Process for membrane production

LAP85AUndetermined Publication Date: 2025-12-12LENZING AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP85
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2006-05-10
Filing Date
2007-05-09
Publication Date
2025-12-12

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The invention relates to a process for producing soluble membranes from cellulosic starting materials using the kraft paper process, which comprises a material boiling step where the starting material is subjected to a steam treatment prior to boiling and where the membrane obtained from boiling undergoes cold extrusion (CCE) in a subsequent processing step.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Process for the production of pulp

[0002] The present invention relates to a method for producing a pulp from a cellulosic starting material using the Kraft process.

[0003] In particular, the invention relates to a process for producing a high-yield pulp suitable for further processing into viscose fibers and lyocell fibers.

[0004] Chemical pulp is predominantly processed into cellulosic fibers using the viscose and lyocell processes. Over the past few years, the cost position of regenerated fibers has deteriorated further compared to competing synthetic fibers. A reduction in pulp costs, which represent the most significant cost factor, would considerably improve the cost position of regenerated fibers.

[0005] Luo et al. demonstrated that conventional kraft pulp, after adjusting the average degree of polymerization (DP) by acid hydrolysis or oxidative degradation, is suitable for the production of cellulosic fibers using the lyocell process [WO 99 / 47733]. Kraft pulps produced according to this prior art have a hemicellulose content of at least 7% wt.%. Lyocell fibers produced from these kraft pulps have a hemicellulose content of at least 5% wt.% to 27% wt.% according to WO 99 / 47733. However, the measurement method used to determine the hemicellulose content is not disclosed.

[0006] However, the presence of low molecular weight molecules has a disadvantageous effect.

[0007] Hemicellulose components affect the process behavior (enrichment of non-fiber-forming hemicellulose components in the spinning bath; high chemical expenditure for depolymerization to adjust the desired DP) and the textile mechanical properties (more than 5 cN / tex lower strength under conditioned conditions compared to lyocell fibers from pre-hydrolysis kraft pulps) of the lyocell fibers produced therefrom.

[0008] Since the development of the "modified power boiling" in the early 1980s, it has been known that lowering the concentration of dissolved wood components in the final phase of boiling results in a significant increase in efficiency and selectivity.

[0009] To reflect this knowledge, it was proposed to add hemicellulose-rich liquor streams, such as those that occur after the end of the co-current cooking phase in continuous cooking processes (e.g., MCC, EMCC), to the cooking process. The high molecular weight hemicelluloses are removed to ensure that the concentration level of dissolved hemicelluloses decreases to less than 10 g / l during the subsequent cooking phase [WO 95 / 00698]. In a further step, the high molecular weight hemicelluloses are concentrated further using pressure-driven membrane separation processes before being reprecipitated on the surface of the cellulose fibers in a post-bleaching step (E-stage) to increase both the yield and the static strength.

[0010] Although this proposal results in an improved pulp yield, the disadvantage is that the non-adsorbed portion of the hemicelluloses (equilibrium reaction) inevitably accumulates in the bleach filtrate, causing increased consumption of bleaching chemicals, and some of it also enters the wastewater.

[0011] The present invention aims to provide a process for the production of pulp which solves in an improved manner the problems of pulp production described above according to the Kraft process.

[0012] This problem is solved by a process for producing a chemical pulp from a cellulosic starting material using the Kraft process, comprising the step of boiling the starting material with a cooking lye, which is characterized in that the starting material is exposed to a steam treatment before boiling and that the pulp obtained by boiling is subjected to a cold alkali extraction (CCE) in the course of further treatment.

[0013] It has been shown that by combining measures such as steam treatment of the starting material before cooking and a CCE stage in further processing, a pulp can be obtained in high yield and purity, which is ideally suited for the production of viscose and lyocell fibers.

[0014] Steam treatment is preferably carried out at a temperature of 120°C or more and a P-factor of 50 or less. These are significantly more intensive conditions than those of "low temperature steaming," as described, for example, in WO 98 / 15687.

[0015] Under the conditions preferred according to the invention, steam treatment results in an increase in the porosity of the pulping material (wood chips) as well as a partial cleavage of the lignin-carbohydrate bonds. However, no chemical cleavage of the glycosidic bonds takes place, as would be the case in a pre-hydrolysis process. Typically, P-factors of more than 50 are achieved in a pre-hydrolysis process. The concept of the "P-factor" is described, for example, in "Handbook of PuIp", Vol. 1, Wiley-VCH 2006, pages 343-345. The intensity of the steam treatment according to the invention is preferably only about one-tenth that of a conventional pre-hydrolysis.

[0016] This means that, in contrast to pre-hydrolysis processes, the steam treatment according to the invention yields a higher pulp yield and thus more economical production. Although the resulting pulp also contains a higher proportion of hemicelluloses, the combination of steam treatment and cold alkali extraction according to the invention apparently ensures that the pulp is nevertheless ideally suited for the production of cellulose fibers.

[0017] For steam treatment, the starting material is preferably treated at a temperature of 150 to 180°C. 0 C treated with medium-pressure steam.

[0018] The raw material can be impregnated before cooking in a manner known per se. If steam treatment is also carried out, the impregnation takes place after the steam treatment.

[0019] In the process according to the invention, the cooking and, if necessary, the steam treatment and / or the impregnation of the starting material can be carried out in the same cooker.

[0020] Preferably, in the process according to the invention, cooking is carried out in the form of continuous batch cooking (CBC). CBC technology is known, for example, from EP 0 891 438 Bl and from Wizani, W., et al. "CBC - Continuous batch cooking. The revolution in kraft cooking" in Pulping process and product quality Conference, 2000, Boston, MA, USA.

[0021] When using CBC technology, the steps of impregnation and hot displacement (i.e., the displacement of the impregnating liquor by cooking liquor) correspond to the procedures commonly used in CBC technology. The kraft pulps produced according to the invention can be subjected to TCF or ECF bleaching in a manner known per se in order to achieve the required purity and whiteness levels.

[0022] In a further preferred embodiment, a portion of the press liquor produced in the cold alkali extraction stage can be purified by means of a membrane separation process, preferably nanofiltration or ultrafiltration, and at least a portion of the retentate from the membrane separation process can be added to the second cooking liquor.

[0023] The purification of the press liquor from a CCE-V process using a membrane separation method is described in WO 2005 / 118923. The resulting retentate contains all of the beta-cellulose present in the press liquor and more than half of the gamma-cellulose. In the case of hardwood pulp, the beta-cellulose solution consists of almost pure xylan.

[0024] The membrane separation process can be carried out in two stages, with the retentate of the first stage being diluted with water between the two separation stages.

[0025] In the second stage, nanofiltration of the diluted retentate or dialysis of the retentate from the first stage can be performed. In both cases, this step increases NaOH recovery while simultaneously concentrating the hemicellulose phase.

[0026] Instead of or in addition to recycling the retentate to the second cooking liquor, the hemicelluloses contained therein, particularly xylans, can be recovered from at least a portion of the retentate from the membrane separation process. US Patent 2005 / 0203291 describes a process for recovering xylans from a phase rich in xylans.

