Conductive sheets, circuit boards and electronic devices
Patent Information
- Application Number
- TW112114999
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-22
- Filing Date
- 2023-04-21
- Publication Date
- 2026-11-01
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Existing conductive compositions used in electronic equipment face issues with metal recyclability, adhesion, conductivity, anti-adhesion during storage, peelability, and reworkability, leading to inefficiencies and environmental concerns.
A conductive composition comprising metal powder and a binder, dissolved in a solvent mixture of nitrogen-containing organic solvent and basic inorganic compound, with specific surface properties and elastic coefficients, allowing for easy peeling and recyclability.
The solution provides a conductive sheet with excellent metal recyclability, high adhesion, conductivity, and improved peelability, reducing waste and enhancing manufacturing efficiency.
Abstract
Description
Technical Field
[0001] This disclosure relates to a conductive composition comprising metal powder (A) and an adhesive (B). Additionally, it relates to a conductive sheet, a terminal block, and an electronic device. Prior Technology
[0002] Printed circuit boards housed within electronic devices are flexible, but connectors and other components that connect to each other are sometimes reinforced with reinforcing plates to prevent deformation. Reinforcing plates may use epoxy glass or similar materials, while metal plates are used to provide electromagnetic noise suppression. In the connection between the printed circuit board and the metal plate, a conductive composition primarily composed of resin is used as the adhesive.
[0003] The adhesive may contain fillers for purposes such as making the metal plate conductive to the printed circuit board or controlling the elastic coefficient. For example, Patent Document 1 discloses connecting a conductor circuit to a reinforcing plate via a bonding layer, and describes using a conductive adhesive containing conductive particles and an adhesive as the bonding layer. Additionally, Patent Document 2 discloses a conductive adhesive sheet containing a thermosetting resin (A), a curing agent (B), conductive microparticles (C), and a compound (D), wherein the compound (D) has a functional group containing at least one element selected from the group consisting of nitrogen, phosphorus, and sulfur, and is selected from at least one element selected from the group consisting of silane coupling agents, silyl compounds, phosphoric acid, and bisphenol S-type epoxy resins.
[0004] Patent Document 3 discloses a conductive composition used in electronic components, etc., comprising: an adhesive containing a resin composition of a methyl phenolic resin having dimethylene ether bonds and a linear polymer with a molecular weight of 1000 or more compatible with the phenolic resin, and metal particles containing Cu powder coated with Ag. Patent Document 4 discloses a conductive paste containing a polyurethane prepolymer having an NCO value of 12% to 14% and a viscosity of 1000 mPa·s to 2000 mPa·s. [Existing Technical Documents] [Patent Literature]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2005-317946 [Patent Document 2] Japanese Patent Application Publication No. 2015-185717 [Patent Document 3] Japanese Patent Application Publication No. 8-217955 [Patent Document 4] Chinese Patent Application Publication No. 109943252 Specification Summary of the Invention
[0006] [The problem that the invention aims to solve]
[0007] Electronic devices equipped with printed circuit boards are being discarded due to exceeding their service life and the emergence of newer models. Furthermore, when conductive components are used as adhesives and processed into desired shapes and sizes to fit the printed circuit boards, a significant amount of terminal material is generated in this process, which is also discarded. In recent years, efforts to recover metal resources from these electronic devices and their manufacturing terminal material have become increasingly active for resource conservation purposes. One method for metal resource recovery involves burning and carbonizing organic matter at high temperatures (incineration), but this method requires a large amount of energy, thus necessitating more efficient alternatives (metal recovery methods).
[0008] Furthermore, in most cases, conductive sheets with a two-layer structure of conductive layer / protective sheet are manufactured and stored in rolls. When stored in rolls, the conductive components tend to adhere to the back of the protective sheet during use, resulting in a problem known as adhesion (anti-adhesion).
[0009] Furthermore, regarding the conductive sheet, after the first adhered material is bonded to the conductive component (temporarily adhered), the protective sheet is peeled off, allowing the second adhered material to adhere to the exposed conductive component. However, due to insufficient strength of the protective sheet or excessive adhesion between the conductive component and the protective sheet, poor peeling (ease of peeling) occurs when the protective sheet is peeled off, resulting in damage to the protective sheet.
[0010] Furthermore, if conductive components are stored at high temperatures, the reaction of the hardener may occur, reducing adhesion. Therefore, conductive components are sometimes stored refrigerated or frozen. However, conductive components taken from refrigerated or frozen storage may sometimes condense due to moisture in the air. If bonding is performed with water droplets (including invisible fine particles) on the adhesive surface, poor adhesion may occur. Therefore, the inability to bond to the substrate before the moisture evaporates is a major cause of reduced production efficiency (immediacy).
[0011] Furthermore, from the perspective of reducing environmental impact, there is a need for a technology to improve the manufacturing yield of printed circuit boards. In the manufacturing process of printed circuit boards, conductive sheets are typically temporarily adhered to the board and bonded using thermoforming. If re-peelability (reprocessability) can be ensured at the temporary adhesion stage, the manufacturing yield can be improved. However, if re-peeling occurs, paste residue is left on the adhered material, sometimes making reprocessing impossible. Additionally, with the thin-film nature of circuit boards, the boards themselves are prone to damage, and there is also the problem of difficulty in ensuring reprocessability at the temporary adhesion stage.
[0012] The purpose of this disclosure is to provide a conductive sheet having a conductive component and a terminal block including the conductive component. The conductive component has excellent metal recyclability, high adhesion and conductivity, prevents adhesion to the protective sheet during storage, and the protective sheet has excellent peelability, water droplet evaporation and reprocessability. [Methods for solving problems]
[0013] This disclosure provides the following conductive components, conductive sheets, terminal blocks, and electronic devices. [1]: The conductive composition disclosed herein is a conductive sheet on which a conductive composition comprising metal powder (A) and an adhesive (B) is disposed on a main surface of a protective sheet (D). The conductive component, when immersed in a solvent component (C) at 30°C for 24 hours, dissolves and leaves a residue containing metallic elements. The peak density Spd of the conductive composition on the non-opposing side of the protective sheet (D) is 1,000 peaks / mm² to 500,000 peaks / mm². The solvent composition (C) contains 5% to 40% by mass of a nitrogen-containing organic solvent (c1) relative to the total mass of the solvent composition (C), and contains 5% to 40% by mass of a basic inorganic compound (c2) relative to the total mass of the solvent composition (C). [2]: The conductive sheet as described in [1], wherein the conductive component has adhesive properties. [3]: The conductive sheet as described in [1] or [2], wherein the adhesive (B) has one or more groups selected from the group consisting of ester group, amide group, amide group, carbamate group and urea group. [4]: The conductive sheet as described in any one of [1] to [3], wherein the adhesive (B) has two or more selected from the group consisting of ester group, amide group, amide group, carbamate group and urea group. [5]: The conductive sheet as described in any one of [1] to [4], wherein the ratio of the unfolded area of the surface of the conductive composition on the non-opposite side to the protective sheet (D) is 0.01 to 4. [6]: The conductive sheet as described in any one of [1] to [5], wherein the highest value (2) of the storage elasticity coefficient (2) of the conductive component at 0°C to 30°C is 0.01 GPa to 100 GPa. The value α obtained by dividing the highest value (2) by the highest value (1) of the storage elasticity coefficient of the protective sheet (D) at 0℃~30℃ is 0.01~30. [7]: The conductive sheet as described in any one of [1] to [6], wherein the maximum value of the storage elastic coefficient of the protective sheet (D) at 0°C to 30°C is 0.01 GPa to 1000 GPa. [8]: A terminal block comprising a metal plate, a conductive component obtained by peeling off a protective sheet (D) of a conductive sheet as described in any one of [1] to [7], and a terminal block substrate. The metal plate is fixed to the wiring circuit board via the conductive component. [9]: An electronic device comprising a terminal block as described in [8].
[10] : A conductive composition comprising metal powder (A) and binder (B) is partially dissolved and partially insoluble when immersed in a solvent composition (C) comprising 5% to 40% by mass of a nitrogen-containing organic solvent (C1) and 5% to 40% by mass of an alkaline inorganic compound (C2) at 30°C for 24 hours, and the insoluble component contains a metal element derived from the metal powder (A).
[11] : The conductive composition as described in
[10] has adhesion.
[12] : The conductive composition as described in
[10] or
[11] , wherein the adhesive (B) has one or more groups selected from the group consisting of ester, amide, amide, carbamate and urea.
[13] : The conductive composition as described in any one of
[10] to
[12] , wherein the adhesive (B) has two or more groups selected from the group consisting of ester group, amide group, amide group, carbamate group and urea group. [The effects of the invention]
[0014] This disclosure provides a conductive sheet having a conductive component with excellent metal recyclability, high adhesion and conductivity, preventing adhesion to protective sheets during storage, and exhibiting excellent peelability, water evaporation resistance, and reprocessability of the protective sheet. This provides a power strip that is easily recyclable. Simple Explanation of the Diagram
[0015] none Implementation
[0016] The conductive components, conductive sheets, and terminal blocks disclosed herein will be described in turn. Furthermore, unless otherwise specified, the "~" indicating a numerical range includes both the lower and upper limits.
