Seal sheet for pneumatic tires
The seal sheet for pneumatic tires, utilizing a thermoplastic elastomer and tackifier, addresses the issue of deteriorating sealing performance by maintaining a specific ratio of properties, ensuring effective sealing and preventing air leakage, thus enhancing tire integrity and mobility.
Patent Information
- Application Number
- PCT/JP2024/010150
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-16
- Filing Date
- 2024-03-15
- Publication Date
- 2024-09-19
AI Technical Summary
Conventional sealants for pneumatic tires deteriorate over time, leading to a decrease in sealing performance and air leakage through holes formed by sharp foreign objects, which compromises tire integrity and mobility.
A seal sheet with a sealing material layer composed of a thermoplastic elastomer, such as styrene-isoprene-styrene block copolymer, and a tackifier, with a specific ratio of storage elastic modulus, probe tack value, and adhesive force, ensuring long-lasting sealing performance by maintaining a product ratio of 12.0 or less, thereby preventing air leakage.
The seal sheet effectively maintains sealing performance over time, preventing air leakage and ensuring the tire remains inflated and functional even after punctures from sharp objects, enhancing mobility and safety.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Seal sheet for pneumatic tires CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority from Japanese Patent Application No. 2023-042005, the entire disclosure of which is incorporated herein by reference.
[0002] The present invention relates to a sealing sheet for a pneumatic tire, and more particularly to a sealing sheet for a pneumatic tire for preventing puncture of the pneumatic tire.
[0003] Conventionally, many moving objects such as bicycles and motorcycles are equipped with wheels fitted with pneumatic tires.
[0004] When such a vehicle is traveling on a road surface, if a foreign object with a sharp tip (e.g., a nail, a piece of glass, etc.) is present on the road surface, the foreign object with a sharp tip may pierce the pneumatic tire, forming a through hole in the pneumatic tire. If such a through hole is formed in the pneumatic tire, air sealed inside the pneumatic tire may leak out through the through hole, causing the pneumatic tire to puncture. If the pneumatic tire punctures, the vehicle will not be able to travel smoothly on the road surface, which is undesirable.
[0005] Therefore, in order to suppress leakage of air through the through holes, it is known to apply a sealant composition to the inner surface of the pneumatic tire to form a sealant layer (for example, Patent Document 1 below).
[0006] Patent Document 1 below discloses that a curable liquid agent such as latex is used as a sealing material composition for forming the sealing material layer.
[0007] US Patent Application Publication No. 2003 / 0136490
[0008] However, when the leakage of air through the through-hole is suppressed by a sealing material layer formed from the above-mentioned curable liquid agent, the sealing property at the through-hole may deteriorate over time. Therefore, although there is a demand for a sealing sheet including a sealing material layer that can suppress deterioration of the sealing property at the through-hole over time, this demand has not yet been fully met.
[0009] Therefore, an object of the present invention is to provide a sealing sheet for a pneumatic tire that can suppress deterioration over time in sealing properties at through holes formed in a pneumatic tire.
[0010] As a result of intensive research by the present inventors, it has been found that in a sealing sheet for a pneumatic tire having a sealing material layer, the value of the storage modulus of the sealing material layer at −20° C. is G′ 1 When the probe tack value of the sealing material layer at 23°C is T and the adhesive strength of the sealing material layer to a tire at 23°C is A1, the storage modulus value G' 1 The ratio of the product of the probe tack value T and the adhesive strength value A1 to the 1 The present inventors have found that by making the ratio (R) of the sealing performance of a through hole formed in a pneumatic tire to be 12.0 or less, deterioration over time of the sealing performance of the through hole can be suppressed. As a result, they have arrived at the present invention.
[0011] That is, the sealing sheet for a pneumatic tire according to the present invention includes a sealing material layer, and the value of the storage modulus of the sealing material layer at −20° C. is G′ 1 When the probe tack value of the sealing material layer at 23° C. is T and the adhesive strength of the sealing material layer to a tire at 23° C. is A1, the storage modulus value G′ is 1 The ratio of the product of the probe tack value T and the adhesive strength value A1 to the 1 ) is 12.0 or less.
[0012] 5 is a cross-sectional view showing the configuration of a sealing sheet for a pneumatic tire according to one embodiment of the present invention; FIG. 6 is a cross-sectional view showing the configuration of a sealing sheet for a pneumatic tire according to another embodiment of the present invention; FIG. 7 is a cross-sectional view showing the configuration of a sealing sheet for a pneumatic tire according to yet another embodiment of the present invention; FIG. 8 is a cross-sectional view showing the configuration of a sealing sheet for a pneumatic tire according to yet another embodiment of the present invention; FIG. 9 is a schematic view showing a bicycle wheel; FIG. 10 is a schematic view showing a bicycle wheel cut in a plane perpendicular to the circumferential direction (cross-sectional view taken along the arrows VI-VI in FIG. 5); FIG. 11 is a schematic view showing a nail pierced in a pneumatic tire equipped with a sealing sheet for a pneumatic tire according to one embodiment of the present invention (enlarged view of part A in FIG. 6); FIG. 12 is a cross-sectional view showing a nail pulled out of a pneumatic tire equipped with a sealing sheet for a pneumatic tire according to one embodiment of the present invention (enlarged view of part A in FIG. 6).
[0013] (Sealing material composition for pneumatic tire) Hereinafter, a sealing material composition for pneumatic tire according to one embodiment of the present invention will be described. Note that, hereinafter, one embodiment of the present invention will be abbreviated as the present embodiment. The sealing material composition for pneumatic tire according to this embodiment is used to form a sealing material layer of a sealing sheet for pneumatic tire according to each embodiment described below.
[0014] The sealing material composition for a pneumatic tire according to the present embodiment preferably contains a thermoplastic elastomer as an organic component. Examples of the thermoplastic elastomer include a styrene-based thermoplastic elastomer and an acrylic-based thermoplastic elastomer.
[0015] Examples of the styrene-based thermoplastic elastomer include styrene-ethylene-butadiene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), styrene-isobutylene-styrene block copolymer (SIBS), styrene-butadiene-styrene block copolymer (SBS), and styrene-ethylene-propylene-styrene block copolymer (SEPS). Examples of the acrylic thermoplastic elastomer include a copolymer of an acrylic acid ester and 2-chloroethyl vinyl ether, a copolymer of an acrylic acid ester and acrylonitrile, and a copolymer of an acrylic acid ester and acrylic acid. Among the above, the pneumatic tire sealing material composition preferably contains the styrene-based thermoplastic elastomer as the thermoplastic elastomer, and more preferably contains at least one of the styrene-isoprene-styrene block copolymer (SIS) and the styrene-isobutylene-styrene block copolymer (SIBS).
[0016] The mass average molecular weight of the thermoplastic elastomer is preferably 20,000 or more and 1,500,000 or less. The mass average molecular weight can be determined as a standard polystyrene equivalent value by GPC (gel permeation chromatography). The mass average molecular weight of the thermoplastic elastomer can be determined by measuring a sample obtained as follows using a TOSOH HLC-8420GPC under the following conditions. [Sample Obtaining Method] (1) A sample taken from a sealing material composition for pneumatic tires containing a thermoplastic elastomer is prepared into a 1.0 g / L THF solution and allowed to stand overnight. (2) The THF solution that has been allowed to stand overnight is filtered through a membrane filter with a pore size of 0.45 μm, and the obtained filtrate is used as the sample. [GPC Measurement Conditions] Column: TSKgel SuperHZM-H, TSKgel SuperHZ4000, TSKgel SuperHZ3000, and TSKgel SuperHZ200 (all manufactured by TOHSOH Corporation) connected in series using a ferrule system Column size: 6.0 mm ID × 150 mm Eluent: THF Flow rate: 0.6 mL / min Column temperature: 40°C Detector: RI Injection volume: 20 μL
[0017] The styrene-based thermoplastic elastomer preferably has a diblock ratio of 10% or more, more preferably 20% or more. The styrene-based thermoplastic elastomer preferably has a diblock ratio of 80% or less. Furthermore, when the styrene-based thermoplastic elastomer is used, the diblock ratio is preferably 40% or more, particularly preferably 50% or more. Furthermore, when the styrene-based thermoplastic elastomer is a styrene-isobutylene-styrene copolymer (SIBS), the diblock ratio is particularly preferably 20% or more. When the diblock ratio of the styrene-based thermoplastic elastomer is within the above-mentioned range, the pneumatic tire sealing material composition can exhibit even more sufficient adhesion over a wide temperature range from low temperatures (e.g., −10°C) to high temperatures (e.g., 60°C).
[0018] The diblock ratio (%) can be calculated by the following formula: Diblock ratio (%)=(parts by mass of diblock copolymer) / (parts by mass of diblock copolymer)×100
[0019] Specifically, the diblock ratio can be calculated from the area ratio of the peak attributable to the diblock copolymer to the peak attributable to the triblock copolymer in the chart obtained by measuring the molecular weight of the styrene-based thermoplastic elastomer by gel permeation chromatography (GPC). The GPC method can be performed in the same manner as described in the method for measuring the mass average molecular weight of a thermoplastic elastomer.
[0020] The styrene content (styrene amount) of the styrene-based thermoplastic elastomer is preferably 10% by mass or more, more preferably 13% by mass or more, and even more preferably 15% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less.
[0021] The diblock ratio of the styrene-based thermoplastic elastomer can be adjusted by changing the ratio of the amount of the polymerization initiator and the amount of the coupling agent used during polymerization (amount of coupling agent / amount of polymerization initiator).
[0022] The sealing material composition for a pneumatic tire preferably contains either a softener or a tackifier as the organic component. The sealing material composition for a pneumatic tire may further contain an antioxidant or the like.
[0023] Examples of the softener include paraffins, waxes, naphthenes, aromatics, asphalts, drying oils (e.g., linseed oil, etc.), animal and vegetable oils, petroleum oils (e.g., process oil, etc.), polybutene, polyisobutylene, ethylene-α-olefin co-oligomer, low-molecular-weight polyethylene glycol, phthalate esters, phosphate esters, stearic acid or its esters, and alkylsulfonate esters. The softeners may be used alone or in combination of two or more. The pneumatic tire sealing material composition preferably contains polybutene as the softener.
[0024] The sealing material composition for pneumatic tires preferably contains 10 parts by mass or more, more preferably 20 parts by mass or more, and even more preferably 40 parts by mass or more of the softener per 100 parts by mass of the thermoplastic elastomer. Also, the sealing material composition for pneumatic tires preferably contains 150 parts by mass or less, more preferably 130 parts by mass or less, and even more preferably 110 parts by mass or less of the softener per 100 parts by mass of the thermoplastic elastomer.
[0025] Examples of the tackifier include rosin-based resins, terpene-based resins, styrene-based resins, petroleum-based resins, phenol-based resins, and hydrogenated resins obtained by hydrogenating these resins. These tackifiers may be used alone or in combination of two or more.
