Method for manufacturing glass plate, method for manufacturing glass substrate for magnetic disk, method for manufacturing magnetic disk, and annular glass plate
Patent Information
- Application Number
- LAP899
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-25
- Filing Date
- 2021-11-25
- Publication Date
- 2026-01-09
AI Technical Summary
The existing methods for manufacturing glass substrates for magnetic disks often result in cracking during the laser chamfering process, which affects the quality and efficiency of the glass substrates used in HDD devices, as they are prone to both immediate and delayed cracking due to residual stress.
A method involving preheating the glass base plate to a specific temperature (Tp) below its glass transition point (Tg), with a controlled average linear expansion coefficient (α), to prevent immediate cracking and delayed cracking by forming a chamfered surface with a laser beam without subsequent annealing, ensuring the glass substrate's integrity and reducing residual stress.
This approach effectively prevents cracking and residual stress in the glass substrates, enhancing their durability and production efficiency by maintaining the glass substrate's flatness and surface quality, allowing for precise chamfering without post-processing annealing treatments.
Smart Images

Figure 00000000_0000_ABST 
Figure 00000000_0001_ABST 
Figure 00000000_0002_ABST
Abstract
Description
Glass plate manufacturing method, magnetic disk glass substrate manufacturing method, magnetic disk manufacturing method, and annular glass plate
[0001] The present invention relates to a method for manufacturing a glass plate including chamfering the edge of a raw glass plate, a method for manufacturing a glass substrate for a magnetic disk, a method for manufacturing a magnetic disk, and a circular glass plate.
[0002]
[0003] HDD (hard disk drive) devices for data recording use magnetic disks in which a magnetic film is provided on a circular-shaped magnetic disk glass substrate. When manufacturing a magnetic disk glass substrate, it is preferable to smooth the end faces of the circular glass plate that forms the final product, the magnetic disk glass substrate, where particles are likely to be generated, in order to prevent fine particles from adhering to the main surface and adversely affecting the performance of the magnetic disk. Furthermore, in order to accurately incorporate the magnetic disk into the HDD device, and further, to make the end faces of the glass plate suitable for gripping by a jig that grips the outer peripheral end face of the glass substrate when forming a magnetic film on the main surface of the glass substrate, it is preferable to align the end faces of the glass plate to a target shape.
[0003] A method for finishing the edges of a sheet, such as a glass sheet, is known as a method for forming the edge of a glass sheet into a target shape (see Patent Document 1). In this finishing method, the edge of the sheet is preheated to a high temperature, the preheated edge is heated with a laser beam, and after heating with the laser beam, the edge is further annealed to reduce residual stress. This prevents unacceptable amounts of residual tensile stress, cracks, or defects from occurring along the edge.
[0004] JP 2010-519164 A
[0005] However, when the edge finishing method is applied to a circular glass plate that is the base material for a magnetic disk glass substrate, cracks may occur in the glass plate after heating by laser irradiation but before annealing, for example, immediately after laser irradiation. Furthermore, annealing after heating by laser irradiation is disadvantageous in terms of production efficiency.
[0006] Therefore, the present invention aims to provide a method for manufacturing a glass plate, a method for manufacturing a glass substrate for a magnetic disk, and a method for manufacturing a magnetic disk, which do not cause cracks in the glass plate after laser light irradiation to chamfer the edge surface, and to provide a circular ring-shaped glass plate that is less likely to crack.
[0007] One aspect of the present invention is a method for manufacturing a glass plate including chamfering an edge surface, the chamfering comprising: irradiating a laser beam onto the edge surface of a raw material glass plate before the chamfering to form a chamfered surface; and heating the raw material glass plate before the irradiation with the laser beam, wherein, when the temperature of the raw material glass plate when heated is Tp [°C], the glass transition point of the raw material glass plate is Tg [°C], and the average linear expansion coefficient of the raw material glass plate is α [1 / °C], then (Tg - Tp)≦−5.67×10 7 - Satisfies α+840.
[0008] (Tg-Tp)≦-3.67×10 7 It is preferable that α+500 is satisfied.
[0009] (Tg-Tp)≦-3.28×10 7 It is preferable that α+428 is satisfied.
[0010] It is preferable that (Tg-Tp)≧50° C. It is more preferable that (Tg-Tp)≧100° C.
[0011] The average linear expansion coefficient α of the glass plate is 20×10 -7 [1 / °C] ~ 60 x 10 -7 It is preferable that the temperature is [1 / °C].
[0012] It is preferable that the glass plate after the chamfering treatment is not subjected to an annealing treatment.
[0013] Another aspect of the present invention is a method for producing a magnetic-disk glass substrate using the above-described glass plate manufacturing method. The raw glass plate has a circular shape. After producing the glass plate using the above-described glass plate manufacturing method, the main surfaces of the produced glass plate are ground and / or polished to produce a magnetic-disk glass substrate.
[0014] Yet another aspect of the present invention is a method for manufacturing a magnetic disk, comprising forming a magnetic film on a main surface of the magnetic disk glass substrate manufactured by the method for manufacturing a magnetic disk glass substrate.
[0015] Yet another aspect of the present invention is a ring-shaped glass plate having a circular hole in the center, the ring-shaped glass plate having a front surface, an inner peripheral edge surface and an outer peripheral edge surface that form the outline of the circular hole, the inner peripheral edge surface and the outer peripheral edge surface having chamfered surfaces, and the maximum value of residual stress at an end of the main surface near the inner peripheral edge surface is greater than the maximum value of residual stress at an end of the main surface near the outer peripheral edge surface. It is preferable that the residual stress at any location on the main surface of the glass plate has a retardation value of 50 nm or less. The glass plate is a glass substrate for a magnetic disk, and it is preferable that the arithmetic mean roughness Ra of the main surface is 0.2 nm or less.
