Chlorine-containing resin composition
Patent Information
- Application Number
- LAP718
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-10-30
- Filing Date
- 2018-07-25
- Publication Date
- 2025-02-21
AI Technical Summary
Chlorine-containing resin compositions using Ca-Zn stabilizers often result in surface defects like scratches and streaks during long-term continuous production, leading to reduced productivity, as the solubility and compatibility issues with Sn-based stabilizers cannot be addressed effectively.
A chlorine-containing resin composition incorporating organic acid zinc, oxidized polyethylene wax, hydrotalcite, and β-diketone compounds or β-diketo metal salts, which suppress the occurrence of surface defects, ensuring stable production even during extended production periods.
The composition effectively prevents scratches and streaks on molded products, maintaining product quality and productivity, and can be used for various applications such as pipes, joints, and automobile parts without causing environmental harm.
Abstract
Description
Chlorine-containing resin composition
[0001] The present invention relates to a chlorine-containing resin composition, and more particularly to a chlorine-containing resin composition that can be suitably used as a material for pipes, joints, building materials, automobile parts, etc.
[0002] Chlorine-containing resins, such as polyvinyl chloride, are highly flexible and easy to process, and also possess physical properties such as flame retardancy. Therefore, they are used in a variety of applications, such as agricultural films, electric wires, pipes, and plastic window frames. Various compositions tailored to the required properties have been proposed (see Patent Documents 1 to 4). Vinyl chloride resin compositions generally lack sufficient thermal stability, and stabilizers are used to impart thermal stability during processing. While Pb-based and Sn-based stabilizers have traditionally been widely used, in recent years, environmental considerations have led to increased use of less toxic, Pb-free Ca-Zn-based stabilizers.
[0003] JP 2001-40217 Publication Special Table 2015-507067 JP 9-40830 JP 10-158451
[0004] When molded articles of chlorine-containing resin compositions are produced using Ca-Zn-based stabilizers, which have been increasingly used in recent years, defects such as fading and striations occur on the surface of the molded articles during long-term continuous production, resulting in a significant decrease in productivity. While Sn-based stabilizers are primarily liquid stabilizers, or even solids with low melting points below the resin softening temperature, Ca-Zn-based stabilizers also contain large amounts of inorganic substances such as hydrotalcite, which have no melting point, and have completely different solubility and compatibility with chlorine-containing resins. Therefore, this problem cannot be addressed by adapting the methods used to improve molded article defects with Sn-based stabilizers, and it is necessary to develop a solution that is tailored to Ca-Zn-based stabilizers.
[0005] The present invention has been made in view of the above-mentioned current situation, and aims to provide a chlorine-containing resin composition which uses a Ca-Zn-based stabilizer and in which the occurrence of smearing or striating on the surface of a molded product is sufficiently suppressed even when the composition is subjected to long-term continuous production.
[0006] The present inventors have conducted various studies on methods for suppressing the occurrence of smearing and striating in chlorine-containing resin compositions using Ca-Zn stabilizers, and have found that when a chlorine-containing resin composition containing an organic acid zinc as a stabilizer further contains a specific oxidized polyethylene wax, hydrotalcite, and a β-diketone compound and / or a β-diketo metal salt, the occurrence of smearing and striating on the surface of molded articles can be sufficiently suppressed even in long-term continuous production, leading to the completion of the present invention.
[0007] That is, the present invention provides a composition comprising (a) a chlorine-containing resin, (b) an organic acid zinc salt, (c) an oxidized polyethylene wax, (d) hydrotalcite, and (e) a β-diketone compound and / or a β-diketo metal salt, wherein the oxidized polyethylene wax (c) has a peak at 1720 cm in FT-IR measurement. -1 Peak and 2930cm -1 The absorbance ratio of the peak (1720 cm -1 Peak absorbance / 2930 cm -1 The chlorine-containing resin composition has a peak absorbance of 0.05 or more.
[0008] The oxidized polyethylene wax (c) preferably has an acid value of 1 mgKOH / g or more.
[0009] The oxidized polyethylene wax (c) has a density of 0.95 g / cm 3 It is preferable that:
[0010] The oxidized polyethylene wax (c) preferably has a melting point of 80° C. or higher.
