Equipment for removing scale from steel plates, equipment for manufacturing steel plates, methods for removing scale from steel plates, and methods for manufacturing steel plates.
Patent Information
- Application Number
- TW113139757
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-10-20
- Filing Date
- 2024-10-18
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-10-17
AI Technical Summary
Existing methods for descaling high-grade electromagnetic steel sheets with high Si content face challenges in balancing descaling property and suppressing fracture generation during cold rolling, as they either deteriorate descaling property or increase the risk of dust explosion.
A sequential descaling process involving a first pickling device, a breaking device, and a second pickling device, with the addition of a pickling inhibitor to the second acid solution, and setting the pickling time in the first pickling to 10-30 seconds, along with optional mechanical pre-treatment, to effectively remove scales while minimizing fracture risk.
The method achieves balanced descaling property and suppresses fracture generation during cold rolling, ensuring efficient scale removal without increasing the risk of dust explosion.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a scale removing device for steel plates, a manufacturing device for steel plates, a scale removing method for steel plates, and a manufacturing method for steel plates. Prior Art
[0002] Electromagnetic steel plates mainly used as core materials for electrical machines are roughly divided into non-oriented electromagnetic steel plates and oriented electromagnetic steel plates. In order to reduce iron loss, they usually contain a large amount of Si or Al for increasing the inherent resistance of steel. Generally, the non-oriented electromagnetic steel plates are manufactured as follows: After melting steel adjusted to a specified composition, a slab as a steel raw material is formed by a continuous casting method or the like, and then the slab is hot-rolled. If necessary, hot-rolled sheet annealing, pickling, cold rolling are performed, and final annealing for recrystallization is carried out. Generally, the oriented electromagnetic steel plates are manufactured as follows: After melting steel adjusted to a specified composition, a steel raw material (slab) is formed by a continuous casting method or the like. Thereafter, hot rolling is performed, and if necessary, hot-rolled sheet annealing, pickling, cold rolling are carried out. If necessary, recrystallization annealing and second cold rolling are carried out, primary recrystallization annealing including decarburization annealing is carried out, and after applying an annealing separating agent, final annealing for secondary recrystallization is carried out.
[0003] Hot-rolled sheet annealing is a step of performing homogenization heat treatment on a hot-rolled steel plate (hot-rolled sheet). By performing homogenization heat treatment, insufficient recrystallization of the hot-rolled sheet can be eliminated, or the crystal grains before cold rolling can be coarsened or made uniform, and the texture of the steel plate before cold rolling can be improved to a texture favorable for magnetic properties, or ridging can be suppressed. Therefore, in high-grade electromagnetic steel plates with a large Si addition amount, hot-rolled sheet annealing is mostly carried out.
[0004] Pickling is a step of removing (descaling) the oxide scale from the surface of the steel plate before cold rolling. If cold rolling is carried out on a steel plate in a state where the oxide scale formed on the surface of the steel plate by hot rolling or hot-rolled sheet annealing remains without pickling, the following problems may occur. That is, the oxide scale is pressed into the surface of the steel plate by the rolling roll, or surface defects are caused because the peeled oxide scale adheres to and is transferred to the roll surface, thus significantly damaging the surface quality of the final product. As the acid solution used in the pickling, any one of hydrochloric acid, sulfuric acid, hydrofluoric acid, and a mixed acid obtained by mixing these acids can be used.
[0005] The scale of a hot-rolled steel sheet for an electromagnetic steel sheet containing a large amount of Si or Al includes an outer scale and a sub-scale. The outer scale includes FeO, Fe₃O₄, Fe₂O₃, etc. formed by the diffusion of Fe from the inside of the steel sheet to the outside. The sub-scale includes Si oxides such as SiO₂ or Fe₂SiO₄ or Al₂O₃, etc. formed by the diffusion of oxygen from the outside to the inside of the steel sheet. In particular, it is known that the descaling property of the sub-scale containing SiO₂ or Al₂O₃ is significantly poor. Therefore, in the descaling of a hot-rolled steel sheet for an electromagnetic steel sheet, the descaling property is improved by performing mechanical descaling treatment such as shot peening to mechanically break the scale before pickling.
[0006] However, in a high-grade electromagnetic steel sheet with a high Si content, if hot-rolled plate annealing is carried out to ensure magnetic properties, the grain size becomes large and the embrittlement of the steel sheet becomes a problem. In particular, if the Si content exceeds 2.5 [mass%], twinning deformation occurs on the steel sheet surface due to shot peening for improving descaling property, and there is a problem that faults such as sheet fracture are likely to occur during cold rolling starting from the twinning deformation.
[0007] The following techniques are disclosed in Patent Document 1: reducing the particle diameter of the shot particles projected by shot peening to less than 0.35 [mm] and reducing the energy of the particles colliding with the steel sheet surface, thereby reducing the amount of strain introduced into the steel sheet surface and suppressing twinning deformation. In addition, the following technique is disclosed in Patent Document 2: when shot peening an electromagnetic steel sheet containing 2.5 [mass%] to 3.5 [mass%] of Si, heating the steel sheet temperature Ts according to the Si content so as to satisfy the relational expression of Ts [°C] ≥ 80 × Si [mass%] - 180, thereby suppressing twinning deformation that is likely to occur under low-temperature and high-strain rate conditions. [Prior Art Documents] [Patent Documents]
[0008] [Patent Document 1] Japanese Patent Laid-Open No. 61-126919 [Patent Document 2] Japanese Patent Laid-Open No. 62-048463 Summary of the Invention
[0009] [Problems to be Solved by the Invention]
[0010] However, in the technology disclosed in Patent Document 1, by making the pellet particle size finer and reducing the collision energy, twin deformation can be suppressed. However, conversely, there is a problem of deterioration of descaling property. In addition, in the technology disclosed in Patent Document 2, by increasing the steel plate temperature Ts, twin deformation can be suppressed. However, the higher the Si content, the higher the required steel plate temperature. Therefore, in a steel plate containing 4.0 [mass%] of Si, which is called the rolling limit, the steel plate temperature Ts obtained from the relational expression is 140 [°C]. As a result, there is a problem that the risk of dust explosion caused by pellet particles becomes high. Therefore, in practice, the technologies disclosed in Patent Document 1 and Patent Document 2 are both difficult to apply to actual production.
[0011] The present invention has been made in view of the above problems, and an object thereof is to provide a descaling device for steel plates, a manufacturing device for steel plates, a descaling method for steel plates, and a manufacturing method for steel plates that can achieve both descaling property of steel plates and suppression of fracture generation during cold rolling. [Means for Solving the Problems]
[0012] In order to solve the above problems and achieve the object, (1) The descaling device for steel plates of the present invention is a descaling device for steel plates that removes the scale of the conveyed steel plates, and is characterized in that a first pickling device that performs first pickling on the steel plates using a first acid solution, a breaking device that mechanically breaks the scale, and a second pickling device that performs second pickling on the steel plates using a second acid solution are sequentially arranged from the upstream side in the conveying direction of the steel plates.
[0013] (2) The descaling device for steel plates of the present invention is characterized in that, in the invention of (1) above, a pickling inhibitor is added to the second acid solution.
[0014] (3) The descaling device for steel plates of the present invention is characterized in that, in the invention of (1) or (2) above, a pickling accelerator is added to the first acid solution, and the pickling time in the first pickling is set to 10 [s] to 30 [s].
[0015] (4) The descaling device for steel plates of the present invention is characterized in that, in any one of the inventions of (1) to (3) above, a preliminary breaking device that mechanically breaks the scale is provided on the upstream side of the first pickling device in the conveying direction of the steel plates.