[0016] According to the above-described methods for manufacturing a glass plate, a glass substrate for a magnetic disk, and a magnetic disk, when the edge surface of the raw glass plate is chamfered by irradiating it with laser light, no cracks occur in the glass plate after the irradiation with the laser light.
[0017] 1A is a perspective view of an example of a glass plate manufactured by a glass plate manufacturing method according to an embodiment, FIG. 1B is a diagram showing an example of the cross-sectional shape of a chamfered surface, and FIG. 1C is a diagram showing an example of the shape of an end face of a raw glass plate before chamfering. It is a diagram showing an example of the formation of a chamfered surface by irradiation with laser light according to an embodiment. It is a diagram showing an example of a region indicating the presence or absence of cracks or the like in a glass plate in a graph having coordinate axes of average linear expansion coefficient α and temperature difference (Tg-Tp).
[0018] Hereinafter, a method for manufacturing a glass plate, a method for manufacturing a glass substrate for a magnetic disk, a method for manufacturing a magnetic disk, and a circular ring-shaped glass plate according to an embodiment will be described in detail.
[0019] In one embodiment, a method for manufacturing a glass sheet includes a chamfering process in which a chamfer is formed on the edge of a raw glass sheet. In the chamfering process, a laser beam is irradiated onto the edge of the raw glass sheet to form a chamfered surface. However, before the chamfering process, the raw glass sheet is heated. This heating process is hereinafter referred to as preheating. That is, by preheating the raw glass sheet, the edge can be easily melted or softened by irradiating the laser beam, thereby forming a chamfered surface. Furthermore, preheating the raw glass sheet can reduce or suppress cracks occurring in the glass sheet immediately after forming the chamfered surface by irradiating the laser beam. However, even if no cracks occur in the glass sheet immediately after forming the chamfered surface, as described above, delayed cracks may occur after a predetermined time has elapsed, immediately before the subsequent process performed after the chamfering process. Hereinafter, delayed cracks are referred to as delayed cracks.
[0020] Therefore, the inventors of the present invention have intensively studied measures to suppress delayed cracking as well as cracking of the glass plate that occurs immediately after irradiation with a laser beam for forming a chamfer due to residual strain generated in the glass plate after chamfering, and have found the following measures: That is, when the temperature of the glass plate when heated is Tp [°C], the glass transition point of the glass plate is Tg [°C], and the average linear expansion coefficient of the glass plate is α [1 / °C], in order to prevent cracking of the glass plate that occurs immediately after irradiation with a laser beam, the following condition must be satisfied: (Tg - Tp) ≦ -5.67 × 10 7 The temperature Tp is set so as to satisfy α + 840. Here, the average linear expansion coefficient α is the linear expansion coefficient at 100°C to 300°C. The glass transition point Tg and the average linear expansion coefficient α can be measured using, for example, a thermomechanical analysis (TMA). By taking the above measures, it is possible to prevent cracking of the glass sheet immediately after irradiation with laser light. Furthermore, by limiting the range of (Tg - Tp), it is possible to prevent delayed cracking of the glass sheet before the subsequent process after the chamfering process, and even the occurrence of cracks.
[0021] FIG. 1( a ) is a perspective view of an example of a glass plate manufactured by a glass plate manufacturing method according to one embodiment, FIG. 1( b ) is a diagram showing an example of a cross-sectional shape of a chamfered surface, and FIG. 1( c ) is a diagram showing an example of a shape of an end face of the glass plate before chamfering.
[0022] The glass plate 1 shown in FIG. 1( a) is a thin, annular glass plate having a circular hole 3 in the center. The glass plate does not have to be annular, and may be a circular plate with a circular periphery without the circular hole 3. Furthermore, the glass plate does not have to be a circular plate with a circular periphery, and may be a rectangular glass plate; the shape is not particularly limited. When the glass plate 1 is annular, it can be used as a raw plate for a magnetic disk glass substrate. When producing this magnetic disk glass substrate, the size of the magnetic disk glass substrate is not limited. In the case of a magnetic disk glass substrate having a nominal diameter of 3.5 inches, for example, the outer diameter (nominal value) is 95 mm to 100 mm and the inner diameter (nominal value) is 25 mm. In the case of a magnetic disk glass substrate having a nominal diameter of 2.5 inches, for example, the outer diameter (nominal value) is 65 mm to 70 mm and the inner diameter (nominal value) is 20 mm. The thickness of the magnetic disk glass substrate is, for example, 0.20 mm to 0.7 mm, preferably 0.30 mm to 0.6 mm, and more preferably 0.30 mm to 0.53 mm. A magnetic film is formed on the main surface of this magnetic disk glass substrate to produce a magnetic disk.
[0023] The glass plate 1 shown in FIG. 1( a) has a chamfered edge formed by chamfering the edge. FIG. 1( b) is a diagram showing an example of the cross-sectional shape of a chamfered edge formed by the present invention. The cross-sectional shape is the shape of the edge when the glass plate 1 is cut radially along a plane passing through the central axis of the glass plate (the rotation axis when the glass plate is to be formed into a magnetic disk glass substrate). As shown in FIG. 1( b), the cross-sectional shape of the edge 5 including the chamfered edge is a curved surface formed by a smooth curve that protrudes radially outward. Hereinafter, the edge 5 including the chamfered edge will also be simply referred to as the edge 5. In the example shown in FIG. 1( b), the edge 5 is a curved surface formed by a smooth curve that protrudes radially outward. However, as another example, the edge 5 may be formed to have two curved surfaces connected to the two main surfaces, respectively, and a sidewall surface located between the two curved surfaces and at the center of the edge, extending linearly in the thickness direction of the glass plate 1. As another example, the glass substrate may have two inclined surfaces connected to the two main surfaces, respectively, and a sidewall surface located between the two inclined surfaces and at the center of the end surface, with both the two inclined surfaces and the sidewall surface extending substantially linearly in the thickness direction. The boundaries between the above surfaces may be rounded or angular. The chamfer length of the glass plate 1 after the chamfering process is defined as the difference between the radius at the most protruding position of the end surface in the radial direction and the radius at the position where the main surface begins to slope toward the end surface, and can be, for example, 30 to 200 μm. In the case of a glass substrate for a magnetic disk, the main surfaces of the glass plate 1 are ground and polished as necessary, and then a magnetic film is formed on the main surface of the glass plate 1 to produce a magnetic disk.