[0027] In contrast to this known method, in a preferred embodiment of the method according to the invention, precipitable hemicelluloses, in particular the xylans, are obtained from the retentate of the membrane separation process by means of a reverse precipitation.

[0028] For the reverse precipitation, an agent from the group consisting of mineral acids, CO2, and mono- or polyhydric alcohols is preferably used. The sedimentation residue can then be washed and mechanically dewatered using suitable equipment (e.g., a washing press).

[0029] The xylans obtained in this way can be at least partially processed into xylo-oligosaccharides. Xylooligosaccharides have various applications, e.g., as a prebiotic food additive.

[0030] For the production of these xylo-oligosaccharides, a process selected from the group consisting of hydrothermolysis and enzymatic hydrolysis can preferably be carried out.

[0031] Another preferred embodiment of the process according to the invention is characterized in that it is coupled with a process for the production of paper pulp and at least a part of the press liquor produced in the cold alkali extraction stage and / or at least a part of the retentate of a membrane separation process carried out on the press liquor is fed to the boiling liquor of a boiling process carried out for the production of paper pulp.

[0032] By coupling the chemical pulp and paper pulp production and utilizing the material flows generated in the CCE step of the process according to the invention in paper pulp production, both a qualitative and economic improvement of the paper pulp production process is possible.

[0033] As described above, the filtrate from the CCE stage or the retentate of a nanofiltered CCE filtrate contains a high hemicellulose content. A cooking liquor enriched with hemicellulose is particularly suitable for the production of high-yield paper pulp with an increased hemicellulose content.

[0034] Another preferred embodiment of the process according to the invention is characterized in that, in addition to any bleaching step carried out, a treatment to adjust the degree of polymerization (DP) is performed on the pulp obtained by boiling during further processing.

[0035] The treatment is preferably selected from the group consisting of oxidative bleaching processes, acid hydrolysis processes and electron irradiation processes. The degradation of phosphorus (DP) in cellulose to a desired DP level can be achieved through both chemical-oxidative processes and electron beam irradiation. Hypochlorite or ozone treatments are best suited as oxidizing agents for DP degradation. A disadvantage of chemical-oxidative processes is that, due to limited accessibility (of the oxidizing agents) to the crystalline regions, chain degradation proceeds very heterogeneously, resulting in a significantly broader molar mass distribution than would be expected from a statistically determined degradation.

[0036] In contrast, electron irradiation shows a largely statistical degradation, so that the polydispersity of the molar mass distribution decreases significantly more with progressive DP degradation than in the case of chemical-oxidative degradation processes, as could be shown using the example of ozone treatment.

[0037] Electron irradiation of cellulose pulps for DP adjustment is a well-known technique and has been investigated by many research groups [e.g., Kukielka, A., et al., Electron-beam treatment of cellulose pidps for production derivatives. Zeszyty Naukowe Politechniki Slaskiej, Chemia, 2001. 146: p. 117-120; Hier, E., et al., Electron-beam stimulation of the reactivity of cellulose pulps for production of derivatives. Radiation Physics and Chemistry, 2002. 63: p. 253-257; Stepanik, TM, DE Ewing, and R. Whitehouse, Electron treatment of wood pulp for the viscose process. Radiation Physics and Chemistry, 2000. 57: p. 337-379].

[0038] In this work, the authors assume that electron irradiation is used as a replacement for the alkaline pre-ripening of finished pulp. Since electron irradiation leaves highly reactive groups (carbonyl groups) in the pulp, subsequent alkaline treatment causes further significant degradation of dimethyl groups (DPs) and the formation of chromophore structures in the alkali cellulose.

[0039] The use of irradiated pulp in the lyocell process has an even more detrimental effect. Here, the reactive groups induce degradation reactions of the solvent NMMO, whose degradation products in turn further damage the cellulose. This is one of the reasons why DP adjustment via electron irradiation has not yet been carried out in practice.

[0040] The present invention circumvents this problem by subjecting the pulp to electron irradiation (“E-beam” treatment) at any position in the fiber line, i.e. during the pulp manufacturing process, from the unbleached pulp to before the final bleaching stage. The electron irradiation of the pulp can preferably be carried out in such a way that the pulp is present in a material density of at least 35%, preferably 40-50% and in a layer thickness of 2 to 6 mm, preferably 3 to 4 mm, and an accelerating voltage of less than 2.5 MeV is used.

[0041] Layer thicknesses between 2 and 6 mm can also be achieved with low

[0042] Acceleration voltages can be irradiated largely homogeneously. The water content present in the cellulose nonwoven fabric must, of course, be taken into account when selecting the irradiation dose. The dose required for a specific degradation of depleted phosphorus (DP) roughly doubles at a fabric density of 50%.

[0043] Another advantageous embodiment of the method according to the invention consists in carrying out an alkaline-oxidative treatment, preferably an alkaline peroxide treatment, after the treatment to adjust the degree of polymerization.

[0044] Particularly labile groups formed by electron beam irradiation are stabilized by this subsequent alkaline peroxide stage and therefore cannot have a detrimental effect on further processing. In a peroxide (P) stage following an EBeam stage, the carbonyl groups are largely oxidized to carboxyl groups. This produces short-chain compounds with strongly chromophoric groups, which are washed into the bleach filtrate. The high-molecular-weight, oxidized residues exist mostly as aldonic acid groups and are thus stable against subsequent alkaline treatments.

[0045] The following are typical process concepts when using electron irradiation:

[0046] TCF bleaching sequence:

[0047] W-EBeam-OP-AZP; W-EBeam-OP-AP, W-EBeam-OP-P, W-OP-AZ-EBeam-P, W-OP-

[0048] A-EBeam-P, W-OP-EBeam-P.

[0049] ECF bleaching sequence:

[0050] W-EBeam-OP-DEP; W-EBeam-OP-DED, W-EBeam-DED, WDE-EBeam-P The abbreviations used mean: W... washing, OP... peroxide-enhanced oxygen delignification, E... alkaline extraction, D... chlorine dioxide stage, Z... ozone stage, P... alkaline peroxide stage.

[0051] Another preferred embodiment of the process according to the invention is characterized in that the cooking step of the pulp is carried out in two stages, wherein in the first stage delignification is carried out by means of a first cooking liquor to a kappa number of 35 to 70 in the case of coniferous woods as starting material and to a kappa number of 30 to 60 in the case of deciduous woods as starting material, and in the second stage the cooking is continued by means of a second cooking liquor until the desired degree of purity of the pulp is reached.

[0052] This embodiment is therefore based on the concept of two-stage power cooking.

[0053] The task of the first cooking stage is to carry out the main part of the bulk delignification. According to the invention, coniferous woods are delignified to a kappa number of 35 to 70 and deciduous woods to a kappa number of 30 to 60.

[0054] The proportion of the H-factor of the first cooking stage, relative to the H-factor of both cooking stages combined, is preferably 40% to 80% in the case of coniferous wood as starting material or 20% to 60% in the case of deciduous wood as starting material.