[0016] (5) The manufacturing equipment for the steel plate of the present invention includes: a hot rolling equipment for obtaining a hot rolled plate by hot rolling a steel raw material; a hot rolled plate annealing equipment for performing hot rolled plate annealing on the hot rolled plate as needed; a scale removing equipment for removing the scale of the hot rolled plate or the hot rolled plate that has undergone the hot rolled plate annealing; a cold rolling equipment for obtaining a cold rolled plate by cold rolling the hot rolled plate from which the scale has been removed; and a final annealing equipment for annealing the cold rolled plate to obtain a cold rolled annealed plate. The manufacturing equipment for the steel plate is characterized in that, as the scale removing equipment, a scale removing equipment for the steel plate of any one of the inventions in (1) to (4) above is used.
[0017] (6) The scale removing method for the steel plate of the present invention is characterized in that the steel plate is pickled by a first pickling device that pickles the steel plate after hot rolling with a first acid solution, and a treatment is performed to mechanically break the scale on the surface of the steel plate pickled by the first pickling device by a breaking device, and the steel plate after being treated by the breaking device is pickled using a second acid solution by a second pickling device.
[0018] (7) The scale removing method for the steel plate of the present invention is characterized in that, in the invention of (6) above, a pickling inhibitor is added to the second acid solution.
[0019] (8) The scale removing method for the steel plate of the present invention is characterized in that, in the invention of (6) or (7) above, a pickling accelerator is added to the first acid solution, and the pickling time by the first pickling device is set to 10 [s] to 30 [s].
[0020] (9) The scale removing method for the steel plate of the present invention is characterized in that, in any one of the inventions in (6) to (8) above, a pretreatment breaking device arranged on the upstream side of the first pickling device in the conveying direction of the steel plate is used to perform a treatment of mechanically breaking the scale.
[0021] (10) The manufacturing method for the steel plate of the present invention includes: a hot rolling step for obtaining a hot rolled plate by hot rolling a steel raw material; a hot rolled plate annealing step for performing hot rolled plate annealing on the hot rolled plate as needed; a scale removing step for removing the scale of the hot rolled plate or the hot rolled plate that has undergone the hot rolled plate annealing; a cold rolling step for obtaining a cold rolled plate by cold rolling the hot rolled plate from which the scale has been removed; and a final annealing step for annealing the cold rolled plate to obtain a cold rolled annealed plate. The manufacturing method for the steel plate is characterized in that, in the scale removing step, a scale removing method for the steel plate of any one of the inventions in (6) to (9) above is used. [Advantages of the Invention]
[0022] The descaling equipment for steel plates, the manufacturing equipment for steel plates, the descaling method for steel plates, and the manufacturing method for steel plates of the present invention achieve the effect of being able to balance the descaling property of the steel plate and the suppression of crack generation during cold rolling. Brief Description of the Drawings
[0023] FIG. 1 is a diagram showing the schematic structure of the descaling equipment for a steel strip according to an embodiment. FIG. 2 is a schematic diagram showing the external scale and internal scale of the scale existing on the surface of the steel strip. Embodiment
[0024] Hereinafter, embodiments of the descaling equipment for steel plates, the manufacturing equipment for steel plates, the descaling method for steel plates, and the manufacturing method for steel plates of the present invention will be described. Furthermore, the present invention is not limited by this embodiment. In addition, it is assumed that "steel strip" is included in "steel plate".
[0025] FIG. 1 is a diagram showing the schematic structure of the descaling equipment 10 for the steel strip 1 according to an embodiment. The descaling equipment 10 removes the scale of the steel strip 1 conveyed along the conveying direction shown by the arrow in FIG. 1. The descaling equipment 10 is configured to be sequentially provided with a payoff reel 2, a welder 3, a first pickling device 4, a breaking device 5, a second pickling device 6, and a tension reel 7 in the conveying direction of the steel strip 1 from the upstream side. The payoff reel 2 rewinds the coil of the hot-rolled steel strip on the input side and sends out the steel strip 1. The welder 3 welds the preceding steel strip 1 and the subsequent steel strip 1. The first pickling device 4 performs first pickling on the steel strip 1 using an acid solution (first acid solution) to remove the easily pickled scale on the surface of the steel strip. The breaking device 5 mechanically breaks the film-like difficult-to-pickle scale on the surface of the steel strip. The second pickling device 6 performs second pickling on the steel strip 1 using an acid solution (second acid solution) to remove the broken difficult-to-pickle scale remaining on the surface of the steel strip along with the dissolution of the base iron. The tension reel 7 winds the steel strip 1 that has undergone second pickling onto a coil.
[0026] Furthermore, in the descaling equipment 10 of the embodiment, a preliminary breaking device for mechanically breaking the scale on the surface of the steel strip may also be provided on the upstream side of the first pickling device 4 and the downstream side of the welder 3 in the conveying direction of the steel strip 1. In addition, as the preliminary breaking device and the breaking device 5, for example, any one of a shot blasting machine, a tension leveling machine, a grinding brush, and a laser cleaning device can be used.
[0027] In addition, in FIG. 1, the steel strip 1 formed by coiling a flat plate of metal, which is a steel material, i.e., a steel plate, into a coil shape is an object to be manufactured (scale removal object), but the object to be manufactured (scale removal object) is not limited to the steel strip 1. For example, the object to be manufactured (scale removal object) may be a flat plate of metal, which is a steel material, i.e., a steel plate. That is, the scale removal device 10 can be used in a method for removing scale from a steel plate in a broad sense.
[0028] Generally, in a scale removal device for a steel plate, after mechanical descaling treatment for mechanically destroying the scale on the surface of the steel plate by a destruction device, the scale is removed by pickling performed by a pickling device.
[0029] The inventors of the present application have repeatedly made efforts in research, and as a result, it has been found that, as shown in FIG. 2, the scale 20 on the surface of the steel plate has a layered structure including an outer scale 21 and an inner scale 22, and the film-like inner scale 222 included in the inner scale 22 exists in a manner covering the base iron 23.
[0030] Here, the outer scale 21 is an iron-based scale generated on the surface of the base iron, which is generally called black scale, and is mainly generated by external oxidation during hot rolling or hot rolling plate annealing, and is a scale soluble in acid mainly composed of FeO, Fe 3O 4, Fe 2O 3, Fe 2SiO 4, etc. At a position closer to the inner layer side than the outer scale 21, an inner scale 22 is generated, and the generation behavior of which is restricted by the diffusion of oxygen. The scale caused by internal oxidation during hot rolling or hot rolling plate annealing is island-like inner scale 221 and film-like inner scale 222. The island-like inner scale 221 exists in an island shape in the metallic iron 223 and is mainly composed of FeO, Fe 2SiO 4, SiO 2, Al 2O 3, FeAl 2O 3, etc. In the island-like inner scale 221, oxides soluble in acid and oxides insoluble in acid are mixedly present, but since the metallic iron 223 itself is soluble in acid, for the oxides insoluble in acid, they can also be peeled off and removed by acid treatment. The film-like inner scale 222 includes amorphous oxides such as SiO 2, Al 2O 3, FeAl 2O 4, Si, and Al. These oxides generated on the innermost layer side with a low oxygen potential are oxides with a very strong binding force to oxygen, so they are insoluble in acid. In addition, the film-like inner scale 222 is formed in a film shape covering the base iron 23, so it cannot be peeled off by dissolving the base iron 23 by acid treatment.
[0031] Then, first, by the first pickling performed by the first pickling device 4, the easily acid-soluble outer scale 21 and the metal iron 223 other than the membranous inner scale 222 in the inner scale 22 (island-shaped inner scale 221 and metal iron 223) are removed. Subsequently, the membranous inner scale 222 is broken by mechanical descaling treatment performed by the breaking device 5 such as shot peening. Then, by the second pickling performed by the second pickling device 6, the remaining membranous inner scale 222 is removed as the base iron 23 dissolves. Thereby, the inventors of the present application have found that it is possible to effectively remove the scale 20 on the surface of the steel sheet while suppressing plate breakage during cold rolling.
[0032] Therefore, in the scale removing apparatus 10 of the embodiment, in the conveying direction of the steel strip 1, the first pickling device 4 and the second pickling device 6 are respectively provided on the upstream side and the downstream side of the breaking device 5. Moreover, in the scale removing apparatus 10 of the embodiment, the scale of the steel strip 1 is removed by pickling (first pickling and second pickling) performed by the first pickling device 4 and the second pickling device 6.