[0026] Examples of rosin-based resins include rosin resins, rosin ester resins, and rosin phenolic resins. Terpene-based resins may be any compound having structural units derived from isoprene, such as terpene resins, aromatic-modified terpene resins, and terpene-phenolic resins. Examples of styrene-based resins include resins obtained by copolymerizing styrene monomers such as α-methylstyrene or β-methylstyrene with aliphatic monomers. Examples of petroleum-based resins include C5 hydrocarbon resins obtained by copolymerizing C5 fractions such as pentene, isoprene, piperine, and 1,3-pentadiene produced by the thermal decomposition of petroleum naphtha; and C9 hydrocarbon resins (aromatic petroleum resins) obtained by copolymerizing C9 fractions such as indene and vinyltoluene produced by the thermal decomposition of petroleum naphtha. Examples of phenol-based resins include alkylphenol resins, xylylene formaldehyde resins, resols, and novolacs.
[0027] The sealing material composition for pneumatic tires preferably contains, as the tackifier, at least one selected from the group consisting of rosin-based resins, terpene-based resins, and petroleum-based resins. The sealing material composition for pneumatic tires preferably contains 50 parts by mass or more of the tackifier per 100 parts by mass of the thermoplastic elastomer, more preferably 70 parts by mass or more, and even more preferably 90 parts by mass or more. The sealing material composition for pneumatic tires preferably contains 400 parts by mass or less of the tackifier per 100 parts by mass of the thermoplastic elastomer, more preferably 380 parts by mass or less, even more preferably 350 parts by mass or less, and even more preferably 140 parts by mass or less.
[0028] Furthermore, the pneumatic tire sealing material composition preferably contains the rosin ester resin, the C9 hydrocarbon resin (aromatic petroleum resin), and the terpene resin as the tackifier. When the pneumatic tire sealing material composition contains the tackifiers in this combination, the terpene resin is preferably contained in an amount of 40 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 70 parts by mass or more, per 100 parts by mass of the thermoplastic elastomer. The terpene resin is preferably contained in an amount of 110 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 90 parts by mass or less, per 100 parts by mass of the thermoplastic elastomer resin. In the above case, the C9 hydrocarbon resin (aromatic petroleum resin) is preferably contained in an amount of 5 parts by mass or more, and even more preferably 7 parts by mass or more, per 100 parts by mass of the thermoplastic elastomer. The C9 hydrocarbon resin (aromatic petroleum resin) is preferably contained in an amount of 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 9 parts by mass or less, per 100 parts by mass of the thermoplastic elastomer. In the above case, the rosin ester resin is preferably contained in an amount of 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 18 parts by mass or more, per 100 parts by mass of the thermoplastic elastomer. The rosin ester resin is preferably contained in an amount of 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 22 parts by mass or less, per 100 parts by mass of the thermoplastic elastomer.
[0029] Furthermore, the pneumatic tire sealing material composition may contain only a C5 hydrocarbon resin as the tackifier. In such a case, the C5 hydrocarbon resin is preferably contained in an amount of 80 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 120 parts by mass or more, per 100 parts by mass of the thermoplastic elastomer. The C5 hydrocarbon resin is preferably contained in an amount of 200 parts by mass or less, more preferably 180 parts by mass or less, even more preferably 160 parts by mass or less, and even more preferably 140 parts by mass or less, per 100 parts by mass of the thermoplastic elastomer. When the pneumatic tire sealing material composition contains only a C5 hydrocarbon resin as the tackifier, it is preferable that the pneumatic tire sealing material composition further contains the softener.
[0030] The pneumatic tire sealing material composition may also contain a copolymer resin of C5 hydrocarbons and C9 hydrocarbons (aromatic hydrocarbons) as the tackifier. In this case, the copolymer resin is preferably contained in a total amount of 40 parts by mass or more, more preferably 60 parts by mass or more, and even more preferably 80 parts by mass or more, per 100 parts by mass of the thermoplastic elastomer. The copolymer resin is preferably contained in a total amount of 400 parts by mass or less, more preferably 300 parts by mass or less, and even more preferably 250 parts by mass or less, per 100 parts by mass of the thermoplastic elastomer.
[0031] The blending of the thermoplastic elastomer, the softener, and the tackifier will be described in further detail. When the thermoplastic elastomer is the styrene-isoprene-styrene copolymer (SIS) and has a diblock ratio of 40% or more, the sheet material layer tends to have a high probe tack value and a low adhesive strength, while the storage modulus tends to decrease. Therefore, in this case, it is preferable that the sealing material composition contains the tackifier resin. This increases the storage modulus of the sheet material layer, specifically, the storage modulus at −20° C. can be increased to a preferred value of 0.5 MPa or more. When the thermoplastic elastomer is the styrene-isoprene-styrene copolymer (SIS) and has a diblock ratio of 30% or less, the sheet material layer tends to have a high storage modulus and a low probe tack value and a low adhesive strength. Therefore, in this case, it is preferable that the sealing material composition contains both the tackifier and the softener. This can increase the probe tack value and adhesive strength of the sealing material layer; specifically, the probe tack value at 23°C can be set to a preferred value of 0.05 MPa or more, and the adhesive strength to a tire at 23°C can be set to a preferred value of 1.0 N / 20 mm or more. When the thermoplastic elastomer is styrene-isobutylene-styrene copolymer (SIBS), the sheet material layer can be provided with a preferred probe tack value, adhesive strength, and storage modulus, so the sheet material composition may consist of styrene-isobutylene-styrene copolymer (SIBS). Preferably, the sheet material composition may contain the softener together with the styrene-isobutylene-styrene copolymer (SIBS) to increase the adhesive strength while decreasing the storage modulus of the sheet material composition.
[0032] Various known anti-aging agents can be used as the anti-aging agent, and examples of the anti-aging agent include phosphorus-based anti-aging agents, phenol-based anti-aging agents, hindered amine-based anti-aging agents, benzotriazole-based anti-aging agents, aromatic amine-based anti-aging agents, and sulfur-based anti-aging agents.
[0033] The pneumatic tire sealing material composition may contain one kind of the above-mentioned antioxidant alone or may contain two or more kinds of the above-mentioned antioxidants. When the pneumatic tire sealing material composition contains the above-mentioned antioxidant, the thermoplastic elastomer contained in the pneumatic tire sealing material composition can be prevented from being deteriorated by oxidation.
[0034] The sealing material composition for pneumatic tires preferably contains 1 part by mass or more of the antioxidant per 100 parts by mass of the thermoplastic elastomer. The sealing material composition for pneumatic tires may contain 2 parts by mass or more, or 3 parts by mass or more of the antioxidant per 100 parts by mass of the thermoplastic elastomer. Furthermore, the sealing material composition for pneumatic tires may contain 10 parts by mass or less, 8 parts by mass or less, or 6 parts by mass or less of the antioxidant per 100 parts by mass of the thermoplastic elastomer.
[0035] The sealing material composition for a pneumatic tire may contain an inorganic component. The sealing material composition for a pneumatic tire may contain an inorganic filler and an inorganic colorant as the inorganic component. The sealing material composition for a pneumatic tire preferably contains the inorganic filler as the inorganic component.
[0036] Examples of the inorganic filler include calcium carbonate (e.g., heavy calcium carbonate and light calcium carbonate), calcium stearate, talc, titanium oxide, silica, and magnesium oxide. Among these, calcium carbonate is preferably used, and among calcium carbonate, heavy calcium carbonate is preferably used. Note that calcium stearate also functions as a lubricant.
[0037] The sealing material composition for pneumatic tires preferably contains 0.1 part by mass or more, more preferably 0.2 part by mass or more, and even more preferably 0.4 part by mass or more of the inorganic filler per 100 parts by mass of the thermoplastic elastomer. The sealing material composition for pneumatic tires preferably contains 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 1 part by mass or less of the inorganic filler per 100 parts by mass of the thermoplastic elastomer.
[0038] As the inorganic colorant, carbon is preferably used, and carbon black is more preferably used.
[0039] The sealing material composition for a pneumatic tire preferably contains the inorganic colorant in an amount of 1 part by mass to 10 parts by mass relative to 100 parts by mass of the thermoplastic elastomer.
[0040] As shown in the Examples section described later, by appropriately selecting and combining the thermoplastic elastomer type, the tackifier type, the softener type, and the inorganic filler type and appropriately adjusting the blending amount of each component, the storage modulus G' can be reduced in a sealing material layer formed using the sealing material composition for a pneumatic tire. 1 The ratio of the product of the probe tack value T and the adhesive strength A1 to the 1 ) can be suitably adjusted to 12.0 or less.
[0041] (Sealing Sheet for Pneumatic Tire) The sealing sheet for a pneumatic tire according to this embodiment includes a sealing material layer. In the sealing sheet for a pneumatic tire according to this embodiment, the value of the storage modulus of the sealing material layer at −20° C. is G′ 1 When the probe tack value of the sealing material layer at 23° C. is T and the adhesive strength of the sealing material layer to a tire at 23° C. is A1, the storage modulus value G′ is 1 The ratio of the product of the probe tack value T and the adhesive strength value A1 to the 1) is 12.0 or less. As described above, in the sealing sheet for a pneumatic tire according to this embodiment, the sealing material layer is formed from the sealing material composition for a pneumatic tire according to this embodiment.
[0042] By satisfying the above-described relationship, the sealing sheet for a pneumatic tire according to this embodiment, when a sealant layer is attached to the inner surface of a pneumatic tire and a through hole is formed in the pneumatic tire by a sharp foreign object (e.g., a nail, a piece of glass, etc.) that has pierced the pneumatic tire and is then pulled out of the pneumatic tire, can suitably fill the through hole with a portion of the sealant layer. As a result, air inside the pneumatic tire can be suitably prevented from leaking to the outside. In other words, the sealing sheet for a pneumatic tire according to this embodiment is provided with a sealant layer that can exhibit good sealing properties.
[0043] The storage modulus G' of the sealing material layer at -20°C 1 can be measured using a dynamic viscoelasticity measuring device (manufactured by TA instruments, trade name "ARES-G2"). The sealing material layer having planar dimensions of φ8 mm x thickness of 1.0 mm can be used as the measurement sample. The measurement sample can be obtained by punching out the sealing material layer having a thickness of 1.0 mm using a jig to have planar dimensions of φ8 mm. The measurement conditions are as follows. [Measurement conditions] Probe: φ8 mm Deformation mode: Sine wave Frequency: 1 Hz Heating rate: 5°C / min Measurement temperature: -60°C to 150°C Then, by reading the value of the storage modulus at -20°C from the obtained data, G' 1 can be obtained.
