AI Technical Summary

Technical Problem

Existing wafer processing methods that use laser cutting and dicing blades result in film peeling and blade clogging, leading to reduced component density on semiconductor wafers due to the need for wider laser processing grooves than dicing grooves.

Method used

A method involving laser processing grooves formed with absorptive wavelengths on the wafer surface, followed by cutting with a dicing blade from the back side, using protective films and sheets to manage debris and fluid contamination, and precise cutting to match groove widths.

Benefits of technology

Increases the number of components per wafer by minimizing the width of the dividing lines, reducing contamination, and maintaining processing quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure TWG2TB001920087_001
    Figure TWG2TB001920087_001
  • Figure TWG2TB001920087_002
    Figure TWG2TB001920087_002
  • Figure TWG2TB001920087_003
    Figure TWG2TB001920087_003
Patent Text Reader

Abstract

[Problem] To provide a wafer processing method that can increase the number of components per wafer. [Solution] A wafer processing method comprising: forming a wafer with components in areas divided by intersecting predetermined dicing lines on the front side; and comprising: a laser processing groove forming step 1002, wherein a laser beam of wavelength having absorbency to the wafer is irradiated onto the front side of the wafer to form a laser processing groove along the predetermined dicing lines; and a cutting step 1005, wherein after performing the laser processing groove forming step 1002, a cutting blade is inserted from the back side of the wafer to the depth of the laser processing groove while the cutting blade cuts the wafer along the predetermined dicing lines to divide the wafer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for processing a wafer on the front side in which components are formed in areas divided by multiple intersecting predetermined dividing lines. [Previous Technology]

[0002] To improve the characteristics of semiconductor devices, low-k insulating films (comprising inorganic films such as SiOF and BSG (SiOB) or polymer films such as polyimide and parylene, i.e., organic films, are widely used as interlayer insulating films in semiconductor devices. Furthermore, semiconductor wafers with metal patterns called TEGs (Test Element Groups) formed on predetermined dicing lines are also widely used.

[0003] Although semiconductor devices are formed by cutting semiconductor wafers along predetermined dicing lines with a cutting blade, if these Low-k films or TEGs are cut with a cutting blade, problems such as Low-k film peeling or cutting blades being clogged with pores and abrasive passivation due to TEGs will occur, resulting in deterioration of processing quality.

[0004] Therefore, a processing method is widely used in which a laser beam is used to cleave the Low-k film or TEG, and a cleaving blade is used to cut the semiconductor wafer (see, for example, Patent Document 1). [Preferred Art Documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 2005-64231 [Summary of the Invention]

[0006] [Problem to be Solved by the Invention] However, in the processing method shown in Patent Document 1, it is necessary to form a laser processing groove with a width wider than the dicing groove formed by the cutting blade; that is, it is necessary to form the width of the predetermined dividing line of the semiconductor wafer to be wider than the width of the dicing groove. Therefore, in the processing method shown in Patent Document 1, there is a problem that the number of semiconductor devices that can be formed from a single semiconductor wafer decreases, and it is desirable to improve this.

[0007] The purpose of this invention is to provide a wafer processing method that can increase the number of components on each wafer.

[0008] [Technical Means for Solving the Problem] In order to solve the above-mentioned problem and achieve the objective, the wafer processing method of the present invention is a method for forming components on a wafer with multiple intersecting predetermined dividing lines on the front side, characterized in that it includes: a laser processing groove forming step, which irradiates the front side of the wafer with a laser beam of wavelength that has absorption properties on the wafer to form a laser processing groove along the predetermined dividing lines; and a cutting step, which, after performing the laser processing groove forming step, cuts the wafer along the predetermined dividing lines with a cutting blade while cutting from the back side of the wafer to the depth of the laser processing groove.

[0009] The wafer processing method may also include a thin-film placement step, in which a thin film is adhered to the front side of the wafer and filled into the laser processing tank after the laser processing tank formation step and before the cutting step, and in the cutting step, cutting fluid is supplied to the processing point where the cutting blade contacts the wafer while the cutting blade cuts the wafer.

[0010] The wafer processing method may also include: a protective film forming step, in which a protective film is formed on the front side of the wafer before the laser processing tank forming step is performed, and the sheet is adhered to the protective film in the sheet placement step; and the wafer processing method may further include: a transfer step, in which an adhesive film is adhered to the back side of the wafer and the sheet is removed from the front side of the wafer after the dicing step; and a protective film removal step, in which the protective film is removed after the transfer step is performed.

[0011] In the wafer processing method, during the cutting step, the cutting blade may also cut to a depth that does not completely cut the wafer.