[0033] Next, an example of the manufacturing method of the steel strip 1 of the embodiment will be described. Generally speaking, the manufacturing method of the steel strip 1 of the embodiment is a method of manufacturing the steel strip 1 by sequentially performing a hot rolling step, an optional hot rolled plate annealing step, a scale removing step, a cold rolling step, and a final annealing step on a steel raw material.
[0034] 〈Steel raw material〉 The composition of the steel raw material is not particularly limited. The scale removing method of the embodiment is particularly effective for descaling a steel strip (electromagnetic steel sheet) with a high Si content (for example, containing 1.0 [mass%] or more of Si) that easily forms a firm membranous scale, but can also be preferably applied to a steel strip with a low Si content. The melting method of the steel raw material is not particularly limited, and a known melting method using a converter or an electric furnace can be adopted. Furthermore, in terms of productivity and other issues, it is preferably made into a slab (steel raw material) by continuous casting after melting, but can also be made into a slab (steel raw material) by a known casting method such as ingot-block rolling or thin slab continuous casting.
[0035] 〈Hot rolling step〉 The hot rolling step is a step of obtaining a hot rolled sheet by subjecting a steel raw material to hot rolling. The hot rolling step is not particularly limited as long as it is a step of heating the steel raw material, performing hot rolling, and obtaining a hot rolled sheet of a specified size, and a common hot rolling step can be applied. As a common hot rolling step, for example, the following hot rolling step can be exemplified: heating the steel raw material to a temperature of 1000 [°C] or higher and 1200 [°C] or lower. Then, hot rolling is performed on the heated steel raw material at a final rolling output side temperature of 800 [°C] or higher and 950 [°C] or lower, cooling is performed after hot rolling is completed, and winding is performed at a winding temperature of 400 [°C] or higher and 700 [°C] or lower, thereby producing a hot rolled sheet having a specified size and shape.
[0036] 〈Hot rolled sheet annealing step〉 The hot rolled sheet annealing step is a step of annealing the hot rolled sheet by heating the hot rolled sheet and holding it at a high temperature. The hot rolled sheet annealing step is not particularly limited, and a common hot rolled sheet annealing step can be applied. Furthermore, this step is not essential and can also be omitted.
[0037] 〈Pickling step〉 The pickling step is a step of subjecting the steel sheet to various treatments including pickling the steel sheet after the hot rolled sheet annealing step or, in the case of omitting the hot rolled sheet annealing step, pickling the hot rolled sheet. The pickling step is performed using the scale removing device 10 of the embodiment.
[0038] 〈Cold rolling step〉 The cold rolling step is a step of subjecting the pickled sheet that has undergone the pickling step to cold rolling. The cold rolling step is not particularly limited as long as it is a step capable of reducing the pickled steel sheet to a desired sheet thickness, and a common cold rolling step can be applied. For example, the following cold rolling step can be exemplified: performing single-pass rolling or multi-pass rolling under the conditions that the reduction ratio in each pass is 10 [%] to 40 [%] and the strain rate is 10 [s -1] to 1000 [s -1] to produce a cold rolled sheet having a specified size and shape. Additionally, a cold rolled sheet having a specified size and shape can also be produced by performing cold rolling two or more times with an intermediate annealing step therebetween as needed. In this case, the conditions of the intermediate annealing step are not particularly limited, and a common intermediate annealing step can be applied.
[0039] 〈Final annealing step〉 The final annealing step is a step of annealing the cold-rolled sheet that has undergone the cold rolling step. The final annealing step is not particularly limited, and a common final annealing step can be applied. For example, the following final annealing step can be exemplified: A cold-rolled annealed sheet is obtained by heating the cold-rolled sheet that has undergone the cold rolling step to an annealing temperature of 700 [°C] or higher and 1050 [°C] or lower and then cooling it. Furthermore, after the final annealing step, an insulating coating is applied to the surface of the cold-rolled annealed sheet, but the method and type of coating are not particularly limited, and a common insulating coating step can be applied.
[0040] The scale removal device 10 of the embodiment can be applied, for example, to the manufacturing equipment of the steel strip 1 for the manufacturing method using the steel strip 1. Moreover, in the manufacturing equipment of the steel strip 1, the scale of the steel strip 1 is removed by the scale removal device 10 to manufacture the steel strip 1. As a result, the steel strip 1 can be manufactured while suppressing fracture caused by twin deformation in cold rolling without causing dust explosion in shot peening and without reducing descaling property. [Examples]
[0041] Hereinafter, the present invention will be specifically described with reference to examples. However, the present invention is not limited to these. For example, regarding the driving conditions of the destruction device for mechanically destroying the film-like difficult-to-pickling scale on the surface of the steel strip, they are reference values and do not limit the present invention. The detailed driving conditions vary depending on the type of the destruction device, the type of the steel strip as the object, or the prior heat treatment. However, the characteristic aspect of the present invention is that after removing the external scale by primary pickling, scale destruction treatment is performed by the destruction device, and as long as the various conditions of primary pickling, secondary pickling, and the destruction device 5 are appropriately adjusted, the optimal values can be found.
[0042] <Manufacture of Steel Strip> First, hot-rolled plate annealing with soaking conditions of 1000 [°C] × 30 [s] was performed on a hot-rolled steel sheet containing C: 0.002 [mass%], Si: 3.7 [mass%], Mn: 0.5 [mass%], and a plate thickness of 2.2 [mm]. Thus, the steel strip 1 for the evaluation experiment of descaling property and cold rollability was manufactured.
[0043] (Evaluation Experiment 1) In Evaluation Experiment 1, a shot peening machine was used as the destruction device 5, and the applicability effect of the first pickling performed by the first pickling device 4 provided on the upstream side of the destruction device 5 in the conveying direction of the steel strip 1 was confirmed. Then, for this purpose, as in Examples 1 to 12 and Comparative Examples 1 to 12, the presence or absence of the first pickling performed by the first pickling device 4, the conditions of shot peening in the destruction device 5, etc. were changed, and an evaluation experiment of descaling property and cold rolling property was conducted.
[0044] Table 1 shows the respective conditions and results of the pickling and rolling experiments in Examples 1 to 12 and Comparative Examples 1 and 2. Furthermore, regarding "scale removal" in Table 1, in terms of descaling property, when scale removal was completed after the second pickling, it was set to "○", and when scale removal was not completed, it was set to "×". In addition, regarding the "fracture generation rate in cold rolling" in Table 1, in terms of cold rolling property, it represents the fracture generation rate when cold rolling was performed after the second pickling to produce a cold rolled sheet.