[0044] The probe tack value T at 23°C can be measured using a probe tack measuring instrument (manufactured by RHESCA, product name "TACKINESS Model TAC-II"). The measurement sample can be obtained by cutting out the sealing material layer having a thickness of 1.0 mm to have planar dimensions of 20 mm x 40 mm. The measurement procedure is as follows: (1) Using double-sided adhesive tape (manufactured by Nitto Denko Corporation, product name "No. 5610"), one side of the measurement sample (planar dimensions 20 mm x 40 mm) is bonded to one side of a glass slide (manufactured by Matsunami Glass Industrial Co., Ltd., planar dimensions 26 mm x 76 mm). The bonding is performed using a 2 kg hand roller. (2) The probe tack value of the exposed surface of the measurement sample is measured using the probe tack measuring instrument. The measurement conditions are as follows: The probe tack value is measured in an environment of 23°C. [Measurement conditions] Measurement mode: Static probe mode Probe terminal: 5 mmφ SUS probe terminal Probe descent speed (Immersion speed): 120 mm / min Test speed (Test speed): 120 mm / min Adhesion load (Preload): 100 gf Adhesion retention time (Prestime): 1 sec The above measurements are performed at any five points on the exposed surface of the measurement sample. The probe tack value T is then obtained by arithmetically averaging the five measured values.
[0045] The adhesive strength value A1 can be measured as follows. The test tire is a tubeless tire (Formula Pro Hookless Tubeless RBCC 700x25C) manufactured by Inoue Rubber Co., Ltd. In the examples described below, a tubeless tire with manufacturer's part number 190636 was used. (1) A small piece 20 mm wide is cut out of the 0.5 mm thick sealing material layer. (2) A polyethylene terephthalate (PET) resin film (25 μm thick) is bonded to one surface of the adhesive strength test specimen to obtain a laminate. (3) The laminate and the test tire are aged for 1 hour under conditions of a temperature of 23°C and a relative humidity of 50% RH. (4) Under conditions of a temperature of 23°C and a relative humidity of 50% RH, the exposed surface of the adhesive strength test specimen in the laminate is attached to the inner surface of the test tire. The adhesion is performed by moving a 2 kg roller back and forth once. (5) The test tire to which the laminate is attached is further aged for 30 minutes under conditions of a temperature of 23°C and a relative humidity of 50% RH, and then the adhesive strength of the test piece for adhesive strength measurement to the test tire is measured using a tensile tester under conditions of a peel angle of 180° and a tensile speed of 300 mm / min. The adhesive strength measurement is performed on three specimens. The arithmetic average of the adhesive strength values obtained for the three specimens is defined as the adhesive strength value A1.
[0046] The adhesive strength value A1 of the sealing material layer is preferably 1.0 N / 20 mm or more, more preferably 2.0 N / 20 mm or more, and even more preferably 2.5 N / 20 mm or more. The adhesive strength value A1 of the sealing material layer is preferably 30 N / 20 mm or less, more preferably 25 N / 20 mm or less, and even more preferably 20 N / 20 mm or less.
[0047] A1 x T / G' 1 is more preferably 11.0 or less, more preferably 10.0 or less, and even more preferably 6.0 or less. 1is within the above range, the sealing material layer in the sealing sheet for a pneumatic tire according to this embodiment can further suppress the air inside the pneumatic tire from leaking out (leaking) to the outside. That is, such a sealing sheet for a pneumatic tire has a sealing material layer that can exhibit even better sealing properties. Specifically, A1×T / G' 1 is within the above range, when the foreign object with a sharp tip is pulled out of the pneumatic tire and a through hole is formed in the pneumatic tire, the sealing material layer in the sealing sheet for pneumatic tires according to this embodiment can follow the foreign object with a sharp tip more effectively, and can therefore suitably seal the through hole formed in the pneumatic tire by the foreign object with a sharp tip.
[0048] A1 x T / G' 1 may be 0.001 or more, 0.01 or more, or 0.02 or more.
[0049] In the sealing material layer of the sealing sheet for a pneumatic tire according to this embodiment, the storage modulus G' 1 The storage modulus G' is preferably 0.50 MPa or more. 1 is within the above range, the sealing material layer in the sealing sheet for a pneumatic tire according to this embodiment can further suppress the air inside the pneumatic tire from leaking out (leaking) to the outside. That is, such a sealing sheet for a pneumatic tire has a sealing material layer that can exhibit even better sealing properties. In the sealing material layer in the sealing sheet for a pneumatic tire according to this embodiment, the storage elastic modulus value G' 1 The storage modulus G' is preferably 1.0 MPa or more, and particularly preferably 1.5 MPa or more. 1When the thickness of the sealant layer in the sealing sheet for a pneumatic tire according to the present embodiment is within the above range, the sealant layer can more effectively follow the sharp-tipped foreign object when the sharp-tipped foreign object is pulled out of the tire, thereby more effectively sealing the through hole formed in the tire by the sharp-tipped foreign object.
[0050] In addition, in the sealing material layer of the sealing sheet for a pneumatic tire according to the present embodiment, the value of the storage elastic modulus G' 1 may be 100 MPa or less, 80 MPa or less, or 60 MPa or less.
[0051] In the sealing material layer of the sealing sheet for a pneumatic tire according to this embodiment, the probe tack value T is preferably 0.05 MPa or more. When the probe tack value T is within the above range, the sealing material layer of the sealing sheet for a pneumatic tire according to this embodiment can exhibit good adhesion to the inner surface of the pneumatic tire. The probe tack value T is more preferably 0.10 or more. Furthermore, the probe tack value may be 2.0 MPa or less, 1.0 MPa or less, or 0.75 MPa or less.
[0052] In the sealing sheet for a pneumatic tire according to this embodiment, the value of the storage modulus G' of the sealing material layer at 23°C 2 The storage modulus G' is preferably 0.50 MPa or less, and more preferably 0.20 MPa or less. 2 The lower limit is usually 0.01 MPa.
[0053] The storage modulus G' 2 is the storage modulus G' 1 The storage modulus at 23°C can be obtained by reading the value of the storage modulus at 23°C from the data obtained by measurement according to the same procedure as in the case of (1).
[0054] When the adhesive strength A2 of the sealing material layer in the sealing sheet for a pneumatic tire according to this embodiment is defined as the value of adhesive strength to a tire at −20° C., the adhesive strength A2 is preferably 1.0 N / 20 mm or more, more preferably 2.0 N / 20 mm or more, and even more preferably 3.0 N / 20 mm or more. The adhesive strength A2 of the sealing material layer in the sealing sheet for a pneumatic tire is preferably 20 N / 20 mm or less, more preferably 18 N / 20 mm or less, even more preferably 16 N / 20 mm or less, and even more preferably 10 N / 20 mm or less.
[0055] The adhesive strength value A2 can be measured as follows. (1') to (4') These are carried out in the same manner as steps (1) to (4) of the measuring method for the adhesive strength value A1. (5') The test tire to which the laminate is attached is cured for 60 minutes at a temperature of -20°C, and then the adhesive strength of the small piece of sheet body to the test tire is measured using a tensile tester at a peel angle of 180° and a tensile speed of 300 mm / min. The adhesive strength measurement is also carried out for three specimens. The arithmetic average of the adhesive strength values obtained for the three specimens is then taken as the adhesive strength value A2.
[0056] Next, a sealing sheet for a pneumatic tire according to another embodiment will be described with reference to Figures 1 and 2. The sealing sheet for a pneumatic tire according to this embodiment includes a substrate layer that is laminated on one surface of the sealing material layer or disposed inside the sealing material layer. That is, the substrate layer may be laminated on one surface of the sealing material layer or may be disposed inside the sealing material layer.
[0057] In the example shown in FIG. 1 , the pneumatic tire sealing sheet 10 according to this embodiment includes a sealing material layer 1 and a substrate layer 2 laminated on one surface of the sealing material layer 1. The sealing material layer 1 is attached to the inner surface of a pneumatic tire mounted on the wheel of a vehicle such as a bicycle or motorcycle. Examples of such pneumatic tires include tubeless tires and tubeless-ready tires. A tubeless tire refers to a tire that does not have a tube on its inner surface, but has an inner liner made of a rubber sheet instead of the tube. A tubeless-ready tire refers to a tire that does not have a tube on its inner surface, and does not have an inner liner either. Examples of vehicles on which such pneumatic tires can be mounted include road bikes, gravel road bikes, cross bikes, and mountain bikes.
[0058] As described above, the sealing material layer 1 is formed from the sealing material composition for a pneumatic tire. For example, the sealing material layer 1 can be obtained by blending and kneading the organic and inorganic components described above in the amounts described above, and then forming (gluing) the resulting composition into a sheet on the substrate layer 2.
[0059] For the kneading, for example, a batch type kneader such as a kneader, a Banbury mixer, or a mixing roll, or a continuous kneader such as a twin-screw kneader is used, and for forming into a sheet, a molding device such as an extruder, a calendar roll, or a press (heat press) is used.
[0060] In addition, when the sealing material composition for a pneumatic tire has hot-melt properties, the sealing material layer 1 may be produced using a hot-melt coater. Specifically, the sealing material layer 1 may be produced by applying the sealing material composition for a pneumatic tire having hot-melt properties to one surface of the substrate layer 2 to a predetermined thickness while heating the composition to a temperature of, for example, about 200°C using the hot-melt coater.
[0061] The thickness of the sealing material layer 1 is preferably 50 μm or more, more preferably 100 μm or more, even more preferably 150 μm or more, and even more preferably 200 μm or more. The thickness of the sealing material layer 1 is preferably 1500 μm or less, more preferably 1200 μm or less, even more preferably 1000 μm or less, and even more preferably 800 μm or less. By having the thickness of the sealing material layer 1 within the above range, the pneumatic tire sealing sheet 10 can be made lightweight and the workability of application to tires with large curved surfaces such as bicycle tires can be improved. Furthermore, in embodiments including a release liner described below, the roll shape is more easily maintained and adhesive overflow can be suppressed.
[0062] The sealant layer 1 may have a single layer structure, or may be formed by laminating two or more layers having different compositions. The single layer structure means a structure formed by one type of sealant composition for pneumatic tires. Therefore, a structure in which multiple layers formed by one type of sealant composition for pneumatic tires are laminated is a single layer structure.
[0063] When the sealing material layer 1 is configured by laminating two or more layers having different compositions, at least one layer has a storage modulus G' 1 The ratio of the product of the probe tack value T and the adhesive strength value A1 to the 1 ) is 12.0 or less. When at least one layer satisfies the above relationship, it is possible to suppress deterioration over time in the sealing property of a through hole formed in a pneumatic tire. Note that, in order to further suppress deterioration over time in the sealing property of a through hole formed in a pneumatic tire, it is preferable that all of the two or more layers having different compositions satisfy the above relationship.
[0064] The substrate layer 2 is made of a sheet material. The substrate layer 2 supports the sealing material layer 1 so as to maintain a predetermined shape. The substrate layer 2 functions to protect the surface of the sealing material layer 1 that is not attached to the adherend (the inner surface of the pneumatic tire). In other words, the substrate layer 2 also functions as an adhesive blocking layer.
