking into consideration peelability after polymerization, etc. Furthermore, there is no upper limit to the contact angle of the hydrophobic cavity surface with pure water, but it is generally 120°. However, this does not mean to limit it to this angle. The mold can be a composite mold with convex and concave curvatures and can be made of materials such as metal or resin. However, it is preferable that the material has good release properties after polymerization and excellent solvent resistance and heat resistance. For molds having a hydrophobic cavity surface, it is preferable that they be made of resin, for example. Resin molds are preferable because they allow for easy production of molds with the shape required for the desired lens design. As for these resin materials, it is preferable to select from those with low molding shrinkage, good surface transfer properties from metal, and excellent dimensional accuracy and solvent resistance, and polypropylene is preferred due to its price and availability. However, it is not limited to polypropylene, and for example, polyethylene, polyethylene terephthalate, polymethylpentene, polysulfone, polyphenylene sulfide, cyclic olefin copolymer, ethylene vinyl alcohol copolymer, etc. may be used. <Monomer Solution> The monomer solution contains (a) a silicone monomer having at least one (meth)acryloyl group, (b) a hydrophilic monomer having at least one vinyl group, (c) at least one crosslinkable monomer, and (d) at least one polymerization initiator. <Silicone Monomer (a)> Silicone monomer (a) is a silicone monomer having a (meth)acryloyl group. Silicone monomer (a) has one (meth)acryloyl group per molecule. In this specification, (meth)acryloyl group means either a methacryloyl group or an acryloyl group. In this specification, it is appropriate that the silicone monomer has a molecular weight of less than 900. The reason will be explained later. Silicone monomer (a) is preferably a silicone monomer that contains one to four silicon atoms in one molecule and has at least one hydroxyl group or polyethylene glycol group in the molecule. By using a silicone monomer having at least one hydroxyl group or polyethylene glycol group in the molecule, a silicone-containing copolymer molded article with excellent hydrophilicity can be obtained. Such a silicone monomer may be, for example, the silicone monomer of (a1) or (a2) below. (a1) One or more silicone monomers containing at least one hydroxyl group and one to four silicon atoms in one molecule; (a2) One or more silicone monomers containing at least one polyethylene glycol group and one to four silicon atoms in one molecule. The silicone monomer (a1) can be, for example, a monomer represented by the following general formula (a1-1) or (a1-2). [In the formula, R1, R2, R3, and R4 are methyl groups, R5 is a hydrogen atom or a methyl group, and a represents an integer from 1 to 3.] The silicone monomer (a2) can be, for example, the monomer represented by the following general formula (a2-1). [In the formula, R1, R2, R3, and R4 are methyl groups, a represents an integer from 1 to 3, and m is from 4 to 8. In the formula, X is one selected from the substituents represented by the following formulas (Y1) or (Y2) (in the formula, R5 is a hydrogen atom or a methyl group).] Furthermore, the silicone monomers of (a1) or (a2) can also be represented by, for example, the following general formula (I). [In the formula, R1, R2, R3, and R4 are methyl groups, a represents an integer from 1 to 3, n represents 0 or 1, and m represents 0 or 4 to 8. However, when n is 1, m is 0, and when n is 0, m is 4 to 8 (a value as a repeated average). X in the formula is one selected from the substituents represented by the above formulas (Y1) to (Y2).] The above-mentioned silicone monomer is suitable in that it has a molecular weight of less than 900, in order to prevent a decrease in the strength of the resulting polymer and to prevent a low silicon content in each monomer molecule, thereby providing sufficient oxygen permeability. If there is a distribution in the number of repeating polyethylene glycol groups, it means that the number-average molecular weight calculated in polystyrene terms by gel permeation chromatography is less than 900. Preferably, the above-mentioned silicone monomer has a molecular weight in the range of 400 to 850. To obtain a molded article (e.g., a lens-shaped article) made of a silicone-containing copolymer having a hydrophilic surface, the above-mentioned silicone monomer is used. By having at least one hydroxyl group or polyethylene glycol group in the molecule, the compatibility with hydrophilic monomers (e.g., hydrophilic monomers having vinyl groups) in the polymerization solution is increased, and a homogeneous monomer mixture (polymerization solution) can be prepared without using a solvent. Silicone monomers with such structures are known compounds. For example, silicone monomers of type (a1) are disclosed in Japanese Patent Publication No. 55-15110 (US Patent No. 4139692), Japanese Patent Publication No. 63-163811, Japanese Patent Publication No. 2001-323024, Japanese Patent Publication No. 2002-113089 (US Patent No. 2004 / 014921), Japanese Patent Publication No. 2002-182167 and U.S. Patent No. 4,395,496, and silicone monomers of type (a2) are disclosed in Japanese Patent Publication No. 4-332760, etc., as one of the materials for contact lenses. The entire contents of these publications are incorporated herein by reference as particularly disclosed. The silicone monomer used in this invention is particularly preferably the monomer represented by the structural formulas A1 to A7 below. In formulas (A1) to (A7), R6 is a hydrogen atom or a methyl group, and in formulas (A4) to (A7), m is 4 to 8. In formulas (A1) and (A2), structural isomers such as those shown in formulas (B1) and (B2) below exist during the monomer synthesis process. In this invention, a mixture of structural isomers may be used, or a compound consisting of only one of the structures may be used. In formula (A3), although the structural formula is not shown, structural isomers exist, similar to formulas (A1) and (A2). [In the formula, R6 is a hydrogen atom or a methyl group] An example of a method for producing a silicone monomer having polyethylene glycol groups in its molecular structure is as follows. In this specification, a polyethylene glycol group refers to an ethylene glycol with an average number of repeating units (average value) in the range of 4 to 8. Specifically, one end of an ethylene glycol such as tetraethylene glycol, pentaethylene glycol, hexaethylene glycol, heptaethylene glycol, or octaethylene glycol is allylated, and then reacted with a tris(trimethylsiloxy)silyl group or a methylbis(trimethylsiloxy)silyl group by a hydrosilylation reaction. Next, a compound having a methacryloyl group on the hydroxyl group of one end (e.g., methacryl chloride, 2-isocyanatoethyl methacrylate) is reacted to obtain the desired silicone monomer. At this time, it is difficult to obtain a glycol with a polyethylene glycol repeating unit of 4 or more as a single product, and it is common for glycols with multiple repeating units to be mixed together. The monomers A4 to A7 used in this invention may have a distribution of m values, with an average value of 4 to 8. Alternatively, when synthesizing the silicone monomer, the precursor glycols may be separated by column preparation or other means to obtain a single repeating number (for example, when m is 4, other numbers (e.g., 3 or 5) are not included) before being used in the synthesis, thereby eliminating the distribution of the glycol repeating number. In order to reduce variations in various physical properties of the resulting lens, including mechanical strength and water wettability, it is preferable that the polyethylene glycol repeating number is undistributed and a single repeating number. When m is 4 or greater, a homogeneous monomer mixture can be obtained due to its excellent compatibility with other copolymer components. When m is 8 or less, it is preferable because the molecular structure does not become too long, thus preventing a decrease in the mechanical strength of the lens. In this specification, "average value" is applied when the number of repeating polyethylene glycol groups in the silicone monomer structure has a distribution, and refers to the number of repeating groups calculated using the peak integral intensity ratio of ethylene oxide units by 1H-NMR analysis of the starting material precursor or final structure. In the silicone-containing copolymer molded article of the present invention and the method for manufacturing a contact lens produced from this silicone-containing copolymer molded article, as described later, the content of the silicone monomer in the monomer solution is preferably, for example, 20 to 56% by mass, relative to the total amount of all monomers. By setting the silicone monomer content to 20% by mass or more, it becomes easier to prepare a monomer mixture that is homogeneous with hydrophilic monomers (hydrophilic monomers having vinyl groups). On the other hand, by setting it to 56% by mass or less, it is possible to prevent the final contact lens from having a hard texture. The silicone monomer content is more preferably 20 to 55% by mass, and even more preferably 25 to 52% by mass. <Hydrophilic monomer (b)> The hydrophilic monomer is a hydrophilic monomer having a vinyl group. By using a hydrophilic monomer having a vinyl group, it is possible to improve the water wettability of the final lens surface. The hydrophilic monomer having a vinyl group can be, for example, one or two selected from N-vinyl-2-pyrrolidone and N-vinyl-N-methylacetamide. In the method for preparing a silicone-containing copolymer molded article of the present invention, a hydrophilic monomer having a vinyl group is used. In the present invention, a silicone-containing copolymer molded article having a hydrophilic surface can be easily obtained without special post-treatment or the use of a high molecular weight hydrophilic polymer after polymerization, and even when polypropylene is used as the mold material. In the silicone-containing copolymer molded article of the present invention and the method for manufacturing a contact lens produced from this silicone-containing copolymer molded article, as described later, the content of hydrophilic monomers having vinyl groups in the monomer solution is preferably 40 to 60% by mass of the total amount of all monomers. By setting the content of hydrophilic monomers having vinyl groups to 40% by mass or more, the hydrophilicity of the lens surface can be increased, and by setting it to 60% by mass or less, a decrease in the mechanical strength of the lens can be prevented. The