Ni-BASED ALLOY

The Ni-based alloy addresses strength, corrosion resistance, and hot workability issues by optimizing element composition and production conditions, resulting in improved mechanical and corrosion performance.

US20260357382A1Pending Publication Date: 2026-11-12DAIDO STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
US19/669156
Authority / Receiving Office
US · United States
Patent Type
Applications(United States)
Current Assignee / Owner
Priority Date
2026-04-10
Filing Date
2026-05-06
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing Ni-based alloys face challenges in achieving high strength, corrosion resistance, and hot workability, particularly in high-temperature and high chloride ion environments, with limitations in manufacturing cost and process efficiency.

Method used

A Ni-based alloy composition with controlled element ranges and optimized production conditions, including specific limits on elements like C, Si, Mn, Cr, Mo, Nb, Ti, B, and others, along with segregation control, enhances strength and corrosion resistance while improving hot workability.

Benefits of technology

The alloy achieves a crack occurrence rate of 1.0% or less at 950 °C, 0.2% proof stress of 880 MPa or more, and corrosion weight loss of 0.35 g/(m2·h) or less, demonstrating excellent mechanical and corrosion properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A Ni-based alloy consisting of, in terms of mass %: C≤0.10%; Si≤1.0%; Mn≤1.0%; Cu≤3.5%; 16.0%≤Cr≤25.0%; 10.0%≤Mo≤17.0%; 3.5%≤Nb≤6.5%; 0.10%≤Ti≤2.00%; 0.15%≤Al≤0.50%; 0%≤B≤0.0200%; 0%≤Mg+Ca+Zr+Hf≤0.0200%; P≤0.05%; S≤0.0050%; Fe≤3.0%; O≤0.0200%; N≤0.0300%; V≤0.20%; Ta≤0.20%; Co≤1.0%; and W≤0.10%, with the balance being Ni and unavoidable impurities, and satisfying the following formulae (1), (2), and (3), 0.0010 mass %≤B+Mg+Ca+Zr+Hf≤0.0200 mass % (1), Nb (seg)=Nb (max)−Nb (min)≤1.5 mass % (2), Mo (seg)=Mo (max)−Mo (min)≤0.6 mass % (3).
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application is based on and claims priority under 35 USC 119 from Japanese Patent Applications No. 2025-077653 filed on May 7, 2025, No. 2025-134620 filed on Aug. 13, 2025, and No. 2026-064809 filed on Apr. 10, 2026, the entire content of which is incorporated herein by reference.TECHNICAL FIELD

[0002] The present invention relates to a Ni-based alloy, and more specifically to a Ni-based alloy excellent in strength, corrosion resistance, and hot workability.BACKGROUND ART

[0003] Since Ni-based alloys (or Ni-based superalloys) are excellent in high-temperature strength, creep characteristics, and corrosion resistance, they are used for geothermal power generation components, petroleum drilling components, jet engine members, gas turbine members, nuclear reactor members, and the like.

[0004] The Ni-based alloy is roughly classified into a solid-solution-hardened alloy and a precipitation-hardened alloy. Examples of the solid-solution-hardened alloy include Ni—Cr—Mo-based alloys such as A625 (Inconel (registered trademark) 625), Hastelloy (registered trademark) C-276, and C-22. Examples of the precipitation-hardened alloy include A625 Plus obtained by hardening A625.

[0005] Various proposals have been made regarding such Ni-based alloys.

[0006] For example, Patent Literature 1 discloses a high-hardness, high-corrosion resistance Ni-based alloy obtained by

[0007] (a) producing an alloy powder containing a predetermined content of C, Si, Mn, Cr, Mo, Nb, Ta, Al, Ti, Fe, N, and O, with the balance being Ni and unavoidable impurities,

[0008] (b) molding and sintering the alloy powder, and

[0009] (c) subjecting the sintered body to a solution heat treatment and an aging treatment.

[0010] This literature discloses that when gamma double prime (Ni3(Nb, Ta)) is age precipitated in a matrix in addition to optimizing an alloy composition, high hardness is obtained without impairing the corrosion resistance of the alloy.

[0011] Among Ni-based alloys in the related art, Ni—Cr—Mo-based alloys such as A625, Hastelloy (registered trademark) C-276, and C-22 generally have a low strength. In contrast, A625 Plus has a strength higher than that of A625, but is insufficient in corrosion resistance under high-temperature and high chloride ion concentration environments required for deep geothermal power generation.

[0012] Since the Ni-based alloy disclosed in Patent Literature 1 is difficult to hot-work, it is necessary to use a powder metallurgy method to produce a component having a predetermined shape. To reduce a manufacturing cost of the component, it is desired to improve hot workability of the Ni-based alloy.

[0013] Patent Literature 1: JP2002-302726ASUMMARY OF INVENTION

[0014] An object of the present invention is to provide a Ni-based alloy excellent in strength, corrosion resistance, and hot workability.

[0015] The present invention has the following configurations.

[0016] 1. A Ni-based alloy consisting of:

[0017] C≤0.10 mass %;

[0018] Si≤1.0 mass %;

[0019] Mn≤1.0 mass %;

[0020] Cu≤3.5 mass %;

[0021] 16.0 mass %≤Cr≤25.0 mass %;

[0022] 10.0 mass %≤Mo≤17.0 mass %;

[0023] 3.5 mass %≤Nb≤6.5 mass %;

[0024] 0.10 mass %≤Ti≤2.00 mass %;

[0025] 0.15 mass %≤Al≤0.50 mass %;

[0026] 0 mass %≤B≤0.0200 mass %;

[0027] 0 mass %≤Mg+Ca+Zr+Hf≤0.0200 mass %;

[0028] P limited to 0.05 mass % or less;

[0029] S limited to 0.0050 mass % or less;

[0030] Fe limited to 3.0 mass % or less;

[0031] O limited to 0.0200 mass % or less;

[0032] N limited to 0.0300 mass % or less;

[0033] V limited to 0.20 mass % or less;

[0034] Ta limited to 0.20 mass % or less;

[0035] Co limited to 1.0 mass % or less; and

[0036] W limited to 0.10 mass % or less,

[0037] with the balance being Ni and unavoidable impurities, and

[0038] satisfying the following formulae (1), (2), and (3),0.0010 mass %≤B+Mg+Ca+Zr+Hf≤0.0200 mass %  Formula (1),Nb (seg)=Nb (max)−Nb (min)≤1.5 mass % Formula  (2), andMo (seg)=Mo (max)−Mo (min)≤0.6 mass %  Formula (3)whereNb (seg) is a degree of Nb segregation,Nb (max) is a maximum value of a content of Nb measured by EPMA surface analysis,Nb (min) is a minimum value of the content of Nb measured by the EPMA surface analysis,

[0043] Mo (seg) is a degree of Mo segregation,

[0044] Mo (max) is a maximum value of a content of Mo measured by the EPMA surface analysis, and

[0045] Mo (min) is a minimum value of the content of Mo measured by the EPMA surface analysis.