[0017] [Conductive components] The conductive composition disclosed herein comprises metal powder (A) and a binder (B). When this conductive composition is immersed in a solvent composition (C) comprising 5% to 40% by mass of a nitrogen-containing organic solvent (C1) and 5% to 40% by mass of a basic inorganic compound (C2) at 30°C for 24 hours, a portion dissolves, and a portion remains insoluble, with the insoluble portion containing metal elements derived from the metal powder (A). In other words, the conductive composition dissolves, leaving a residue. This residue contains metal elements derived from the metal powder (A).
[0018] Here, dissolution in this disclosure is defined as the phenomenon where, when an article is immersed in a solvent composition (C) and brought into contact with the solvent composition (C), a portion of the article dissolves into the solvent composition (C) and cannot maintain its original shape. That is, the article does not need to be completely dissolved into the solvent composition (C), and insoluble components (residues) may still exist.
[0019] The metal element contained in the insoluble component (residue) when the conductive composition of this invention is dissolved in the solvent composition (C) includes elements derived from the metal powder (A). The solvent composition (C) functions as an adhesive (B). Through the decomposition caused by the solvent in the solvent composition (C), the adhesive (B) is decomposed and dissolved into the solvent composition (C), leaving an insoluble metal powder (A) in the residue, thereby allowing for efficient and good recovery of the metal powder (A) from the conductive composition. Regarding the conductive layer of this invention, when immersed in the solvent composition (C) at 30°C for 24 hours, it dissolves and leaves a residue containing metal elements derived from the metal powder (A).
[0020] [Metallic powder (A)] Metal powder (A) is used for the purpose of imparting conductivity to conductive components. The metal powder (A) is preferably a conductive metal such as gold, platinum, silver, copper, and nickel, or their alloys. Alternatively, composite microparticles having a core and a coating layer formed from a material with higher conductivity than the core, covering the surface of the core, can be used instead of single-component microparticles. From the viewpoint of cost reduction, composite microparticles are preferred. The core is preferably a conductive metal or its alloy, more preferably selected from nickel, silicon dioxide, and copper. The coating layer can be any conductive material, preferably a conductive metal or a conductive polymer. Examples of conductive metals include gold, platinum, silver, tin, manganese, and indium, and their alloys. Among these, silver is preferred in terms of conductivity.
[0021] Metal powder (A) can be used alone or in combination with two or more types.
[0022] The composite microparticles preferably have a coating layer at a ratio of 1 to 40 parts by mass relative to 100 parts by mass of the core, more preferably 5 to 30 parts by mass. Coating at 1 to 40 parts by mass maintains conductivity while further reducing costs. Furthermore, the composite microparticles preferably have a coating layer that completely covers the core. However, in practice, there are cases where part of the core is exposed. In such cases, if the conductive material covers more than 70% of the surface area of the core, conductivity is easily maintained.
[0023] The shape of the metal powder (A) is not limited as long as it achieves the desired conductivity. For example, it is preferably spherical, flake-shaped, leaf-shaped, dendritic, plate-shaped, needle-shaped, rod-shaped, grape-shaped, or amorphous block-shaped. In order to efficiently form a longitudinal conductive path between the metal reinforcement plate and the terminal block, it is more preferably spherical or dendritic.
[0024] Regarding the average particle size of the metal powder (A), when the metal powder (A) is spherical, dendritic, needle-like, rod-like, grape-like, or amorphous, the average particle size D50 is preferably 5 μm to 20 μm, more preferably 5.5 μm to 15 μm, and even more preferably 6 μm to 10 μm. By keeping the average particle size D50 within the range of 5 μm to 20 μm, both adhesion and conductivity can be considered. Furthermore, the average particle size D50 can be determined using a laser diffraction-scattering particle size distribution measuring device.
[0025] Furthermore, when the metal powder (A) is in the form of spheres, dendrites, needles, rods, grapes, or irregular lumps, from the viewpoint of balancing adhesion and conductivity, it is preferable that D10 is 1 μm to 15 μm and D90 is 10 μm to 30 μm. D10, D90, and the average particle size D50 can also be determined using a laser diffraction-scattering particle size distribution measuring device.
[0026] Furthermore, when the metal powder (A) is in the form of spheres, dendrites, needles, rods, grapes, or irregular lumps, it is preferable that D 90 / D 10 is 1.5 to less than 8.0. By optimizing the filling state of the metal powder (A) in the conductive composition within this range, the conductivity is particularly excellent.
[0027] When the metal powder (A) is in the form of flakes, leaves, or plates, the average particle size D50 of the metal powder (A) is preferably 5 μm to 50 μm, more preferably 6.5 μm to 30 μm, and even more preferably 8 μm to 20 μm. By keeping the average particle size D50 within the range of 5 μm to 50 μm, both adhesion and conductivity can be considered.
[0028] Furthermore, when the metal powder (A) is in the form of flakes, leaves, or plates, from the viewpoint of balancing adhesion and conductivity, it is preferable that D10 is 1 μm to 25 μm and D90 is 10 μm to 100 μm.
[0029] Furthermore, when the metal powder (A) is in the form of flakes, leaves, or plates, it is preferable that the D 90 / D 10 ratio is 1.5 to less than 8.0. By optimizing the filling state of the metal powder (A) in the conductive composition within this range, the conductivity is particularly excellent.
[0030] The content of metal powder (A) in the conductive composition is preferably 40% to 90% by mass, more preferably 45% to 80% by mass, and even more preferably 50% to 70% by mass. By setting the above-mentioned addition amount, metal recyclability, adhesion and conductivity can be balanced.
[0031] [Adhesive (B)] The binder (B) serves as the matrix for the conductive components and functions to disperse and support the metal powder (A). The binder (B) requires decomposition by the solvent component (C), and is therefore preferably an organic material. The composition of the binder (B) is not particularly limited as long as it possesses the functions described above, but it is preferably a resin (b-1). In this disclosure, the resin (b-1) is defined as an organic material that is solid, semi-solid, or solidified at room temperature and has a weight-average molecular weight (Mw) of 5,000 or more, having a softening or melting range.
[0032] The adhesive (B) utilizes a solvent composition (C) with a strong solvent-induced decomposition effect, where specific chemical bonds are broken down by the solvent and dissolved into the solvent composition (C). The adhesive (B) preferably has one or more functional groups selected from the group consisting of ester, amide, amide, carbamate, and urea groups. By having the aforementioned functional groups in the conductive composition, the decomposition of the solvent composition (C) can be more efficient, the molecular chain of the adhesive (B) is further refined, more adhesive (B) dissolves into the solvent composition (C), and the amount of adhesive (B)-derived components in the residue can be reduced.
[0033] The effect is further enhanced when the adhesive (B) has two or more groups selected from the group consisting of ester, amide, amide, carbamate, and urea. By having two or more groups, multiple effects can be achieved, thereby more efficiently decomposing the adhesive (B). As a preferred example, a combination of one or more groups selected from ester, amide, amide, urea, and ester with a carbamate group can be exemplified.
[0034] [Resin(b-1)] The resin (b-1) is not particularly limited in composition or molecular structure except for the weight average molecular weight (Mw) mentioned above. It is preferably a resin having one or more chemical bonds selected from the group consisting of amide bonds, amide bonds, carbamate bonds and urea bonds. Furthermore, from the viewpoint of exhibiting the function of dispersing and supporting metal powder (A), resin (b-1) is preferably a thermosetting resin, thermoplastic resin, UV-curable resin or other photocurable resin, natural resin or elastomer, and from the viewpoint of imparting excellent adhesion to conductive components, resin (b-1) is preferably a thermosetting resin (b-2).
[0035] [Thermosetting resin (b-2)] Thermosetting resin (b-2) is a thermosetting resin among resins (b-1). Thermosetting property is defined as "an irreversible increase in the elastic modulus due to polymerization and / or cross-linking reactions caused by heat".
[0036] Regarding the thermosetting property described above, when the thermosetting resin (b-2) has reactive functional groups, it can be manifested by the reaction of the reactive functional groups with each other. Alternatively, it can be manifested by the reaction of the reactive functional groups assembled in the thermosetting resin (b-2) and the curing agent (H) described later.
[0037] Examples of thermosetting resins (b-2) include epoxy resins, phenolic resins, polyacrylic resins, polyester resins, polyurethane resins, polyamide resins, polyimide resins, polyamide-amide resins, urea resins, polyurethane urea resins, melamine resins, and polyolefin resins. Among these, the thermosetting resin (b-2) preferably has one or more groups selected from the group consisting of ester, amide, amide, carbamate, and urea groups. The amide, amide, carbamate, and urea bonds achieve strong adhesion through the interaction of the non-covalent electron pairs of the nitrogen atoms contained in the bonds with the adhered material. By having the thermosetting resin (b-2) selected from two or more groups selected from the group consisting of ester, amide, amide, carbamate, and urea groups, the adhesion-enhancing effect described above can be further improved.