[0055] The H-factor defines the relative rate of lignin dissolution and depends on the cooking time and temperature. An H-factor of 1 corresponds to a cooking time of 1 hour at 100°C. The H-factor expresses the cooking time and cooking temperature as a single variable. It represents a relative reaction rate (referenced to a temperature of 100°C). 0C, where the reaction rate is by definition 1), which is calculated using an Arrhenius approach with a specific activation energy, is integrated over the time of boiling.

[0056] Preferably, during the transition from the first to the second cooking stage, the first cooking liquor is replaced by the second. For example, in the case of a continuous cooking process, the supply of the first cooking liquor can be stopped and simultaneously the supply of the second cooking liquor from a second tank can be started. Selecting suitable flow rates ensures a largely complete introduction of the cooking liquor during both cooking phases. The first cooking liquor preferably has an EA (effective alkali) concentration of 10 g / L to 30 g / L, preferably 15 g / L to 25 g / L, particularly preferably 20 g / L, and a sulfidity of 50% to 120%, preferably 100%. The sulfidity S is defined according to the test method SCAN-N 30:85 as S = 2[HS] / ([OH]+[HS]).

[0057] In another preferred embodiment, the composition of the second cooking liquor differs from that of the first cooking liquor.

[0058] The composition of the second cooking liquor can be adapted to the respective requirements for pulp quality, particularly by adding suitable liquor streams.

[0059] Preferably, the second cooking liquor can be enriched with a liquor selected from the group consisting of the filtrate of a subsequent washing stage, a white liquor from causticization, and the press liquor from a cold alkali extraction stage.

[0060] Preferably, in the inventive method, both cooking stages are carried out in the form of continuous batch cooking (CBC). This technology offers, in particular, greater flexibility with regard to the design of the second cooking stage. In the case of modified continuous cooking processes, the addition of either hemicellulose-rich or hemicellulose-poor cooking liquor in the countercurrent cooking zone (MCC and EMCC / ITC cooking processes) or in the extended cooking zone (EMCC / ITC cooking processes) is advantageous.

[0061] The present invention also relates to the use of the chemical pulps produced according to the invention for the production of viscose and lyocell fibers.

[0062] The methods for producing viscose and lyocell fibers are known to experts.

[0063] Lyocell fibers, which are obtainable by spinning a chemical pulp produced according to the invention, are characterized in particular by the following features:

[0064] Their hemicellulose content (H) is preferably more than 3.5 wt.% and is therefore somewhat higher than the hemicellulose content of lyocell fibers, which are produced from high-quality and complex (i.e., especially with comparatively low yield) pre-hydrolysis Kraft pulps, as described, for example, in WO 94 / 12719, are produced. The H content can be less than 5 wt.%.

[0065] Despite this increased hemicellulose content, the mercerization yield of the lyocell fiber according to the invention (according to the measurement method described below) is 90% or more. Thus, the lyocell fiber according to the invention exhibits a significantly higher mercerization resistance than lyocell fibers produced from a non-inventive kraft pulp with a high hemicellulose content, as described, for example, in WO 99 / 47733.

[0066] The strength of the lyocell fiber according to the invention is 37 cN / tex or more in the conditioned state and is therefore in the same range of values ​​that could previously only be achieved using high-quality and expensively produced pre-hydrolysis kraft pulps.

[0067] Lyocell fibers produced according to the invention also differ from those produced from such high-quality pre-hydrolysis kraft pulps in that the mean molar mass of the xylans isolable from the fiber is 20 kDa or more (see the measurement method described below). In contrast, xylans from lyocell fibers derived from high-quality pre-hydrolysis kraft pulps (or sulfite pulps) have a mean molar mass (Mw) of < 10 kDa.

[0068] In summary, the lyocell fibers according to the invention are thus clearly distinguishable from previously known fibers and have the advantage that they exhibit excellent fiber properties despite the use of the chemical pulp which can be produced relatively cheaply according to the inventive process.

[0069] The present invention also relates to a viscose fiber obtainable by spinning a chemical pulp produced according to the invention.

[0070] The viscose fiber according to the invention is characterized in particular by its hemicellulose content (H) being more than 2.0 wt.% and its mercerization resistance being 90% or higher. Despite the high hemicellulose content, the strength of the viscose fiber according to the invention is comparable to that of the best viscose fibers produced from high-quality pre-hydrolysis kraft pulp (or sulfite pulp). In particular, the viscose fiber according to the invention can achieve a strength in conditioned exhibit a condition of 23 cN / tex or more and an elongation in conditioned condition of 18% or more.

[0071] The present invention will be explained in more detail below with reference to the figures and examples.

[0072] Figure 1 shows a diagram of the basic concept of the inventive method and its possible applications.

[0073] Figure 2 shows a plot of marginal viscosity vs. kappa number of one- and two-stage CBC boilings of spruce wood.

[0074] Figure 3 shows temperature and hydroxide ion profiles of single- and two-stage softwood CBC boiling processes.

[0075] Figure 4 shows a plot of total yield vs. kappa number of one- and two-stage Eucalyptus g / oZm / ws-CBC boils with and without hemicellulose enrichment.

[0076] Figure 5 shows a plot of marginal viscosity number vs. kappa number of one- and two-stage Eucalyptus globulus-CBC boils with and without hemicellulose enrichment.

[0077] Figure 6 shows the molar mass distribution of Eucalyptus globulus kefir cell.

[0078] Figure 7 shows the comparison of the molar mass distribution of a CBC* pulp with a VISCBC pulp.

[0079] Figure 8 shows the strengths of normal viscose fibers produced from different cellulose materials in the conditioned state.

[0080] Figure 9 illustrates the influence of the amount of ozone applied and the radiation dose on the DP degradation of differently pretreated CBC and LH sulfite pulps.

[0081] Figure 10 shows the molar mass distribution of a CBC pulp degraded to a GVZ of 440 ml / g using EBeam and ozone.

[0082] Figure 11 shows the molar mass distribution of a xylane isolated from a CCE filtrate by reverse precipitation in mineral acid. Figure 12 shows the molar mass distribution of xylans isolated from cellulose and fibers produced therefrom using DMSO (graphical evaluation of the GPC analysis)

[0083] Figure 13 compares the intensity of the preferred steam treatment (CBC*) according to the invention with a pre-hydrolysis process (VISCBC). The P-factor of the steam treatment preferred according to the invention is less than 50; the P-factor of the VISCBC pre-hydrolysis is 700.

[0084] Figure 1 schematically illustrates the basic concept of the inventive method and its various possible applications.

[0085] Variant A demonstrates the production of paper pulp with high strength potential: This involves combining a two-stage kraft process (as batch or, for example, CBC-V) with a TCF or ECF bleaching sequence. The two-stage operation allows for optimal adjustment of the cooking conditions to the specific requirements.

[0086] Variant B illustrates the concept of producing high-yield paper pulp (pulp with increased hemicellulose content): The process is essentially the same as in Variant A. However, the boiling liquor for the second boiling stage is enriched with high-molecular-weight hemicellulose from hemicellulose-rich liquor. This hemicellulose-rich liquor can, in particular, originate from a CCE process, which is carried out in a process C coupled with process B to produce high-yield lyocell pulp. The hemicellulose-rich liquor can be, for example, (a) the CCE filtrate or (b) the retentate of a nanofiltered CCE filtrate.