[0046] 2. The Ni-based alloy according to the above 1, having a crack occurrence rate at 950 °C of 1.0% or less,

[0047] in which the “crack occurrence rate” indicates a ratio (=n×100 / n0) of the number n of compression test pieces having no cracks after a 50% compression test to a total number no (n0≥5) of compression test pieces when the total number no of compression test pieces is subjected to the 50% compression test, and

[0048] the “50% compression test” indicates a test in which the compression test piece having a diameter of 15 mm and a height of 22.5 mm is prepared from the Ni-based alloy after a solution heat treatment, and the compression test piece is subjected to compression until the height of the compression test piece reaches 50%+2.5%.

[0049] 3. The Ni-based alloy according to the above 1, having a 0.2% proof stress at 25 °C of 880 MPa or more,

[0050] in which the “0.2% proof stress” indicates a stress at which a strain is 0.2% when a standard test piece with a parallel portion having a diameter of 6 mm is prepared from the Ni-based alloy after an aging treatment in accordance with ASTM E8 and the standard test piece is subjected to a tensile test in accordance with ASTM E8.

[0051] 4. The Ni-based alloy according to the above 1, having a corrosion weight loss of 0.35 g / (m2·h) or less,

[0052] in which the “corrosion weight loss” indicates a value obtained by preparing a cylindrical test piece having a diameter of 10 mm and a height of 50.0 mm from the Ni-based alloy after a hot working, after a solution heat treatment, or after an aging treatment, measuring a mass loss after immersing the cylindrical test piece in a boiling 5% sulfuric acid aqueous solution for 6 hours, and dividing the mass loss by a total surface area of the cylindrical test piece and an immersion time.

[0053] In a precipitation-hardened Ni-based alloy, when S segregates at a grain boundary, the hot workability decreases. In contrast, B has an effect of preventing the segregation of S at the grain boundary by preferentially segregating B itself at the grain boundary. Each of Mg, Ca, Zr, and Hf has an effect of preventing the segregation of S at the grain boundary by bonding with S to form a sulfide. Therefore, when an appropriate content of at least one element selected from the group consisting of B, Mg, Ca, Zr, and Hf is added to the precipitation-hardened Ni-based alloy, the hot workability of the Ni-based alloy is improved.

[0054] When components and production conditions are optimized such that component segregation (in particular, segregation of Nb and segregation of Mo) is prevented in a state after a solution heat treatment and an appropriate amount of a gamma double prime phase is precipitated after an aging treatment, both high strength and high corrosion-resistance can be achieved.DESCRIPTION OF EMBODIMENTS

[0055] Hereinafter, an embodiment of the present invention will be described in detail.1. Ni-Based Alloy1.1. Components

[0056] The Ni-based alloy according to the present invention contains the following elements, with the balance being Ni and unavoidable impurities. Types of added elements, component ranges thereof, and reasons for limitation thereof are as follows.1.1.1. Main Components(1) C≤0.10 Mass %:

[0057] In the present invention, C is an element that may be contained as an impurity. When a content of C is excessive, carbides of Nb and Ti are likely to be formed. As a result, a precipitation amount of the gamma double prime (Ni3Nb or Ni3(Nb,Ta)) phase, which is a strengthening phase, decreases, and the strength may decrease. Therefore, the content of C needs to be 0.10 mass % or less. The content of C is preferably 0.050 mass % or less, more preferably 0.020 mass % or less, and still more preferably 0.010 mass % or less.

[0058] The smaller the content of C, the better. However, extreme reduction in the content of C causes an increase in manufacturing cost. Considering the manufacturing cost, the content of C is preferably 0.0005 mass % or more.(2) Si≤1.0 Mass %:

[0059] In the present invention, Si is an element that may be contained as an impurity. Si is effective as a deoxidizer at a time of melting, but when a content of Si becomes excessive and excessive Si is dissolved in a matrix, toughness may decrease. Therefore, the content of Si needs to be 1.0 mass % or less. The content of Si is preferably 0.30 mass % or less, more preferably 0.20 mass % or less, and still more preferably 0.15 mass % or less.

[0060] The smaller the content of Si, the better. However, extreme reduction in the content of Si causes an increase in manufacturing cost. Considering the manufacturing cost, the content of Si is preferably 0.07 mass % or more.(3) Mn≤1.0 Mass %:

[0061] In the present invention, Mn is an element that may be contained as an impurity. When a content of Mn is excessive, MnS is excessively formed, and the corrosion resistance may decrease. Therefore, the content of Mn needs to be 1.0 mass % or less. The content of Mn is preferably 0.50 mass % or less, more preferably 0.20 mass % or less, and still more preferably 0.10 mass % or less.

[0062] An appropriate content of Mn forms an appropriate content of MnS to prevent deterioration of the hot workability due to S. However, when the deterioration of the hot workability due to S can be prevented by another method, it is not necessary to add Mn, and smaller the content of Mn, the better. However, extreme reduction in the content of Mn causes an increase in manufacturing cost. Considering the manufacturing cost, the content of Mn is preferably 0.05 mass % or more.(4) Cu≤3.5 Mass %:

[0063] The Ni-based alloy does not necessarily contain Cu. However, Cu has an effect of improving the corrosion resistance of the matrix by Cu dissolving in the matrix. To achieve such an effect, a content of Cu is preferably 0.05 mass % or more.

[0064] In contrast, when the content of Cu is excessive, a component balance in the matrix is lost. As a result, the precipitation amount of the gamma double prime phase may decrease, and the strength may decrease. Therefore, the content of Cu needs to be 3.5 mass % or less. The content of Cu is preferably 1.0 mass % or less, more preferably 0.30 mass % or less, and still more preferably 0.10 mass % or less.(5) 16.0 Mass %≤Cr≤25.0 Mass %:

[0065] Cr is an element that most effectively improves the corrosion resistance of the Ni-based alloy. When an appropriate content of Cr is dissolved in the matrix, a Cr-based oxide film excellent in corrosion resistance is formed on a surface, and thus, the corrosion resistance of the matrix is improved. To obtain high corrosion-resistance, a content of Cr needs to be 16.0 mass % or more. The content of Cr is preferably 18.0 mass % or more and more preferably 20.0 mass % or more.

[0066] In contrast, when the content of Cr is excessive, a σ phase (an intermetallic compound containing Cr as a main component) is likely to be precipitated. When the σ phase precipitates, not only corrosion resistance but also toughness decreases. Therefore, the amount of Cr needs to be 25.0 mass % or less. The amount of Cr is preferably 24.0 mass % or less, more preferably 23.0 mass % or less, and still more preferably 22.0 mass % or less.(6) 10.0 Mass %≤Mo≤17.0 Mass %:

[0067] Mo is an element that effectively improves the corrosion resistance of the Ni-based alloy. Mo has an effect of improving the corrosion resistance by densifying the Cr-based oxide film. To obtain high corrosion-resistance, a content of Mo needs to be 10.0 mass % or more.