[0038] The adhesive (B) may further include a hardener (H). The hardener (H) in this disclosure is a substance that promotes or regulates the hardening reaction, defined as a substance with a molecular weight or weight average molecular weight (Mw) of less than 5,000. A hardening reaction is defined as "the irreversible increase in the elastic modulus caused by polymerization and / or cross-linking of a prepolymer or polymeric composition through means such as heating, radiation, or a catalyst." In the adhesive (B), from the viewpoint that polymerization and / or cross-linking are formed through stimulation such as heat, resulting in strong adhesion of the conductive component, the adhesive (B) of this disclosure preferably includes a hardener (H). The curing agent (H) may be appropriately selected from known compounds that exhibit curing properties through combination with the thermosetting resin (b). Examples of curing agents (H) include: epoxy compounds, oxetane compounds, cyclosulfide compounds, aziridine compounds, isocyanate compounds, amine compounds, isocyanate compounds, imidazole compounds, and acid anhydrides.
[0039] The epoxy compounds are preferably glycidyl ether type epoxy compounds, glycidyl amine type epoxy compounds, glycidyl ester type epoxy compounds, or cyclic aliphatic (alicyclic) epoxy compounds.
[0040] Examples of glycidyl ether type epoxy compounds include: bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, bisphenol AD type epoxy compounds, cresol phenolic varnish type epoxy compounds, phenolic varnish type epoxy compounds, α-1-naphthol phenolic varnish type epoxy compounds, bisphenol A type phenolic varnish type epoxy compounds, dicyclopentadiene type epoxy compounds, tetrabromobisphenol A type epoxy compounds, brominated phenolic varnish type epoxy compounds, tris(glycidyloxyphenyl)methane, and tetra(glycidyloxyphenyl)ethane.
[0041] Examples of glycidylamine-type epoxy compounds include: tetraglycidyldiaminodiphenylmethane, triglycidylp-aminophenol, triglycidylm-aminophenol, and tetraglycidylm-phenylenediamine.
[0042] Examples of glycidyl ester type epoxy compounds include: diglycidyl phthalate, hexahydrodiglycidyl phthalate, and tetrahydrodiglycidyl phthalate.
[0043] Examples of such cyclic aliphatic (alicyclic) epoxy compounds include: epoxycyclohexylmethyl-epoxycyclohexane carboxylate and bis(epoxycyclohexyl) adipate.
[0044] Examples of oxetane compounds include: 1,4-bis{[(3-ethyloxetane-3-yl)methoxy]methyl}benzene, 3-ethyl-3-{[(3-ethyloxetane-3-yl)methoxy]methyl}oxetane, 1,3-bis[(3-ethyloxetane-3-yl)methoxy]benzene, 4,4'-bis[(3-ethyl-3-oxetane-butyl)methoxymethyl]biphenyl, ester compounds of (2-ethyl-2-oxetane-butyl)ethanol and terephthalic acid, ether compounds of (2-ethyl-2-oxetane-butyl)ethanol and phenolic varnish resins, and ester compounds of (2-ethyl-2-oxetane-butyl)ethanol and polycarboxylic acid compounds.
[0045] Examples of cyclic sulfur compounds include: bis(1,2-cyclothioethyl) sulfide, bis(1,2-cyclothioethyl) disulfide, bis(2,3-cyclothiopropyl) sulfide, bis(2,3-cyclothiopropylthio)methane, bis(2,3-cyclothiopropyl) disulfide, bis(2,3-cyclothiopropyl dithio)methane, bis(2,3-cyclothiopropyl dithio)ethane, and bis(6,7-cyclothio-3,4-dithioheptyl) sulfide. Bis(6,7-cyclothio-3,4-dithioheptyl) disulfide, 1,4-dithiazide-2,5-bis(2,3-cyclothiopropyldithiomethyl), 1,3-bis(2,3-cyclothiopropyldithiomethyl)benzene, 1,6-bis(2,3-cyclothiopropyldithiomethyl)-2-(2,3-cyclothiopropyldithioethylthio)-4-thiohexane, 1,2,3-tris(2,3-cyclothiopropyldithio)propane.
[0046] Examples of aziridine compounds include: trimethylolpropane-tri-a-2-aziridine propionate, tetramethylolmethane-tri-a-2-aziridine propionate, N,N'-diphenylmethane-4,4'-bis(1-aziridine carboxylated amide), and N,N'-hexamethylene-1,6-bis(1-aziridine carboxylated amide).
[0047] Examples of amine compounds include: diethyltriamine, triethyltetraamine, methylenebis(2-chloroaniline), methylenebis(2-methyl-6-methylaniline), 1,5-naphthalene diisocyanate, and n-butyl benzyl phthalate.
[0048] Examples of isocyanate compounds include: toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylene diisocyanate, dicyclohexylmethane diisocyanate, 1,5-naphthalene diisocyanate, tetramethylxylene diisocyanate, and trimethylhexamethylene diisocyanate.
[0049] Examples of imidazole compounds include: 2-methylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methylimidazole, and 1-cyanoethyl-2-undecylimidazole ontyl trimellitate.
[0050] Examples of acid anhydrides include: tetrahydrophthalic anhydride, dodecenyl succinic anhydride, methyl benzoic anhydride, trimellitic anhydride, and pyromellitic dianhydride.
[0051] When the thermosetting resin (b-2) is set to 100 parts by weight, the content of the curing agent (H) is preferably 1 part by weight to 70 parts by weight, more preferably 3 parts by weight to 50 parts by weight, and even more preferably 3 parts by weight to 30 parts by weight. By using a curing agent (H) content of 1 part by mass or more, the conductive composition can be set to a B-stage curing state. B-stage curing is a method in which the curing agent (H) partially undergoes a curing reaction by heating the conductive composition at a specified temperature and time. By performing B-stage curing, the strength of the conductive composition can be improved while maintaining its adhesion, and the anti-blocking property can be improved by increasing the elasticity of the conductive composition. In addition, by using a curing agent (H) content of 70 parts by mass or less, the formation of excessive cross-linking structures during the curing of the conductive composition can be suppressed, and the solubility of the adhesive (B) in the solvent composition (C) can be improved.
[0052] The step of heating the conductive component and attaching it to the substrate is preferably heat pressing. Applying pressure improves adhesion to the substrate. The heat pressing conditions can be appropriately selected based on the composition of the conductive component or the material, size, and shape of the substrate. For example, preferably, it is 130°C to 200°C, 1 MPa to 10 MPa, and 3 to 60 minutes.
[0053] Regarding the excellent adhesion to metal plates and wiring circuit boards, the adhesive (B) is preferably present in a proportion of 10% to 60% by mass of the total solid components of the conductive composition.
[0054] The conductive composition disclosed herein preferably has voids. The presence of voids in the conductive composition promotes the penetration of the solvent composition (C), thereby improving metal recovery. The presence or absence of voids or the porosity can be adjusted using any of the known methods; by using dendritic metal powder as the metal powder (A), voids can be relatively easily created.
[0055] The porosity of the conductive component is preferably 0.5% to 60%. By setting the porosity to 0.5% or higher, the penetration of the solvent component (C) is promoted, metal recoverability is improved, and the evaporation of condensation generated during removal from the cold storage is facilitated, thus improving timeliness. Furthermore, by setting the porosity to 60% or lower, the accumulation of excessive condensation can be suppressed, further improving timeliness. A porosity of 1.0% to 30% is more preferably preferred.
[0056] Furthermore, in this specification, "porosity" refers to the proportion of void area derived from a microscopic image of a cross-section of the conductive component. The specific calculation method is as follows. A scanning electron microscope (SEM) or laser microscope is suitable for observing the cross-section of the conductive component. If the cross-section is observed vertically, a contrast difference is generated between the conductive component and the voids, allowing the shape of the voids to be identified. For the cross-sectional image of the conductive component, the image analysis software "GIMP 2.10.6" is used to binarize the conductive component portion and the void portion into black and white. Then, by counting the number of pixels in the black and white areas, the proportion of the void area is calculated based on the ratio of the number of pixels.
[0057] The porosity of the conductive component can be suitably controlled using known methods such as foaming agents that generate voids through arbitrary triggering such as heat, preferably by controlling the porosity based on the shape or content of the metal powder (A). In the case of metal powder (A), especially when it is a high-volume dendritic (dendritic) material, the effect disclosed herein readily creates visible voids, which is superior compared to other metal powders. Furthermore, as the content of metal powder (A) increases, there is a tendency for the porosity to increase.
[0058] [Solvent Composition (C)] The solvent composition (C) disclosed herein comprises a nitrogen-containing organic solvent (c1) and a basic inorganic compound (c2). From the viewpoint of enabling the solvent composition (C) to efficiently act as a solubilizer on the adhesive (B), the solvent composition (C) comprises 5% to 40% by mass of the nitrogen-containing organic solvent (c1) relative to the total mass of the solvent composition (C). The content of the nitrogen-containing organic solvent (c1) is preferably 10% to 30% by mass. The nitrogen-containing organic solvent (c1) can be any organic solvent containing nitrogen atoms in its molecule without particular restriction. Specifically, N-methyl-2-pyrrolidone, n-propyl bromide, γ-butyrolactone, monoethanolamine, diethanolamine, and triethanolamine can be used, and the appropriate type can be selected according to the composition of the adhesive (B) being dissolved.
