Secondary battery and electronic apparatus
By setting grooves on the surface of the negative electrode sheet of the lithium-ion battery and controlling its parameters, combining to increase the polymer content of the bonding layer and the heat-resistant material layer of the separator, the deformation and heat accumulation problems of the lithium-ion battery during the circulation process are solved. , improves the cycle stability and safety of the battery.
Patent Information
- Application Number
- PCT/CN2023/085089
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-28
AI Technical Summary
Lithium-ion batteries will experience deformation and heat accumulation during repeated charge and discharge cycles, resulting in cycle stability and safety issues.
By setting grooves on the surface of the negative electrode sheet, adjusting the width, spacing and thickness of the electrode assembly, adjusting the contact area and adhesion between the negative electrode sheet and the separator, increasing the polymer content of the adhesive layer, and in A heat-resistant material layer is provided on the separator to improve the stability of the negative electrode sheet and the cycle stability and safety of the lithium-ion battery.
It effectively reduces the risk of cycling attenuation and thermal runaway of lithium-ion batteries, and improves the charging speed and safety performance of the battery.
Smart Images

Figure CN2023085089_28112024_PF_FP_ABST
Abstract
Description
Secondary battery and electronic device Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electronic device. Background Art
[0002] Secondary batteries, such as lithium-ion batteries, have a wide range of applications in consumer electronics due to their high specific energy, high operating voltage, low self-discharge rate, compact size, and light weight. With the widespread use of lithium-ion batteries, the market has placed increasingly higher demands on their performance.
[0003] During repeated charge and discharge cycles, lithium-ion batteries accumulate internal stress, causing deformation. This can lead to problems such as excessive thickness and accelerated cycle decay, impacting the battery's cycling stability. Furthermore, as heat accumulates within the battery during cycling, if this heat cannot be dissipated promptly, it increases the risk of thermal runaway, impacting the battery's safety.
[0004] Summary of the Invention
[0005] The purpose of this application is to provide a secondary battery and an electronic device to improve the cycle stability and safety of lithium-ion batteries.
[0006] It should be noted that in the application content, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solutions are as follows:
[0007] In a first aspect, the present application provides a secondary battery comprising an electrode assembly, the electrode assembly comprising a positive electrode sheet, a negative electrode sheet, and a separator, the separator being disposed between the positive electrode sheet and the negative electrode sheet, the negative electrode sheet comprising a negative current collector and a negative active material layer, wherein the surface of the negative active material layer opposite the positive electrode sheet comprises a groove, the groove having a width of W mm and a spacing of S mm between the grooves; and the thickness of the electrode assembly being T1 mm, satisfying the following: W ≥ S × T1 / 1000. The present application meets the scope of the present application by regulating the groove width, the groove spacing, and the thickness of the electrode assembly. The present application can adjust the contact area between the surface of the negative electrode sheet and the separator according to lithium-ion batteries of different thicknesses, thereby adjusting the bonding interface between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, alleviating deformation problems of the lithium-ion battery, and improving the cycle stability and safety of the lithium-ion battery.
[0008] In some embodiments of the present application, W≤2×S×T1. By adjusting the groove width, groove spacing, and electrode assembly thickness to meet the scope of the present application, the present application can adjust the bonding interface between the negative electrode plate and the separator, improve the deformation of the plate in the XY direction, and improve the stability of the negative electrode plate, thereby improving the deformation problem of the lithium-ion battery and improving the cycle stability and safety of the lithium-ion battery.
[0009] In some embodiments of the present application, S×T1 / 400≤W≤S×T1 / 2. By adjusting the groove width, groove spacing, and electrode assembly thickness to meet the requirements of the present application, the present application can increase the effective bonding area between the grooves on the surface of the negative electrode plate and the separator, thereby increasing the bonding force between the negative electrode plate and the separator, improving the stability of the negative electrode plate, alleviating deformation issues of the lithium-ion battery, and improving the cycling stability and safety of the lithium-ion battery.
[0010] In some embodiments of the present application, 0.05 ≤ S ≤ 10, and 0.02 ≤ W ≤ 0.5. By regulating the groove width and groove spacing within the above ranges, the present application can increase the contact area between the first adhesive layer in the separator and the grooves on the surface of the negative electrode active material layer, thereby increasing the bonding force between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, alleviating the deformation problem of the lithium-ion battery, and improving the cycling stability and safety of the lithium-ion battery.
[0011] In some embodiments of the present application, the OI value of the negative electrode sheet and S satisfy: S / OI≤0.5; in one embodiment, 0.0025≤S / OI≤0.2; in one embodiment, 0.005≤S / OI≤0.03. 004 / C 110 , C 004 is the peak area obtained from the (004) plane diffraction line pattern in the X-ray diffraction spectrum, C 110 is the peak area obtained from the (110) plane diffraction line pattern in the X-ray diffraction pattern.
[0012] While increasing the bonding force between the negative electrode plate and the separator, it reduces the expansion and deformation of the plate in the XY direction, effectively reducing the side reactions of the lithium-ion battery under high-rate charging conditions, and can also improve the polarization degree of the lithium-ion battery during the charging process, thereby increasing the charging speed of the lithium-ion battery.
[0013] In some embodiments of the present application, a bonding layer is provided on the surface of the separator facing the negative electrode sheet, and the bonding layer includes a polymer; wherein, based on the mass of the bonding layer, the content of the polymer is 30% to 100%. Through the synergistic effect of the above structural design and material selection, the bonding force between the negative electrode sheet and the separator can be increased, the stability of the negative electrode sheet can be improved, the deformation problem of the lithium-ion battery can be improved, and the cycle stability and safety of the lithium-ion battery can be improved.
[0014] In some embodiments of the present application, the thickness of the bonding layer is T2 μm, and the depth of the groove is H μm, satisfying: H ≤ T2 + 20, which can increase the contact area between the bonding layer in the separator and the groove on the surface of the negative electrode active material layer, thereby increasing the bonding force between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, improving the deformation problem of the lithium-ion battery, and improving the cycle stability and safety of the lithium-ion battery.