[0012] In the wafer processing method, the sheet may not have a paste layer. In the sheet placement step, the sheet may be heated and the sheet may be adhered to the front side of the wafer.

[0013] [Effect of the Invention] The present invention has the effect of increasing the number of components on each wafer.

Implementation Method

[0015] The embodiments for carrying out the present invention will be described in detail with reference to the accompanying drawings. The present invention is not limited to the contents described in the following embodiments. Furthermore, the constituent elements described below include those readily conceived and substantially the same as those skilled in the art to which this invention pertains. Moreover, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications to the configuration are possible without departing from the spirit of the present invention.

[0016] [Embodiment 1] A wafer processing method according to Embodiment 1 of the present invention will be described with reference to the figures. FIG1 is a perspective view of the wafer to be processed by the wafer processing method of Embodiment 1. FIG2 is a flowchart showing the process of the wafer processing method of Embodiment 1.

[0017] The processing method of Embodiment 1 is the processing method of the wafer 1 shown in FIG. 1. The wafer 1 to be processed by the processing method of Embodiment 1 is a circular semiconductor wafer or optical element wafer, etc., with silicon, sapphire, gallium arsenide or SiC (silicon carbide) as substrate 2. Multiple intersecting predetermined dividing lines 4 are provided on the front side 3 of the wafer 1, and elements 5 are formed in the grid-like areas divided by the predetermined dividing lines 4 on the front side 3.

[0018] Component 5 is, for example, an integrated circuit such as IC (Integrated Circuit) or LSI (Large Scale Integration), an image sensor such as CCD (Charge Coupled Device) or CMOS (Complementary Metal Oxide Semiconductor), or a memory (semiconductor memory device).

[0019] In Embodiment 1, as shown in FIG1, the wafer 1 has an element layer 6, which is an organic film, on the substrate 2. The element layer 6 includes: a low-dielectric-constant insulating film (hereinafter referred to as a Low-k film) composed of inorganic films such as SiOF and BSG (SiOB) or polymer films such as polyimide-based and parylene-based, i.e., organic films or silicon oxide (SiOCH); and a circuit layer composed of conductive metal patterns or metal films.

[0020] Component 5 is formed by laminating a Low-k film and a circuit layer. The circuit layer constitutes the circuit of component 5. Therefore, component 5 is formed by mutually laminating Low-k films of component layer 6 on substrate 2 and circuit layers laminated between the Low-k films. In the predetermined dividing line 4, component layer 6, in addition to TEG (Test Elementary Group), is also formed by Low-k films laminated on substrate 2.

[0021] Furthermore, in Embodiment 1, a TEG (not shown) is formed on the wafer 1 along the predetermined dicing line 4. The TEG is an evaluation element used to identify design or manufacturing problems in the element 5. If the wafer 1 is cut from the front side 3 with a dicing blade, the element layer 6, which is like a Low-k film, and the TEG are easily peeled off from the substrate 2.

[0022] The wafer processing method of Embodiment 1 is a method of dividing the constructed wafer 1 into individual elements 5 along a predetermined dividing line 4. As shown in FIG2, the wafer processing method of Embodiment 1 includes: a protective film forming step 1001, a laser processing tank forming step 1002, a protective film removal step 1003, a wafer placement step 1004, and a dicing step 1005.

[0023] (Protective film formation step) Figure 3 is a side view schematically showing the protective film formation step of the wafer processing method shown in Figure 2 in partial cross-section. Figure 4 is a cross-sectional view schematically showing the main part of the wafer after the protective film formation step of the wafer processing method shown in Figure 2.

[0024] The protective film forming step 1001 is a step performed before the laser processing tank forming step 1002, in which the protective film coating device 20 shown in FIG3 forms a protective film 25 (shown in FIG4) on the front side 3 of the wafer 1. In addition, in Embodiment 1, in the protective film forming step 1001, an adhesive film 10 with a diameter larger than that of the wafer 1 is adhered to the back side 7 of the back side of the front side 3 of the wafer 1, and an annular frame 11 is adhered to the outer periphery of the adhesive film 10, and the wafer 1 is supported by the annular frame 11.

[0025] In Embodiment 1, in the protective film forming step 1001, the protective film coating device 20 attracts and holds the back side 7 of the wafer 1 on the holding surface of the rotary table 21 through the adhesive film 10, and clamps the annular frame 11 with the clamping part 22 provided around the rotary table 21. In the protective film forming step 1001, as shown in FIG3, the protective film coating device 20 rotates the rotary table 21 about its axis and drips water-soluble resin 24 from the water-soluble resin supply nozzle 23 onto the center of the front side 3 of the wafer 1.