[0045] [Table 1] (Table 1) No. First Pickling Shot Peening Second Pickling Scale Removal Fracture Generation Rate in Cold Rolling [%] Acid Solution Temperature [°C] Time [s] Particle Velocity [m / s] Projection Density [kg / m 2] Acid Solution Temperature [°C] Time [s] Example 1 Hydrochloric Acid 80 20 10 12.5 Hydrochloric Acid 80 20 ○ 0 Example 2 Hydrochloric Acid 80 20 20 12.5 Hydrochloric acid 80 20 ○ 0 Example 3 Hydrochloric acid 80 20 30 12.5 Hydrochloric acid 80 20 ○ 0 Example 4 Hydrochloric acid 80 20 40 12.5 Hydrochloric acid 80 20 ○ 0 Example 5 Hydrochloric acid 80 20 50 12.5 Hydrochloric acid 80 20 ○ 0 Example 6 Hydrochloric acid 80 20 60 12.5 Hydrochloric acid 80 20 ○ 0 Comparative Example 1 Hydrochloric acid 80 20 100 12.5 Hydrochloric acid 80 20 ○ 25 Example 7 Hydrochloric acid 80 20 10 25 Hydrochloric acid 80 20 ○ 0 Example 8 Hydrochloric acid 80 20 20 25 Hydrochloric acid 80 20 ○ 0 Example 9 Hydrochloric acid 80 20 30 25 Hydrochloric acid 80 20 ○ 0 Example 10 Hydrochloric acid 80 20 40 25 Hydrochloric acid 80 20 ○ 0 Example 11 Hydrochloric acid 80 20 50 25 Hydrochloric acid 80 20 ○ 0 Example 12 Hydrochloric acid 80 20 60 25 Hydrochloric acid 80 20 ○ 0 Comparative Example 2 Hydrochloric acid 80 20 100 25 Hydrochloric acid 80 20 ○ 27
[0046] [Example 1] In Example 1, there is a first pickling performed by the first pickling device 4. As the conditions for the first pickling, the acid solution is set as hydrochloric acid, the temperature of the acid solution is set as 80 [°C], and the pickling time is set as 20 [s]. In addition, in Example 1, as the conditions for shot peening in the destruction device 5, the particle velocity is set as 10 [m / s], and the projection density is set as 12.5 [kg / m2]. In addition, in Example 1, as the conditions for the second pickling performed by the second pickling device 6, the acid solution is set as hydrochloric acid, the temperature of the acid solution is set as 80 [°C], and the pickling time is set as 20 [s]. As a result, in Example 1, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0047] [Example 2] In Example 2, as the conditions for shot peening in the destruction device 5, the particle velocity is set as 20 [m / s], and other than that, the conditions are the same as those in Example 1. As a result, in Example 2, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0048] [Example 3] In Example 3, as the conditions for shot peening in the destruction device 5, the particle velocity is set as 30 [m / s], and other than that, the conditions are the same as those in Example 1. As a result, in Example 3, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0049] [Example 4] In Example 4, as the conditions for shot peening in the destruction device 5, the particle velocity was set to 40 [m / s], and other conditions were the same as those in Example 1. As a result, in Example 4, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0050] [Example 5] In Example 5, as the conditions for shot peening in the destruction device 5, the particle velocity was set to 50 [m / s], and other conditions were the same as those in Example 1. As a result, in Example 5, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0051] [Example 6] In Example 6, as the conditions for shot peening in the destruction device 5, the particle velocity was set to 60 [m / s], and other conditions were the same as those in Example 1. As a result, in Example 6, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0052] [Comparative Example 1] In Comparative Example 1, as the conditions for shot peening in the destruction device 5, the particle velocity was set to 100 [m / s], and other conditions were the same as those in Example 1. As a result, in Comparative Example 1, the scale removal was completed, and the fracture generation rate of cold rolling was 25 [%].
[0053] [Example 7] In Example 7, as the conditions for shot peening in the destruction device 5, the projection density was set to 25 [kg / m 2], and other conditions were the same as those in Example 1. As a result, in Example 7, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0054] [Example 8] In Example 8, as the conditions for shot peening in the destruction device 5, the projection density was set to 25 [kg / m 2], and other conditions were the same as those in Example 2. As a result, in Example 8, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0055] [Example 9] In Example 9, as the conditions for shot peening in the destruction device 5, the projection density was set to 25 [kg / m 2], and other conditions were the same as those in Example 3. As a result, in Example 9, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0056] [Example 10] In Example 10, as the conditions for shot peening in the destruction device 5, the projection density was set to 25 [kg / m 2], and other than that, the conditions were the same as those in Example 4. As a result, in Example 10, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0057] [Example 11] In Example 11, as the conditions for shot peening in the destruction device 5, the projection density was set to 25 [kg / m 2], and other than that, the conditions were the same as those in Example 5. As a result, in Example 11, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0058] [Example 12] In Example 12, as the conditions for shot peening in the destruction device 5, the projection density was set to 25 [kg / m 2], and other than that, the conditions were the same as those in Example 6. As a result, in Example 12, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0059] [Comparative Example 2] In Comparative Example 2, as the conditions for shot peening in the destruction device 5, the projection density was set to 25 [kg / m 2], and other than that, the conditions were the same as those in Comparative Example 1. As a result, in Comparative Example 2, the scale removal was completed, and the fracture generation rate in cold rolling was 27 [%].
[0060] As can be seen from Table 1, as in Comparative Example 1 and Comparative Example 2, under the conditions where the first pickling by the first pickling device 4 is carried out and the particle velocity of shot peening in the destruction device 5 is extremely high at 100 [m / s], the scale removal is completed, but the fracture generation rate in cold rolling increases.
[0061] On the other hand, it can be seen that as in Examples 1 to 12, under the conditions where the first pickling by the first pickling device 4 is carried out and the particle velocity of shot peening in the destruction device 5 is low, it is possible to balance scale removal and suppression of fracture generation in cold rolling.
[0062] That is, in Examples 1 to 12, by the first pickling performed by the first pickling device 4, the external scale 21 and the internal scale 22 that are easily pickled on the surface of the steel strip are removed, and the film-like internal scale 222 that is difficult to pickle is exposed to the surface. Moreover, since the mechanical scale breaking treatment is directly performed on the exposed film-like internal scale 222, even if the particle velocity of the shot peening in the breaking device 5 is low, the film-like internal scale 222 can be broken. Therefore, even when the particle velocity of the shot peening in the breaking device 5 is low, by performing the second pickling by the second pickling device 6, the scale removal is completed. Thus, in Examples 1 to 12, even when the mechanical scale breaking treatment by the breaking device 5 is weak, the scale removal is completed, so that the processing damage to the base iron 23 can be suppressed, and the fracture generation rate in cold rolling can be reduced.
[0063] (Evaluation Experiment 2) In Evaluation Experiment 2, in order to confirm the effect of the additive on the pickling acid solution of the second pickling performed by the second pickling device 6, as in Examples 13 to 24, conditions such as the time of the second pickling and the presence or absence of the additive were changed, and an evaluation experiment on descaling property and cold rolling property was conducted. Table 2 shows the respective conditions and evaluation results of Examples 13 to 24 in Evaluation Experiment 2.