content of hydrophilic monomers having vinyl groups is more preferably 45 to 60% by mass, and even more preferably 45 to 55% by mass. <Crosslinkable monomer (c)> Crosslinkable monomers can crosslink hydrophilic monomers having vinyl groups or monomers having (meth)acrylate groups, thereby imparting heat resistance and solvent resistance to copolymers. The content of the crosslinkable monomer in the monomer solution is appropriately in the range of 0.02 to 4% by mass relative to the total amount of all monomers. The crosslinkable monomer may be, for example, at least one monomer selected from the group consisting of (c1), (c2), and (c3): (c1) one or more monomers containing two or more vinyl groups in one molecule; (c2) one or more monomers containing two or more allyl groups in one molecule; (c3) one or more monomers having two or more (meth)acrylate groups in one molecule. In this specification, "(meth)acrylate group" means acrylate group or methacrylate group. The crosslinkable monomer (c1) contains two or more vinyl groups in one molecule and is therefore effective in crosslinking the hydrophilic monomer (b). The crosslinkable monomer (c1) can be, for example, one or more selected from 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, and triethylene glycol divinyl ether. The crosslinkable monomer (c2) contains two or more allyl groups in one molecule and is therefore effective in crosslinking the hydrophilic monomer (b). The crosslinkable monomer (c2) can be one or more selected from, for example, triallyl isocyanurate, trimethylolpropanediallyl ether, and pentaerythritol triallyl ether. The crosslinkable monomer (c3) has a "(meth)acrylate" group and therefore tends to selectively crosslink with silicone monomers having a "(meth)acrylate" group belonging to monomer (a). Furthermore, monomer (c3) also tends to selectively crosslink with siloxane macromonomers, silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomers that do not contain silicon atoms in their molecular structure, as described later. Monomer (c3) can be one or more selected from, for example, ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate. The content of crosslinkable monomers (c1) and (c2) is preferably in the range of 0.02 to 1% by mass, based on the total amount of all monomers. When the amount of crosslinkable monomers (c1) and (c2) used is 0.02% by mass or more, heat resistance and solvent resistance are imparted, and when it is 1% by mass or less, the resulting silicone-containing copolymer can be prevented from becoming brittle. The content of crosslinkable monomers (c1) and (c2) is more preferably 0.1 to 0.8% by mass, based on the total amount of all monomers. When the amount of crosslinkable monomers (c3) used is 0.1% by mass or more, mechanical strength and durability are imparted, and when it is 3% by mass or less, the resulting soft contact lenses can be prevented from becoming brittle. The content of crosslinkable monomers (c3) is more preferably 0.2 to 2% by mass. The crosslinkable monomers (c1), (c2), and (c3) may be used individually or in combination, and the total amount of each monomer when used in combination is in the range of 0.02 to 4% by mass. <Polymerization Initiator (d)> The polymerization initiator has a 10-hour half-life temperature (T10) of 70°C or higher and 100°C or lower. By using a polymerization initiator within the above T10 range, a silicone-containing copolymer molded article having a hydrophilic surface, which is the objective of the present invention, can be obtained from a monomer solution containing monomers (a), (b), and (c) through a two-step polymerization process described later: step P1 (maintaining at a temperature within the range of the polymerization initiator's T10 to 35°C lower than T10 for 1 hour or more) and step P2 (maintaining at a temperature higher than the polymerization initiator's T10 for 1 hour or more). According to the inventors' findings, when a polymerization initiator with a T10 of less than 70°C was used in the two-stage polymerization process, only molded articles with deformed lens shapes were obtained, making them unsuitable for use as contact lenses. Alternatively, even if a lens-shaped molded article was obtained, the relative composition ratio of silicon atoms on the lens surface increased, resulting in poor surface wettability (see experimental results for Comparative Examples 1, 2, 4, and 5 of this application). Furthermore, when a polymerization initiator with a T10 exceeding 100°C was used in the two-stage polymerization process, the resulting molded articles were brittle and could not be removed from the mold (see experimental results for Comparative Examples 3 and 6 of this application). Examples of polymerization initiators include azo polymerization initiators or organic peroxide polymerization initiators having a T10 of 70°C or higher and 100°C or lower. Specific examples of polymerization initiators with a T10 of 70°C or higher and 100°C or lower include the following compounds: (d1) 1,1'-Azobis(cyclohexane-1-carbonitride) [Wako Pure Chemical Industries, Ltd., CAS: 2094-98-6, T10: 88°C (in toluene)], (d2) t-butylperoxy-2-ethylhexanoate [NOF Corporation, trade name: Perbutyl O, CAS: 3006-82-4, T10: 72.1°C (in benzene)], (d3) 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane [NOF Corporation, trade name: PerhexaTMH, CAS: 104066-39-9, T10: 86.7°C (in benzene)], (d4) 1,1-di(t-hexylperoxy)cyclohexane [NOF Corporation, trade name: Perhexa HC, CAS: 27215-08-3, 22743-71-1, T10: 87.1℃ (in benzene)], (d5) t-hexylperoxyisopropyl carbonate [NOF Corporation, trade name: Perhexyl I, CAS: 132929-84-1, T10: 95.0℃ (in benzene)], (d6) t-butylperoxy-3,5,5-trimethylhexanoate [NOF Corporation, trade name: Perbutyl 355, CAS: 13122-18-4, T10: 97.1℃ (in benzene)], (d7) t-butyl peroxylaurate [NOF Corporation, trade name: Perbutyl L, CAS: 2123-88-8, T10: 98.3℃ (in benzene)]. The T10 of the polymerization initiator can be calculated by measurement, but the manufacturer's published value may also be referred to. The content of the polymerization initiator can be determined by considering the composition of the monomer mixed solution and the conditions of the polymerization process, and for example, it can be in the range of 0.1 to 1% by mass of the total amount of the monomer mixed solution. Preferably, it is in the range of 0.2 to 0.9% by mass. In the method for preparing silicone-containing copolymer molded articles of the present invention, the above polymerization initiator and polymerization conditions are used in combination. The reactivity of monomers varies greatly depending on the functional group, and it is known that the reactivity differs significantly between monomers having methacryloyl or acryloyl groups and monomers having vinyl groups. The half-life of the polymerization initiator is a convenient indicator that represents the decomposition rate at a constant temperature. Optimization of the polymerization reaction is also performed by considering T10. However, when producing copolymers using a mixture of multiple monomers, optimization cannot be easily achieved solely from T10. Furthermore, the direction of optimization differs depending on the selection of physical properties that serve as indicators for optimization. In the present invention, as a result of various studies from the viewpoint of obtaining silicone-containing copolymer molded articles having a hydrophilic surface, although the detailed mechanism is not necessarily clear, it was found that silicone-containing copolymer molded articles having a hydrophilic surface can be obtained by using a polymerization initiator with a T10 in the range of 70°C to 100°C, and further by going through a polymerization process including the P1 and P2 steps described later. While there is no intention to be overly theoretical, it is presumed that in step P1, the polymerization reaction proceeds relatively slowly due to the slow decomposition rate of the initiator, forming blocks in which similar monomers preferentially polymerize. Subsequently, in step P2, curing proceeds while maintaining these blocks to some extent. As a result, it is presumed that the copolymer structure is divided into parts rich in monomers having methacryloyl or acryloyl groups and parts rich in hydrophilic monomers having vinyl groups. Consequently, when the resulting copolymer is hydrated, the parts rich in hydrophilic monomers having vinyl groups are more easily exposed on the copolymer surface, thus yielding a silicone-containing copolymer molded product with a hydrophilic surface. Furthermore, Patent Document 4 describes 1,1'-azobis(cyanocyclohexane) as a polymerization initiator (page 14, line 3). 1,1'-azobis(cyanocyclohexane) has a T10 of 88°C. However, it is only listed here as an example of an azo-based initiator. The polymerization initiator used in the examples is only V-64, 2,2'-azobis-2-methylpropanenitrile [CAS: 78-67-1, T10: 65°C] (T10 less than 70°C). Moreover, Patent Document 4 does not even suggest that a silicone-containing copolymer molded article having a hydrophilic surface can be obtained by using a polymerization initiator with a T10 of 70°C or higher and 100°C or lower, and by going through a polymerization process including the P1 and P2 steps described later. Furthermore, in Patent Document 5, only 2,2'-azobis(2,4-dimethylpentanenitrile) [CAS: 4419-11-8, T10: 51°C] and azobisisobutyronitrile [CAS: 78-67-1, T10: 65°C] are used as polymerization initiators in the examples. Patent Document 5 does not even suggest that a silicone-containing copolymer molded article having a hydrophilic surface can be obtained by using a polymerization initiator with a T10 of 70°C or higher and 100°C or lower, and by going through a polymerization process including the P1 and P2 steps described later. The monomer solution may contain at least one monomer selected from the group consisting of (a1) and (a2) below, at least one monomer selected from the group consisting of (b), and at least one monomer selected from the group consisting of (c1), (c2), and (c3). (a1) One or more silicone monomers containing at least one hydroxyl group and one to four silicon atoms in one molecule, (a2) One or more silicone monomers containing at least one polyethylene glycol group and one to four silicon atoms in one molecule, (b) One or more hydrophilic monomers having vinyl groups, (c1) One or more monomers containing two or more vinyl groups in one molecule, (c2) One or more monomers containing two or more allyl groups in one molecule, (c3) One or more monomers having two or more (meth)acrylate groups in one molecule. The content of the silicone monomer (a1) to (a2) units in the silicone-containing copolymer molded article is in the range of 20 to 56% by mass, the content