[0026] The water-soluble resin 24 that is dripped is coated on the entire surface of the front side 3 of the wafer 1 by the centrifugal force generated by the rotation of the rotating table 24, flowing from the center side to the outer periphery.

[0027] Furthermore, the water-soluble resin 24 is, for example, a water-soluble resin such as polyvinyl alcohol (PVA) or polyvinylpyrrolidone (PVP). In the protective film formation step 1001, by curing the water-soluble resin 24 coated on the entire surface of the front side 3 of the wafer 1, a water-soluble protective film 25 covering the entire surface of the front side 3 of the wafer 1 is formed, as shown in FIG4. Furthermore, the element layer 6 is omitted in FIG3.

[0028] (Laser processing trench formation step) Figure 5 is a side view schematically showing the laser processing trench formation step of the wafer processing method shown in Figure 2 in partial cross-section. Figure 6 is a cross-sectional view schematically showing the main part of the wafer after the laser processing trench formation step of the wafer processing method shown in Figure 2.

[0029] The laser processing groove forming step 1002 is the step in which the laser processing apparatus 30 shown in FIG. 5 irradiates the front side 3 of the wafer 1 with a laser beam 33 of a wavelength that has absorption properties on the wafer 1 to form a laser processing groove 35 along the predetermined dividing line 4 (as shown in FIG. 6). In Embodiment 1, in the laser processing groove forming step 1002, the laser processing apparatus 30 attracts and holds the back side 7 of the wafer 1 to the holding surface of the chuck stage 31 through the adhesive film 10, and clamps the annular frame 11 with a clamping part (not shown) provided around the chuck stage 31.

[0030] In the laser processing tank forming step 1002, the laser processing apparatus 30 moves the chuck stage 31 and the laser beam irradiation unit 32 relative to each other along the predetermined dividing line 4, and as shown in FIG. 5, irradiates the predetermined dividing line 4 from the front side 3 of the laser beam irradiation unit 32 with a wavelength that has absorption properties for the substrate 2 of the wafer 1 through the protective film 25. In addition, in Embodiment 1, in the laser processing tank forming step 1002, the laser processing apparatus 30 sets the focusing point at a predetermined position on the front side 3 of each predetermined dividing line 4, that is, at the center in the width direction, and irradiates the laser beam 33.

[0031] In the laser processing trench formation step 1002, since the laser beam 33 has a wavelength that absorbs the wafer 1, as shown in FIG6, the component layer 6 on the dicing predetermined line 4 and the substrate 2 are ablated to break the component layer 6 on the dicing predetermined line 4, and a laser processing trench 35 reaching the substrate 2 is formed along the dicing predetermined line 4. In the laser processing trench formation step 1002, laser processing trenches 35 are formed on all the dicing predetermined lines 4.

[0032] Furthermore, in Embodiment 1, a laser processing groove 35 is formed at a predetermined position on the dividing line 4, i.e., at the center in the width direction. In the laser processing groove forming step 1002, a laser beam 33 is irradiated onto the wafer 1, and debris is generated during the formation of the laser processing groove 35. The generated debris adheres to the protective film 25.

[0033] (Protective film removal step) Figure 7 is a side view schematically showing the protective film removal step of the wafer processing method shown in Figure 2 in partial cross-section. Protective film removal step 1003 is the step of removing the protective film 25 from the front side 3 of the wafer 1.

[0034] In the protective film removal step 1003, the cleaning device 40 holds the back side 7 of the wafer 1 against the holding surface of the rotary table 41 through the adhesive film 10, and clamps the annular frame 11 with the clamping part 42 provided around the rotary table 41. In the protective film removal step 1003, as shown in FIG7, the cleaning device 40 supplies cleaning liquid 44 composed of pure water from the cleaning liquid supply nozzle 43 to the center of the front side 3 of the wafer 1 while the rotary table 41 is rotating around the axis. The cleaning liquid 44 supplied to the front side 3 of the wafer 1 is cleaned on the front side 3 of the wafer 1 by the centrifugal force generated by the rotation of the rotary table 41, flowing from the center side to the outer periphery, thus removing the protective film 25 and debris from the front side 3 of the wafer 1. In addition, the component layer 6 is omitted in FIG7.

[0035] (Wafer Placement Step) Figure 8 is a schematic cross-sectional view showing the main part of the wafer, i.e., the protective film, adhered to the front side of the wafer in the wafer placement step of the wafer processing method shown in Figure 2. Figure 9 is a perspective view of the wafer after the wafer placement step of the wafer processing method shown in Figure 2.