[0015] In some embodiments of the present application, the cross-sectional area of the groove is A μm 2 , satisfying: 0.3×(W×H) < A < 0.95×(W×H), 2 ≤ H ≤ 50; in one embodiment, 0.35×(W×H) < A < 0.8×(W×H). By regulating the relationship between A, W and H to satisfy the above relationship, and synergistically regulating H within the above range, the bonding area between the surface of the negative electrode sheet and the separator can be effectively increased, especially the bonding area between the side of the groove and the separator, thereby increasing the bonding force between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, improving the deformation problem of the lithium-ion battery, and improving the cycle stability and safety of the lithium-ion battery.
[0016] In some embodiments of the present application, the polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, styrene-butadiene copolymer, polyacrylonitrile, butadiene-acrylonitrile polymer, polyacrylic acid, polyacrylate or acrylate-styrene copolymer. By regulating the separator to contain the above polymer in the present application, it is beneficial to improve the interfacial bonding force and heat resistance of the separator.
[0017] In some embodiments of the present application, along the width direction of the negative electrode sheet, the groove forms a structure penetrating the negative electrode sheet, wherein the groove includes a first section with a width of W1 and a second section with a width of W2, satisfying 1.2 < W1 / W2 < 1.8. By the above structure and regulating the relationship between the widths of the first section and the second section within the above range, the contact area between the surface of the negative electrode sheet and the separator can be effectively increased, thereby increasing the bonding force between the negative electrode sheet and the separator.
[0018] In some embodiments of the present application, the grooves are formed along the width of the negative electrode sheet without penetrating the entire sheet. This structure improves the localized bonding between the negative electrode sheet and the separator, facilitates stress release of the negative electrode active material during cycling, and further improves the cycling performance and cyclic expansion of the secondary battery. It also reduces the difficulty of preparing the grooves, thereby reducing production costs.
[0019] In a second aspect, the present application provides an electronic device comprising the secondary battery described in the aforementioned embodiment, thereby providing the electronic device with good cycle stability and safety.
[0020] The present application provides a secondary battery and an electronic device, wherein, when observed in the thickness direction of the negative electrode sheet, the surface of the negative electrode active material layer of the negative electrode sheet has grooves. The present application meets the scope of the present application by regulating the width of the grooves, the spacing between the grooves and the thickness of the electrode assembly. The contact area between the surface of the negative electrode sheet and the separator can be adjusted according to lithium-ion batteries of different thicknesses, thereby increasing the bonding force between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, improving the deformation problem of the lithium-ion battery, and improving the cycle stability and safety of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings described herein are used to provide further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0022] FIG1 is a schematic structural diagram of an electrode assembly in some embodiments of the present application;
[0023] FIG2 is a schematic diagram of the cross-sectional structure of an electrode assembly along its thickness direction in some embodiments of the present application;
[0024] FIG3 is a schematic diagram of the cross-sectional structure of a negative electrode sheet along its thickness direction in some embodiments of the present application;
[0025] FIG4 is a top view of a negative electrode sheet along its thickness direction in some embodiments of the present application;
[0026] FIG5 is a schematic diagram of a cross-sectional structure of a diaphragm along its thickness direction in some embodiments of the present application;
[0027] FIG6 is a schematic structural diagram of a diaphragm according to some other embodiments of the present application viewed along its thickness direction;
[0028] FIG7 is a schematic diagram of the structure of a groove in a negative electrode plate in some embodiments of the present application;
[0029] FIG8 is a schematic diagram of the structure of the groove in the negative electrode sheet in some other embodiments of the present application;
[0030] FIG9 is a schematic diagram of the structure of the groove in the negative electrode plate in some further embodiments of the present application.
[0031] Figure numerals: 10-electrode assembly, 20-positive electrode sheet, 21-positive electrode current collector, 22-positive electrode active material layer, 30-negative electrode sheet, 31-negative electrode current collector, 32-negative electrode active material layer, 40-separator, 41-substrate layer, 42-heat-resistant material layer, 321-groove, 431-bonding layer, 3211-first section, 3212-second section, 3213-third section. DETAILED DESCRIPTION
[0032] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described below with reference to the accompanying drawings and examples. It is clear that the described embodiments are only a portion of the embodiments of this application, not all of them. All other embodiments obtained by those skilled in the art based on the embodiments in this application without creative effort are within the scope of protection of this application.
[0033] It should be noted that in the specific implementation, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solution is as follows:
[0034] In a first aspect, the present application provides a secondary battery, as shown in FIG1 , comprising an electrode assembly 10. The X direction is the length of the electrode assembly 10, the Y direction is the width of the electrode assembly 10, and the Z direction is the thickness of the electrode assembly 10. As shown in FIG2 , the electrode assembly 10 comprises a positive electrode sheet 20, a negative electrode sheet 30, and a separator 40. The separator 40 is disposed between the positive electrode sheet 20 and the negative electrode sheet 30. The positive electrode sheet 20 comprises a positive current collector 21 and a positive active material layer 22. The negative electrode sheet 30 comprises a negative current collector 31 and a negative active material layer 32. The surface of the negative active material layer 32 opposite the positive electrode sheet 20 comprises a groove 321. As shown in FIG3 and FIG4 , the width of the groove 321 is W mm, and the spacing between the grooves 321 is S mm. As shown in FIG1 , the thickness of the electrode assembly 10 is T1 mm, satisfying the following: W ≥ S × T1 / 1000. In this application, the width of the groove refers to the width of the groove at the surface of the negative electrode plate; the spacing of the grooves refers to the distance between two adjacent grooves. In this application, the negative electrode active material layer 32 can be provided on one side or on both sides.
[0035] The present application meets the scope of the present application by regulating the width of the grooves, the spacing between the grooves and the thickness of the electrode assembly. It can adjust the contact area between the surface of the negative electrode plate and the diaphragm according to lithium-ion batteries of different thicknesses, thereby increasing the bonding force between the negative electrode plate and the diaphragm, improving the stability of the negative electrode plate, improving the deformation problem of the lithium-ion battery, and improving the cycle stability and safety of the lithium-ion battery.