of the hydrophilic monomer (b) unit is in the range of 40 to 60% by mass, and the content of the crosslinkable monomer (c1) to (c3) units is in the range of 0.02 to 4% by mass. The monomer solution may further contain at least one auxiliary monomer selected from the group consisting of siloxane macromonomers, silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomers that do not contain silicon atoms in their molecular structure. In this specification, siloxane macromonomer means a monomer with a molecular weight of 900 or more. In addition to the four components (a) to (d) above, the silicone-containing copolymer of the present invention may also contain siloxane macromonomers, silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomers that do not contain silicon atoms in their molecular structure, in order to improve oxygen permeability. Examples of siloxane macromonomers include those described in Japanese Patent Publication No. 2001-311917, Japanese Patent Publication No. 2001-183502, and Japanese Patent Publication No. 11-502949. The entire contents of these publications are incorporated herein by reference as particularly disclosed. Macromonomers of the following general formulas (C1) and (C2) are particularly preferred. When removing contact lenses from a mold after polymerization in the mold, if a method is used in which mechanical force is applied to the mold to remove the lenses, it is preferable to add siloxane macromonomers having a urethane structure as a component because this imparts impact resistance to the lenses, allowing them to be removed from the mold without damage. In the above formula (C1), R7 is a hydrogen atom or a methyl group, r is 0 to 10, and p is 8 to 60. More preferably r is 0 to 8, and even more preferably 0 to 5. Also, more preferably p is 8 to 50, and even more preferably 8 to 40. In formula (C2), R8 is a hydrogen atom or a methyl group, q is 9 to 15, and t is 0 to 3. More preferably q is 9 to 13, and even more preferably 9 to 12. t is preferably 0 to 2. Examples of silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure include one or more monomers such as tris(trimethylsiloxy)-γ-methacryloxypropylsilane, tris(trimethylsiloxy)-γ-acryloxypropylsilane, 3-[tris(trimethylsiloxy)silyl]propyl methacryloyloxyethyl succinate, methacryloxymethylbis(trimethylsiloxy)methylsilane, 3-methacryloxypropylbis(trimethylsiloxy)methylsilane, methacryloxymethyltris(trimethylsiloxy)silane, methacryloxypropylbis(trimethylsiloxy)silanol, and mono(meth)acryloyl-terminated polydimethylsiloxane represented by the following general formula (C3). In formula (C3), R8 is a hydrogen atom or a methyl group, q is 4 to 8, and t is 0 to 3. Preferably q is 4 to 6. Preferably t is 0 to 2. These siloxane macromonomers and silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure can be used in a range of 0 to 25% by mass relative to the monomer solution. By limiting the content of these siloxane macromonomers and silicone monomers to 25% by mass or less, a homogeneous monomer mixture solution can be prepared without the monomer mixture becoming cloudy, and furthermore, deterioration of the wettability of the lens surface can be prevented. Examples of monomers that do not contain silicon atoms in their molecular structure include one or more monomers selected from 2-hydroxyethyl (meth)acrylate, methacrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, and 2-methacryloyloxyethyl phosphorylcholine, and can be used in amounts less than 10% by mass. In particular, N,N-dimethylacrylamide, which is often used as a component of silicone-containing copolymers, is preferably not used because it worsens the water wettability of the lens surface after polymerization. By keeping the content of these monomers below 10%, a decrease in the silicone content in the monomer mixture can be prevented, and as a result, high oxygen permeability can be provided. The content of monomers that do not contain silicon atoms in their molecular structure is more preferably 2 to 8% by mass, and even more preferably 3 to 7% by mass. In this specification, "(meth)acrylate" means both acrylate and methacrylate. Furthermore, the silicone-containing copolymer molded article of the present invention may contain, for example, polymerizable ultraviolet absorbers and polymerizable dyes as copolymerization components to impart ultraviolet absorption ability to the resulting soft contact lenses or to color them for the purpose of improving visibility. Specific examples of the polymerizable ultraviolet absorbers include 5-chloro-2-[2-hydroxy-5-(β-methacryloyloxyethyl carbamoyloxyethyl)]phenyl-2H-benzotriazole, 2-[2-hydroxy-5-(β-methacryloyloxyethyl carbamoyloxyethyl)]phenyl-2H-benzotriazole, 5-chloro-2-[2-hydroxy-4-(p-vinylbenzyloxy-2-hydroxypropyloxy)]phenyl-2H-benzotriazole, 4-methacryloxy-2-hydroxybenzophenone, and 2-(2'-hydroxy-5'-methacryloxyethylphenyl)-2H-benzotriazole. Specific examples of the polymerizable dyes include 1,4-bis(4-vinylbenzylamino)anthraquinone, 1-p-hydroxybenzylamino-4-p-vinylbenzylaminoanthraquinone, 1-anilino-4-methacryloylaminoanthraquinone, 1,4-bis[4-(2-methacryloxyethyl)phenylamino]-9,10-anthraquinone, and 4-(5-hydroxy-3-methyl-1-phenyl-4-pyrazolylmethylene)-3-methacrylamino-1-phenyl-2-pyrazolin-5-one. In addition, phthalocyanine dyes such as AlcianBlue8GX and AlcianGreen2GX can also be included in the contact lens material of the present invention as colorants. The content of the polymerizable ultraviolet absorber and polymerizable dye is affected by the thickness of the lens made from this material, so it is appropriate to have a content of 5% by mass or less, particularly preferably 0.02 to 3% by mass, relative to the total amount of copolymer components. Limiting the amount used to 5% by mass or less prevents a decrease in the mechanical strength of the resulting contact lens and is also preferable from the standpoint of safety for contact lenses that come into direct contact with the body. <Polymerization Process> The monomer solution is polymerized in a mold-type cavity having a hydrophobic cavity surface. Polymerization is carried out in two steps: Step P1, in which the monomer solution is maintained at a temperature range from T10 to 35°C lower than T10 for at least one hour, and Step P2, in which the monomer solution is maintained at a temperature higher than T10 for at least one hour. In this specification, polymerization in Step P1 is sometimes referred to as "gelation," and polymerization in Step P2 is sometimes referred to as "cure." <Step P1> The polymerization initiator contained in the monomer solution is maintained at a temperature range of T10 to 35°C lower than T10 for at least 1 hour. The maintenance temperature in Step P1 is preferably in the range of 10°C lower than T10 to 35°C lower than T10, more preferably in the range of 15°C lower than T10 to 35°C lower than T10, and even more preferably in the range of 20°C lower than T10 to 35°C lower than T10. <Step P2> Step P2 is performed after Step P1, in which the polymerization initiator contained in the monomer solution is maintained at a temperature higher than T10 for 1 hour or more. The maintenance temperature in Step P2 is preferably in the range of 5°C higher than T10 to 50°C higher than T10, more preferably in the range of 10°C higher than T10 to 50°C higher than T10, and even more preferably in the range of 15°C higher than T10 to 50°C higher than T10. The monomer solution consisting of the above components is polymerized after being injected, for example, into a contact lens manufacturing mold having a contact lens shape. When injecting the monomer solution, the mold may be used immediately after molding, or it may be used after being stored for about 10 to 40 hours to stabilize the curvature of the mold. Alternatively, before using the mold, the mold surface may be sufficiently depressurized to remove moisture, oxygen, and other substances that may affect the reaction, and then purged with an inert gas such as nitrogen or argon before injecting the monomer solution into the mold. Furthermore, when injecting the monomer solution, the monomer solution may be used after removing dissolved oxygen by bubbling it with an inert gas such as nitrogen or argon, or it may be used without removing the dissolved oxygen. As for the polymerization method, it is preferable to use thermal polymerization with the aforementioned polymerization initiator. The heating conditions are as described above. The atmosphere during polymerization may be air, but it is preferable to polymerize in an inert gas atmosphere such as nitrogen or argon in order to improve the polymerization rate of monomers and reduce the amount of unreacted monomers. When polymerizing in an inert gas atmosphere such as nitrogen or argon, it is preferable that the pressure inside the polymerization furnace be 1 kgf / cm2 or less. Furthermore, polymerization can be carried out in the presence of a suitable diluent. A suitable diluent can be any that dissolves homogeneously with the monomer components used, such as alcohols (e.g., ethanol, tert-butanol, n-hexanol, octanol) or esters (e.g., ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, butyl propionate). Using a diluent can facilitate injection into a mold due to a decrease in the viscosity of the monomer mixture, and can also reduce the elastic modulus of the resulting lens. The amount of diluent used is preferably 20% by mass or less of the total amount of monomer components. The polymerization schedule involves maintaining the monomer solution at a temperature range of T10 to 35°C lower than T10 for at least one hour during step P1. The holding time in step P1 is preferably 5 hours or more and 14 hours or less. A holding time of 5 hours or more makes it easier to obtain a good hydrophilic surface when transitioning to curing, and when polymerized into a lens shape, it makes it easier to obtain a circular lens after swelling. However, if it exceeds 14 hours, the total polymerization time (the combined time of "gelation" and "curing") becomes too long, resulting in poor production efficiency, so it is preferable to keep it at 14 hours or less. The holding time for "gelation" is more preferably 6 to 12 hours. Note that the maintenance time (holding time) does not include the heating time to reach the maintenance (holding) temperature in step P1, but the heating time within the maintenance (holding) temperature range is included in the maintenance time (holding time). Similarly, this refers to the time excluding the heating time from the maintenance (holding) temperature in process P1 to the maintenance (holding) temperature in process P2, while the heating time within the maintenance (holding) temperature range is included in the maintenance time (holding time is