Cold rolled and heat-treated steel sheet and a method of manufacturing thereof

A cold-rolled and heat-treated steel sheet with a specific composition and microstructure addresses the challenge of achieving high strength and formability, ensuring adequate liquid metal embrittlement resistance, suitable for automotive parts that need both strength and ease of forming, thereby reducing material usage and improving fuel efficiency.

US20260357367A1Pending Publication Date: 2026-11-12ARCELORMITTAL SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
US19/137151
Authority / Receiving Office
US · United States
Patent Type
Applications(United States)
Current Assignee / Owner
Filing Date
2022-12-14
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing high-strength steel sheets face challenges in achieving both high formability and strength while maintaining adequate liquid metal embrittlement resistance, which is crucial for automotive applications requiring weldability and reduced material usage for improved fuel efficiency.

Method used

A cold-rolled and heat-treated steel sheet with specific chemical composition and microstructure, including controlled ferrite-enriched layers, is developed to achieve an ultimate tensile strength of 1150 MPa, hole expansion ratio above 22%, and total elongation above 13%, along with improved weldability and resistance to liquid metal embrittlement.

Benefits of technology

The steel sheet exhibits enhanced mechanical properties, including high strength, formability, and resistance to liquid metal embrittlement, making it suitable for automotive parts that require both strength and ease of forming, while reducing material usage for improved fuel efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A cold rolled and heat-treated steel sheet, the steel including, 0.15%≤carbon≤0.25%, 2.2%≤manganese≤3%, 1.1%≤silicon≤2%, 0%≤aluminum≤0.09%, 0.05%≤molybdenum≤0.5%, 0.001%≤titanium≤0.06%, 0.001%≤boron≤0.010%, 0%≤phosphorus≤0.02%, 0%≤sulfur≤0.03%, 0%≤nitrogen≤0.09%, 0%≤chromium≤1%, 0%≤copper≤2%, 0%≤niobium≤0.06%, 0%≤vanadium≤0.1%, 0%≤calcium≤0.005%, 0%≤Magnesium≤0.05%, 0%≤Zirconium≤0.05%, 0%≤Cerium≤0.1%, and the balance including iron and unavoidable impurities, the steel sheet having a core microstructure including 15% to 70% of Bainite, 15% to 70% of Partitioned martensite, 10% to 30% of ferrite, 9% to 22% of residual austenite in Bainite and Partitioned Martensite and 0% to 5% fresh martensite in area fractions, and a ferrite-enriched layer extending up to 90 microns of the steel sheet.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a cold rolled and heat-treated steel sheet which is suitable for use as a steel sheet for vehicles.BACKGROUND

[0002] Automotive parts are required to satisfy two inconsistent necessities, namely ease of forming and strength. However in recent years a third requirement of improvement in fuel consumption is also bestowed upon automobiles in view of global environment concerns. Thus, now automotive parts must be made of material having high formability in order to fit in the criteria of ease of fit in the intricate automobile assembly and at same time improve strength for vehicle crashworthiness and durability while reducing weight of vehicle to improve fuel efficiency. Furthermore the steel part must be weldable while not suffering from liquid metal embrittlement.SUMMARY OF THE INVENTION

[0003] Therefore, intense Research and development endeavors have been undertaken to reduce the amount of material utilized in vehicles by increasing the strength of material. Conversely, an increase in strength of steel sheets decreases formability, and thus the development of materials having both high strength and high formability is necessitated.

[0004] Earlier research and developments in the field of high strength and high formability steel sheets have resulted in several methods for producing high strength and high formability steel sheets, some of which are enumerated herein for conclusive appreciation of the present invention:

[0005] EP3128027 is a high-strength cold-rolled steel sheet having a composite structure containing 0.15 to 0.25% by mass of C, 1.8 to 3.0% by mass of Mn, and 0.0003 to 0.0050% by mass of B, and having a ferrite volume fraction of 20% to 50%, a retained austenite volume fraction of 7% to 20%, a martensite volume fraction of 1% to 8%, and the balance containing bainite and tempered martensite, and in the composite structure, ferrite has an average crystal grain diameter of 5 μm or less, retained austenite has an average crystal grain diameter of 0.3 to 2.0 μm and an aspect ratio of 4 or more, martensite has an average crystal grain diameter of 2 μm or less, a metal phase containing both bainite and tempered martensite has an average crystal grain diameter of 7 μm or less, the ratio of the volume fraction of tempered martensite to the volume fraction of a metal structure other than ferrite is 0.60 to 0.85, and the average C concentration in retained austenite is 0.65% by mass or more. However, EP3128027 does not demonstrate adequate LME resistance.

[0006] The known prior art related to the manufacture of high strength and high formability steel sheets is inflicted by one or the other lacuna: hence there lies a need for a cold rolled steel sheet having strength greater than 1100 MPa and a method of manufacturing the same.

[0007] It is an object of the present invention to solve these problems by making available cold-rolled and heat-treated steel sheets that simultaneously have:

[0008] an ultimate tensile strength greater than or equal to 1150 MPa and preferably above 1180 MPa,

[0009] a hole expansion ratio greater than or above 22% and preferably above 25%,

[0010] an adequate liquid metal embrittlement resistance, and

[0011] total elongation value greater than or above 13%.

[0012] In a preferred embodiment, the cold-rolled and heat-treated steel sheet shows a yield strength value greater than or above 750 MPa and preferably above 800 MPa.

[0013] Preferably, such steel can also have a good suitability for forming, in particular for rolling with good weldability and coat ability.