[0087] The variant C mentioned earlier in Figure 1 leads to a high-yield lyocell pulp for the production of lyocell fibers with the highest textile mechanical strength properties: The basic scheme follows the same procedure as variant A. However, the cooked pulp is treated here, either directly after washing and sorting or after each bleaching or depolymerization stage (“DEPOLY”), preferably after an O stage, in a CCE finishing stage.

[0088] In conjunction with parallel paper pulp production, see Scheme B, CCE filtrate can be used to strengthen white liquor, preferably in the second boiling stage. If paper pulp production is insufficient or nonexistent, the lye can be recycled after purification by nanofiltration. The permeate (b) is returned to the CCE stage, and hemicelluloses can be obtained from the retentate (c).

[0089] Variant D in Figure 1 shows a preferred embodiment of the inventive process for the production of high-yield dissolving pulps, which is in particular

[0090] (a) Viscose pulp for fibers with high textile mechanical properties,

[0091] (b) all other dissolving pulps which are derivatized to cellulose esters or ethers.

[0092] The basic scheme proceeds according to variant C. To improve the cellulose reactivity, the wood is subjected to a steam activation treatment (DA stage), in which the composite structure of the wood is greatly loosened, with the aim of selectively separating the low molecular weight hemicelluloses in the subsequent alkaline boiling.

[0093] Examples

[0094] Example 1 - Two-stage CBC cooking of spruce wood

[0095] Spruce wood is cooked in a 10.8 l experimental cooker using the continuous batch cooking (CBC) process to produce pulp with kappa numbers between 16 and 42. The single-stage reference cooking process has the following conditions:

[0096] Impregnation: [OH-] = 0.37 mol / l, [HS-] = 0.22 mol / l; mean temperature 120 0 C,

[0097] 30 min (filling direction from bottom to top) Heating: Displacement of the impregnating lye by preset cooking lye

[0098] (Displacement direction from top to bottom). After 28 minutes, the

[0099] Target temperature of 160 0 C reaches boiling point: Boiling solution is pumped from top to bottom through the kettle at a flow rate of twice the kettle volume per hour: 160

[0100] 0 C, [OH-] = 0.62 mol / 1, [HS-] = 0.30 mol / 1, H factors: 800 - 1600.

[0101] Impregnation and heating of the inventive two-stage CBC boiling process were carried out analogously to the single-stage variant.

[0102] Cooking level 1: 160 0 C, [OH-] = 0.48 mol / 1, [HS-] = 0.48 mol / 1, H factor = 750 = constant Cooking level 2: 160 0 C, [OH-] = 0.62 mol / 1, [HS-] = 0.32 mol / 1, the H factor was varied from 100 to 600

[0103] Two variants of the two-stage CBC boiling process were carried out, the only difference being the concentration of dissolved substances:

[0104] a) DS ~ 80 g / l (standard) b) DS ~ 40 g / l (low solid CBC)

[0105] The experimental results are summarized in Figure 2 using a selectivity plot (limiting viscosity vs. kappa number). The results show that the already high selectivity of the single-stage CBC cooking process can be further improved by the two two-stage variants.

[0106] Figure 3 shows temperature and hydroxide ion profiles of the one- and two-stage softwood CBC boiling processes described above.

[0107] As shown in Figure 3, a two-stage operation does not result in an increase in cooking time, provided the delignification levels are the same. The hydroxide ion concentration at the cooker outlet shows a rapid increase during the second cooking stage and reaches the target concentration halfway through the selected cooking time.

[0108] Example 2 — Two-stage CBC boiling of Eucalyptus globulus

[0109] Eucalyptus globulus is processed into pulp with kappa numbers between 13 and 28 in a 10.8 1 large experimental cooker according to the CBC-V (continuous batch cooking) method.

[0110] The one-stage reference cooking process has the following conditions:

[0111] Impregnation: [OH-] = 0.38 mol / l, [HS-] = 0.25 mol / l; average temperature 120 °C, 30 min (filling direction from bottom to top). Heating: displacement of the impregnating liquor by preset cooking liquor.

[0112] (Displacement direction from top to bottom). After 30 minutes, the

[0113] Target temperature of 155 °C reached. Boiling stage: Boiling solution is pumped from top to bottom through the kettle at a flow rate of twice the kettle volume per hour: 155

[0114] °C, [OH-] = 0.65 mol / 1, [HS-] = 0.34 mol / 1, H factors: 200 - 500. Impregnation and heating of the two-stage CBC cooking process were carried out analogously to the single-stage variant.

[0115] Cooking level 1: 155 0 C, [OH-I = 0.46 mol / l, [HS-] = 0.37 mol / l, H-factor = 180 = constant, cooking stage 2: 155 0 C, [OH-] = 0.62 mol / 1, [HS-] = 0.37 mol / 1, the H factor was varied from 100 to 400.

[0116] In a second variant, the cooking liquor of the second stage was produced with the hemi-rich filtrate of a CCE treatment.

[0117] The conditions in cooking stage 2 were set as follows: 155 °C, [OH-] = 0.37 mol / l, [HS-] = 0.16 mol / l, beta-cellulose concentration (from CCE filtrate) = 10 g / l, H-factor = 150 - 400.

[0118] As can be seen from Figure 4, the yield could be significantly improved across the entire kappa number range for both the “simple” two-stage variant (“two-stage”) and the hemicellulose-enhanced two-stage variant (“hemi-add”) compared to the single-stage operating mode.

[0119] The advantage of the two-stage process is also evident in the digestion selectivity, which is shown in Figure 5 as a plot of marginal viscosity number vs. kappa number.

[0120] It is noticeable that the cooking selectivity, i.e. the marginal viscosity at a certain kappa number, is very high after all CBC cookings compared to conventionally produced eucalyptus g / oZm / ws cookings.

[0121] Example 3 — Production of high-yield chemical pulps for further processing into viscose and lyocell fibers

[0122] Before the CBC cooking process began, the wood was subjected to steam activation (DA) by heating the contents of the cooker to a temperature of approximately 165°C using medium-pressure steam. 0 C was brought in. The CBC cooking was carried out in a single stage.

[0123] The combination of the DA+CBC processes will subsequently be referred to as "CBC*" for better identification. CB C* pulp was produced after O-delignification. Cold alkali extraction was performed to remove alkali-soluble hemicelluloses. The DP (dimethyl sulfide) content was adjusted during the post-bleaching stage by ozone treatment (Z). Subsequent P (phosphorus) bleaching served to stabilize the cellulose and achieve the desired final whiteness. A pre-hydrolysis kraft pulp was produced as a reference using the "VISCBC" technology (modified Visbatch process, see Wizani, W., et al. "CBC - Continuous batch cooking. The revolution in kraft cooking" in Pulping process cmdproduct quality Conference, 2000, Boston, MA, USA).

[0124] Table 1 below shows the most important characteristics of unbleached pulp.

