All-optical nonlinear modulation metasurface-based diffractive optical computing device and preparation method therefor
By combining optical diffraction metasurfaces, plasmons and nonlinear two-dimensional material layers in metasurface diffractive light computing devices, the optical nonlinear coefficient of nonlinear optical materials is improved, solving the problem of high energy consumption and response in existing technologies. It solves the problem of slow speed and realizes non-linear computing functions with low power consumption and high-density integration.
Patent Information
- Application Number
- PCT/CN2023/087674
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-03
AI Technical Summary
Existing nonlinear materials have low optical nonlinear coefficients, all-optical nonlinear devices have high energy consumption, large size, and slow response speed, making them difficult to apply to the needs of nonlinear modulation devices in artificial intelligence optical computing chips.
Using an all-optical nonlinear modulation metasurface diffraction light computing device, through the composite of optical diffraction metasurface, plasmons and nonlinear two-dimensional material layers, the resonance enhancement effect of plasmons is used to improve nonlinear two-dimensional materials. The equivalent all-optical nonlinear coefficient of the layer realizes nonlinear optical absorption with low power consumption and low optical threshold.
It greatly reduces the power consumption of the device, making it more sensitive to low light, meeting the needs of nonlinear modulation devices in artificial intelligence optical computing chips, and achieving high-density integration and complex computing functions.
Smart Images

Figure CN2023087674_03102024_PF_FP_ABST
Abstract
Description
All-optical nonlinear modulated metasurface diffraction optical computing device and its preparation method
[0001] Priority information
[0002] This application requests the priority of the Chinese patent application with patent application number 202310309887.1 and application name “All-optical nonlinear modulated metasurface diffraction optical computing device and its preparation method” filed with the State Intellectual Property Office of China on March 27, 2023, and the entire contents are incorporated by reference in this disclosure. Technical Field
[0003] The present application belongs to the field of artificial intelligence optical computing technology, and specifically relates to an all-optical nonlinearly modulated metasurface diffraction optical computing device and a preparation method thereof. Background Art
[0004] Deep neural networks, artificial intelligence (AI) inspired by biological neural networks, have flourished in recent years, enabling statistics, inference, and prediction based on massive amounts of multidimensional data. Diffraction neural networks utilize the wave propagation properties of light to perform calculations, offering advantages such as high integration, high computational parallelism, high computational speed, and large computational scale. However, in the inference and computational process of optical neural networks, the coherent interactions between different light beams and the interaction between light and matter are essentially linear effects, limiting their computational capabilities to linear operations.
[0005] Nonlinear activation, a hallmark of biological neural networks, is crucial for the brain to complete complex tasks with extremely low power consumption. Therefore, implementing a nonlinear activation layer is a necessary condition and a key foundation for all-optical deep neural networks to accomplish complex functions-based tasks. However, existing nonlinear materials have low optical nonlinear coefficients, and all-optical nonlinear devices have high energy consumption, large size, and slow response speed, making them difficult to apply.
[0006] Summary of the Invention
[0007] The present application aims to improve at least one of the above technical problems to at least some extent.
[0008] To improve the above technical problems, the present application provides an all-optical nonlinear modulated metasurface diffraction optical computing device, the all-optical nonlinear modulated metasurface diffraction optical computing device comprising an optical diffraction metasurface, a metal layer, a first insulating layer, a nonlinear two-dimensional material layer, a second insulating layer, a plasmon and a protective layer, wherein the metal layer is located on one side of the optical diffraction metasurface, the first insulating layer is located on the side of the metal layer away from the optical diffraction metasurface, the nonlinear two-dimensional material layer is located on the side of the first insulating layer away from the metal layer, the second insulating layer is located on the side of the nonlinear two-dimensional material layer away from the first insulating layer, the plasmon is located on the side of the second insulating layer away from the nonlinear two-dimensional material layer, and the protective layer is located on the side of the plasmon away from the second insulating layer. Thus, the present application combines the optical diffraction metasurface with the plasmon and the nonlinear two-dimensional material layer to enhance the light absorption of the nonlinear optical material, achieve nonlinear optical absorption with low power consumption and low optical threshold, and be applied to low-power diffraction optical computing devices, thereby realizing an all-optical nonlinear computing function device, which can meet the current demand for nonlinear modulation devices in artificial intelligence optical computing chips. Moreover, the all-optical nonlinear modulation device of the present application uses an optical diffraction metasurface to be compounded with plasmons and nonlinear two-dimensional material layers, and utilizes the resonance enhancement effect of plasmons to greatly improve the equivalent all-optical nonlinear coefficient of the nonlinear two-dimensional material layer, making it more sensitive to weak light and greatly reducing the power consumption of the device.