[0014] The present invention provides a cold rolled and heat-treated steel sheet, the steel comprising, in weight percentage,

[0015] 0.15%≤carbon≤0.25%,

[0016] 2.2%≤manganese≤3%,

[0017] 1.1%≤silicon≤2%,

[0018] 0%≤aluminum≤0.09%,

[0019] 0.05%≤molybdenum≤0.5%,

[0020] 0.001%≤titanium≤0.06%,

[0021] 0.001%≤boron≤0.010%,

[0022] 0%≤phosphorus≤0.02%,

[0023] 0%≤sulfur≤0.03%,

[0024] 0%≤nitrogen≤0.09%,

[0025] and optionally one or more of the following elements

[0026] 0%≤chromium≤1%,

[0027] 0%≤copper≤2%,

[0028] 0%≤niobium≤0.06%,

[0029] 0%≤vanadium≤0.1%,

[0030] 0%≤calcium≤0.005%,

[0031] 0%≤Magnesium≤0.05%,

[0032] 0%≤Zirconium≤0.05%,

[0033] 0%≤Cerium≤0.1%,and the balance including iron and unavoidable impurities, the steel sheet having a core microstructure comprising 15% to 70% of Bainite, 15% to 70% of Partitioned martensite, 10% to 30% of ferrite, 9% to 22% of residual austenite in Bainite and Partitioned Martensite and 0% to 5% fresh martensite in area fractions, and a ferrite-enriched layer extending up to 90 microns from both surfaces of said steel sheet, such ferrite-enriched layer having two sub layers wherein a first sub-layer which is adjacent to the surface of the steel sheet has an average ferrite percentage from 40% to 80% in area fraction with a gradient of ferrite (ΔF) that is from 20% to 70%, ΔF being the difference between the ferrite content of the top of first sub-layer and the ferrite content of the bottom of said second sub-layer and a second sub-layer which is topmost layer of the ferrite enriched layer, said second sub-layer having a ferrite percentage from 70% to 98% in area fraction and including internal oxides of manganese and silicon.

[0034] Another object of the present invention is to make available a method for the manufacturing of these sheets that is compatible with conventional industrial applications while being robust towards manufacturing parameters shifts.

[0035] The present invention also provides a method of manufacturing of a cold rolled and heat-treated steel sheet comprising the following successive steps:

[0036] providing a steel composition as disclosed above to obtain a semi-finished product,

[0037] reheating said semi-finished product to a temperature from 1000 °C to 1280 °C;

[0038] rolling the said semi-finished product completely in the austenitic range wherein the hot rolling finishing temperature is greater than or equal to 850 °C to obtain a hot rolled steel sheet,

[0039] cooling the sheet at a cooling rate above 30 °C / s to a temperature below or equal to 550 °C; and coiling the said hot rolled sheet and keeping the temperature of coiled sheet below 500 °C,

[0040] cooling the said hot rolled sheet,

[0041] performing optional scale removal process on said hot rolled steel sheet,

[0042] subjecting the hot rolled steel sheet to an optional annealing at a temperature from 350 °C to 750 °C during 1 h to 96 h cold rolling the said hot rolled steel sheet with a reduction rate from 35 to 70% to obtain a cold rolled steel sheet,

[0043] annealing the said cold rolled steel sheet in a two steps heating during which the dew point is controlled from −15 °C to +15 °C and wherein:

[0044] the first step starts from heating the steel sheet from room temperature to a temperature HT1 from 600 °C to 800 °C, with a heating rate HR1 from 2 °C / s to 70 °C / s,

[0045] the second step starts from heating further the steel sheet from HT1 to a soaking temperature TA from Ac3−10 °C and Ac3+100 °C, with a heating rate HR2 from 0.1 °C / s to 10 °C / s or less, HR2 being lower than HR1,

[0046] then perform annealing at TA during 10 to 1000 seconds, the dew point being controlled from −10 °C to +10 °C during the annealing,

[0047] then cooling the said cold rolled steel sheet wherein:

[0048] an optional first step of cooling the cold rolled steel sheet starts from TA down to a temperature CT1 from 580 °C to 860 °C, with a cooling rate CR1 from 0.01 °C / s to 15 °C / s;

[0049] a cooling step starts from CT1 or TA down to a temperature CT2 from Ms−30 °C to 20 °C, with a cooling rate CR2 of at least 10 °C / s,

[0050] then heating the cold rolled steel sheet from CT2 temperature to an overaging temperature TOA from 250 °C to 580 °C at an average heating rate HR3 from 1 °C / s to 100 °C / s,

[0051] then the said cold rolled steel sheet is overaged at TOA during 5 to 500 seconds, and

[0052] then the said cold rolled steel sheet is cooled to room temperature to obtain a cold rolled and heat-treated steel sheet.

[0053] The cold rolled heat treated steel sheet of the present invention is coated with zinc or zinc alloys, or with aluminum or aluminum alloys to improve its corrosion resistance.DETAILED DESCRIPTION

[0054] Other characteristics and advantages of the present invention will become apparent from the following detailed description of the present invention.

[0055] Carbon is present in the steel from 0.15% to 0.25%. Carbon is an element necessary for increasing the strength of a steel sheet by delaying the formation of ferrite and bainite during cooling after annealing. Carbon also plays a pivotal role in austenite stabilization. A content less than 0.15% would not allow stabilizing austenite, thereby decreasing strength as well as ductility. On the other hand, at a carbon content exceeding 0.25%, a weld zone and a heat-affected zone are significantly hardened, and thus the mechanical properties of the weld zone are impaired. Preferable limit for carbon is from 0.16% to 0.24% and more preferred limit is from 0.17% to 0.22%.