[0064] [Table 2] (Table 2) No. First Pickling Shot Peening Second Pickling Scale Removal Fracture in Cold Rolling Generation Rate [%] Acid Solution Temperature [°C] Time [s] Additive Particle Velocity [m / s] Projection Density [kg / m 2] Acid Solution Temperature [°C] Time [s] Additive Example 13 Hydrochloric Acid 80 20 - 30 15 Hydrochloric acid 80 10 - ○ 0 Example 14 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 20 - ○ 0 Example 15 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 30 - ○ 0 Example 16 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 40 - ○ 0 Example 17 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 50 - ○ 0 Example 18 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 60 - ○ 0 Example 19 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 10 Pickling inhibitor ○ 0 Example 20 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 21 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 30 Pickling inhibitor ○ 0 Example 22 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 40 Pickling inhibitor ○ 0 Example 23 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 50 Pickling inhibitor ○ 0 Example 24 Hydrochloric acid 80 20 - 30 15 Hydrochloric acid 80 60 Pickling inhibitor ○ 0
[0065] [Example 13] In Example 13, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was set as hydrochloric acid, the temperature of the acid solution was set as 80 [°C], the pickling time was set as 20 [s], and no additive was added. In addition, in Example 13, as the conditions for shot peening in the breaking device 5, the particle velocity was set as 30 [m / s], and the projection density was set as 15 [kg / m 2]. In addition, in Example 13, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was set as hydrochloric acid, the temperature of the acid solution was set as 80 [°C], the pickling time was set as 10 [s], and no additive was added. As a result, in Example 13, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0066] [Example 14] In Example 14, as the conditions for the second pickling performed by the second pickling device 6, the pickling time was set to 20 [s], and other than that, the conditions were the same as those in Example 13. As a result, in Example 14, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0067] [Example 15] In Example 15, as the conditions for the second pickling performed by the second pickling device 6, the pickling time was set to 30 [s], and other than that, the conditions were the same as those in Example 13. As a result, in Example 15, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0068] [Example 16] In Example 16, as the conditions for the second pickling performed by the second pickling device 6, the pickling time was set to 40 [s], and other than that, the conditions were the same as those in Example 13. As a result, in Example 16, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0069] [Example 17] In Example 17, as the conditions for the second pickling performed by the second pickling device 6, the pickling time was set to 50 [s], and other than that, the conditions were the same as those in Example 13. As a result, in Example 17, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0070] [Example 18] In Example 18, as the conditions for the second pickling performed by the second pickling device 6, the pickling time was set to 60 [s], and other than that, the conditions were the same as those in Example 13. As a result, in Example 18, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0071] [Example 19] In Example 19, as the conditions for the second pickling performed by the second pickling device 6, a pickling inhibitor was added to the acid solution, and other than that, the conditions were the same as those in Example 13. As a result, in Example 19, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0072] [Example 20] In Example 20, as the conditions for the second pickling performed by the second pickling device 6, a pickling inhibitor was added to the acid solution, and other than that, the conditions were the same as those in Example 14. As a result, in Example 20, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0073] [Example 21] In Example 21, as the conditions for the second pickling performed by the second pickling device 6, a pickling inhibitor was added to the acid solution, and other than that, the conditions were the same as those in Example 15. As a result, in Example 21, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0074] [Example 22] In Example 22, as the conditions for the second pickling performed by the second pickling device 6, a pickling inhibitor was added to the acid solution, and other than that, the conditions were the same as those in Example 16. As a result, in Example 22, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0075] [Example 23] In Example 23, as the conditions for the second pickling performed by the second pickling device 6, a pickling inhibitor was added to the acid solution, and other than that, the conditions were the same as those in Example 17. As a result, in Example 23, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0076] [Example 24] In Example 24, as the conditions for the second pickling performed by the second pickling device 6, a pickling inhibitor was added to the acid solution, and other than that, the conditions were the same as those in Example 18. As a result, in Example 24, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0077] As can be seen from Table 2, as in Examples 13 to 24, as the conditions for the second pickling performed by the second pickling device 6, regardless of whether a pickling inhibitor is added to the acid solution, even if the time of the second pickling is increased, it is possible to balance scale removal and suppression of fracture generation in cold rolling.
[0078] (Evaluation Experiment 3) In Evaluation Experiment 3, as in Examples 25 to 41 and Comparative Example 3, the effects of additives on the acid solution for the first pickling were confirmed, and the applicability of preliminary destruction, which mechanically destroys the scale on the surface of the steel strip before the first pickling, was confirmed. Then, for this purpose, the conditions such as the time of the first pickling, the presence or absence of additives, and the presence or absence of preliminary destruction were changed, and evaluation experiments on descaling properties and cold rolling properties were conducted. Table 3 shows the respective conditions and evaluation results of Examples 25 to 41 and Comparative Example 3 in Evaluation Experiment 3. Furthermore, in Evaluation Experiments 1 to 5, except for Evaluation Experiment 3, preliminary destruction was not carried out.
[0079] [Table 3] (Table 3) No. Shot peening (preliminary destruction) First pickling Shot peening Second pickling Scale Removal Cold rolling fracture Generation rate [%] Particle velocity [m / s] Projection density [kg / m 2] Acid solution Temperature [°C] Time [s] Additive Particle velocity [m / s] Projection density [kg / m 2] Acid solution Temperature [°C] Time [s] Additive Comparative Example 3 - - Hydrochloric acid 80 5 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor × 0 Example 25 - - Hydrochloric acid 80 10 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 26 - - Hydrochloric acid 80 15 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 27 - - Hydrochloric acid 80 20 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 28 - - Hydrochloric acid 80 25 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 29 - - Hydrochloric acid 80 30 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 30 - - Hydrochloric acid 80 5 Pickling accelerator 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 31 - - Hydrochloric acid 80 10 Pickling accelerator 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 32 - - Hydrochloric acid 80 15 Pickling accelerator 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 33 - - Hydrochloric acid 80 20 Pickling accelerator 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 34 - - Hydrochloric acid 80 25 Pickling accelerator 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 35 - - Hydrochloric acid 80 30 Pickling accelerator 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 36 30 10 Hydrochloric acid 80 5 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 37 30 10 Hydrochloric acid 80 10 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 38 30 10 Hydrochloric acid 80 15 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 39 30 10 Hydrochloric acid 80 20 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 40 30 10 Hydrochloric acid 80 25 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0 Example 41 30 10 Hydrochloric acid 80 30 - 30 10 Hydrochloric acid 80 20 Pickling inhibitor ○ 0
[0080] [Comparative Example 3] In Comparative Example 3, the preliminary destruction treatment was not carried out before the first pickling by the first pickling device 4. As the conditions for the first pickling by the first pickling device 4, the acid solution was set as hydrochloric acid, the temperature of the acid solution was set as 80 [°C], the pickling time was set as 5 [s], and no additive was added. Further, in Comparative Example 3, as the conditions for shot peening in the destruction device 5, the particle velocity was set as 30 [m / s], and the projection density was set as 10 [kg / m2]. Further, in Comparative Example 3, as the conditions for the second pickling by the second pickling device 6, the acid solution was set as hydrochloric acid, the temperature of the acid solution was set as 80 [°C], the pickling time was set as 20 [s], and a pickling inhibitor was added as an additive. As a result, in Comparative Example 3, the scale removal was not completed, and the fracture generation rate of cold rolling was 0 [%].
[0081] [Example 25] In Example 25, before the first pickling by the first pickling device 4, no preliminary destruction treatment was carried out. As the conditions for the first pickling by the first pickling device 4, the acid solution was set to hydrochloric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 10 [s], and no additives were added. In addition, in Example 25, as the conditions for shot peening in the destruction device 5, the particle velocity was set to 30 [m / s], and the projection density was set to 10 [kg / m 2]. In addition, in Example 25, as the conditions for the second pickling by the second pickling device 6, the acid solution was set to hydrochloric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 20 [s], and a pickling inhibitor was added as an additive. As a result, in Example 25, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0082] [Example 26] In Example 26, as the conditions for the first pickling by the first pickling device 4, the pickling time was set to 15 [s], and other than that, the same conditions as in Example 25 were set. As a result, in Example 26, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0083] [Example 27] In Example 27, as the conditions for the first pickling by the first pickling device 4, the pickling time was set to 20 [s], and other than that, the same conditions as in Example 25 were set. As a result, in Example 27, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0084] [Example 28] In Example 28, as the conditions for the first pickling by the first pickling device 4, the pickling time was set to 25 [s], and other than that, the same conditions as in Example 25 were set. As a result, in Example 28, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0085] [Example 29] In Example 29, as the conditions for the first pickling by the first pickling device 4, the pickling time was set to 30 [s], and other than that, the same conditions as in Example 25 were set. As a result, in Example 29, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0086] [Example 30] In Example 30, as the conditions for the first pickling performed by the first pickling device 4, the pickling time was set to 10 [s], and a pickling accelerator was added as an additive to the pickling solution. Other than that, the conditions were the same as those in Example 25. As a result, in Example 30, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0087] [Example 31] In Example 31, as the conditions for the first pickling performed by the first pickling device 4, a pickling accelerator was added as an additive to the pickling solution. Other than that, the conditions were the same as those in Example 25. As a result, in Example 31, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0088] [Example 32] In Example 32, as the conditions for the first pickling performed by the first pickling device 4, a pickling accelerator was added to the pickling solution. Other than that, the conditions were the same as those in Example 26. As a result, in Example 32, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0089] [Example 33] In Example 33, as the conditions for the first pickling performed by the first pickling device 4, a pickling accelerator was added to the pickling solution. Other than that, the conditions were the same as those in Example 27. As a result, in Example 33, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0090] [Example 34] In Example 34, as the conditions for the first pickling performed by the first pickling device 4, a pickling accelerator was added to the pickling solution. Other than that, the conditions were the same as those in Example 28. As a result, in Example 34, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0091] [Example 35] In Example 35, as the conditions for the first pickling performed by the first pickling device 4, a pickling accelerator was added to the pickling solution. Other than that, the conditions were the same as those in Example 29. As a result, in Example 35, the scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0092] [Example 36] In Example 36, shot peening as a preliminary destruction treatment is performed before the first pickling by the first pickling device 4. As conditions for the shot peening, the particle velocity is set to 30 [m / s] and the projection density is set to 10 [kg / m2]. Further, in Example 36, as conditions for the first pickling by the first pickling device 4, the acid solution is hydrochloric acid, the temperature of the acid solution is set to 80 [°C], the pickling time is set to 5 [s], and no additives are added. Further, in Example 36, as conditions for the shot peening in the destruction device 5, the particle velocity is set to 30 [m / s] and the projection density is set to 10 [kg / m2]. Further, in Example 36, as conditions for the second pickling by the second pickling device 6, the acid solution is hydrochloric acid, the temperature of the acid solution is set to 80 [°C], the pickling time is set to 20 [s], and a pickling inhibitor is added as an additive to the acid solution. As a result, in Example 36, the scale removal is completed and the fracture generation rate of cold rolling is 0 [%].