[0125] Table 1: Characterization of unbleached E. globulus pulp: CBC* pulp

[0126] (Paper pulp) and VISCBC cooking process, as a reference for a conventional

[0127] Chemical pulp.

[0128] Parameter CBC* VISCBC

[0129] Wood #134 #141 / 142

[0130] P-factor 0 490

[0131] Yield, sorted % 100.0 52.9 37.2

[0132] Cellulose yield % wood 46.1 41.0 34.9

[0133] Kappa number 13.1 6.0

[0134] Infinite viscosity ml / g 1281 963

[0135] Whiteness % ISO 37.7 42.8

[0136] R18-20°C % Pulp 92.6 96.9

[0137] R18-50°C % Pulp 84.4 96.2

[0138] Xylan % Pulp 16.0 18.4 3.1

[0139] % Wood 16.0 9.7 1 ,1

[0140] The P-factor expresses the intensity of pre-hydrolysis. The calculation is based on the same concept as the H-factor, but using a different activation energy (123 kJ / mol).

[0141] The yield (cellulose content) of the CBC* pulp was 15.7 percentage points (6.1 percentage points) higher than in comparison to the VISCBC reference pulp (see Table 1).

[0142] The CBC* and VISCBC pulps were subsequently bleached using an OZP-TCF sequence. To reduce the low molecular weight hemicelluloses, the CBC* pulps underwent cold alkali extraction (CCE stage) after O-delignification.

[0143] The CCE treatment was carried out at two different NaOH concentration levels, 50 g / l and 100 g / l. White hydroxide solution with a sulfide content of 26% served as the alkali source. All other conditions, such as temperature (3O₂), were controlled. 0 C), residence time (30 min) and substance density (10%) were kept constant in both experiments. Post-bleaching was carried out using a ZP sequence for all pulps, with the primary purpose of ozone bleaching being to adjust the DP to the level required for regenerated pulp (DPv 950–1200, corresponding to a limiting viscosity of 420–500 ml / g). The most important process and pulp data (within the context of pulp bleaching) are listed in Table 2 below.

[0144] Table 2: Characterization of the bleached high-yield E. globulus-CBC*-CCE chemical pulps and, as a reference, a bleached VISCBC chemical pulp.

[0145] Parameter Units CBC* -Reference CBC-CCE50 CBC*-CCE100 VISCBC-Reference

[0146] OZPO CCE ZPO CCE ZPOZP

[0147] Conditions

[0148] temperature • c 110 50 80 110 30 50 70 110 30 50 70 110 50 80

[0149] Time spent (min): 60, 240, 60, 30, 120, 60, 30, 120, 60, 300

[0150] Fabric density % 12 10 10 12 10 10 10 12 10 10 10 12 10 10

[0151] NaOH consumption kg / t 25 12 25 6 25 6 25 9 3

[0152] NaOH concentration g / ι 50 100

[0153] 02-part pressure bar 10 10 10 10

[0154] Ozone application kg / t 11 87 6 8 3.5 2.8

[0155] Peroxide conversion kg / t 10 5 6

[0156] Pulp parameters

[0157] Total yield % / wood 51.7 50.83 50.3 51.7 47.1 46.9 46.6 51.7 45.2 45.1 44.9 36.6 36.4 36.2

[0158] Kappa number 7.7 1.2 0.5 7.7 4.5 0.5 0.3 7.7 2.9 0.4 0.3 1.8 0.4 0.2

[0159] Whiteness %iso 66.4 84 89.0 66.4 90.2 92.5 664 91 .4 93.6 70.2 88.2 92.4

[0160] Limit viscosity ml / g 893 498 470 893 984 490 475 893 1026 490 465 650 490 455

[0161] R18-20% 93.1 96.1 96.4 98.7 97.8 97.0

[0162] Xylan % 17.3 9.6 9.3 4.7 4.2 2.9

[0163] Table 2 clearly shows that the CCE-treated CBC* pulps exhibit an R18 level comparable to that of highly refined pre-hydrolysis kraft pulps (VISCBC reference). However, the yield of the bleached CBC*-CCE pulps is 8.7–10.4 percentage points higher than that of the reference pulp.

[0164] The yield advantage is primarily due to the higher cellulose content. The higher xylan content (alkali-resistant) of the CBC*~CCE pulps also contributes to the higher yield, although this proportion decreases with increasing NaOH concentration in the CCE stage.

[0165] A simple balance shows that CCE treatment very selectively removes non-cellulosic polysaccharides, while intensive pre-hydrolysis also causes massive cellulose degradation.

[0166] An important criterion for the evaluation of chemical pulps, especially with regard to their further processing properties, is the molar mass distribution. The molar mass distribution of Eucalyptus globulus krazQllstoϊfen is shown in Figure 6.

[0167] The upper part of Figure 6 shows unbleached CBC pulp produced by a two-stage CBC cooking process. The terms "CBC-two-stage" and "CBC hemi-add" refer to the pulp produced according to Example 2, with and without hemicellulose enrichment, respectively. The curve "β-Xylan" refers to xylan isolated from the CCE stage. The lower part of Figure 6 depicts the following pulps:

[0168] (a) CBC*: unbleached CBC pulp after steam activation

[0169] (b) CBC*depoly: CBC* after TCF bleaching

[0170] (c) CBC*-CCE: CBC* after CCE treatment at 100 g / l NaOH concentration

[0171] (d) (c) TCF bleached.

[0172] The molar mass distribution was determined by GPC in LiCl / DMAc and MALLS detection [Schelosky, N., T. Röder, and T. Baidinger, Molecular mass distribution of cellulose products by size exclusion chromatography in DMAC / LiCl. Das Papier, 1999. 53(12): p. 728-738].

[0173] The lower part of Figure 6 clearly shows that the CCE treatment removes the low molecular weight carbohydrate fraction very effectively and selectively.

[0174] A comparison with the molar mass distribution of conventional, highly refined chemical pulps produced according to a pre-hydrolysis Kraft process (VISCBC) shows (see Figure 7) that the CCE treatment with the higher NaOH concentration level enables a narrower distribution (lower polydispersity) than in the comparison pulps. Figure 7 compares a VISCBC pulp with a “CBC* CCElOO Depoly” pulp, defined as a CBC* pulp that has undergone a CCE process with 100 g / l NaOH and has been subjected to a depolymerization treatment (TCF bleaching).

[0175] Further processing into regenerated fibers

[0176] 1. Viscose fibers:

[0177] An important criterion for the further processing of chemical pulps is the achievable viscosity quality, which is determined by the filter value according to Treiber [Sixta, H., et al, Evaluation of new organosob dissolving pulps. Part I: Preparation, analytical characterization and viscose processability. Cellulose, 2004. 11(1): p. 73-83.], the mean particle content and particle distribution in the size range of 3-150 μm (determination using the PAMAS measuring device [Sixta et al., Cellulose, 2004. 11(1): p. 73-83]) was assessed.

[0178] Table 3 below shows that the steam activation treatment prior to CBC boiling is the crucial step in improving the resulting viscosity quality. The subsequent CCE treatment leads to a further improvement in viscosity quality, with the effect increasing as expected with rising NaOH concentration.