[0036] In some embodiments of the present application, W≤2×S×T1. By regulating the groove width, groove spacing, and electrode assembly thickness to meet the scope of the present application, the present application can effectively increase the bonding area between the grooves on the surface of the negative electrode plate and the separator, thereby increasing the bonding force between the negative electrode plate and the separator, improving the stability of the negative electrode plate, improving the deformation problem of the lithium-ion battery, and improving the cycle stability and safety of the lithium-ion battery.
[0037] In some embodiments of the present application, S×T1 / 400≤W≤S×T1 / 2. By adjusting the groove width, groove spacing, and electrode assembly thickness to meet the requirements of the present application, the present application can effectively increase the bonding area between the grooves on the surface of the negative electrode sheet and the separator, thereby increasing the bonding force between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, alleviating deformation issues of the lithium-ion battery, and improving the cycling stability and safety of the lithium-ion battery.
[0038] In some embodiments of the present application, 0.05 ≤ S ≤ 10, and 0.02 ≤ W ≤ 0.5. Without being limited by any theory, by regulating the groove width and groove spacing within the above ranges, the present application can increase the contact area between the first bonding layer in the separator and the grooves on the surface of the negative electrode active material layer, thereby increasing the bonding force between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, alleviating the deformation problem of the lithium-ion battery, and improving the cycling stability and safety of the lithium-ion battery.
[0039] In some embodiments of the present application, the OI value of the negative electrode sheet and S satisfy: S / OI≤0.5; in one embodiment, 0.0025≤S / OI≤0.2; in one embodiment, 0.005≤S / OI≤0.03. 004 / C 110 , C 004 is the peak area obtained from the (004) plane diffraction line pattern in the X-ray diffraction spectrum, C 110 is the peak area obtained from the (110) plane diffraction line pattern in the X-ray diffraction pattern.
[0040] The inventors have discovered that as the OI value increases, the lithium ion transport tortuosity of the graphite in the negative electrode active material increases, leading to increased polarization during the charging process of the lithium-ion battery. At the same time, when the OI value is low, the battery tends to deform in the XY directions. Without being limited to any theory, the present invention regulates the groove spacing and the OI value of the negative electrode plate within the above ranges. This increases the adhesion between the negative electrode plate and the separator while reducing the XY expansion deformation of the plate. This effectively reduces the side reactions of the lithium-ion battery under high-rate charging conditions and improves the polarization degree of the lithium-ion battery during charging, thereby increasing the charging speed of the lithium-ion battery.
[0041] In some embodiments of the present application, a bonding layer is provided on the surface of the separator opposite to the negative electrode plate, and the bonding layer includes a polymer; wherein the content of the polymer is 30% to 100% based on the mass of the bonding layer.
[0042] For example, in some embodiments of the present application, as shown in FIG5 , the separator 40 includes a substrate layer 41 and an adhesive layer 431 disposed on the surface of the substrate layer 41 , wherein the adhesive layer 431 includes a polymer and a heat-resistant material. Through the synergistic effect of the above-mentioned structural design and material selection, it is possible to increase the bonding force between the negative electrode sheet and the separator, improve the stability of the negative electrode sheet, improve the deformation problem of the lithium-ion battery, and improve the cycle stability and safety of the lithium-ion battery. In addition, only one coating process is required to obtain an adhesive layer containing both a polymer and a heat-resistant material, which simplifies the process steps and helps reduce production costs. Based on the mass of the adhesive layer, the content of the polymer is 30% to 80%, and the content of the heat-resistant material is 20% to 70%.
[0043] For example, in other embodiments of the present application, as shown in FIG6 , a separator 40 includes a substrate layer 41, with a heat-resistant material layer 42 and an adhesive layer 431 sequentially disposed on the surface of the substrate layer 41. The heat-resistant material layer 42 includes a heat-resistant material, and based on the mass of the adhesive layer, the polymer content is 100%. Through the synergistic effect of the above structural design and material selection, the bonding force between the negative electrode plate and the separator can be increased, the stability of the negative electrode plate can be improved, the deformation problem of the lithium-ion battery can be improved, and the cycling stability and safety of the lithium-ion battery can be improved.
[0044] The present application does not particularly limit the heat-resistant material of the heat-resistant material layer, as long as it can achieve the purpose of this application. For example, the heat-resistant material can include at least one of a ceramic material or a heat-resistant polymer material. The ceramic material can include at least one of Al2O3, boehmite, SiO2, TiO2, MgO, ZnO, ZrO2, or SnO2; the heat-resistant polymer material can include at least one of polyimide and its derivatives, aromatic nylon and its improved products, phenolic resin, or polytetrafluoroethylene.
[0045] In some embodiments of the present application, as shown in FIG. 3, the depth of the groove 321 is H μm, and as shown in FIG. 5, the thickness of the first adhesive layer 431 is T2 μm, satisfying: H ≤ T2 + 20. By controlling the relationship between H and T2 to meet the above conditions, the contact area between the first adhesive layer in the separator and the groove on the surface of the negative electrode active material layer can be increased, thereby increasing the adhesion between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, improving the deformation problem of the lithium-ion battery, and enhancing the cycle stability and safety of the lithium-ion battery.
[0046] In some embodiments of the present application, as shown in FIG. 3, the depth of the groove 321 is H μm, and as shown in FIG. 6, the thickness of the adhesive layer 431 is T2 μm, satisfying: H ≤ T2 + 20. Preferably, H ≤ T2 + 15. By controlling the relationship between H and T2 to meet the above conditions, the contact area between the adhesive layer in the separator and the groove on the surface of the negative electrode active material layer can be increased, thereby increasing the adhesion between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, improving the deformation problem of the lithium-ion battery, and enhancing the cycle stability and safety of the lithium-ion battery.