[0068] In contrast, when the amount of Mo is excessive, the formation of the σ phase is promoted, and the toughness may decrease. Therefore, the content of Mo needs to be 17.0 mass % or less. The content of Mo is preferably 15.0 mass % or less, 13.0 mass % or less, or 11.0 mass % or less.(7) 3.5 mass %≤Nb≤6.5 Mass %:

[0069] Nb has an effect of precipitating the gamma double prime phase in the matrix and improving the strength of the Ni-based alloy. To obtain a high strength, a content of Nb needs to be 3.5 mass % or more. The content of Nb is preferably 4.5 mass % or more.

[0070] In contrast, when the content of Nb is excessive, the hot workability may decrease. Therefore, the content of Nb needs to be 6.5 mass % or less. The content of Nb is preferably 5.5 mass % or less.(8) 0.10 Mass %≤Ti≤2.00 mass %:

[0071] Ti has an effect of stabilizing the gamma double prime phase and preventing precipitation of the σ phase. To obtain such an effect, a content of Ti needs to be 0.10 mass % or more.

[0072] In contrast, when the content of Ti is excessive, the gamma double prime phase may become unstable. In addition, the hot workability may deteriorate. Therefore, the content of Ti needs to be 2.00 mass % or less. The content of Ti is preferably 1.00 mass % or less, more preferably 0.70 mass % or less, and still more preferably 0.50 mass % or less.(9) 0.15 Mass %≤Al≤0.50 Mass %:

[0073] Al has an effect of stabilizing the gamma double prime phase and preventing precipitation of the σ phase. To obtain such an effect, a content of Al needs to be 0.15 mass % or more.

[0074] In contrast, when the content of Al is excessive, the gamma double prime phase may become unstable. Therefore, the content of Al needs to be 0.50 mass % or less. The content of Al is preferably 0.30 mass % or less.(10) 0 Mass %≤B≤0.0200 mass %:In a precipitation-hardened Ni-based alloy, when S segregates at a grain boundary, the hot workability decreases. In contrast, B has an effect of preventing the segregation of S at the grain boundary by preferentially segregating B itself at the grain boundary. Therefore, to improve the hot workability, B is preferably added. However, when sufficient hot workability is obtained by other elements, a content of B may be 0 mass %.

[0076] In contrast, when the content of B is excessive, a boride precipitates, and the toughness may decrease. Therefore, the content of B needs to be 0.0200 mass % or less. The content of B is preferably 0.0100 mass % or less.(11) 0 Mass %≤Mg+Ca+Zr+Hf≤0.0200 Mass %:

[0077] Each of Mg, Ca, Zr, and Hf has an effect of preventing the segregation of S at the grain boundary by bonding with S to form a sulfide. To improve the hot workability, it is preferable to add at least one element selected from the group consisting of Mg, Ca, Zr, and Hf. However, when sufficient hot workability is obtained by other elements, a total content of Mg, Ca, Zr, and Hf may be 0 mass %.

[0078] In contrast, when the total content of Mg, Ca, Zr, and Hf is excessive, a hard inclusion may precipitate, and the toughness may decrease. Therefore, the total content needs to be 0.0200 mass % or less. The total content is more preferably 0.0100 mass % or less.1.1.2. Component Balance

[0079] The Ni-based alloy according to the present invention satisfies the following formula (1).0.0010 mass %≤B+Mg+Ca+Zr+Hf≤0.0200 mass %  Formula (1)

[0080] Formula (1) represents a suitable range of a total content of B, Mg, Ca, Zr, and Hf. All of these elements have an effect of improving the hot workability of the Ni-based alloy. As long as Formula (1) is satisfied, the Ni-based alloy may contain any one of these elements, or may contain two or more thereof.

[0081] When the total content of B, Mg, Ca, Zr, and Hf is too small, the hot workability may deteriorate. Therefore, the total content needs to be 0.0010 mass % or more.

[0082] In contrast, when the total content of these elements is excessive, a hard inclusion precipitates, and the toughness may decrease. Therefore, the total content needs to be 0.0200 mass % or less.1.1.3. Component Segregation

[0083] The Ni-based alloy according to the present invention further satisfies the following formulae (2) and (3) in addition to Formula (1).Nb (seg)=Nb (max)−Nb (min)≤1.5 mass %  Formula (2)Mo (seg)=Mo (max)−Mo (min)≤0.6 mass %  Formula (3)whereNb (seg) is a degree of Nb segregation,

[0086] Nb (max) is a maximum value of the content of Nb measured by EPMA surface analysis,

[0087] Nb (min) is a minimum value of the content of Nb measured by the EPMA surface analysis,

[0088] Mo (seg) is a degree of Mo segregation,

[0089] Mo (max) is a maximum value of the content of Mo measured by the EPMA surface analysis, and

[0090] Mo (min) is a minimum value of the content of Mo measured by the EPMA surface analysis.

[0091] The degree of Nb segregation and the degree of Mo segregation are calculated from

[0092] electron probe microanalyzer (EPMA) surface analysis measurements results at any cross section. A measurement region of the EPMA may be set in consideration of inclusion of carbide and noise. For example, the measurement region can be 3 mm×3 mm, and the number of divisions can be 400×400. When the degree of Nb segregation and the degree of Mo segregation are calculated, measured raw data is subjected to pretreatment. For example, as a pretreatment for calculating the degree of Nb segregation, a carbide portion and a noise affected portion are removed from the raw data. Even when the degree of Mo segregation is calculated, the same pretreatment can be performed.

[0093] In the Ni-based alloy according to the present invention, a zero ductility temperature is lowered in a positive segregation portion of Nb, and the hot workability decreases. In a negative segregation portion of Nb, the gamma double prime phase is not sufficiently precipitated, and a high 0.2% proof stress is not obtained. Therefore, the degree of Nb segregation needs to be 1.5 mass % or less.

[0094] In the Ni-based alloy according to the present invention, the zero ductility temperature is lowered in a positive segregation portion of Mo, and the hot workability decreases. In a negative segregation portion of Mo, high corrosion-resistance is not obtained. Therefore, the degree of Mo segregation needs to be 0.6 mass % or less.1.1.4. Unavoidable Impurities

[0095] The Ni-based alloy according to the present invention may contain unavoidable impurities. Here, the “unavoidable impurities” are components contained due to various factors, such as a raw material and a production step when the Ni-based alloy is industrially produced, and a content thereof is within a range that does not adversely affect properties of the Ni-based alloy according to the present invention.