[0065] The sheet material can be made of various known materials. The base material layer 2 is preferably made of a sheet material selected from the group consisting of a fiber sheet, a foam sheet, a solidreat, and a multilayer sheet made by laminating at least two of these materials.
[0066] Examples of the various known materials that can be used include organic materials such as cotton, wool, hemp, pulp (cellulose), rubber, and plastics, inorganic materials such as carbon, glass, ceramics, and metals, and mixtures thereof. Examples of the sheet material that can be used include organic fiber sheets, inorganic fiber sheets, foamed rubber sheets, foamed plastic sheets, solid rubber sheets (non-foamed sheets), solid plastic sheets (non-foamed sheets), solid metal sheets, and solid metal sheets laminated with solid plastic sheets. Among these, a fiber sheet is preferred as the sheet material.
[0067] The fibers constituting the fiber sheet may be synthetic resin fibers such as synthetic plastic fibers and synthetic rubber fibers; natural fibers such as cellulose fibers; or organic fibers such as semi-synthetic fibers. The fibers constituting the fiber sheet may be metal fibers such as copper fibers, aluminum fibers, and iron fibers; glass fibers; basalt fibers; alumina fibers; ceramic fibers such as rock wool; or inorganic fibers such as carbon fibers. The fibers constituting the fiber sheet are preferably synthetic resin fibers. Examples of the synthetic resin fibers include fibers made of thermoplastic resins and fibers made of thermosetting resins. The synthetic resin fibers are preferably fibers made of thermoplastic resins.
[0068] Examples of the thermoplastic resin include polyolefin resins such as polyethylene (PE) and polypropylene (PP); polyester resins such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polylactic acid (PLA), and polybutylene succinate (PBS); polyamide resins such as polyamide 6 and polyamide 6,6; and cellulose resins such as cellulose acetate. These thermoplastic resins may be used alone or in combination of two or more. Among these, polyolefin resins and polyester resins are preferably used as the thermoplastic resin. Furthermore, polypropylene (PP) is preferably used as the polyolefin resin, and polyethylene terephthalate (PET) is preferably used as the polyester resin.
[0069] The fiber sheet may be a nonwoven fabric sheet or a woven fabric sheet. The nonwoven fabric sheet may be one manufactured by various known methods. The nonwoven fabric sheet may be one manufactured by either a dry method or a wet method. Examples of the nonwoven fabric sheet include a spunbonded nonwoven fabric sheet, a thermally bonded nonwoven fabric sheet, a chemically bonded nonwoven fabric sheet, a stitchbonded nonwoven fabric sheet, a needlepunched nonwoven fabric sheet, a meltblown nonwoven fabric sheet, a spunlaced nonwoven fabric sheet, and a steamjet nonwoven fabric sheet.
[0070] The nonwoven fabric sheet has a basis weight of 10 g / m 2 It is preferable that the content is 20 g / m or more. 2 More preferably, it is 30 g / m or more. 2 It is more preferable that the basis weight of the nonwoven fabric sheet is 200 g / m or more. 2 Preferably, the weight is 180 g / m or less. 2 More preferably, it is 160 g / m or less. 2It is more preferable that the basis weight is not more than 1 / 2 mm. When the basis weight is within the above range, the base material layer 2 made of the nonwoven fabric sheet has sufficient tensile strength. In addition, peeling of the sealant layer 1 from the inner surface of the tire, which would otherwise occur if the base material layer 2 were too rigid, can be suppressed.
[0071] The woven fabric sheet can be manufactured using various known looms. The woven fabric sheet may be woven by any weaving method. Examples of the woven fabric sheet include a plain weave sheet, a twill weave sheet, and a satin weave sheet.
[0072] The above-described fiber sheet has the advantage of having higher puncture resistance when pierced by sharp foreign objects (e.g., nails, glass fragments, etc.) compared to solid rubber sheets or solid plastic sheets. On the other hand, if the base layer 2 is composed solely of the fiber sheet, components such as the tackifier contained in the sealing material layer 1 may migrate into the base layer 2. To sufficiently suppress such component migration, the sheet material constituting the base layer 2 is preferably a multilayer sheet formed by laminating the fiber sheet and the solid sheet. In such a multilayer sheet, the sealing material layer 1 is preferably laminated on the exposed surface of the solid sheet. An example of such a multilayer sheet is one formed by laminating a fiber sheet and a solid sheet of polyolefin resin (e.g., a polyethylene sheet or a polypropylene sheet) that is thinner than the fiber sheet. The sheet material constituting the base layer 2 may also be a multilayer sheet formed by laminating a spunbond nonwoven fabric and a meltblown nonwoven fabric that has finer fibers and a denser weave than the spunbond nonwoven fabric. In such a multilayer sheet, it is preferable that a sealing material layer 1 is laminated on the exposed surface of the meltblown nonwoven fabric.
[0073] The sheet material constituting the base layer 2 may also be a solid plastic sheet (non-foamed sheet). Examples of such solid plastic sheets include thermoplastic polyurethane films made using a thermoplastic polyurethane resin. Commercially available thermoplastic polyurethane films include "Tough Grace TG88-I 25 / 50" manufactured by Takeda Sangyo Co., Ltd. "Tough Grace TG88-I 25 / 50" is a 25 μm-thick urethane film with a 50 μm-thick polyethylene release liner laminated on one surface. As described above, when the base layer 2 is constructed by laminating a release liner on one surface of a urethane film, the release liner is peeled off from one surface of the urethane film after the sealing material layer 1 is laminated on the other surface (exposed surface) of the urethane film.
[0074] The thickness of the substrate layer 2 is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and even more preferably 20 μm or more. The thickness of the substrate layer 2 is preferably 3 mm or less, more preferably 2 mm or less, and even more preferably 1 mm or less. When the thickness of the substrate layer 2 is within the above range, the pneumatic tire sealing sheet 10 can be made lightweight, and the workability of application to tires with large curved surfaces such as bicycle tires can be improved. Furthermore, in embodiments including a release liner described below, the roll shape is more easily maintained.
[0075] As in the modified example shown in Fig. 2, the sealing sheet 10 for a pneumatic tire according to this embodiment may include a sealing material layer 1 and a substrate layer 2 disposed inside the sealing material layer 1. Even when the sealing sheet 10 for a pneumatic tire is configured as shown in Fig. 2, the substrate layer 2 can support the sealing material layer 1 so as to maintain a predetermined shape. The sealing sheet 10 for a pneumatic tire according to the modified example shown in Fig. 2 can be produced by impregnating the sheet material that will become the substrate layer 2 in the sealing material composition for a pneumatic tire.
[0076] Next, a sealing sheet for a pneumatic tire according to still another embodiment will be described with reference to FIG.
[0077] As shown in Fig. 3, the sealing sheet 10 for a pneumatic tire according to this embodiment comprises a sealing material layer 1, an optional substrate layer 2 laminated on one surface of the sealing material layer 1, and an adhesive layer 3 laminated on the other surface (exposed surface) of the sealing material layer 1. In the sealing sheet 10 for a pneumatic tire, if the adhesive strength of the sealing material layer 1 to the adherend (the inner surface of the pneumatic tire) is insufficient, a configuration including an adhesive layer 3 as shown in Fig. 3 can be adopted. That is, in such a sealing sheet 10 for a pneumatic tire, it is preferable that the adhesive layer 3 ensures adhesion to the adherend (the inner surface of the pneumatic tire).
[0078] The sealing sheet 10 for a pneumatic tire according to this embodiment shown in Figure 3 can be produced by obtaining the sealing sheet 10 for a pneumatic tire as shown in Figure 1, and then forming (gluing) a pressure-sensitive adhesive composition containing predetermined amounts of organic and inorganic components into a sheet on the exposed surface of the sealing material layer 1 to obtain a pressure-sensitive adhesive layer 3. The pressure-sensitive adhesive composition can be obtained using various kneading machines, as with the sealing material composition. Furthermore, the sheet formation can be carried out using a molding device such as an extruder, a calendar roll, or a press (heat press), as described above.
[0079] The adhesive layer 3 preferably has an adhesive strength A1' to a tire at 23° C. of 10 N / 20 mm or more, more preferably 20 N / 20 mm or more.
[0080] The pressure-sensitive adhesive layer 3 may contain butyl rubber as an organic component.
[0081] Butyl rubber is a copolymer (isobutylene-isoprene) of isobutene (isobutylene) and a small amount of isoprene. Examples of butyl rubber include synthetic butyl rubber and recycled butyl rubber. The pressure-sensitive adhesive layer 3 preferably contains synthetic butyl rubber as a main component. Based on the total amount of butyl rubber, the pressure-sensitive adhesive layer 3 preferably contains 70% by mass or more of synthetic butyl rubber, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 100% by mass. In other words, it is particularly preferable that all of the butyl rubber contained in the pressure-sensitive adhesive layer 3 is synthetic butyl rubber. This is because the recycled butyl rubber is obtained by recycling rubber products (e.g., tires, tubes, etc.) obtained from butyl rubber with oil such as pine oil or mineral oil, and therefore the recycled butyl rubber contains residual oil as an impurity.
[0082] The mass average molecular weight of the butyl rubber is preferably 30,000 or more and 1,500,000 or less. The mass average molecular weight can be determined as a standard polystyrene equivalent value from GPC (gel permeation chromatography) measurement. The GPC method can be performed in the same manner as described in the method for measuring the mass average molecular weight of a thermoplastic elastomer. The mass average molecular weight of the butyl rubber is more preferably 200,000 or more, and even more preferably 300,000 or more. Furthermore, the mass average molecular weight of the butyl rubber is more preferably 800,000 or less, and even more preferably 700,000 or less.
[0083] The pressure-sensitive adhesive layer 3 may contain an elastomer component other than butyl rubber as an organic component. Examples of the elastomer component other than butyl rubber include rubbers other than butyl rubber and thermoplastic elastomers.
[0084] Examples of rubbers other than butyl rubber include polyisobutylene rubber, acrylic rubber, silicone rubber, urethane rubber, vinyl alkyl ether rubber, polyvinyl alcohol rubber, polyvinylpyrrolidone rubber, polyacrylamide rubber, cellulose rubber, natural rubber, butadiene rubber, chloroprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, isoprene rubber, and ethylene-propylene rubber (EPDM).
[0085] The thermoplastic elastomer may be the same as that described above.
[0086] The PSA layer 3 may contain only the thermoplastic elastomer as the rubber other than the butyl rubber. In such a case, the PSA layer 3 may contain 70% by mass or more of the butyl rubber and 30% by mass or less of the thermoplastic elastomer, where the total content of the butyl rubber and the thermoplastic elastomer is taken as 100% by mass. In addition, in the above case, the PSA layer 3 may contain 80% by mass or more of the butyl rubber and 20% by mass or less of the thermoplastic elastomer. Furthermore, in the above case, the PSA layer 3 may contain 1% by mass or more, 2% by mass or more, or 3% by mass or more of the thermoplastic elastomer.
