Authority / Receiving Office
US · United States
Patent Type
Applications(United States)
Current Assignee / Owner
Priority Date
2024-01-12
Filing Date
2026-06-18
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Current methods for preparing cellulose fibers face issues of low strength, toxicity, and high cost due to the use of crosslinking agents like glutaraldehyde and Genipin, and the processes are complex and environmentally harmful.

Method used

A method involving the preparation of an oxidized sugar crosslinking agent using periodate-oxidized sugar and barium chloride, combined with cellulose in an ionic liquid, followed by wet spinning and crosslinking treatment to enhance cellulose fiber strength, using safe and renewable materials.

Benefits of technology

The method results in cellulose fibers with improved fracture strength, reduced environmental impact, and lower production costs, utilizing a simple and safe process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a method for preparing oxidized-sugar-crosslinked cellulose fibers, which includes the following steps: dissolving 10-20 parts by weight of sugar and 20-40 parts by weight of periodate in 300-500 parts by weight of deionized water, stirring, then adding 10-20 parts by weight of barium chloride and stirring at 5-10 °C for 1-2 hours; filtering the mixture and leaving the filtrate to obtain the oxidized sugar crosslinking agent; weighing 50-100 parts by weight of cellulose and adding it to a container containing 200-300 parts by weight of ionic liquid, heating and stirring to prepare a cellulose fiber dissolution solution, preparing cellulose fibers according to a wet spinning process; immersing the cellulose fibers in an oxidized sugar solution, crosslinking is carried out at 30-60 °C for 10-120 minutes; after crosslinking is complete, removing and draining, and drying at 105-125 °C to obtain the oxidized sugar crosslinked cellulose fibers.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application is a continuation of International Application No. PCT / CN2024 / 135114, filed on Nov. 28, 2024, which claims priority to Chinese Patent Application No. 202410048404.1, filed on Jan. 12, 2024. Both of which are hereby incorporated by reference in their entireties.TECHNICAL FIELD

[0002] The present disclosure relates to a method for preparing oxidized-sugar-crosslinked cellulose fibers.BACKGROUND

[0003] Low cost, renewable, and biodegradable cellulose resources are the most abundant organic raw materials in nature. Through chemical modification, they can be endowed with specific properties, making them functional materials that can meet various purposes, such as cellulose fibers. However, cellulose fibers prepared directly have the disadvantage of low strength, which limits their application fields. The modification of cellulose fibers is becoming a hot topic of concern for researchers both domestically and internationally.

[0004] In CN112342644B, a method for preparing antibacterial nanocellulose fibers is disclosed. The method includes the following steps: (1) preparation of menthol composite zinc oxide microcapsules: mixing menthol liquid paraffin solution with chitosan acid solution, then adjusting the pH value to 5.5-6.5 to obtain mixed solution I, mixing the mixed solution I with nano zinc oxide to obtain mixed solution II, adding glutaraldehyde in the mixed solution II for crosslinking, and filtering to obtain the mixed solution; (2) blended spinning: mixing the menthol composite zinc oxide microcapsules with the spinning adhesive solution evenly, performing acid bath spinning, and preparing antibacterial nanocellulose fibers through spinning post-treatment.

[0005] In CN115944777A, a gelatin / glass fiber biomimetic scaffold crosslinked with Genipin and its preparation method and application are disclosed. This method of biomimetic scaffold includes a composite scaffold dispersed with SiO2CaOP2O5 fibers, and the SiO2CaOP2O5 fibers are uniformly distributed and staggered in gelatin. The gelatin crosslinked with Genipin at the fiber overlap is used to fix the fibers.

[0006] The literature of Research on Glutaraldehyde Crosslinking Modified Regenerated Cellulose Fibers and Research on Glutaraldehyde Surface Crosslinking Modified Cellulose Membranes record the modification of cellulose fibers using glutaraldehyde as a crosslinking agent. Under physiological conditions, due to their high reactivity and volatility, small molecule aldehydes can react with proteins and DNA in the body, making them typically toxic and carcinogenic. Besides that, highly volatile small molecule aldehydes are harmful to operators and the environment.