[0011] The oxidized polyethylene wax (c) preferably has a melt viscosity at 140°C of 1000 cps or less.
[0012] The (d) hydrotalcite preferably has an oil absorption of 50 ml / 100 g or less.
[0013] The chlorine-containing resin composition preferably further contains (f) dipentaerythritol hexastearate.
[0014] The chlorine-containing resin composition preferably contains a plasticizer in an amount of 5% by weight or less based on the total weight of the composition.
[0015] The chlorine-containing resin composition preferably further contains calcium carbonate in an amount of 30 parts by mass or less per 100 parts by mass of the chlorine-containing resin.
[0016] The chlorine-containing resin composition of the present invention uses an environmentally friendly, low-toxicity stabilizer, and yet is sufficiently suppressed in the occurrence of smearing or striations on the surface of molded articles even after long-term continuous production. Therefore, the composition can be suitably used as a material for various molded articles such as pipes, fittings, building materials, and automobile parts.
[0017] An example of the present invention will be specifically described below, but the present invention is not limited to the following description and can be modified and applied as appropriate within the scope that does not change the gist of the present invention.
[0018] <Chlorine-Containing Resin Composition> The chlorine-containing resin composition of the present invention contains (a) a chlorine-containing resin, (b) an organic acid zinc salt, (c) an oxidized polyethylene wax, (d) hydrotalcite, and (e) a β-diketone compound and / or a β-diketo metal salt. These components may each contain one type, or two or more types. Furthermore, the composition may also contain other components. Each of components (a) to (e) will be described below in order.
[0019] [Chlorine-containing resin] The chlorine-containing resin is not particularly limited as long as it is a resin (polymer) containing chlorine atoms, but vinyl chloride resins are preferred, as this allows for the production of molded articles with excellent flexibility and flame retardancy.
[0020] Examples of vinyl chloride resins include homopolymers such as polyvinyl chloride, chlorinated polyvinyl chloride, polyvinylidene chloride, and chlorinated polyethylene; copolymers such as vinyl chloride-vinyl acetate copolymer, vinyl chloride-ethylene-vinyl acetate copolymer, vinyl chloride-ethylene copolymer, vinyl chloride-propylene copolymer, vinyl chloride-styrene copolymer, vinyl chloride-isobutylene copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-urethane copolymer, vinyl chloride-acrylic acid ester copolymer, vinyl chloride-styrene-maleic anhydride copolymer, vinyl chloride-styrene-acrylonitrile copolymer, vinyl chloride-butadiene copolymer, vinyl chloride-isoprene copolymer, vinyl chloride-chlorinated propylene copolymer, vinyl chloride-vinylidene chloride-vinyl acetate copolymer, vinyl chloride-maleic acid ester copolymer, vinyl chloride-methacrylic acid ester copolymer, vinyl chloride-acrylonitrile copolymer, and vinyl chloride-maleimide copolymer; and the like. Blends of chlorine-containing resins and chlorine-free resins may also be used, and the polymerization method for obtaining the vinyl chloride resin is not particularly limited.
[0021] [Organic Zinc Acid] The chlorine-containing resin composition of the present invention contains an organic zinc acid, which stabilizes the chlorine in the chlorine-containing resin and suppresses discoloration during processing and use. The organic zinc acid is a low-toxicity stabilizer that does not contain Pb. Such Pb-free stabilizers that are not classified as Sn-based stabilizers are generally referred to as Ca-Zn-based stabilizers. The term Ca-Zn-based stabilizer does not only refer to stabilizers containing both Ca and Zn, but also includes stabilizers containing only Zn and stabilizers that contain neither Ca nor Zn and also do not contain Sn. Furthermore, stabilizers that contain a metal element other than Pb, such as Sn, as an auxiliary agent in addition to Ca and Zn, may also be included in the Ca-Zn-based stabilizer. In the present invention, even if a stabilizer contains Sn, if the content of Sn when added to a chlorine-containing resin is 0.5 parts by mass or less per 100 parts by mass of the chlorine-containing resin, the stabilizer is classified as a Ca-Zn-based stabilizer, and if the Sn content is more than 0.5 parts by mass, the stabilizer is classified as a Sn-based stabilizer.