synonymous). In step P2, the maintenance time at a temperature higher than T10 of the polymerization initiator is 1 hour or more, and preferably in the range of 4 to 10 hours from the viewpoint of completing polymerization. In both steps P1 and P2, the temperature can be maintained without changing it during each step, or it can be varied within a predetermined range during each step. For example, in step P1, the temperature can be gradually increased within the range of T10 of the polymerization initiator to a temperature 35°C lower than T10. More specifically, for example, (i) the temperature can be maintained at 30°C lower than T10 for a certain time t1, and then (ii) the temperature can be maintained at 20°C lower than T10 for a further time t2. In this case, the maintenance time of 1 hour or more in step P1 means the time from the start of heating in (i) to the end of heating in (ii), including the time for raising the temperature from (i) to (ii). Similarly, in step P2, the temperature can also be gradually increased at a temperature higher than T10 of the polymerization initiator. More specifically, for example, (iii) the temperature can be maintained at 10°C higher than T10 for a certain period of time t1, and then (iv) the temperature can be maintained at 20°C higher than T10 for another period of time t2. In this case, the maintenance time of 1 hour or more in step P2 means the time from the start of heating in (iii) to the end of heating in (iv), including the time it takes to raise the temperature from (iii) to (iv). More specifically in step P2, the temperature can be gradually raised to a maximum temperature of 130°C or less, and then further heated for, for example, 4 to 10 hours to complete the polymerization. The polymerization schedule (set temperature and time) in steps P1 and P2 is not intended to be limited to the above example and can be selected as appropriate. After polymerization, the copolymer molded product (e.g., lens shape) removed from the mold can be used to extract and remove unpolymerized monomers and oligomers using a solvent (e.g., methanol, ethanol, isopropyl alcohol, methanol aqueous solution, ethanol aqueous solution, isopropyl alcohol aqueous solution, etc.). Subsequently, by immersing the product in physiological saline or a soft contact lens storage solution, the desired hydrated silicone hydrogel molded product (e.g., contact lens) can be obtained. The water content of the silicone hydrogel molded article of the present invention is preferably 35% or more and less than 60%. More preferably, the water content is 35% or more and 55% or less, and even more preferably, 35% or more and 50% or less. The hydrophilic surface of the hydrated silicone hydrogel molded article obtained by the manufacturing method of the present invention has a contact angle with pure water of 60° or less, without any post-treatment to improve the surface wettability of the molded article after polymerization. Preferably, the contact angle with pure water is 55° or less, more preferably 50° or less, and even more preferably 45° or less. There is no particular lower limit to the contact angle with pure water, but in reality it is 10° or more or 15° or more. In this invention, "special post-treatment" refers to methods for improving the water wettability of the contact lens surface, such as plasma treatment, graft treatment, base treatment, acid treatment, and biocompatible LbL coating as disclosed in Japanese Patent Publication No. 2005-538767. A hydrophilic surface is defined as having a contact angle of 60° or less when measured using the droplet method with pure water. When the mold having a hydrophobic cavity surface is a double-sided cast mold for molding polyalkylene contact lenses, the silicone hydrogel molded product is a silicone hydrogel soft contact lens. <Silicone-containing copolymer molded articles and silicone hydrogel molded articles> The present invention encompasses silicone-containing copolymer molded articles and silicone hydrogel molded articles prepared by the method of the present invention described above. Silicone hydrogel molded articles include silicone hydrogel soft contact lenses. Furthermore, the present invention relates to a silicone-containing copolymer molded article having a hydrophilic surface containing at least one monomer unit selected from the group consisting of the following (a1) and (a2), a monomer unit of the following (b), and at least one monomer unit selected from the group consisting of (c1) to (c3), and having a contact angle with pure water of 60° or less (however, the contact angle is the contact angle of the silicone hydrogel molded article in which the silicone-containing copolymer molded article contains water). (a1) One or more units derived from a silicone monomer containing at least one hydroxyl group and 1 to 4 silicon atoms in one molecule, (a2) One or more units of a silicone monomer unit containing at least one polyethylene glycol group and 1 to 4 silicon atoms in one molecule, (b) One or more units derived from a hydrophilic monomer having a vinyl group, (c1) One or more units of a monomer unit containing two or more vinyl groups in one molecule, (c2) One or more units of a monomer unit containing two or more allyl groups in one molecule, (c3) One or more units of a monomer having two or more (meth)acrylate groups in one molecule. The silicone monomer (a1) can be, for example, a monomer represented by the following general formula (a1-1) or (a1-2). 0034 [In the formula, R1, R2, R3, and R4 are methyl groups, R5 is a hydrogen atom or a methyl group, and a represents an integer of 1 to 3.] The silicone monomer (a2) can be, for example, a monomer represented by the following general formula (a2-1). 0035 [In the formula, R1, R2, R3, and R4 are methyl groups, a represents an integer of 1 to 3, and m is 4 to 8. X in the formula is one selected from the substituents represented by the following formula (Y1) or (Y2) (in the formula, R5 is a hydrogen atom or a methyl group).] 0036 The hydrophilic monomer (b) can be one or two selected from N-vinyl-2-pyrrolidone and N-vinyl-N-methylacetamide. The crosslinkable monomer (c1) is, for example, one or more selected from 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, and triethylene glycol divinyl ether. The crosslinkable monomer (c2) is, for example, one or more selected from triallyl isocyanurate, trimethylolpropane diallyl ether, and pentaerythritol triallyl ether. The crosslinkable monomer (c3) is, for example, one or more selected from ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate. The content of the silicone monomer (a1) and (a2) units is in the range of 20 to 56% by mass, the content of the hydrophilic monomer (b) units is in the range of 40 to 60% by mass, and the content of the monomers (c1), (c2), and (c3) units is in the range of 0.02 to 4% by mass. The silicone-containing copolymer molded article further contains at least one additional monomer unit selected from the group consisting of siloxane macromonomer units, silicone monomer units that do not contain a hydroxyl group or a polyethylene glycol group in the molecular structure, and monomer units that do not contain a silicon atom in the molecular structure, and the content of the additional monomer unit can be appropriately determined according to the type of the monomer. Each component of the silicone-containing copolymer molded article is the same as that described in the method for producing the silicone-containing copolymer molded article of the present invention. The hydrophilic surface of the water-containing silicone hydrogel molded article is a hydrophilic surface having a contact angle of 60° or less with respect to pure water, and is obtained without performing a post-treatment for improving the surface water wettability of the lens-shaped material after polymerization. The contact angle with respect to pure water is the contact angle obtained by measuring the contact angle by the droplet method using pure water. <Precursor for Silicone Hydrogel Soft Contact Lenses> The present invention includes a precursor for silicone hydrogel soft contact lenses, which is a silicone-containing copolymer molded article of the present invention and has a contact lens shape. <Soft Contact Lenses> The present invention includes soft contact lenses obtained by immersing the silicone hydrogel soft contact lens precursor of the present invention in physiological saline or soft contact lens storage solution to a hydrated state. The soft contact lens, in the aforementioned water-containing state, may have a water content of, for example, 35% or more and less than 60%. Preferably, the water content may be 38% or more and 55% or less, and more preferably 40% or more and 50% or less. The water-containing soft contact lenses of the present invention can be soft contact lenses with a replacement frequency of up to one month. The replacement frequency can be any number of days within one month; for example, the water-containing soft contact lenses of the present invention can be of the daily type (so-called one-day type) or the two-week type. However, this is not intended to limit the possibilities. <Packaged Soft Contact Lens Products> The present invention includes packaged soft contact lens products in which the soft contact lenses and physiological saline solution or soft contact lens storage solution are stored in a sealed container. Existing soft contact lens storage solutions and sealed containers can be used as they are. The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Ingredients Used] The names and abbreviations of the chemical substances used in the following examples and comparative examples are shown below. (a) Silicone monomer having at least one hydroxyl group or polyethylene glycol group in its molecular structure 3Si-GMA: (3-methacrylate-2-hydroxypropoxy)propylbis(trimethylsiloxy)methylsilane [CAS: 69861-02-5] The relative content ratio in 3Si-GMA was 75% by mass of structure (D1) and 25% by mass of structure (D2) below. 4Si-GMA: (3-methacrylateoxy-2-hydroxypropoxy)propyltris(trimethylsiloxy)silane [CAS: 71223-14-8] The relative content ratio in 4Si-GMA was 82% by mass of structure (D3) and 18% by mass of structure (D4). 