[0047] In some embodiments of the present application, as shown in FIG. 3, the cross-sectional area of the groove 321 is A μm 2 , satisfying: 0.3×(W×H) < A < 0.95×(W×H), 2 ≤ H ≤ 50; in one embodiment, 0.35×(W×H) < A < 0.8×(W×H). In the present application, the cross-sectional area of the groove refers to the area of the cross-section formed by the groove in the cross-section of the negative electrode sheet along its own thickness direction. By controlling the relationship between A, W, and H to meet the above conditions and coordinately controlling H within the above range, the bonding area between the surface of the negative electrode sheet and the separator can be effectively increased, especially the bonding area between the side of the groove and the separator, thereby increasing the adhesion between the negative electrode sheet and the separator, improving the stability of the negative electrode sheet, improving the deformation problem of the lithium-ion battery, and enhancing the cycle stability and safety of the lithium-ion battery.
[0048] In some embodiments of the present application, the polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride - hexafluoropropylene copolymer, styrene - butadiene copolymer, polyacrylonitrile, butadiene - acrylonitrile polymer, polyacrylic acid, polyacrylate, or acrylate - styrene copolymer, which is beneficial to improving the interfacial adhesion of the separator.
[0049] In some embodiments of the present application, as shown in FIG. 7, along the width direction of the negative electrode tab 30, the groove 321 forms a structure that penetrates the negative electrode tab. The groove 321 includes a first segment 3211 with a width of W1 and a second segment 3212 with a width of W2, satisfying 1.2 < W1 / W2 < 1.8. As can be seen from FIG. 7, the groove 321 that penetrates through is composed of a first segment 3211, a second segment 3212, and a third segment 3213. By the above structure and regulating the relationship between the widths of the first segment and the second segment within the above range, the contact area between the surface of the negative electrode tab and the separator can be effectively increased, thereby increasing the adhesion between the negative electrode tab and the separator.
[0050] In some embodiments of the present application, as shown in FIG. 8, along the width direction of the negative electrode tab 30, the groove 321 forms a structure that does not penetrate the negative electrode tab. As can be seen from FIG. 8, the groove 321 has a first segment 3211, a second segment 3212, and a third segment 3213. Among them, the first segment 3211, the second segment 3212, and the third segment 3213 do not overlap, and the third segment 3213 is located between the first segment 3211 and the second segment 3212. The first segment 3211, the second segment 3212, and the third segment 3213 can be arranged in parallel, thereby forming the groove 321 that is not penetrated. Among them, when observing along the length direction of the tab, there is a first overlapping region between the first segment 3211 and the second segment 3212, and there is a second overlapping region between the second segment 3212 and the third segment 3213. Among them, in the width direction of the tab, the lengths of the first overlapping region and the second region are less than 30% of the width of the tab. Through the above structure, the local adhesion performance between the negative electrode tab and the separator can be improved, and at the same time, it is beneficial to the stress release of the negative electrode active material during the cycling process, thereby further improving the cycling performance and cycling expansion of the secondary battery, and it is also beneficial to reducing the process difficulty when preparing the groove, thereby reducing the production cost.
[0051] In some embodiments of the present application, as shown in FIG9 , along the width direction of the negative electrode plate 30, the groove 321 forms a structure that does not penetrate the negative electrode plate. As can be seen from FIG9 , the groove 321 has a first section 3211 and a second section 3212, wherein the first section 3211 and the second section 3212 do not overlap, and the first section 3211 and the second section 3212 can be arranged in parallel, thereby forming a groove 321 that is not arranged through. Among them, when observed along the length direction of the plate, there is a first overlapping area between the first section 3211 and the second section 3212, wherein in the width direction of the plate, the length of the first overlapping area is less than 30% of the width of the plate. Through the above structure, the local bonding performance between the negative electrode plate and the diaphragm can be improved, and at the same time, it is beneficial to release the stress of the negative electrode active material during the cycle, thereby achieving further improvement in the cycle performance and cycle expansion of the secondary battery, and it is also beneficial to reduce the process difficulty when preparing the groove, thereby reducing production costs.
[0052] It is understood that the electrode assembly of the present application can be a wound structure, and its electrode sheet generally has a long side and a short side after being unfolded. In one embodiment of the present application, the electrode assembly is a wound structure, and the width direction is the direction in which the short side of the electrode sheet extends after being unfolded, and the length direction is the direction in which the long side of the electrode sheet extends after being unfolded. The electrode sheet of the present application includes a positive electrode sheet 20 and a negative electrode sheet 30.
[0053] The secondary battery of the present application may include any device that undergoes an electrochemical reaction, as long as it can achieve the purpose of the present application. For example, the secondary battery may include but is not limited to: lithium-ion secondary battery (lithium-ion battery), sodium-ion secondary battery, lithium polymer secondary battery or lithium-ion polymer secondary battery, etc. The battery structure of the present application includes but is not limited to soft-pack battery, square hard-shell battery or cylindrical hard-shell battery, etc.
[0054] The present application has no special restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a composite current collector, etc. The present application has no special restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 10μm. In the present application, the negative electrode active material layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of the negative electrode current collector or a partial area of the negative electrode current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved.
[0055] The present application does not particularly limit the type of negative electrode active material, as long as the purpose of the present application can be achieved. For example, the negative electrode active material may include graphite, a mixture of graphite and silicon materials such as silicon, silicon oxide or silicon carbide, and the above-mentioned graphite may be selected from artificial graphite or natural graphite. Optionally, the negative electrode active material layer also includes at least one of a conductive agent, a thickener, and a binder. The present application does not particularly limit the types of conductive agents, thickeners and binders in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the negative electrode binder may include but is not limited to at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoride, polyethylene, polypropylene, polyacrylic acid, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin or nylon. The present application does not particularly limit the mass ratio of the negative electrode active material, conductive agent, thickener, and binder in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the mass ratio of the negative electrode active material, conductive agent, thickener, and binder in the negative electrode active material layer is (96-98):(0-1.5):(0.5-1.5):(1.0-1.9).
[0056] The present application has no particular limitation on the OI value of the negative electrode sheet, as long as the purpose of the invention can be achieved. For example, the OI value can be 5 to 30.
