A polarizing plate with a hard coating and an image display device comprising the polarizing plate with the hard coating.
Patent Information
- Application Number
- TW110131489
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-25
- Filing Date
- 2021-08-25
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-08-24
AI Technical Summary
Polarizing plates with hard coat layers in image display devices are prone to damage and cracking in non-rectangular shapes, particularly in special-shaped processed portions.
A polarizing plate design with a protective layer, intermediate layer, and hard coating sequence, where the intermediate layer has a thickness of 0.1 μm to 8 μm and a shear failure strength of 10 MPa or more, forming a compatible region between the protective and hard coat layers to enhance durability.
Significantly suppresses damage and cracks in the hard-coated parts of the special-shaped processed portions, ensuring improved adhesion durability and scratch resistance.
Smart Images

Figure TWG2TB001919879_001 
Figure TWG2TB001919879_002 
Figure TWG2TB001919879_003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a polarizing plate with a hard coating and an image display device comprising the polarizing plate with the hard coating. [Previous Technology]
[0002] Polarizing plates are widely used in image display devices such as mobile phones and laptops to achieve image display and / or improve the performance of such image display. When the surface of an image display device is damaged due to external contact, the visibility of the displayed image may decrease. Therefore, in order to protect the surface of the image display device, there are cases where a polarizing plate with a hard coating is formed on the surface side (visibility side) (a polarizing plate with a hard coating) is used. In recent years, there has been a desire to process optical thin films into shapes other than rectangles (irregular processing: for example, forming notches and / or through holes). However, with the irregular processing part of a polarizing plate with a hard coating, there is a problem that the hard coating is prone to damage and / or cracking. Previous Art Documents Patent Documents
[0003] Patent Document 1: Japanese Patent Application Publication No. 2012-234163 [Summary of the Invention]
[0004] Problem to be solved by the invention The present invention was made to solve the above-mentioned prior art problems. Its main objective is to provide an optical film with a hard coating that significantly suppresses damage and cracks of the hard coating in irregularly shaped processing parts.
[0005] Means for Solving the Problem An embodiment of the present invention comprises a polarizing plate with a hard coating, which sequentially includes a polarizing element, a protective layer, an intermediate layer with a thickness of 0.1µm to 8µm, and a hard coating, and has an irregular shape other than a rectangle; and the intermediate layer has a shear strength of 10MPa or more per 1µm thickness. In one embodiment, the intermediate layer includes a region in which the components of the hard coating and the protective layer are compatible. In one embodiment, the thickness of the intermediate layer is 0.3µm to 5µm. In one embodiment, the shear strength of the intermediate layer is 14MPa or more per 1µm thickness. In one embodiment, the thickness of the hard coating is 5µm or less. In one embodiment, the protective layer is composed of a cellulose triacetate film. In one embodiment, the aforementioned irregular shape is selected from the group consisting of: through holes, V-shaped notches, U-shaped notches, recesses that are approximately boat-shaped when viewed from above, rectangular recesses that are rectangular when viewed from above, R-shaped recesses that are approximately bathtub-shaped when viewed from above, and combinations thereof. According to another aspect of the invention, an image display device is provided. This image display device includes the aforementioned polarizing plate with a hard coating on the viewing side.
[0006] Effects of the Invention According to an embodiment of the present invention, in a polarizing plate with a hard coating having an irregular shape (irregular processing section) other than a rectangle, an intermediate layer representing a region of compatibility is formed between the protective layer and the hard coating, and the thickness of the intermediate layer and the shear failure strength per unit thickness are optimized, thereby realizing a polarizing plate with a hard coating that significantly suppresses damage and cracks of the hard coating in the irregular processing section.
Implementation Method
[0008] The following description refers to specific embodiments of the present invention with reference to the drawings, but the present invention is not limited to these embodiments. In addition, the drawings are shown schematically for ease of viewing, and the proportions such as length, width, and thickness, as well as the angles in the drawings, are different from the actual figures.
[0009] In this specification, "hard coating layer" can be used as a general term for hard surface treatment layers with surface protection functions. Therefore, hard coating layer not only includes general hard coating layers, but may also include anti-reflective layers, anti-sticking layers, anti-glare layers, and anti-adhesion layers.
[0010] A. Schematic diagram of a polarizing plate with a hard coating. Figure 1 is a schematic cross-sectional view of a polarizing plate with a hard coating according to an embodiment of the present invention. The polarizing plate 100 with a hard coating in the figure sequentially includes a polarizing element 10, a protective layer 20, an intermediate layer 30, and a hard coating 40. The intermediate layer 30 represents the region on which the components of the hard coating 40 and the components of the protective layer 20 are compatible. In the embodiment of the present invention, the thickness of the intermediate layer is 0.1µm to 8µm, and the shear breaking strength per 1µm thickness of the intermediate layer is 10MPa or more. According to the embodiment of the present invention, in a polarizing plate with a hard coating having an irregular shape (irregular processing section) other than a rectangle, an intermediate layer is formed between the protective layer and the hard coating, and the thickness of the intermediate layer and the shear breaking strength per unit thickness are within the range described above, thereby significantly suppressing the damage and cracking of the hard coating in the irregular processing section. Shear failure strength is the force required to cut (break) the layers of a single film or laminate, and can be calculated, for example, using a SAICAS (Surface and Interfacial Cutting Analysis System). The specific procedure for calculating shear failure strength is illustrated in Figure 2. Figure 2 shows a laminate with a hard coating, intermediate layer, and protective layer arranged sequentially from top to bottom. The shear strength obtained by obliquely cutting this laminate using a precision oblique cutting device (e.g., DAIPLA WINTES CO., LTD., "SAICAS DN-20") is the shear failure strength. Oblique cutting can be performed by making the cutter move in both horizontal and vertical directions. The shear failure strength T (MPa) can be calculated using the following formula. T(MPa) = FH(kN) / (2 × Wd(m2) × cotφ) Here, FH is the horizontal load caused by the cutter, W is the width of the cutter (m), d is the vertical displacement of the cutter (m), and φ is the shear angle. Furthermore, the shear angle can vary depending on cutting conditions and the material of the object being cut, but is approximately 45°. In addition, the thickness of the interlayer is substantially proportional to the shear failure strength; therefore, the shear failure strength per 1µm of interlayer thickness can be calculated. For example, when measuring the shear failure strength of an interlayer with a thickness of 0.5µm, the measured value can be doubled; while when measuring the shear failure strength of an interlayer with a thickness of 2.0µm, the measured value can be half-doubled.