[0056] Manganese content of the steel of the present invention is from 2.2% to 3%. Manganese is an element that imparts strength as well as stabilizes austenite to obtain residual austenite. An amount of at least 2.2% of manganese is necessary to provide the strength and hardenability of the steel sheet by delaying the formation of Ferrite as well as to stabilize austenite. Thus, a higher percentage of Manganese such as 2.3 to 2.8% is preferred. But when manganese is more than 3%, this produces adverse effects such as slowing down the transformation of austenite to bainite during the isothermal holding for bainite transformation, leading to a reduction of ductility. Additionally, when the manganese is above 3% not enough bainite is formed and the formation of martensite is beyond the targeted limit thus elongation decreases. Moreover, a manganese content above 3% would also reduce the weldability of the present steel.

[0057] Silicon content of the steel of the present invention is from 1.1% to 2%. Silicon as a constituent retards the precipitation of carbon as carbides in bainite during the soaking after cooling from high temperature. Thus, during formation of carbide free bainite, austenite is enriched in carbon. Therefore, due to the presence of 1.1% of silicon, Austenite is stabilized at room temperature. Additionally, silicon retards carbides precipitation in martensite. In both cases, carbides in bainite or carbides in martensite are also responsible of elongation decrease. Preventing carbides by the presence of Si is important. However, adding more than 2% of silicon does not improve the mentioned effect and leads to problems such as liquid metal embrittlement as well as Silicon more than 2% in the steel of the present invention makes Zn not soluble in the grains. Thus, when welding, liquid Zn goes along the grain boundaries, instead of going into the grains causing liquid metal embrittlement. Therefore, the concentration is controlled within an upper limit of 2%. Preferred limit for silicon for the present steel is from 1.2% to 1.9% and more preferably from 1.2% to 1.8%.

[0058] The content of aluminum of the steel of the present invention is from 0 to 0.09%. Aluminum is added during the steel making for deoxidizing the steel to trap oxygen. Higher than 0.09% will increase the Ac3 point, thereby lowering the productivity. Additionally, within such range, aluminum bounds nitrogen in the steel to form aluminum nitride to reduce the size of the grains. But, whenever the content of aluminum exceeds 0.09% in the present invention, the amount and size of aluminum nitrides are detrimental to hole expansion and bending. Preferable limit for aluminum is 0% to 0.06% and more preferably 0% to 0.05%.

[0059] Molybdenum is an essential element that is present from 0.05% to 0.5% in the steel of the present invention. Molybdenum plays an effective role in improving hardenability and hardness, and delays the formation of ferrite and bainite during the cooling after annealing, when added in an amount of at least 0.05%. Mo is also beneficial for the toughness of the hot rolled product resulting in an easier manufacturing. However, the addition of Molybdenum excessively increases the cost of the addition of alloy elements, so that for economic reasons its content is limited to 0.5%. Molybdenum also facilitates the formation of Ferrite microstructure on the surface up to the thickness depth of 50 microns measured from the outer surface because Ac3 is increased a little, for the same soaking and dew point temperatures thereby increasing the formation of Ferrite on the surface steel of the present invention. The preferable limit for Molybdenum is from 0.06% to 0.3% and more preferably from 0.07% to 0.2%.

[0060] Titanium is an essential element which is added to the steel of the present invention from 0.001% to 0.06%, preferably from 0.001% to 0.03%. As niobium, it is involved in carbo-nitrides which plays a role in hardening. But it is also involved to form TiN appearing during solidification of the cast product. The amount of Ti is limited to 0.06% to avoid coarse TiN detrimental for hole expansion. In case the titanium content is below 0.001% it does not impart any effect on the steel of the present invention.

[0061] Boron is a mandatory element, which can be added from 0.001 to 0.010%, preferably from 0.001% to 0.004%, to harden the steel. Boron imparts hardenability and strength to the steel of the present invention. However, when boron is added more than 0.010% the rollability of the steel sheet is found to be significantly lowered. Further the segregation may happen at grain boundaries which is detrimental for the formability.

[0062] Phosphorus content of the steel of the present invention is limited to 0.02%. Phosphorus is an element which hardens in solid solution. Therefore, a small amount of phosphorus, of at least 0.002% can be advantageous, but phosphorus has its adverse effects such as a reduction of the spot weldability and the hot ductility, particularly due to its tendency to segregation at the grain boundaries or co-segregation with manganese. For these reasons, its content is preferably limited to a maximum of 0.015%.

[0063] Sulfur is not an essential element but may be contained as an impurity in steel. The sulfur content is preferably as low as possible but is 0.03% or less and preferably at most 0.005%, from the viewpoint of manufacturing cost. Further if higher sulfur is present in steel it combines to form sulfide especially with Mn and Ti which are detrimental for bending, hole expansion and elongation of the steel of the present invention.

[0064] Nitrogen is limited to 0.09% to avoid ageing of material and to minimize the precipitation of nitrides during solidification which are detrimental for mechanical properties of the Steel such as bending and hole expansion ratio.

[0065] Chromium is an optional element of the steel of the present invention, the content is from 0% to 1%. Chromium provides strength and hardening to the steel, but when used above 1% impairs surface finish of the steel.

[0066] Copper may be added as an optional element in an amount of 0% to 2% to increase the strength of the steel of the present invention and to improve its corrosion resistance. A minimum of 0.01% is preferred to get such effects. However, when its content is above 2%, it can degrade the surface aspects.

[0067] Niobium is an optional element that can be added to the steel from 0% to 0.06%, preferably from 0.0010 to 0.03%. It is suitable for forming carbonitrides to impart strength to the steel according to the invention by precipitation hardening. Because niobium delays the recrystallization during the heating, the microstructure formed at the end of the holding temperature after the complete annealing is finer. This leads to the hardening of the product. But when the niobium content is above 0.06% the amount of carbo-nitrides is not favorable for the present invention as large amounts of carbo-nitrides tend to reduce the ductility of the steel.