[0009] According to an embodiment of the present application, the optical diffraction metasurface includes a base layer, an active layer and a flat layer; the active layer is located on one side of the base layer, the active layer includes a plurality of active units arranged in an array, and the metal layer is located on the side of the flat layer away from the base layer; the material forming the active layer includes any one of silicon and oxide; the material forming the flat layer includes silicon dioxide.
[0010] According to an embodiment of the present application, the planar layer satisfies any one of the following conditions:
[0011] The flat layer is located between adjacent active units, and the thickness of the flat layer is equal to the thickness of the active unit;
[0012] The flat layer includes a first flat portion and a second flat portion, the first flat portion is located between adjacent active units, the thickness of the first flat portion is equal to the thickness of the active unit, the second flat portion covers the first flat portion and the active unit, and the thickness of the second flat portion is less than or equal to 20 nm.
[0013] According to an embodiment of the present application, the all-optical nonlinearly modulated metasurface diffraction optical computing device satisfies at least one of the following conditions: the thickness of the base layer is 100 to 250 μm; the thickness of the active layer is 100 to 300 nm; the material forming the metal layer includes at least one of gold and silver; the thickness of the metal layer is 1 to 5 nm; the material forming the first insulating layer includes hexagonal boron nitride; and the thickness of the first insulating layer is 5 to 10 nm.
[0014] According to an embodiment of the present application, the nonlinear two-dimensional material layer includes nonlinear two-dimensional material sublayers, and the number of the nonlinear two-dimensional material sublayers is 1-4; when the number of the nonlinear two-dimensional material sublayers is greater than 1, multiple nonlinear two-dimensional material sublayers are stacked; the material forming the nonlinear two-dimensional material sublayer includes any one of black phosphorus, PdSe2, PdS2, InSe, MoS2, WS2, and WSe2; the thickness of the nonlinear two-dimensional material sublayer is 0.5 to 20 nm.
[0015] According to an embodiment of the present application, when the number of the nonlinear two-dimensional material sub-layers is greater than one, the materials of the multiple nonlinear two-dimensional material sub-layers are different from each other.
[0016] According to an embodiment of the present application, when the material forming the active layer is silicon, the material forming the nonlinear two-dimensional material sublayer includes any one of black phosphorus, PdSe2, PdS2, and InSe; when the material forming the active layer is oxide, the material forming the nonlinear two-dimensional material sublayer includes any one of MoS2, WS2, and WSe2.
[0017] According to an embodiment of the present application, the all-optical nonlinear modulated metasurface diffraction optical computing device satisfies at least one of the following conditions: the material forming the second insulating layer includes hexagonal boron nitride; the thickness of the second insulating layer is 1 to 5 nm; the material forming the plasmon includes WO 3-x , gold, and silver; the form of the material forming the plasmon includes at least one of nanowires and quantum dots; the length of the nanowire is 50 to 150 nm, and the width of the nanowire is 5 to 20 nm; the diameter of the quantum dot is less than 40 nm; the material forming the protective layer includes at least one of SiO2 and Al2O3; the thickness of the protective layer is 15 to 50 nm.
[0018] The present application also provides a method for preparing an all-optical nonlinearly modulated metasurface diffraction optical computing device, the method comprising: providing an optical diffraction metasurface; forming a metal layer on one side of the optical diffraction metasurface; forming a first insulating layer on a side of the metal layer away from the optical diffraction metasurface; forming a nonlinear two-dimensional material layer on a side of the first insulating layer away from the metal layer; forming a second insulating layer on a side of the nonlinear two-dimensional material layer away from the first insulating layer; forming plasmons on a side of the second insulating layer away from the nonlinear two-dimensional material layer; and forming a protective layer on a side of the plasmons away from the second insulating layer.
[0019] According to an embodiment of the present application, the optical diffraction metasurface is formed by: providing a composite structure having a base layer and an active material layer; forming a photoresist layer on a side of the active material layer away from the base layer; patterning the photoresist layer to obtain a structure having a patterned adhesive layer; etching the structure having the patterned adhesive layer using the patterned adhesive layer as a mask to form an active layer from the active material layer, wherein the active layer includes a plurality of active units arranged in an array to obtain a structure having an active layer; immersing the structure having the active layer in an acetone solution, and removing the patterned adhesive layer using an ultrasonic bath to obtain a metasurface having an active layer; forming a flat layer on one side of the base layer so that the flat layer at least covers the area between adjacent active units to obtain an optical diffraction metasurface.