[0024] FIG. 1( c) shows an example of the shape of the end face 7 of the glass workpiece before chamfering. By irradiating this end face 7 with a laser beam (described later), the corners at the boundary between the main surface of the glass workpiece and the end face 7 melt, resulting in a curved surface, as shown in FIG. 1( b), for example, resulting in chamfering. The end face 7 of the glass workpiece before chamfering is a surface that is approximately perpendicular to the main surface of the glass workpiece. This surface is preferable because irradiating the end face 7 with a laser beam (described later) allows the end face 5, including the chamfered surface, to be formed symmetrically with respect to both main surfaces. Note that the shape of the end face 7 shown in FIG. 1( c) is merely an example, and is not limited to a shape that is approximately perpendicular to the main surface. The corners may be rounded or inclined relative to the main surface.
[0025] Before irradiating the glass plate with the laser beam for chamfering, the glass plate shown in FIG. 1(c) is preheated. In this preheating process, the glass plate is placed in a space containing a heater or other device to raise the temperature of the entire glass plate to temperature Tp. Examples of heaters that can be used include a halogen lamp heater, a carbon heater, and an infrared heater such as a sheath heater. The temperature of the glass plate is maintained at a substantially uniform temperature, with little variation across the glass plate. A substantially uniform temperature means, for example, that the difference between the maximum and minimum temperatures is 50°C or less. By maintaining the temperature of the glass plate at a substantially uniform temperature Tp, the temperature when irradiating the edge surface 7 of the glass plate with the laser beam can be uniform along the entire circumference of the edge surface 7. As a result, the shape of the chamfer, which is affected by the melting state of the glass at the edge surface 7 of the glass plate, can be stably formed with a consistent shape in the circumferential direction. Furthermore, preheating the glass plate so that its temperature is approximately uniform across its main surfaces reduces the temperature difference in the radial direction from the edge of the annular glass plate toward the center during laser irradiation, thereby reducing the maximum (peak) residual strain near the edge, as described below. This is preferable because it helps to prevent problems (such as cracks, back-breaking, and fissures) after chamfering with laser light. On the other hand, if only the edge 7 of the glass plate and the edge of the main surface near this edge 7 are locally heated to temperature Tp, glass, which has relatively low thermal conductivity, does not conduct heat toward the center of the glass plate, resulting in a large temperature difference between the edge of the main surface and the area radially inward from this edge. Irradiating the glass plate with laser light in this state further increases the temperature difference due to the additional heating by the laser light, which is undesirable because it is more likely to locally generate high residual strain (residual stress).
[0026] The temperature Tp is the temperature of the glass plate 10 at the start of irradiation with the laser beam L. The glass plate at temperature Tp can also be irradiated with laser beam while being irradiated with infrared rays or the like by a heater to maintain temperature Tp. FIG. 2 illustrates an example of forming a chamfered surface by laser beam irradiation. Specifically, as shown in FIG. 2 , a circular glass plate 10 having a circular hole 16 has a main surface 12 and an end surface 14. The main surface 12 typically has substantially the same shape on the front and back sides (hereinafter, also referred to as a pair of main surfaces). The end surface 14 is substantially perpendicular to the main surface 12. In the example shown in FIG. 2 , the outer peripheral end surface is the end surface 14 to be shaped by the laser beam L. However, the inner peripheral end surface along the circular hole 16 can also be shaped by the laser beam L. In this embodiment, the end surface 14 is irradiated with the laser beam L, and the laser beam L is moved relative to the end surface 14 in the circumferential direction of the circular glass plate 10 to machine the end surface 14 into a target shape. The laser beam L can be applied, for example, by collimating the laser beam L emitted from a laser source (not shown) through an optical system including a collimator, converging the laser beam L through a focusing lens 24, and then irradiating the expanding laser beam L onto the end face 14. When irradiating the inner peripheral end face with the laser beam L, for example, the laser beam L can be incident from above the main surface of the glass plate 10 and reflected by a reflecting mirror installed in the circular hole. When both the outer peripheral end face and the inner peripheral end face are chamfered, they can be performed simultaneously or separately. When performing these separately, the order of the steps is not important. Preheating can be performed after each chamfering step or all at once, but the latter method can improve production efficiency.
[0027] Meanwhile, the glass plate 10 is rotated at a constant speed around the center of the glass plate 10. The laser beam L and the end face 14 are moved relative to each other in the circumferential direction of the circular glass plate 10, and the laser beam L is irradiated along the entire circumference of the end face 14 of the glass plate 10. The laser beam L is preferably irradiated onto the end face 14 from a direction normal to the irradiating position of the end face 14. The normal direction here includes not only a completely normal direction (a tilt angle of 0 degrees from the normal direction) but also an allowable tilt angle of 10 degrees or less relative to the normal direction. The laser beam L may also be irradiated onto the end face 14 at an angle of 0 degrees ±45 degrees relative to the normal direction of the end face 14 at the irradiating position.
[0028] Such an annular glass plate 10 can be obtained, for example, by a separation method using laser light from a pre-fabricated glass plate. The glass plate that forms the annular glass plate 10 is produced, for example, by a floating method or a down-draw method. Alternatively, it may be produced by press-molding a block of molten glass using a mold. The thickness of the glass plate that forms the glass plate 10 is thicker than the target thickness of the final product, a magnetic disk glass substrate, by the amount of grinding and polishing allowance, for example, about 10 to 300 μm.