[0068] Vanadium is an optional element which may be added to the steel of the present invention from 0% to 0.1%, preferably from 0.001% to 0.1%. As niobium, it is involved in carbo-nitrides so plays a role in hardening. But it is also involved to form VN appearing during solidification of the cast product. The amount of V is limited to 0.1% to avoid coarse VN detrimental for hole expansion. In case the vanadium content is below 0.001% it does not impart any effect on the steel of the present invention.

[0069] Calcium is an optional element which may be added to the steel of the present invention from 0% to 0.005%, preferably from 0.001% to 0.005%. Calcium is added to steel of the present invention as an optional element especially during the inclusion treatment. Calcium contributes towards the refining of the steel by decreasing the detrimental sulfur content in globularizing it.

[0070] Other elements such as cerium, magnesium or zirconium can be added individually or in combination in the following proportions: Ce≤0.1%, Mg≤0.05% and Zr≤0.05%. Up to the maximum content levels indicated, these elements make it possible to refine the inclusion grain during solidification.

[0071] The remainder of the composition of the steel consists of iron and inevitable impurities resulting from processing.

[0072] The core microstructure of the steel sheet according to the invention comprises 15% to 70% Bainite, 15% to 70% of Partitioned martensite, 10% to 30% of Ferrite, 9% to 22% of Residual Austenite in Bainite and partitioned martensite, 0% to 5% of Fresh martensite by area fraction.

[0073] Bainite is the matrix of the steel and is present from 15% to 70%. In the frame of the present invention, bainite can comprise of upper bainite, lower bainite, granular bainite, carbide-free bainite and / or lath bainite. Bainite of the present invention contains film like austenite in the grains and this Bainite provides an improved elongation as well as the hole expansion to the steel of the present invention when controlled in the invention range. The preferred presence for bainite is from 18% to 65% and more preferably from 22% to 62%.

[0074] Partitioned martensite is contained in an amount of 15% to 70% to achieve the strength level of 1150 MPa or more. If the martensite amount reaches beyond 70%, it would have detrimental impact on ductility. Partitioned martensite of the present steel can be in the form of laths wherein the lath thickness is more than 0.1 micron and film like austenite is present between these lathes. Martensite, that is formed during the cooling after annealing, is transformed into Partitioned martensite during the heating to the overaging temperature. The preferred presence of the partitioned martensite for the steel of the present invention is from 18% to 65% and more preferably from 18% to 60%.

[0075] Residual Austenite is contained in an amount of 9% to 22% and imparts ductility of the present steel. In the frame of the present invention, Residual Austenite can comprise film-like austenite and / or blocky austenite. Film-like Austenite of the present invention can be present in the bainite and partitioned martensite and shows an aspect ratio above 3. Blocky Austenite can be present in form of islands in bainite showing an aspect ratio below 2 and can act as an effective carbon trap thereby assisting in formation of Bainite. Blocky austenite is less than 5 microns in the biggest dimension of the grains and preferably less than 3 microns and can form during the overaging holding.

[0076] The retained austenite of the present invention preferably contains carbon from 0.4 to 0.7%. It is preferred to have residual austenite from 9% to 20% and more preferably from 9% to 16%. It is preferred to have blocky austenite with the characteristics described above.

[0077] Ferrite is present from 10% to 30% in the steel, except at the surface layer which is rich in ferrite. Such ferrite may comprise polygonal ferrite, lath ferrite, acicular ferrite, plate ferrite or epitaxial ferrite. The presence of ferrite in the present invention impart the steel with formability and elongation. Presence of ferrite has also negative impacts due to the fact that ferrite increases the gap in hardness with hard phases such as martensite and bainite and reduces local ductility. If ferrite presence is above 30% the targeted tensile strength is not achieved as well as hole expansion rate can decrease due to the increase of the amount of interfaces between ferrite and hard phases. Hence the preferred presence is from 12% to 28% and more preferably from 14% to 25%.

[0078] Fresh Martensite can be present in the steel according to the invention, as isolated phases. Fresh martensite may also be present from 0% to 5% and preferably from 0% to 3%.

[0079] In addition to this core microstructure of the steel sheet, the steel sheet also includes a ferrite-enriched layer on both surfaces of the steel sheet up to a thickness of 90 microns. This ferrite-enriched layer is further divided into two sub-layers wherein the first sub-layer is formed adjacent to the surface of the steel sheet and showing an average ferrite percentage from 40% to 80% in area fraction, preferably from 42% to 78% more preferably from 43% to 70%. This first sub-layer can have a thickness from 30 microns to 70 microns. In addition, this first sub-layer has a gradient ferrite presence referred to as ΔF. Ferrite present on the top of the first sub layer and at the bottom of the first sub layer have a difference in the presence of ferrite from 20 to 70%. ΔF is determined as follows:ΔF=(ferrite content of top of first sub-layer−ferrite content of bottom of first sub-layer) 20%≤ΔF≤70%

[0080] When ΔF is less than 20% then the LME properties are not good and when ΔF is greater than 70% then the amount of ferrite is not enough to have a sufficiently thick second sub layer which is detrimental for the LME properties due to the reduction the presence of ferrite at the bottom of second sublayer of Ferrite enriched layer. The preferred ΔF is from 22% to 60% and more preferably from 24% to 55%.

[0081] The second sub-layer constitutes the topmost layer of the ferrite enriched layer is adjacent to first sub-layer. The second sub-layer has a ferrite percentage from 70% to 98% in area fraction, preferably from 72% to 96%, more preferably from 74% to 94% and in addition to the ferrite this second sub-layer constitutes of internal oxides of manganese and silicon. This second sub-layer preferably has a thickness from 1 micron to 15 microns and preferably from 3 to 10 microns.