[0007] Crosslinking modification can effectively improve the strength of cellulose fibers, and researchers have found that glutaraldehyde and Genipin have good crosslinking effects. Glutaraldehyde is a bifunctional chemical crosslinking agent, which has the advantage of being able to crosslink under solution and steam conditions, but there is potential toxicity issues related to residual unreacted crosslinking agent groups. Genipin is an excellent natural crosslinking agent for protein materials, which has been proven to be much less toxic than glutaraldehyde and other commonly used synthetic crosslinking reagents. However, its high cost (Sigma 25 mg Genipin priced at 1562 RMB) is the main drawback of practical use. Although cellulose fibers prepared by current technologies have excellent properties, the process is relatively complex, and crosslinking agents are toxic or costly.

[0008] Based on the above issues, a method for preparing oxidized-sugar-crosslinked cellulose fibers is provided.SUMMARY

[0009] The purpose of the present disclosure is to provide a simple, safe, and low-cost method for preparing oxidized-sugar-crosslinked cellulose fibers.

[0010] In order to achieve the above objectives, the present disclosure adopts the following technical solution.

[0011] A method for preparing oxidized-sugar-crosslinked cellulose fibers, including the following steps:

[0012] A. preparation of oxidized sugar crosslinking agent: dissolving 10-20 parts by weight of sugar and 20-40 parts by weight of periodate in 300-500 parts by weight of deionized water, stirring at 20-25 °C for 6-24 hours, then adding 10-20 parts by weight of barium chloride and stirring at 5-10 °C for 1-2 hours; filtering the mixture and leaving the filtrate to obtain the oxidized sugar crosslinking agent for later use;

[0013] B. preparation of cellulose fibers: weighing 50-100 parts by weight of cellulose and adding it to a container containing 200-300 parts by weight of ionic liquid, heating and stirring at 85-105 °C for 2-8 hours to prepare a cellulose fiber dissolution solution, preparing cellulose fibers according to a wet spinning process;

[0014] C. crosslinking treatment of cellulose fibers: immersing the cellulose fibers in an oxidized sugar solution, with a mass ratio of 30-70:10-90 between cellulose fibers and oxidized sugar crosslinking agent; crosslinking is carried out at 30-60 °C for 10-120 minutes; after crosslinking is complete, removing and draining, and drying at 105-125 °C to obtain the oxidized sugar crosslinked cellulose fibers.

[0015] In an embodiment of the present disclosure, the sugar is one or more of glucose, galactose, fructose, sucrose, maltose, raffinose, maltotriose, and maltotetrose.

[0016] In an embodiment of the present disclosure, the periodate salt is sodium periodate or potassium periodate.

[0017] In an embodiment of the present disclosure, the cellulose is sugarcane bagasse cellulose, cotton cellulose, or poplar cellulose.

[0018] In an embodiment of the present disclosure, the ionic liquid is 1,3-dimethylimidazolium hexafluorophosphate, 1,3-dimethylimidazolium tetrafluoroborate, or 1,3-dimethylimidazolium bis(trifluoromethylsulfonyl)imide.

[0019] In an embodiment of the present disclosure, during the wet spinning process for preparing cellulose fibers, the coagulation bath is a mixture of ionic liquid and water, and a mass concentration of the ionic liquid in the mixture is not more than 60%, and a coagulation bath temperature is 5-10 °C.

[0020] After adopting the technical solution of the present disclosure, oxidized sugar cross-linked cellulose fibers were prepared under environmentally friendly material processing conditions. Sugar is the most basic food additive in daily life, non-toxic, renewable, and widely present in plants in nature. After being oxidized by periodate salts, highly active aldehyde groups can be introduced into sugar molecules that do not have reactive groups, rendering them a new type of bio-based crosslinking agent. The present disclosure completely precipitates excess periodate salts by adding barium chloride, without the need for extensive water filtration and cleaning, reducing wastewater generation. Through research, it has been found that with the increase of temperature and the prolongation of time, the reaction intensifies, and the cellulose fibers undergo browning, and fracture strength is significantly improved. The process of the present disclosure is simple, safe, and can reduce enterprise costs.DESCRIPTION OF EMBODIMENTS