[0020] According to an embodiment of the present application, the method satisfies at least one of the following conditions: the metal layer is formed by evaporation coating; the first insulating layer is formed on the metal layer by fixed-point transfer; the nonlinear two-dimensional material layer is formed on the first insulating layer by fixed-point transfer; the second insulating layer is formed on the nonlinear two-dimensional material layer by fixed-point transfer; the plasmon is formed by spin coating; forming the plasmon includes: mixing the material forming the plasmon with ethanol to prepare a coating solution, coating the coating solution on the side of the second insulating layer away from the nonlinear two-dimensional material layer, and drying to obtain the plasmon; the protective layer is formed by evaporation coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] FIG1 is a schematic diagram of the structure of an all-optical nonlinearly modulated metasurface diffraction optical computing device in one embodiment of the present application;
[0022] FIG2 is a perspective view of a base layer and an active layer in an optical diffraction metasurface in one embodiment of the present application;
[0023] FIG3 is a schematic diagram of the structure of an optical diffraction metasurface in one embodiment of the present application;
[0024] FIG4 is a schematic structural diagram of an optical diffraction metasurface in another embodiment of the present application;
[0025] FIG5 is a diagram showing the all-optical nonlinear function of a device in one embodiment of the present application;
[0026] FIG6 is a diagram showing the all-optical nonlinear function of a device in another embodiment of the present application;
[0027] FIG7 is a diagram showing the all-optical nonlinear function of a device in another embodiment of the present application;
[0028] FIG8 is a diagram showing the all-optical nonlinear function of a device in another embodiment of the present application;
[0029] FIG9 is a flow chart of a method for preparing an all-optical nonlinearly modulated metasurface diffraction optical computing device in one embodiment of the present application.
[0030] Description of Reference Numerals
[0031] 100-optical diffraction metasurface, 110-base layer, 120-active layer, 121-active unit, 130-flat layer, 200-metal layer, 300-first insulating layer, 400-nonlinear two-dimensional material layer, 500-second insulating layer, 600-plasmon, 700-protective layer. DETAILED DESCRIPTION
[0032] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this area or according to the product specifications. Reagents used that do not specify the manufacturer are conventional products that can be obtained commercially.
[0033] The present application provides an all-optical nonlinearly modulated metasurface diffraction optical computing device. Referring to Figure 1, the all-optical nonlinearly modulated metasurface diffraction optical computing device includes: an optical diffraction metasurface 100, a metal layer 200, a first insulating layer 300, a nonlinear two-dimensional material layer 400, a second insulating layer 500, a plasmon 600 and a protective layer 700. The metal layer 200 is located on one side of the optical diffraction metasurface 100, the first insulating layer 300 is located on the side of the metal layer 200 away from the optical diffraction metasurface 100, the nonlinear two-dimensional material layer 400 is located on the side of the first insulating layer 300 away from the metal layer 200, the second insulating layer 500 is located on the side of the nonlinear two-dimensional material layer 400 away from the first insulating layer 300, the plasmon 600 is located on the side of the second insulating layer 500 away from the nonlinear two-dimensional material layer 400, and the protective layer 700 is located on the side of the plasmon 600 away from the second insulating layer 500. The protective layer 700 can encapsulate the device and protect the internal structure of the device. Therefore, the present application combines the optical diffraction metasurface 100 with the plasmon 600 and the nonlinear two-dimensional material layer 400, and applies it to low-power diffraction optical computing devices, which can meet the needs of nonlinear modulation devices in current artificial intelligence optical computing chips. Moreover, the present application utilizes the resonance enhancement effect of the plasmon 600 to greatly improve the equivalent all-optical nonlinear coefficient of the nonlinear two-dimensional material layer 400, making it more sensitive to weak light and greatly reducing the power consumption of the device. In addition, the all-optical nonlinear modulation device of the present application is combined with the low-dimensional material by the optical diffraction metasurface 100. The size of a single structure, that is, a single neuron on the metasurface is on the order of hundreds of nanometers, and the size of the entire device is on the order of hundreds of microns. A single device can integrate millions of neurons, which has the advantage of high-density integration.
[0034] For ease of understanding, the working mechanism of the all-optical nonlinearly modulated metasurface diffraction optical computing device is explained here: This application can achieve heterogeneous integration of an all-optical nonlinear modulation layer and an optical diffraction metasurface 100. Through the localized surface plasmon resonance effect of the plasmon 600, the light absorption of the nonlinear optical material is enhanced, achieving low power consumption and low optical threshold nonlinear optical absorption, thereby obtaining an all-optical nonlinear computing function device. At the same time, the metasurface is prepared through an inverse design algorithm and an optical neural network is introduced for calculation and training, thereby obtaining the modulation of the amplitude and phase of the optical signal that needs to be modulated online, realizing an on-chip nonlinear optical device with all-optical modulation and real-time training and updating.