[0011] In this embodiment of the invention, the polarizing plate with a hard coating has an irregular shape other than a rectangle. In this specification, "having an irregular shape other than a rectangle" means that the top view shape of the polarizing plate with a hard coating has a shape other than a rectangle (including rectangles and cases where corners are cut off). "Irregular shape" refers to an irregularly shaped processing section. Therefore, "a polarizing plate with a hard coating having an irregular shape other than a rectangle" (hereinafter sometimes referred to as "irregularly shaped polarizing plate") includes not only cases where the entire irregularly shaped polarizing plate (i.e., the outer edge used to define the top view shape of the polarizing plate) is other than a rectangle, but also cases where an irregularly shaped processing section is formed in the portion that recedes inward from the outer edge of the rectangular polarizing plate. In the case of a polarizing plate with a hard coating, damage and / or cracks of the hard coating are prone to occur in the irregularly shaped processing section, but according to this embodiment of the invention, such damage and cracks can be significantly suppressed. As shown in Figures 3 and 4, irregularly shaped (machined) parts can include through holes and machined parts that appear as concave portions when viewed from above. Representative examples of concave portions include shapes resembling a boat, rectangles, R-shapes resembling a bathtub, V-shaped notches, and U-shaped notches. Another example of an irregularly shaped (machined) part is shown in Figures 5 and 6, which corresponds to the shape of a car dashboard. This shape has an outer edge that forms an arc along the direction of rotation of the instrument needle, and includes a portion with an outer edge that forms a V-shape (including an R-shape) that convexes inward in the direction of the surface. Of course, the shape of irregularly shaped (machined) parts is not limited to the examples shown in the figures. For example, the shape of a through hole can be any suitable shape (e.g., ellipse, triangle, square, pentagon, hexagon, octagon) in addition to the approximately circular shape shown in the examples, depending on the purpose. Furthermore, the through hole can be located in any suitable position depending on the purpose. The through-hole can be provided at approximately the center of the long side end of the rectangular polarizing plate, as shown in Figure 4; it can be provided at a predetermined position at the long side end; or it can be provided at the corner of the polarizing plate. Although not shown, it can be provided at the short side end of the rectangular polarizing plate; or it can be provided at the center of the irregularly shaped polarizing plate, as shown in Figure 5 or Figure 6. As shown in Figure 4, multiple through-holes can also be provided. Furthermore, the shapes of the examples can be appropriately combined depending on the purpose. For example, through-holes can be formed at any position on the irregularly shaped polarizing plate in Figure 3; or V-shaped notches and / or U-shaped notches can be formed at any appropriate position on the outer edge of the irregularly shaped polarizing plate in Figure 5 or Figure 6. The irregularly shaped polarizing plate is suitable for use in image display devices such as automotive dashboards, smartphones, tablet PCs, or smartwatches. Furthermore, when the irregular shape includes an R-shape, its radius of curvature is, for example, 0.2 mm or more, or, for example, 1 mm or more, or, for example, 2 mm or more. On the other hand, the radius of curvature is, for example, 10 mm or less, or, for example, 5 mm or less.
[0012] In a polarizing plate with a hard coating, another protective layer (not shown) may be disposed on the side opposite to the protective layer 20 of the polarizing element 10, depending on the requirements. Furthermore, for convenience, the protective layer 20 is sometimes referred to as the outer protective layer, and the other protective layer as the inner protective layer. In addition, in a polarizing plate with a hard coating, any suitable functional layer may be disposed on the side opposite to the protective layer 20 of the polarizing element 10 (or, when another protective layer is present, the other protective layer is opposite to the polarizing element). Representative examples of functional layers include a phase retardation layer and a conductive layer. The type, quantity, and combination of functional layers can be appropriately set according to the purpose. For example, the optical characteristics (e.g., refractive index characteristics, in-plane phase difference, Nz coefficient, photoelastic coefficient), thickness, and placement position of the phase retardation layer can be appropriately set according to the purpose.
[0013] In practical use, an adhesive layer (not shown) can be provided as the outermost layer of the polarizing plate with a hard coating, opposite to the hard coating, so that the polarizing plate with the hard coating can be attached to the image display unit. Furthermore, before the polarizing plate with the hard coating is put into use, a release film should be temporarily attached to the surface of the adhesive layer. By temporarily attaching the release film, the roll of the polarizing plate with the hard coating can be formed while protecting the adhesive layer.
[0014] The following provides a more detailed description of the constituent elements of a polarizing plate with a hard coating.
[0015] B. Polarizing element A polarizing element is represented as being constructed of a resin film containing a dichroic substance. Regarding the resin film, any suitable resin film suitable for use as a polarizing element may be used. A representative resin film is a polyvinyl alcohol-based resin (hereinafter referred to as "PVA-based resin") film. The resin film may be a single-layer resin film or a laminate of two or more layers.
[0016] A specific example of a polarizing element composed of a single-layer resin film may be a PVA-based resin film that has undergone iodine dyeing and stretching treatment (represented by uniaxial stretching). The aforementioned iodine dyeing can be performed, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. Stretching can be performed after dyeing or during dyeing. Alternatively, stretching can be performed before dyeing. Depending on the requirements, the PVA-based resin film may undergo swelling treatment, crosslinking treatment, washing treatment, drying treatment, etc. For example, immersing the PVA-based resin film in water for washing before dyeing not only removes dirt or anti-adhesive agents from the surface of the PVA-based film but also causes the PVA-based resin film to swell, thereby preventing uneven dyeing.