[0179] Table 3: Viscose quality, measured by the filter value and mean particle volume of reference and test pulps

[0180] Pulp # Filter value Particle volume ppm

[0181] VISCBC reference 73 / 05 364 28

[0182] CBC reference 14 / 05 34 156

[0183] CBC* 74 / 05 180 58

[0184] CBC-CCE50 75 / 05 223 34

[0185] CBC*-CCE100 15 / 05, 7 / 06 306 28

[0186] Table 3 shows that the quality of the viscose produced from the CBC*-CCE100 pulp is almost equivalent to that produced from the VISCBC reference pulp. The viscoses were filtered and spun on a laboratory spinning machine with 20 holes (φ 50 μm) at a total of 4 different draw ratios.

[0187] The strengths of the manufactured normal viscose fibers in the conditioned state are summarized in Figure 8. Fibers made from a) CBC paper pulp, b) CBC*-CCE pulp, and c) a VISCBC reference pulp are compared.

[0188] The results demonstrate that the CBC*-CCE pulp is equivalent to the reference chemical pulp (VISCBC) with regard to further processing into viscose fibers. The slightly lower fiber elongation is due to less complete filtration, which This is recognizable by a slightly increased proportion of small particles in the size range of 5-10 μm.

[0189] The following table compares the chemical and physical properties of the cellulose materials used and the viscose fibers produced from them (using a standard spinning process):

[0190] Table 4: Chemical-physical properties of the pulp and the viscose fibers produced therefrom (standard quality) .

[0192] The pulp “Solucell” is a VISCBC pulp.

[0193] According to the invention, the hemicellulose content is understood to be the sum of the non-glucose-containing sugar components (calculated as anhydrous sugars) after total hydrolysis (two-stage hydrolysis with sulfuric acid) of the pulp or fiber. Measurement is performed using anion exchange chromatography combined with pulsed amperometry as the detection method. The measurement methodology is described in U. Mais, H. Sixta, ACS Symposium Series 2004, 864, 94, and H. Sixta et al. Proceedings of the 1st ISWPC 2001, Vol. 3, pp. 655-658.

[0194] Method for determining the mercerization yield:

[0195] De-animation:

[0196] The fibers are extracted for 3 hours using a Soxhlet extractor with 96% EtOH and left overnight at 50°C. 0 Dried under vacuum.

[0197] Mercerization yield:

[0198] 2.00 g of deavived fiber (weighed weight Mi) is processed at 20 0C is mixed with 50 mL of NaOH, with a concentration of 250 g / L, in a beaker and vigorously stirred (pounded) with a glass rod for 3 minutes. The fiber slurry is then filtered through a G3 frit and washed neutrally with deionized water. After drying, the fiber is weighed again (weighing M2). The mercerization yield is the quotient of M2 / M[ (%).

[0199] 2. Lyocell fiber.

[0200] It is known that depolymerized kraft paper pulp is suitable for the production of high-quality lyocell fibers [WO 99 / 47733]. Kraft boiling (possibly in two stages) with steam pre-activation provides the basis for the production of lyocell fibers with significantly improved textile-mechanical properties. The results of spinning in a Davenport laboratory spinning mill demonstrate that cold alkali extraction of kraft paper pulp raises the textile-mechanical properties to the level of lyocell fibers from the highest-quality chemical pulps (VISCBC) (Table 5).

[0201] Table 5: Strength properties of lyocell fibers produced using a Davenport laboratory spinning system from CBC paper and chemical pulps

[0202] Conditioned fiber data, 1.3 dtex pulps Strength Elongation # cN / tex %

[0203] VISCBC reference L66 40.7 12.7

[0204] 9? C "P_?. f ? r -e D? L32 30, 0_ 10,1

[0205] " C~BC*-CCE~5Ö " L53~54 36~Ö~ Ϊ2~,5~ '

[0206] CBC*-CCE100 L22 41 ,0 10,4 The following table summarizes the results of further experiments on the production of lyocell fibers from various cellulose materials:

[0207] Table 6: Chemical and physical properties of the pulp and the lyocell fibers produced from it

[0209] The pulp “High Hemi” is a pulp conforming to the principles of WO 99 / 47733. The pulp “Solucell” is a VISCBC pulp.

[0210] The table shows that the lyocell fibers spun from celluloses produced according to the invention (CBC*-CCE100) exhibit excellent properties with regard to fiber strength and mercerization yield, comparable to lyocell fibers made from a high-quality VISCBC cellulose, despite the favorable production of the cellulose and higher hemicellulose content.

[0211] The lyocell fibers according to the invention significantly surpass the properties of fibers produced from a pulp corresponding to the teaching of WO 99 / 47733. Example 4 - Controlled DP adjustment of high-yield chemical pulps

[0212] In laboratory experiments, the behavior of ozone bleaching and electron beam irradiation ("EBeam") with respect to the degradation of DP in OP-(CCE)-A and OP-(CCE)-D pre-bleached CBC, CBC*-CCE50, and CBC*-CCE100 pulps was compared. For comparison, a hardwood sulfite pulp ("LH-sulfite") was also electron beam irradiated.

[0213] Ozone bleaching was carried out at 10% substance density and pH 2.0 by mixing in a high-shear mixer under fluidizing conditions.

[0214] The EBeam treatment was carried out at an acceleration voltage of 10 MeV by the company IBA SA, Louvain-La-Neuve in a Rhodotron Accelerator after drying the cellulose sheets.

[0215] All pulps were peroxide bleached after Z- or EBeam treatment (70 °C, 10 kg NaOH / t, 7 kg H2O2 / t, 120 min, 10% bulk density, 0.5 kg Mg II ions / t).

[0216] The results in Figure 9 show that the extent of chain splitting (CSP, calculated according to formula 10) 4 / P r 10 4 The ozone application rate (P0(P ≡ DPv calculated from SCAN GVZ values; ,... after degradation,0• • • before degradation)) as a function of the ozone application rate depends very strongly on the concentration of hemicelluloses (and also lignin, not shown) in the pulp. The higher the hemicellulose content, the higher the ozone application required to achieve a specific cellulose precipitate (CSP).

[0217] The hemicellulose-poor CBC-CCEl OO pulp requires only about 3 kg O3 / t for a KSP of 5.6 (GVZ degradation from 750 ml / g to 420 ml / g), while a CBC pulp with a four times higher xylan content (see Table 2) requires more than 12 kg O3 / t for the same degradation performance.

[0218] In contrast, electron irradiation requires a dose that is largely independent of the type and composition of the pulp.

[0219] Table 7 confirms, based on the copper number and carboxyl group contents, the stabilizing effect of an alkaline solution following the degradation processes. Peroxide treatment. The P-stage results in an additional KSP of approximately 0.6 - 1.2 after both degradation processes, depending on the specific conditions.