[0035] According to an embodiment of the present application, with reference to Figures 3 and 4, an optical diffraction metasurface 100 includes a base layer 110, an active layer 120, and a flat layer 130; the active layer 120 is located on one side of the base layer 110. Referring to Figure 2, the active layer 120 includes a plurality of active units 121 arranged in an array, with the plurality of active units 121 spaced apart. A metal layer 200 is located on the side of the flat layer 130 away from the base layer 110; the material forming the active layer 120 includes any one of silicon and an oxide; the material forming the oxide includes any one of TiO2 and ZnO, and the material forming the flat layer 130 includes silicon dioxide. Thus, the optical diffraction metasurface 100 can be made to have the effect of nonlinear diffraction calculation.
[0036] According to an embodiment of the present application, the flat layer satisfies any of the following conditions: with reference to FIG3 , the flat layer 130 may be located between adjacent active units 121, and the thickness of the flat layer 130 is equal to the thickness of the active unit 121; or, with reference to FIG4 , the flat layer 130 includes a first flat portion and a second flat portion, the first flat portion is connected to the second flat portion, the first flat portion is located between adjacent active units 121, the thickness of the first flat portion is equal to the thickness of the active unit 121, the second flat portion covers the first flat portion and the active unit 121, and the thickness of the second flat portion is less than or equal to 20 nm. In other words, the flat layer is at least located between adjacent active units 121. Both of the above-mentioned flat layer structures can enable the optical diffraction metasurface 100 to have the effect of nonlinear diffraction calculation.
[0037] According to some embodiments of the present application, the thickness of the base layer 110 is 100-250 μm, for example, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, and 250 μm.
[0038] According to some embodiments of the present application, the thickness of the active layer 120 is 100 to 300 nm, for example, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, and 300 nm.
[0039] According to some embodiments of the present application, when the material forming the active layer 120 is silicon, SOI (silicon on insulator) can be used as the raw material for preparing the optical diffraction metasurface 100. The bottom and top of the SOI are both silicon layers, and the middle is a silicon dioxide layer. The bottom silicon layer and the middle silicon dioxide layer of the SOI can be used as the base layer 110, and the top silicon layer of the SOI can be used as the active material layer. After a series of treatments, the active material layer can obtain a patterned silicon layer, which is the active layer 120.
[0040] In other embodiments of the present application, when the material forming the active layer 120 is oxide, the material forming the base layer 110 can be any one of Al 2 O 3 , SiO 2 , and ITO.
[0041] According to an embodiment of the present application, when the material forming the active layer 120 is silicon, the corresponding optical diffraction metasurface 100 can respond in the infrared band. When the material forming the active layer 120 is oxide, the corresponding optical diffraction metasurface 100 can respond in the visible light band.
[0042] According to some embodiments of the present application, the structural parameters of the optical diffraction metasurface 100 can be calculated by an inverse design algorithm in simulation software. For example, the dimensional parameters of the optical diffraction metasurface 100 can be calculated.
[0043] According to an embodiment of the present application, the material forming the metal layer 200 includes at least one of gold and silver; and the thickness of the metal layer 200 is 1 to 5 nm.
[0044] According to an embodiment of the present application, the material forming the first insulating layer 300 includes hexagonal boron nitride and has a thickness of 5 to 10 nm. Thus, the first insulating layer 300 can enhance the plasmon effect of the metal layer, thereby enhancing the nonlinear effect of the two-dimensional material layer.
[0045] According to some embodiments of the present application, the material forming the nonlinear two-dimensional material sublayer includes any one of black phosphorus, PdSe2, PdS2, InSe, MoS2, WS2, and WSe2.
[0046] According to an embodiment of the present application, the nonlinear two-dimensional material layer 400 includes nonlinear two-dimensional material sublayers, and the number of nonlinear two-dimensional material sublayers is 1-4; when the number of nonlinear two-dimensional material sublayers is greater than 1, multiple nonlinear two-dimensional material sublayers are stacked. Since each nonlinear two-dimensional material sublayer can correspond to a nonlinear function, the nonlinear two-dimensional material layer 400 of the present application can include multiple nonlinear two-dimensional material sublayers, which can realize a combination of multiple nonlinear function forms (such as ReLU, tanh, sigmoid, softplus). According to the requirements of the complexity of the diffraction neural network calculation task, nonlinear materials with different nonlinear function forms are selected to complete higher-order nonlinear calculations, which has the advantages of high network calculation flexibility, strong randomness, and high complexity.
[0047] According to some embodiments of the present application, the thickness of the nonlinear two-dimensional material sublayer is 0.5 to 20 nm.
[0048] According to an embodiment of the present application, when the number of nonlinear two-dimensional material sub-layers is greater than one, the materials of the multiple nonlinear two-dimensional material sub-layers are different from each other. Thus, the device can realize a combination of multiple nonlinear function forms.