4Si-4PEG: Silicone monomer obtained in Synthesis Example 1 4Si-6PEG: Silicone monomer obtained in Synthesis Example 2 (b) Hydrophilic monomers having a vinyl group NVP: N-vinyl-2-pyrrolidone [CAS: 88-12-0] VMA: N-vinyl-N-methylacetamide [CAS: 3195-78-6] (c) Crosslinkable monomers having two or more vinyl or allyl groups in the molecule TAIC: Triallyl isocyanurate [CAS: 1025-15-6] BDVE: 1,4-butanediol divinyl ether [CAS: 3891-33-6] TEGDVE: Triethylene glycol divinyl ether [CAS: 765-12-8] (c) Crosslinkable monomers having two or more (meth)acrylate groups EDMA: Ethylene glycol dimethacrylate [CAS: 97-90-5] 4G: Tetraethylene glycol dimethacrylate [CAS: 109-17-1] (d) Polymerization initiators with a 10-hour half-life temperature of 70°C or higher and 100°C or lower V-40: 1,1'-azobis(cyclohexane-1-carbonitride) Wako Pure Chemical Industries, Ltd., CAS: 2094-98-6, 10-hour half-life temperature: 88°C Perbutyl O: t-butylperoxy-2-ethylhexanoate [NOF Corporation, CAS: 3006-82-4, 10-hour half-life temperature: 72.1°C] Perhexa HC: 1,1-di(t-hexylperoxy)cyclohexane [NOF Corporation, CAS: 27215-08-3, 22743-71-1, 10-hour half-life temperature: 87.1°C] Perhexyl I: t-hexylperoxyisopropyl carbonate [NOF Corporation, CAS: 132929-84-1, 10-hour half-life temperature: 95.0°C (e) Siloxane macromonomers Macromer A: Siloxane macromonomer obtained in Synthesis Example 3 Macromer B: Siloxane macromonomer obtained in Synthesis Example 4 FM-0711: Monomethacryloyl-terminated polydimethylsiloxane [JNC Corporation, Product name: Cylaprene FM-0711] (f) Silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure: TRIS: Tris(trimethylsiloxy)-γ-methacryloxypropylsilane [CAS: 17096-07-0] MCR-M07: Monomethacloyloxypropyl-terminated polydimethylsiloxane [Gelest, Product Code: MCR-M07, CAS: 146632-07-7] (g) Monomers that do not contain silicon atoms in their molecular structure HEMA: 2-hydroxyethyl methacrylate [CAS: 868-77-9] DMAA: N,N-dimethylacrylamide [CAS: 2680-03-7] 2-MEA: 2-methoxyethyl acrylate [CAS: 3121-61-7] (h) Polymerization initiators and photopolymerization initiators with a T10 of less than 70°C or greater than 100°C V-65: 2,2'-azobis(2,4-dimethylvaleronitrile) [Wako Pure Chemical Industries, Ltd., CAS: 4419-11-8, 10-hour half-life temperature: 51°C] V-60: 2,2'-azobisisobutyronitrile [Wako Pure Chemical Industries, Ltd., CAS: 78-67-1, 10-hour half-life temperature: 65°C] V-30: 1-[(1-cyano-1-methylethyl)azo]formamide [Wako Pure Chemical Industries, Ltd., CAS: 10288-28-5, 10-hour half-life temperature: 104°C] Darocur1173: 2-hydroxy-2-methyl-1-phenylpropan-1-one [Sigma-Aldrich, CAS: 7473-98-5] Synthesis Example 1: Synthesis of a silicone monomer with only 4 repeating units in the PEG moiety. Commercial tetraethylene glycol was purchased, and the number of repeating units in the PEG moiety was reduced to only 4 by column purification (Compound 1). Next, one end of the tetraethylene glycol was protected with trityl chloride (Compound 2), and the other end was allylated with allyl chloride (Compound 3). To Compound 3 (15.0 g: 31.47 mmol), tris(trimethylsiloxy)silane (9.34 g: 31.47 mmol) and Platinum-divinyltetramethyldisiloxane complex in xylene (300 μL) were added, and the mixture was heated without solvent at 35°C for 3 days. After confirming the disappearance of the starting material by TLC, Compound 4 (15.8 g) was obtained by column purification. Next, 25 mL of chloroform and triethylsilane (827 mg: 7.11 mmol) were added to compound 4 (5.0 g: 6.47 mmol), and Boron Trifluoride Diethyl Ether Complex (917.7 mg: 6.47 mmol) was added dropwise under water cooling, followed by stirring for 30 minutes. After confirming the target product by TLC and LC-MS, the reaction solution was diluted with chloroform, washed with saturated saline solution, dried over anhydrous sodium sulfate, and concentrated to obtain the unpurified target product. After column purification and overnight drying with a vacuum pump, the target compound 5 (2.27 g) was obtained. Figure 1 shows the ¹H-NMR spectrum of compound 5, and Figure 2 shows the MALDI-TOF MS spectrum. From the ¹H-NMR spectrum, peaks originating from the ethylene oxide unit (3.6 ppm) and the tris(trimethylsiloxy)propylsilane structure (3.4 ppm, 1.6 ppm, 0.4 ppm, 0.1 ppm) were detected. Furthermore, from the MALDI-TOF MS spectrum, m / z = 553, corresponding to the sodium adduct ion of the target compound, was detected, and ions with other unit counts (e.g., 3 or 5) were not detected, confirming that the obtained compound has only 4 repeating ethylene oxide units. The measurement conditions for 1H-NMR are as follows: Observation frequency: 600 MHz; Measurement solvent: CDCl3; Measurement temperature: 300 K; Chemical shift reference: Measurement solvent [7.25 ppm] The measurement conditions for MALDI-TOF MS are as follows: Laser light source: N2 laser (wavelength: 337 nm) Measurement mode: Reflector mode, positive ion mode Measurement mass range (m / z): 20 to 1500 Number of accumulations: 1000 Ionization reagent: Sodium trifluoroacetate (THF solution) Next, the siloxane compound shown in E1 was reacted with methacryloyl chloride and 1,8-diazabicyclo[5.4.0]-7-undecene as a catalyst in n-hexane solvent. The resulting solution was filtered through glass fiber filter paper, washed with methanol, then saturated saline solution, dried over anhydrous sodium sulfate, and then purified by column chromatography, followed by removal of the solvent to obtain the monomer of formula E2 (hereinafter referred to as 4Si-4PEG). Synthesis Example 2: Synthesis of a Silicone Monomer with Only 6 Repeats in the PEG Portion Commercial hexaethylene glycol was purchased, and the number of repeats in the PEG portion was reduced to only 6 by column purification (Compound 6). Next, one end of the hexaethylene glycol was protected with trityl chloride (Compound 7), and the other end was allylated with allyl chloride (Compound 8). To Compound 8 (17.8 g: 31.47 mmol), tris(trimethylsiloxy)silane (9.34 g: 31.47 mmol) and Platinum-divinyltetramethyldisiloxane complex in xylene (300 μL) were added, and the mixture was heated without solvent at 35°C for 3 days. After confirming the disappearance of the starting material by TLC, column purification was performed to obtain Compound 9 (17.6 g). Next, compound 9 (5.56 g: 6.47 mmol) was mixed with 25 mL of chloroform and triethylsilane (827 mg: 7.11 mmol). Boron Trifluoride Diethyl Ether Complex (917.7 mg: 6.47 mmol) was added dropwise under water cooling, and the mixture was stirred for 30 minutes. After confirming the target product by TLC and LC-MS, the reaction solution was diluted with chloroform, washed with saturated saline solution, dried over anhydrous sodium sulfate, and concentrated to obtain the unpurified target product. After column purification and overnight drying with a vacuum pump, compound 10 (2.40 g) was obtained. The ¹H-NMR spectrum of compound 10 is shown in Figure 3, and the MALDI-TOF MS spectrum is shown in Figure 4. From the ¹H-NMR spectrum, peaks originating from the ethylene oxide unit (3.6 ppm) and the tris(trimethylsiloxy)propylsilane structure (3.4 ppm, 1.6 ppm, 0.4 ppm, 0.1 ppm) were detected. Furthermore, from the MALDI-TOF MS spectrum, m / z = 641, corresponding to the sodium adduct ion of the target product, was detected, and ions with other unit counts (e.g., 5 or 7) were not detected, confirming that the obtained compound has only 6 repeating units of ethylene oxide. Next, the siloxane compound shown in E3 was reacted with 2-isocyanatoethyl methacrylate using dibutyltin dilaurate as a catalyst in methylene chloride solvent. The resulting solution was purified by column chromatography and then the solvent was removed by distillation to obtain the monomer of formula E4 (hereinafter referred to as 4Si-6PEG). Synthesis Example 3 Synthesis of Macromer A 35 g of carbinol-modified polydimethylsiloxane (Shin-Etsu Chemical Co., Ltd., product name: KF-6001, degree of polymerization: 20, hydroxyl group equivalent: 920 g / mol), 8.29 g (37.3 mmol) of isophorone diisocyanate, and 0.03 g of dibutyltin dilaurate were placed in a 100 mL three-necked flask and stirred at 25°C for 48 hours under a nitrogen stream. Next, 4.97 g (42.9 mmol) of 2-hydroxyethyl acrylate and 20 mL of methylene chloride were added and the mixture was continued to stir at 25°C for 96 hours under a nitrogen stream. After the reaction was complete, the mixture was washed with 200 mL of distilled water, dried over anhydrous sodium sulfate, and the solvent was removed by distillation to obtain the target product (40 g). The obtained compound was confirmed to have the structure shown below, and molecular weight measurement by gel permeation chromatography revealed a number-average molecular weight of 2400 (polystyrene equivalent). The gel permeation chromatography measurement conditions are as follows: Column: Shodex KF-402.5HQ (2 columns) Eluent: THF Flow rate: 0.3 mL / min Detector: RI Column temperature: 40°C Synthesis Example 4 Synthesis of Macromer B In a 100 mL three-necked flask, 35 g of carbinol-modified polydimethylsiloxane (Shin-Etsu Chemical Co., Ltd., product name: KF-6001, degree of polymerization: 20, hydroxyl equivalent: 920 g / mol), 8.29 g (37.3 mmol) of isophorone diisocyanate, and 0.03 g of dibutyltin dilaurate were added and stirred under a nitrogen stream at 25°C for 48 hours. Next, 13.6 g of polyethylene glycol monoacrylate (NOF Corporation, product name: Bremmer AE-200, hydroxyl equivalent: 317 g / mol) and 20 mL of methylene chloride were added and the mixture was continued to stir under a nitrogen stream at 25°C for 120 hours. After the reaction was complete, the mixture was washed with 200 mL of distilled water, dried over anhydrous sodium sulfate, and the solvent was removed by distillation to obtain the target product (45 g). The obtained compound was confirmed to have the structure shown below, and molecular weight measurement by gel permeation chromatography revealed a number-average molecular weight of 2550 (polystyrene equivalent). Example 1 (Example using a polymerization initiator with a 10-hour half-life temperature of 70°C or higher and 100°C or lower) 1.5 g (15% by mass) of macromer A obtained in Synthesis Example 3, 3 g (30% by mass) of 3Si-GMA, 0.5 g (5% by mass) of HEMA, 5 g (50% by mass) of NVP, 0.03 g of 4G (0.3% by mass relative to the total amount of macromer A, 3Si-GMA, HEMA, and NVP), 0.03 g of TEGDVE (0.3% by mass relative to the total amount of macromer A, 3Si-GMA, HEMA, and NVP), and 0.06 g of perbutyl O (0.6% by mass relative to the total amount of macromer A, 3Si-GMA, HEMA, and NVP) were placed in a 20 mL brown glass bottle and stirred at room temperature for about 16 hours. This monomer mixture was poured into a double-sided cast mold made of polypropylene for the manufacture of contact lenses (with a contact angle of 105° on the cavity surface). After assembling the upper and lower molds, the mold was placed in a pressure polymerization furnace. After purging the inside of the polymerization furnace with nitrogen for 20 minutes, polymerization was carried out under conditions of 0.2 kgf / cm2 according to the polymerization schedule shown below. [Gelling conditions] The temperature was raised from room temperature to 50°C in 10 minutes, and then maintained at 50°C for 8 hours. [Cure conditions] After the gelling conditions were