[0057] The present application does not particularly limit the material of the diaphragm substrate layer, and those skilled in the art can select it according to actual needs, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm substrate layer may include but is not limited to at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film can be used.
[0058] The present application has no particular limitation on the thickness of the first adhesive layer and / or the second adhesive layer in the diaphragm, as long as the purpose of the invention of the present application can be achieved. For example, the thickness of the first adhesive layer and / or the second adhesive layer can be 1 μm to 20 μm.
[0059] The secondary battery of the present application also includes an electrolyte. The present application has no particular restrictions on the electrolyte. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, at least one of ethylene carbonate (also known as ethylene carbonate, abbreviated as EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl propionate (EP), propyl propionate (PP), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), vinylene carbonate (VC) or fluoroethylene carbonate (FEC) is mixed in a certain mass ratio to obtain a non-aqueous organic solvent, and then a lithium salt is added to dissolve and mix evenly. The present application has no particular restrictions on the above-mentioned "mass ratio", as long as the purpose of the present application can be achieved. The present application has no restrictions on the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, lithium bis(oxalatoborate) (LiBOB), or lithium difluoroborate. The present application does not particularly limit the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt is 1.0 mol / L to 2.0 mol / L.
[0060] The positive electrode sheet of the present application may include a positive electrode active material layer and a positive electrode current collector. The present application does not particularly limit the type of positive electrode active material, as long as the objectives of the present application can be achieved. For example, the positive electrode active material may include at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide, or lithium iron manganese phosphate. In the present application, the positive electrode active material may also include non-metallic elements, such as at least one of fluorine, phosphorus, boron, chlorine, silicon, or sulfur, which can further improve the stability of the positive electrode active material. The positive electrode active material layer of the present application may also include a conductive agent and a binder. The present application does not particularly limit the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer. Those skilled in the art may select the ratio according to actual needs, as long as the objectives of the present application can be achieved. For example, the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer is (96-98):(1-3):(2-3).
[0061] The present application has no special restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector, etc. The present application has no special restrictions on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm. In the present application, the positive electrode active material layer can be provided on one surface in the thickness direction of the positive electrode current collector, or on two surfaces in the thickness direction of the positive electrode current collector. It should be noted that the "surface" here can be the entire area of the positive electrode current collector or a partial area of the positive electrode current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved.
[0062] This application does not particularly limit the preparation method of the negative electrode sheet, as long as it can achieve the purpose of this application. For example, the preparation method of the negative electrode sheet includes but is not limited to the following steps: dispersing the negative electrode active material, conductive agent, thickener, and binder in deionized water and mixing to form a uniform negative electrode slurry, coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing, and then forming grooves on the surface of the negative electrode sheet. After cutting and slitting, the negative electrode sheet with the structure shown in Figure 3 is obtained.
[0063] This application does not particularly limit the preparation method of the positive electrode sheet, as long as it can achieve the purpose of this application. For example, the preparation method of the positive electrode sheet includes but is not limited to the following steps: dispersing the active material, conductive agent, and binder in NMP solvent to form a uniform positive electrode slurry, coating the positive electrode slurry on the positive electrode current collector, drying, cold pressing, cutting, and slitting to obtain the positive electrode sheet.
[0064] The present application does not particularly limit the shape of the groove, as long as it can achieve the purpose of this application. For example, when viewed along the length of the negative electrode sheet, the shape of the groove can include at least one of a square, rectangle, trapezoid, triangle, or semicircle; when viewed along the thickness of the negative electrode sheet, the shape of the groove can include at least one of a straight line, an oblique line, a broken line, or a curved line.
[0065] The present application has no particular restrictions on the method for preparing the groove, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to laser etching processing, mechanical processing or pore-forming agent processing. Taking laser etching processing as an example, the width and depth of the groove usually increase with the increase of laser power, and the spacing of the groove can usually be adjusted by the processing rate of the laser. Therefore, technicians can adjust the width, depth, spacing and other parameters of the groove by adjusting parameters such as the laser power, processing rate and the tape speed of the pole piece. In the present application, as shown in Figure 1, the electrode assembly includes a straight area and a bending area. In the preparation process of lithium-ion batteries, technicians can set the groove in the bending area according to design requirements, that is, set the groove in the area where the electrode pole piece in the electrode assembly is bent, thereby improving the interface bonding performance of the negative pole piece in this area, thereby improving the cycle stability and safety of the lithium-ion battery.
[0066] This application does not particularly limit the preparation method of the secondary battery; any preparation method known in the art may be used, as long as the objectives of this application are achieved. For example, the preparation method of the secondary battery includes, but is not limited to, the following steps: stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence, and performing winding and folding operations as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting an electrolyte into the packaging bag and sealing it to obtain the secondary battery.
[0067] In a second aspect, the present application provides an electronic device comprising the secondary battery described in the aforementioned embodiment, thereby providing the electronic device with good cycle stability and safety.
[0068] The present application does not particularly limit the electronic device, and the electronic device may be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, a power tool, a flashlight, a camera, a large household battery or a lithium-ion capacitor, etc.
[0069] Example
[0070] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods.
[0071] Test methods and equipment:
[0072] Adhesion force F test between negative electrode and separator:
[0073] Cut a negative electrode sheet with a separator attached, measuring 15mm x 60mm in width x length. Using double-sided tape measuring 20mm x 100mm in width x length, secure the sample to a steel plate, with the test surface facing downward. Insert one end of a paper tape, the same width as the sample and 150mm longer than the sample, underneath the sample and secure with crepe tape. Secure the steel plate to the bottom of a high-speed rail tensile testing machine. Secure the other end of the paper tape to the machine's fixture and start the machine. Once the tension stabilizes, the tensile force reading represents the bond strength.
[0074] Electrode assembly thickness T1 test:
[0075] In an environment of (25±3)°C, the thickness of the lithium-ion battery is measured with a micrometer and recorded as T0. The lithium-ion battery is then disassembled and the thickness of the disassembled packaging bag is measured and recorded as T3. The thickness of the electrode assembly is T1 = T0-T3.