[0021] In order to better understand the technical solution of the present disclosure, a more detailed explanation will be provided below in combination with the embodiments.Example 1

[0022] A preparation method of sugarcane bagasse cellulose fiber is made according to the following parameters:

[0023] weighing 50 g of sugarcane bagasse cellulose and adding it to a three necked flask containing 200 g of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid; placing it in an oil bath and heating and stirring at 85 °C for 8 hours to prepare a sugarcane bagasse cellulose fiber dissolution solution; after regular filtration and vacuum degassing, sugarcane bagasse cellulose fibers are prepared using wet spinning forming technology; wet spinning includes the following steps: preparing spinning solution; squeezing the original solution from the nozzle to form a fine stream; the original liquid fine stream solidifies into primary fibers; raw fibers can be rolled up or directly subjected to post-treatment; the coagulation bath used for solidification is a mixture of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid and water, with a mass concentration of 20% for the ionic liquid and a coagulation bath temperature of 5 °C; after stretching, washing with water, and drying, sugarcane bagasse cellulose fibers are obtained. Using an electronic universal testing machine to measure the strength of cellulose fibers. The fracture strength of cellulose fibers prepared under these conditions reached 11 MPa.Example 2

[0024] A method for preparing oxidized sugar crosslinked cellulose fibers is made according to the following parameters:

[0025] (1) preparation of oxidized sugar crosslinking agent: weighing 5.42 g of sucrose and 19.50 g of sodium periodate and dissolving them in 300 g of deionized water; stirring at 25 °C for 24 hours, then adding 11.20 g of barium chloride and stirring at 5 °C for 1 hour to ensure sufficient precipitation of periodate; then filtering the mixture and keeping the filtrate; at this point, the filtrate is clear and transparent, and contains an oxidized glucose crosslinking agent; the filtrate is stored at 5 °C for future use;

[0026] (2) weighing 50 g of sugarcane bagasse cellulose and adding it to a three necked flask containing 200 g of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid; placing it in an oil bath and heating and stirring at 85 °C for 8 hours to prepare a sugarcane bagasse cellulose fiber dissolution solution; after regular filtration and vacuum degassing, sugarcane bagasse cellulose fibers are prepared using wet spinning forming technology; the coagulation bath is a mixture of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid and water, with a mass concentration of 20% ionic liquid and a coagulation bath temperature of 5 °C; after stretching, washing with water, and drying, sugarcane bagasse cellulose fibers are obtained;

[0027] (3) crosslinking treatment of sugarcane bagasse cellulose fibers: the sugarcane bagasse cellulose fibers are immersed in an oxidized glucose solution, with a mass ratio of 30:70 between sugarcane bagasse cellulose fibers and oxidized glucose; crosslinking is carried out at 30 °C for 10 minutes, and after crosslinking is completed, they are taken out, drained, and placed in a 105 °C constant temperature oven to complete the surface chemical crosslinking reaction, resulting in oxidized sucrose crosslinked sugarcane bagasse cellulose fibers; using an electronic universal testing machine to measure the strength of cellulose fibers; the fracture strength of sugarcane bagasse cellulose fibers prepared under these conditions reached 16 MPa.Example 3

[0028] A method for preparing oxidized sugar crosslinked cellulose fibers is made according to the following parameters:

[0029] (1) preparation of oxidized sucrose crosslinking agent: weighing 8.5 g of sucrose and 19.50 g of sodium periodate and dissolving them in 300 g of deionized water; stirring at 25 °C for 24 hours, then adding 11.20 g of barium chloride and stirring at 5 °C for 1 hour to ensure sufficient precipitation of periodate; then filtering the mixture and keeping the filtrate; at this point, the filtrate is clear and transparent and contains oxidized sucrose crosslinking agent, the filtrate is stored at 5 °C for future use;