[0096] Among the unavoidable impurities, C, Si, and Mn need to be limited to the above-described ranges.

[0097] Among the unavoidable impurities, P, S, Fe, O, N, V, Ta, Co, and W need to be limited to the following ranges.(1) P≤0.05 Mass %:

[0098] In the present invention, P is an element that may be contained as an impurity. When a content of P is excessive, the hot workability may decrease. Therefore, the content of P needs to be 0.05 mass % or less.

[0099] The smaller the content of P, the better. However, extreme reduction in the content of P causes an increase in manufacturing cost. Therefore, the content of P is preferably 0.005 mass % or more.(2) S≤0.0050 Mass %:

[0100] In the present invention, S is an element that may be contained as an impurity. When a content of S is excessive, the hot workability may decrease. Therefore, the content of S needs to be 0.0050 mass % or less.

[0101] The smaller the content of S, the better. However, extreme reduction in the content of S causes an increase in manufacturing cost. Therefore, the content of S is preferably 0.0005 mass % or more.(3) Fe≤3.0 Mass %:

[0102] In the present invention, Fe is an element that may be contained as an impurity. When a content of Fe is excessive, the corrosion resistance may decrease. Therefore, the content of Fe needs to be 3.0 mass % or less. The content of Fe is preferably 2.0 mass % or less, and more preferably 1.0 mass % or less.

[0103] The smaller the content of Fe, the better. However, extreme reduction in the content of Fe causes an increase in manufacturing cost. Considering the manufacturing cost, the content of Fe is preferably 0.01 mass % or more.(4) O≤0.0200 Mass %:

[0104] In the present invention, O is an element that may be contained as an impurity. When a content of O is excessive, an alloy element is consumed to form an oxide, and the corrosion resistance may decrease. Therefore, the content of O needs to be 0.0200 mass % or less.

[0105] The smaller the content of O, the better. However, extreme reduction in the content of O causes an increase in manufacturing cost. Considering the manufacturing cost, the content of O is preferably 0.001 mass % or more.(5) N≤0.0300 Mass %:

[0106] In the present invention, N is an element that may be contained as an impurity. When a content of N is excessive, the alloy element is consumed to form an nitride, and the corrosion resistance may decrease. Therefore, the content of N needs to be 0.0300 mass % or less.

[0107] The smaller the content of N, the better. However, extreme reduction in the content of N causes an increase in manufacturing cost. Considering the manufacturing cost, the content of N is preferably 0.005 mass % or more.(6) V≤0.20 Mass %:

[0108] In the present invention, Vis an element that may be contained as an impurity. When a content of V is excessive, a V-based carbonitride is formed, and the toughness may decrease. Therefore, the content of V needs to be 0.20 mass % or less.

[0109] The smaller the content of V, the better. However, extreme reduction in the content of V causes an increase in manufacturing cost. Considering the manufacturing cost, the content of V is preferably 0.005 mass % or more.(7) Ta≤0.20 mass %:

[0110] In the present invention, Ta is an element that is substituted for a part of Nb to form the gamma double prime phase Ni3(Nb, Ta). Since the Ni-based alloy according to the present invention basically uses the gamma double prime phase Ni3Nb, Ta is not essential. Therefore, a lower limit value of a content of Ta is 0 mass %.

[0111] In contrast, when the content of Ta is excessive, deformation resistance in a hot working temperature range increases, and workability may decrease. Therefore, the content of Ta needs to be 0.20 mass % or less.(8) Co≤1.0 mass %:

[0112] In the present invention, Co is an element that may be contained as an impurity. When a content of Co is excessive, the component balance in the matrix is lost. As a result, the precipitation amount of the gamma double prime phase may decrease, and the strength may decrease. When the content of Co is excessive, cost is increased. Therefore, the content of Co needs to be 1.0 mass % or less.

[0113] The smaller the content of Co, the better. However, extreme reduction in the content of Co causes an increase in manufacturing cost. Therefore, the amount of Co is preferably 0.005 mass % or more.(9) W≤0.10 Mass %:

[0114] In the present invention, W is an element that may be contained as an impurity. When a content of W is excessive, the component balance in the matrix is lost. As a result, the precipitation amount of the gamma double prime phase may decrease, and the strength may decrease. When the content of W is excessive, cost is increased. Therefore, the content of W needs to be 0.10 mass % or less.

[0115] The smaller the content of W, the better. However, extreme reduction in the content of W causes an increase in manufacturing cost. Therefore, the content of W is preferably 0.0001 mass % or more.1.2. Properties

[0116] As will be described later, the Ni-based alloy according to the present invention is produced by melting and casting a raw material blended to have a predetermined component, hot-working an obtained ingot, subjecting a hot-worked body to the solution heat treatment, and subjecting a solution-heat-treated body to the aging treatment. In this case, when components and heat treatment conditions are optimized, the Ni-based alloy according to the present invention exhibits excellent properties.1.2.1. Crack Occurrence Rate

[0117] A “crack occurrence rate” indicates a ratio (=n×100 / n0) of the number n of compression test pieces having no cracks after a 50% compression test to a total number no (n0≥5) of compression test pieces when the total number no (n0≥5) of compression test pieces is subjected to a 50% compression test.

[0118] The “50% compression test” indicates a test in which the compression test piece having a diameter of 15 mm and a height of 22.5 mm is prepared from the Ni-based alloy after the solution heat treatment, and the compression test piece is subjected to compression until the height of the compression test piece reaches 50%+2.5%.

[0119] A “crack occurrence rate at 950 °C” refers to a crack occurrence rate when the 50% compression test is performed using a compression test piece heated to 950 °C.

[0120] Since the Ni-based alloy according to the present invention contains an appropriate content of B, Mg, Ca, Zr, and Hf, the Ni-based alloy exhibits high hot workability in a state after the solution heat treatment. A quality of hot workability can be evaluated by the crack occurrence rate at 950 °C.

[0121] In the Ni-based alloy according to the present invention, when the components are optimized, the crack occurrence rate at 950 °C is 1.0% or less in a state after the solution heat treatment. When the components are further optimized, the crack occurrence rate at 950 °C is 0.1% or less.1.2.2. 0.2% Proof Stress

[0122] A “0.2% proof stress” indicates a stress at which a strain is 0.2% when a standard test piece with a parallel portion having a diameter of 6 mm is prepared from the Ni-based alloy after the aging treatment in accordance with ASTM E8 and the standard test piece is subjected to a tensile test in accordance with ASTM E8.

[0123] The Ni-based alloy according to the present invention is a precipitation-hardened alloy. Therefore, when the solution heat treatment and the aging treatment are performed under appropriate conditions, the gamma double prime phase is precipitated in the matrix, and high strength is exhibited in both the low temperature range and the high temperature range.