[0049] According to an embodiment of the present application, when the material forming the active layer 120 is silicon, the material forming the nonlinear two-dimensional material sublayer includes any one of black phosphorus, PdSe2, PdS2, and InSe; these materials have the characteristic of responding to infrared light. When the material forming the active layer 120 is silicon, the corresponding optical diffraction metasurface 100 can respond in the infrared band. Therefore, the optical diffraction metasurface 100 and the nonlinear two-dimensional material layer 400 cooperate with each other to enable the device of the present application to have nonlinear saturation absorption characteristics in the infrared band.
[0050] When the material forming the active layer 120 is an oxide, the material forming the nonlinear two-dimensional material sublayer includes any one of MoS2, WS2, and WSe2, which have the characteristic of responding to visible light. When the material forming the active layer 120 is an oxide, the corresponding optical diffraction metasurface 100 can respond in the visible light band. Therefore, the optical diffraction metasurface 100 and the nonlinear two-dimensional material layer 400 cooperate with each other to enable the device of the present application to have nonlinear saturation absorption characteristics in the visible light band.
[0051] The all-optical nonlinearly modulated metasurface diffraction optical computing device of the present application can adopt different optical diffraction metasurface 100 materials and nonlinear two-dimensional material layer 400 materials according to different application scenarios. It has nonlinear saturation absorption characteristics for the visible light to infrared band. The nonlinear activation function is introduced in the optical diffraction neural network calculation process, which can realize complex tasks such as multi-object recognition, classification, numerical logic operations, etc. in complex scenes.
[0052] Since the nonlinear two-dimensional material layer 400 can have multiple nonlinear two-dimensional material sub-layers, by adjusting the number of layers and specific materials of the nonlinear two-dimensional material sub-layers, the device can realize a combination of multiple nonlinear function forms.
[0053] Referring to FIG. 5 , in one embodiment of the present application, the device may have an all-optical nonlinear function form of ReLU.
[0054] 6 , in one embodiment of the present application, the device may have an all-optical nonlinear function form of Tanh.
[0055] 7 , in one embodiment of the present application, the device may have an all-optical nonlinear function form of Sigmoid.
[0056] 8 , in one embodiment of the present application, the device may have an all-optical nonlinear function form of Softplus. Softplus=Log(1+e x )
[0057] According to an embodiment of the present application, the material forming the second insulating layer 500 includes hexagonal boron nitride (h-BN); the thickness of the second insulating layer 500 is 1 to 5 nm. Thus, the second insulating layer 500 can effectively prevent thermal effects generated when the plasmons 600 and the nonlinear two-dimensional material layer 400 come into contact.
[0058] According to an embodiment of the present application, the material forming the plasmon 600 includes WO 3-x , gold, silver, among which WO 3-x The value range of x is: 0≤x≤1. In this way, the plasmon 600 can have a resonance enhancement effect, which can significantly increase the equivalent all-optical nonlinear coefficient of the nonlinear two-dimensional material layer 400, making it more sensitive to weak light and significantly reducing the power consumption of the device.
[0059] According to an embodiment of the present application, the material forming plasmons 600 comprises at least one of nanowires and quantum dots; the nanowires are 50 to 150 nm long and 5 to 20 nm wide; and the quantum dots have a diameter of 40 nm or less. This further increases the effective all-optical nonlinear coefficient of the nonlinear two-dimensional material layer 400, making it more sensitive to weak light and further reducing device power consumption.
[0060] According to an embodiment of the present application, the material forming the protective layer 700 includes at least one of SiO2 and Al2O3, and the thickness of the protective layer 700 is 15 to 50 nm, thereby effectively protecting the internal structure of the device.
[0061] The present application also provides a method for preparing an all-optical nonlinearly modulated metasurface diffraction optical computing device. Referring to FIG9 , the method includes:
[0062] S100, providing an optical diffraction metasurface;
[0063] According to an embodiment of the present application, an optical diffraction metasurface is formed by: providing a composite structure having a base layer and an active material layer, forming a photoresist layer on a side of the active material layer away from the base layer, and patterning the photoresist layer to obtain a structure having a patterned adhesive layer; etching the structure having the patterned adhesive layer using the patterned adhesive layer as a mask to form an active layer of the active material layer, wherein the active layer includes a plurality of active units arranged in an array to obtain a structure having an active layer; immersing the structure having the active layer in an acetone solution, and removing the patterned adhesive layer using an ultrasonic bath to obtain a metasurface having an active layer; forming a flat layer on one side of the base layer so that the flat layer at least covers the area between adjacent active units to obtain an optical diffraction metasurface.