completed, the temperature was raised to 80°C in 5 minutes, maintained at 80°C for 2 hours, then raised from 80°C to 100°C in 10 minutes, maintained at 100°C for 40 minutes, and then raised from 100°C to 120°C in 10 minutes, and then maintained at 120°C for 1 hour to complete the polymerization. The polymerized lenses were removed from the mold and immersed in a 50 vol% ethanol aqueous solution for 4 hours. The solution was then replaced with distilled water and a rinsing solution for soft contact lenses (HOYA Corporation, product name: Pure Soak S) to obtain soft contact lenses. The following evaluations and measurements were performed using the obtained soft contact lenses. The results are shown in Table 1. The obtained contact lenses had a contact angle of 50° and possessed a hydrophilic surface. [Properties of the monomer mixture] A portion of the monomer mixture before polymerization was placed in a transparent glass bottle and visually evaluated according to the following evaluation criteria. Evaluation Criteria G (Good): The monomer mixture is dissolved and homogeneous. B (Bad): The monomer mixture separates into two phases and does not dissolve. [Appearance Evaluation] The obtained soft contact lenses were visually evaluated according to the following evaluation criteria. Evaluation Criteria G (Good): The lens is transparent and has a circular shape. B (Bad): The lens is cloudy or, even if transparent, has an irregular shape and is unsuitable as a contact lens. [Water Content] The weight (Ww) of soft contact lenses in the water-saturated state, which reached equilibrium swelling at 23°C, and the weight (Wd) of the dry state, which was dried in a vacuum dryer at 70°C for 4 hours, were measured, and the water content was calculated using the following formula: Water content (%) = (Ww - Wd) / Ww × 100 [Oxygen Permeability Coefficient] The oxygen permeability coefficient was measured using lenses of different thicknesses according to the polarography method described in ISO 18369-4. A Rehder Development Company O2 Permometer Model 201T was used for the measurements. The lens thickness was plotted on the x-axis, and the t / Dk values obtained by measurement were plotted on the y-axis. The reciprocal of the slope of the regression line was defined as the oxygen permeability coefficient. [Contact Angle Measurement (Droplet Method)] The water wettability of the soft contact lens surface was evaluated by contact angle measurement. After wiping off moisture from the soft contact lens surface, the lens was attached to a holder, and the contact angle was measured using the droplet method with pure water. A contact angle meter manufactured by Kyowa Interface Science Co., Ltd. was used for the measurement, and the droplet size was set to approximately 1.5 mm using a syringe. A smaller value indicates better water wettability. [Surface Composition Analysis] Hydrated soft contact lenses were re-dried, and the types and amounts of elements present on the contact lens surface (to a depth of several tens of nm) were analyzed by XPS. The measurement was performed near the center of the front curve surface of the soft contact lens, and the surface composition ratio is expressed in atomic percent. The XPS measurement conditions are as follows: Irradiation X-ray: Al-Kα monochromator, φ100 μm; Photoelectron extraction angle: 45 degrees; Charge neutralization: 10 V; Ar ion + 20 μA electron beam simultaneous irradiation. Example 2 A lens was prepared in the same manner as in Example 1, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-40 and the gelation conditions were changed as described below. The resulting contact lens had a contact angle of 40° and possessed a hydrophilic surface (Table 1). [Gelling conditions] The temperature was raised from room temperature to 55°C in 10 minutes, then maintained at 55°C for 8 hours, and then raised from 55°C to 80°C in 5 minutes, and then maintained at 80°C for 2 hours. [Cure conditions] After the gelling conditions were completed, the temperature was raised to 100°C in 10 minutes, then maintained at 100°C for 40 minutes, and then raised from 100°C to 120°C in 10 minutes, and then maintained at 120°C for 1 hour to complete the polymerization. Example 3 A lens was prepared in the same manner as in Example 1, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to perhexa HC and the gelation conditions were changed as described below. The resulting contact lens had a contact angle of 33° and possessed a hydrophilic surface (Table 1). [Gelling conditions] Same as in Example 2. [Cure conditions] Same as in Example 2. Example 4 A lens was prepared in the same manner as in Example 1, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to perhexyl I and the gelation conditions were changed as follows. The resulting contact lens had a contact angle of 53° and possessed a hydrophilic surface (Table 1). [Gelling conditions] The temperature was raised from room temperature to 70°C in 10 minutes, then maintained at 70°C for 8 hours, and then raised from 70°C to 80°C in 5 minutes, and maintained at 80°C for 2 hours. [Cure conditions] Same as in Example 2. Comparative Example 1 (Example using a polymerization initiator with a T10 of less than 70°C) A lens was prepared in the same manner as in Example 1, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-65. The surface of the obtained contact lens had a low proportion of nitrogen elements, which are thought to be derived from N-vinyl-2-pyrrolidone, and conversely, a high distribution of silicon elements derived from the silicone component, and the contact angle of the lens surface was 102°, indicating poor water wettability (Table 1). Comparative Example 2 (Example using a polymerization initiator with a T10 of less than 70°C) A lens was prepared in the same manner as in Example 1, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-60. The surface of the obtained contact lens had a low proportion of nitrogen elements, which are thought to be derived from N-vinyl-2-pyrrolidone, and conversely, a high distribution of silicon elements derived from the silicone component, and the contact angle of the lens surface was 102°, indicating poor water wettability (Table 1). Comparative Example 3 (Example using a polymerization initiator with a T10 exceeding 100°C) A lens was prepared in the same manner as in Example 1, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-30 and the gelation conditions were changed as follows. The resulting contact lens was brittle and could not be removed from the mold (Table 1). [Gelling Conditions] The temperature was raised from room temperature to 70°C in 10 minutes, then maintained at 70°C for 8 hours. Subsequently, the temperature was raised from 70°C to 80°C in 5 minutes, then maintained at 80°C for 2 hours. Furthermore, the temperature was raised from 80°C to 100°C in 10 minutes, then maintained at 100°C for 40 minutes. [Cure Conditions] After the gelling conditions were completed, the temperature was raised from 100°C to 120°C in 10 minutes, then maintained at 120°C for 1 hour to complete the polymerization. As shown in Table 1, in Examples 1 to 4, which used polymerization initiators with a T10 of 70°C or higher and 100°C or lower, and maintained the gelation conditions at a temperature within the range of the polymerization initiator's T10 to 35°C lower than T10 for at least 1 hour (P1 step), and maintained the curing conditions at a temperature higher than the polymerization initiator's T10 for at least 1 hour (P2 step), the amount of silicon elements derived from the silicone component on the contact lens surface could be reduced, and contact lenses with a hydrophilic surface could be obtained without any post-treatment after polymerization. On the other hand, in Comparative Examples 1 and 2, which used polymerization initiators with a T10 of less than 70°C under similar conditions, a large amount of silicon elements derived from the silicone component was distributed on the lens surface, resulting in poor water wettability. Furthermore, in Comparative Example 3, which used a polymerization initiator with a T10 exceeding 100°C, the polymerized lens was brittle, and it was not possible to remove the lens from the mold. Example 5 (Example using a polymerization initiator with a T10 of 70°C or higher and 100°C or lower) In a 20 mL brown glass bottle, 1.5 g (15% by mass) of macromer B obtained in Synthesis Example 4, 2.5 g (25% by mass) of 3Si-GMA, 0.8 g (8% by mass) of FM-0711, 0.5 g (5% by mass) of HEMA, 4.7 g (47% by mass) of NVP, 0.05 g of 4G (0.5% by mass relative to the total amount of macromer B, 3Si-GMA, FM-0711, HEMA, and NVP), 0.03 g of BDVE (0.3% by mass relative to the total amount of macromer B, 3Si-GMA, FM-0711, HEMA, and NVP), and 0.06 g of perbutyl O (0.6% by mass relative to the total amount of macromer B, 3Si-GMA, FM-0711, HEMA, and NVP) were added, and the mixture was stirred at room temperature for approximately 16 hours. This monomer mixture was poured into a double-sided cast mold made of polypropylene for contact lens fabrication. After assembling the upper and lower molds, the mold was placed in a pressure polymerization furnace. After purging the inside of the polymerization furnace with nitrogen for 20 minutes, polymerization was carried out under conditions of 0.2 kgf / cm2 according to the polymerization schedule shown below. [Gelling conditions] The temperature was raised from room temperature to 50°C in 10 minutes, and then maintained at 50°C for 8 hours. [Cure conditions] Same as in Example 1. The polymerized lenses were removed from the mold and immersed in a 50 vol% ethanol aqueous solution for 4 hours. This was then replaced with distilled water and a rinsing solution for soft contact lenses (HOYA Corporation, product name: Pure Soak S) to obtain soft contact lenses. The results are shown in Table 2. The obtained contact lenses had a contact angle of 48° and possessed a hydrophilic surface. Example 6 A lens was prepared in the same manner as in Example 5, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-40 and the gelation conditions were changed as described below. The resulting contact lens had a contact angle of 40° and possessed a hydrophilic surface (Table 2). [Gelling conditions] The temperature was raised from room temperature to 60°C in 10 minutes, then maintained at 60°C for 8 hours, and then raised from 60°C to 80°C in 5 minutes, and maintained at 80°C for 2 hours. [Cure conditions] Same as in Example 2. Example 7 A lens was prepared in the same manner as in Example 6, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to perhexa HC and the gelation conditions were changed as described below. The resulting contact lens had a contact angle of 32° and possessed a hydrophilic surface (Table 2). [Gelling