[0029] The cross-sectional intensity distribution of the laser beam L irradiated onto the end face 14 can be a single mode. That is, the cross-sectional intensity distribution of the laser beam L can be a Gaussian distribution. When the width of the beam (irradiation spot) of such laser beam L at the irradiation position on the end face 14 in the thickness direction of the glass plate 10 is W1 [mm], the thickness of the glass plate 10 is Th [mm], and the average power density of the laser beam L is Pd [W / mm]. 2], the irradiation of the laser beam L is preferably performed under irradiation conditions where W1>Th and Pd×Th is 0.8 to 15 [W / mm]. Here, the beam of the laser beam L is preferably irradiated so that it extends beyond both sides of the glass plate 10 in the thickness direction, as shown in FIG. 2. Furthermore, by making the widths extending beyond both sides of the end face 14 equal, the chamfering can be performed evenly on both sides of the glass plate 10 in the thickness direction, and the shapes of the two chamfered surfaces can be made equal. The average power density Pd is the total power P [W] of the laser beam L divided by the area of the beam in the portion irradiated by the laser beam L. When the beam of the laser beam L has an elliptical shape with a minor axis radius of W1 / 2 and a major axis radius of W2 / 2 (see FIG. 2), the average power density Pd is 4×P / W1 / W2 / π [W / mm]. 2 ] (π is the ratio of the circumference of a circle to its diameter). The average power density Pd is, for example, 1 to 30 [W / mm 2 ] can be used.
[0030] Here, an example of the laser light L is CO 2 Laser light is used, but it is sufficient if the oscillation wavelength is absorbed by the glass. 2 The laser light is not limited to laser light. For example, CO laser (oscillation wavelength: about 5 μm or 10.6 μm), Er-YAG laser (oscillation wavelength: about 2.94 μm), etc. can be used. 2 When using laser light, the wavelength is preferably 3 μm or more. Furthermore, a wavelength of 11 μm or less is more preferable. If the wavelength is shorter than 3 μm, the glass may not absorb the laser light well, and the end surface 14 of the glass plate 10 may not be sufficiently heated. Furthermore, if the wavelength is longer than 11 μm, it may be difficult to obtain a laser device. The oscillation mode of the laser light source is not particularly limited and may be continuous wave (CW) light, pulsed wave light, or modulated CW light. However, with pulsed wave light and modulated CW light, if the relative movement speed of the laser light L is high, there is a risk of unevenness in the shape of the chamfered surface in the movement direction. In this case, the oscillation and modulation frequency is preferably 1 kHz or more, more preferably 5 kHz or more, and even more preferably 10 kHz or more. The relative movement speed between the laser light L and the end surface of the glass plate 10 is, for example, 0.7 to 100 mm / s.
[0031] The width W1 of the beam and the length W2 (described later) can be set by adjusting the irradiation position of the laser beam L on the glass plate 10 using, for example, two cylindrical lenses. The width W1 can be determined using a beam profiler, and the length W2 can be determined from the beam shape measured by the beam profiler and the diameter D of the glass plate. The chamfered glass plate 10, i.e., the main surfaces of the glass plate 1, are then ground and / or polished, and then cleaned as appropriate to produce a magnetic disk glass substrate. If necessary, the edge of the glass plate 1 can also be polished. The glass plate 1 may also be chemically strengthened before, after, or between grinding and polishing of the main surfaces.
[0032] In this embodiment, the end face 14 of the glass plate 1 is irradiated with laser light L as shown in FIG. 2 to form the chamfered surface. However, the irradiation of the laser light L locally raises the temperature of the irradiated portion of the surface of the end face 14. This results in a difference in thermal expansion between the irradiated portion and the radially inner region, leading to cracks occurring near the end face 14 of the glass plate 1 immediately after the chamfered surface is formed. Even if no cracks occur in the glass plate 1 immediately after the chamfered surface is formed, delayed cracks may be detected immediately before the subsequent process performed after the chamfering process. Therefore, in this embodiment, the glass plate 10 is preheated before the end face 14 is irradiated with laser light L to form the chamfered surface. Here, when the temperature of the glass plate 10 when preheated is Tp [°C], the glass transition point of the glass plate 10 is Tg [°C], and the average linear expansion coefficient of the glass plate 10 is α [1 / °C], (Tg - Tp) ≦ -5.67 × 10 7 The temperature Tp of the preheating of the glass plate 10 is set so as to satisfy α+840. In this case, (Tg-Tp)≦-3.67×10 7 It is preferable to set the temperature Tp of the preheating of the glass plate 10 so as to satisfy α+500, in order to prevent the occurrence of delayed cracks. 7Setting the temperature Tp so that α + 428 is satisfied is preferable in terms of preventing cracks. Setting the temperature Tp in this way suppresses the occurrence of cracks and delayed cracks, eliminating the need to anneal the chamfered glass plate 10 to reduce residual strain, as was done in the past. Here, annealing refers to a process in which the chamfered glass plate 10 is heated to a temperature above the strain point of the glass, and then slowly cooled to reduce residual strain (residual stress) within the glass.