[0220] Table 7: Copper number and carboxyl group content of CBC*-CCE100 pulps after Z-, EBeam, or subsequent alkaline peroxide bleaching

[0221] OP-CCE100-AZP

[0222] Copper value % 0.85 0.72 COOH mmol / kg 34 37

[0223] OP-CCE100-D-Ebeam-P Ebeam P

[0224] Copper value % 0.79 0.65 COOH mmol / kg 33 40

[0225] The advantage of electron beam depolymerization is evident in the significantly narrower polydispersity distribution of the finished pulp. Figure 10 shows that the CBC paper pulp depolymerized by electron beam depolymerization exhibits a considerably narrower distribution than CBC pulp degraded with ozone. When depolymerized to a total polydispersity (TDP) of 440 ml / g, the polydispersity index (PDI) was 4.3 for the electron beam-treated pulp and only 3.5 for the electron beam-treated pulp. The analysis was performed on the finished pulp after a final polymerization stage.

[0226] Example 5 — Production of high-yield paper pulp

[0227] The use of hemicellulose-rich cooking liquor in the second cooking stage primarily increases the pulp yield. As shown in Example 2, the average yield increase (at a hemiconcentration of approximately 10 g / l in the cooking liquor) is about 2 percentage points compared to the single-stage variant over a wide kappa number range (see Figure 4).

[0228] The reprecipitation of xylan on the pulp surface is clearly recognizable as an increase in the low molecular weight fraction in the molar mass distribution, see Figure 6 above, and influences both the surface properties and the mechanical strength. The high uronic acid content (GIcA) of the xylans (XyI), GlcA:Xyl ratio approximately 0.05:1, results in an increase in the hydrophilicity of the pulp surface. Example 6 - Production of Xylan products

[0229] 1. Isolation of xylan from the CCE filtrate

[0230] Using a pilot nanofiltration system (NF) equipped with a polyethersulfone membrane, Nadir N30 F, cut-off 300, a CCE filtrate was pre-filtered using a candle filter (Profile Star ABL A4007J) to filter out residual fibers and undissolved particles.

[0231] The NF system was operated at a temperature of 40 °C, a pressure of 25 bar and a specific flow rate of 5 l / m 2 The process was operated for .h. The beta-cellulose (xylan) concentration in the feed was approximately 15 g / l, and the NaOH concentration was 90 g / l. At equilibrium, the flow rates and thus also the alkali loads in the permeate to retentate ratio were 0.82:0.18.

[0232] Due to the low cut-off of the membrane, the total amount of beta-cellulose in the retentate was at a concentration of approximately 85 g / l. The retentate was diluted with water at a ratio of 1:1.5 and fed back into the NF.

[0233] The NF conditions of the second stage were comparable to those of the first stage, except that the permeate volume decreased to approximately 70% of the feed volume. The retentate from the second NF stage now contained beta-cellulose at a concentration of approximately 115 g / L and a NaOH concentration of approximately 32 g / L (hemi-lye).

[0234] This substrate was used to isolate beta-cellulose (xylan) by reverse precipitation with mineral acid. For this purpose, approximately 0.1 parts of sulfuric acid diluted 1:3 with water were mixed with 1 part of hemihydroxide solution, resulting in a pH between 4 and 5.

[0235] After approximately 6-8 hours, a dirty-white precipitate forms with a consistency of approximately 10-15 wt%. This precipitate was then centrifuged, washed, and dried. A xylan content of 74 wt% was detected in this solid. Based on the total carbohydrate content, the xylan content was 97.5%. The molar mass distribution of this xylan powder, determined by GPC, shows a mass-averaged molar mass of 24.4 kg / mol and a number-averaged molar mass of 10.6 kg / mol (see Figure 11). 2. Further processing of the xylan powder into xylo-oligosaccharides (XOS)

[0236] XOS was produced from xylan in two ways: (A) hydrothermolytically, (B) enzymatically.

[0237] (A)Hydrothermolytic XOS production:

[0238] 318 g of dry xylan were diluted in 9.08 L of water (xylan concentration 35 g / L) and treated in an 11 L pressure reactor at 120°C for 5 h with continuous circulation. The circulation rate was 75 L / h. The pH of the hydrolysate after completion of the reaction was 3.13.

[0239] The solution was then neutralized to pH 6.5–7.0 with 0.3 N NaOH. The water-soluble products were centrifuged at 4000 rpm for 60 min. The isolated amount of XOS was 189.7 g of freeze-dried powder, corresponding to a yield of 59.6% based on the xylan used. The hydrothermolytically prepared XOS mixture shows a relatively uniform composition over the investigated DP range (see Table 8 below).

[0240] (B) Enzymatic hydrolysis:

[0241] XOS2. 10

[0242] 90 g of moist xylan (equivalent to 40 g of dry xylan) were suspended in 900 mL of water (44.4 g / L) and 50 mg of Pentopan Mono BG (1.25 mg / g xylan) were added. The mixture was stirred in a fermenter at 50°C for 2 h. The enzyme was then deactivated by heating to 99°C for 10 minutes. The remaining insoluble components were removed by centrifugation, and the aqueous solution was freeze-dried. The XOS yield, based on the amount of xylan used, was 75%.

[0243] XOS2

[0244] The reaction was carried out in a 7L fermenter with a 6L fill level, with a xylan concentration of 20 g / L (120 g xylan). Preparation was also performed using the enzyme Pentopan Mono BG, but with an increased concentration of 1 g / L (50 mg / g xylan). Fermentation was carried out at 40°C. 0 C was carried out for 96 hours. The reprocessing was performed as follows: As described above, the XOS yield was 78% based on the amount of xylan used (93.66 g XOS). The product consists predominantly of xylobiose (Table 8).

[0245] Table 8: Relative mass fractions of the individual, neutral XOS

[0246] Product Hydroenzymatic distribution thermal XOS 2-10 XOS2

[0247] Weight %

[0248] X1 11 ,2 0,1 4,7

[0249] X2 9.7 13.0 83.1

[0250] X3 10.6 21.0 12.2

[0251] X4 12.2 16.0

[0252] X5 12.5 11 ,0

[0253] X6 12.0 7.9

[0254] X7 12.6 7.2

[0255] X8 10.3 7.2

[0256] X9 9.0 6.9

[0257] X10 9.7

[0258] XOS 100.0 100.1 100.0

[0259] Example 7 - Molar mass distribution (MMV) of hemicelluloses (xylans) isolated from pulps and fibers produced according to the invention

[0260] The use of the new generation of chemical pulps of the category “CBC*-CCE” for the production of high-strength lyocell textile fibers can be clearly demonstrated by the molar mass distribution (MMV) of the hemicelluloses isolated from the fibers (in the case of hardwoods, these are almost exclusively xylans) in combination with the high strengths and the high mercerization yield.

[0261] The hemicelluloses are extracted and purified from the substrates (pulp or fibers) using DMSO according to the method of D. Evtuguin et al. (Carboh. Res. 338 (2003) 597). Fibers are first dehydrated with EtOH (25 g Soxhlet with 1 L EtOH, 6 h). The isolated xylan (5 mg) is suspended in DMAc (1 mL) and dissolved in molecularly dispersed form by the addition of LiCl (8 mg) at room temperature. The molar mass distribution is determined by GPC under the following conditions: mobile phase: LiCl / DMAc; temperature: room temperature; column: Mixed A from Polymer Labs; detection: MALLS (Wyatt) / RI; refractive index increment: 0.136 mL / g.