[0017] Specific examples of polarizing elements obtained using a laminate include a laminate consisting of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizing element obtained using a resin substrate and a laminate coated with a PVA-based resin layer formed on the resin substrate. A polarizing element obtained using a resin substrate and a laminate coated with a PVA-based resin layer formed on the resin substrate can be manufactured, for example, by the following steps: coating a PVA-based resin solution onto a resin substrate and drying it to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer; and extending and dyeing the laminate to form a polarizing element from the PVA-based resin layer. In this embodiment, extending typically includes immersing the laminate in an aqueous boric acid solution and extending it. Furthermore, if necessary, extending may further include air-stretching the laminate at a high temperature (e.g., above 95°C) before extending it in the aqueous boric acid solution. The resulting resin substrate / polarizing element laminate can be used directly (i.e., the resin substrate can also be used as a protective layer for the polarizing element), or the resin substrate can be peeled off from the resin substrate / polarizing element laminate and then used with any suitable protective layer that meets the purpose of the peeled area. Detailed descriptions of the manufacturing method of the polarizing element are provided, for example, in Japanese Patent Application Publication No. 2012-73580 and Japanese Patent No. 6470455. The entire contents of these publications are incorporated herein by reference.
[0018] The thickness of the polarizing element should preferably be less than 25µm, more preferably 1µm to 12µm, even more preferably 3µm to 12µm, and especially preferably 3µm to 8µm. If the thickness of the polarizing element is within the above range, curling during heating can be well suppressed, and good appearance durability during heating can be obtained.
[0019] The polarizing element should preferably exhibit absorption dichroism at any wavelength between 380 nm and 780 nm. The transmittance of the polarizing element is, for example, 41.5% to 46.0%, preferably 43.0% to 46.0%, and more preferably 44.5% to 46.0%. The polarization degree of the polarizing element is preferably above 97.0%, more preferably above 99.0%, and even more preferably above 99.9%.
[0020] C. Both the outer and inner protective layers (sometimes collectively referred to as protective layers) are formed of any suitable thin film that can be used as a protective layer for a polarizing element. Specific examples of materials that form the main component of the thin film include cellulose resins such as cellulose triacetate (TAC), or transparent resins such as polyester, polyvinyl alcohol, polycarbonate, polyamide, polyimide, polyether ether, polyether ether, polystyrene, polynorbornene, polyolefin, (meth)acrylic acid, and acetate. Also, thermosetting or UV-curing resins such as (meth)acrylic acid, carbamate, (meth)acrylate carbamate, epoxy, and polysiloxane are also examples. Other examples include glassy polymers such as silicate polymers. Alternatively, the polymer film described in Japanese Patent Application Publication No. 2001-343529 (WO01 / 37007) may also be used. As a material for this film, for example, a resin composition containing a thermoplastic resin having substituted or unsubstituted amide groups on the side chains and a thermoplastic resin having substituted or unsubstituted phenyl and nitrile groups on the side chains can be used. Examples include a resin composition comprising an alternating copolymer of isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer. The polymer film may, for example, be an extruded product of the aforementioned resin composition.
[0021] The outer protective layer is preferably made of cellulose triacetate (TAC) film or acrylic resin film, and more preferably of TAC film. By making the outer protective layer of the aforementioned film, an intermediate layer with the desired thickness and shear strength can be well formed.
[0022] In one embodiment, the inner protective layer (when present) is preferably optically isotropic. In this specification, "optically isotropic" means that the in-plane phase difference Re(550) is 0 nm to 10 nm, and the phase difference Rth(550) in the thickness direction is -10 nm to +10 nm. In another embodiment, the inner protective layer may also be a phase difference film, a brightness enhancement film, a diffusion film, etc.
[0023] The thickness of the protective layer can be any appropriate thickness. The thickness of the protective layer should preferably be 5µm~200µm, 15µm~45µm is better, and 20µm~40µm is even better.
[0024] D. Hard Coating The hard coating preferably has a pencil hardness of H or higher, more preferably 2H or higher, and even more preferably 3H or higher. On the other hand, the pencil hardness of the hard coating is preferably 6H or lower, and more preferably 5H or lower. If the pencil hardness of the hard coating is within the above range, excellent surface protection properties can be imparted when the polarizing plate with the hard coating is applied to an image display device. The pencil hardness can be determined according to the "Pencil Hardness Test" of JIS K 5400.
[0025] The thickness of the hard coating is preferably less than 5µm, more preferably 0.5µm to 4µm, and even more preferably 1µm to 3.5µm. Excellent scratch resistance can be achieved when the thickness of the hard coating is within the specified range. Furthermore, by appropriately selecting the materials of the hard coating and the protective layer, an intermediate layer with the desired thickness and shear strength can be well formed.
[0026] The hard coating can be made of any suitable material as long as the effects of the embodiments of the present invention can be obtained. For example, the hard coating can be a hardened layer of a thermosetting resin or a resin that cures under ionizing radiation (e.g., visible light, ultraviolet light). Ultraviolet-curable resins are preferred because they allow for easy operation and high-efficiency formation of the hard coating. Specific examples of ultraviolet-curable resins include polyester-based, (meth)acrylate-based, urethane-based, amide-based, polysiloxane-based, epoxy-based, and unsaturated polyester-based ultraviolet-curable resins. (Meth)acrylate-based ultraviolet-curable resins include urethane (meth)acrylate, polyester (meth)acrylate, and epoxy (meth)acrylate. Ultraviolet-curable resins may contain ultraviolet-curable monomers, oligomers, or polymers. Ideally, an ultraviolet-curable resin composition may be included that contains acrylic monomer components or oligomer components, and these acrylic monomer components or oligomer components preferably have two or more, more preferably three to six, ultraviolet-polymerizable functional groups. In contrast, UV-curable resins contain photopolymerization initiators.