[0033] FIG. 3 shows an example of a region indicating the presence or absence of cracks in the raw glass plate 10 in a graph with the average linear expansion coefficient α and the temperature difference (Tg-Tp) as coordinate axes. Lines L1, L2, and L3 in FIG. 3 separate the regions of the raw glass plate 10 where "cracks," "delayed cracks," and "cracking" occur. "Cracks" refers to cracks that occur immediately after the chamfer is formed. "Delayed cracks" refers to cracks that do not occur immediately after the chamfer is formed but occur with a probability of approximately 50-70% within approximately one hour after chamfering. Unlike "cracks" occurring immediately after the chamfer is formed or "delayed cracks," "cracks" refer to cracks or fractures that occur in the glass plate 1 during subsequent processes (grinding and polishing of the main surfaces), which are rare. Line L1 separates the cases where "cracks" occur from the cases where "cracks" do not occur. Line L2 separates the cases where "delayed cracks" do not occur from the cases where "delayed cracks" do occur. The line L3 is a line that separates the case where a "crack" occurs from the case where a "crack" does not occur. In the area located above the line L1, a "crack" occurs. In the area R located below the line L1, the area A In the region R located at or below the line L2, no cracks occur. B In this case, neither "cracks" nor "delayed cracks" occur. C In this case, neither "cracks" nor "delayed cracks" occur, and neither "cracking" nor "fractures" occur. In this way, the occurrence of "cracks", "delayed cracks" or "fractures" can be determined by the average linear expansion coefficient α and the temperature difference (Tg - Tp).
[0034] Therefore, in order to prevent the occurrence of "cracks" immediately after the formation of the chamfered surface, the temperature difference (Tg-Tp) is in the region R A ~R C The temperature Tp may be set in accordance with the average linear expansion coefficient α and Tg of the glass plate 1 so that the line L1 is located at (Tg-Tp)=-5.67×10 7 Since it is expressed as α + 840, (Tg - Tp) ≦ -5.67 × 10 7 The temperature Tp is set so as to satisfy α+840. Furthermore, in order to prevent the occurrence of "delayed cracking," the temperature difference (Tg-Tp) is set in the region R where it is equal to or lower than the line L2. B , R C The temperature Tp may be set in accordance with the average linear expansion coefficient α and Tg of the glass plate 1 so that the line L2 is located at (Tg-Tp)=-5.67×10 7 Since it is expressed as α + 840, (Tg - Tp) ≦ -3.67 × 10 7 The temperature Tp is set so as to satisfy α+500. Furthermore, in order to prevent the occurrence of "cracks," the temperature difference (Tg-Tp) is set in the region R where it is equal to or lower than the line L3. C The temperature Tp may be set in accordance with the average linear expansion coefficient α and Tg of the glass plate 1 so that the line L3 is located at (Tg-Tp)=-3.28×10 7 Since it is expressed as α + 428, (Tg - Tp) ≦ -3.28 × 10 7 The temperature Tp is set so as to satisfy α+428.
[0035] According to one embodiment, it is preferable to satisfy (Tg - Tp) ≥ 50°C. If the difference between the preheating temperature Tp and the glass transition temperature Tg is less than 50°C, the glass plate 10 may deform, resulting in a deterioration (increase) in flatness, which is undesirable. Deterioration in flatness is undesirable because it increases the amount of machining required in the thickness direction in subsequent processes. Here, flatness refers to the PV value (the difference between the highest and lowest values in the height direction) of flatness across the entire main surface, which can be measured using a flatness tester, for example. Furthermore, a deterioration in flatness refers to a change in flatness of 30 μm or more. Satisfying (Tg - Tp) ≥ 100°C is more preferable because it suppresses the deterioration in flatness to 15 μm or less.
[0036] The average linear expansion coefficient α of the glass plate 1 is not particularly limited. However, when the glass plate 1 is ultimately used as a substrate for a magnetic disk in a hard disk drive device, it is preferably 100×10 -7 According to one embodiment, the average linear expansion coefficient α is 20×10 -7 [1 / °C] ~ 60 x 10 -7 [1 / °C]. The average linear expansion coefficient α is preferably 60×10 -7 When the average linear expansion coefficient α is greater than [1 / °C], the applicable upper limit of (Tg-Tp) is relatively small, and the temperature Tp is close to the glass transition temperature Tg, so that strict temperature control of the temperature Tp is required. If the temperature Tp and the glass transition temperature Tg are too close, there is a risk that the glass plate 1 will soften and the flatness will deteriorate. In addition, when the average linear expansion coefficient α is less than 20×10 -7 If the average linear expansion coefficient α is less than [1 / °C], when the glass plate is used for a magnetic disk of a hard disk drive device, the difference in the linear expansion coefficient with the material of the spindle of the hard disk drive device becomes too large, and there is a risk that the glass plate will break when the spindle expands due to heat. -7 From the above viewpoint, the lower limit of the average linear expansion coefficient α is preferably 30×10 -7 It is more preferable that the temperature is [1 / °C].