[0124] In the Ni-based alloy according to the present invention, when the components and the heat treatment conditions are optimized, the 0.2% proof stress at 25 °C is 880 MPa or more in a state after the aging treatment. When the components and the heat treatment conditions are further optimized, the 0.2% proof stress at 25 °C is 900 MPa or more or 940 MPa or more in the state after the aging treatment.1.2.3. Corrosion Weight Loss

[0125] A “corrosion weight loss” indicates a value obtained by preparing a cylindrical test piece having a diameter of 10 mm and a height of 50.0 mm from the Ni-based alloy after the hot working, after the solution heat treatment, or after the aging treatment, measuring a mass loss after immersing the cylindrical test piece in a boiling 5% sulfuric acid aqueous solution for 6 hours, and dividing the mass loss by a total surface area of the cylindrical test piece and an immersion time.

[0126] Since the components of the Ni-based alloy according to the present invention are optimized, the Ni-based alloy exhibits high corrosion-resistance in any one or more states after the hot working, after the solution heat treatment, or after the aging treatment.

[0127] In the Ni-based alloy according to the present invention, when the components are optimized, the corrosion weight loss is 0.35 g / (m2·h) or less in any one or more states after the hot working, after the solution heat treatment, or after the aging treatment. When the components are further optimized, the corrosion weight loss is 0.33 g / (m2·h) or less or 0.30 g / (m2·h) or less in any one or more states after the hot working, after the solution heat treatment, or after the aging treatment.2. Method for Producing Ni-Based Alloy

[0128] A method for producing a Ni-based alloy according to the present invention includes:

[0129] a first step of melting and casting a raw material blended to have a predetermined composition;

[0130] a second step of subjecting an ingot to homogenization heat treatment as necessary;

[0131] a third step of subjecting the ingot or a homogenization-heat-treated body to coarse hot-working as necessary;

[0132] a fourth step of subjecting the ingot, the homogenization-heat-treated body, or a coarse hot-worked body to fine hot-working;

[0133] a fifth step of subjecting a fine-hot-worked body to the solution heat treatment as necessary;

[0134] a sixth step of subjecting the coarse-hot-worked body or the solution-heat-treated body to cold working as necessary; and

[0135] a seventh step of subjecting the fine-hot-worked body, the solution-heat-treated body, or a cold-worked body to the aging treatment.2.1. First Step

[0136] First, the raw materials blended to have a predetermined composition are melted and cast (first step). A method for melting and casting the raw materials is not particularly limited in the present invention, and an optimum method can be selected depending on a purpose thereof.

[0137] The melting is preferably vacuum melting using a vacuum induction furnace. Since segregation is likely to occur in the Ni-based alloy according to the present invention, secondary melting such as electroslag remelting (ESR) or vacuum arc remelting (VAR) is preferably performed when segregation is significant.2.2. Second Step

[0138] Next, as necessary, the ingot is subjected to the homogenization heat treatment (second step). The homogenization heat treatment is performed in the case where segregation of the ingot is significant. Therefore, in the case where the segregation of the ingot is small (for example, in the case where a size of the ingot is relatively small), the homogenization heat treatment can be omitted.

[0139] Conditions of the homogenization heat treatment are not particularly limited as long as the segregation of the ingot can be removed or reduced. Specifically, the homogenization heat treatment is preferably performed at 1150 °C to 1280 °C for 12 hours or more.2.3. Third Step

[0140] Next, as necessary, the ingot or the homogenization-heat-treated body is subjected to the coarse hot-working (third step). In the case where the size of the ingot is relatively large and a multi-stage process is required until the ingot is processed into a final product shape, the coarse hot-working is performed to process the ingot into an intermediate material, such as billet and bloom, having an appropriate size and shape. Therefore, in the case where the size of the ingot is relatively small, the coarse hot-working can be omitted.

[0141] A method and conditions of the coarse hot-working are not particularly limited as long as the method and conditions enable the ingot to be processed into the intermediate material having an appropriate size and shape. Examples of the coarse hot-working include hot-forging and hot-rolling.

[0142] In the case where a working temperature of the coarse hot-working is too low or too high, cracking is likely to occur in a workpiece. Therefore, the coarse hot-working is preferably performed in a temperature range of 1200 °C to 900 °C.2.4. Fourth Step

[0143] Next, the ingot, the homogenization-heat-treated body, or the coarse hot-worked body is subjected to the fine hot-working (fourth step). The fine hot-working is performed to process the ingot or the intermediate material into a final product shape or a shape close thereto. The fine hot-working may be performed only once or may be performed a plurality of times.

[0144] A method and conditions of the fine hot-working are not particularly limited as long as the method and the conditions enable the ingot or the intermediate material to be processed into a final product shape or a shape close thereto. Since details of the method and the conditions of the fine hot-working are the same as those of the coarse hot-working, a description thereof will be omitted.

[0145] In the case where the fine hot-working is performed a plurality of times, the solution heat treatment to be described later may be performed in the middle.2.5. Fifth Step

[0146] Next, as necessary, the solution heat treatment is performed on the fine-hot-worked body (fifth step). The solution heat treatment is performed to dissolve a precipitate in the matrix.

[0147] Conditions of the solution heat treatment are not particularly limited as long as the conditions enable the precipitate to be dissolved in the matrix. Specifically, a temperature of the solution heat treatment is preferably 1000 °C to 1080 °C. A time of approximately 0.5 hours to 1.0 hour is sufficient for the solution heat treatment. A cooling method may be any of air cooling, oil cooling, and water cooling.

[0148] In the state where the fine hot-working is ended, the precipitate may be sufficiently dissolved in the matrix. In such a case, the solution heat treatment can be omitted.2.6. Sixth Step

[0149] Next, as necessary, the cold working is performed on the coarse hot-worked body or the solution-heat-treated body (sixth step). Since hardness is extremely large after the aging treatment, in the case where the cold working is necessary, the cold working is preferably performed before the aging treatment. A method of cold working is not particularly limited. Examples of the cold working include cutting and grinding.2.7. Seventh Step

[0150] Next, the fine hot-worked body, the solution-heat-treated body, or the cold-worked body is subjected to the aging treatment (seventh step). Accordingly, a Ni-based alloy having a high strength and high corrosion-resistance is obtained.

[0151] As conditions of the aging treatment, optimum conditions can be selected depending on the purpose. Specific examples of the aging treatment method include:

[0152] (a) one-stage aging in which the aging treatment is performed for a long time at a low temperature to a high temperature; and

[0153] (b) two-stage aging in which first stage aging is performed at a high temperature, and then second stage aging is performed at a low temperature. In the present invention, any of the methods may be used.

[0154] In the case of one-stage aging, the aging treatment is preferably performed at 600 °C. to 800 °C for 8 hours to 48 hours. Even in the one-stage aging, when an aging treatment temperature and an aging treatment time are optimized, a Ni-based alloy having the 0.2% proof stress of 880 MPa or more is obtained.