[0093] [Example 37] In Example 37, shot peening as a preliminary destruction treatment is performed before the first pickling by the first pickling device 4. As conditions for the shot peening, the particle velocity is set to 30 [m / s] and the projection density is set to 10 [kg / m2], and other than that, the same conditions as in Example 25 are set. As a result, in Example 37, the scale removal is completed and the fracture generation rate of cold rolling is 0 [%].
[0094] [Example 38] In Example 38, shot peening as a preliminary destruction treatment is performed before the first pickling by the first pickling device 4. As conditions for the shot peening, the particle velocity is set to 30 [m / s] and the projection density is set to 10 [kg / m2], and other than that, the same conditions as in Example 26 are set. As a result, in Example 38, the scale removal is completed and the fracture generation rate of cold rolling is 0 [%].
[0095] [Example 39] In Example 39, shot peening as a preliminary destruction treatment is performed before the first pickling by the first pickling device 4. As conditions for the shot peening, the particle velocity is set to 30 [m / s] and the projection density is set to 10 [kg / m2], and other than that, the same conditions as in Example 27 are set. As a result, in Example 39, the scale removal is completed and the fracture generation rate of cold rolling is 0 [%].
[0096] [Example 40] In Example 40, shot peening as a preliminary destruction treatment was performed before the first pickling by the first pickling device 4. As conditions for the shot peening, the particle velocity was set to 30 [m / s] and the projection density was set to 10 [kg / m 2]. Other than this, the conditions were the same as those in Example 28. As a result, in Example 40, scale removal was completed and the fracture generation rate in cold rolling was 0 [%].
[0097] [Example 41] In Example 41, shot peening as a preliminary destruction treatment was performed before the first pickling by the first pickling device 4. As conditions for the shot peening, the particle velocity was set to 30 [m / s] and the projection density was set to 10 [kg / m 2]. Other than this, the conditions were the same as those in Example 29. As a result, in Example 41, scale removal was completed and the fracture generation rate in cold rolling was 0 [%].
[0098] From Table 3, it can be seen that under the conditions of Comparative Example 3, scale removal was not completed. That is, it can be seen that when no mechanical preliminary destruction treatment of the scale was performed before the first pickling by the first pickling device 4, no pickling accelerator was added to the acid solution used in the first pickling by the first pickling device 4, and the pickling time of the first pickling was 5 [s], scale removal was not completed. The reason is considered to be that a part of the easily pickled scale such as the external scale was not removed by the preliminary destruction treatment (shot peening), and in addition, the pickling time of the first pickling was short, so the removal of the easily pickled scale such as the external scale was not completed. Therefore, the inner layer of film-like difficult-to-pickle scale was not exposed, and the mechanical destruction did not fully play its role.
[0099] In addition, from Table 3, it can be seen that under the conditions of Examples 30 to 35, scale removal was completed. That is, it can be seen that when no mechanical preliminary destruction treatment of the scale was performed before the first pickling by the first pickling device 4, a pickling accelerator was added to the acid solution used in the first pickling by the first pickling device 4, and the pickling time of the first pickling was 5 [s] or more, scale removal was completed. The reason is considered to be that due to the effect of the pickling accelerator, even if the pickling time of the first pickling was as short as 5 [s] as in Example 30, the removal of the easily pickled scale such as the external scale was completed in advance.
[0100] In addition, as can be seen from Table 3, under the conditions of Examples 36 to 41, scale removal was completed. That is, it can be seen that scale removal was completed under the conditions that a preliminary destruction treatment (shot peening) was carried out before the first pickling by the first pickling device 4, no pickling accelerator was added to the acid solution used in the first pickling by the first pickling device 4, and the pickling time of the first pickling was 5 [s] or more. The reason is considered to be that a part of the easily pickled scale such as the external scale was removed by the preliminary destruction treatment (shot peening). In addition, by introducing cracks into the remaining easily pickled scale, the reactivity with the acid solution was improved, so that even if the pickling time of the first pickling was as short as 5 [s] as in Example 36, the removal of the easily pickled scale was completed in advance.
[0101] (Evaluation Experiment 4) In Evaluation Experiment 4, a grinding brush was used as the destruction device 5, and the applicability of the first pickling performed by the first pickling device 4 provided on the upstream side of the destruction device 5 in the conveyance direction of the steel strip 1 was confirmed. Then, for this purpose, as in Examples 42 to 47, the conditions of the grinding brush in the destruction device 5 carried out after the first pickling by the first pickling device 4 were changed, and evaluation experiments on descaling property and cold rolling property were carried out. Table 4 shows the respective conditions and results of the pickling and rolling experiments in Examples 42 to 47.
[0102] [Table 4] (Table 4) No. First Pickling Grinding Brush Second Pickling Scale Removal Fracture Generation Rate [%] of Cold Rolling Acid Solution Temperature [°C] Time [s] Torque [Nm] per Plate Width of 1000 [mm] Acid Solution Temperature [°C] Time [s] Example 42 Hydrochloric Acid 80 20 500 Hydrochloric Acid 80 20 ○ 0 Example 43 Hydrochloric acid 80 20 750 Hydrochloric acid 80 20 ○ 0 Example 44 Hydrochloric acid 80 20 1000 Hydrochloric acid 80 20 ○ 0 Example 45 Hydrochloric acid 80 20 1250 Hydrochloric acid 80 20 ○ 0 Example 46 Hydrochloric acid 80 20 1500 Hydrochloric acid 80 20 ○ 0 Example 47 Hydrochloric acid 80 20 1750 Hydrochloric acid 80 20 ○ 0
[0103] [Example 42] In Example 42, there is a first pickling performed by the first pickling device 4. As the conditions for the first pickling, the acid solution is set to hydrochloric acid, the temperature of the acid solution is set to 80 [°C], and the pickling time is set to 20 [s]. In addition, in Example 42, as the conditions for the grinding brush in the breaking device 5, the torque per 1000 [mm] of plate width is set to 500 [Nm]. In addition, in Example 42, as the conditions for the second pickling performed by the second pickling device 6, the acid solution is set to hydrochloric acid, the temperature of the acid solution is set to 80 [°C], and the pickling time is set to 20 [s]. As a result, in Example 42, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0104] [Example 43] In Example 43, as the conditions for the grinding brush in the breaking device 5, the torque per 1000 [mm] of plate width is set to 750 [Nm], and other than that, the conditions are the same as those in Example 42. As a result, in Example 43, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0105] [Example 44] In Example 44, as the conditions for the grinding brush in the breaking device 5, the torque per 1000 [mm] of plate width is set to 1000 [Nm], and other than that, the conditions are the same as those in Example 42. As a result, in Example 44, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0106] [Example 45] In Example 45, as the conditions for the grinding brush in the breaking device 5, the torque per 1000 [mm] of plate width is set to 1250 [Nm], and other than that, the conditions are the same as those in Example 42. As a result, in Example 45, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0107] [Example 46] In Example 46, as the conditions for the grinding brush in the breaking device 5, the torque per 1000 [mm] of plate width is set to 1500 [Nm], and other than that, the conditions are the same as those in Example 42. As a result, in Example 46, the scale removal is completed, and the fracture generation rate of cold rolling is 0 [%].