[0037] By pre-heating and irradiating with laser light L in this manner, a ring-shaped glass plate 1 having chamfered surfaces at its inner and outer peripheral end faces and free of cracks immediately after laser light irradiation can be produced. Here, the maximum residual stress at the portion of the main surface near the inner peripheral end face of the glass plate 1 (a ring-shaped region on the main surface within 3 mm in the radial direction, with the radius of the inner peripheral end face as the reference (zero)), i.e., the end of the main surface near the inner peripheral end face, is preferably greater than the maximum residual stress at the portion of the main surface near the outer peripheral end face (a ring-shaped region on the main surface within 3 mm in the radial direction, with the radius of the outer peripheral end face as the reference (zero)), i.e., the end of the main surface near the outer peripheral face. By pre-heating the entire main surface of the glass plate to a substantially uniform temperature, residual stress peaks can be formed at the end of the main surface near the inner peripheral end face and the end of the main surface near the outer peripheral end face, respectively, when the residual stress is measured in the radial direction of the glass plate 1. The residual stress induced at the end and the end of the main surface by irradiating with laser light is usually compressive stress. On the other hand, when a magnetic disk glass substrate or even a magnetic disk is manufactured using the annular glass plate 1 and the magnetic disk is installed in an HDD device, the main surface edge or end face on the inner peripheral edge side of the magnetic disk may come into strong contact with the spindle, spacer, clamper, etc. of the HDD device, potentially resulting in scratches. In such cases, the residual stress suppresses scratches on the magnetic disk due to such contact. That is, the above-described effect can be achieved by making the retardation value at the main surface edge on the inner peripheral edge side greater than the retardation value at the main surface edge on the outer peripheral edge side. The residual stress at the main surface edge near the inner peripheral edge side preferably has a retardation value of 50 nm or less, more preferably 20 nm or less. Furthermore, the residual stress at the main surface edge near the outer peripheral edge side preferably has a retardation value of 30 nm or less. Furthermore, the residual stress in a region on the main surface of the glass plate 1 excluding the main surface end portion on the inner peripheral edge face side and the main surface end portion on the outer peripheral edge face side (hereinafter also referred to as the intermediate region) is preferably smaller than the maximum value of the residual stress in the main surface end portion on the inner peripheral edge face side and / or the main surface end portion on the outer peripheral edge face side. The residual stress in this intermediate region is preferably 20 nm or less, more preferably 10 nm or less, in terms of retardation value.Furthermore, at any location on the main surface of the glass plate 1, the residual stress is preferably 50 nm or less in retardation value, more preferably 20 nm or less. In the present invention, the residual stress value is expressed as a retardation value. The retardation value can be measured using, for example, a two-dimensional birefringence evaluation device such as the PA-200 manufactured by Photonic Lattice. When examining the distribution of retardation values on the main surface of the glass plate 1, the measurement resolution may be, for example, about 0.05 to 0.2 mm in the in-plane direction. To obtain the glass plate 1 described above, the region R shown in FIG. 3 is used. C Within the range satisfying the above condition, for example, the temperature Tp during the chamfering of the inner peripheral edge surface may be set lower than the temperature Tp during the chamfering of the outer peripheral edge surface. For the same glass plate 1, the glass transition point Tg and the average linear expansion coefficient α remain unchanged, so lowering the temperature Tp increases (Tg - Tp), resulting in increased residual stress. To obtain the glass plate 1 described above, it is preferable to perform the processes in the following order: (1) preheating, (2) chamfering of the outer peripheral edge surface, and (3) chamfering of the inner peripheral edge surface. This order facilitates natural cooling to lower the temperature of the glass plate during the chamfering of the inner peripheral edge surface, so preheating can be performed only once.
[0038] When producing a magnetic disk glass substrate from the glass plate 1, after the above-mentioned chamfering process, the glass plate 1 is used as an intermediate glass plate before becoming a magnetic disk glass substrate, and main surfaces of the glass plate 1 are subjected to grinding and / or polishing processes. Of these, the grinding process does not have to be performed. When both the grinding process and the polishing process are performed, the glass plate 1 is ground and then polished. In the grinding process, for example, a double-side grinding machine equipped with a planetary gear mechanism is used to perform grinding on both main surfaces of the glass plate 1. Specifically, the glass plate 1 is held in a holding hole provided in a holding member (carrier) of the double-side grinding machine, and both main surfaces of the glass plate 1 are ground. The double-side grinding machine has a pair of upper and lower surface plates (upper and lower surface plates), and the glass plate 1 is sandwiched between the upper and lower surface plates. Then, by moving either the upper or lower surface plate, or both, and moving the glass plate 1 and each surface plate relative to each other while supplying coolant, both main surfaces of the glass plate 1 can be ground. For example, a grinding member made of a sheet of fixed abrasive grains in which diamond is fixed with a resin can be attached to the surface plate and the grinding process can be performed. By performing the grinding process, the flatness of the main surfaces can be reduced. The flatness of the main surfaces after the grinding process is, for example, 10 μm or less in terms of the PV value of flatness.
[0039] Next, a first polishing is performed on the main surfaces of the ground glass plate 1. Specifically, the glass plate 1 is held in holding holes provided in a polishing carrier of a double-side polishing machine, and both main surfaces of the glass plate 1 are polished. The purpose of the first polishing is to remove scratches and distortions remaining on the main surfaces after the grinding process, or to roughly adjust (reduce) minute surface irregularities (microwaviness and roughness).
[0040] In the first polishing process, a double-sided polishing machine having a configuration similar to that of the double-sided polishing machine used in the above-described fixed abrasive grinding process is used to polish the glass plate 1 while applying a polishing slurry. In the first polishing process, a polishing slurry containing loose abrasive grains is used. The loose abrasive grains used in the first polishing process include abrasive grains such as cerium oxide or zirconia. As with the double-sided polishing machine, the glass plate 1 is sandwiched between a pair of upper and lower platens. Flat polishing pads (e.g., resin polishers) having an overall circular ring shape are attached to the top and bottom surfaces of the lower platen. Either the upper or lower platen, or both, are then moved to move the glass plate 1 relative to the platen, thereby polishing both main surfaces of the glass plate 1. The size of the polishing abrasive grains is preferably within the range of 0.5 to 3 μm in average particle size (d50).
[0041] After the first polishing or the second polishing, the glass plate 1 may be chemically strengthened. In this case, a mixed molten liquid of potassium nitrate and sodium nitrate, for example, is used as a chemical strengthening liquid, and the glass plate 1 is immersed in the chemical strengthening liquid. This allows a compressive stress layer to be formed on the surface of the glass plate 1 by ion exchange.