[0082] The ferrite enriched layer formed on the surface preferably comprises any or all possible ferrite kinds and notably polygonal ferrite, lath ferrite, acicular ferrite, plate ferrite or epitaxial ferrite. This ferrite layer imparts the steel sheet of the invention with resistance against the liquid metal embrittlement (LME).

[0083] The remaining part of this surface layer comprises bainite and / or residual austenite and / or martensite.

[0084] A steel sheet according to the invention can be produced by any suitable method. A preferred method consists in providing a semi-finished casting of steel with a chemical composition according to the invention. The casting can be done either into ingots or continuously in form of thin slabs or thin strips, i.e. with a thickness ranging from approximately 220 mm for slabs up to several tens of millimeters for thin strips.

[0085] For example, a slab will be considered as a semi-finished product. A slab having the above-described chemical composition is manufactured by continuous casting wherein the slab preferably underwent a direct soft reduction during casting to ensure the elimination of central segregation and porosity reduction. The slab provided by a continuous casting process can be used directly at a high temperature after the continuous casting or may be first cooled to room temperature and then reheated for hot rolling.

[0086] The temperature of the slab which is subjected to hot rolling is preferably at least 1000 °C, preferably above 1200 °C and must be below 1280 °C. In case the temperature of the slab is lower than 1000 °C, excessive load is imposed on a rolling mill, and further, the temperature of the steel may decrease to a ferrite transformation temperature during finishing rolling, whereby the steel will be rolled in a state in which transformed ferrite contained in the structure. Further, the temperature must not be above 1280 °C because this is industrially expensive.

[0087] The temperature of the slab is preferably sufficiently high so that hot rolling can be completed entirely in the austenitic range, the finishing hot rolling temperature remaining above 850 °C and preferably above 900 °C. It is necessary that the final rolling be performed above 850 °C, because below this temperature the steel sheet exhibits a significant drop in rollability. A final rolling temperature from 900 to 950 °C is preferred to have a structure that is favorable to recrystallization and rolling.

[0088] The sheet obtained in this manner is then cooled at a cooling rate above 30 °C / s to a temperature which is equal or below 550 °C. The cooling temperature is kept below 550 °C to avoid oxidation of alloying elements such as manganese, silicon and chromium. Preferably, the cooling rate will be less than or equal to 65 °C / s and above 35 °C / s. Thereafter the hot rolled steel sheet is coiled and the coiling temperature must be below 550 °C. Thereafter the temperature of the coiled hot rolled steel sheet must be kept below 550 °C to avoid oxidation of Silicon, Manganese on the surface of hot rolled coil as these oxides forms cracks on the surface of the hot rolled steel sheet. Thereafter the coiled hot rolled steel sheet is allowed to cool down to room temperature. Then the hot rolled sheet is subjected to on optional scale removal process such as pickling to remove scale formed during hot rolling and ensure that there is no scale on the surface of the hot rolled steel sheet before subjecting it to an optional hot band annealing.

[0089] The hot rolled sheet may be subjected to an optional hot band annealing at a temperature from 350 °C to 750 °C during 1 to 96 hours. The temperature and time of such hot band annealing is selected to ensure softening of the hot rolled sheet to facilitate the cold rolling of the hot rolled steel sheet.

[0090] The hot rolled steel sheet is then cooled down to room temperature, thereafter, the hot rolled sheet is cold rolled with a thickness reduction from 35 to 70% to obtain a cold rolled steel sheet.

[0091] The cold rolled steel sheet is then subjected to annealing to impart the steel of the present invention with targeted microstructure and mechanical properties.

[0092] In the annealing, the cold rolled steel sheet is subjected to two steps of heating to reach the soaking temperature TA from Ac3−30 °C to Ac3+100 °C, during the two step heating the dewpoint is maintained from −15 °C to +15 °C to provide the steel of the present invention with a ferrite rich layer on surface to have adequate Liquid metal embrittlement resistance, the preferred dew point is maintained from −10 °C to +10 °C. The Ac3 for the present steel is determined by a dilatometry test as per the method described in article published in the journal “TECHNIQUES DE L'INGENIEUR, MESURES ET ANALYSE; FRA; PARIS: TECH.-ING.; DA. 1981; VOL. 20; NO 59; P1280” by M. Murat.

[0093] In step one cold rolled steel sheet is heated from room temperature to temperature HT1 which is in a range from 600 °C to 800 °C at a heating rate HR1 from 2 °C / s to 70 °C / s. It is preferred to have HR1 rate from 5 °C / s to 60 °C / s and more preferably from 10 °C / s to 50 °C / s. The preferred HT1 temperature is from 625 °C to 775 °C, more preferably from 640 °C to 750 °C.

[0094] Thereafter in a subsequent second step of heating, the cold rolled steel sheet is heated from temperature HT1 to the soaking temperature TA which is in the temperature range from Ac3−10 °C to Ac3+100 °C at a heating rate HR2 from 0.1 °C / s to 10 °C / s. It is preferred to have a HR2 rate from 0.1 °C / s to 8 °C / s and more preferably from 0.1 °C / s to 5 °C / s. HR2 being always lower than HR1.

[0095] The preferred TA temperature is from Ac3−25 °C to Ac3+75 °C, more preferably from Ac3−20 °C to Ac3+50 °C. Dew point is maintained from −10 °C to +10 °C at the soaking temperature and preferably from −5 °C to +5 °C to provide the present steel with the ferrite-enriched layer at the surface with the targeted depth.