[0087] The pressure-sensitive adhesive layer 3 may contain 70% by mass or more, 80% by mass or more, 90% by mass or more, or even 100% by mass of synthetic butyl rubber as the butyl rubber. The pressure-sensitive adhesive layer 3 may contain the butyl rubber as described above and, in addition, may contain only a thermoplastic elastomer as a rubber other than the butyl rubber. The butyl rubber content and the thermoplastic elastomer content may be as described above.
[0088] The pressure-sensitive adhesive layer 3 preferably contains 8% by mass or more, and more preferably 10% by mass or more, of the elastomer component. The pressure-sensitive adhesive layer 3 may contain 100% by mass, 90% by mass or less, 70% by mass or less, or 50% by mass or less of the elastomer component. The elastomer component is a general term that refers to butyl rubber, rubbers other than butyl rubber, and thermoplastic elastomers.
[0089] The pressure-sensitive adhesive layer 3 may contain, as organic components other than the elastomer component, a softener, a tackifier, an antioxidant, etc. As the softener, the tackifier, and the antioxidant, the same ones as those described above can be used.
[0090] The pressure-sensitive adhesive layer 3 may contain an inorganic component. The pressure-sensitive adhesive layer 3 may contain an inorganic filler and an inorganic colorant as the inorganic components. The pressure-sensitive adhesive layer 3 preferably contains an inorganic filler as the inorganic component. The inorganic filler and the inorganic colorant may be the same as those described above. The pressure-sensitive adhesive layer 3 preferably contains calcium carbonate as the inorganic filler. The content of the inorganic filler in the pressure-sensitive adhesive layer 3 is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 70% by mass or less.
[0091] The pressure-sensitive adhesive layer 3 preferably contains 500 parts by mass or less, more preferably 450 parts by mass or less, and even more preferably 400 parts by mass or less of the inorganic component per 100 parts by mass of the elastomer component. The pressure-sensitive adhesive layer 3 preferably contains 50 parts by mass or more, more preferably 150 parts by mass or more, and even more preferably 270 parts by mass or more of the inorganic component per 100 parts by mass of the elastomer component.
[0092] The thickness of the pressure-sensitive adhesive layer 3 is preferably 50 μm or more, more preferably 100 μm or more, and is preferably 500 μm or less, more preferably 400 μm or less.
[0093] Next, a sealing sheet for a pneumatic tire according to still another embodiment will be described with reference to FIG.
[0094] As shown in Figure 4, the sealing sheet 10 for a pneumatic tire according to this embodiment includes a sealing material layer 1 and a release liner 4 laminated on the sealing material layer 1. In this embodiment, the sealing material layer 1 has a first surface, which is an adhesive surface to be adhered to the tire, and a second surface opposite the first surface. The release liner 4 is laminated on the second surface. According to this embodiment, when attaching the sealing material layer 1 to a tire, the sealing material layer 1 can be brought into contact with the tire while pressing the outer surface of the release liner 4 with a finger or the like. This makes it easy to adapt the sealing material layer 1 to the tire.
[0095] From the viewpoint of improving the workability of this operation, the tensile modulus of the release liner 4 at 23°C is preferably 4000 MPa or less. This improves the workability of attaching the release liner 4 to tires having a curved surface with a large curvature, such as bicycle tires. Furthermore, the tensile modulus of the release liner 4 at 23°C is more preferably 1000 MPa or more. This makes it possible to prevent damage to the release liner 4 due to pressure during the above-mentioned operation.
[0096] The tensile modulus of the release liner 4 at 23°C is calculated from the results of a tensile test. The tensile test is carried out under the following measurement conditions. [Measurement conditions] Test environment: 23°C ± 2°C, 50% RH ± 10% RH Test piece shape: Width 10 mm, length 50 mm Tensile speed: 300 mm / min Chuck distance: 10 mm The tensile modulus E is calculated from the slope of the stress-strain curve for the strain at two specified points (the ratio of the tensile stress within the tensile proportional limit to the corresponding strain). t Specifically, ε of the stress-strain curve is calculated. 1 = 0.10 is the stress at σ1 , ε 2 = 0.05 is the stress at σ 2 When t Is E t = (σ 2 -σ 1 ) / (ε 2 -ε 1 If there is no straight line in the stress-strain curve, the slope of the tangent at the deformation start point is taken as the tensile modulus.
[0097] The thickness of the release liner 4 is preferably 0.02 mm or more, more preferably 0.05 mm or more, and even more preferably 0.08 mm or more. The thickness of the release liner layer 4 is preferably 0.8 mm or less, more preferably 0.5 mm or less, and even more preferably 0.3 mm or less. When the thickness of the release liner 4 is within the above range, the sealing sheet 10 for a pneumatic tire can be easily attached to the curved surface of the tire with good conformability, thereby improving the sealing properties. Furthermore, in embodiments including a release liner described below, the roll shape is more easily maintained.
[0098] Before use (e.g., during storage), the sealing sheet 10 for a pneumatic tire according to this embodiment may be wound into a roll shape with the release liner 4 on the outside and the sealing material layer 1 on the inside for compactness. In this case, the tolerance of the thickness of the sealing material layer 1, based on the average thickness of the sealing material layer 1, is preferably 25% or less of the average thickness, more preferably less than 20%. This makes it easier for the inner peripheral surface of the sealing material layer 1 in the nth turn to come into contact with the outer peripheral surface of the release liner 4 in the (n-1)th turn, making it easier to maintain the roll shape.
[0099] Both side edge portions of the release liner 4 are preferably dry edge portions 41 where the sealant layer 1 is not laminated. The width of each dry edge portion 41 is preferably 1 mm or more. This makes it possible to prevent adhesive from spilling out from the release liner 4 when the pneumatic tire sealing sheet 10 is rolled up. This can facilitate the work of attaching the sealant layer 1 to the tire. Furthermore, by pinching the dry edge portions 41, the release liner 4 can be easily peeled from the sealant layer 1 attached to the tire. Furthermore, during peeling, inadvertent peeling of the sealant layer 1 adhered to the tire can be suppressed.
[0100] The release liner 4 may be, for example, a resin film or a paper film. Examples of resin films include polyethylene terephthalate resin film, polyethylene film, and polypropylene film. It is preferable that at least the surface of the release liner 4 that is laminated with the sealing material layer 1 is treated with a surface treatment agent. Examples of surface treatment agents include silicone-based surface treatment agents and fluorine-based surface treatment agents.
[0101] In this embodiment, a pressure-sensitive adhesive layer 3 may be laminated on the surface of the sealing material layer 1 opposite to the second surface.
[0102] Next, matters common to the above embodiments will be mainly described.
[0103] The thickness of the sealing sheet 10 for a pneumatic tire according to each embodiment is preferably 50 μm or more, more preferably 100 μm or more, even more preferably 150 μm or more, even more preferably 200 μm or more, and particularly preferably 500 μm or more. The thickness of the sealing sheet 10 for a pneumatic tire is preferably 2500 μm or less, more preferably 2000 μm or less, even more preferably 1500 μm or less, and particularly preferably 1000 μm or less.
[0104] In embodiments including a release liner 4, the ratio of the thickness of the pneumatic tire sealing sheet 10 to the thickness of the release liner 4 (thickness of the pneumatic tire sealing sheet 10 / thickness of the release liner 4) is preferably 30 or less, more preferably 25 or less, even more preferably 20 or less, and particularly preferably 10 or less. The ratio of the thickness of the pneumatic tire sealing sheet 10 to the thickness of the release liner 4 is preferably 0.5 or more, more preferably 1 or more, and even more preferably 2 or more. This allows the pneumatic tire sealing sheet 10 to be easily attached with good conformability to the curved surface of the tire, thereby improving sealing properties. Furthermore, the roll shape is more easily maintained, and adhesive overflow can be suppressed.
[0105] The sealing sheet 10 for a pneumatic tire according to each embodiment has a mass per unit volume of 1500 g / m 2 Preferably, the weight is 1300 g / m or less. 2 More preferably, it is 1200 g / m or less. 2 It is more preferable that the mass per unit volume is within the above range. When the mass per unit volume is within the above range, the sealing sheet for a pneumatic tire according to each embodiment can be made relatively lightweight.
[0106] The sealing sheet 10 for a pneumatic tire according to each embodiment has a mass per unit volume of 50 g / m 2 It is preferable that the content is 100 g / m or more. 2 More preferably, it is 200 g / m or more. 2 When the mass per unit volume is within the above-mentioned range, the sealing sheet for a pneumatic tire according to each embodiment can stably exhibit sealing properties.
[0107] When the sealing sheet for a pneumatic tire is composed only of the sealing material layer 1, the mass per unit volume of the sealing sheet for a pneumatic tire means the mass per unit volume of the sealing material layer 1. When the sealing sheet for a pneumatic tire includes a substrate layer 2 in addition to the sealing material layer 1 as shown in Figures 1 and 2, the mass per unit volume of the sealing sheet for a pneumatic tire means the sum of the mass per unit volume of the sealing material layer 1 and the mass per unit volume of the substrate layer 2. When the sealing sheet for a pneumatic tire includes a substrate layer 2 and a pressure-sensitive adhesive layer 3 in addition to the sealing material layer 1 as shown in Figure 3, the mass per unit volume of the sealing sheet for a pneumatic tire means the sum of the mass per unit volume of the sealing material layer 1, the mass per unit volume of the substrate layer 2, and the mass per unit volume of the pressure-sensitive adhesive layer 3. The mass here does not include the release liner.
[0108] The sealing sheet 10 for a pneumatic tire according to each embodiment is preferably configured in a tape shape. 0 (mm), and the dimension in the width direction of the sealing sheet 10 for a pneumatic tire to be attached to the inside of the pneumatic tire (tape width: mm) is W 1 When the tape width W 1 is the width W of the pneumatic tire 0 The width W of the pneumatic tire is preferably 10% or more. 0 The tape width W 1 The ratio (W 1 / W 0 × 100) may be 25% or more, 50% or more, or 100% or more. 1Preferably, the width corresponds to the width of a bicycle tire in accordance with the ETRTO standard, and is more preferably 25 to 62 mm. Such a pneumatic tire sealing sheet 10 can cover the inner surface of the ground contact portion 110 of the pneumatic tire 100 shown in FIG. 6, covering a portion of the inner surface of the sidewall portion 120. This allows the pneumatic tire sealing sheet 10 to reliably cover the ground contact portion 110, which is relatively prone to through-holes. Furthermore, the inner surface of the pneumatic tire 100, where it transitions from the ground contact portion 110 to the sidewall portion 120, is a curved surface with a large curvature, and therefore a sheet provided with the release liner described above is effective for such a curved surface. Note that the width here does not include the release liner.
[0109] (Examples of Use of the Pneumatic Tire Seal Sheet) Next, examples of use of the pneumatic tire seal sheet 10 according to each embodiment will be described. Below, an example will be described in which the pneumatic tire seal sheet 10 according to the present embodiment is attached to the inner surface of a bicycle tire.