[0155] In the case of two-stage aging,

[0156] (a) the first stage aging is preferably performed at 700 °C to 800 °C for 8 hours to 16 hours, and

[0157] (b) the second stage aging is preferably performed at 600 °C to 700 °C for 8 hours to 16 hours.

[0158] Low-temperature aging at 600 °C to 700 °C alone takes a long time to precipitate a sufficient amount of gamma double prime phase. Therefore, the precipitation of the gamma double prime phase is promoted by performing the first stage aging treatment at a higher temperature than the second stage aging treatment. Next, a sufficient amount of gamma double prime phase is precipitated by performing the second stage aging at a low temperature. As a result, the two-stage aging can precipitate a large amount of gamma double prime phase in a shorter time than the low-temperature aging treatment at 600 °C to 700 °C. Accordingly, a Ni-based alloy having the 0.2% proof stress of 900 MPa or more, or 940 MPa or more is obtained.3. Effects

[0159] In the precipitation-hardened Ni-based alloy, when S segregates at the grain boundary, the hot workability decreases. In contrast, B has an effect of preventing the segregation of S at the grain boundary by preferentially segregating B itself at the grain boundary. Each of Mg, Ca, Zr, and Hf has an effect of preventing the segregation of S at the grain boundary by bonding with S to form a sulfide. Therefore, when an appropriate content of at least one element selected from the group consisting of B, Mg, Ca, Zr, and Hf is added to the precipitation-hardened Ni-based alloy, the hot workability of the Ni-based alloy is improved.

[0160] When components and production conditions are optimized such that component segregation (in particular, segregation of Nb and segregation of Mo) is prevented in the state after the solution heat treatment and an appropriate amount of the gamma double prime phase is precipitated after the aging treatment, both high strength and high corrosion-resistance can be achieved.EXAMPLESExamples 1 to 17 and Comparative Examples 1 to 151. Preparation of Samples

[0161] In a vacuum induction furnace, 50 kg of a raw material having a composition shown in Table 1 and Table 2 was vacuum melted to obtain an ingot. Among the obtained ingots, ingots other than that of Comparative Example 15 were subjected to a homogenization heat treatment at 1200 °C for 24 hours. The ingot of Comparative Example 15 was not subjected to the homogenization heat treatment. Next, hot forging was performed in a temperature range of 900 °C to 1200 °C to produce a round bar having a diameter of 20 mm. The round bar was subjected to the solution heat treatment at 1050 °C for 1 hour, and then cooled with water.

[0162] In Examples 1, 2, 4 and 6, a one-stage aging treatment was performed at 700 °C to 780 °C for 24 to 48 hours.

[0163] In other Examples and Comparative Examples, two stage aging treatment was performed under the following conditions.

[0164] (a) First stage: an aging treatment at 720 °C to 760 °C for 8 to 16 hours.

[0165] (b) Second stage: an aging treatment at 610 °C to 630 °C for 8 to 16 hours.

[0166] Specific aging treatment conditions of each sample were set in consideration of a balance between proof stress and corrosion resistance.TABLE 1Compositions (mass %)CSiMnPSCrMoAlTiNbBExample 10.0020.100.030.0050.001221.4010.430.191.383.750.0059Example 20.0040.040.050.0040.000917.2313.890.171.413.830.0050Example 30.0040.080.040.0020.000616.1215.240.221.533.790.0059Example 40.0050.050.060.0060.001319.3710.780.210.245.090.0041Example 50.0030.050.050.0040.001020.9810.430.210.195.620.0023Example 60.0070.060.060.0050.000918.7210.550.180.175.360.0058Example 70.0050.070.070.0020.001019.3313.290.220.215.780.0048Example 80.0050.060.060.0020.000624.6711.040.170.186.220.0047Example 90.0040.090.060.0040.000722.7412.210.160.206.390.0051Example 100.0050.070.070.0030.001221.4411.430.200.195.770.0047Example 110.0070.030.060.0060.001120.4010.480.210.195.080.0048Example 120.0070.090.060.0030.001221.4412.210.160.216.22Example 130.0070.060.060.0020.005020.9910.500.210.205.020.0023Example 140.0050.070.070.0060.000620.8710.550.200.215.050.0020Example 150.0050.060.060.0040.000721.0510.560.180.224.980.0021Example 160.0030.050.060.0050.001221.0210.700.160.184.670.0025Example 170.0030.090.040.0020.000920.4214.420.241.213.850.0042Compositions (mass %)OtherB + Mg + Ca +MgCaZrHfONNicompositionsZr + HfExample 10.00380.00200.0098Bal.—0.0097Example 20.00390.00110.0073Bal.—0.0090Example 30.00170.00080.0160Bal.—0.0076Example 40.00310.00090.0135Bal.—0.0072Example 50.00240.00110.0092Bal.—0.0047Example 60.00360.00290.00240.0187Bal.—0.0122Example 70.00230.00290.0142Bal.—0.0071Example 80.00380.00060.0197Bal.—0.0086Example 90.00250.00060.0198Bal.—0.0076Example 100.00260.00080.0088Bal.—0.0073Example 110.00300.00120.0135Bal.Fe: 1.50.0078Example 120.00520.01840.0198Bal.—0.0052Example 130.00250.00090.0092Bal.V: 0.120.0048Example 140.00260.00140.0080Bal.Ta: 0.130.0046Example 150.00240.00150.0110Bal.Co: 0.70.0045Example 160.00210.00240.0092Bal.W: 0.100.0046Example 170.00340.01320.0120Bal.Cu: 2.20.0076TABLE 2Composition (mass %)CSiMnPSCrMoAlTiNbBComparative0.0030.060.030.0020.007518.7210.430.220.243.750.0036Example 1Comparative0.0020.070.050.0060.001015.5210.810.210.193.830.0058Example 2Comparative0.0030.060.040.0040.000926.7215.240.210.173.790.0048Example 3Comparative0.0040.090.040.0050.001022.749.460.180.215.090.0047Example 4Comparative0.0050.070.030.0020.000621.4317.340.220.175.620.0051Example 5Comparative0.0040.060.050.0020.000721.1211.150.050.215.360.0047Example 6Comparative0.0050.090.060.0060.001021.0513.290.660.183.790.0041Example 7Comparative0.0040.050.030.0060.000924.6210.810.210.035.090.0058Example 8Comparative0.0030.050.050.0020.001021.4915.240.182.255.620.0041Example 9Comparative0.0030.060.040.0050.000621.1410.810.210.212.800.0047Example 10Comparative0.0070.070.060.0020.000718.7210.240.220.196.700.0051Example 11Comparative0.0050.070.030.0040.000619.3315.240.210.175.82Example 12Comparative0.0080.050.010.0040.000617.8010.700.130.295.900.0052Example 13Comparative0.0060.050.020.0040.000817.7010.600.320.225.780.0049Example 14Comparative0.0050.090.060.0070.000921.7912.190.150.196.350.0051Example 15Composition (mass %)OtherB + Mg + Ca +MgCaZrHfONNicompositionsZr + HfComparative0.00110.0073Bal.—0.0036Example 1Comparative0.00080.0160Bal.—0.0058Example 2Comparative0.00090.0135Bal.—0.0048Example 3Comparative0.00110.0092Bal.—0.0047Example 4Comparative0.00080.0198Bal.—0.0051Example 5Comparative0.00290.0142Bal.—0.0047Example 6Comparative0.00060.0197Bal.—0.0041Example 7Comparative0.00080.0160Bal.—0.0058Example 8Comparative0.00090.0135Bal.—0.0041Example 9Comparative0.00240.0160Bal.—0.0047Example 10Comparative0.00290.0135Bal.—0.0051Example 11Comparative0.00060.0092Bal.—0.0000Example 12Comparative0.00060.0092Bal.—0.0052Example 13Comparative0.00060.0092Bal.Ta: 0.50.0049Example 14Comparative0.00250.00060.0090Bal.—0.0076Example 152. Test Method2.1. 0.2% Proof StressFrom the round bar after the aging treatment, a standard tensile test piece with a parallel portion having a diameter of 6 mm in accordance with ASTM E8 was prepared. The obtained tensile test piece was subjected to a tensile test at 25 °C in accordance with ASTM E8. The 0.2% proof stress was determined from an obtained stress-strain curve.2.2 Corrosion Weight Loss