[0076] Negative electrode OI value test:
[0077] The 004 diffraction line pattern and 110 diffraction line pattern in the X-ray diffraction pattern of the carbon coating in the negative electrode were tested in accordance with the Mechanical Industry Standard of the People's Republic of China JB / T 4220-2011 "Method for Determination of Lattice Parameters of Artificial Graphite". The experimental conditions are as follows: X-rays use CuKα radiation, and CuKα radiation is removed by a filter or a monochromator. The working voltage of the X-ray tube is (30-35) kV, and the working current is (15-20) mA. The scanning speed of the counter is 1 / 4 (°) / min. When recording the 004 diffraction line pattern, the scanning range of the diffraction angle 2θ is 53° to 57°. When recording the 110 diffraction line pattern, the scanning range of the diffraction angle 2θ is 75° to 79°. The c-axis length of the unit cell length obtained from the 004 diffraction line pattern is recorded as C 004 The a-axis length of the unit cell obtained from the 110 diffraction line pattern is recorded as C 110 The OI value is calculated by the following formula: OI value = C 004 / C 110
[0078] Adhesive layer thickness T2 test:
[0079] The portion of the diaphragm in the electrode assembly that is not arranged opposite to the positive electrode active material layer or the negative electrode active material layer is selected, and the diaphragm cross section is prepared by ion beam profiling (CP), and then the bonding layer thickness T2 is measured by scanning electron microscopy (ZEISS Sigma / X-max).
[0080] Measurement of groove depth H, groove width W, groove spacing S, and groove cross-sectional area A:
[0081] A VK-1050 laser confocal microscope was used to image the groove area, acquiring optical and depth information of the pole piece within the microscope's field of view. The pole piece surface was scanned in laser confocal mode at 20x magnification. After scanning, the acquired measurement data was processed in the instrument's associated data analysis software. The reference plane was set using the "Reference Plane Setup" function in the "Process Image" section. The "Smoothing" function was then selected, with a "5×5" size and "Simple Average" type selected to smooth the image. After processing, the groove parameters were measured using the "Profile Measurement" function.
[0082] Groove depth H and groove width W: As shown in Figure 3, the difference between the deepest part of the groove and the reference surface is the groove depth, and the distance between the intersection points of the groove and the reference surface is the groove width. Measurements were taken along the same groove at 10 μm intervals for a total of 20 times. The average of these 20 depth and width values was calculated and recorded as the groove depth H and width W.
[0083] Groove Spacing S: For adjacent grooves (two adjacent grooves are considered adjacent if the overlap is greater than 50% of their respective lengths when viewed along the length of the pole piece), the distance between the midpoints of the groove widths in the perpendicular direction is the groove spacing. Measurements are taken along the selected grooves at intervals of 10 μm for a total of 20 times, and the average value is calculated and recorded as the groove spacing S.
[0084] Groove area A: Use a VK-1050 laser confocal microscope to photograph the groove area and obtain the optical and depth information of the electrode within the field of view of the microscope. At a magnification of 20 times, use the laser confocal mode to scan the surface of the electrode. After scanning, obtain the depth data relative to the baseline at each pixel width. Within the above groove width range, the depth (h i ) is integrated, A=∑ i h i *w0 is the cross-sectional area A of the groove.
[0085] Capacity retention and thickness expansion rate test of lithium-ion batteries:
[0086] At 25°C, the lithium-ion battery was charged at a constant current rate of 0.7C to a voltage of 4.5V, then charged at a constant voltage of 4.5V to a current of 0.05C, and then discharged at a constant current rate of 1C to a voltage of 3.0V. This was considered a charge and discharge cycle process. After repeating 500 charge and discharge cycles, the capacity retention rate and thickness expansion rate of the lithium-ion battery were tested.
[0087] Capacity retention rate of lithium-ion battery after 500 cycles = discharge capacity after 500th cycle / discharge capacity after first cycle × 100%;
[0088] Thickness expansion rate of the lithium-ion battery after 500 cycles = thickness of the lithium-ion battery after the 500th cycle / thickness of the lithium-ion battery at the first cycle × 100%.
[0089] Lithium-ion battery negative electrode cycle interface test:
[0090] After 500 cycles, the lithium-ion battery is charged at a constant current rate of 0.7C at 25°C to a voltage of 4.5V, and then charged at a constant voltage of 4.5V to a current of 0.05C. The battery is then disassembled and the operator observes the cycle interface of the negative electrode plate with the naked eye. If intermittent dot-like purple spots, lithium deposition, or lithium deposition on the purple spots appear on the surface of the negative electrode plate, it is determined that the negative electrode plate has a slight interface problem; if large-area continuous purple spots, lithium deposition, or lithium deposition on the purple spots appear on the main body of the negative electrode plate, it is determined that the negative electrode plate has a serious interface problem.
[0091] Lithium-ion battery hot box pass rate test:
[0092] Place the lithium-ion battery in a sealed temperature-controlled box and charge it at a constant current rate of 0.7C at 25°C to a voltage of 4.5V. Then charge it at a constant voltage of 4.5V to a current of 0.05C. Then, heat the temperature-controlled box at (5±2)°C / min. When the temperature reaches 130°C, keep the temperature constant for 60 minutes. After the temperature-controlled box cools naturally, observe whether the lithium-ion battery catches fire or explodes. If the lithium-ion battery does not catch fire or explode, it passes. 100 lithium-ion batteries are tested for each embodiment or comparative example. The hot box pass rate (%) = number of passed batteries / 100×100%.