[0096] As mentioned above, the ferrite-enriched layer according to the invention is formed during annealing. Carbon reacts with oxygen to form carbon monoxide that escapes from the steel, resulting in a decarburization of the surface layer, such layer having a microstructure enriched in ferrite and extending from the surface of the sheet up to the depth of 90 microns. This ferrite-enriched layer forms during the heating before annealing and during soaking thanks to the control of dew point. The dew point is controlled from −15 °C to +15 °C during the heating before annealing and from −10 °C to +10 °C during the soaking by using conventional means known by the man skilled in the art, like water injection for example.

[0097] Then the cold rolled steel sheet is held at the annealing soaking temperature TA during 10 to 1000 seconds to ensure adequate transformation to Austenite microstructure of the strongly work-hardened initial structure.

[0098] The cold rolled steel sheet is then cooled in a cooling process wherein the first step of cooling is optional and this first steps starts from TA, the cold rolled steel sheet being cooled down, at a cooling rate CR1 from 0.01 °C / s to 15 °C / s, to a temperature CT1 which is in a range from 580 °C to 860 °C. In a preferred embodiment, the cooling rate CR1 for such first step of cooling is from 0.02 °C / s to 5 °C / s. The preferred T1 temperature for such first step is from 590 °C to 850 °C.

[0099] In the second step of cooling, the cold rolled steel sheet is cooled from CT1 or TA to a temperature CT2 which is from Ms−30 °C to 20 °C, at a cooling rate CR2 of at least 10 °C / s. In a preferred embodiment, the cooling rate CR2 for the second step of cooling is at least 20 °C / s and more preferably at least 25 °C / s. The preferred CT2 temperature for such second step is from Ms−50 °C to 100 °C. Whenever step one of cooling is not performed then CT1 is equal to TA.

[0100] In a subsequent step the cold rolled steel sheet is heated to an overaging temperature range TOA from 250 °C to 580 °C from CT2 temperature at a heating rate HR3 from 1 °C / s to 100 °C / s. During this step, martensite formed during cooling after annealing is transformed into partitioned martensite, thereby assisting in formation of bainite during the holding at TOA temperature. Then the cold rolled steel sheet is held at TOA temperature for over-aging for 5 to 500 seconds allowing the bainite of the present invention to be formed.

[0101] Then the cold rolled steel sheet can be brought to the temperature of a hot dip coating bath, which can be from 420 °C to 680 °C, depending on the nature of the coating. The coating can be made with zinc or a zinc-based alloy or with aluminum or with an aluminum-based alloy.

[0102] Alternatively, the cold rolled steel sheet may also be coated by any of the known industrial processes such as Electro-galvanization, JVD, PVD, Hot dip (GI), GA or ZM etc., which do not require the steel sheet to be brought to the above described range of temperature after overaging. In that case, the steel sheet can be cooled down to room temperature before being coated in a subsequent step.

[0103] An optional post batch annealing, preferably done at 170 to 210 °C during 12 h to 30 h can be performed after annealing on a coated product in order to ensure degassing for coated products.EXAMPLES

[0104] The following tests and examples presented herein are non-restricting in nature and must be considered for purposes of illustration only and will display the advantageous features of the present invention and expound the significance of the parameters chosen by inventors after extensive experiments and to further establish the properties that can be achieved by the steel according to the invention.

[0105] Samples of the steel sheets according to the invention and to some comparative grades were prepared with the compositions gathered in table 1 and the processing parameters gathered in table 2. The corresponding microstructures of those steel sheets were gathered in table 3 and the properties in table 4.

[0106] Table 1 depicts the steels with the compositions expressed in percentages by weight.

[0107] Table 1 also shows Martensite transformation Ms and Ac3 temperatures of inventive steel and reference steel. Ms and Ac3 for all inventive and reference steels are determined through dilatometry tests as per the method described in article published in the journal “TECHNIQUES DE L'INGENIEUR, MESURES ET ANALYSE; FRA; PARIS: TECH.-ING.; DA. 1981; VOL. 20; NO 59; P1280” by M. Murat.TABLE 1composition of the trialsTrialsCMnSiAlMoTiBPSNCrAc3MsI10.1942.791.750.0290.0870.020.00330.0080.00110.0040.027850315I20.1942.791.750.0290.0870.020.00330.0080.00110.0040.027850300I30.1942.791.750.0290.0870.020.00330.0080.00110.0040.027850300I40.1942.791.750.0290.0870.020.00330.0080.00110.0040.027850295I50.1892.671.750.0230.0870.0280.00260.0110.00180.00390.02855300I60.1942.791.750.0290.0870.020.00330.0080.00110.0040.027850315I70.1942.791.750.0290.0870.020.00330.0080.00110.0040.027850315R10.1892.671.750.0230.0870.0280.00260.0110.00180.00390.02855330R20.1942.791.750.0290.0870.020.00330.0080.00110.0040.027850330R30.1902.701.730.0250.1170.0050.00030.0130.00170.00440.027850320R40.1882.681.760.0270.0010.0250.00190.0080.00330.00370.02840330underlined values: not according to the invention

[0108] Table 2 gathers the annealing process parameters implemented on steels of Table 1.