[0059] From the viewpoint of making the solvent composition (C) alkaline and promoting the decomposition of the adhesive (B) by the solvent, the solvent composition (C) contains 5% to 40% by mass of an alkaline inorganic compound (C2) relative to the total mass of the solvent composition (C). Substances exhibiting the aforementioned function can be used without particular limitation; the alkaline inorganic compound (C2) may be, for example, at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, ammonium hydroxide, sodium bicarbonate, sodium dihydrogen phosphate, sodium phosphate, trisodium phosphate, potassium dihydrogen phosphate, and tripotassium phosphate. From the viewpoint of imparting better solubility to the solvent composition (C), the content of the alkaline inorganic compound (C2) is preferably 10% to 30% by mass.
[0060] From the viewpoint of imparting fluidity, it is appropriate to add an organic solvent for dilution or an additive that promotes the decomposition of the binder (B) to the solvent composition (C). From the viewpoint of facilitating the handling of the solvent composition (C), it is preferable to use glycerol with low volatility.
[0061] [Conductive sheet] The conductive sheet of this embodiment is a conductive sheet on one main surface (only one surface) of a protective sheet (D) having a conductive composition comprising metal powder (A) and an adhesive (B). In other words, this conductive sheet is a sheet-like article having a conductive composition on the protective sheet (D). Furthermore, the conductive composition included in the conductive sheet is a non-flowing solid at room temperature and is formed as a layer of a certain thickness, also referred to as a conductive layer. When this conductive layer is immersed in a solvent composition (C) at 30°C for 24 hours, it will dissolve and leave residue, which contains metal elements.
[0062] [Protective Film (D)] The protective sheet (D) is suitable for use if the film has been demolded on one or both sides. Examples of substrates for the protective sheet (D) include: plastic sheets made of polyethylene terephthalate, polyethylene naphthalate, polyvinyl fluoride, polyvinylidene fluoride, rigid polyvinyl chloride, polyvinylidene chloride, nylon, polyimide, polystyrene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polycarbonate, polyacrylonitrile, polybutene, flexible polyvinyl chloride, polyvinylidene fluoride, polyethylene, polypropylene, polyurethane, ethylene-vinyl acetate copolymer, polyvinyl acetate, etc.; paper types such as cellophane, woodfree paper, kraft paper, coated paper, etc.; various non-woven fabrics, synthetic papers, metal foils, or composite films composed of these. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred from the viewpoint of improving peelability.
[0063] The surface of the protective film (D) can be treated with a matte finish as needed. Examples of matte finishes include: sandblasting, etching, coating, chemical matting, and kneading.
[0064] Protective film (D) can be obtained, for example, by applying a release agent to a substrate. Release agents that can be used include: hydrocarbon resins such as polyethylene and polypropylene, higher fatty acids and their metal salts, higher fatty acid soaps, waxes, animal and vegetable oils, mica, talc, silicone surfactants, silicone oil, silicone resins, fluorinated surfactants, fluororesins, fluorinated silicone resins, melamine resins, acrylic resins, etc. The application method for the release agent can be any of the known methods, such as gravure coating, matte coating, die coating, lip coating, corner wheel coating, blade coating, roller coating, knife coating, spray coating, bar coating, spin coating, and dip coating.
[0065] The maximum value (1) of the storage elastic coefficient (1) of the protective sheet (D) at 0℃~30℃ is preferably 0.01 GPa~1000 GPa, more preferably 0.1 GPa~100 GPa. With the maximum value (1) of the storage elastic coefficient (1) of the protective sheet (D) at 0℃~30℃ being between 0.01 GPa and 1000 GPa, when the protective sheet (D) is peeled off from the conductive component after heat lamination, the protective sheet (D) will not elongate or break, and can be easily peeled off.
[0066] The highest value (2) of the storage elastic coefficient of the conductive composition (conductive layer) at 0°C to 30°C is preferably 0.01 GPa to 100 GPa, more preferably 1 GPa to 10 GPa. Since the highest value (2) of the storage elastic coefficient of the conductive composition at 0°C to 30°C is within this range, the conductive composition will not elongate or break when the protective sheet (D) is peeled off from the conductive composition after heat lamination, and can be easily peeled off. The storage elastic coefficients of the conductive composition and the protective sheet (D) can be determined using a dynamic viscoelasticity measuring device.
[0067] The value α obtained by dividing the highest value (2) of the storage elasticity coefficient of the conductive composition (conductive layer) at 0℃~30℃ by the highest value (1) of the storage elasticity coefficient of the protective sheet (D) at 0℃~30℃ is preferably 0.01~30, more preferably 0.1~15. With α being 0.01~30, the protective sheet (D) can be easily peeled off from the conductive composition after heat lamination.
[0068] [Density at the summit point (Spd) and the ratio of unfolded area (Sdr)] In the conductive sheet disclosed herein, the peak density Spd of the conductive component (conductive layer) on the surface that is not facing the protective sheet (D) (non-facing side) has a peak density of 1,000 to 500,000 per mm². By setting the contact points with the adherend within this range, excessive adhesion to the adherend can be suppressed, thereby improving reprocessability. The peak density Spd is preferably 10,000 to 300,000 per mm², and more preferably 25,000 to 250,000 per mm².
[0069] The peak density Spd (hereinafter sometimes simply referred to as Spd) of an interface is defined in International Organization for Standardization (ISO) 25178-2:2012, representing the number of peaks in each defined region (unit area).
[0070] From the viewpoint of balancing adhesion and anti-adhesion, the conductive sheet disclosed herein preferably has an unfolded area ratio (Sdr) of 0.01 to 4 for the non-facing surface of the conductive component (conductive layer) that is not facing the protective sheet (D). The conductive sheet is stored or transported in a rolled state. When the conductive sheet is unwound from the rolled state, adhesion to the back of the protective sheet (D) sometimes occurs. By setting the Sdr of the conductive layer surface to the aforementioned specific range, the unevenness of each defined area can be made dense. This reduces the contact area between the surface of the conductive component and the back of the protective sheet (D) in the rolled form, thus balancing adhesion and anti-adhesion.
[0071] The unfolded area ratio Sdr (hereinafter sometimes simply referred to as Sdr) of an interface is defined in ISO 25178-2:2012 and is an indicator of how much the unfolded area (surface area) of a defined region increases relative to the area of the defined region. Furthermore, the Sdr of a flat surface is 0 (zero).
[0072] In this disclosure, the peak density Spd and the unfolded area ratio Sdr are values obtained according to ISO 25178-2:2012. Specifically, they can be calculated as follows: measurement data are acquired using a laser microscope (manufactured by KEYENCE, VK-X100), and the acquired measurement data are imported into analysis software (including the analysis application "VK-H1XA" of the ISO 25178-2:2012 surface property measurement module "VK-H1XR", both manufactured by KEYENCE), and the ISO 25178-2:2012 surface property measurement is performed.
[0073] The inventors further discovered that by having a surface area ratio Sdr of 0.01 to 4.0 for the conductive component whose surface is not facing the protective sheet (D), water droplets evaporate easily. Because water droplets evaporate easily, the evaporation time of condensation generated when removed from a cold storage facility can be shortened, for example. As a result, the waiting time for the adhesion process to the object being adhered to can be shortened (hereinafter also referred to as immediacy), thus improving work efficiency. From the viewpoint of improving immediacy, the surface area ratio Sdr is preferably 0.1 to 3.0, and more preferably 0.25 to 2.0.
[0074] [Control methods for Spd and Sdr] The methods for controlling the peak density Spd and unfolded area ratio Sdr of the conductive sheet surface disclosed herein can utilize existing known methods for adjusting the surface shape of an object. Spd and Sdr can be achieved using different methods or a combination of methods. Examples include: a method of polishing the surface using abrasive paper; shot peening by blowing abrasive material onto the surface of the conductive composition using compressed air; forming a conductive composition on a film with a specified peak density Spd and unfolded area ratio Sdr, removing the film after laminating a protective film, and transferring the surface irregularities; pressing a film with a specified peak density Spd and unfolded area ratio Sdr onto a conductive composition and transferring the surface irregularities; and a method of controlling surface irregularities by containing particulate matter in the conductive composition.
[0075] From the perspective of balancing thinness and conductivity, the thickness of the conductive component (conductive layer) in the conductive sheet is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and even more preferably 30 μm to 70 μm.
[0076] [Manufacturing method of conductive sheet] The conductive sheet disclosed herein can be obtained, for example, by coating a conductive component onto a protective sheet (D) and drying it, followed by stage B curing as needed. The coating method can be appropriately selected from known methods, taking into account factors such as the film thickness of the adhesive. Specific examples of coating methods include: gravure coating, mating coating, die coating, lip coating, corner wheel coating, blade coating, roller coating, knife coating, spray coating, bar coating, spin coating, and dip coating.