[0093] Example 1
[0094] <Preparation of negative electrode sheet>
[0095] Artificial graphite (OI value 14), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 97.5:1:1.5, and deionized water was added to form a slurry with a solid content of 75 wt%. The mixture was then stirred evenly. The slurry was evenly coated on one surface of a 4 μm thick negative electrode current collector copper foil and dried at 85°C to produce a negative electrode sheet with a 50 μm thick negative electrode active material layer. The above steps were then repeated on the other surface of the negative electrode sheet to produce a negative electrode sheet coated with negative electrode active material on both sides. The resulting negative electrode sheet was then cold pressed, and grooves were etched into the surface of the negative electrode active material layer using laser processing. After striping and cutting, the tab welding area was cleaned and the tabs were welded to produce the negative electrode sheet. Parameters such as groove depth H, groove width W, groove spacing S, and groove cross-sectional area A are shown in Table 1.
[0096] <Preparation of positive electrode sheet>
[0097] Lithium cobalt oxide, polyvinylidene fluoride, and conductive agent Super P were mixed in a mass ratio of 96:2:2, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 75wt%, which was then stirred evenly. The slurry was evenly coated on one surface of a 9μm thick positive electrode current collector aluminum foil and dried at 95°C to obtain a positive electrode sheet with a positive electrode active material layer thickness of 60μm. The above steps were then repeated on the other surface of the negative electrode sheet to obtain a positive electrode sheet with positive electrode active material coated on both sides. The obtained positive electrode sheet was then cold pressed, slit, and cut, and the tab welding area was cleaned. The tabs were then welded to obtain the positive electrode sheet.
[0098] <Preparation of Electrolyte>
[0099] Ethylene carbonate, diethyl carbonate, methyl ethyl carbonate and vinylene carbonate are mixed in a mass ratio of 8:85:5:2 to obtain a non-aqueous organic solvent. LiPF6 lithium salt is then mixed with the non-aqueous organic solvent in a mass ratio of 8:92 to obtain an electrolyte.
[0100] <Preparation of Separator>
[0101] <Preparation of Base Material Layer>
[0102] A polypropylene film with a thickness of 5 μm was used.
[0103] <Preparation of Heat-Resistant Material Layer>
[0104] The mass ratio of aluminum oxide ceramic particles, butadiene-styrene polymer, and deionized water was 35:10:55. A total of 30 kg of butadiene-styrene polymer and deionized water were added to a 60-liter dual planetary mixer and dispersed at 45°C for 3 hours. Then, 16.1 kg of aluminum oxide ceramic powder was added to the mixer and dispersed at high speed at 45°C for 2 hours. The mixture was then ball-milled in a nano-grinder for 1.5 hours using 6-μm diameter spherical zirconium oxide beads to obtain a heat-resistant material layer adhesive.
[0105] The substrate was coated by transfer coating, with a coating speed of 6 m / min and a coating amount of 0.18 mg / cm 2 The coating thickness was 1.5 μm. A three-stage drying process was used, with each oven section measuring 3 meters long and set at 50°C, 60°C, and 60°C, to form a substrate layer with a single-sided heat-resistant material layer. The above steps were then repeated on the other side of the substrate layer to form a double-sided heat-resistant material layer.
[0106] <Preparation of Adhesive Layer>
[0107] Core-shell polymer particles are used, with a styrene-acrylate copolymer shell and an acrylate polymer core. The total swelling degree is 450%, and the particle size is 0.45 μm. The polymer adhesive layer is prepared by adding 25 parts by mass of a core-shell polymer emulsion (40% solids content), 40 parts by mass of deionized water, and 35 parts by mass of ethanol. The preparation process involves first adding 50 kg of deionized water and ethanol solvent to a dual planetary mixer and mixing at 25°C for one hour. Then, 16.7 kg of the core-shell polymer emulsion is added and dispersed at 45°C for two hours to obtain the polymer adhesive layer.
[0108] The heat-resistant material layer of the porous substrate was coated on the surface by gravure roller coating to form a double-sided coating structure. The quality and thickness of the coating on both sides were consistent. The coating speed was 6m / min and the coating amount was controlled to 0.036mg / cm 2 The drying is carried out in three stages, each stage is 3m long, and the set temperatures of the oven are 50℃, 60℃, and 60℃; after drying, a single-layer polymer bonding layer of particle accumulation is obtained, and the thickness of the bonding layer is 2μm.
[0109] <Preparation of lithium-ion batteries>
[0110] The positive electrode sheet, separator, and negative electrode sheet prepared above were stacked in order, with the groove of the negative electrode sheet facing the positive electrode sheet and the separator positioned between the positive and negative electrode sheets to provide isolation. The electrodes were wound to form an electrode assembly, the thickness of which is shown in Table 1. The electrode assembly was placed in an aluminum-plastic film packaging bag, dried, and then injected with electrolyte. The lithium-ion battery was obtained through vacuum packaging, standing, formation, degassing, and trimming.
[0111] Example 2 to Example 25
[0112] Except for adjusting the preparation parameters such as the electrode assembly thickness T1, graphite OI value, bonding layer thickness T2, groove depth H, groove width W, groove spacing S and groove cross-sectional area A in <Preparation of negative electrode sheet> and <Preparation of lithium-ion battery> as shown in Table 2, the rest are the same as Example 1.
[0113] Example 26
[0114] Except for adjusting the "Preparation of Diaphragm", the remaining parameters were adjusted according to Table 2 based on Example 9.
[0115] <Preparation of diaphragm>:
[0116] <Preparation of Base Material Layer>
[0117] A polypropylene film with a thickness of 9 μm was used.
[0118] <Preparation of Adhesive Layer>
[0119] Polyvinylidene fluoride and aluminum oxide ceramic particles were mixed in a mass ratio of 60:40, and NMP was added as a solvent to prepare a bonding layer slurry with a solid content of 75 wt%. The mixture was then stirred evenly. The bonding layer slurry was applied to one substrate layer and dried at 90°C to form a bonding layer. The thickness of the bonding layer is shown in Table 2. The above steps were then repeated on the other substrate layer to form a double-sided bonding layer, thus completing the separator.
[0120] Example 27
[0121] The process was the same as in Example 26 except that the type of polymer was changed to polyvinylidene fluoride-hexafluoropropylene copolymer in <Preparation of Separator>.