[0168] A cylindrical sample having a diameter of 10 mm and a height of 50 mm was prepared from the round bar after the aging treatment. The entire surface of the sample was dry polished using #400 paper. The obtained cylindrical sample was immersed in a boiling 5% sulfuric acid aqueous solution for 6 hours. The corrosion weight loss was calculated using a mass change before and after the immersion test.2.3 Hot Workability (Crack Occurrence Rate)

[0169] A compression test piece having a diameter of 15 mm and a height of 22.5 mm was produced from the round bar after the solution heat treatment. The number of test pieces was six. The obtained compression test pieces were subjected to a 50% compression test at 950 °C. After the compression test, the presence or absence of cracks was visually evaluated, and the crack occurrence rate was calculated.2.4. Degree of Nb Segregation and Degree of Mo Segregation

[0170] A cross section parallel to a longitudinal direction of the round bar was cut out, and an area of 3 mm×3 mm was subjected to EPMA surface analysis with the division number of 400×400. An obtained measured value (raw data) was subjected to a pretreatment for removing a carbide portion and a noise affected portion. The degree of Nb segregation and the degree of Mo segregation were calculated using data obtained by the pretreatment.3. Results

[0171] Results are shown in Table 3. The following can be understood from Table 3.

[0172] Regarding the “crack occurrence rate”, “Good” indicates that the crack occurrence rate is 0%, and “Poor” indicates that the crack occurrence rate is 16% or more (cracking occurs in one or more compression test pieces).

[0173] Regarding the “degree of Nb segregation”, “Good” indicates that the degree of Nb segregation is 1.5 mass % or less, and “Poor” indicates that the degree of Nb segregation is more than 1.5 mass %.

[0174] Regarding the “degree of Mo segregation”, “Good” indicates that the degree of Mo segregation is 0.6 mass % or less, and “Poor” indicates that the degree of Mo segregation is more than 0.6 mass %.

[0175] (1) In Comparative Example 1, the hot workability is poor. This is considered to be because the content of S was excessive.

[0176] (2) In Comparative Example 2, the 0.2% proof stress is low, and the corrosion weight loss is large. This is considered to be because the content of Cr was small.

[0177] (3) In Comparative Example 3, the 0.2% proof stress is low. This is considered to be because the σ phase, which is an embrittlement phase, is precipitated due to the excessive content of Cr.

[0178] (4) In Comparative Example 4, the corrosion weight loss is large. This is considered to be because the content of Mo was small.

[0179] (5) In Comparative Example 5, the hot workability is poor. This is considered to be because the formation of the σ phase was promoted due to the excessive content of Mo.

[0180] (6) In Comparative Example 6, the 0.2% yield strength is low. This is considered to be because the precipitation amount of the gamma double prime phase is small due to a small content of Al.

[0181] (7) In Comparative Example 7, the 0.2% proof stress is low. This is considered to be because the gamma double prime phase became unstable and the precipitation amount of the gamma double prime phase decreased due to the excessive content of Al.

[0182] (8) In Comparative Example 8, the 0.2% proof stress is low. This is considered to be because the content of Ti was small.

[0183] (9) In Comparative Example 9, the hot workability is poor. This is considered to be because the content of Ti was excessive.

[0184] (10) In Comparative Example 10, the 0.2% proof stress is low. This is considered to be because the precipitation amount of the gamma double prime phase is small due to a small content of Nb.

[0185] (11) In Comparative Example 11, the corrosion weight loss is large, and the hot workability is also poor. This is considered to be because the content of Nb was excessive.

[0186] (12) In Comparative Example 12, the hot workability is poor. This is considered to be because none of the elements B, Mg, Ca, Zr, and Hf was contained.

[0187] (13) In Comparative Example 13, the 0.2% proof stress is low. This is considered to be because the precipitation amount of the gamma double prime phase is small due to a small content of Al.

[0188] (14) In Comparative Example 14, the hot workability is poor. This is considered to be because the deformation resistance in the hot working temperature range increased due to an excessive content of Ta.

[0189] (15) In Comparative Example 15, the 0.2% proof stress is low, the corrosion weight loss is large, and the hot workability is poor. This is considered to be because segregation occurred because the homogenization heat treatment was not performed, and the segregation was not eliminated even after the solution heat treatment. Specifically, it is considered that the 0.2% proof stress decreases because the gamma double prime phase is not sufficiently precipitated in the negative segregation portion of Nb. It is considered that the corrosion weight loss increases in the negative segregation portion of Mo because the corrosion resistance decreases. It is considered that the hot workability decreases because the zero ductility temperature decreases in the positive segregation portion of Mo or Nb.

[0190] (16) In Examples 1 to 17, the 0.2% proof stress is high, the corrosion weight loss is small, and the hot workability is good.