[0027] The hard coating can be formed by any suitable method. The hard coating is preferably formed by applying a hard coating forming resin composition to the protective layer and allowing it to dry, then irradiating the dried coating film with ultraviolet light to harden it. An intermediate layer can be well formed by directly applying the hard coating forming resin composition to the protective layer.
[0028] Details of the hard coating are described in, for example, Japanese Patent Application Publication No. 2011-237789 and Japanese Patent Application Publication No. 2016-224443. The descriptions in these publications are incorporated herein by reference.
[0029] E. Intermediate Layer The intermediate layer represents the incompatible region, as described above, containing the components of the hard coating and the protective layer. In other words, the intermediate layer is a permeation layer formed by the hard coating components (essentially components for forming the hard coating) penetrating into the protective layer. By forming the intermediate layer, the protective layer and the hard coating can adhere firmly through the intermediate layer, significantly suppressing damage, cracking, and peeling of the hard coating. In the intermediate layer, the concentration of the protective layer components preferably increases continuously from the hard coating side to the protective layer side. This continuous change in the concentration of the protective layer components prevents the formation of interfaces within the intermediate layer due to concentration variations. As a result, interface reflection within the intermediate layer can be suppressed, resulting in a polarizing plate with minimal interference unevenness and a hard coating. Preferably, the concentration of the protective layer components increases continuously from the hard coating to the intermediate layer, and also continuously from the intermediate layer to the protective layer. That is, it is preferable not to form a clear interface between the hard coating and the intermediate layer, or a clear interface between the intermediate layer and the protective layer. If the above configuration is adopted, a polarizing plate with a hard coating can be obtained with less interference unevenness.
[0030] The thickness of the intermediate layer is as described above, ranging from 0.1µm to 8µm, preferably from 0.3µm to 7.7µm, more preferably from 1.0µm to 7.5µm, and especially preferably from 1.2µm to 7.5µm. Furthermore, the thickness of the intermediate layer can be less than 5.0µm, less than 2.0µm, or less than 1.5µm. If the thickness of the intermediate layer is greater than 8µm, it may not be sufficient to suppress damage and / or cracking of the hard coating in the irregularly shaped processing section. If the thickness of the intermediate layer is less than 0.1µm, the hard coating may peel off under high temperature and high humidity conditions.
[0031] The shear strength per 1µm thickness of the intermediate layer is 10MPa or more, preferably 14MPa or more, as described above. For example, the shear strength per 1µm thickness of the intermediate layer can be 16MPa or more, or 20MPa or more, or 25MPa or more, or 40MPa or more, or 70MPa or more, or 100MPa or more, or 120MPa or more. For example, the shear strength per 1µm thickness of the intermediate layer can be 200MPa or less. If the shear strength per 1µm thickness of the intermediate layer is within the above range, damage and / or cracking of the hard coating in the irregularly shaped processing section can be significantly suppressed.
[0032] The thickness and shear failure strength of the intermediate layer can be adjusted by appropriately combining and setting the following conditions: the constituent materials and surface properties of the substrate (which will eventually become the protective layer) when forming the hard coating, the constituent materials of the hard coating, the composition of the components used to form the hard coating (e.g., the concentration of solid components, solvent composition, or the type, quantity or amount of additives), and the formation conditions of the hard coating (e.g., the drying or heating conditions of the coating film, the amount or method of ultraviolet irradiation).
[0033] F. Image Display Device The polarizing plate with a hard coating according to the embodiments of the present invention, as described above, is suitable for use in image display devices. Therefore, image display devices including polarizing plates with hard coatings are also included in the embodiments of the present invention. An image display device typically includes an image display unit and a polarizing plate with a hard coating bonded to the image display unit through an adhesive layer. The polarizing plate with a hard coating is typically disposed on the viewing side of the image display unit, and the hard coating is disposed such that it is on the viewing side. Examples of image display devices include liquid crystal display devices, organic electroluminescent (EL) display devices, and quantum dot display devices.
[0034] Examples The present invention will be specifically described below by way of examples, but the present invention is not limited to these examples. The evaluation items of the examples are as follows. Furthermore, unless otherwise specified, "parts" and "%" in the examples refer to weight.
[0035] (1) The thickness was measured using an interferometric film thickness gauge (manufactured by Otsuka Electronics Co., Ltd., product name "MCPD-3000"). (2) The shear failure strength was measured using a precision oblique cutting device (e.g., manufactured by DAIPLA WINTES CO., LTD., "SAICAS DN-20 type"). The laminate of hard coating, intermediate layer (in the comparative example, there was no intermediate layer formed) and protective layer used in the examples and comparative examples was obliquely cut, and the shear failure strength was obtained from the shear strength during cutting. The cutting conditions were as follows. Cutting tool: made of single crystal diamond. Tool width: 1 mm. Cutting tool angle: 10°. Horizontal speed of cutting tool: 1 µm / s. Vertical speed of cutting tool: 0.05 µm / s. The shear failure strength T (MPa) of the intermediate layer was calculated using the following formula and converted into the amount per µm thickness. T(MPa)=FH(kN) / (2×Wd(m2)×cotφ) Here, FH is the horizontal load caused by the cutter, W is the width of the cutter (m), d is the vertical displacement of the cutter (m), and φ is 45°. (3) Damage or cracks in the hard coating The periphery of the through hole in the polarizing plate with hard coating of the embodiment and comparative example was photographed with an optical microscope (magnification: ×5x). The presence or absence of damage or cracks in the hard coating (including the intermediate layer if there is an intermediate layer) caused by the formation of the through hole was confirmed by visual inspection of the photographed images, and evaluated according to the following criteria. Good: No damage or cracks were found. Poor: Damage and / or cracks were found. (4) Adhesion and durability of the hard coating: After placing the polarizing plates with hard coatings of the examples and comparative examples under high temperature and high humidity conditions (in an oven at 65°C and 90%RH) for 72 hours, the presence or absence of hard coating (including the intermediate layer if present) was visually inspected, and evaluated according to the following criteria. Good: No peeling confirmed. Poor: Peeling confirmed. (5) Scratch resistance: The polarizing plates with hard coatings of the examples and comparative examples were placed on a glass plate with the side without hard coating facing down. Steel wool #0000 was uniformly applied to the smooth section of a cylinder with a diameter of 11 mm, and the test specimen surface was rubbed 10 times at a speed of approximately 100 mm per second under a load of 1.0 kg. The damage condition of the hard coating surface was visually inspected, and evaluated according to the following criteria. Good: No scratches confirmed. Poor: Scratch confirmed.