[0064] According to some specific embodiments of the present application, a silicon-based optical diffraction metasurface is formed in the following manner: a double-sided polished SOI substrate having a top Si active layer of 100 to 200 nm thick and a substrate layer composed of SiO2 and Si of 100 to 250 μm thick is used. The spin coater speed is set to 3000 to 5000 r / min, the time is set to 20s to 80s, and an electron beam photoresist of model ARN7520.17 is evenly applied to the surface of the SOI substrate. The spin-coated sample is placed on a baking table, the baking temperature is set to 60 to 120°C, and baking is carried out for 1 to 2 minutes. The photoresist layer is patterned using an electron beam exposure method to form an m×n array, the length of the rectangular unit is 200 to 800 nm, the width of the rectangular unit is 100 to 200 nm, and the electron exposure metering is set to 18 to 40 nC / cm 2The electron beam current was adjusted between 50 and 150 pA. The exposed substrate was then immersed in AR300-47 developer for 100 to 120 seconds for development. The surface developer was then washed off by immersion in isopropyl alcohol for 30 to 60 seconds, resulting in a structure with a patterned adhesive layer. The patterned adhesive layer was then used as a mask for deep silicon etching using inductively coupled plasma (ICP) etching. The etching power was 70 to 90 W, C₄F₄ and SF₆ gas flow rates were 30 to 50 sccm and 50 to 100 sccm, respectively, and the etching time was 20 to 30 seconds, transferring the pattern from the photoresist layer to the Si layer. Depending on the length, width, and etching depth of the pattern designed by electron beam exposure, rectangular metasurfaces with lengths of 200 to 800 nm, widths of 100 to 200 nm, and heights of 100 to 300 nm were obtained. The resulting structure is immersed in an acetone solution and the electron beam photoresist is removed using an ultrasonic bath. Electron beam evaporation is then used to deposit SiO2 on the sample to a thickness of 120 to 320 nm. Rapid thermal annealing is then used at 1000 to 1200°C for 1 to 2 minutes to planarize the deposited SiO2 layer. Finally, chemical mechanical polishing (CMP) is used to grind and polish the SiO2 using a lapping solution composed of abrasives (Al2O3, SiO2, or ZrO2), an acid or base (KOH or NH2OH), and pure water. The polished thickness is 100 to 320 nm. The metasurface is then post-cleaned with deionized water to remove particles and other chemical contaminants, and then dried in an oven at 60 to 120°C to obtain a silicon-based optical diffraction metasurface.
[0065] According to some embodiments of the present application, when the material forming the active layer is oxide, the step includes: providing a base layer, forming the active layer on one side of the base layer, and obtaining a composite structure having the base layer and the active layer.
[0066] According to some specific embodiments of the present application, the oxide optical diffraction metasurface is formed by selecting a double-sided polished Al2O3, SiO2 or ITO transparent substrate. The substrate is placed in a high vacuum electron beam coating chamber, and the electron beam in the coating machine bombards a 99.99% pure TiO2 or ZnO block to reach the evaporation temperature. The film deposition rate is Deposit an oxide layer with a thickness of 80 to 150 nm. Set the spin coater speed to 3000 to 5000 r / min, the time to 60 to 80 s, and evenly apply electron beam photoresist model ARN7520.17 on the surface of the above oxide layer. Place the spin-coated sample on a baking table, set the baking temperature to 60 to 120 ° C, and bake for 1 to 2 minutes. Use electron beam exposure to pattern the photoresist layer to form an m×n array, with a rectangular unit length of 200 to 800 nm, a rectangular unit width of 100 to 200 nm, and an electron exposure metering setting of 18 to 40 nC / cm 2 The electron beam current was adjusted between 50 and 150 pA. The exposed structure was developed by immersing it in AR300-47 developer for 100 to 120 seconds and then rinsing it in isopropyl alcohol for 30 to 60 seconds to remove the developer. The patterned resist layer was then used as a mask to etch the oxide substrate using inductively coupled plasma (ICP) etching. The etching power was 150 to 200 W, the O2 gas flow rate was 30 to 50 sccm, and the etching time was 20 to 40 seconds, transferring the pattern from the photoresist layer to the oxide layer. Depending on the length, width, and etching depth of the pattern designed by electron beam exposure, rectangular metasurfaces with lengths of 200 to 800 nm, widths of 100 to 200 nm, and heights of 100 to 300 nm were obtained. The substrate was then immersed in an acetone solution and the electron beam photoresist was removed using an ultrasonic bath. The acetone was then rinsed off with alcohol. Electron beam evaporation is then used to deposit 120 to 320 nm of SiO2 on the sample, followed by rapid thermal annealing at 1000 to 1200°C for 1 to 2 minutes to flatten the deposited SiO2 layer. Finally, chemical mechanical polishing (CMP) is used to grind and polish the SiO2 using a grinding solution composed of abrasives (Al2O3, SiO2, or ZrO2), an acid or base (KOH or NH2OH), and pure water. The polishing thickness is 100 to 320 nm, and the metasurface is then post-cleaned with deionized water to remove particles and other chemical contaminants. The surface is then dried in an oven at 60 to 120°C to obtain an oxide optical diffraction metasurface.