conditions] The temperature was raised from room temperature to 60°C in 10 minutes, then maintained at 60°C for 8 hours, and then raised from 60°C to 80°C in 5 minutes, and maintained at 80°C for 2 hours. [Cure conditions] Same as in Example 2. Example 8 A lens was prepared in the same manner as in Example 5, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to perhexyl I and the gelation conditions were changed as described below. The resulting contact lens had a contact angle of 44° and possessed a hydrophilic surface (Table 2). [Gelling conditions] The temperature was raised from room temperature to 65°C in 10 minutes, then maintained at 65°C for 8 hours, and then raised from 65°C to 80°C in 5 minutes, and maintained at 80°C for 2 hours. [Cure conditions] Same as in Example 2. Comparative Example 4 (Example using a polymerization initiator with a T10 of less than 70°C): A lens was prepared in the same manner as in Example 5, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-65. The resulting contact lens was not circular but had an irregular shape and was not suitable as a contact lens (Table 2). Comparative Example 5 (Example using a polymerization initiator with a T10 of less than 70°C) A lens was prepared in the same manner as in Example 5, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-60. The resulting contact lens was not circular but had an irregular shape and was not suitable as a contact lens (Table 2). Comparative Example 6 (Example using a polymerization initiator with a T10 exceeding 100°C) A lens was prepared in the same manner as in Example 5, except that the polymerization initiator in the monomer composition of the soft contact lens was changed to V-30 and the gelation conditions were changed as follows. The resulting contact lens was brittle and could not be removed from the mold (Table 2). [Gelling Conditions] The temperature was raised from room temperature to 65°C in 10 minutes, then maintained at 65°C for 8 hours. Subsequently, the temperature was raised from 65°C to 80°C in 5 minutes, then maintained at 80°C for 2 hours. Furthermore, the temperature was raised from 80°C to 100°C in 10 minutes, then maintained at 100°C for 40 minutes. [Cure Conditions] After the gelling conditions were completed, the temperature was raised from 100°C to 120°C in 10 minutes, then maintained at 120°C for 1 hour to complete the polymerization. As shown in Table 2, in Examples 5 to 8, where a polymerization initiator with a T10 of 70°C or higher and 100°C or lower was used, and the gelation conditions were maintained for at least 1 hour within a temperature range of 35°C lower than the T10 of the polymerization initiator (P1 step), and the curing conditions were maintained for at least 1 hour at a temperature higher than the T10 of the polymerization initiator (P2 step), contact lenses with a hydrophilic surface could be obtained without any post-treatment after polymerization. On the other hand, in Comparative Examples 4 and 5, where polymerization initiators with a T10 of less than 70°C were used under similar conditions, the lenses deformed and were not suitable as contact lenses. Furthermore, in Comparative Example 6, where a polymerization initiator with a T10 exceeding 100°C was used, the polymerized lenses were brittle and could not be removed from the mold. Examples 9-12 and Comparative Examples 7-8 (when various structures of silicone monomers were modified using polymerization initiators with a T10 of 70°C or higher and 100°C or lower): Monomer mixtures were prepared with the compositions shown in Table 3, and lenses were fabricated in the same manner as in Example 1. The gelation and curing conditions were as follows. [Gelling conditions] The temperature was raised from room temperature to 60°C in 10 minutes, then maintained at 60°C for 8 hours, and then raised from 60°C to 80°C in 5 minutes, and maintained at 80°C for 2 hours. [Cure conditions] Same as in Example 2. As shown in Table 3, when a silicone monomer having at least one hydroxyl group or polyethylene glycol group in its molecular structure and containing four silicon atoms was used, a transparent contact lens with a hydrophilic surface could be obtained. On the other hand, when a silicone monomer that did not contain a hydroxyl group or polyethylene glycol group in its molecular structure and contained four or more silicon atoms was used, the resulting contact lens became cloudy when hydrated, making it unsuitable as a contact lens, or a homogeneous monomer mixture solution could not be obtained. Examples 13-20 Lenses were prepared in the same manner as in Example 1, except that monomer mixtures were prepared with the compositions shown in Table 4. The gelation and curing conditions were all as follows. [Gelling conditions] The temperature was raised from room temperature to 55°C in 10 minutes, then maintained at 55°C for 8 hours, and then raised from 55°C to 80°C in 5 minutes, and maintained at 80°C for 2 hours. [Cure conditions] Same as in Example 2. Comparative Example 9: A lens was prepared in the same manner as in Example 13, except that a monomer mixture was prepared with the composition shown in Table 4. The resulting lens had poor surface water wettability because it contained N,N-dimethylacrylamide as a component of the lens. Comparative Example 10 A monomer mixture was prepared with the composition shown in Table 4, and the monomer mixture was poured into a double-sided cast mold made of polypropylene for contact lens fabrication. The upper and lower molds were then assembled. Polymerization was completed by irradiating this mold with light in the 280-390 nm region with an irradiation intensity of 11 mW / cm2 for 20 minutes. The resulting lens had poor surface water wettability. Comparative Example 11 A monomer mixture with the same composition as in Example 20 was prepared, and this monomer mixture was poured into a double-sided cast mold for contact lens manufacturing made of polypropylene. After assembling the upper and lower molds, the mold was placed in a pressure polymerization furnace. After purging the inside of the polymerization furnace with nitrogen for 30 minutes, polymerization was carried out under conditions of 0.2 kgf / cm2 according to the polymerization schedule shown below. [Gelling conditions] The temperature was raised from room temperature to 55°C in 20 minutes, then maintained at 55°C for 40 minutes, and then raised from 55°C to 80°C in 5 minutes, and maintained at 80°C for 40 minutes. [Cure conditions] After the gelling conditions were completed, the temperature was raised from 80°C to 100°C in 10 minutes, and then maintained at 100°C for 40 minutes to complete the polymerization. The polymerized lenses were removed from the mold and immersed in a 50 vol% ethanol aqueous solution for 4 hours. This was then replaced with distilled water and a rinsing solution for soft contact lenses (Hoya Corporation, product name: Pure Soak S) to obtain soft contact lenses. The resulting contact lenses were not circular but irregularly shaped and were unsuitable as contact lenses. Comparative Example 12 A monomer mixture with the same composition as in Example 20 was prepared, and a lens was fabricated in the same manner as in Comparative Example 11, except that the gelation conditions were changed as follows. The resulting contact lens was brittle and could not be removed from the mold. [Gelling conditions] Polymerization was completed by raising the temperature from room temperature to 80°C in 25 minutes, and then holding it at 80°C for 90 minutes. As shown in Table 4, in Examples 13 to 20, where a polymerization initiator with a T10 of 70°C or higher and 100°C or lower was used, and the gelation conditions were maintained for at least 1 hour within a temperature range of 35°C lower than the T10 of the polymerization initiator (P1 step), and the curing conditions were maintained for at least 1 hour at a temperature higher than the T10 of the polymerization initiator (P2 step), silicone hydrogel contact lenses having a hydrophilic surface could be obtained without any post-treatment after polymerization. On the other hand, even under similar polymerization conditions, Comparative Example 9, which contained N,N-dimethylacrylamide as a monomer component, resulted in a lens with poor surface wettability and was not suitable as a contact lens without post-polymerization treatment. Similarly, Comparative Example 10, which employed photopolymerization, also resulted in a lens with poor surface wettability and was not suitable as a contact lens without post-polymerization treatment. Furthermore, even when using a polymerization initiator with a T10 of 70°C or higher and 100°C or lower, Comparative Example 11, where the maintenance time under curing conditions equivalent to the P2 step was less than one hour, deformed the lens and was not suitable as a contact lens. Moreover, even when maintained for more than one hour within a temperature range of T10 to 35°C lower than T10, Comparative Example 12, which did not undergo the P2 step, resulted in a brittle lens after polymerization, making it impossible to remove the lens from the mold. This invention is useful in the field of contact lenses.
Claims
1. A method for producing a silicone-containing copolymer molded article having a hydrophilic surface and containing silicone monomer units, hydrophilic monomer units, and crosslinkable monomer units, wherein the polymerization initiator has a half-life temperature of 10 hours (hereinafter abbreviated as T10) of 70°C or higher and 100°C or lower, and the polymerization is carried out in a P1 step of maintaining the temperature of the polymerization initiator contained in the monomer solution within a range from T10 to 35°C lower than T10 for 1 hour or more, and in a P2 step of maintaining the temperature of the polymerization initiator contained in the monomer solution at a temperature higher than T10 for 1 hour or more.
2. The method according to claim 1, wherein the maintenance temperature in step P1 is in the range of 10°C lower than T10 to 35°C lower than T10.
3. The method according to claim 1 or 2, wherein the maintenance temperature in step P2 is in the range of 5°C higher than T10 to 50°C higher than T10.
4. The method according to any one of claims 1 to 3, wherein the polymerization initiator is an azo polymerization initiator or an organic peroxide polymerization initiator.
5. The method according to any one of claims 1 to 4, wherein the content of the silicone monomer (a) units in the silicone-containing copolymer molded article is in the range of 20 to 56% by mass, the content of the hydrophilic monomer (b) units is in the range of 40 to 60% by mass, and the content of the crosslinkable monomer (c) units is in the range of 0.02 to 4% by mass.