[0022] The organic acid in the organic acid zinc salt is not particularly limited, and examples thereof include acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, 2-ethylhexyl acid, neodecanoic acid, capric acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, isostearic acid, stearic acid, 12-hydroxystearic acid, behenic acid, montanic acid, benzoic acid, monochlorobenzoic acid, p-t-butylbenzoic acid, dimethylhydroxybenzoic acid, 3,5-di-t-butyl-4-hydroxybenzoic acid, toluic acid, dimethylbenzoic acid, ethylbenzoic acid, cumic acid, n-propylbenzoic acid, aminobenzoic acid, N,N-dimethylaminobenzoic acid, acetoxybenzoic acid, salicylic acid, p-t-octylsalicylic acid, elaidic acid, oleic acid, and the like. monovalent organic carboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, hydroxyphthalic acid, chlorophthalic acid, aminophthalic acid, maleic acid, fumaric acid, citraconic acid, metaconic acid, itaconic acid, aconitic acid, and thiodipropionic acid; and monoester or monoamide compounds of divalent organic carboxylic acids, and di- or triesters of trivalent or tetravalent organic carboxylic acids such as butanetricarboxylic acid, butanetetracarboxylic acid, hemimellitic acid, trimellitic acid, mellophanic acid, and pyromellitic acid. Among these, higher fatty acids having 12 to 20 carbon atoms are preferred. Specifically, zinc salts of myristic acid, palmitic acid, isostearic acid, stearic acid, and the like are preferred, as they have suitable lubricity and compatibility with chlorine-containing resins.
[0023] The content of the organic acid zinc salt is not particularly limited, and is preferably, for example, 0.01 parts by mass or more relative to 100 parts by mass of the chlorine-containing resin. This can suppress discoloration. More preferably, it is 0.1 parts by mass or more. Furthermore, it is preferably 5 parts by mass or less, which can further improve heat resistance, prevent deterioration of the appearance of the molded product, and improve color tone. More preferably, it is 2 parts by mass or less.
[0024] [Oxidized Polyethylene Wax] The chlorine-containing resin composition of the present invention has a peak at 1720 cm in FT-IR measurement. -1 Peak and 2930cm -1 The absorbance ratio of the peak (1720 cm -1 Peak absorbance / 2930 cm -1 The peak absorbance (peak absorbance) of the oxidized polyethylene wax is 0.05 or more. -1 The peak at 2930 cm appears as the oxidation of polyethylene wax progresses. -1 The peaks are those of hydrocarbon bonds, which indicate polyethylene wax. By using an oxidized polyethylene wax in which the ratio of these peaks is 0.05 or more, i.e., a polyethylene wax that has been oxidized to a certain degree or more, it is possible to effectively reduce surface defects in molded articles.
[0025] The oxidized polyethylene wax preferably has an acid value of 1 mgKOH / g or more. When the acid value is 1 mgKOH / g or more, compatibility with resins is improved, and the effect of suppressing defective appearance of molded articles is more sufficiently exhibited. The acid value of the oxidized polyethylene wax is more preferably 5 mgKOH / g or more, and even more preferably 10 mgKOH / g or more. Also, it is preferably 30 mgKOH / g or less.
[0026] Oxidized polyethylene wax has a density of 1.00 g / cm 3 It is preferable that the density is 1.00 g / cm or less. 3 When the density of the oxidized polyethylene wax is 0.95 g / cm or less, the melt viscosity of the resin is reduced, and the moldability is further improved. 3 The following is the result.
[0027] The oxidized polyethylene wax preferably has a melting point of 80°C or higher. When the melting point is 80°C or higher, the amount of sublimates and the like is reduced, and the chlorine-containing resin composition of the present invention can exhibit the effect of reducing surface defects in molded articles during molding processability. The melting point of the oxidized polyethylene wax is more preferably 85°C or higher, and even more preferably 90°C or higher. The melting point of the oxidized polyethylene wax is usually 150°C or lower.
[0028] The oxidized polyethylene wax preferably has a viscosity of 1000 cps or less at 140°C. When the viscosity is 1000 cps or less at 140°C, the chlorine-containing resin composition of the present invention has excellent moldability. The viscosity of the oxidized polyethylene wax at 140°C is preferably 800 cps or less, more preferably 500 cps or less.