[0108] [Example 47] In Example 47, as the conditions for the grinding brush in the breaking device 5, the torque per plate width of 1000 [mm] was set to 1750 [Nm], and other than that, the conditions were the same as those in Example 42. As a result, in Example 47, scale removal was completed, and the fracture generation rate in cold rolling was 0 [%].
[0109] As can be seen from Table 4, as in Examples 42 to 47, when the first pickling by the first pickling device 4 is carried out, regardless of the magnitude of the torque per plate width of 1000 [mm] as the conditions for the grinding brush in the breaking device 5, it is possible to balance scale removal and suppression of fracture generation in cold rolling.
[0110] (Evaluation Experiment 5) Next, as Evaluation Experiment 5, the effects of the conditions of the acid solution (type, temperature, and time) or the type of the breaking device 5 (shot peening machine, tension leveler, grinding brush, and laser cleaning device) were confirmed. Then, for this purpose, evaluation experiments on descaling properties and cold rolling properties were carried out according to the conditions (Examples 48 to 63 and Comparative Examples 4 to 7) in which the acid solution and the breaking device 5 were changed. Table 5 shows the respective conditions and evaluation results of Examples 48 to 63 and Comparative Examples 4 to 7 in Evaluation Experiment 5.
[0111] [Table 5] (Table 5) No. First Pickling Breaking Device Second Pickling Scale Removal Fracture in Cold Rolling Generation Rate [%] Acid Solution Temperature [°C] Time [s] Additive Type Acid Solution Temperature [°C] Time [s] Additive Example 48 Hydrochloric Acid 90 20 Pickling Accelerator Shot Peening Machine Hydrochloric acid 90 20 Pickling inhibitor ○ 0 Example 49 Hydrochloric acid 95 20 Pickling accelerator Tension leveling machine Hydrochloric acid 95 20 Pickling inhibitor ○ 0 Example 50 Hydrochloric acid 85 20 Pickling accelerator Grinding brush Hydrochloric acid 85 20 Pickling inhibitor ○ 0 Example 51 Hydrochloric acid 75 20 Pickling accelerator Laser cleaning device Hydrochloric acid 75 20 Pickling inhibitor ○ 0 Comparative Example 4 Hydrochloric acid 80 20 Pickling accelerator None Hydrochloric acid 80 20 Pickling inhibitor × 2 Example 52 Sulfuric acid 90 20 - Shot peening machine Sulfuric acid 90 15 - ○ 0 Example 53 Sulfuric acid 95 20 - Stretch leveling machine Sulfuric acid 95 15 - ○ 0 Example 54 Sulfuric acid 85 20 - Grinding brush Sulfuric acid 85 15 - ○ 0 Example 55 Sulfuric acid 75 20 - Laser cleaning device Sulfuric acid 75 15 - ○ 0 Comparative Example 5 Sulfuric acid 80 20 - None Sulfuric acid 80 15 - × 3 Example 56 Hydrochloric acid + Nitric acid 90 25 - Shot peening machine Hydrochloric acid + Nitric acid 90 25 - ○ 0 Example 57 Hydrochloric acid + Nitric acid 95 25 - Tension leveling machine Hydrochloric acid + Nitric acid 95 25 - ○ 0 Example 58 Hydrochloric acid + Nitric acid 85 25 - Grinding brush Hydrochloric acid + Nitric acid 85 25 - ○ 0 Example 59 Hydrochloric acid + Nitric acid 75 25 - Laser cleaning device Hydrochloric acid + Nitric acid 75 25 - ○ 0 Comparative Example 6 Hydrochloric acid + Nitric acid 80 25 - None Hydrochloric acid + Nitric acid 80 25 - × 3 Example 60 Hydrochloric acid + hydrofluoric acid 90 15 - Shot peening machine Hydrochloric acid + nitric acid 90 10 - ○ 0 Example 61 Hydrochloric acid + hydrofluoric acid 95 15 - Stretch leveling machine Hydrochloric acid + nitric acid 95 10 - ○ 0 Example 62 Hydrochloric acid + hydrofluoric acid 85 15 - Grinding brush Hydrochloric acid + nitric acid 85 10 - ○ 0 Example 63 Hydrochloric acid + hydrofluoric acid 75 15 - Laser cleaning device Hydrochloric acid + nitric acid 75 10 - ○ 0 Comparative Example 7 Hydrochloric acid + hydrofluoric acid 80 15 - None Hydrochloric acid + Nitric acid 80 10 - × 2
[0112] [Example 48] In Example 48, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was set to hydrochloric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 20 [s], and a pickling accelerator was added as an additive to the acid solution. In addition, in Example 48, the type of the breaking device 5 was set to a shot peening machine. In addition, in Example 48, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was set to hydrochloric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 20 [s], and a pickling inhibitor was added as an additive to the acid solution. As a result, in Example 48, scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0113] [Example 49] In Example 49, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 95 [°C], the type of the breaking device 5 was set to a tension leveler, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 95 [°C]. Other than that, the conditions were the same as those in Example 48. As a result, in Example 49, scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0114] [Example 50] In Example 50, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 85 [°C], the type of the breaking device 5 was set to a grinding brush, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 85 [°C]. Other than that, the conditions were the same as those in Example 48. As a result, in Example 50, scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0115] [Example 51] In Example 51, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 75 [°C], the type of the destruction device 5 was set to a laser cleaning device, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 75 [°C]. Other than that, the conditions were the same as those in Example 48. As a result, in Example 51, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0116] [Comparative Example 4] In Comparative Example 4, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was hydrochloric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 20 [s], and a pickling accelerator was added as an additive to the acid solution. In addition, in Comparative Example 4, there was no destruction device 5. In addition, in Comparative Example 4, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was hydrochloric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 20 [s], and a pickling inhibitor was added as an additive to the acid solution. As a result, in Comparative Example 4, the scale removal was not completed, and the fracture generation rate of cold rolling was 2 [%].
[0117] [Example 52] In Example 52, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was sulfuric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 20 [s], and no additive was added. In addition, in Example 52, the type of the destruction device 5 was set to a shot peening machine. In addition, in Example 52, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was sulfuric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 15 [s], and no additive was added. As a result, in Example 52, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0118] [Example 53] In Example 53, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 95 [°C], the type of the destruction device 5 was set to a tension leveler, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 95 [°C]. Other than that, the conditions were the same as those in Example 52. As a result, in Example 53, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0119] [Example 54] In Example 54, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 85 [°C], the type of the destruction device 5 was set to a grinding brush, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 85 [°C]. Other than this, the conditions were the same as those in Example 52. As a result, in Example 54, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0120] [Example 55] In Example 55, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 75 [°C], the type of the destruction device 5 was set to a laser cleaning device, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 75 [°C]. Other than this, the conditions were the same as those in Example 52. As a result, in Example 55, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0121] [Comparative Example 5] In Comparative Example 5, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was set to sulfuric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 20 [s], and no additive was added. In addition, in Comparative Example 5, no destruction device 5 was provided. In addition, in Comparative Example 5, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was set to sulfuric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 15 [s], and no additive was added. As a result, in Comparative Example 5, the scale removal was not completed, and the fracture generation rate of cold rolling was 3 [%].