[0110] 5 and 6 are schematic diagrams showing a bicycle wheel. The wheel 1000 includes a pneumatic tire 100 and a wheel 200 on which the pneumatic tire 100 is mounted. The wheel 200 may be of a disc type or a spoke type. The wheel 200 shown in FIG. 5 is of a spoke type.
[0111] The wheel 200 is located at the center of the wheel 1000 and includes a disc-shaped hub 210 that is rotatably mounted on a bicycle fork (not shown), multiple spokes 220 that extend radially outward from the outer periphery of the hub 210, and a rim 230 that is fixed by the spokes 220. As shown in FIG. 6 , the rim 230 includes a base portion 231 to which the outer ends of the spokes 220 are fixed. The base portion 231 is cylindrical, with the rotational axis of the wheel 1000 as its central axis. The dimension of the base portion 231 in the axial direction (the width direction W of the pneumatic tire 100) is approximately the same as the width of the pneumatic tire 100. The rim 230 includes a pair of flanges 232 that extend outward in the radial direction D from both axial ends of the base portion 231. The pneumatic tire 100 is mounted on the wheel 200 by inserting both ends in the width direction W into the flanges 232.
[0112] As shown in Figure 6, the rim 230 has a base portion 231 and flange portions 232 extending outward in the radial direction D from both ends of the base portion 231, which have an inverted U-shaped cross section in a plane perpendicular to the circumferential direction C of the wheel 1000. On the other hand, the pneumatic tire 100 has a U-shaped cross section. The U-shaped bottom portion of the pneumatic tire 100 facing the base portion 231 forms a ground contact portion 110 that comes into contact with the ground. The pneumatic tire 100 has sidewall portions 120 that extend inward in the radial direction D from both ends of the ground contact portion 110 in the width direction W of the pneumatic tire 100. The pneumatic tire 100 has bead portions 140 that protrude slightly axially outward at the end of the sidewall portion 120 opposite the ground contact portion 110. In the wheel 200, the tip of the flange 232 has a shape (hook-like) that is bent inward in the width direction W, and both ends of the pneumatic tire 100 in the width direction W are disposed inside the flange 232. The pneumatic tire 100 is mounted to the rim 230 with the bead portions 140 and the sidewall portions 120 near the bead portions 140 abutting against the inside of the flange 232, and with the bead portions 140 engaged with the tip of the flange 232.
[0113] The wheel 1000 is equipped with a valve 240 for pressurizing a gas such as air or nitrogen gas into an internal space S surrounded by the rim 230 and the pneumatic tire 100. In this embodiment, when gas is pressurized through the valve 240, the pair of side wall portions 120 of the pneumatic tire 100 spaced apart in the width direction W are deformed in directions away from each other and come into strong contact with the flange portion 232. This causes the pneumatic tire 100 to be firmly fixed to the rim 230.
[0114] The wheel 1000 is not provided with a tube that expands in the internal space S. As shown in Fig. 6, the wheel 1000 is provided with a sealing sheet 10 for a pneumatic tire on the inner surface of the pneumatic tire 100. Note that Fig. 6 omits detailed configuration of the sealing sheet 10 for a pneumatic tire. That is, Fig. 6 shows the configuration of the sealing sheet 10 for a pneumatic tire from which the sealing material layer 1, the base material layer 2, etc. are omitted.
[0115] Next, with reference to FIGS. 7A and 7B, the mechanism of action exhibited when the sealing sheet for a pneumatic tire 10 is attached to the inner surface of the pneumatic tire 100 will be described.
[0116] As shown in FIG. 7A , when a nail N penetrates a pneumatic tire 100, a through-hole H is formed in the pneumatic tire 100 from the outer surface (the surface in contact with the road) toward the inner surface. If the pneumatic tire 100 is ridden on a road surface with the nail N still embedded in it, the wheel 200 on which the pneumatic tire 100 is mounted may be damaged by the nail N. Therefore, the bicycle rider typically pulls the nail N out of the pneumatic tire 100. As a result, the through-hole H is exposed in the pneumatic tire 100 (see FIG. 7B ). In order to seal the exposed through-hole H, the sealant layer 1 included in the pneumatic tire sealing sheet 10 must have physical properties that allow it to follow the outward withdrawal of the nail N when it is pulled outward. That is, the sealant layer 1 must have physical properties that allow it to firmly adhere to the rod-shaped portion of the nail N and, as shown in FIG. 7B , have appropriate hardness to follow the outward withdrawal of the nail N and fill the exposed portion of the through-hole H. Furthermore, in a state where a sealant has been formed by the sealing material layer 1 filling a portion of the exposed through-hole H, it is necessary to prevent the sealant from being extruded to the outside of the pneumatic tire 100 by the internal pressure of the pneumatic tire 100 that increases when the bicycle is ridden on a road surface. To achieve this, the sealing material layer 1 that forms the sealant needs to have an appropriate hardness. Taking the above into consideration, the sealing material layer 1 needs to have adhesive properties that allow it to firmly adhere to the rod-shaped portion of the nail N, as well as appropriate viscoelastic properties that prevent it from being extruded to the outside of the pneumatic tire 100 when it fills a portion of the through-hole H or becomes a sealant inside the through-hole H.
[0117] Here, in the sealing sheet 10 for a pneumatic tire according to this embodiment, the sealing material layer 1 has a storage modulus G', which is a parameter of the viscoelastic property. 1 and the probe tack value T and the adhesive force A1, which are parameters relating to adhesiveness, satisfy a specific relationship. 1 The ratio of the product of the probe tack value T and the adhesive strength A1 to the1 ) satisfies the specific relationship that the ratio of the surface area of the through-hole H to the surface area of the pneumatic tire 100 is 12.0 or less. Therefore, the sealing material layer 1 can form a sealant so as to suitably fill a part of the through-hole H exposed in the pneumatic tire 100, and can sufficiently prevent the sealant from being pushed out to the outside of the pneumatic tire 100 due to the internal pressure of the pneumatic tire 100 that increases when the tire is driven on a road surface.
[0118] As shown in FIG. 6 , if the length along the inner wall surface 100a from the lowest point 100b of the inner wall surface 100a of the pneumatic tire 100 to the top end of the pneumatic tire 100 is L (mm), the pneumatic tire sealing sheet 10 is preferably attached so as to cover at least an area of 0.1L on each side in the width direction W from the lowest point 100b. In other words, the pneumatic tire sealing sheet 10 is preferably provided so as to cover 10% or more of the width direction length (2L) along the inside of the pneumatic tire 100. The pneumatic tire sealing sheet 10 is more preferably provided so as to cover 15% or more of the width direction length (2L) along the inside surface of the pneumatic tire 100, and even more preferably so as to cover 20% or more. Note that the pneumatic tire sealing sheet 10 may be provided so as to cover 100% or less of the width direction length (2L) along the inside surface of the pneumatic tire 100. As described above, by attaching the sealing sheet 10 for pneumatic tires to the inner wall surface 100a of the pneumatic tire 100, it is possible to effectively prevent punctures from occurring when a foreign object with a sharp tip, such as a nail, pierces the pneumatic tire 100.
[0119] The matters disclosed by this specification include the following.
[0120] (1) A sealing material layer is provided, and the value G' of the storage modulus of the sealing material layer at -20°C is 1 When the probe tack value of the sealing material layer at 23° C. is T and the adhesive strength of the sealing material layer to a tire at 23° C. is A1, the storage modulus value G′ 1The ratio of the product of the probe tack value T and the adhesive strength value A1 to the 1 ) is 12.0 or less.
[0121] (2) The storage modulus G' 1 The sealing sheet for a pneumatic tire according to (1) above, wherein the compressive strength is 0.50 MPa or more.
[0122] (3) The sealing sheet for a pneumatic tire according to (1) or (2) above, wherein the probe tack value T is 0.05 MPa or more.
[0123] (4) The sealing sheet for a pneumatic tire according to any one of (1) to (3) above, wherein the sealing material layer contains a thermoplastic elastomer as an organic component.
[0124] (5) The sealing sheet for a pneumatic tire according to (4) above, wherein the thermoplastic elastomer is a styrene-based thermoplastic elastomer.
[0125] (6) The sealing sheet for a pneumatic tire according to (5) above, wherein the styrene-based thermoplastic elastomer has a diblock ratio of 10% or more and 80% or less.
[0126] (7) The sealing sheet for a pneumatic tire according to any one of (1) to (6) above, wherein the adhesive strength value A1 is 1.0 N / 20 mm or more.
[0127] (8) The sealing sheet for a pneumatic tire according to any one of (1) to (7), wherein when the adhesive strength value A2 of the sealing material layer to the tire at −20° C. is set to A2, the adhesive strength value A2 is 1.0 N / 20 mm or more.
[0128] (9) The sealing sheet for a pneumatic tire according to any one of (1) to (8) above, wherein the tire is a tubeless tire or a tubeless-ready tire.
[0129] (10) The sealing sheet for a pneumatic tire according to any one of (1) to (9) above, further comprising a substrate layer laminated on one surface of the sealing material layer or disposed inside the sealing material layer.
[0130] (11) The sealing sheet for a pneumatic tire according to any one of (1) to (10) above, wherein the sealing material layer is configured by laminating two or more layers having different compositions.
[0131] (12) The sealing sheet for a pneumatic tire according to (10) or (11) above, wherein the base layer is made of a sheet material selected from the group consisting of a fiber sheet, a foamed sheet, a solid sheet, and a multilayer sheet formed by laminating at least two of these.
[0132] (13) Mass per unit volume: 1500 g / m 2 The sealing sheet for a pneumatic tire according to any one of (10) to (12) above, wherein:
[0133] (14) The sealing sheet for a pneumatic tire according to any one of (10) to (13) above, which is configured in a tape-like shape and has a width that is 10% or more of the width of the pneumatic tire as defined by the ETRTO standard. (15) The sealing sheet for a pneumatic tire according to any one of (1) to (14) above, which is configured in a tape-like shape and further comprises a release liner laminated on the sealant layer, the release liner being laminated on the side of the sealant layer opposite to the side that adheres to the tire. (16) The sealing sheet for a pneumatic tire according to (15) above, in which the release liner has a tensile modulus at 23°C of 4000 MPa or less. (17) The sealing sheet for a pneumatic tire according to (15) or (16) above, which is in a roll shape wound so that the release liner is disposed on the outside, and in which the tolerance of the thickness of the sealant layer, based on the average thickness of the sealant layer, is 25% or less of the average thickness. (18) The sealing sheet for a pneumatic tire according to any one of (15) to (17) above, wherein both side edge portions of the release liner are dry edge portions where the sealing material layer is not laminated. (19) The sealing sheet for a pneumatic tire according to (18) above, wherein each dry edge portion has a width of 1 mm or more.