6. The method according to any one of claims 1 to 5, wherein the silicone monomer (a) is at least one monomer selected from the group consisting of (a1) and (a2) below: (a1) one or more silicone monomers containing at least one hydroxyl group and one to four silicon atoms in one molecule; (a2) one or more silicone monomers containing at least one polyethylene glycol group and one to four silicon atoms in one molecule.
7. The silicone monomer (a1) is a monomer represented by the following general formula (a1-1) or (a1-2), [wherein, R 1 , R 2 , R 3 and R 4 are methyl groups, R 5 is a hydrogen atom or a methyl group, and a represents an integer of 1 to 3.], The method according to claim 6, wherein the silicone monomer (a2) is a monomer represented by the following general formula (a2-1). [In the formula, R 1 , R 2 , R 3 and R 4 are methyl groups, a represents an integer of 1 to 3, and m is 4 to 8. X in the formula is one selected from the substituents represented by the following formula (Y1) or (Y2) (wherein, R 5 is a hydrogen atom or a methyl group.).] 8. The method according to any one of claims 1 to 7, wherein the hydrophilic monomer (b) is one or two selected from N-vinyl-2-pyrrolidone and N-vinyl-N-methylacetamide.
9. The method according to any one of claims 1 to 8, wherein the crosslinkable monomer (c) is at least one monomer selected from the group consisting of (c1), (c2), and (c3): (c1) one or more monomers containing two or more vinyl groups in one molecule, (c2) one or more monomers containing two or more allyl groups in one molecule, (c3) one or more monomers having two or more (meth)acrylate groups in one molecule.
10. The method according to claim 9, wherein the monomer (c1) is one or more selected from 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, and triethylene glycol divinyl ether; the monomer (c2) is one or more selected from triallyl isocyanurate, trimethylolpropanediallyl ether, and pentaerythritol triallyl ether; and the monomer (c3) is one or more monomers selected from ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate.
11. The method according to any one of claims 1 to 10, wherein the monomer solution further contains at least one auxiliary monomer selected from the group consisting of siloxane macromonomers, silicone monomers that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomers that do not contain silicon atoms in their molecular structure.
12. The method according to any one of claims 1 to 11, wherein the hydrophilic surface of the silicone-containing copolymer molded article has a contact angle with pure water of 60° or less, without any post-treatment to improve the surface wettability of the molded article surface after polymerization (however, the contact angle is the contact angle of a silicone hydrogel molded article in which the silicone-containing copolymer molded article has been hydrated).
13. The method according to any one of claims 1 to 12, wherein the mold having a hydrophobic cavity surface is a double-sided cast mold for molding polyalkylene contact lenses, and the silicone-containing copolymer molded product is a precursor for silicone hydrogel soft contact lenses.
14. A silicone-containing copolymer molded article prepared by the method described in any one of claims 1 to 13.
15. A monomer unit consisting of at least one monomer unit selected from the group consisting of (a1) and (a2) below, the monomer unit of (b) below, and at least one monomer unit selected from the group consisting of (c1) to (c3) (however, it may further include (g) a monomer unit that does not contain a silicon atom in its molecular structure, and (g) the monomer that does not contain a silicon atom in its molecular structure is selected from 2-hydroxyethyl (meth)acrylate, methacrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-methacryloyloxyethyl phosphorylcholine, etc. A silicone-containing copolymer molded article having a hydrophilic surface with a contact angle of 60° or less with respect to pure water (where the contact angle is the contact angle of a silicone hydrogel molded article made by impregnating a silicone-containing copolymer molded article with water), wherein the content of the silicone monomer (a1) to (a2) units is in the range of 20 to 56% by mass, the content of the monomer (b) unit is in the range of 40 to 60% by mass, the content of the monomer (c1) to (c3) units is in the range of 0.02 to 4% by mass, and the content of monomer units that do not contain silicon atoms in the molecular structure of (g) is in the range of less than 10% by mass. (a1) One or more units derived from a silicone monomer containing at least one hydroxyl group and one to four silicon atoms in one molecule and having a molecular weight of less than 900; (a2) One or more units derived from a silicone monomer containing at least one polyethylene glycol group and one to four silicon atoms in one molecule and having a molecular weight of less than 900; (b) One or more units derived from a hydrophilic monomer having a vinyl group; (c1) One or more monomer units containing two or more vinyl groups in one molecule; (c2) One or more monomer units containing two or more allyl groups in one molecule; (c3) One or more monomers having two or more (meth)acrylate groups in one molecule.
16. A silicone-containing copolymer molded article containing at least one monomer unit selected from the group consisting of (a1) and (a2) below, the monomer unit of (b) below, at least one monomer unit selected from the group consisting of (c1) to (c3) below, and the siloxane macromonomer unit of (e), having a hydrophilic surface with a contact angle to pure water of 60° or less, and having a water content of 35% or more and less than 60% (wherein the contact angle and water content are the contact angle and water content of a silicone hydrogel molded article obtained by hydrating a silicone-containing copolymer molded article, respectively). (a1) One or more units derived from a silicone monomer containing at least one hydroxyl group and 1 to 4 silicon atoms in one molecule and having a molecular weight of less than 900; (a2) One or more units derived from a silicone monomer containing at least one polyethylene glycol group and 1 to 4 silicon atoms in one molecule and having a molecular weight of less than 900; (b) One or more units derived from a hydrophilic monomer having a vinyl group; (c1) One or more monomer units containing two or more vinyl groups in one molecule; (c2) One or more monomer units containing two or more allyl groups in one molecule; (c3) One or more monomers having two or more (meth)acrylate groups in one molecule; (e) One or more macromonomers of general formulas (C1) and (C2), in formula (C1), R 7 R is a hydrogen atom or a methyl group, r is 0 to 10, and p is 8 to 60. In formula (C2), R 8 is a hydrogen atom or a methyl group, q is 9 to 15, and t is 0 to 3.
17. A silicone-containing copolymer molded article according to claim 16, wherein r is 0 to 8, p is 8 to 50, q is 9 to 13, and t is 0 to 2.
18. The silicone-containing copolymer molded article according to claim 16, wherein the siloxane macromonomer unit of (e) is (E5) or (E6) below. Macromer A 19. The silicone monomer (a1) is a monomer represented by the following general formula (a1-1) or (a1-2), [wherein R 1 , R 2 , R 3 and R 4 is a methyl group, R 5 R is a hydrogen atom or a methyl group, and a represents an integer from 1 to 3. ], The silicone-containing copolymer molded article according to any one of claims 15 to 18, wherein the silicone monomer (a2) is a monomer represented by the following general formula (a2-1). [In the formula, R 1 , R 2 , R 3 and R 4 R is a methyl group, a is an integer from 1 to 3, and m is from 4 to 8. In the formula, X is one selected from the substituents represented by the following formulas (Y1) or (Y2) (wherein R 5 (This is a hydrogen atom or a methyl group.) 20. The silicone-containing copolymer molded article according to any one of claims 15 to 19, wherein the hydrophilic monomer (b) is one or two selected from N-vinyl-2-pyrrolidone and N-vinyl-N-methylacetamide.
21. A silicone-containing copolymer molded article according to any one of claims 15 to 20, wherein the monomer (c1) is one or more selected from 1,4-butanediol divinyl ether, diethylene glycol divinyl ether, and triethylene glycol divinyl ether; the monomer (c2) is one or more selected from triallyl isocyanurate, trimethylolpropanediallyl ether, and pentaerythritol triallyl ether; and the monomer (c3) is one or more monomers selected from ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate.
22. A silicone-containing copolymer molded article according to any one of claims 16 to 21, wherein the content of the silicone monomer (a1) and (a2) units is in the range of 20 to 56% by mass, the content of the monomer (b) unit is in the range of 40 to 60% by mass, and the content of the monomer (c1), (c2), and (c3) units is in the range of 0.02 to 4% by mass.
23. A silicone-containing copolymer molded article according to any one of claims 16 to 22, wherein the content of the siloxane macromonomer units in (e) is 25% by mass or less.
24. The silicone-containing copolymer molded article according to any one of claims 16 to 23, further comprising at least one additional monomer unit selected from the group consisting of silicone monomer units that do not contain hydroxyl groups or polyethylene glycol groups in their molecular structure, and monomer units that do not contain silicon atoms in their molecular structure.
25. A hydrophilic surface having a contact angle to pure water of 60° or less is obtained without any post-treatment to improve the surface wettability of the lens-shaped material after polymerization (provided that the contact angle is the contact angle of a silicone hydrogel molded product in which a silicone-containing copolymer molded product has been impregnated with water), as described in any one of claims 15 to 24.
26. A silicone-containing copolymer molded article according to any one of claims 14 to 25, and a precursor for silicone hydrogel soft contact lenses having a contact lens shape.
27. A silicone hydrogel soft contact lens obtained by hydrating the silicone hydrogel soft contact lens precursor described in claim 26 with physiological saline or a soft contact lens storage solution.
28. The soft contact lens according to claim 27, wherein the silicone hydrogel soft contact lens, when hydrated, has a water content of 35% or more and less than 60%.
29. The soft contact lens according to claim 27 or 28, wherein the silicone hydrogel soft contact lens in the hydrated state is a soft contact lens with a replacement frequency of up to one month.
30. The soft contact lens according to claim 29, wherein the silicone hydrogel soft contact lens, which has been hydrated, is of the type that is replaced daily or every two weeks.
31. A packaged soft contact lens product comprising a soft contact lens according to any one of claims 27 to 30 and physiological saline solution or soft contact lens storage solution stored in a sealed container.