[0036] <Example 1> 1. Fabrication of Polarizing Plate A strip-shaped amorphous polyethylene terephthalate (PET) film (thickness: 100µm) with a Tg of approximately 75°C was used as the thermoplastic resin substrate, and one side of the resin substrate was subjected to corona treatment. 13 parts by weight of potassium iodide were added to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (degree of polymerization 4200, degree of saponification 99.2 mol%) and acetyl acetylated modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER") in a 9:1 ratio, and the resulting solution was dissolved in water to prepare a PVA aqueous solution (coating solution). The above-mentioned PVA aqueous solution was coated onto the corona-treated side of the resin substrate and dried at 60°C, thereby forming a PVA-based resin layer with a thickness of 13µm, thus producing a laminate. The resulting laminate was uniaxially stretched 2.4 times along its longitudinal direction (long side) in an oven at 130°C (air-assisted stretching treatment). Next, the laminate was immersed in an insoluble bath (a boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at 40°C for 30 seconds (insoluble treatment). Then, it was immersed in a dyeing bath (an iodine aqueous solution prepared by mixing iodine and potassium iodide in a 1:7 weight ratio with 100 parts by weight of water) at 30°C for 60 seconds while adjusting the concentration, to achieve the desired monomer transmittance (Ts) of the final polarizer (dyeing treatment). Finally, it was immersed in a crosslinking bath (a boric acid aqueous solution prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) at 40°C for 30 seconds (crosslinking treatment). Then, while immersing the laminate in a boric acid aqueous solution (4 wt% boric acid concentration, 5 wt% potassium iodide concentration) at a liquid temperature of 70°C, it is uniaxially stretched longitudinally (long side direction) between rollers with different circumferential speeds to achieve a total elongation ratio of 5.5 times (water stretching treatment). Afterwards, the laminate is immersed in a washing bath at a liquid temperature of 20°C (an aqueous solution of 4 wt% potassium iodide mixed with 100 wt% water) (washing treatment). Then, it is dried in an oven maintained at approximately 90°C while its contact surface temperature is maintained at approximately 75°C using SUS heated rollers (drying shrinkage treatment). Following the above method, a polarizing element with a thickness of approximately 5µm is formed on a resin substrate, thereby obtaining a polarizing plate having a resin substrate / polarizing element configuration.
[0037] 2. Formation of the hard coating and intermediate layer: The film-forming components of the hard coating are prepared as follows: 50 parts by weight of UV-curable acrylic resin (manufactured by Toa Synthetic Co., Ltd., trade name "M-920", 100% solids) and 50 parts by weight of UV-curable acrylic resin (manufactured by Mitsubishi Chemical Co., trade name "UV1700-TL", 80% solids). For every 100 parts by weight of the resin solids of these resins, 3 parts by weight of photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907") and 0.15 parts by weight of leveling agent (manufactured by Kyoei Chemical Co., Ltd., trade name "LE-303", 40% solids) are mixed. The mixture is diluted with a MIBK / cyclopentanone mixed solvent (70 / 30 by weight) to a solids concentration of 30% to prepare a coating solution for forming the hard coating. As the substrate (which will ultimately become the protective layer), a TAC film (manufactured by FUJIFILM, trade name "TJ25", thickness 25µm) is prepared. The aforementioned hard coating forming liquid is applied to one side of the substrate (the side in contact with the air surface during TAC film casting: side A) using a bar coater to form a coating film. Next, the substrate with the coating film is heated at 80°C for 1 minute to dry the coating film. Then, the coating film is hardened by irradiation with ultraviolet light at a cumulative intensity of 300 mJ / cm² using a high-pressure mercury lamp. A substrate / hardened coating laminate is obtained in the above manner. The overall thickness of the hardened coating film is 2.6µm, of which the thickness of the hard coating layer is 1.3µm and the thickness of the intermediate layer is 1.3µm. The shear strength per 1µm thickness of the intermediate layer is 125MPa.