[0134] It should be noted that the sealing sheet for a pneumatic tire according to the present invention is not limited to the above-described embodiment. Furthermore, the sealing sheet for a pneumatic tire according to the present invention is not limited by the above-described effects. The sealing sheet for a pneumatic tire according to the present invention can be modified in various ways without departing from the gist of the present invention.
[0135] The present invention will now be described in more detail with reference to examples. The following examples are intended to explain the present invention in more detail, but are not intended to limit the scope of the present invention.
[0136] First, the raw materials shown in Table 1 below will be described. (1) Elastomer Component (a) Thermoplastic Elastomer Styrene-Isoprene-Styrene Copolymer (SIS) SIS1: Styrene Amount 15% by Mass, Diblock Ratio 78% SIS2: Styrene Amount 16% by Mass, Diblock Ratio 56% SIS3: Styrene Amount 14% by Mass, Diblock Ratio 26% Styrene-Isobutylene-Styrene Copolymer (SIBS) SIBS1: Styrene Amount 14% by Mass, Diblock Ratio 26% Note that SIS1 is manufactured by Nippon Zeon Corporation under the trade name "Quintac 3520," SIS2 is manufactured by Nippon Zeon Corporation under the trade name "Quintac 3433N," SIS3 is manufactured by Nippon Zeon Corporation under the trade name "Quintac 3421," and SIBS1 is manufactured by Kaneka Corporation under the trade name "SIBSTAR (registered trademark) 062M."(b) Butyl rubber (IIR) JSR BUTYL 268 (manufactured by JSR Corporation, mass average molecular weight 500,000) (2) Tackifier Tackifier 1: Terpene resin a (manufactured by Yasuhara Chemical Co., Ltd., trade name "YS Resin PX1150N", softening point 115°C) Tackifier 2: Terpene resin b (manufactured by Yasuhara Chemical Co., Ltd., trade name "YS Resin PX300N", softening point 30°C) Tackifier 3: Aromatic petroleum resin (manufactured by Kraton Corporation, trade name "SYLVARES SA140", softening point 137°C) Tackifier 4: Rosin ester (manufactured by Arakawa Chemical Industries, Ltd., trade name "Pensel D-160", softening point 150 to 165°C) Tackifier 5: C5 hydrocarbon (manufactured by TonenGeneral Sekiyu K.K., trade name "T-REZ" RC093, softening point 93 ° C, number average molecular weight 890) Tackifier 6 Copolymer resin of C5 hydrocarbon and C9 hydrocarbon (aromatic hydrocarbon) (trade name "Quintac N180" manufactured by Nippon Zeon Co., Ltd., softening point 80 ° C) (3) Softener Paraffin oil 1 Idemitsu Kosan Co., Ltd., trade name "Diana Process Oil NS-90S") Hydrocarbon 1 DAELIM CORPORATION, trade name "PB1300" (number average molecular weight 1280) Hydrocarbon 2 ENEOS Corporation, trade name "Nippon Oil Polybutene HV-300" Paraffin oil 2 Idemitsu Kosan Co., Ltd., trade name "Diana Process Oil PW-90" (4) Inorganic filler Calcium carbonate Heavy calcium carbonate (manufactured by Maruo Calcium Co., Ltd., sieve residue (350 mesh) 0.5% or less (JIS (5) Coloring agent Carbon: Seast 3H (carbon black, manufactured by Tokai Carbon Co., Ltd.).
[0137] Rubber components (thermoplastic elastomer and butyl rubber), a tackifier, a softener, an inorganic filler, and a colorant were blended in the blending ratios (parts by mass) shown in Table 1 below, and heated to obtain sealing material compositions for pneumatic tires according to Examples 1 to 13 and Comparative Examples 1 and 2. Note that, hereinafter, the sealing material compositions for pneumatic tires will be simply referred to as sealing material compositions.
[0138] Example 1 The sealing material composition according to Example 1 was applied to the exposed surface (the surface on which the release liner was not attached) of a substrate layer (a urethane film with a release liner (trade name "Tough Grace TG88-I 25 / 50" manufactured by Takeda Sangyo Kaisha, Ltd.; the urethane film was 25 μm thick and the release liner (made of polyethylene) was 50 μm thick) to form a sealant layer. Specifically, the exposed surface of the substrate layer was coated with a hot melt coater while heating to 150° C. to form a sealant layer to a thickness of 0.5 mm. Next, the pressure-sensitive adhesive composition according to Example 1 was applied to the exposed surface of the sealant layer to form a pressure-sensitive adhesive layer. Specifically, the pressure-sensitive adhesive composition according to Example 1 was transfer-coated onto the exposed surface of the sealant layer using calendar rolls (four 8-inch rolls) while heating to 80° C. to form a pressure-sensitive adhesive layer. The pressure-sensitive adhesive composition according to Example 1 contained 10 parts by mass of SIS2 as a thermoplastic elastomer and 10 parts by mass of JSR butyl rubber. The seal sheet for a pneumatic tire according to Example 1 contained 90 parts by mass of BUTYL 268, 15 parts by mass of tackifier 5, 260 parts by mass of hydrocarbon polybutene (PB1300) as a softener, 380 parts by mass of calcium bicarbonate, and 3 parts by mass of carbon (SEAT 3H). The entire urethane film with release liner was then peeled off to obtain the seal sheet for a pneumatic tire according to Example 1. In other words, the seal sheet for a pneumatic tire according to Example 1 did not include a substrate layer. Hereinafter, the seal sheet for a pneumatic tire will be simply referred to as the seal sheet.
[0139] [Example 2] A sealing sheet according to Example 2 was obtained in the same manner as in Example 1, except that only the release liner was peeled off from the urethane film with the release liner. That is, the sealing sheet according to Example 2 had a urethane film with a thickness of 25 μm as the base layer.
[0140] Example 3 A sealing sheet according to Example 3 was obtained in the same manner as in Example 2, except that the mass of the sealing material layer and the total mass of the sealing sheet were changed as shown in Table 2.
[0141] [Example 4] A sealing sheet according to Example 4 was obtained in the same manner as in Example 2, except that the sealing composition according to Example 4 was used instead of the sealing composition according to Example 2, and the pressure-sensitive adhesive layer was not formed.
[0142] Example 5 A sealing sheet according to Example 5 was obtained in the same manner as in Example 4, except that the sealing composition according to Example 5 was used instead of the sealing composition according to Example 4.
[0143] Example 6 A sealing sheet according to Example 6 was obtained in the same manner as in Example 2, except that the sealing composition according to Example 6 was used instead of the sealing composition according to Example 2.
[0144] Example 7 A sheet according to Example 7 was obtained in the same manner as in Example 1, except that the sealing material composition according to Example 7 was used instead of the sealing material composition according to Example 1.
[0145] [Example 8] A sealing sheet according to Example 8 was obtained in the same manner as in Example 2, except that a sealing material composition for forming a first layer and a sealing material composition for forming a second layer were used instead of the sealing material composition according to Example 2, and a pressure-sensitive adhesive layer was not formed. The sealing material composition for forming the first layer had the same composition as the sealing material composition according to Example 1, and the sealing material composition for forming the second layer had the same composition as the sealing material composition according to Example 4. In the sealing sheet according to Example 8, sealing material layers were formed in the order of the first layer and the second layer on the substrate layer. That is, in the sealing sheet according to Example 8, the second sealing material layer had an exposed surface (adhesive surface). In addition, in the sealing sheet according to Example 8, the thickness of the first sealing material layer was 0.15 mm, and the thickness of the second sealing material layer was 0.8 mm.
[0146] Example 9 A sealing sheet according to Example 9 was obtained in the same manner as in Example 4, except that the base material layer was not formed.
[0147] Example 10 A sealing sheet according to Example 10 was obtained in the same manner as in Example 9, except that the modulus of elasticity of the release liner was set to 3600 MPa.
[0148] Example 11 A sealing sheet according to Example 11 was obtained in the same manner as in Example 9, except that the modulus of elasticity of the release liner was set to 4200 MPa.
[0149] Example 12 A sealing sheet according to Example 12 was obtained in the same manner as in Example 9, except that the thickness tolerance of the sheet material layer was set to 25%.
[0150] Example 13 A sealing sheet according to Example 13 was obtained in the same manner as in Example 9, except that the tolerance of the thickness of the sheet material layer was set to 40%.
[0151] Comparative Example 1 A sealing sheet according to Comparative Example 1 was obtained in the same manner as in Example 4, except that the sealing composition according to Comparative Example 1 was used instead of the sealing composition according to Example 4.
[0152] Comparative Example 2 A sealing sheet according to Comparative Example 2 was obtained in the same manner as in Example 4, except that the sealing composition according to Comparative Example 2 was used instead of the sealing composition according to Example 4.
[0153] Comparative Example 3 A sealing material layer (EPDM layer) was formed on the exposed surface (the surface without the release liner) of a substrate layer (a urethane film with a release liner (Tough Grace TG88-I 25 / 50, manufactured by Takeda Sangyo Kaisha; the urethane film was 25 μm thick and the release liner (made of polyethylene) was 50 μm thick) using ethylene propylene diene rubber (EPDM, manufactured by Mitsui Chemicals, Inc.) instead of the sealing material composition of Example 2. The sealing material layer was formed by coating the ethylene propylene diene rubber to a thickness of 0.5 mm using calendar rolls (four 8-inch rolls) while heating it to 140°C. Next, a pressure-sensitive adhesive layer was formed on the sealing material layer in the same manner as in Example 1, to obtain a laminate in which the release liner, sealing material layer, and pressure-sensitive adhesive layer were laminated in this order. The release liner was then peeled off from the laminate to obtain a sealing sheet of Comparative Example 3.
[0154]
[0155] [Probe Tack Value] The probe tack value T was measured for the sealing material layer of the sealing sheet according to each example except for Comparative Example 3 according to the method described in the above embodiment. The results are shown in Tables 2 to 5 below.
[0156] [Storage Modulus] For the sealing material layer of the sealing sheet according to each example other than Comparative Example 3, the storage modulus G' at -20°C was measured according to the method described in the above embodiment. 1 and the storage modulus G' at 23°C 2 The results are shown in Table 2 below. 1 The ratio of T to G' 1 ) are also shown in the following Table 2. Furthermore, for the sealing sheets provided with the pressure-sensitive adhesive layer (Examples 1 to 3 and 7), the G' 2 The ratios are also shown in the following Tables 2 to 5. The storage modulus of the pressure-sensitive adhesive layer at 23° C. was measured in the same manner as for the sealing material layer.
[0157] [Adhesion] For the sealing material layer of the sealing sheet according to each example except Comparative Example 3, the adhesion to the test tire was measured according to the method described in the above embodiment. The adhesion of the sealing material layer was measured as a value (A2) at -20°C and a value (A1) at 23°C. For the sealing sheets provided with an adhesive layer (Examples 1 to 3 and 7), the adhesion of the adhesive layer to the tubeless tire was also measured. The adhesion of the adhesive layer was also measured as a value (A2') at -20°C and a value (A1') at 23°C. The results are shown in Tables 2 to 5 below.