[0036] The sheet placement step 1004 is performed after the laser processing tank formation step 1002 and before the cutting step 1005. It involves attaching the sheet, i.e., the protective film 12 shown in FIG. 8, to the front side 3 of the wafer 1 and filling a portion of the protective film 12 into the laser processing tank 35. In Embodiment 1, in the sheet placement step 1004, as shown in FIG. 8, the protective film 12 is attached as a sheet to the front side 3 of the wafer 1. The protective film 12 includes a substrate layer 121 and a paste layer 122 deposited on the substrate layer 121.

[0037] The substrate layer 121 is made of a flexible and non-adhesive resin. The paste layer 122 is made of a flexible and adhesive resin. In Embodiment 1, the thickness 123 of the paste layer 122 (shown in FIG8) is greater than the depth 36 of the laser processing groove 35 from the front side 3 (shown in FIG6).

[0038] In the wafer placement step 1004, as shown in FIG9, a protective film 12 in the shape of a disc with a diameter larger than that of wafer 1 is adhered to the front side 3 of wafer 1, and an annular frame 13 is adhered to the outer edge of the protective film 12, thereby supporting wafer 1, and the adhesive film 10 is peeled off from the back side 7. In Embodiment 1, in the wafer placement step 1004, the protective film 12 is pressed onto the front side 3 of wafer 1, and a portion of the protective film 12, i.e., the adhesive layer 122, is filled into the laser processing tank 35.

[0039] (Cutting Steps) Figure 10 is a side view schematically showing the cutting steps of the wafer processing method shown in Figure 2 in partial cross-section. Figure 11 is a cross-sectional view schematically showing the main part of the wafer after the cutting steps of the wafer processing method shown in Figure 2.

[0040] Cutting step 1005 is performed after laser processing tank formation step 1002. As shown in FIG10, the cutting device 50 cuts the wafer 1 along the predetermined dividing line 4 with the cutting blade 54 while cutting the wafer 1 from the back side 7 of the wafer 1 to the depth reaching the laser processing tank 35. In cutting step 1005, the cutting device 50 attracts and holds the front side 3 of the wafer 1 on the holding surface of the chuck stage 51 through the protective film 12, and clamps the annular frame 13 with the clamping part 52 provided around the chuck stage 51.

[0041] In the cutting step 1005, the cutting device 50 takes an infrared camera to photograph the back side 7 of the wafer 1, or to photograph the front side 3 of the wafer 1 through the protective film 12 and the chuck table 51, and performs alignment. The alignment is to align the cutting blade 54 of the cutting unit 53 with the predetermined dividing line 4. In the cutting step 1005, as shown in FIG10, the cutting device 50 moves the chuck table 51 and the cutting blade 54 relative to each other along the predetermined dividing line 4, while supplying cutting fluid (not shown) to the processing point where the cutting blade 54 contacts the wafer 1, and cutting the wafer 1 at a predetermined position (i.e., the center in the width direction) of the predetermined dividing line 4 of the wafer 1 to a depth that reaches the laser processing tank 35 but does not reach the holding surface of the chuck table 51, and cuts the wafer 1 with the cutting blade 54.

[0042] In Embodiment 1, in the cutting step 1005, the cutting apparatus 50 causes the cutting blade 54 to cut into the wafer 1 at a depth shallower than the thickness of the substrate 2 of the wafer 1 and not reaching the protective film 12. Thus, in the cutting step 1005, the cutting blade 54 cuts to a depth that does not completely cut through the protective film 12.

[0043] Thus, in the cutting step 1005, since the cutting blade 54 cuts into the center of the width direction of the predetermined dividing line 4 at the aforementioned depth, as shown in FIG11, the laser processing groove 35 is exposed at the bottom of the cutting groove 55 formed by the cutting of the cutting blade 54, and the predetermined dividing line 4 is divided by the cutting groove 55 and the laser processing groove 35. In the cutting step 1005, all the predetermined dividing lines 4 are cut by the cutting blade 54, cutting grooves 55 are formed on all the predetermined dividing lines 4, and the wafer 1 is divided into individual components 5, thus ending the wafer processing method. In addition, FIG10 omits the paste layer 122. Furthermore, the individual components 5 divided into components are picked up from the paste layer 122 of the protective film 12.

[0044] The wafer processing method described above forms a laser processing groove 35 by irradiating the front side 3 of the wafer 1 with a laser beam 33, and cuts the predetermined dividing line 4 from the back side 7 of the wafer 1 with a cutting blade 54, so that the width of the predetermined dividing line 4 of the wafer 1 is equal to the width of the cutting groove 55.