[0029] In this specification, the acid value, density, melting point and viscosity at 140°C of the oxidized polyethylene wax are all measured by the methods described in the Examples.
[0030] Examples of oxidized polyethylene waxes include the Hiwax series manufactured by Mitsui Chemicals, Inc., the Sanwax series manufactured by Sanyo Chemical Industries, Ltd., the Viscol series manufactured by Sanyo Chemical Industries, Ltd., the Lubax series manufactured by Nippon Seiro Co., Ltd., and the AC series manufactured by Honeywell, among which waxes that satisfy the above physical properties can be used as appropriate.
[0031] The content of the oxidized polyethylene wax in the chlorine-containing resin composition of the present invention is preferably 0.01 to 2.0 parts by mass per 100 parts by mass of the chlorine-containing resin. This more satisfies the effect of suppressing appearance defects in molded articles. The content is more preferably 0.01 to 1.5 parts by mass, and even more preferably 0.01 to 1.0 part by mass.
[0032] [Hydrotalcite] The hydrotalcite contained in the chlorine-containing resin composition of the present invention is not particularly limited, but it is preferable that the hydrotalcite contains magnesium element (Mg) and / or zinc element (Zn) and aluminum element (Al).
[0033] The hydrotalcite-type powder is particularly preferably a powder represented by the following general formula (1): {(Mg) x (Zn) y} (Al) z (OH) 2 (A n- ) x/n ・mH 2 O (1) (wherein, A n-represents an n-valent interlayer anion. x, y, and z are numbers satisfying 0<x<1, 0≦y<1, 0.2≦z≦0.4, and x+y+z=1, and the ratio of x+y to z {(x+y) / z} is 2.2 or less. n and m are numbers satisfying 1≦n≦4 and 0≦m, respectively. This further improves the heat resistance and thermal stability of the chlorine-containing resin composition.
[0034] In the general formula (1), the n-valent interlayer anion is not particularly limited, but from the viewpoint of reactivity and reduction of environmental load, hydroxide ion (OH - ), carbonate ions (CO 3 2- ) and sulfate ions (SO 4 2- Among these, carbonate ions are preferred.
[0035] x, y, and z are numbers that satisfy the relationships 0<x<1, 0≦y<1, 0.2≦z≦0.4, and x+y+z=1, and the ratio of x+y to z {(x+y) / z} is 2.2 or less. Here, one in which y=0 is called an Mg / Al-based hydrotalcite, and one in which 0<y is called a zinc-modified hydrotalcite. Either of these can be suitably used in the present invention.
[0036] The ratio of x+y to z {(x+y) / z} is preferably 2.1 or less, more preferably 2.05 or less. There is no particular lower limit, but the ratio is preferably 1.9 or more, more preferably 2.0 or more.
[0037] n is a number that satisfies the relationship 1≦n≦4, and may be appropriately adjusted depending on the valence of the interlayer anion.
[0038] The hydrotalcite preferably has an oil absorption of 50 ml / 100 g or less. This improves the gloss of molded articles obtained from the chlorine-containing resin composition of the present invention. The oil absorption of the hydrotalcite is more preferably 45 ml / 100 g or less, and even more preferably 40 ml / 100 g or less. Furthermore, from the viewpoint of heat resistance, it is preferably 5 ml / 100 g or more, and more preferably 10 ml / 100 g or more.
[0039] In this specification, the oil absorption of the hydrotalcite-type powder is measured in accordance with JIS K5101-13-1 (2004: refined linseed oil method).
[0040] The shape of the hydrotalcite particles is not particularly limited, and examples thereof include plate-like, spherical, and disc-like shapes. Among these, plate-like and disc-like shapes are preferred. The particle shape can be observed using a scanning electron microscope or the like.
[0041] The average particle size of the hydrotalcite particles is preferably, for example, 0.1 μm or more and 2.0 μm or less. This improves dispersibility in chlorine-containing resins and further enhances the effects of the present invention. It is more preferably 0.3 μm or more and more preferably 1.5 μm or less.
[0042] In this specification, the average particle size can be measured as D50 using, for example, a laser diffraction particle size distribution analyzer (HORIBA LA950). D50 means the 50% cumulative particle size on a volume basis.