[0158] [Evaluation of Sealing Property] Using the sealing sheet according to each example, the sealing property was evaluated when a through-hole was formed in a pneumatic tire. The sealing property evaluation was performed according to the following procedure. The sealing property evaluation was performed in an environment at a temperature of 23°C. (1) The sealing sheet according to each example was cut into a piece of sealing sheet with planar dimensions of 30 mm x 50 mm to obtain a small piece of sealing sheet, and then the small piece of sealing sheet was attached to the inside of the test tire. If the small piece of sealing sheet had an adhesive layer, the small piece of sealing sheet was attached to the inside of the test tire via the adhesive layer. If the small piece of sealing sheet did not have an adhesive layer, the small piece of sealing sheet was attached to the inside of the test tire via a sealing material layer. (2) The test tire with the small piece of sealing sheet attached to the inside was mounted on a wheel (manufactured by Shimano, product name "WH-RS500", rim profile: width 20.8 mm, height 24 mm). The test tire is mounted on the wheel without injecting a sealant into the inside of the test tire. (3) After injecting air into the inside of the test tire to a specified pressure (95 psi (approximately 0.66 MPa)), the pressure change is observed over a certain period of time (approximately one day), and the leak rate V of the reference tire (Ref) is calculated. 1(psi / min) is calculated. In other words, the leak rate when no through-hole is formed in the test tire is calculated. The pressure is measured by attaching a pressure gauge (manufactured by TOPEAK, product name "Shuttle Gauge Digital APG01000") to a valve provided on the wheel. The pressure measurement is performed with the test tire and the wheel unit stationary. The following pressure measurements are also performed in the same manner as above. (4) After again inflating the inside of the test tire mounted on the wheel to the specified pressure (95 psi (approximately 0.66 MPa)), a round nail with a diameter of 2.1 mm (φ2.1 mm) is thrust to a depth of 20 mm into the location of the small piece where the sheet sticker is affixed. The round nail is then pulled out of the test tire, forming a through-hole in the test tire. (5) The time when the through hole was formed (i.e., when the round nail was pulled out) was set as the observation starting point (0 min), and the pressure change was observed over a certain period of time (about 5 minutes), and the leak rate V after the through hole was formed was calculated. 2 (psi / min). Next, the leak rate V 2 and leak rate V 1 The difference between 2 -V 1 ) is calculated, and the calculated value (relative velocity) is used as the leak velocity V 3 That is, the leak rate V 3 The closer to 0 the value is, the more effective the sealing effect of the sealing sheet is. Taking the above into consideration, the sealing performance was evaluated according to the following criteria: Excellent: 0≦V 3 ≦0.50 Good: 0.50<V 3 ≦3.0 Impossible: 3.0<V 3 Leak rate V 3 The values and the evaluation results of the sealing properties are shown in Tables 2 to 5 below.
[0159] [Evaluation of Adhesion to R Surface] Using the seal sheet of each example, the adhesion to the R surface (curved surface) of a tire was evaluated. (Evaluation Procedure) A test sample with planar dimensions of 35 mm x 100 mm was cut out from the seal sheet of each example, and the test sample was attached to the inner surface of the test tire by applying a load of 5 kg three times. When evaluating a seal sheet without a base layer, the load was applied to the seal material layer (located between the release liner and the test tire) via a release liner. On the other hand, when evaluating a seal sheet with a base layer, the load was applied to the seal material layer (located between the base layer and the tire) via the base layer. (Evaluation Criteria) Evaluation was performed according to the following evaluation criteria. Good (◯): The area ratio that has peeled off and lifted from the R surface is less than 50%. Slightly poor (Δ): The area ratio that has lifted off from the R surface is less than 50%, but one region in one direction of the surface direction of the test sample has peeled off and lifted. Poor (×): The area ratio that has peeled off and lifted from the R surface is 50% or more.
[0160] [Evaluation of the amount of sealant overflow] The amount of sealant (glue) overflow was evaluated using the seal sheet according to each example. (Evaluation procedure) A square test sample with planar dimensions of 1 cm x 1 cm was cut out from the seal sheet according to each example. The test sample was sandwiched between two release liners and then further sandwiched between SUS304 plates with a thickness of 3 mm. A load of 200 g was applied to both sides of the two SUS304 plates, and the plates were left standing in this state in an environment of 50°C for 3 days. After leaving the plates standing, the overflow length of the part of the sealant that overflowed the most from the original dimensions (1 cm x 1 cm) was measured. (Evaluation criteria) If the overflow length was less than 1 mm, the seal sheet was evaluated as one in which sealant overflow was suppressed.
[0161] [Evaluation of Roll Shape Retention] The roll shape retention was evaluated using the sealing sheet according to each example. (Measurement of Thickness Tolerance / Average Thickness) A first measurement point was selected in the longitudinal direction of the sealing sheet according to each example. The thickness was measured in 5 mm increments from one end of the width including the first measurement point to the other end. Next, the thickness was measured in 5 mm increments from one end of the width including a second measurement point 30 cm away from the first measurement point in the longitudinal direction to the other end. Using all the thickness measurements, the average, maximum, and minimum values were calculated. The calculated average value was taken as the "average thickness" (mm) of the sealing sheet, and the difference between the maximum and minimum values was taken as the "thickness tolerance" (mm). A 1 / 100 dial gauge was used to measure the thickness. (Evaluation Criteria) Based on the amount of overflow obtained in the evaluation of the amount of overflow of the sealing material described above and the value calculated using the formula (thickness tolerance / average thickness), the roll shape retention was evaluated according to the following evaluation criteria. Good (○): Protrusion amount is less than 2 mm, and (thickness tolerance / average thickness) is less than 0.20. Slightly poor (△): Protrusion amount is less than 2 mm, and (thickness tolerance / average thickness) is 0.20 or more but less than 0.35. Poor (×): Protrusion amount is 2 mm or more, or (thickness tolerance / average thickness) is 0.35 or more.
[0162] The thickness and mass of the base material layer, the thickness and mass of the sealing material layer, the thickness and mass of the sealing material layer, the thickness and mass of the adhesive layer, and the total mass of the sealing sheet are also shown in Tables 2 to 5. In the sealing sheet according to Example 8, the sealing material layer was configured by laminating two layers (first and second layers) with different compositions, so in the column for Example 8 in Table 3 below, the thickness and mass of each layer are listed, and the combined thickness and mass of the two layers are also shown.
[0163]
[0164]
[0165]
[0166]
[0167] From Tables 2 to 5, when the sealing sheet prepared using the sealing material composition according to each example was used, the leak rate V3 is a relatively small value, and it can be seen that the evaluation of the sealing property is good (excellent or fair). In addition, when the sealing sheets according to Examples 1 to 5 and 8 to 13 were used, the leak rate V 3 In contrast, when the sealing sheets according to the comparative examples were used, the leak rate V 3 It can be seen that as the value of increases, the evaluation of the sealing property worsens (fail). Regarding the adhesion to the R surface of Example 11, the high tensile modulus of elasticity of the release liner made the workability during adhesion poor, and it was evaluated as poor (×), but the adhesion of the sealing material layer itself was similar to that of Example 4.
[0168] REFERENCE SIGNS LIST 1 sealant layer 2 substrate layer 3 adhesive layer 10 seal sheet for pneumatic tire
Claims
1. A sealant layer is provided, and the value of the storage modulus of the sealant layer at -20°C is G' 1 where T is the probe tack value of the sealing material layer at 23° C., and A1 is the value of the adhesive strength of the sealing material layer to a tire at 23° C., and 1 The ratio of the product of the probe tack value T and the adhesive strength value A1 (A1×T / G′ 1 ) is 12.0 or less.
2. The storage modulus value G' 1 The sealing sheet for a pneumatic tire according to claim 1 , wherein the compressive strength is 0.50 MPa or more.
3. The sealing sheet for pneumatic tires according to claim 1 or 2, wherein the probe tack value T is 0.05 MPa or more.
4. The sealing sheet for a pneumatic tire according to claim 1 or 2, wherein the sealing material layer contains a thermoplastic elastomer as an organic component.
5. The sealing sheet for pneumatic tires according to claim 4, wherein the thermoplastic elastomer is a styrene-based thermoplastic elastomer.
6. The sealing sheet for pneumatic tires according to claim 5, wherein the styrene-based thermoplastic elastomer has a diblock ratio of 10% or more and 80% or less.
7. The sealing sheet for pneumatic tires according to claim 1 or 2, wherein the adhesive strength value A1 is 1.0 N / 20 mm or more.
8. The sealing sheet for pneumatic tires according to claim 1 or 2, wherein when the adhesive strength value A2 of the sealing material layer to the tire at -20°C is 1.0 N / 20 mm or more.
9. The sealing sheet for a pneumatic tire according to claim 1 or 2, wherein the tire is a tubeless tire or a tubeless ready tire.
10. The sealing sheet for a pneumatic tire according to claim 1 or 2, further comprising a base layer laminated on one surface of the sealing material layer or disposed inside the sealing material layer.
11. The sealing sheet for pneumatic tires according to claim 1 or 2, wherein the sealing material layer is constructed by laminating two or more layers having different compositions.
12. The sealing sheet for a pneumatic tire according to claim 10, wherein the base layer is made of a sheet material selected from the group consisting of a fiber sheet, a foamed sheet, a solid sheet, and a multi-layer sheet formed by laminating at least two of these.
13. The mass per unit area is 1500 g / m 2 The sealing sheet for a pneumatic tire according to claim 10, wherein:
14. The sealing sheet for a pneumatic tire according to claim 10, which is configured in a tape shape and has a width that is 10% or more of the width of the pneumatic tire as indicated by the ETRTO standard.
15. The sealing sheet for a pneumatic tire according to claim 14, further comprising a release liner laminated on said sealing material layer, said release liner being laminated on the side of said sealing material layer opposite to the side adhesively bonded to said tire.
16. The sealing sheet for a pneumatic tire according to claim 15, wherein the release liner has a tensile modulus of elasticity at 23°C of 4000 MPa or less.
17. The sealing sheet for pneumatic tires according to claim 15, which is in the form of a roll wound with the release liner disposed on the outside, and the tolerance of the thickness of the sealing material layer, based on the average thickness of the sealing material layer, is 25% or less of the average thickness.
18. The sealing sheet for a pneumatic tire according to claim 17, wherein both side edge portions of the release liner are dry edges where the sealing material layer is not laminated.
19. The sealing sheet for a pneumatic tire according to claim 18, wherein the width of each dry edge portion is 1 mm or more.
Citation Information
Patent Citations
Tubeless tire compound and a system and method for retrofitting non-tubeless tires
US20030136490A1
Tire safety upgrading new material and manufacturing method thereof
CN112280233A
Pneumatic article equipped with self-sealing composition
JP2011502856A
Self-sealing elastomer composition
JP2011525435A
Tires with a built-in self-sealing layer
JP2012533669A