[0042] Next, the glass plate 1 is subjected to a second polishing process. The second polishing process aims to finish the main surfaces. This is mirror polishing. A double-sided polishing machine having the same configuration as the double-sided polishing machine used for the first polishing process is also used for the second polishing process. Specifically, the glass plate 1 is held in a holding hole provided in a polishing carrier of the double-sided polishing machine, and both main surfaces of the glass plate 1 are polished. In the second polishing process, the type and particle size of the free abrasive grains are different from those in the first polishing process, and the hardness of the resin polisher is also different. The hardness of the resin polisher is preferably lower than that in the first polishing process. For example, a polishing liquid containing colloidal silica as free abrasive grains is supplied between the polishing pad of the double-sided polishing machine and the main surfaces of the glass plate 1, and the main surfaces of the glass plate 1 are polished. The size of the abrasive grains used in the second polishing process is preferably within the range of 5 to 50 nm in average particle size (d50). The roughness of the main surfaces of the glass plate 1 after the second polishing treatment is 0.2 nm or less in terms of arithmetic mean roughness Ra when measured using, for example, an AFM. The necessity of chemical strengthening treatment can be appropriately selected taking into account the glass composition and other requirements. Furthermore, in addition to the first and second polishing treatments, another polishing treatment may be added, or the polishing treatments for the two main surfaces may be completed with a single polishing treatment. The order of the above treatments may also be changed as appropriate. In this way, the main surfaces of the glass plate 1 are polished to obtain a magnetic disk glass substrate that satisfies the conditions required for a magnetic disk glass plate. Thereafter, at least a magnetic film is formed on the glass plate 1 (magnetic disk glass substrate) produced by polishing the main surfaces, thereby producing a magnetic disk.
[0043] As described above, in the manufacturing method of the glass plate 1, the main surfaces of the chamfered glass plate 1 are ground or polished. In this case, after the edge chamfering process, polishing of the edge surfaces is not performed before grinding or polishing of the main surfaces. Alternatively, even if polishing of the edge surfaces is performed, the amount of removal by polishing of the edge surfaces can be kept to 5 μm or less. Therefore, production costs can be reduced by reducing the amount of edge surface polishing. This is because the laser light L can form a chamfered surface (edge surface) with minimal surface irregularities. In other words, the irradiation of the laser light L can form a fire-polished surface on the edge surface (including the chamfered surface and side wall surface). The fire-polished surface is formed by heating and melting the glass surface, and is a smooth surface with few scratches or microcracks. The surface roughness of the chamfered surface (edge surface) formed by irradiation of the laser light L can be, for example, 50 nm or less in arithmetic mean roughness Ra (JIS B0601 2001). The arithmetic mean roughness Ra is more preferably 30 nm or less, and even more preferably 20 nm or less. The arithmetic mean roughness Ra of the end face can be measured, for example, by a laser microscope.
[0044] According to one embodiment, the glass plate 1 can be made of glass having a glass transition temperature Tg of 500°C or higher. The glass transition temperature Tg is preferably 650°C or higher, and more preferably 750°C or higher. The higher the glass transition temperature Tg, the more the glass plate 1 can be prevented from thermal contraction when heated and from deformation (such as warpage of the substrate) caused by the thermal contraction. Therefore, taking into consideration the heat treatment when forming a magnetic film or the like of a magnetic disk on a magnetic disk glass substrate, the glass transition temperature Tg is preferably 650°C or higher, and more preferably 750°C or higher.
[0045] In this embodiment, aluminosilicate glass, soda-lime glass, borosilicate glass, etc. can be used as the material for the glass plate 1 or the raw glass plate 10. Furthermore, amorphous glass is more preferable in that it allows the production of a magnetic disk glass substrate excellent in the flatness of the main surfaces and the strength of the substrate.
[0046] The composition of the glass plate 1 or the raw glass plate 10 of this embodiment is not limited, but preferably contains, in mole percent, SiO 2 50 to 75%, Al 2 O 3 1 to 15%, B 2 O 3 0 to 15%, Li 2 O, Na 2 O and K 2 O in a total of 0 to 35%, at least one component selected from MgO, CaO, SrO, BaO and ZnO in a total of 0 to 20%, and ZrO 2 , TiO 2 , La 2 O 3 , Y 2 O 3 , Ta 2 O 5 , Nb 2 O 5 and HfO 2 The amorphous aluminosilicate glass has a composition containing 0 to 10% in total of at least one component selected from the above.
[0047] Experimental Example: To verify the effectiveness of the manufacturing method for a glass plate 1 according to this embodiment, various raw glass plates 10 with different mean linear expansion coefficients α were prepared. Glass plates 1 were fabricated by varying the temperature Tp during preheating of the raw glass plates 10. The glass plates 1 were visually inspected for cracks and delayed cracks. Furthermore, glass plates without cracks or delayed cracks were ground and polished, and then visually inspected for cracks. The glass plate 1 had an outer diameter of 95 mm, an inner diameter of the bore of 25 mm, and a thickness Th of 0.7 mm. During preheating, the entire main surface of the raw glass plate 10 was heated using an infrared heater. This preheating also simultaneously heated the inner and outer peripheral edges. The temperature Tp of the raw glass plate 10 was measured using a non-contact thermometer (thermography). When the temperature of the main surface of the glass plate 10 was measured during heating, it was found that the temperature was Tp at the central portion of the main surface, and the temperature was approximately uniform over the entire main surface, including the vicinity of the inner and outer peripheral end faces. The irradiation conditions of the laser beam L were width W1 = 1 mm, length W2 = 10 mm, and average power density Pd = 5.1 [W / mm2 The laser beam L was moved at a speed of 20 mm / sec along the edge 14. The outer peripheral edge of the raw glass plate 10 was chamfered first, and then the inner peripheral edge was chamfered. Pre-heating was performed at a temperature Tp before the outer peripheral edge was chamfered, and the outer peripheral edge and inner peripheral edge were chamfered in this order while maintaining the temperature. After the chamfering, no annealing treatment was performed to reduce residual stress in the main surfaces.