[0077] [Manufacturing method of the junction box] As an example, the manufacturing method of this terminal block can be described as follows: a method of laminating a circuit board substrate for a printed terminal block, a conductive component, and a metal plate, pressing and bonding them together, and then mounting electronic components on the substrate. An example of the manufacturing method of the terminal block is described below.
[0078] First, a conductive varnish is applied to the protective sheet (D) and allowed to dry to prepare a conductive sheet (step a). Next, with the exposed surface of the conductive layer (the non-facing surface of the protective sheet (D)) in contact with the metal plate, a heat-lamination is performed to deposit the conductive sheet onto the metal plate (step b). Then, the protective sheet (D) is peeled off (step c), and with the exposed conductive material in contact with the wiring circuit board, a heat-lamination is performed (step d). Afterward, the conductive material is hardened by heating and pressing, resulting in a wiring board with a metal plate fixed to the wiring circuit board (step e).
[0079] [Electronic Devices] This junction box can be used in all existing, known products that use printed junction boxes. Specifically, it can be used in electronic devices such as mobile phones, smartphones, personal computers (PCs), digital cameras, and LCD monitors. It is particularly suitable for use in transportation equipment such as automobiles, trams, ships, and airplanes. [Example]
[0080] The following examples and comparative examples illustrate this disclosure in detail, but this disclosure is not limited to these examples. The mixing ratio represents a value other than the solvent, converted to solid components. Additionally, "parts" means "parts by mass".
[0081] [Average particle size of metal powder (A) with D10, D50, and D90] The average particle size D50 was measured using a laser diffraction-scattering particle size distribution measuring device LS13320 (manufactured by Beckman Coulter). This value was obtained by measuring the conductive filler using a tornado dry powder sample module, and represents the particle size at the 50% cumulative value in the cumulative particle size distribution. Furthermore, the refractive index was set to 1.6. D10 and D90, the average particle sizes at the 10% and 90% cumulative values in the cumulative particle size distribution, respectively, were measured in the same manner.
[0082] [Acid value of thermosetting resin (b-2)] According to the neutralization titration method of Japanese Industrial Standards (JIS) K 0070, the acid value (mg KOH / g) was determined by converting the solid composition. Approximately 1 g of the sample was accurately measured into a co-stoppered Erlenmeyer flask, and 100 mL of a tetrahydrofuran / ethanol mixture (volume ratio: tetrahydrofuran / ethanol = 2 / 1) was added to dissolve it. Phenolphthalein solution was added as an indicator, and titration was performed using 0.1 N alcoholic potassium hydroxide solution, with the endpoint determined when the indicator remained pale red for 30 seconds. The acid value was calculated using the following formula (unit: mg KOH / g). Acid value (mgKOH / g) = (5.611 × a × F) / S in, S: Sample volume (g) a: 0.1 N alcoholic potassium hydroxide solution consumed (mL) F: 0.1 N Force value of alcoholic potassium hydroxide solution
[0083] [Weight-average molecular weight (Mw) of thermosetting resin (b-2)] Mw was determined using a gel permeation chromatography (GPC) system, HPC-8020 (manufactured by Tosoh Corporation). GPC is a liquid chromatography instrument that separates and quantifies substances dissolved in a solvent (THF: tetrahydrofuran) based on differences in molecular size. In this study, two LF-604 (manufactured by Showa Denko Corporation: rapid analysis GPC column, 6 mm ID × 150 mm) columns were connected in series on a column at a flow rate of 0.6 mL / min and a column temperature of 40°C. Mw was determined using polystyrene conversion.
[0084] <Preparation of Conductive Components> The following shows the raw materials used in the manufacture of each conductive component.
[0085] <Ingredients> Metal powder (A) A1: Silver-coated copper powder: D50=5.7 μm, D10=2.1 μm, D90=12.8 μm, dendritic (manufactured by Mitsui Metals & Minerals). A2: Silver-coated copper powder: D50=31.2 μm, D10=12.9 μm, D90=44.6 μm, dendritic (manufactured by Mitsui Metals Mining). A3: Silver-coated copper powder: D50=10.8 μm, D10=3.2 μm, D90=29.5 μm, spherical (Showa Denko Materials Manufacturing Co., Ltd.) A4: Silver-coated copper powder: D50=7.5 μm, D10=1.5 μm, D90=11.3 μm, spherical (Showa Denko Materials Manufacturing Co., Ltd.) A5: Silver-coated copper powder: D50=11.3 μm, D10=3.8 μm, D90=29.5 μm, flake form (manufactured by DOWA Holdings) Adhesive (B) Thermosetting resin (b-2) P1: Polyester resin (thermosetting resin with ester groups): Acid value 36 mgKOH / g, Mw=27,000 (manufactured by Toyo Chemical Co., Ltd.) P2: Polyimide resin (thermosetting resin with amide groups): Acid value = 22 mgKOH / g, Mw = 55,000 (manufactured by Toyo Chemical Co., Ltd.) P3: Polyamide resin (thermosetting resin with amide groups): Acid value = 28 mgKOH / g, Mw = 49,000 (manufactured by Toyo Chemical Co., Ltd.) P4: Polymaleimide resin (thermosetting resin with maleimide groups): Acid value = 13 mgKOH / g, Mw = 98,000 (manufactured by Toyo Chemical Co., Ltd.) P5: Polyurethane-Imidium Resin (a thermosetting resin containing urethane and amide groups): Acid value = 11 mgKOH / g, Mw = 100,000 (manufactured by Toyo Chemical Co., Ltd.) P6: Polyacrylic acid resin (a thermosetting resin that does not possess ester, amide, amide, carbamate, or urea groups): Acid value = 17 mgKOH / g, Mw = 120,000 (manufactured by Toyo Chemical Co., Ltd.) P7: Polyolefin resin (a thermosetting resin that does not possess ester, amide, amide, carbamate, or urea groups): Acid value = 26 mgKOH / g, Mw = 85,000 (manufactured by Toyo Chemical Co., Ltd.) Hardener (H) H1: Bisphenol A type epoxy compound (jER834, molecular weight = 470, manufactured by Mitsubishi Chemical). Protective film (D) D1: A protective film made of 50 μm polyethylene terephthalate (PET) film that has undergone a matte treatment using sandblasting and is coated with a silicone release agent. D2: A protective film coated with silicone stripper after a 50 μm polyethylene naphthalate (PEN) film has undergone a matte treatment using sandblasting. D3: A protective film made of 38 μm polypropylene (PP) film that has undergone a matte finish treatment using sandblasting and is coated with a silicone release agent.
[0086] <Fabrication of Conductive Components and Conductive Sheets> [Example 1] 100 parts by weight of polyurethane amide resin (P5) as the thermosetting resin (b-2) and 225 parts by weight of dendritic metal powder (A1) as the metal powder (A) were placed in a container. 20 parts by weight of epoxy compound (H1) as the hardener (H) were added, along with methyl ethyl ketone (MEK) to bring the concentration of non-volatile components to 45% by weight, and the mixture was stirred for 10 minutes to prepare a conductive varnish.
[0087] Next, the prepared conductive composition varnish was applied to the peel-off surface (only one side) of the protective sheet (D1) with a thickness of 60 μm after drying using a scraper, and dried in an electric oven at 120°C for 2 minutes to obtain a conductive sheet (a laminate of protective sheet (D1) / conductive layer).
[0088] [Examples 2-27 and Comparative Examples 1-3] Except for setting the types and amounts of each component as shown in Tables 1 to 4, the same procedure as in Example 1 was followed to obtain conductive sheets for Examples 2 to 27 and Comparative Examples 1 to 3. Specifically, for Examples 16 to 21, Spd and Sdr were adjusted to desired values by drying in an electric oven followed by polishing the surface of the conductive components.
[0089] <Methods for confirming solubility> The following method was used to confirm whether the conductive component (conductive layer) dissolved in the solvent component (C) and whether the residue contained metal (solubility). The conductive sheet was cut into pieces 45 mm wide and 100 mm long, and the protective sheet (D) was peeled off. The obtained conductive component was immersed in 100 g of solvent component (C) at 30°C (containing monoethanolamine as a nitrogen-containing organic solvent (C1): 20% by mass, potassium hydroxide as a basic inorganic compound (C2): 15% by mass, and glycerol: 65% by mass). After 2 hours of ultrasonic treatment and standing for 22 hours, if the conductive component showed a finer shape compared to before immersion, it was considered "dissolved." The presence of metal in the insoluble components (residue) was then confirmed. If there was no change in shape compared to before immersion, it was considered "insoluble." Furthermore, if the shape change was not clearly visible to the naked eye, the mass of the sample before and after immersion was compared. A mass loss of less than 5% was considered "insoluble."