[0043] The specific surface area (SSA) of the hydrotalcite is, for example, 1 m 2 / g or more, 50m 2 / g or less. This improves the dispersibility in chlorine-containing resins, and further improves the effects of the present invention. 2 / g or more, more preferably 10m 2 / g or more, and more preferably 40m 2 / g or less, more preferably 30m 2 When the specific surface area is in this range, a resin composition having excellent heat resistance can be obtained.
[0044] In this specification, the specific surface area refers to the BET specific surface area (also referred to as SSA) obtained by the BET method. The BET method is a gas adsorption method in which gas particles such as nitrogen are adsorbed onto solid particles and the specific surface area is measured from the amount of adsorption. The specific surface area is determined by calculating the monomolecular adsorption amount VM using the BET formula from the relationship between the pressure P and the adsorption amount V. Specifically, the BET specific surface area is measured under the following conditions:
[0045] [Measurement conditions for specific surface area] Machine used: Macsorb Model HM-1220 manufactured by Mountec Co., Ltd. Adsorption gas: nitrogen (N 2 Degassing conditions for the external degassing device: 105°C - 15 minutes Degassing conditions for the specific surface area measuring device: 105°C - 5 minutes
[0046] In the hydrotalcite, particles in the powder may have a coating layer. In this case, it is preferable that the physical properties of the hydrotalcite containing particles having the coating layer satisfy the above-mentioned physical properties (particle shape, average particle diameter, specific surface area, etc.). The coating layer is not particularly limited, but it is preferable that the coating layer is formed by performing a surface treatment using a surface treatment agent.
[0047] The surface treatment agent is not particularly limited, and examples thereof include higher fatty acids, higher fatty acid metal salts (metal soaps), anionic surfactants, phosphate esters, and coupling agents such as silane coupling agents, titanium coupling agents, and aluminum coupling agents. One or more of these may be used.
[0048] More specific examples of the surface treatment agent include higher fatty acids such as stearic acid, oleic acid, erucic acid, palmitic acid, and lauric acid; metal salts of these higher fatty acids such as lithium salts, sodium salts, and potassium salts; sulfate ester salts of higher alcohols such as stearyl alcohol and oleyl alcohol; sulfate ester salts of polyethylene glycol ether, amide-bonded sulfate ester salts, and ether-bonded sulfonates; anionic surfactants such as ester-bonded sulfonates, amide-bonded alkylaryl sulfonates, and ether-bonded alkylaryl sulfonates; mono- or di-substituted or unmodified alkylaryl sulfonates of orthophosphoric acid and oleyl alcohol, stearyl alcohol, or the like; are diesters or mixtures thereof, and examples thereof include phosphate esters such as their acid form or alkali metal salts or amine salts; silane coupling agents such as vinylethoxysilane, γ-methacryloxypropyltrimethoxysilane, vinyltris(2-methoxyethoxy)silane, γ-aminopropyltrimethoxysilane; titanium coupling agents such as isopropyl triisostearoyl titanate, isopropyl tris(dioctylpyrophosphate)titanate, isopropyl tridecylbenzenesulfonyl titanate; and alkali coupling agents such as acetoalkoxyaluminum diisopropylate.
[0049] The amount of the surface treatment agent used is not particularly limited, but for example, it is preferable to adjust the amount of the surface treatment agent used so that the amount of coating with the surface treatment agent is in the range of 0.1 to 30 mass%, more preferably 0.1 to 20 mass%, relative to 100 mass% of the finally obtained hydrotalcite containing particles having a coating layer.
[0050] In the resin composition, the content of hydrotalcite is, for example, preferably 0.05 parts by mass or more and preferably 10 parts by mass or less per 100 parts by mass of the chlorine-containing resin. This further improves heat resistance and thermal stability. It is more preferably 0.1 parts by mass or more, more preferably 8 parts by mass or less, and even more preferably 5 parts by mass or less.
[0051] [β-Diketone Compound, β-Diketo Metal Salt] The chlorine-containing resin composition of the present invention contains a β-diketone compound and / or a β-diketo metal salt, which can improve colorability during molding.