[0122] [Example 56] In Example 56, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was set to hydrochloric acid + nitric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 25 [s], and no additive was added. In addition, in Example 56, the type of the destruction device 5 was set to a shot peening machine. In addition, in Example 56, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was set to hydrochloric acid + nitric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 25 [s], and no additive was added. As a result, in Example 56, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0123] [Example 57] In Example 57, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 95 [°C], the type of the breaking device 5 was set to a tension leveling machine, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 95 [°C]. Other than that, the conditions were the same as those in Example 56. As a result, in Example 57, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0124] [Example 58] In Example 58, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 85 [°C], the type of the breaking device 5 was set to a grinding brush, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 85 [°C]. Other than that, the conditions were the same as those in Example 56. As a result, in Example 58, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0125] [Example 59] In Example 59, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 75 [°C], the type of the breaking device 5 was set to a laser cleaning device, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 75 [°C]. Other than that, the conditions were the same as those in Example 56. As a result, in Example 59, the scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0126] [Comparative Example 6] In Comparative Example 6, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was set to hydrochloric acid + nitric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 25 [s], and no additive was added. In addition, in Comparative Example 6, no breaking device 5 was provided. In addition, in Comparative Example 6, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was set to hydrochloric acid + nitric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 25 [s], and no additive was added. As a result, in Comparative Example 6, the scale removal was not completed, and the fracture generation rate of cold rolling was 3 [%].
[0127] [Example 60] In Example 60, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was set to hydrochloric acid + hydrofluoric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 15 [s], and no additives were added. Further, in Example 60, the type of the breaking device 5 was set to a shot peening machine. Further, in Example 60, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was set to hydrochloric acid + nitric acid, the temperature of the acid solution was set to 90 [°C], the pickling time was set to 10 [s], and no additives were added. As a result, in Example 60, scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0128] [Example 61] In Example 61, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 95 [°C], the type of the breaking device 5 was set to a tension leveler, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 95 [°C]. Other than that, the conditions were the same as those in Example 60. As a result, in Example 61, scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0129] [Example 62] In Example 62, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 85 [°C], the type of the breaking device 5 was set to a grinding brush, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 85 [°C]. Other than that, the conditions were the same as those in Example 60. As a result, in Example 62, scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0130] [Example 63] In Example 63, as the conditions for the first pickling performed by the first pickling device 4, the temperature of the acid solution was set to 75 [°C], the type of the breaking device 5 was set to a laser cleaning device, and as the conditions for the second pickling performed by the second pickling device 6, the temperature of the acid solution was set to 75 [°C]. Other than that, the conditions were the same as those in Example 60. As a result, in Example 63, scale removal was completed, and the fracture generation rate of cold rolling was 0 [%].
[0131] [Comparative Example 7] In Comparative Example 7, as the conditions for the first pickling performed by the first pickling device 4, the acid solution was set to hydrochloric acid + hydrofluoric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 15 [s], and no additive was added. Further, in Comparative Example 7, the breaking device 5 was not provided. Further, in Comparative Example 7, as the conditions for the second pickling performed by the second pickling device 6, the acid solution was set to hydrochloric acid + nitric acid, the temperature of the acid solution was set to 80 [°C], the pickling time was set to 10 [s], and no additive was added. As a result, in Comparative Example 7, the scale removal was not completed, and the fracture generation rate in cold rolling was 2 [%].
[0132] As can be seen from Table 5, as in Comparative Examples 4 to 7, under the conditions where the breaking device 5 was not provided and the mechanical breaking treatment of the scale was not performed, regardless of the type of the acid solution used in the first pickling and the second pickling or the presence or absence of an additive, the scale removal was not completed, and fractures occurred in cold rolling. It is considered that the reason is that since a large amount of scale remained, the remaining scale became the starting point of fracture, increasing the fracture generation rate in cold rolling. On the other hand, as can be seen from Table 5, as in Examples 48 to 63, under the conditions where the mechanical breaking treatment of the scale was performed by the breaking device 5, regardless of the conditions of the acid solution used in the first pickling and the second pickling, the presence or absence of an additive, and the type of the breaking device 5, the scale removal was completed. In addition, fractures in cold rolling did not occur. [Industrial Applicability]
[0133] The present invention can provide a scale removal device for a steel sheet, a manufacturing device for a steel sheet, a method for removing scale from a steel sheet, and a method for manufacturing a steel sheet that can balance the descaling property of the steel sheet and the suppression of fracture generation in cold rolling.
[0134] 1: Steel strip 2: Uncoiler 3: Welder 4: First pickling device 5: Breaking device 6: Second pickling device 7: Tension coiler 10: Scale removal device 20: Scale 21: External scale 22: Internal scale 23: Base iron 221: Island-shaped internal scale 222: Film-shaped internal scale 223: Metallic iron
Claims
1. A steel plate scale removal device, which removes scale from a steel plate containing 1.0 mass% or more of Si, characterized in that, starting from the upstream side in the conveying direction of the steel plate, there are sequentially arranged a pre-destruction device for mechanically destroying the scale, a first pickling device for performing a first pickling on the steel plate using a first acid solution, a destruction device for mechanically destroying the scale, and a second pickling device for performing a second pickling on the steel plate using a second acid solution, wherein a pickling accelerator is added to the first acid solution, the pickling time in the first pickling is set to 10[s] to 30[s], and the first pickling performed by the first pickling device removes the external scale on the surface of the steel plate, exposing the film-like internal scale, and the destruction device destroys the exposed film-like internal scale.
2. The steel plate scale removal equipment as described in claim 1, wherein, A pickling inhibitor is added to the second acid solution.
3. A steel plate manufacturing apparatus, comprising: A hot rolling mill for obtaining a hot-rolled plate by hot rolling a steel raw material; a hot-rolled plate annealing mill for annealing the hot-rolled plate as needed; a scale removal mill for removing scale from the hot-rolled plate or the hot-rolled plate that has undergone the hot-rolled plate annealing; a cold rolling mill for obtaining a cold-rolled plate by cold rolling the hot-rolled plate with the scale removed; and a final annealing mill for annealing the cold-rolled plate to obtain a cold-rolled annealed plate, wherein the steel plate manufacturing equipment is characterized in that, as the scale removal mill, a scale removal mill for steel plates as described in claim 1 or claim 2 is used.
4. A method for removing scale from a steel plate, characterized in that: the scale is mechanically destroyed by a pre-prepared destructive device; the steel plate is pickled by a first pickling device that pickles a hot-rolled steel plate containing 1.0 mass% or more of Si using a first acid solution; the scale on the surface of the steel plate after pickling by the first pickling device is mechanically destroyed by the destructive device; the steel plate after treatment by the destructive device is pickled by a second acid solution using a second pickling device; a pickling accelerator is added to the first acid solution; the pickling time performed by the first pickling device is set to 10[s] to 30[s]; and the external scale on the surface of the steel plate is removed by the first pickling device to expose the membranous internal scale; the exposed membranous internal scale is destroyed by the destructive device.
5. The method for removing scale from steel plates as described in claim 4, wherein, A pickling inhibitor is added to the second acid solution.
6. A method for manufacturing a steel plate, comprising: a hot rolling step, obtaining a hot-rolled plate by hot rolling a steel raw material; a hot-rolled plate annealing step, performing hot-rolled plate annealing on the hot-rolled plate as needed; a scale removal step, removing scale from the hot-rolled plate or the hot-rolled plate after hot-rolled plate annealing; a cold rolling step, obtaining a cold-rolled plate by cold rolling the hot-rolled plate after removing the scale; and a final annealing step, annealing the cold-rolled plate to obtain a cold-rolled annealed plate, wherein the method for manufacturing the steel plate is characterized in that, in the scale removal step, a scale removal method for steel plates as described in claim 4 or claim 5 is used.
Citation Information
Patent Citations
Device for removing oxide layer on surface of hot steel rolling belt
CN1354052A
Descaling method for stainless steel strip and apparatus therefor
JP2002275666A
PICKLING METHOD FOR HIGH Si HIGH Mn-CONTAINING HOT ROLLED STEEL SHEET
JP2016194153A
ACID CLEANING METHOD OF HIGH Si HIGH Mn-CONTAINING HOT ROLLED STEEL SHEET AND MANUFACTURING METHOD OF HIGH Si HIGH Mn-CONTAINING STEEL SHEET
JP2018168426A
Process for laser descaling of a running metal product, and device for implementing it
TW201827149A