[0045] Therefore, even for a wafer 1 with a TEG or device layer 6, compared to conventional processing methods that form laser processing grooves 35 by irradiating the front side 3 with a laser beam 33 and then cutting between the laser processing grooves 35, the wafer processing method of Embodiment 1 can better suppress the width of the predetermined dividing line 4. As a result, even for a wafer 1 with a TEG or device layer 6, the wafer processing method of Embodiment 1 can increase the number of devices 5 on each wafer 1.

[0046] Generally, in the processing method, after the front side 3 of the wafer 1 is irradiated with a laser beam 33 in the laser processing tank forming step 1002, if it is cut from the back side 7 with a cutting blade 54, sometimes the cutting fluid containing cutting chips during the cutting process will seep into the front side 3 of the wafer 1 through the laser processing tank 35 and contaminate the front side 3 of the wafer 1. Even if the back side 7 of the exposed wafer 1 is cleaned after cutting, the dirt on the front side 3 of the wafer 1 cannot be removed. Furthermore, even if the wafer is transferred after cutting and an attempt is made to clean the front side 3, the dirt on the front side 3 of the wafer 1 cannot be removed because the cutting fluid evaporates after cutting and the dirt adheres tightly to the front side 3 of the wafer 1.

[0047] However, in the wafer processing method of Embodiment 1, in the wafer placement step 1004, since the protective film 12 of the paste layer 122 is pre-filled in the laser processing tank 35, in the cutting step 1005, the cutting fluid containing cutting chips can be prevented from winding into the front side 3 of the wafer 1 and adhering to the front side 3.

[0048] Furthermore, in the wafer processing method of Embodiment 1, in the protective film forming step 1001 before the laser processing tank forming step 1002, since a protective film 25 is formed on the front side 3 of the wafer 1, it is possible to suppress the attachment of debris generated when the laser beam 33 is irradiated to the front side 3 of the wafer 1.

[0049] [Embodiment 2] The wafer processing method of Embodiment 2 will be described with reference to the figures. FIG12 is a flowchart showing the process of the wafer processing method of Embodiment 2. FIG13 is a perspective view schematically showing the wafer after the wafer placement step of the wafer processing method shown in FIG12. FIG14 is a cross-sectional view schematically showing the main part of the wafer shown in FIG13. FIG15 is a cross-sectional view schematically showing the main part of the wafer after the dicing step of the wafer processing method shown in FIG12. FIG16 is a side view schematically showing the wafer backside cleaning step of the wafer processing method shown in FIG12 in partial cross-section. FIG17 is a perspective view schematically showing the wafer after the transfer step of the wafer processing method shown in FIG12. FIG18 is a side view schematically showing the protective film removal step of the wafer processing method shown in FIG12 in partial cross-section.

[0050] Furthermore, in Figures 12, 13, 14, 15, 16, 17, and 18, the same symbols are used for parts identical to those in Embodiment 1, and the descriptions are omitted. As shown in Figure 12, the wafer processing method of Embodiment 2 includes: a protective film formation step 1001, a laser processing tank formation step 1002, a wafer placement step 1004, a dicing step 1005, a wafer backside cleaning step 1010, a transfer step 1011, and a protective film removal step 1003. In the wafer processing method of Embodiment 2, the protective film formation step 1001 and the laser processing tank formation step 1002 are the same as those in Embodiment 1.

[0051] Similar to Embodiment 1, the wafer placement step 1004 of the wafer processing method in Embodiment 2 is performed after the laser processing tank formation step 1002 and before the cutting step 1005. This involves attaching a thin sheet, i.e., the resin sheet 14 shown in FIG. 13, to the front side 3 of the wafer 1, and filling a portion of the resin sheet 14 into the laser processing tank 35. Furthermore, in Embodiment 2, as shown in FIG. 14, in the wafer placement step 1004, a resin sheet 14 having only a substrate layer 141 and no adhesive paste layer is used as a thin sheet and is attached to the front side 3 of the wafer 1 through a protective film 25.

[0052] The substrate layer 141 is made of a flexible and non-adhesive thermoplastic resin. The thermoplastic resin constituting the substrate layer 141, i.e. the resin sheet 14, is made of polyester resins such as polyethylene terephthalate and polyethylene naphthalate, or polyolefin resins such as polyethylene, polypropylene, and polystyrene.