[0052] The β-diketone compound is not particularly limited, but suitable examples include acetylacetone and alkanoyl aroyl methanes and diaroyl methanes such as stearoyl acetyl methane, benzoyl acetyl methane, dibenzoyl methane, stearoyl benzoyl methane, octyl benzoyl methane, bis(4-octyl benzoyl) methane, 4-methoxy benzoyl benzoyl methane, bis(4-carboxymethyl benzoyl) methane, 2-carboxymethyl benzoyl acetyl octyl methane, and 2-benzoyl cyclohexane. Suitable β-diketo metal salts are metal salts of the above-mentioned β-diketone compounds. The metal species of the metal salt is not particularly limited, but examples include calcium and zinc.
[0053] The content of the β-diketone compound and / or β-diketo metal salt in the resin composition is preferably 2.0 parts by mass or less, more preferably 0.01 to 1.0 part by mass, per 100 parts by mass of the chlorine-containing resin.
[0054] [Release Agent] The chlorine-containing resin composition of the present invention preferably contains a release agent. Examples of the release agent include dipentaerythritol hexastearate and pentaerythritol tetrastearate. Among these, dipentaerythritol hexastearate is preferred. This can more sufficiently prevent the chlorine-containing resin composition of the present invention from causing smearing or streaking.
[0055] When the chlorine-containing resin composition of the present invention contains a mold release agent, the content thereof is not particularly limited, but is preferably 0.01 to 5.0 parts by mass, more preferably 0.01 to 2.0 parts by mass, per 100 parts by mass of the chlorine-containing resin.
[0056] [Filler] The chlorine-containing resin composition of the present invention preferably also contains a filler. This improves the dimensional stability and strength of the molded article, making the resin composition preferable for use in molded articles. The filler also functions as a neutralizing agent.
[0057] The filler is not particularly limited, and examples thereof include inorganic powders such as inorganic salts, inorganic oxides, and inorganic hydroxides, such as salts, oxides, hydroxides, and composite oxides of zinc, titanium, iron, cerium, barium, calcium, silicon, aluminum, magnesium, strontium, boron, and zirconium. The salts are not particularly limited, and examples thereof include sulfates, carbonates, chlorides, acetates, and nitrates. Specific examples thereof include calcium carbonate, zinc carbonate, magnesium carbonate, silica, zinc oxide, titanium oxide, cerium oxide, iron oxide, barium sulfate, strontium sulfate, magnesium sulfate, silicon oxide, aluminum oxide, magnesium oxide, zinc silicate, zinc titanate, barium titanate, and talc, with calcium carbonate being preferred.
[0058] Among calcium carbonates, the one with a specific surface area (BET specific surface area) of 25m 2 / g or less is preferable. 2 / g or less, more preferably 20m 2 / g or less, particularly preferably 18m 2 / g or less, and the lower limit is 0.1 m 2 / g or more is preferable. 2 If the content exceeds the above range, adverse effects such as plate-out may occur during processing.
[0059] When the resin composition contains a filler, the content thereof is not particularly limited, and is preferably, for example, 40 parts by mass or less relative to 100 parts by mass of the chlorine-containing resin. If the content exceeds 40 parts by mass, plate-out may not be suppressed. It is more preferably 30 parts by mass or less, and even more preferably 1 to 30 parts by mass. It is even more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less, and the lower limit is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and even more preferably 3 parts by mass or more. Most preferably, it is a resin having a specific surface area of 20 m 2 The calcium carbonate content of 1 / g or less is within these preferred ranges.
[0060] [Other Components] The chlorine-containing resin composition of the present invention may further contain other components as necessary, such as various additives such as a heat resistance aid, a lubricant other than the oxidized polyethylene wax (c) above, an ultraviolet absorber, an antioxidant, a crosslinking aid, and a plasticizer. The additives are not particularly limited, and examples thereof include heat resistance aids such as polyhydric alcohol compounds such as dipentarythritol and epoxy compounds such as epoxy resins; lubricants such as stearic acid monoglyceride, palmitic acid monoglyceride, stearic acid, palmitic acid, and polyethylene waxes other than the oxidized polyethylene wax of (c) above; ultraviolet absorbers such as benzophenone compounds, benzotriazole compounds, and aromatic benzoate compounds; antioxidants such as phenol compounds; crosslinking aids such as trimethylolpropane trimethacrylate and dipentaerythritol hexaacrylate; and plasticizers such as dioctyl phthalate (DOP), trioctyl trimellitate (TOTM), and dioctyl adipate (DOA).