[0262] The results of the MMV determination of the hemicelluloses isolated from cellulose and lyocell fibers produced therefrom are summarized in Table 9 and Figure 12. Table 9: MMV of xylans isolated from cellulose and lyocell fibers produced therefrom using DMSO: numerical evaluation of mass and number means

[0264] The pulp “Solucell-1772” is a VISCBC pulp.

[0265] The results of the GPC measurements of the xylans isolated from pulp and fibers allow the following conclusions:

[0266] • The profile of xylan-MMV in the pulp is reflected in the fiber - despite degradation.

[0267] • Xylans from CBC*-CCE pulps are significantly higher molecular weight and more polydisperse than those from conventional pre-hydrolysis Kraft pulps (PHK).

[0268] • Xylans from lyocell fibers produced using a CBC*-CCE pulp exhibit a mass mean (Mw) of > 20 kDa. In contrast, xylans from lyocell fibers derived from currently commercially available PHK pulps (or sulfite pulps) exhibit a mass mean (Mw) of < 10 kDa.

Claims

Claims:

1. A process for producing chemical pulp from a cellulosic starting material using the Kraft process, comprising the step of boiling the starting material with a cooking lye, characterized in that the starting material is subjected to steam treatment before boiling and that the pulp obtained by boiling is subjected to a potassium alkali extraction (CCE) in the course of further treatment.

2. Method according to claim 1, characterized in that the steam treatment is carried out at a temperature of 120°C or more and a P-factor of 50 or less.

3. Method according to claim 1 or 2, characterized in that for steam treatment the starting material is treated with medium-pressure steam at a temperature of 150 to 1800°C.

4. Method according to one of the preceding claims, characterized in that the starting material is subjected to impregnation before cooking.

5. Method according to one of the preceding claims, characterized in that the boiling, steam treatment and optionally the impregnation of the starting material are carried out in the same cooker.

6. Method according to one of the preceding claims, characterized in that the cooking is carried out in the form of a continuous batch cooking (CBC).

7. Method according to one of the preceding claims, characterized in that at least a part of the press liquor produced in the cold alkali extraction stage is purified by means of a membrane separation process, preferably nanofiltration or ultrafiltration.

8. Method according to claim 7, characterized in that the membrane separation process is carried out in two stages, wherein a dilution of the retentate of the first stage with water is carried out between the two separation stages.

9. Method according to one of claims 7 and 8, characterized in that the hemicelluloses, in particular xylans, contained therein are obtained from at least a part of the retentate of the membrane separation process.

10. Method according to claim 9, characterized in that precipitable hemicelluloses, in particular xylans, are obtained from the retentate of the membrane separation process by means of a reverse precipitation.

11. Method according to claim 10, characterized in that for reverse precipitation an agent selected from the group consisting of mineral acids, CO2 and mono- or polyhydric alcohols is used.

12. Method according to one of claims 9 to 11, characterized in that the obtained xylans are at least partially further processed to xylo-oligosaccharides.

13. Method according to claim 12, characterized in that a method selected from the group consisting of hydrothermolysis and enzymatic hydrolysis is carried out to produce the xylo-oligosaccharides.

14. A method according to one of the preceding claims, characterized in that it is coupled with a method for producing paper pulp and at least a part of the press liquor produced in the cold alkali extraction stage and / or at least a part of the retentate of a membrane separation process carried out on the press liquor is fed to the boiling liquor of a boiling process carried out for the production of paper pulp.

15. Method according to one of the preceding claims, characterized in that, in addition to any bleaching step carried out, a treatment to adjust the degree of polymerization (DP) is performed on the pulp obtained by boiling during further treatment.

16. Method according to claim 15, characterized in that a treatment selected from the group consisting of oxidative bleaching processes, acid hydrolytic processes and electron irradiation processes is carried out.

17. Method according to claim 16, characterized in that electron irradiation of the pulp is carried out, wherein the pulp is present in a material density of at least 35%, preferably 40-50% and in a layer thickness of 2 to 6 mm, preferably 3 to 4 mm, and an accelerating voltage of less than 2.5 MeV is used.

18. Method according to one of claims 15 to 17, characterized in that, after the treatment to adjust the degree of polymerization, an alkaline-oxidative treatment, preferably an alkaline peroxide treatment, is carried out.

19. Method according to one of the preceding claims, characterized in that the cooking step of the pulp is carried out in two stages, wherein in the first stage delignification is carried out by means of a first cooking liquor to a kappa number of 35 to 70 in the case of coniferous wood as starting material and to a kappa number of 30 to 60 in the case of deciduous wood as starting material, and in the second stage the cooking is continued by means of a second cooking liquor until the desired purity of the pulp is reached.

20. Method according to claim 19, characterized in that the proportion of the H-factor of the first cooking stage, based on the H-factor of both cooking stages together, is 40% to 80% in the case of coniferous wood as starting material or 20% to 60% in the case of deciduous wood as starting material.

21. Method according to claim 19 or 20, characterized in that, during the transition from the first to the second cooking stage, the first cooking liquor is replaced by the second cooking liquor.

22. Method according to one of claims 19 to 21, characterized in that the first cooking liquor has an EA concentration of 10 g / L to 30 g / L, preferably 15 g / L to 25 g / L, particularly preferably 20 g / L, and a sulfidity of 50% to 120%, preferably 100%.

23. Method according to one of claims 19 to 22, characterized in that the composition of the second cooking liquor differs from that of the first cooking liquor.

24. Method according to claim 23, characterized in that the second cooking liquor is enriched with a liquor selected from the group consisting of the filtrate of a subsequent washing stage, a white liquor from causticization, the press liquor from a cold alkali extraction stage and the retentate of a membrane separation process carried out on a press liquor from a cold alkali extraction stage.

25. Method according to one of claims 19 to 24, characterized in that both cooking stages are carried out in the form of continuous batch cooking (CBC).

26. Use of a chemical pulp produced according to a process according to any one of claims 1 to 25 for the production of viscose and lyocell fibers.

27. Lyocell fiber obtainable by spinning a chemical pulp produced according to a process according to any one of claims 1 to 25.

28. Lyocell fiber according to claim 27, characterized in that its hemicellulose content H is more than 3.5 wt.% and its mercerization yield is 90% or more.

29. Lyocell fiber according to claim 28, characterized in that the H content is less than 5 wt.%.

30. Lyocell fiber according to claim 28 or 29, characterized in that its strength in the conditioned state is 37 cN / tex or more.

31. Lyocell fiber according to one of claims 28 to 30, characterized in that the mean molar mass of the xylans isolable from the fiber is 20 kDa or more.

32. Viscose fiber obtainable by spinning a chemical pulp produced according to a process according to any one of claims 1 to 25.

33. Viscose fiber according to claim 32, characterized in that its hemicellulose content H is more than 2.0 wt.% and its mercerization yield is 90% or more.

34. Viscose fiber according to claim 32 or 33, characterized in that its strength in the conditioned state is 23 cN / tex or more and its elongation in the conditioned state is 18% or more.