[0090] Whether the residue contains metals is determined by qualitative analysis using an inductively coupled plasma (ICP) luminescence spectrophotometer (AMETEK SPECTRO ARCOS (registered trademark): FHS12) on the residue. This analysis confirms the presence of metal elements, and if metal elements are present, the residue is deemed to contain metals.
[0091] <Methods for determining the density at the mountain peak (Spd) and the unfolded area ratio (Sdr)> The density Spd and the unfolded area ratio Sdr of the peak point of the conductive component (conductive layer) on the non-opposing surface with respect to the protective sheet (D) were determined using the following method. The surface of the conductive component was measured using a laser microscope (KEYENCE VK-X100). After acquiring the measurement data, the data was imported into analysis software (including the analysis application "VK-H1XA" of the ISO 25178-2:2012 surface property measurement module "VK-H1XR", both manufactured by KEYENCE), and the ISO 25178-2:2012 surface property measurement was performed. The conditions were set as follows: S-filter: 1 μm, L-filter: 0.2 mm.
[0092] <Determination of the highest value of the storage elasticity coefficient of conductive components (conductive layer) and protective sheet (D) at 0℃~30℃> The maximum values of the storage elasticity coefficients of the conductive component and the protective sheet (D) at 0°C to 30°C were determined by the following method. The thickness of the conductive layer was set to 60 μm, and the thickness of the protective sheet was set to the value stated in the raw material. First, prepare a test sample with a width of 5 mm and a length of 30 mm. Place the sample in a dynamic viscoelasticity measuring device (Dynamic Viscoelasticity Measuring Device DVA-200, manufactured by IT Measurement & Control Co., Ltd.) and perform dynamic viscoelasticity measurement under the conditions of heating rate: 10℃ / min, measurement frequency: 1 Hz, and strain: 0.08%. Read the stored elastic coefficient E' from the obtained dynamic viscoelasticity curve at 0℃~30℃ and calculate the highest value.
[0093] <Evaluation> For each of the obtained conductive components, the metal recyclability, adhesion, conductivity, anti-adhesion, peelability, immediacy, and reprocessability were evaluated according to the following methods. The evaluation results are shown in Table 5.
[0094] [Metal recyclability] Metal recyclability is evaluated by the ratio of the metal component (M1) remaining after the adhesive (B) is carbonized and decomposed by exposing the conductive component (conductive layer) to high temperature to carbonize the adhesive (B) and decompose it, to the residue (M2) obtained after the conductive component (conductive layer) is immersed in the solvent component (C) and decomposed. The conductive sheets prepared in each embodiment and comparative example were cut into sizes of 45 mm in width and 100 mm in length, and the protective sheet (D) was peeled off. The obtained conductive composition was placed in an electric furnace at 600°C for 10 hours, and the mass of the metal component (M1) was measured after removal. Similarly, the conductive sheet was cut into pieces 45 mm wide and 100 mm long, and the protective sheet (D) was peeled off. The obtained conductive composition was immersed in 100 g of solvent composition (C) at 30°C (containing monoethanolamine as a nitrogen-containing organic solvent (C1): 20% by mass, potassium hydroxide as a basic inorganic compound (C2): 15% by mass, and glycerol: 65% by mass). The mixture was then ultrasonically treated for 2 hours and allowed to stand for 22 hours to allow the residue to settle. Then, the solvent composition (C-1) of the supernatant was replaced with isopropanol, and the mixture was allowed to stand again for 5 hours. The supernatant was then removed, and the residue (M2) was air-dried for 3 days before its mass was measured. The value of M1 divided by M2 was calculated, and the metal recovery was evaluated according to the following criteria. +++: Excellent (M1 / M2 is above 0.95). ++: Excellent (M1 / M2 is above 0.80 but less than 0.95). +: Practical (M1 / M2 is 0.50 or higher but less than 0.80). NG: Not usable (M1 / M2 less than 0.50).
[0095] [Continue the force] The conductive sheets prepared in the various embodiments and comparative examples were cut into pieces 25 mm wide and 100 mm long. The conductive sheet was then overlapped onto a 30 mm wide and 150 mm long stainless steel (SUS) plate (with a 2 μm thick nickel layer formed on the surface of a commercially available SUS304 plate with a thickness of 0.2 mm) in contact with the exposed surface of the conductive composition (conductive layer). Subsequently, the conductive sheet and the SUS plate were rolled together using a roller laminator at 130°C, 3 kgf / cm², and 0.5 m / min. The protective sheet (D) was then peeled off, and a gold-plated copper foil (copper foil with a thickness of 25 μm that has undergone gold plating) was overlapped onto the exposed surface of the conductive composition. The conductive composition and the gold-plated copper foil were then rolled together using a roller laminator at 130°C, 3 kgf / cm², and 0.5 m / min to obtain a pre-pressed laminate. Then, the pre-pressed laminate was heated and pressed at 150°C and 2 MPa, and then left to stand (cured) at 180°C for 30 minutes to obtain the evaluation sample (SUS plate with conductive adhesive).
[0096] Subsequently, using a tensile testing machine (EZ-TEST, a small benchtop testing machine manufactured by Shimadzu Corporation), at a tensile speed of 50 mm / min, the adhesion strength of the conductive components of the evaluation specimen relative to the gold-plated surface was used as an indicator in a 90° peel test, and the adhesion was evaluated according to the following evaluation criteria. +++: Excellent (with a strength of 3 N / cm or higher). ++: Excellent (with a strength of 2 N / cm or more but less than 3 N / cm). +: Practical (with a strength of 1 N / cm or more but less than 2 N / cm). NG: Not practical (strength less than 1 N / cm).
[0097] [Electrical Conductivity] Using conductive sheets (20 mm wide and 20 mm long) prepared in the various embodiments and comparative examples, the conductive sheets are overlapped onto the SUS plate in such a manner that a 2 μm thick nickel layer is formed on the surface of a commercially available SUS304 plate with a width of 20 mm and a length of 20 mm, and the exposed surface of the conductive composition is in contact with the conductive composition. Then, the conductive sheets and the SUS plate are rolled together using a roll laminator at 90°C, 3 kgf / cm², and 1 m / min to obtain an SUS plate with conductive sheets.
[0098] Next, after peeling off the protective sheet (D) from the SUS board with the conductive sheet, it is punched into a square with one side of 10 mm using a punching machine. Then, an SUS board with conductive composition is obtained (hereinafter referred to as "SUS board with conductive composition"). Then, the exposed conductive composition surface of the SUS board with conductive composition (the non-facing surface of the conductive composition and the SUS board) is overlapped onto a separately manufactured wiring circuit board (flexible printed wiring board), and the SUS board with conductive composition and the flexible printed wiring board are bonded using a roller laminator at 130°C, 3 kgf / cm2, and 1 m / min. Then, these are heat-pressed at 170°C, 2 MPa, and 5 minutes, and then heated at 160°C for 60 minutes using an electric oven to obtain an evaluation sample. Furthermore, regarding the aforementioned wiring circuit substrate, copper foil circuits with a thickness of 32 μm are formed on both sides of a 75 μm thick polyimide film. An insulating cover film with an adhesive thickness of 37.5 μm, featuring a square shape with one side measuring 0.7 mm and an opening area of 0.49 mm², is deposited on the copper foil circuits. Additionally, an insulating cover film with an adhesive thickness of 37.5 μm without through-holes is deposited on another copper foil circuit (the copper foil circuits and cover films are symmetrically arranged relative to the polyimide film to prevent warping of the wiring circuit substrate).
[0099] Next, using a resistance meter and a BSP probe (model: MCP-TP05P, manufactured by Mitsubishi Chemical Analysis Technology), the resistance (connection resistance value) between the SUS plate and the copper foil circuit of the evaluation sample was measured. The conductivity was evaluated according to the following evaluation criteria based on this measured value. +++: Good (connection resistance value is less than 20 mΩ). ++: Practical (connection resistance value is 20 mΩ or higher but less than 100 mΩ). +: Applicable (connection resistance value is 100 mΩ or higher but less than 300 mΩ). NG: Not practical (connection resistance value is above 300 mΩ).
[0100] [Anti-adhesion] Two conductive sheets (50 mm wide and 50 mm long) prepared in each of the embodiments and comparative examples were prepared. The conductive sheets were then overlapped such that the exposed surface of the conductive component of one conductive sheet was in contact with the exposed surface of the protective sheet (D) of the other conductive sheet (i.e., the surface without release agent). After being weighed 2 kg, the sheets were allowed to stand at 40°C and atmospheric pressure for 3 days. Then, after removing the weight, the conductive sheets were pulled apart, and the area of the conductive component transferred to the protective sheet (D) was used as an indicator. The anti-adhesion properties were evaluated according to the following evaluation criteria. +++: Good (transfer area less than 5%). ++: Practical (transfer area is 5% or more but less than 10%). +: Practical (transfer area is 10% or more but less than 20%). NG: Not practical (transfer area is more than 20%).