[0061] The chlorine-containing resin composition of the present invention preferably has a plasticizer content of 5% by weight or less relative to the total composition. Poor appearance is more likely to occur in molded articles obtained from hard resin compositions with a low plasticizer content. Therefore, the effects of the present invention are more pronounced when the resin composition is a hard one with a low plasticizer content. The plasticizer content is more preferably 1.0% by weight or less, and even more preferably 0.01% by weight or less.
[0062] Examples are given below to explain the present invention in detail, but the present invention is not limited to these examples.
[0063] 1. Raw Materials The raw materials listed in Tables 1-1 and 1-2 below are as follows: (a) Chlorine-containing vinyl chloride resin: TK-1000, manufactured by Shin-Etsu Chemical Co., Ltd., degree of polymerization 1000
[0064] (b) Organic zinc salt zinc stearate: SZ-P (Ca-Zn stabilizer) manufactured by Sakai Chemical Industry Co., Ltd.
[0065] (c) Oxidized polyethylene wax AC polyethylene 629A: manufactured by Honeywell AC polyethylene 656: manufactured by Honeywell AC polyethylene 307A: manufactured by Honeywell AC polyethylene 316A: manufactured by Honeywell AC polyethylene 6A: manufactured by Honeywell
[0066] (d) Hydrotalcite Synthesis was carried out by the hydrotalcite production procedure described in Example 4 of Japanese Patent No. 5,056,014, while varying the molar ratios of magnesium sulfate, aluminum sulfate, and zinc sulfate and the production conditions, and for each production run, the oil absorption and specific surface area were measured by the methods described below, and the hydrotalcite-type powders listed in Tables 1-1 and 1-2 were selected.
[0067] (e) β-diketone compound, β-diketo metal salt dibenzoylmethane: Rhodia Stab 83P, manufactured by Rhodia Corporation
[0068] (f) Filler calcium carbonate: KS-1000 manufactured by Calfine Co., Ltd., specific surface area 1.15 m 2 / g
[0069] (g) Other ingredients: Calcium stearate: SC-P (Ca-Zn stabilizer) manufactured by Sakai Chemical Industry Co., Ltd.; Dipentaerythritol: Dipentalit 300 manufactured by Koei Chemical Co., Ltd.; Polyethylene wax: Hiwax 220MP manufactured by Mitsui Chemicals, Inc.; Ester wax (dipentaerythritol hexastearate): Lykestar SL-02 manufactured by Riken Vitamin Co., Ltd.
[0070] Examples 1 to 8, Comparative Examples 1 to 7 The physical properties of the oxidized polyethylene wax and hydrotalcite used in the examples and comparative examples, and the formulations of the components of the resin compositions prepared containing these oxidized polyethylene waxes and hydrotalcites are shown in Tables 1-1 and 1-2. The physical properties of the oxidized polyethylene wax and hydrotalcite were measured using the following measurement methods. Tables 1-1 and 1-2 also show the evaluation results of the striations and gloss on the surface of molded articles of the obtained resin compositions, which were evaluated using the following methods.
[0071] <Measurement of physical properties of oxidized polyethylene wax> [Acid value] Measured in accordance with ASTM D-1386. [Density] Measured in accordance with ASTM D-1505. [Melting point (dropping point)] Measured in accordance with ASTM D-3954. [Viscosity at 140°C] The viscosity at 140°C was measured using a Brookfield viscometer. [FT-IR peak intensity ratio] Measured by Fourier transform infrared spectroscopy using the following device and measurement method. Manufacturer: Thermo Fisher Scientific Model: NICOLET 4700 Measurement method: ATR method / single reflection (plate used: diamond prism plate) Measurement procedure: (1) Measure the background without placing anything on the plate. (2) After measuring the background, press about one teaspoon of sample onto the plate and measure. (3) After the sample measurement, "Advanced ATR correction" is performed and the result is used as the measurement result. <Measurement of physical properties of hydrotalcite> [Oil absorption] Measured in accordance with JIS K5101-13-1 (2004: refined linseed oil method).