[0109] Further, before performing the annealing treatment on the steels of the present invention as well as reference, the samples were heated to a temperature from 1000 °C to 1280 °C and then subjected to hot rolling with finishing temperature above 850 °C. The cooling rate after hot rolling was above 30 °C / s until cooling down below 550 °C. All cold rolled steel sheets were coated in a zinc bath at temperature 460 °C after the over aging holding.TABLE 2process parameters of the trialsCoilingHBACR reduc-TrialsTemp (°C)Pickling(°C)t (h)Picklingtion (%)I1461YES58010YES42I2461YES58010YES42I3438YES5957YES42I4461YES58010YES42I5453YES65010YES51I6453YES58010YES50I7461YES58010YES42R1453YES65010YES51R2461YES58010YES42R3426YES58010YES42R4456YES58010YES50Table 2A: HBA: hot band annealing of steel sheetAnnealingDew pointDew pointduringduringholdingHR1HT1HR2TASoakingheatingsoakingCR1CT1CR2CT2HR3TOATimeTrials(°C / s)(°C)(°C / s)(°C)time (s)(°C)(°C)(°C / s)(°C)(°C / s)(°C)(°C / s)(°C)(s)I1216981.1832205200.47763821744426103I2157001.9850130003.1600332406344565I3357301.282021000—562206944510I4135603.682020500—552276744565I5357301.283021000—752307044565I6237400.78825199370.068205523340435101I735730181521000—542205540065R1227201.2870330−2−2—4530545465100R2227201.2880260−2−20.03870552705546565R3207260.75830227−500.078253124570465113R4257001.7830130−4−40.03810702577044565I = according to the invention; R = reference; underlined values: not according to the invention.

[0110] Table 3 gathers the results of tests conducted in accordance of standards of different microscopes such as Scanning Electron Microscope for determining microstructural composition of both the inventive steel and reference trials. Ferrite and fresh martensite are measured by image analysis done through Scanning Electron Microscope at 3000X. Bainite is measured by symmetry. Residual Austenite is measure by image analysis done through X-ray diffraction.TABLE 3microstructures of the trials:Steel SheetTotal AustenitePartitionedFreshin PartitionferritebainiteMartensiteMartensiteMartensite andTrials(%)(%)(%)(%)Bainite (%)I1154243012I2206020010I3182557013I4212455013I5174241013I6184042013I7205030013R1 06830216R2 05050012R3 92764012R4 150490 8I = according to the invention; R = reference; underlined values: not according to the invention.TABLE 3Ashows the presence of Ferrite and internal oxides in Ferrite layer:First Sub layerSecond Sub layerThicknessAv.ThicknessFerriteInternalTrials(microns)Ferrite (%)TopBottomΔF(microns)(%)OxideI15050593425776Si, MnI25044552530675Si, MnI35064814338887Si, MnI45065814536888Si, MnI55055793049793Si, MnI65063814140785Si, MnI75065834736890Si, MnR1503075 075885Si, MnR2502772 075885Si, MnR35060704525882Si, MnR45058803545787Si, MnI=according to the invention; R=reference; underlined values: not according to the invention.

[0112] Table 4 gathers the mechanical and surface properties of both the inventive steel and reference steel. The tensile strength, yield strength and total elongation tests are conducted in accordance with ISO 6892-1 standards and the test for Hole expansion ratio is conducted accordance with ISO 16630 standards.Table 4: Mechanical and Surface Properties of the Trials:

[0113] The susceptibility of LME of the trials was evaluated by the resistance spot welding method. To this end, for each trial, one steel sheet corresponding respectively to trials I1 to I7 and to trials R1 to R4 which were spot welded with two additional steel sheets to build a three-sheet stack-up including successively:

[0114] one steel sheet corresponding to trials I1 to I7 and to trials R1 to R4,

[0115] a sheet of 1.5 mm of an Interstitial free galvanized steel comprising 0.003% of carbon and 0.11% of manganese, and

[0116] a sheet of 1.5 mm of an Interstitial free galvanized steel comprising 0.003% of carbon and 0.11% of manganese.

[0117] Welding conditions were according to standard ISO-18278-2. The type of the welding electrode was F1 with a face diameter of 6 mm; the damping force of the electrode was set at 450 daN. The welding cycle is as follows:CurrentWeldingCoolWeld time(Hz)time (ms)time (ms)Cycle50380260

[0118] Each trial was reproduced 10 times to produce 10 spot welds at a current level defined as the upper welding limit of the current range from Imax to Imax+10%, Imax being comprised between 0.9 and 1.1*Iexp, Iexp being the intensity beyond which expulsion appears during welding, determined according to ISO standard 18278-2.

[0119] The cracks length in the 10 spot-welded joints was then evaluated after cross-sectioning through the surface crack and using an optical microscope. A grade was considered as providing enough LME resistance if less than 60% of the spots had a crack longer than 200 μm.

[0120] The yield strength YS, the tensile strength TS and the total elongation TE are measured according to ISO standard ISO 6892-1, published in October 2009. The hole expansion ratio is measured according to ISO standard 16630:2009.TotalHoleTSelongationexpansionLMEYSTrials(MPa)(%)ratio (%)resistance(MPa)I1122315.941OK1030I2122713.535OK1067I3126715  33OK832I4123014.131OK971I5119515.640OK895I6124613.331OK944I7120616.128OK912R1126712.345NOT OK651R2121014.440NOT OK931R3121215.230NOT OK949R4120115.843NOT OK953I = according to the invention; R = reference; underlined values: not according to the invention.

[0121] It can be seen from the table above that the trials according to the invention all meet the properties targets.