[0030] (2) weighing 50 g of sugarcane bagasse cellulose and adding it to a three necked flask containing 200 g of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid; placing it in an oil bath and heating and stirring at 85 °C for 8 hours to prepare a sugarcane bagasse cellulose fiber dissolution solution; after filtration and vacuum degassing, sugarcane bagasse cellulose fibers were prepared using wet spinning forming technology; the coagulation bath is a mixture of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid and water, with a mass concentration of 20% ionic liquid and a coagulation bath temperature of 5 °C; after stretching, washing with water, and drying, sugarcane bagasse cellulose fibers are obtained;

[0031] (3) crosslinking treatment of sugarcane bagasse cellulose fibers: the sugarcane bagasse cellulose fibers are immersed in an oxidized sucrose solution, with a mass ratio of 30:70 between sugarcane bagasse cellulose fibers and oxidized sucrose; crosslinking is carried out at 30 °C for 10 minutes, and after crosslinking is completed, they are taken out, drained, and placed in a constant temperature oven at 105 °C to complete the surface chemical crosslinking reaction and obtain oxidized sucrose crosslinked sugarcane bagasse cellulose fibers; using an electronic universal testing machine to measure the strength of cellulose fibers; the fracture strength of sugarcane bagasse cellulose fibers prepared under these conditions reached 18.5 MPa.Example 4

[0032] A method for preparing oxidized sugar crosslinked cellulose fibers is made according to the following parameters:

[0033] (1) preparation of oxidized sucrose crosslinking agent: weighing 10.26 g of sucrose and 19.50 g of sodium periodate and dissolving them in 300 g of deionized water; stirring at 25 °C for 24 hours, then adding 11.20 g of barium chloride and stirring at 5 °C for 1 hour to ensure sufficient precipitation of periodate; then filtering the mixture and keeping the filtrate; at this point, the filtrate is clear and transparent, and contains oxidized sucrose crosslinking agent; the filtrate is stored at 5 °C for future use;

[0034] (2) weighing 50 g of sugarcane bagasse cellulose and adding it to a three necked flask containing 200 g of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid; placing it in an oil bath and heating and stirring at 85 °C for 8 hours to prepare a sugarcane bagasse cellulose fiber dissolution solution; after filtration and vacuum degassing, sugarcane bagasse cellulose fibers were prepared using wet spinning forming technology; the coagulation bath is a mixture of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid and water, with a mass concentration of 20% ionic liquid and a coagulation bath temperature of 5 °C; after stretching, washing with water, and drying, sugarcane bagasse cellulose fibers are obtained;

[0035] (3) crosslinking treatment of sugarcane bagasse cellulose fibers: the sugarcane bagasse cellulose fibers were immersed in an oxidized sucrose solution, with a mass ratio of 30:70 between sugarcane bagasse cellulose fibers and oxidized sucrose; crosslinking is carried out at 30 °C for 10 minutes; after crosslinking is complete, removing and draining the fibers, and placing them in a constant temperature oven at 105 °C to complete the surface chemical crosslinking reaction and obtaining oxidized sucrose crosslinked sugarcane bagasse cellulose fibers; using an electronic universal testing machine to measure the strength of cellulose fibers; the fracture strength of sugarcane bagasse cellulose fibers prepared under these conditions reached 22 MPa.Example 5

[0036] A method for preparing oxidized sugar crosslinked cellulose fibers is made according to the following parameters:

[0037] (1) preparation of oxidized sucrose crosslinking agent: weighing 12.25 g of sucrose and 19.50 g of sodium periodate and dissolving them in 300 g of deionized water; stirring at 25 °C for 24 hours, then adding 11.20 g of barium chloride and stirring at 5 °C for 1 hour to ensure sufficient precipitation of periodate; then filtering the mixture and keeping the filtrate; at this point, the filtrate is clear and transparent, and contains oxidized sucrose crosslinking agent; the filtrate is stored at 5 °C for future use;