[0067] S200, forming a metal layer on one side of the optical diffraction metasurface;
[0068] According to an embodiment of the present application, the metal layer is formed by evaporation coating.
[0069] According to some embodiments of the present application, step S200 includes: placing the optical diffraction metasurface prepared in step S100 into a thermal evaporation or electron beam high vacuum coating chamber, bombarding a metal block with a purity of 99.99% by an electron beam in the evaporation coating machine to make it reach the evaporation temperature, and the deposition rate of the film is A metal layer with a thickness of 1 to 5 nm is deposited.
[0070] In some embodiments of the present application, the metal layer is gold or silver.
[0071] S300, forming a first insulating layer on a side of the metal layer away from the optical diffraction metasurface;
[0072] According to an embodiment of the present application, the material forming the first insulating layer includes hexagonal boron nitride.
[0073] According to an embodiment of the present application, the first insulating layer is formed on the metal layer by a fixed-point transfer method.
[0074] In some embodiments of the present application, transferring the first insulating layer to the metal layer via a fixed-point transfer method includes: transferring a block of the first insulating layer material onto Scotch tape using a mechanical peeling method, repeatedly folding the Scotch tape in half, and then adhering polydimethylsiloxane (PDMS) to the Scotch tape to absorb a small amount of nanometer-thick hexagonal boron nitride. Using a microscope in a fixed-point transfer operating system, the PDMS is moved so that the hexagonal boron nitride attached to the PDMS contacts the metal layer, the PDMS is slowly lowered to adhere the hexagonal boron nitride to the metal layer, and the sample stage temperature is raised to 35-70°C to allow the hexagonal boron nitride material on the PDMS to fall onto the metal layer.
[0075] S400, forming a nonlinear two-dimensional material layer on a side of the first insulating layer away from the metal layer;
[0076] According to an embodiment of the present application, the nonlinear two-dimensional material layer is formed on the first insulating layer by a fixed-point rotation method.
[0077] According to some embodiments of the present application, the nonlinear two-dimensional material layer includes nonlinear two-dimensional material sublayers, and the number of nonlinear two-dimensional material sublayers is 1-4. When the number of nonlinear two-dimensional material sublayers is greater than one, the nonlinear two-dimensional material layer can be obtained by sequentially transferring the multiple nonlinear two-dimensional material sublayers onto the first insulating layer.
[0078] S500, forming a second insulating layer on a side of the nonlinear two-dimensional material layer away from the first insulating layer;
[0079] According to an embodiment of the present application, the second insulating layer is formed on the nonlinear two-dimensional material layer by a fixed-point transfer method.
[0080] S600 , forming plasmons on a side of the second insulating layer away from the nonlinear two-dimensional material layer.
[0081] According to an embodiment of the present application, plasmons are formed by spin coating.
[0082] In some embodiments of the present application, forming plasmons includes: mixing a plasmon-forming material with ethanol, ultrasonicating the mixed solution in an ultrasonic machine for 12 to 24 hours to allow the plasmon-forming material and the ethanol to fully mix, preparing a coating solution, and evenly coating the coating solution on a side of the second insulating layer away from the nonlinear two-dimensional material layer using a spin coater, followed by drying to obtain plasmons. According to some embodiments of the present application, the drying temperature is 80 to 120°C, and the drying time is 30 to 60 seconds.
[0083] According to some specific embodiments of the present application, 2 to 10 mg of WO can be weighed. 3-x Or 1-5 mL of gold or silver quantum dots were dissolved in 10 mL of ethanol and magnetically stirred at 80°C until completely dissolved.
[0084] S700 , forming a protective layer on a side of the plasmon away from the second insulating layer.
[0085] Thus, the protective layer can encapsulate the device and protect the internal structure of the device.
[0086] According to an embodiment of the present application, the protective layer is formed by evaporation coating.
[0087] In general, the method of the present application has the advantages of simple operation, strong controllability, and good repeatability.
[0088] In some embodiments of the present application, the all-optical nonlinearly modulated metasurface diffraction optical computing device prepared by this method has the same structure as the all-optical nonlinearly modulated metasurface diffraction optical computing device described above. Therefore, this method has all the characteristics and advantages of the all-optical nonlinearly modulated metasurface diffraction optical computing device described above, which will not be repeated here.
[0089] The present application is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present application in any way.