[0038] 3. Fabrication of the polarizing plate with a hard coating: The substrate / hardened coating laminate obtained in step 2 above is bonded to the surface of the polarizing element of the resin substrate / polarizing element laminate (polarizing plate) obtained in step 1 above using an acrylic adhesive, with the substrate and polarizing element adjacent to each other. Next, the resin substrate is peeled off, and a general TAC film for irregular processing substrate is bonded to the peeled surface using an active energy line hardening adhesive (thickness 0.7µm). The active energy line hardening adhesive is applied using an MCD coating machine (manufactured by Fuji Machinery Co., Ltd.) (groove shape: honeycomb, gravure roller line count: 1000 lines / inch, rotation speed 140% / relative production line speed). Next, visible light is irradiated from both sides by an active energy line irradiation device to harden the active energy line hardening adhesive, and then it is dried with hot air at 70°C for 3 minutes to obtain a polarizing plate with a hard coating consisting of a hard coating layer / intermediate layer / protective layer / polarizing element / substrate. Furthermore, the active energy line curing adhesive is prepared as follows: 12 parts by weight of free radical polymerizable compound (a), 35 parts by weight of free radical polymerizable compound (b), 40 parts by weight of free radical polymerizable compound (c), 10 parts by weight of oligomer compound (d), 2 parts by weight of photopolymerization initiator (e), and 1 part by weight of photosensitizer (f) are mixed and stirred at 50°C for 1 hour to obtain the active energy line curing adhesive. In addition, the free radical polymerizable compound (a) is HEAA (hydroxyethyl acrylamide) (manufactured by KJ Chemicals Corporation); the free radical polymerizable compound (b) is ACMO (acrylamide morphofolin) (manufactured by KJ Chemicals Corporation); the free radical polymerizable compound (c) is LIGHT ACRYLATE 1,9ND-A (1,9-nonanediol diacrylate) (manufactured by Kyoeisha Chemical Co., Ltd.); the oligomer compound (d) is ARUFON UG-4010 (epoxy-modified acrylic oligomer) (manufactured by Toa Synthetic Co., Ltd.); the photopolymerization initiator (e) is Omnirad907 (2-methyl-1-(4-methylthiophenyl)-2-morphofolinylpropane-1-one) (manufactured by IGM Resins BV Co., Ltd.); and the photosensitizer (f) is KAYACURE DETX-S (2,4-diethyl-9-oxothiosulfate) (manufactured by Nippon Kayaku Co., Ltd.).
[0039] 4. Shape processing of the polarizing plate with hard coating The polarizing plate with hard coating obtained in step 3 above is punched to a length of 142.0 mm and a width of 66.8 mm, and has an R portion of 7.0 mm at each of the four corners. The punching is performed with the absorption axis of the polarizing element in the direction of the short side. A through hole with a diameter of 4.0 mm is formed at a distance of 2 mm from the long side and 2 mm from the short side. The through hole is formed by end milling. The feed rate of the end mill is 750 mm / min, the rotation speed is 10000 rpm, and the chip amount is 0.1 mm / cut. The polarizing plate with hard coating and through hole is obtained in accordance with the above method. The obtained polarizing plate with hard coating is evaluated in steps (3) to (5) above. The results are listed in Table 1.
[0040] <Example 2> A hardened coating film with an overall thickness of 7.4 µm was formed using the following hard coating forming liquid. Otherwise, a polarizing plate with a hard coating having through holes was obtained in the same manner as in Example 1. The thickness of the hard coating was 3.0 µm, and the thickness of the intermediate layer was 4.4 µm. The shear breaking strength of the intermediate layer per 1 µm thickness was 14 MPa. The obtained polarizing plate with the hard coating was subjected to the same evaluation as in Example 1. The results are listed in Table 1. As the film forming component of the hard coating, 100 parts by weight of UV-curable acrylic resin (manufactured by DIC Corporation, trade name "LUXYDIR 17-806", 80% solids) was prepared. For every 100 parts by weight of resin solids, 3 parts by weight of photopolymerization initiator (manufactured by BASF Corporation, trade name "OMNIRAD907") and 0.01 parts by weight of leveling agent (manufactured by DIC Corporation, trade name "GRANDIC PC4100", 10% solids) were mixed. The mixture was diluted with a PGME / cyclopentanone mixed solvent (65 / 35 by weight) to a solids concentration of 36%, and a coating solution for hard coating formation was prepared.
[0041] <Example 3> Using a 40µm thick TAC film (manufactured by FUJIFILM, trade name "TJ40") as the substrate (protective layer), using the following hard coating forming liquid, the coating before curing was heated at 60°C for 1 minute to form a hard coating film with an overall thickness of 10.1µm. Otherwise, a polarizing plate with a hard coating having through holes was obtained in the same manner as in Example 1. The thickness of the hard coating was 3.3µm, and the thickness of the intermediate layer was 6.8µm. The shear breaking strength per 1µm thickness of the intermediate layer was 18MPa. The obtained polarizing plate with the hard coating was subjected to the same evaluation as in Example 1. The results are listed in Table 1. The film forming component of the hard coating was prepared as 100 parts by weight of UV-curable acrylic resin (manufactured by DIC, trade name "LUXYDIR 17-806", 80% solids). For every 100 parts by weight of the aforementioned resin solids, mix 3 parts by weight of photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907") and 0.01 parts by weight of leveling agent (manufactured by DIC, trade name "GRANDIC PC4100", solids content 10%). Dilute this mixture with a PGME / cyclopentanone mixed solvent (weight ratio 50 / 50) to a solids content concentration of 36% to prepare a coating solution for hard coating formation.
[0042] <Example 4> A polarizing plate with a hard coating and through holes was obtained by using a 25µm thick TAC film (manufactured by FUJIFILM, trade name "TJ25UL") as the substrate (protective layer) and a hard coating film with an overall thickness of 9.3µm formed using the anti-glare layer forming liquid described below. The polarizing plate was obtained in the same manner as in Example 1. The thickness of the anti-glare layer was 1.8µm, and the thickness of the intermediate layer was 7.5µm. The shear strength per 1µm thickness of the intermediate layer was 27MPa. The obtained hard-coated polarizing plate was subjected to the same evaluation as in Example 1. The results are listed in Table 1. The film-forming components of the anti-glare layer are prepared as follows: 50 parts by weight of UV-curable carbamate acrylate resin (manufactured by Mitsubishi Chemical Co., trade name "UV1700B") and 50 parts by weight of polyfunctional acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #300") with neopentyl tert-ol triacrylate as the main component. For every 100 parts by weight of the total solids content of the resins, 2 parts by weight of acrylic and styrene copolymer particles (manufactured by Sekisui Chemicals Co., Ltd., "Techpolymer SSX1055QXE") are mixed as anti-glare layer forming particles; 1.5 parts by weight of synthetic bentonite (manufactured by Kunimine Industries Co., Ltd., "SUMECTON SAN") is mixed as a thixotropic agent; 3 parts by weight of photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907") is mixed; and 0.15 parts by weight of leveling agent (manufactured by DIC, trade name "GRANDIC PC4100", 10% solids content) is mixed. This mixture is then diluted with a toluene / cyclopentanone mixed solvent (80 / 20 by weight) to a solids content concentration of 50% to prepare an anti-glare layer forming coating solution.