[0191] (17) In Examples 1 to 3 and 17, the 0.2% proof stress is slightly low. This is considered to be because the precipitated gamma double prime phase is reduced due to a low content of Nb.TABLE 30.2%CorrosionProofweightHotDegreeDegreestresslosswork-of Nbof MoMPag / m2 · habilitysegregationsegregationExample 18870.33GoodGoodGoodExample 28890.32GoodGoodGoodExample 38900.31GoodGoodGoodExample 49450.35GoodGoodGoodExample 59600.32GoodGoodGoodExample 69730.34GoodGoodGoodExample 79750.24GoodGoodGoodExample 89760.26GoodGoodGoodExample 99750.18GoodGoodGoodExample 109600.27GoodGoodGoodExample 119580.34GoodGoodGoodExample 129740.30GoodGoodGoodExample 139750.32GoodGoodGoodExample 149440.31GoodGoodGoodExample 159420.31GoodGoodGoodExample 169450.32GoodGoodGoodExample 178840.17GoodGoodGoodComparative8870.34PoorGoodGoodExample 1Comparative6804.25GoodGoodGoodExample 2Comparative8600.14GoodGoodGoodExample 3Comparative97613.52GoodGoodGoodExample 4Comparative8910.15PoorGoodGoodExample 5Comparative8650.26GoodGoodGoodExample 6Comparative8720.18GoodGoodGoodExample 7Comparative8420.17GoodGoodGoodExample 8Comparative8850.14PoorGoodGoodExample 9Comparative5400.31GoodGoodGoodExample 10Comparative9770.41PoorGoodGoodExample 11Comparative8830.17PoorGoodGoodExample 12Comparative8410.35GoodGoodGoodExample 13Comparative9120.34PoorGoodGoodExample 14Comparative8780.42PoorPoorPoorExample 15

[0192] Although the embodiment of the present invention has been described in detail above, the present invention is not limited to the above embodiment, and various modifications can be made without departing from the gist of the present invention.

[0193] The present application is based on Japanese Patent Applications No. 2025-077653 filed on May 7, 2025, No. 2025-134620 filed on Aug. 13, 2025, and No. 2026-064809 filed on Apr. 10, 2026, and the contents thereof are incorporated herein by reference.INDUSTRIAL APPLICABILITY

[0194] The Ni-based alloy according to the present invention can be used for geothermal power generation components, oil / gas drilling components, jet engine members, gas turbine members, nuclear reactor components, and the like.

Claims

1. A Ni-based alloy consisting of:C≤0.10 mass %;Si≤1.0 mass %;Mn≤1.0 mass %;Cu≤3.5 mass %;16.0 mass %≤Cr≤25.0 mass %;10.0 mass %≤Mo≤17.0 mass %;3.5 mass %≤Nb≤6.5 mass %;0.10 mass %≤Ti≤2.00 mass %;0.15 mass %≤Al≤0.50 mass %;0 mass %≤B≤0.0200 mass %;0 mass %≤Mg+Ca+Zr+Hf≤0.0200 mass %;P limited to 0.05 mass % or less;S limited to 0.0050 mass % or less;Fe limited to 3.0 mass % or less;O limited to 0.0200 mass % or less;N limited to 0.0300 mass % or less;V limited to 0.20 mass % or less;Ta limited to 0.20 mass % or less;Co limited to 1.0 mass % or less; andW limited to 0.10 mass % or less,with the balance being Ni and unavoidable impurities, andsatisfying the following formulae (1), (2), and (3),0.0010 mass %≤B+Mg+Ca+Zr+Hf≤0.0200 mass %  Formula (1),Nb (seg)=Nb (max)−Nb (min)≤1.5 mass %  Formula (2), andMo (seg)=Mo (max)−Mo (min)≤0.6 mass %  Formula (3)whereNb (seg) is a degree of Nb segregation,Nb (max) is a maximum value of a content of Nb measured by EPMA surface analysis,Nb (min) is a minimum value of the content of Nb measured by the EPMA surface analysis,Mo (seg) is a degree of Mo segregation,Mo (max) is a maximum value of a content of Mo measured by the EPMA surface analysis, andMo (min) is a minimum value of the content of Mo measured by the EPMA surface analysis.

2. The Ni-based alloy according to claim 1, satisfying 10.0 mass %≤Mo≤11.0 mass %.

3. The Ni-based alloy according to claim 1, satisfying 4.5 mass %≤Nb≤5.5 mass %.

4. The Ni-based alloy according to claim 1, satisfying 0.10 mass %≤Ti≤0.50 mass %.

5. The Ni-based alloy according to claim 1, satisfying 0.15 mass %≤Al≤0.30 mass %.

6. The Ni-based alloy according to claim 1, having a crack occurrence rate at 950 °C of 1.0% or less,wherein the “crack occurrence rate” indicates a ratio (=n×100 / n0) of the number n of compression test pieces having no cracks after a 50% compression test to a total number no (n0≥5) of compression test pieces when the total number no of compression test pieces is subjected to the 50% compression test, andthe “50% compression test” indicates a test in which the compression test piece having a diameter of 15 mm and a height of 22.5 mm is prepared from the Ni-based alloy after a solution heat treatment, and the compression test piece is subjected to compression until the height of the compression test piece reaches 50%+2.5%.

7. The Ni-based alloy according to claim 1, having a 0.2% proof stress at 25 °C of 880 MPa or more,wherein the “0.2% proof stress” indicates a stress at which a strain is 0.2% when a standard test piece with a parallel portion having a diameter of 6 mm is prepared from the Ni-based alloy after an aging treatment in accordance with ASTM E8 and the standard test piece is subjected to a tensile test in accordance with ASTM E8.

8. The Ni-based alloy according to claim 7, having the 0.2% proof stress at 25 °C of 900 MPa or more,wherein the “0.2% proof stress” indicates a stress at which a strain is 0.2% when a standard test piece with a parallel portion having a diameter of 6 mm is prepared from the Ni-based alloy after an aging treatment in accordance with ASTM E8 and the standard test piece is subjected to a tensile test in accordance with ASTM E8.

9. The Ni-based alloy according to claim 1, having a corrosion weight loss of 0.35 g / (m2·h) or less,wherein the “corrosion weight loss” indicates a value obtained by preparing a cylindrical test piece having a diameter of 10 mm and a height of 50.0 mm from the Ni-based alloy after a hot working, after a solution heat treatment, or after an aging treatment, measuring a mass loss after immersing the cylindrical test piece in a boiling 5% sulfuric acid aqueous solution for 6 hours, and dividing the mass loss by a total surface area of the cylindrical test piece and an immersion time.

10. The Ni-based alloy according to claim 9, having the corrosion weight loss of 0.33 g / (m2·h) or less,wherein the “corrosion weight loss” indicates a value obtained by preparing a cylindrical test piece having a diameter of 10 mm and a height of 50.0 mm from the Ni-based alloy after a hot working, after a solution heat treatment, or after an aging treatment, measuring a mass loss after immersing the cylindrical test piece in a boiling 5% sulfuric acid aqueous solution for 6 hours, and dividing the mass loss by a total surface area of the cylindrical test piece and an immersion time.