[0122] Comparative Example 1
[0123] Except for the difference in <Preparation of Negative Electrode Sheet> from Example 1, the rest is the same as Example 1.
[0124] <Preparation of negative electrode sheet>
[0125] Artificial graphite (OI value 14), conductive carbon black (SP), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 96.5:1:1:1.5, and deionized water was added to form a slurry with a solid content of 75 wt%. The mixture was then stirred evenly. The slurry was evenly coated on one surface of a 6 μm thick negative electrode current collector copper foil and dried at 85°C to obtain a negative electrode sheet with a 50 μm thick negative electrode active material layer. The above steps were then repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet coated with negative electrode active material on both sides. The sheet was then slit and cut, dried at 110°C under vacuum for 4 hours, and welded to the tabs to obtain the negative electrode sheet.
[0126] Comparative Example 2
[0127] Except that in <Preparation of Separator>, the thickness of the adhesive layer is adjusted to 5 μm to control the adhesive force F between the negative electrode sheet and the separator to be 12 N / m, the rest is the same as Comparative Example 1.
[0128] Comparative Example 3 to Comparative Example 4
[0129] Except for adjusting the preparation parameters such as the electrode assembly thickness T1, groove width W, and groove spacing S in <Preparation of Negative Electrode Sheet> and <Preparation of Lithium-ion Battery> as shown in Table 1, the rest is the same as Example 1.
[0130] Table 2
[0131] Note: “ / ” in Table 2 indicates no relevant preparation parameters.
[0132] As shown in Table 1, from Examples 1 to 2 and Comparative Examples 1 to 4, it can be seen that in the lithium-ion battery of the present application, by providing grooves on the surface of the negative electrode active material layer opposite the positive electrode sheet, and regulating the relationship between the groove width, groove spacing, and electrode assembly thickness within the scope of the present application, the adhesion between the negative electrode sheet and the separator can be improved. Furthermore, the hot box pass rate of the lithium-ion battery is significantly improved, and the thickness expansion rate of the lithium-ion battery after cycling is also significantly reduced, indicating that the lithium-ion battery of the present application has excellent cycling stability and safety, especially at high temperatures.
[0133] Referring to Tables 2 and 3, the groove spacing, groove width, adhesive layer thickness, and groove depth generally also affect the performance of the lithium-ion battery. From Examples 1 to 25, it can be seen that when W ≥ S × T1 / 1000 is satisfied, by regulating the above parameters within the scope of this application, a lithium-ion battery with excellent cycle stability and safety can be obtained.
[0134] The cross-sectional area of the groove also generally affects the performance of the lithium-ion battery. From Examples 13 to 15, it can be seen that when 0.3×fW×H)<A<0.9.5×fW×H), by regulating the above parameters within the scope of this application, a lithium-ion battery with excellent cycle stability and safety can be obtained.
[0135] The structure of the bonding layer in the diaphragm, the type of polymer in the bonding layer, and the type of heat-resistant material in the heat-resistant material layer usually also affect the performance of the lithium-ion battery. It can be seen from Examples 26 to 27 that, when W≥S×T1 / 1000 is satisfied, by regulating the above parameters within the scope of this application, a lithium-ion battery with excellent cycle stability and safety can be obtained.
[0136] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "includes," or any other variants thereof are intended to cover non-exclusive inclusions, such that a process, method, article, or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such process, method, article, or device. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of additional identical elements in the process, method, article, or device comprising the element.
[0137] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A secondary battery, comprising an electrode assembly, wherein the electrode assembly comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer, wherein: The surface of the negative electrode active material layer opposite to the positive electrode plate has a groove, the width of the groove is W mm, and the spacing of the grooves is S mm; The thickness of the electrode assembly is T1 mm, satisfying: W ≥ S × T1 / 1000.
2. The secondary battery according to claim 1, wherein W≤2×S×T1.
3. The secondary battery according to claim 1, wherein S×T1 / 400≤W≤S×T1 / 2.
4. The secondary battery according to claim 1, wherein At least one of the following conditions is met: (a) 0.05≤S≤10; (b)0.02≤W≤0.
5.
5. The secondary battery according to claim 1, wherein The OI value of the negative electrode plate and the S satisfy: S / OI≤0.5; Where, OI value = C 004 / C 110 , C 004 is the peak area obtained from the (004) plane diffraction line pattern in the X-ray diffraction spectrum, C 110 It is the peak area obtained from the (110) plane diffraction line pattern in the X-ray diffraction spectrum.
6. The secondary battery according to claim 5, wherein 0.005≤S / OI≤0.03,8≤OI≤25.
7. The secondary battery according to claim 1, wherein A bonding layer is provided on the surface of the separator opposite to the negative electrode plate, and the bonding layer includes a polymer; Wherein, based on the mass of the bonding layer, the content of the polymer is 30% to 100%.
8. The secondary battery according to claim 7, wherein The bonding force between the separator and the negative electrode plate is FN / m, satisfying F>3.
9. The secondary battery according to claim 7, wherein The thickness of the bonding layer is T2 μm, and the depth of the groove is H μm, satisfying: H≤T2+20.
10. The secondary battery according to claim 9, wherein The cross-sectional area of the groove is A μm 2 , satisfying: 0.3×(W×H)<A<0.95×(W×H), 2≤H≤50.
11. The secondary battery according to claim 10, wherein 0.35×(W×H)<A<0.8×(W×H).
12. The secondary battery according to claim 7, wherein The polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, styrene-butadiene copolymer, polyacrylonitrile, butadiene-acrylonitrile polymer, polyacrylic acid, polyacrylate or acrylate-styrene copolymer.
13. The secondary battery according to claim 1, wherein Along the width direction of the negative electrode sheet, the groove forms a structure penetrating the negative electrode sheet; The groove includes a first section with a width of W1 and a second section with a width of W2, satisfying 1.2<W1 / W2<1.
8.
14. The secondary battery according to claim 1, wherein Along the width direction of the negative electrode plate, the groove forms a structure that does not penetrate the negative electrode plate. 15 . An electronic device comprising the secondary battery according to claim 1 .