[0038] (2) weighing 50 g of sugarcane bagasse cellulose and adding it to a three necked flask containing 200 g of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid; placing it in an oil bath and heating and stirring at 85 °C for 8 hours to prepare a sugarcane bagasse cellulose fiber dissolution solution; after filtration and vacuum degassing, sugarcane bagasse cellulose fibers were prepared using wet spinning forming technology; the coagulation bath is a mixture of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid and water, with a mass concentration of 20% ionic liquid and a coagulation bath temperature of 5 °C; after stretching, washing with water, and drying, sugarcane bagasse cellulose fibers are obtained;

[0039] (3) crosslinking treatment of sugarcane bagasse cellulose fibers: the sugarcane bagasse cellulose fibers are immersed in an oxidized sucrose solution, with a mass ratio of 30:70 between sugarcane bagasse cellulose fibers and oxidized sucrose; crosslinking is carried out at 30 °C for 10 minutes, and after crosslinking is completed, they are taken out, drained, and placed in a constant temperature oven at 105 °C to complete the surface chemical crosslinking reaction and obtain oxidized sucrose crosslinked sugarcane bagasse cellulose fibers; using an electronic universal testing machine to measure the strength of cellulose fibers; the fracture strength of sugarcane bagasse cellulose fibers prepared under these conditions reached 19.1 MPa.

[0040] With the increase of the concentration of the oxidized sugar solution, the hydroxyl groups on the molecular chains of regenerated cellulose fibers fully react with their aldehyde groups, thereby enhancing the intermolecular forces and increasing the degree of crosslinking, thus improving the mechanical properties of the fibers. When the amount of oxidized sugar crosslinking agent increases to a certain value, the density of crosslinking points becomes too high, which limits the sliding between molecules and leads to a decrease in the mechanical properties of the fiber.Examples 6-8

[0041] Under the same conditions as example 4 except for the change in crosslinking time, the properties of sugarcane bagasse cellulose fibers obtained are shown in the following table.TABLE 1CrosslinkingCrosslinkingFracture strength ofreactionreactionsugarcane bagasseNumbertemperature (°C)time (min)cellulose fibers (Mpa)Example 4301022.00Example 6451024.45Example 7601026.50Example 8751025.10

[0042] With the increase of reaction temperature, the movement speed of regenerated cellulose molecules increases, thereby promoting the reaction; as a result, the mechanical properties of sucrose cellulose fibers gradually increase; increasing the temperature can improve the reaction rate and fluidity of reactants, and enhance the speed of crosslinking reaction. But the speed of crosslinking reaction has a certain limit, and when the temperature reaches a certain value, increasing the reaction temperature has little effect on the mechanical properties of fibers.Example 9

[0043] A method for preparing oxidized sugar crosslinked cellulose fibers is made according to the following parameters:

[0044] (1) preparation of oxidized sucrose crosslinking agent: weighing 10.26 g of sucrose and 19.50 g of sodium periodate and dissolving them in 300 g of deionized water; stirring at 25 °C for 24 hours, then adding 11.20 g of barium chloride and stirring at 5 °C for 1 hour to ensure sufficient precipitation of periodate; then filtering the mixture and keeping the filtrate; at this point, the filtrate is clear and transparent, and contains oxidized sucrose crosslinking agent; the filtrate is stored at 5 °C for future use;

[0045] (2) weighing 50 g of sugarcane bagasse cellulose and adding it to a three necked flask containing 200 g of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid; placing it in an oil bath and heating and stirring at 85 °C for 8 hours to prepare a sugarcane bagasse cellulose fiber dissolution solution; after filtration and vacuum degassing, sugarcane bagasse cellulose fibers were prepared using wet spinning forming technology; the coagulation bath is a mixture of 1,3-dimethylimidazolium hexafluorophosphate ionic liquid and water, with a concentration of 20% ionic liquid and a coagulation bath temperature of 5 °C; after stretching, washing with water, and drying, sugarcane bagasse cellulose fibers are obtained;