[0053] In Embodiment 2, in the wafer placement step 1004, the back side 7 of the wafer 1 and the annular frame 15 are placed on a heated holding stage with a diameter larger than that of the wafer 1, and a circular resin sheet 14 with a diameter larger than that of the wafer 1 is placed on the front side 3 of the wafer 1 and the annular frame 15. In Embodiment 2, in the wafer placement 1004, while heating the resin sheet 14 through the wafer 1 and pressing the resin sheet 14 onto the wafer 1 with rollers, the resin sheet 14 is softened. As shown in FIG. 13, the resin sheet 14 is heat-pressed to the front side 3 of the wafer 1 through the protective film 25, and the annular frame 15 is heat-pressed to the outer edge of the resin sheet 14. In Embodiment 2, the wafer placement step 1004 involves peeling the adhesive film 10 from the back side 7 of the wafer 1.

[0054] Furthermore, in Embodiment 2, during the wafer placement step 1004, the resin wafer 14 is heated while being pressed onto the wafer 1, so as shown in FIG. 14, a portion of the resin wafer 14 is filled into the laser processing tank 35. Thus, in Embodiment 2, during the wafer placement step 1004, the resin wafer 14 is heated and adhered to the protective film 25, thereby adhering the resin wafer 14 to the front side 3 of the wafer 1.

[0055] Furthermore, in Embodiment 2, during the sheet placement step 1004, there is a concern that if the heating temperature of the resin sheet 14 exceeds the melting point of the resin sheet 14, the shape of the resin sheet 14 will become unsustainable. Therefore, it is desirable to heat the resin sheet 14 to a temperature above the softening point and below the melting point. In addition, during heating, the heat source can also be set to a temperature higher than the melting point of the resin sheet 14.

[0056] In Embodiment 2, in the sheet arrangement step 1004, it is desirable to heat the resin sheet 14 to a temperature 20°C or higher below its melting point and below its melting point. For example, in Embodiment 2, in the sheet arrangement step 1004, if the resin sheet 14 is made of polyethylene terephthalate, it is desirable to heat the resin sheet 14 to a temperature of 240°C or higher and 260°C or lower; if the resin sheet 14 is made of polyethylene naphthalate, it is desirable to heat the resin sheet 14 to a temperature of 245°C or higher and 265°C or lower; if the resin sheet 14 is made of polypropylene, it is desirable to heat the resin sheet 14 to a temperature of 145°C or higher and 165°C or lower; and if the resin sheet 14 is made of polystyrene, it is desirable to heat the resin sheet 14 to a temperature of 220°C or higher and 240°C or lower.

[0057] Furthermore, in this invention, during the wafer placement step 1004, the back side 7 of the wafer 1 and the annular frame 15 can be placed on a holding stage at room temperature, and a circular resin sheet 14 with a diameter larger than that of the wafer 1 can be placed on the front side 3 of the wafer 1 and the annular frame 15. While pushing the resin sheet 14 with a heating roller that has been heated to a predetermined temperature, the heating roller rotates on the resin sheet 14, thereby performing heat pressing. Furthermore, in this invention, during the wafer placement step 1004, after the resin sheet 14 has been brought into close contact with the wafer 1, the resin sheet 14 can be heat-pressed onto the wafer 1 by using hot air jets from a heating gun or heating from a heating lamp, etc.

[0058] Furthermore, in the present invention, in the sheet placement step 1004, similarly to Embodiment 1, the protective film 12 can also be adhered as a sheet to the front side 3 of the wafer 1.

[0059] Similar to Embodiment 1, the dicing step 1005 of the wafer processing method in Embodiment 2 is performed after the laser processing tank formation step 1002. The dicing blade 54 cuts into the wafer 1 from the back surface 7 of the wafer 1 at a predetermined position along the predetermined dicing line 4 (i.e., the center in the width direction) to a depth reaching the laser processing tank 35, and the dicing blade 54 cuts along the predetermined dicing line 4 to divide the wafer 1. Furthermore, in the dicing step 1005 of the wafer processing method in Embodiment 2, similar to Embodiment 1, cutting fluid is supplied to the processing point where the dicing blade 54 contacts the wafer 1 while the dicing blade 54 cuts the wafer 1.

[0060] In Embodiment 2, in the cutting step 1005, the cutting apparatus 50 causes the cutting blade 54 to cut into the wafer 1 to a depth that reaches the laser processing groove 35 and is shallower than the thickness of the substrate 2 but does not reach the resin sheet 14. Thus, in Embodiment 2, in the cutting step 1005, the cutting blade 54 cuts to a depth that does not completely cut through the resin sheet 14.

[0061] Thus, in the cutting step 1005, since the cutting blade 54 cuts into the center of the width direction of the predetermined dividing line 4 at the aforementioned depth, as shown in FIG15, the laser processing groove 35 is exposed at the bottom of the cutting groove 55 formed by the cutting blade 54, and the predetermined dividing line 4 is divided by the cutting groove 55 and the laser processing groove 35. In the cutting step 1005, all the predetermined dividing lines 4 are cut by the cutting blade 54, forming cutting grooves 55 on all the predetermined dividing lines 4, and the wafer 1 is divided into individual components 5.