[0072] <Molding> The resin composition was used in a laboratory extruder (Toyo Seiki Co., Ltd., Conical 2D20C model) equipped with a suction sizing (a device for smoothing the surface of molded products) and a cooling function, and pipes were extruded for 5 consecutive hours. The pipes were then cut at regular lengths to obtain molded pipes. The extrusion conditions were set as follows: Cylinder temperatures, from the position closest to the raw material inlet, were 175°C for Cylinder 1, 180°C for Cylinder 2, and 185°C for Cylinder 3; adapter mold temperatures were 185°C, Mold 1 180°C, and Mold 2 205°C. Molds for pipes were used.
[0073] <Evaluation of Resin Composition> [Scoring] The occurrence of scoring in the pipe molded product obtained after a predetermined time has elapsed since the start of extrusion molding (i.e., the occurrence of scratches in the pipe molded product) was visually inspected and rated according to the following criteria. ⊚: No scratches were observed in the pipe molded product after 5 hours. ◯: Scratches were observed in the pipe molded product after 3 hours. Δ: Scratches were observed in the pipe molded product after 1 hour. ×: Scratches were observed in the pipe molded product after 1 hour. [Gloss] The gloss of the pipe molded product obtained after a predetermined time has elapsed since the start of extrusion molding was visually inspected and rated according to the following criteria. ⊚: It was confirmed that the gloss was maintained in the pipe molded product after 5 hours. ◯: Gloss was observed after 3 hours, but the gloss was lost in the pipe molded product after 5 hours, and the surface of the molded pipe was confirmed to be faded. Δ: Gloss was observed after 1 hour, but the gloss was lost in the pipe molded product after 3 hours, and the surface of the molded pipe was confirmed to be faded. x: It was confirmed that there was no gloss immediately after molding and the surface of the molded pipe was in a faded state.
[0074]
[0075] From the results of Tables 1-1 and 1-2, the FT-IR measurement showed that -1 Peak and 2930cm -1It has been confirmed that the inclusion of an oxidized polyethylene wax having an absorbance ratio of 0.05 or more to the peak of Ca-Zn stabilizer can effectively suppress the occurrence of defects on the surface of a molded product of a chlorine-containing resin composition using a Ca-Zn stabilizer.
Claims
1. A composition comprising (a) a chlorine-containing resin, (b) an organic acid zinc salt, (c) an oxidized polyethylene wax, (d) hydrotalcite, and (e) a β-diketone compound and / or a β-diketo metal salt, wherein the (c) oxidized polyethylene wax has a peak at 1720 cm in FT-IR measurement. -1 Peak and 2930cm -1 The absorbance ratio of the peak (1720 cm -1 Peak absorbance / 2930 cm -1 A chlorine-containing resin composition characterized in that the peak absorbance (absorbance) is 0.05 or more.
2. The chlorine-containing resin composition according to claim 1, wherein the oxidized polyethylene wax (c) has an acid value of 1 mgKOH / g or more.
3. The (c) oxidized polyethylene wax has a density of 0.95 g / cm 3 3. The chlorine-containing resin composition according to claim 1, wherein:
4. The chlorine-containing resin composition according to any one of claims 1 to 3, characterized in that the oxidized polyethylene wax (c) has a melting point of 80°C or higher.
5. A chlorine-containing resin composition according to any one of claims 1 to 4, characterized in that the (c) oxidized polyethylene wax has a melt viscosity of 1000 cps or less at 140°C.
6. A chlorine-containing resin composition according to any one of claims 1 to 5, characterized in that the (d) hydrotalcite has an oil absorption of 50 ml / 100 g or less.
7. The chlorine-containing resin composition according to any one of claims 1 to 6, further comprising (f) dipentaerythritol hexastearate.
8. A chlorine-containing resin composition according to any one of claims 1 to 7, characterized in that the content of the plasticizer in the chlorine-containing resin composition is 5% by weight or less based on the total weight of the composition.
9. The chlorine-containing resin composition according to any one of claims 1 to 8, further comprising 30 parts by mass or less of calcium carbonate per 100 parts by mass of the chlorine-containing resin.