Claims

1-15. (canceled)16. A cold rolled and heat-treated steel sheet, the steel comprising, in weight percentage,0.15%≤carbon≤0.25%,2.2%≤manganese≤3%,1.1%≤silicon≤2%,0%≤aluminum≤0.09%,0.05%≤molybdenum≤0.5%,0.001%≤titanium≤0.06%,0.001%≤boron≤0.010%,0%≤phosphorus≤0.02%,0%≤sulfur≤0.03%,0%≤nitrogen≤0.09%,and optionally one or more of the following elements0%≤chromium≤1%,0%≤copper≤2%,0%≤niobium≤0.06%,0%≤vanadium≤0.1%,0%≤calcium≤0.005%,0%≤Magnesium≤0.05%,0%≤Zirconium≤0.05%,0%≤Cerium≤0.1%,a balance including iron and unavoidable impurities,the steel sheet having: a core microstructure comprising 15% to 70% of Bainite, 15% to 70% of Partitioned martensite, 10% to 30% of ferrite, 9% to 22% of residual austenite in Bainite and Partitioned Martensite and 0% to 5% fresh martensite in area fractions; and a ferrite-enriched layer extending up to 90 microns from both surfaces of the steel sheet, the ferrite-enriched layer having a first sub-layer adjacent to a surface of the steel sheet and having an average ferrite percentage from 40% to 80% in area fraction with a gradient of ferrite (ΔF) from 20% to 70%, ΔF being the difference between the ferrite content of the top of first sub-layer and the ferrite content of the bottom of said second sub-layer and having a second sub-layer, the second sub-layer being a topmost layer of the ferrite enriched layer, the second sub-layer having a ferrite percentage from 70% to 98% in area fraction and including internal oxides of manganese and silicon.

17. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the composition includes 2.3% to 2.8% of manganese.

18. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the composition includes 0.16% to 0.24% of Carbon.

19. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the composition includes 1.2% to 1.9% of Silicon.

20. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the composition includes 0.06% to 0.3% of Molybdenum.

21. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the core microstructure contains 18% to 65% of bainite.

22. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the core microstructure contains residual 9% to 20% of residual austenite in bainite and partitioned martensite.

23. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the core microstructure contains 18% to 65% of partitioned martensite.

24. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the steel sheet has a tensile strength greater than or equal to 1150 MPa, and a hole expansion ratio of 22% or more.

25. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the steel sheet has a total elongation of 13% or more.

26. The cold rolled and heat-treated steel sheet as recited in claim 16 wherein the first sub-layer has a thickness from 30 microns to 70 microns.

27. A method of manufacturing of a cold rolled and heat-treated steel sheet comprising the following successive steps:providing a steel composition comprising, in weight percentage,0.15%≤carbon≤0.25%,2.2%≤manganese≤3%,1.1%≤silicon≤2%,0%≤aluminum≤0.09%,0.05%≤molybdenum≤0.5%,0.001%≤titanium≤0.06%,0.001%≤boron≤0.010%,0%≤phosphorus≤0.02%,0%≤sulfur≤0.03%,0%≤nitrogen≤0.09%,and optionally one or more of the following elements0%≤chromium≤1%,0%≤copper≤2%,0%≤niobium≤0.06%,0%≤vanadium≤0.1%,0%≤calcium≤0.005%,0%≤Magnesium≤0.05%,0%≤Zirconium≤0.05%,0%≤Cerium≤0.1%,a balance including iron and unavoidable impurities, to obtain a semi-finished product; reheating the semi-finished product to a temperature from 1000 °C to 1280 °C;rolling the semi-finished product completely in the austenitic range wherein a hot rolling finishing temperature is greater than or equal to 850 °C to obtain a hot rolled steel sheet;cooling the hot rolled steel sheet at a cooling rate above 30 °C / s to a temperature below or equal to 550 °C; and coiling the hot rolled steel sheet and keeping the temperature of the coiled hot rolled steel sheet below 500 °C;cooling the hot rolled steel sheet;performing an optional scale removal process on the hot rolled steel sheet;subjecting the hot rolled steel sheet to an optional annealing at a temperature from 350 °C to 750 °C during 1 h to 96 h cold rolling the hot rolled steel sheet with a reduction rate from 35 to 70% to obtain a cold rolled steel sheet;annealing the cold rolled steel sheet in a two step heating during which the dew point is controlled from −15 °C to +15 °C and wherein:the first step starts from heating the steel sheet from room temperature to a temperature HT1 from 600 °C to 800 °C, with a heating rate HR1 from 2 °C / s to 70 °C / s,the second step starts from heating further the steel sheet from HT1 to a soaking temperature TA from Ac3−10 °C and Ac3+100 °C, with a heating rate HR2 from 0.1 °C / s to 10 °C / s or less, HR2 being lower than HR1,then annealing at TA during 10 to 1000 seconds, the dew point being controlled from −10 °C to +10 °C during the annealing;then cooling the said cold rolled steel sheet wherein:an optional first step of cooling the cold rolled steel sheet starts from TA down to a temperature CT1 from 580 °C to 860 °C, with a cooling rate CR1 from 0.01 °C / s to 15 °C / s;a cooling step starts from CT1 or TA down to a temperature CT2 from Ms-30 °C to 20 °C, with a cooling rate CR2 of at least 10 °C / s;then heating the cold rolled steel sheet from CT2 temperature to an overaging temperature TOA from 250 °C to 580 °C at an average heating rate HR3 from 1 °C / s to 100 °C / s;then overaging the cold rolled steel sheet at TOA for 5 to 500 seconds;then the cold rolled steel sheet is cooled to room temperature to obtain a cold rolled and heat-treated steel sheet.

28. The method as recited in claim 27 wherein the HT1 temperature is from 625 °C to 775 °C.

29. A method comprising employing the steel sheet produced according to the method as recited in claim 27 for the manufacture of structural or safety parts of a vehicle.

30. A method comprising employing the steel sheet as recited in claim 16 for the manufacture of structural or safety parts of a vehicle.

31. A vehicle comprising a part obtained according to the method as recited in claim 30.

31. A vehicle comprising a part obtained according to the method as recited in claim 29.