[0062] The wafer backside cleaning step 1010 is a step that cleans the backside 7 of wafer 1 after the dicing step 1005. In the wafer backside cleaning step 1010, the cleaning apparatus 60 holds the front side 3 of wafer 1 on the holding surface of the rotary table 61 through the resin sheet 14, and clamps the annular frame 15 with the clamping part 62 provided around the rotary table 61. In the wafer backside cleaning step 1010, as shown in FIG16, the cleaning apparatus 60 supplies cleaning fluid 64 composed of pure water from the cleaning fluid supply nozzle 63 to the center of the backside 7 of wafer 1 while the rotary table 61 is rotating around the axis. The cleaning fluid 64 supplied to the backside 7 of wafer 1 is cleaned by the centrifugal force generated by the rotation of the rotary table 61, flowing from the center side to the outer periphery on the backside 7 of wafer 1, and removing dicing chips and the like from the backside 7 of wafer 1. In addition, the component layer 6 is omitted in FIG16.

[0063] Transfer step 1011 is the step of attaching the adhesive film 17 shown in FIG. 17 to the back side 7 of the wafer 1 and removing the resin 14 from the front side 3 of the wafer 1 after performing the cutting step 1005. In transfer step 1011, similar to the protective adhesive film 12, the adhesive film 17 is attached to the back side 7 of the wafer 1, and the adhesive film 17 has a substrate layer and a paste layer laminated on the substrate layer.

[0064] In transfer step 1011, as shown in FIG17, a paste layer of a disc-shaped adhesive film 17 with a diameter larger than that of wafer 1 is adhered to the back side 7 of wafer 1, and an annular frame 18 is adhered to the outer edge of the adhesive film 17, thereby supporting wafer 1, and the resin sheet 14 is peeled off from the front side 3. Furthermore, in this invention, the adhesive film 17 may also be similar to the resin sheet 14, having only a substrate layer and no paste layer.

[0065] The protective film removal step 1003 of the wafer processing method in Embodiment 2 is a step of removing the protective film 25 from the front side 3 of the wafer 1 after performing the transfer step 1011. In the protective film removal step 1003, the cleaning device 40 attracts and holds the back side 7 of the wafer 1 on the holding surface of the rotary table 41 through the adhesive film 17, and clamps the annular frame 18 with the clamping part 42. As shown in FIG18, similarly to Embodiment 1, the protective film 25 and the debris are removed from the front side 3 of the wafer 1. In addition, the component layer 6 is omitted in FIG18.

[0066] In the wafer processing method of Embodiment 2, a laser processing groove 35 is formed by irradiating the front side 3 of the wafer 1 with a laser beam 33, and a cutting blade 54 is used to cut the predetermined dividing line 4 from the back side 7 of the wafer 1. Therefore, similar to Embodiment 1, the effect of increasing the number of components 5 on each wafer 1 is achieved.

[0067] Furthermore, in the wafer processing method of Embodiment 2, in the wafer placement step 1004, since a portion of the resin wafer 14 is pre-filled in the laser processing tank 35, in the cutting step 1005, the cutting fluid containing cutting chips can be prevented from winding around the front side 3 of the wafer 1 and adhering to the front side 3.

[0068] Furthermore, in the wafer processing method of Embodiment 2, in the protective film forming step 1001 before the laser processing tank forming step 1002, since a protective film 25 is formed on the front side 3 of the wafer 1, it is possible to suppress the attachment of debris to the front side 3 of the wafer 1.

[0069] Furthermore, in the wafer processing method of Embodiment 2, since a protective film 25 is left in advance in the dicing step 1005, in addition to further reducing the concern that dirt may adhere to the front side 3 of the wafer 1 during dicing, the concern that dirt may adhere to the front side 3 of the wafer 1 in the transfer step 1011 can also be suppressed.

[0070] Furthermore, in the wafer processing method of Embodiment 2, in the wafer placement step 1004, similarly to Embodiment 1, when the protective film 12 is adhered to the front side 3 of the wafer 1, since the protective film 12 is adhered to the front side 3 through the protective film 25, the concern that a portion of the paste layer 122 of the protective film 12 may adhere to and remain on the front side 3 of the wafer 1 can be suppressed.