[0046] (3) strong crosslinking treatment of sugarcane bagasse cellulose fibers: the sugarcane bagasse cellulose fibers are immersed in an oxidized sucrose solution, with a mass ratio of 30:70 between sugarcane bagasse cellulose fibers and oxidized sucrose; the fibers are crosslinked at 60 °C for 120 minutes, and after crosslinking is complete, they are taken out, drained, and placed in a constant temperature oven at 105 °C to complete the surface chemical crosslinking reaction and obtain oxidized sucrose strongly crosslinked sugarcane bagasse cellulose fibers; using an electronic universal testing machine to measure the strength of cellulose fibers; the fracture strength of sugarcane bagasse cellulose fibers prepared under these conditions reached 35 MPa.Examples 10-13

[0047] Except for crosslinking time, all other parameters are the same as in example 9. The properties of sugarcane bagasse cellulose fibers obtained are shown in the following table.TABLE 2CrosslinkingCrosslinkingFracture strength ofreactionreactionsugarcane bagasseNumbertemperature (°C)time (min)cellulose fibers (Mpa)Example 10603027.20Example 11606029.45Example 12609031.70Example 96012035.00Example 136015031.25

[0048] With the increase of crosslinking time, the hydroxyl groups on the cellulose molecular chain bind more with the aldehyde groups of the oxidation pool crosslinking agent, and the intermolecular forces increase, resulting in an increase in the mechanical properties of the fiber; as the reaction continues, the number of cross-linking chains between molecules increases, thereby forming a large number of network structures, and the density of cross-linking points between fibers increases; stress concentration occurs during stretching, making the fibers brittle and leading to a decrease in their mechanical properties.

[0049] The protection scope of the present disclosure is not limited to this embodiment. For example, it can be increased or decreased proportionally according to the substance content of the present disclosure. Anyone who makes similar changes to it is considered not to deviate from the protection scope of the present disclosure.

Claims

1. A method for preparing oxidized-sugar-crosslinked cellulose fibers, comprising the following steps:A. preparation of oxidized sugar crosslinking agent: dissolving 10-20 parts by weight of sugar and 20-40 parts by weight of periodate in 300-500 parts by weight of deionized water, stirring at 20-25 °C for 6-24 hours, then adding 10-20 parts by weight of barium chloride and stirring at 5-10 °C for 1-2 hours; filtering the mixture and leaving the filtrate to obtain the oxidized sugar crosslinking agent for later use;B. preparation of cellulose fibers: weighing 50-100 parts by weight of cellulose and adding it to a container containing 200-300 parts by weight of ionic liquid, heating and stirring at 85-105 °C for 2-8 hours to prepare a cellulose fiber dissolution solution, preparing cellulose fibers according to a wet spinning process;C. crosslinking treatment of cellulose fibers: immersing cellulose fibers in an oxidized sugar solution, with a mass ratio of 30-70:10-90 between cellulose fibers and oxidized sugar crosslinking agent; crosslinking is carried out at 30-60 °C for 10-120 minutes; after crosslinking is complete, removing and draining, and drying at 105-125 °C to obtain oxidized sugar crosslinked cellulose fibers.

2. The method for preparing oxidized-sugar-crosslinked cellulose fibers according to claim 1, wherein the sugar is one or more of glucose, galactose, fructose, sucrose, maltose, raffinose, maltotriose, and maltotetrose.

3. The method for preparing oxidized-sugar-crosslinked cellulose fibers according to claim 2, wherein the periodate salt is sodium periodate or potassium periodate.

4. The method for preparing oxidized-sugar-crosslinked cellulose fibers according to claim 3, wherein the cellulose is sugarcane bagasse cellulose, cotton cellulose, or poplar cellulose.

5. The method for preparing oxidized-sugar-crosslinked cellulose fibers according to claim 4, wherein the ionic liquid is 1,3-dimethylimidazolium hexafluorophosphate, 1,3-dimethylimidazolium tetrafluoroborate, or 1,3-dimethylimidazolium bis (trifluoromethylsulfonyl)imide.

6. The method for preparing oxidized-sugar-crosslinked cellulose fibers according to claim 5, wherein during the wet spinning process for preparing cellulose fibers, the coagulation bath is a mixture of ionic liquid and water, and a mass concentration of ionic liquid in the mixture is not more than 60%, and a coagulation bath temperature is 5-10 °C.