[0101] [Easy to peel] The conductive sheets prepared in the various embodiments and comparative examples were cut into pieces 25 mm wide and 100 mm long. The conductive sheets were then overlapped onto a 30 mm wide and 150 mm long SUS plate (with a 2 μm thick nickel layer formed on the surface of a commercially available 0.2 mm thick SUS304 plate) with the exposed surface of the conductive composition in contact with the plate. Subsequently, the conductive sheets and the SUS plate were rolled together using a roll laminator at 130°C, 3 kgf / cm², and 0.5 m / min to obtain an evaluation sample.
[0102] Subsequently, using a tensile testing machine (EZ-TEST small benchtop testing machine, manufactured by Shimadzu Corporation), at a tensile speed of 50 mm / min, the peel strength of the protective sheet (D) of the evaluation specimen relative to the conductive component in the 90° peel test was used as an indicator, and the peelability was evaluated according to the following evaluation criteria. +++: Excellent (peel strength less than 50 g / 50 mm). ++: Excellent (peel strength is 50 g / 50 mm or more but less than 100 g / 50 mm). +: Applicable (peel strength of 100 g / 50 mm or more but less than 400 g / 50 mm). NG: Not applicable (peel strength above 400 g / 50 mm).
[0103] [Immediacy] The conductive sheets prepared in the various embodiments and comparative examples were cut into pieces 25 mm wide and 100 mm long, and left to stand in a freezer (-15°C) for 10 hours. Then, they were removed and left to stand in an environment of 23°C and 50%RH for 3 minutes. Next, the conductive sheet was overlapped onto a 30 mm wide and 150 mm long SUS plate (with a 2 μm thick nickel layer formed on the surface of a commercially available 0.2 mm thick SUS304 plate) with the exposed surface of the conductive composition (conductive layer) in contact with the plate. Then, using a roll laminator at 90°C, 3 kgf / cm², and 0.5 m / min, the conductive sheet and the SUS plate were roll-laminated. The protective sheet was then peeled off from the conductive sheet to obtain an SUS plate with a conductive layer.
[0104] Next, the gold-plated surface of an electroless gold-plated sheet (manufactured by Taiyo Industrial Co., Ltd.) cut to a width of 30 mm and a length of 200 mm was attached to the exposed conductive layer of an SUS board with a conductive layer, and roll-laminated under the same conditions as described above. Then, these were hot-pressed together at 170°C, 2 MPa, and 3 minutes respectively. Following this, they were heated in an electric oven at 160°C for 60 minutes to obtain evaluation samples. The areas where the conductive layer was present on the obtained evaluation samples were observed from the electroless gold-plated sheet side, and the degree of appearance defects (expansion caused by the evaporation of water droplets on the conductive layer) was graded from a to d (expansion evaluation). a: The area of expansion is more than 5% but less than 10% relative to the area of the conductive layer. b: The area of expansion is more than 10% but less than 15% relative to the area of the conductive layer. c: The area of expansion is more than 15% but less than 20% relative to the area of the conductive layer. d: The area of expansion is less than 5% relative to the area of the conductive layer.
[0105] For the evaluation samples obtained above, a tensile testing machine (small benchtop testing machine EZ-TEST, manufactured by Shimadzu Corporation) was used. The part of the sample without the SUS plate attached was installed in the tensile testing machine. Under the condition of tensile speed of 50 mm / min, the adhesion strength of the conductive layer of the evaluation sample relative to the electroless gold-plated surface in the 180° peel test was measured. The results were graded from a to d (adhesion strength). a: The strength is then above 6 N / cm. b: The strength is above 3 N / cm but less than 6 N / cm. c: The strength is above 1 N / cm but less than 3 N / cm. d: The strength is less than 1 N / cm.
[0106] Furthermore, the respective results are used as indicators to evaluate adhesion according to the following evaluation criteria. +++: Both expansion rating and adhesion strength are 'a' (excellent). ++: Expansion evaluation, adhesion strength, either a and the other b, or both b (excellent). +: Expansion evaluation, followed by strength, either is c and there is no d (practical). NG: Either or both of the expansion rating and adhesion strength are d (not practical).
[0107] [Reprocessability] Reprocessability was evaluated by the area of residual conductive layer and the arithmetic mean height of the conductive layer after peeling off the temporary adhesive layer from the polyimide. The exposed conductive layer of a conductive sheet cut to a width of 50 mm and a length of 50 mm was bonded to a polyimide film (Kapton 300H) cut to a width of 70 mm and a length of 70 mm. Temporary bonding was performed by passing the film through a roller laminator (transport speed: 1 m / min, temperature: 90°C, pressure: 3 kgf / cm²). The conductive layer in the resulting temporary adhesive laminate was peeled off from the end, and the area of the residual conductive layer on the polyimide was divided by the area of the conductive layer before bonding to calculate the residual paste rate. Subsequently, five arbitrary points were selected from the paste residue area, and the surface was measured using a laser microscope (KEYENCE VK-X100). The acquired measurement data were then imported into analysis software (including the analysis application "VK-H1XA" of the ISO 25178 surface property measurement module "VK-H1XR", both manufactured by KEYENCE), and ISO 25178 surface property measurements were performed to calculate the arithmetic mean height (conditions set as S-filter: 1 μm, L-filter: 0.2 mm). The obtained paste residue rate and arithmetic mean height were used for evaluation according to the following criteria. +++: When the paste residue rate is below 5% and there is some paste residue, its arithmetic mean height is less than 20% of the adhesive layer thickness. Extremely good. ++: The paste residue rate is between 5% and 15%, and its arithmetic mean height is less than 20% of the adhesive layer thickness. Good. +: The paste residue rate is below 15%, and the arithmetic mean height of the paste residue is 20%~50% of the adhesive layer thickness. Practical. NG: Paste residue rate greater than 15%, and / or the arithmetic mean height of the paste residue is greater than 50% of the adhesive layer thickness. Not suitable for practical use.
[0108] [Table 1] Example 1 2 3 4 5 6 7 conductive sheet electrical conductivity Composition Adhesive (B) thermosetting properties Resin (b-2) P5 P1 P2 P3 P4 P6 P5 100 100 100 100 100 100 100 hardener (H) H1 H1 H1 H1 H1 H1 H1 20 20 20 20 20 20 20 Metal powder (A) type A1 A1 A1 A1 A1 A1 A1 quantity 225 225 225 225 225 225 65 Particle size [μm,D 50] 5.7 5.7 5.7 5.7 5.7 5.7 5.7 Particle size [μm,D 10] 2.1 2.1 2.1 2.1 2.1 2.1 2.1 Particle size [μm,D 90] 12.8 12.8 12.8 12.8 12.8 12.8 12.8 D 90 / D 10 6.1 6.1 6.1 6.1 6.1 6.1 6.1 type - - - - - - - quantity 0 0 0 0 0 0 0 Particle size [μm,D 50] - - - - - - - Particle size [μm,D 10] - - - - - - - Particle size [μm,D 90] - - - - - - - D 90 / D 10 - - - - - - - content [quality%] 65% 65% 65% 65% 65% 65% 35% 0℃~30℃ Storage elasticity coefficient Maximum value (2) [GPa] 2.2 3 2.9 2.7 2.1 2.5 2.2 Sdr 0.62 0.62 0.62 0.62 0.62 0.62 0.25 Spd [pieces / mm 2] 76,000 76,000 76,000 76,000 76,000 76,000 2,300 Protect Film (D) type D1 D1 D1 D1 D1 D1 D1 0℃~30℃ Storage elasticity coefficient Maximum value (1) [GPa] 3 3 3 3 3 3 3 α 0.7 1.0 1.0 0.9 0.7 0.8 0.7 Porosity [%] 6.0 6.0 6.0 6.0 6.0 6.0 0.8 Does the residue contain metals (soluble)? Include Include Include Include Include Include Include