[0071] Furthermore, the present invention is not limited to the above-described embodiments. That is, various modifications and implementations can be made without departing from the spirit of the present invention. In addition, in the wafer placement step 1004 of the wafer processing method of Embodiment 1, the resin sheet 14 shown in Embodiment 2 can also be adhered as a sheet to the front side 3 of the wafer 1. [Simplified Explanation of the Diagram]

[0014] Figure 1 is a perspective view of the wafer to be processed in the wafer processing method of Embodiment 1. Figure 2 is a flowchart showing the process of the wafer processing method of Embodiment 1. Figure 3 is a side view schematically showing the protective film formation step of the wafer processing method shown in Figure 2 in partial cross-section. Figure 4 is a cross-sectional view schematically showing the main part of the wafer after the protective film formation step of the wafer processing method shown in Figure 2. Figure 5 is a side view schematically showing the laser processing tank formation step of the wafer processing method shown in Figure 2 in partial cross-section. Figure 6 is a cross-sectional view schematically showing the main part of the wafer after the laser processing tank formation step of the wafer processing method shown in Figure 2. Figure 7 is a side view schematically showing the protective film removal step of the wafer processing method shown in Figure 2 in partial cross-section. Figure 8 is a cross-sectional view schematically showing the main part of the sheet, i.e., the protective film, adhered to the front side of the wafer in the sheet placement step of the wafer processing method shown in Figure 2. Figure 9 is a perspective view of the wafer after the wafer placement step in the wafer processing method shown in Figure 2. Figure 10 is a side view schematically showing the dicing step in the wafer processing method shown in Figure 2 in partial cross-section. Figure 11 is a cross-sectional view schematically showing the main portion of the wafer after the dicing step in the wafer processing method shown in Figure 2. Figure 12 is a flowchart showing the wafer processing method of Embodiment 2. Figure 13 is a perspective view of the wafer after the wafer placement step in the wafer processing method shown in Figure 12. Figure 14 is a cross-sectional view schematically showing the main portion of the wafer shown in Figure 13. Figure 15 is a cross-sectional view schematically showing the main portion of the wafer after the dicing step in the wafer processing method shown in Figure 12. Figure 16 is a side view schematically showing the wafer backside cleaning step in the wafer processing method shown in Figure 12 in partial cross-section. Figure 17 is a perspective view of the wafer after the transfer step in the wafer processing method shown in Figure 12. Figure 18 is a side view, schematically showing a partial cross-section, of the protective film removal step in the wafer processing method shown in Figure 12.

Claims

1. A wafer fabrication method comprising forming components on a wafer whose front side is divided into regions by intersecting predetermined dicing lines, and comprising: a laser processing trench forming step, wherein a laser beam of a wavelength having absorption properties on the wafer is irradiated onto the front side of the wafer to form a laser processing trench along the predetermined dicing lines; a dicing step, wherein, after performing the laser processing trench forming step, a dicing blade is inserted from the back side of the wafer to the depth of the laser processing trench while the dicing blade cuts the wafer along the predetermined dicing lines to divide the wafer; and a sheet placement step, wherein, after performing the laser processing trench forming step and before performing the dicing step, a sheet with a thickness greater than the depth of the laser processing trench is adhered to the front side of the wafer and the sheet is filled into the laser processing trench; wherein... In the wafer placement step, the wafer is filled into the laser processing tank, and in the cutting step, the cutting blade cuts into the wafer to a depth that does not reach the wafer.

2. The wafer fabrication method as described in claim 1, wherein, It features: In this cutting step, cutting fluid is supplied to the processing point where the cutting blade contacts the wafer, while the wafer is cut with the cutting blade.

3. The wafer fabrication method as described in claim 2, wherein, The wafer processing method includes: a protective film forming step, in which a protective film is formed on the front side of the wafer before the laser processing tank forming step; and a wafer placement step, in which the wafer is adhered to the protective film. The wafer processing method further includes: a transfer step, in which an adhesive film is adhered to the back side of the wafer and the wafer is removed from the front side of the wafer after the cutting step. And a protective film removal step, which removes the protective film after the transfer step is performed.

4. The wafer processing method as described in claim 2 or 3, wherein, In this cutting step, the cutting blade is made to cut to a depth that does not completely sever the sheet.

5. The wafer processing method as described in claim 1 or 3, wherein, The sheet does not have a paste layer. In the sheet placement step, the sheet is heated and then adhered to the front side of the wafer.

Citation Information

Patent Citations

  • Protection sheet for semiconductor wafer dicing and semiconductor wafer dicing method using it

    JP2008004836A

  • Method of processing substrate

    JP2020031211A

  • Manufacturing method of semiconductor device with metal film

    JP2020077709A

  • Processing method and thermocompression bonding method for workpiece

    JP2020178008A