[0043] <Example 5> A polarizing plate was manufactured in the same manner as in Example 1. On the other hand, a hard coating and an intermediate layer were formed as follows. The resin contained in the hard coating was prepared as follows: 50 parts by weight of UV-curable acrylic resin (manufactured by Shin-Nakamura Chemical Co., trade name "A-DCP", 100% solids) and 50 parts by weight of UV-curable acrylic resin (manufactured by Mitsubishi Chemical Co., trade name "UV1700-TL", 80% solids). For every 100 parts by weight of the resin solids of the aforementioned resins, 5 parts by weight of photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907") and 0.2 parts by weight of leveling agent (manufactured by Kyoeisha Chemical Co., trade name "LE-303", 40% solids) were mixed. The mixture was diluted with a MIBK / cyclopentanone mixed solvent (weight ratio 60 / 40) to a solids concentration of 30% to prepare a coating liquid for forming the hard coating. As the substrate (which will ultimately become the protective layer), a TAC film (manufactured by FUJIFILM, trade name "TJ25UL") was prepared. The above-mentioned hard coating forming liquid was applied to one side of the substrate (the side in contact with the air surface during TAC film casting: side A) using a bar coater to form a coating film. Next, the substrate with the coating film was heated at 60°C for 1 minute to dry the coating film. Then, the coating film was hardened by irradiation with ultraviolet light at a cumulative intensity of 220 mJ / cm² using a high-pressure mercury lamp. A substrate / hardened coating laminate was obtained in the above manner. The thickness of the hard coating layer was 2.8 µm, and the thickness of the intermediate layer was 0.4 µm. The shear strength per 1 µm thickness of the intermediate layer was 148 MPa. The following procedure was performed in the same manner as in Example 1 to obtain a polarizing plate with a hard coating and through-holes. The obtained polarizing plate with the hard coating was subjected to the same evaluation as in Example 1. The results are listed in Table 1.
[0044] <Example 6> A polarizing plate was manufactured in the same manner as in Example 1. On the other hand, a hard coating and an intermediate layer were formed as follows. The resin contained in the hard coating was prepared as follows: 50 parts by weight of UV-curable acrylic resin (manufactured by Shin-Nakamura Chemical Co., trade name "A-DCP", 100% solids) and 50 parts by weight of UV-curable acrylic resin (manufactured by Mitsubishi Chemical Co., trade name "UV1700-TL", 80% solids). For every 100 parts by weight of the resin solids of the aforementioned resins, 5 parts by weight of photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907") and 0.1 parts by weight of leveling agent (manufactured by Kyoeisha Chemical Co., trade name "LE-303", 40% solids) were mixed. The mixture was diluted with a MIBK / cyclopentanone mixed solvent (weight ratio 60 / 40) to a solids concentration of 30% to prepare a coating liquid for forming the hard coating. As the substrate (which will ultimately become the protective layer), a TAC film (manufactured by FUJIFILM, trade name "TJ25UL") was prepared. The above-mentioned hard coating forming liquid was applied to one side of the substrate (the side in contact with the air surface during TAC film casting: side A) using a bar coater to form a coating film. Next, the substrate with the coating film was heated at 60°C for 1 minute to dry the coating film. Then, the coating film was hardened by irradiation with ultraviolet light at a cumulative intensity of 260 mJ / cm² using a high-pressure mercury lamp. A substrate / hardened coating laminate was obtained in the above manner. The thickness of the hard coating layer was 2.5 µm, and the thickness of the intermediate layer was 0.7 µm. The shear strength per 1 µm thickness of the intermediate layer was 86 MPa. The following procedure was performed in the same manner as in Example 1 to obtain a polarizing plate with a hard coating and through-holes. The obtained polarizing plate with the hard coating was subjected to the same evaluation as in Example 1. The results are listed in Table 1.
[0045] <Comparative Example 1> The overall thickness of the hardened coating was set to 6.6µm. A 25µm thick TAC film (manufactured by Konica Minolta, trade name "KC2UA") was used as the substrate (protective layer). A hard coating was formed on the B-side of the TAC film (the side that contacts the support surface during TAC film casting). Otherwise, a polarizing plate with through holes and a hard coating was obtained in the same manner as in Example 2. The thickness of the hard coating was 2.7µm, and the thickness of the intermediate layer was 3.9µm. The shear strength of the intermediate layer was 9MPa. The obtained polarizing plate with the hard coating was subjected to the same evaluation as in Example 1. The results are listed in Table 1.
[0046] <Comparative Example 2> A hardened coating film with an overall thickness of 8.7 µm was formed using the following hard coating forming liquid. Otherwise, a polarizing plate with a hard coating having through holes was obtained in the same manner as in Comparative Example 1. The thickness of the hard coating was 3.3 µm, and the thickness of the intermediate layer was 5.4 µm. The shear breaking strength of the intermediate layer was 9 MPa. The obtained polarizing plate with the hard coating was subjected to the same evaluation as in Example 1. The results are listed in Table 1. As the film forming component of the hard coating, 100 parts by weight of UV-curable acrylic resin (manufactured by DIC Corporation, trade name "LUXYDIR 17-806", 80% solids) was prepared. For every 100 parts by weight of the resin solids of the aforementioned resin, 3 parts by weight of photopolymerization initiator (manufactured by BASF Corporation, trade name "OMNIRAD907") and 0.01 parts by weight of leveling agent (manufactured by DIC Corporation, trade name "GRANDIC PC4100", 10% solids) were mixed. The mixture was diluted with a PGME / cyclopentanone / butyl acetate mixed solvent (weight ratio 9 / 40 / 51) to a solids concentration of 36%, and a coating solution for hard coating formation was prepared.