[0048] Table 1 below shows the crack occurrence level under each condition. In the "crack occurrence level" column, "C" means that "crack" occurred immediately after laser light irradiation. "B" means that "crack" did not occur immediately after laser light irradiation, but "delayed crack" occurred. "A" means that "crack" did not occur immediately after laser light irradiation, nor did "delayed crack" occur, but "crack" did occur. "AA" means that "crack", "delayed crack", and "crack" did not occur after laser light irradiation.
[0049]
[0050] From the results in Table 1, (Tg-Tp)≦−5.67×10 7 By preheating the material so as to satisfy α+840 (conditions 6 to 15), it is clear that no cracks occur immediately after laser irradiation. 7 It can be seen that preheating to satisfy α+500 (conditions 16 to 25) prevents delayed cracking. Also, (Tg-Tp)≦-3.28×10 7It can be seen that preheating to satisfy α + 428 (conditions 26 to 30) prevents the occurrence of cracks. Next, under conditions 26 to 28, the temperature Tp during the chamfering of the inner peripheral edge surface was adjusted to be 20°C lower than the temperature Tp during the chamfering of the outer peripheral edge surface, to produce an annular glass plate 1. The main surfaces were then polished to an arithmetic mean roughness Ra of 0.2 nm or less to obtain a magnetic disk glass substrate (conditions 31 to 33). The retardation of the annular glass plate 1 obtained under each of conditions 31 to 33 before main surface polishing and the magnetic disk glass substrate after main surface polishing was measured. The retardation values and distributions before and after main surface polishing were nearly identical under all conditions. Specifically, under all conditions, the maximum residual stress on the main surfaces was 50 nm or less, and peaks of retardation were observed near the outer and inner peripheral end faces in the radial direction. The maximum residual stress at the main surface end near the inner peripheral end face was greater than the maximum residual stress at the main surface end near the outer peripheral end face. Furthermore, the maximum residual stress at the main surface end near the inner peripheral end face was 50 nm or less, the maximum residual stress at the main surface end near the outer peripheral end face was 30 nm or less, and the residual stress in the intermediate region was 20 nm or less. Furthermore, the surface roughness Ra of the outer peripheral end face and the inner peripheral end face was 50 nm or less.
[0051] In addition, annular glass plates 1 were produced under the same conditions as Condition 30 except for changing (Tg - Tp) (Conditions 34 to 37). The cracking level under these conditions was AA. Under these conditions, the flatness of the raw glass plate and the glass plate was measured before and after the laser irradiation treatment including pre-heating, and the increase in flatness was calculated. The results are shown in Table 2.
[0052] The results in Table 2 show that the increase in flatness can be suppressed to 30 μm or less when (Tg - Tp) ≧ 50° C. Furthermore, it can be seen that the increase in flatness can be suppressed even further to 15 μm or less when (Tg - Tp) ≧ 100° C.
[0053] The method for manufacturing a glass plate, the method for manufacturing a glass substrate for a magnetic disk, the method for manufacturing a magnetic disk, and the annular glass plate of the present invention have been described in detail above. However, the present invention is not limited to the above-described embodiments and examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.
[0054] REFERENCE SIGNS LIST 1 glass plate 3 circular hole 5, 7 end face 10 raw glass plate 12 main surface 14 end face 16 circular hole 24 focusing lens
Claims
1. A method for manufacturing a glass plate including chamfering treatment of an end face, wherein the chamfering treatment includes a step of irradiating a laser beam onto an end face of a glass substrate before the chamfering treatment to form a chamfered surface, and a step of heating the glass substrate before the irradiation of the laser beam, and when the temperature of the glass substrate when heated is Tp [°C], the glass transition point of the glass substrate is Tg [°C], and the average linear expansion coefficient of the glass substrate is α [1 / °C], (Tg - Tp) ≤ -5.67×10 7 ·α + 840 is satisfied. A method for manufacturing a glass plate, characterized by this.
2. The manufacturing method of the glass sheet according to claim 1, which satisfies (Tg - Tp) ≤ -3.67×10 7 ·α + 500.
3. The manufacturing method of the glass sheet according to claim 1 or 2, which satisfies (Tg - Tp) ≤ -3.28×10 7 ·α + 428.
4. The method for manufacturing a glass plate according to any one of claims 1 to 3, which satisfies (Tg - Tp) ≥ 50°C.
5. The average linear expansion coefficient α of the glass substrate is 20×10 -7 [1 / °C] to 60×10 -7 [1 / °C]. The method for manufacturing a glass plate according to any one of claims 1 to 4.
6. The method for manufacturing a glass plate according to any one of claims 1 to 5, wherein the glass green sheet after the chamfering process is not subjected to an annealing process.
7. A method for manufacturing a glass substrate for a magnetic disk using the method for manufacturing a glass plate according to any one of claims 1 to 6, wherein the glass green sheet has an annular shape, and after manufacturing the glass plate using the method for manufacturing the glass plate, grinding and / or polishing is performed on the main surface of the manufactured glass plate to manufacture a glass substrate for a magnetic disk.
8. A method for manufacturing a magnetic disk, wherein a magnetic film is formed on the main surface of the glass substrate for a magnetic disk manufactured by the method for manufacturing a glass substrate for a magnetic disk according to claim 7.
9. An annular glass plate having a circular hole in the center, the annular glass plate having a main surface, an inner peripheral end surface forming the contour of the circular hole, and an outer peripheral end surface, the inner peripheral end surface and the outer peripheral end surface having chamfered surfaces, and the maximum value of the residual stress at the end of the main surface near the inner peripheral end surface being greater than the maximum value of the residual stress at the end of the main surface near the outer peripheral end surface.
10. The annular glass plate according to claim 9, wherein the residual stress is 50 [nm] or less in terms of retardation value at any location on the main surface of the glass plate.
11. The annular glass plate according to claim 9 or 10, wherein the glass plate is a glass substrate for a magnetic disk, and the arithmetic mean roughness Ra of the main surface is 0.2 nm or less.