[0109] [Table 2] Example 8 9 10 11 12 13 14 conductive sheet electrical conductivity Composition Adhesive (B) thermosetting properties Resin (b-2) P5 P5 P5 P5 P5 P5 P5 100 100 100 100 100 100 100 Hardener (H) H1 H1 H1 H1 H1 H1 H1 20 20 20 20 20 20 20 Metal powder (A) type A1 A1 A1 A2 A3 A4 - quantity 90 550 1300 225 225 225 0 Particle size [μm,D 50] 5.7 5.7 5.7 31.2 10.8 7.5 - Particle size [μm,D 10] 2.1 2.1 2.1 12.9 3.2 1.5 - Particle size [μm,D 90] 12.8 12.8 12.8 44.6 29.5 11.3 - D 90 / D 10 6.1 6.1 6.1 3.5 9.2 7.5 - type - - - - - - A5 quantity 0 0 0 0 0 0 225 Particle size [μm,D 50] - - - - - - 11.3 Particle size [μm,D 10] - - - - - - 3.8 Particle size [μm,D 90] - - - - - - 29.5 D 90 / D 10 - - - - - - 7.8 content [quality%] 43% 82% 92% 65% 65% 65% 65% 0℃~30℃ Storage elasticity coefficient Maximum value (2) [GPa] 2.2 2.2 2.2 2.2 2.2 2.2 2.2 Sdr 0.30 1.40 2.40 2.70 0.43 0.52 0.37 Spd [pieces / mm 2] 9,800 265,000 489,000 57,000 32,000 44,000 21,000 Protect Film (D) type D1 D1 D1 D1 D1 D1 D1 0℃~30℃ Storage elasticity coefficient Maximum value (1) [GPa] 3 3 3 3 3 3 3 α 0.7 0.7 0.7 0.7 0.7 0.7 0.7 Porosity [%] 1.2 28.0 58.0 19.0 0.4 0.3 0.2 Does the residue contain metals (soluble)? Include Include Include Include Include Include Include
[0110] [Table 3] Example 15 16 17 18 19 20 twenty one conductive sheet electrical conductivity Composition Adhesive (B) thermosetting properties Resin (b-2) P5 P5 P5 P5 P5 P5 P5 100 100 100 100 100 100 100 Hardener (H) H1 H1 H1 H1 H1 H1 H1 20 20 20 20 20 1 2 Metal powder (A) type A1 A1 A1 A1 A1 A1 A1 quantity 170 225 225 225 225 185 190 Particle size [μm,D 50] 5.7 5.7 5.7 5.7 5.7 5.7 5.7 Particle size [μm,D 10] 2.1 2.1 2.1 2.1 2.1 2.1 2.1 Particle size [μm,D 90] 12.8 12.8 12.8 12.8 12.8 12.8 12.8 D 90 / D 10 6.1 6.1 6.1 6.1 6.1 6.1 6.1 type A5 - - - - - - quantity 55 0 0 0 0 0 0 Particle size [μm,D 50] 11.3 - - - - - - Particle size [μm,D 10] 3.8 - - - - - - Particle size [μm,D 90] 29.5 - - - - - - D 90 / D 10 7.8 - - - - - - content [quality%] 65% 65% 65% 65% 65% 65% 65% 0℃~30℃ Storage elasticity coefficient Maximum value (2) [GPa] 2.2 2.2 2.2 2.2 2.2 0.02 0.13 Sdr 0.51 0.005 0.05 3.50 4.20 0.62 0.62 Spd [pieces / mm 2] 64,000 1,100 10,500 320,000 400,000 76,000 76,000 Protect Film (D) type D1 D1 D1 D1 D1 D1 D1 0℃~30℃ Storage elasticity coefficient Maximum value (1) [GPa] 3 3 3 3 3 3 3 α 0.7 0.7 0.7 0.7 0.7 0.01 0.04 Porosity [%] 3.5 6.0 6.0 6.0 6.0 6.0 6.0 Does the residue contain metals (soluble)? Include Include Include Include Include Include Include
[0111] [Table 4] Example Comparative example twenty two twenty three twenty four 25 26 27 1 2 3 conductive sheet electrical conductivity Composition Adhesive (B) thermosetting properties Resin (b-2) P5 P5 P5 P5 P5 P5 P7 P5 P5 100 100 100 100 100 100 100 100 100 hardener (H) H1 H1 H1 H1 H1 H1 H1 H1 H1 10 32 51 72 20 20 20 20 20 Metal powder (A) type A1 A1 A1 A1 A1 A1 A1 A1 A1 quantity 200 250 280 315 225 225 225 52 2500 Particle size [μm,D 50] 5.7 5.7 5.7 5.7 5.7 5.7 5.7 5.7 5.7 Particle size [μm,D 10] 2.1 2.1 2.1 2.1 2.1 2.1 2.1 2.1 2.1 Particle size [μm,D 90] 12.8 12.8 12.8 12.8 12.8 12.8 12.8 12.8 12.8 D 90 / D 10 6.1 6.1 6.1 6.1 6.1 6.1 6.1 6.1 6.1 type - - - - - - - - - quantity 0 0 0 0 0 0 0 0 0 Particle size [μm,D 50] - - - - - - - - - Particle size [μm,D 10] - - - - - - - - - Particle size [μm,D 90] - - - - - - - - - D 90 / D 10 - - - - - - - - - content [quality%] 65% 65% 65% 65% 65% 65% 65% 30% 95% 0℃~30℃ Storage elasticity coefficient Maximum value (2) [GPa] 1.1 15 43 101 2.20 2.20 1.9 2.2 2.2 Sdr 0.62 0.62 0.62 0.62 0.62 0.62 0.62 0.09 2.70 Spd [pieces / mm 2] 76,000 76,000 76,000 76,000 76,000 76,000 76,000 800 513,000 Protect Film (D) type D1 D1 D1 D1 D2 D3 D1 D1 D1 0℃~30℃ Storage elasticity coefficient Maximum value (1) [GPa] 3 3 3 3 5 0.008 3 3 3 α 0.4 5.0 14.3 33.7 0.4 275.0 0.6 0.7 0.7 Porosity [%] 6.0 6.0 6.0 6.0 6.0 6.0 6.0 0.4 68.0 Does the residue contain metals (soluble)? Include Include Include Include Include Include Insoluble Include Include
[0112] [Table 5] Example Comparative example 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 twenty one twenty two twenty three twenty four 25 26 27 1 2 3 evaluate Metal recyclability +++ ++ +++ +++ +++ + + ++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ ++ ++ + +++ +++ NG + +++ Then force +++ ++ ++ ++ ++ +++ +++ +++ ++ + ++ +++ +++ +++ +++ +++ +++ ++ + +++ +++ +++ +++ +++ +++ +++ +++ ++ +++ + electrical conductivity +++ +++ +++ +++ +++ + + ++ +++ +++ +++ ++ ++ +++ +++ +++ +++ +++ + +++ +++ +++ +++ +++ +++ +++ +++ + + +++ Anti-adhesion +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ + ++ +++ +++ + ++ +++ +++ +++ +++ +++ +++ +++ ++ +++ Easy to peel +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ + +++ + +++ +++ +++ Immediacy +++ +++ +++ +++ +++ +++ ++ +++ +++ ++ ++ ++ ++ ++ +++ + ++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ +++ + + Reprocessing +++ +++ +++ +++ +++ +++ + ++ ++ + +++ +++ +++ ++ +++ + ++ ++ + +++ +++ +++ +++ +++ +++ +++ +++ +++ NG NG
[0113] Comparative Example 1, which is insoluble in the solvent composition (C), has issues regarding metal recyclability. Furthermore, Comparative Examples 2 and 3, which have Spd values outside the range of 1000 to 500,000, have issues regarding reprocessability. In contrast, the conductive sheets of Examples 1 to 27, which have a conductive layer having a Spd value in the range of 1,000 particles / mm² to 500,000 particles / mm², are soluble in the solvent composition (C), and whose residue contains metal elements, demonstrate excellent metal recyclability, adhesion, conductivity, anti-adhesion, easy peeling, immediacy, and reprocessability.
[0114] none
Claims
1. A conductive sheet having a conductive composition comprising metal powder (A) and an adhesive (B) disposed on a main surface of a protective sheet (D), wherein the conductive composition dissolves and leaves residue after being immersed in a solvent composition (C) at 30°C for 24 hours, the residue comprising a metal element, and the peak density Spd of the surface of the conductive composition on the non-opposite side of the protective sheet (D) is 1,000 to 500,000 per mm², wherein the solvent composition (C) comprises 5% to 40% by mass of a nitrogen-containing organic solvent (C1) relative to the total mass of the solvent composition (C), and 5% to 40% by mass of an alkaline inorganic compound (C2) relative to the total mass of the solvent composition (C), wherein the conductive composition has porosity of 1.0% to 30%.
2. The conductive sheet as claimed in claim 1, wherein, The conductive component has adhesive properties.
3. The conductive sheet as described in claim 1 or 2, wherein, The adhesive (B) has one or more groups selected from the group consisting of ester group, amide group, amide group, carbamate group and urea group.
4. The conductive sheet as described in claim 1 or 2, wherein, The adhesive (B) has two or more groups selected from the group consisting of ester, amide, amide, carbamate and urea.
5. The conductive sheet as described in claim 1 or 2, wherein, The surface area ratio Sdr of the conductive component that is on the non-opposite side to the protective sheet (D) is 0.01 to 4.
6. The conductive sheet as claimed in claim 1 or 2, wherein, The highest value (2) of the storage elastic coefficient of the conductive component at 0℃~30℃ is 0.01 GPa~100 GPa, and the value α obtained by dividing the highest value (2) by the highest value (1) of the storage elastic coefficient of the protective sheet (D) at 0℃~30℃ is 0.01~30.
7. The conductive sheet as claimed in claim 1 or 2, wherein, The maximum storage elasticity coefficient of the protective sheet (D) at 0℃~30℃ is 0.01 GPa~1000 GPa.
8. A terminal block comprising a metal plate, a conductive component obtained by peeling off a protective sheet (D) of a conductive sheet as described in any one of claims 1 to 7, and a terminal block substrate, wherein the metal plate is fixed to the terminal block substrate via the conductive component.
9. An electronic device comprising a terminal block as described in claim 8.
Citation Information
Patent Citations
Conductive adhesive sheet, electromagnetic wave shield sheet and printed wiring board
JP2015185717A