[0047] <Comparative Example 3> A polarizing plate with a hard coating and through holes was obtained by setting the overall thickness of the hard coating to 1.6 µm and using a 20 µm thick polycarbonate (PC) resin film (an extruded film manufactured by Mitsubishi Chemical Co. under the trade name "DURABIO") as the substrate (protective layer). Otherwise, the process was the same as in Example 2. The hard coating thickness was 1.6 µm, and no intermediate layer was formed. The obtained hard-coated polarizing plate was subjected to the same evaluation as in Example 1. The results are listed in Table 1.
[0048] <Comparative Example 4> A polarizing plate with a hard coating and through holes was obtained by setting the overall thickness of the hard coating to 1.4 µm and using a 26 µm thick cyclic olefin resin (COP) film (manufactured by ZEON Corporation, Japan, trade name "ZF12") as the substrate (protective layer). Otherwise, the process was the same as in Example 2. The hard coating thickness was 1.4 µm, and no intermediate layer was formed. The obtained hard-coated polarizing plate was subjected to the same evaluation as in Example 1. The results are listed in Table 1.
[0049] <Comparative Example 5> A polarizing plate with a hard coating and through holes was obtained by setting the overall thickness of the hard coating to 10.4 µm and using a 40 µm thick acrylic resin film (manufactured by Nitto Denko Corporation, trade name "HX-40UF") as the substrate (protective layer). Otherwise, the process was the same as in Example 2. The thickness of the hard coating was 1.2 µm, and the thickness of the intermediate layer was 9.2 µm. The shear strength of the intermediate layer was 17 MPa. The obtained hard-coated polarizing plate was subjected to the same evaluation as in Example 1. The results are listed in Table 1.
[0050] <Reference Example> The hard-coated polarizing plates manufactured according to the configurations described in Examples 1-4 and Comparative Examples 1-5 were punched to a length of 142.0 mm and a width of 66.8 mm. The punching was performed with the absorption axis of the polarizing element in the direction of the shorter side. The end face was machined by cutting 0.5 mm at a time using a machining tool with four sides forming a 10-degree angle. The feed rate of the machining tool was 600 mm / min and the rotation speed was 6000 rpm. A rectangular (i.e., non-irregularly shaped) hard-coated polarizing plate with end face machined was obtained in the above manner. After the obtained hard-coated polarizing plates were evaluated in (3) above, good results were obtained for all hard-coated polarizing plates.
[0051] [Table 1]
[0052] <Evaluation> As can be clearly seen from Table 1, according to the embodiments of the present invention, in the polarizing plate with a hard coating having an irregularly shaped processing section, an intermediate layer is formed between the protective layer and the hard coating, and the thickness of the intermediate layer and the shear strength per unit thickness are set to a predetermined value or higher, thereby significantly suppressing damage and cracking of the hard coating in the irregularly shaped processing section. Furthermore, the hard coating of the polarizing plate with a hard coating according to the embodiments of the present invention also exhibits excellent adhesion durability and scratch resistance.
[0053] Industrial Applicability The polarizing plate with hard coating of the present invention is suitable for use in image display devices, especially for image display devices with irregularly shaped processing parts, such as car dashboards, smartphones, tablet PCs or smartwatches. [Simplified Explanation of the Diagram]
[0007] Figure 1 is a schematic cross-sectional view of a polarizing plate with a hard coating according to an embodiment of the present invention. Figure 2 is a schematic diagram illustrating the specific procedure for calculating the shear failure strength. Figure 3 is a schematic top view illustrating an example of an irregularly shaped or irregularly shaped processing part of a polarizing plate with a hard coating according to an embodiment of the present invention. Figure 4 is a schematic top view illustrating a modified example of an irregularly shaped or irregularly shaped processing part of a polarizing plate with a hard coating according to an embodiment of the present invention. Figure 5 is a schematic top view illustrating yet another modified example of an irregularly shaped or irregularly shaped processing part of a polarizing plate with a hard coating according to an embodiment of the present invention. Figure 6 is a schematic top view illustrating yet another modified example of an irregularly shaped or irregularly shaped processing part of a polarizing plate with a hard coating according to an embodiment of the present invention.
Claims
1. A polarizing plate with a hard coating, comprising, in sequence, a polarizing element, a protective layer, an intermediate layer with a thickness of 0.1µm to 8µm, and a hard coating, and having an irregular shape other than a rectangle; the protective layer is composed of a cellulose triacetate film, the intermediate layer is a miscible region containing components of the hard coating and the protective layer, the intermediate layer has a shear breaking strength of 40MPa or more per 1µm thickness, and does not form an interface between the hard coating and the intermediate layer, or between the intermediate layer and the protective layer.
2. The polarizing plate with a hard coating as claimed in claim 1, wherein the thickness of the aforementioned intermediate layer is 0.3µm to 5µm.
3. A polarizing plate with a hard coating as requested in claim 1 or 2, wherein the thickness of the aforementioned hard coating is less than 5µm.
4. The polarizing plate with a hard coating as claimed in claim 1 or 2, wherein the aforementioned irregular shape is selected from the group consisting of: through holes, V-shaped notches, U-shaped notches, recesses that are approximately boat-shaped when viewed from above, rectangular recesses that are rectangular when viewed from above, R-shaped recesses that are approximately bathtub-shaped when viewed from above, and combinations thereof.
5. An image display device comprising, on the viewing side, a polarizing plate with a hard coating as claimed in any one of claims 1 to 4.
Citation Information
Patent Citations
Polarizing film, polarizing film with adhesive layer, and image display device
JP2019219527A
Hard coat film, polarizing plate, and image display apparatus
KR1020140134228A
Convex side polarizing plate for curved surface image display panel
TW201730594A