[0090] Example 1
[0091] The method for preparing an all-optical nonlinearly modulated metasurface diffraction optical computing device includes:
[0092] (1) Provide an SOI substrate, which includes a 100nm thick top Si layer and a 100μm thick SiO2 and Si substrate layer. Spin coat the SOI substrate in a coating machine. Press the suction key, set the rotation speed to 4000r / min, set the coating time to 30s, and drop ARN7520.17 electron beam negative glue on the surface of the SOI substrate. Press the start key to evenly coat the electron beam glue on the surface of the SOI substrate. Then place the sample on a coating table and bake it at 85℃ for 1min. Then use a JSM-6460LV scanning electron microscope with a nano-graphic imaging system to pattern the photoresist layer to form an m×n array. The length of the rectangular unit is 600nm, the width of the rectangular unit is 200nm, and the electron exposure dose used is set to 35nC / cm 2 The electron beam current was adjusted to 100 pA. The exposed substrate was immersed in AR300-47 developer for 120 seconds for development and then immersed in deionized water for 30 seconds for fixing.
[0093] The resulting structure was then deep-etched onto the Si layer using an ICP 550-F ICP etcher, using the patterned resist as a mask. The etching power was 80W, C₄F₄ and SF₆ gas flow rates were 50 sccm and 100 sccm, respectively, for 25 seconds. The pattern of the photoresist layer was transferred to the Si layer. This resulted in rectangular metasurface units measuring 600 nm in length, 200 nm in width, and 120 nm in height. The substrate was then immersed in an acetone solution and the electron beam photoresist removed using an ultrasonic bath. A 220 nm layer of SiO₂ was deposited on the sample using electron beam evaporation. Rapid thermal annealing (RTA) was then used at 1000–1200°C for 1–2 minutes to planarize the deposited SiO₂ layer. The SiO₂ was then polished using chemical mechanical polishing (CMP) using a slurry composed of Al₂O₃ abrasive, KOH, and pure water. The polishing thickness was 220 nm so that SiO2 was located between the active units. The metasurface was then post-cleaned with deionized water to remove particles and other chemical contaminants, and then placed in an 80°C oven for drying to obtain an optical diffraction metasurface.
[0094] (2) Using high vacuum electron beam evaporation coating better than 10 -9 Torr (vacuum degree is higher than 10 -9 Torr is lower, such as 10 -10 A 2 nm gold film was evaporated on the optical diffraction metasurface in a cavity environment with an evaporation rate of A metal layer is formed on one side of the optical diffraction metasurface.
[0095] (3) A 5 nm thick h-BN nanosheet was obtained by mechanical exfoliation, using two sheets of PDMS from Gel Pak to be folded in half and attached to a glass slide. The h-BN nanosheet was then transferred using a metallographic microscope fixed-point transfer system. The PDMS was slowly lowered to bond the two layers together. The sample stage temperature was raised to 40°C, allowing the material on the PDMS to fall onto the metal layer, forming a first insulating layer on the metal layer.
[0096] (4) A 2 nm thick black phosphorus nanosheet was obtained by mechanical exfoliation, i.e., folding two sheets of PDMS from Gel Pak in half and attaching them to a glass slide. The black phosphorus, MoS2, and WSe2 multilayer structures were then sequentially transferred onto the h-BN nanosheet using fixed-point transfer, forming a nonlinear two-dimensional material layer on the first insulating layer.
[0097] (5) Then, a 3 nm thick h-BN material is point-transferred onto the surface of the nonlinear two-dimensional material layer to form a second insulating layer on the nonlinear two-dimensional material layer.
[0098] (6) Prepared WO with a length of 100 nm and a width of 5 nm 3-x 1mg WO nanowires 3-x The nanowire powder was dissolved in 10 mL of alcohol and ultrasonicated for 24 hours to prepare a coating solution. The device obtained in step (5) was adsorbed on a spin coater and spin-coated at 500 rpm for 5 seconds, then at 2500 rpm for 20 seconds to ensure that the coating solution was evenly coated on the surface of the second insulating layer. The sample was then placed on a baking table and baked at 85°C for 1 minute to form plasmons on the second insulating layer.
[0099] (7) 20 nm of Al2O3 was deposited on the plasmon by evaporation coating to obtain an all-optical nonlinear modulated metasurface diffraction optical computing device.
[0100] Example 2
[0101] The all-optical nonlinear modulated metasurface diffraction optical computing device was prepared by referring to the method of Example 1. The other steps are the same as those of Example 1, except that:
[0102] (1) Select a double-sided polished Al2O3, SiO2 or ITO transparent substrate. Place the substrate in a high vacuum electron beam coating chamber. The electron beam in the coating machine bombards the 99.99% pure TiO2 or ZnO block to reach the evaporation temperature. The film deposition rate is Deposit an oxide layer with a thickness of 80 to 300 nm. Set the spin coater speed to 3000 to 5000 r / min, the time to 60 to 80 s, and evenly apply electron beam photoresist model ARN7520.17 on the surface of the above oxide layer. Place the spin-coated sample on a glue baking table, set the baking temperature to 60 to 120 ° C, and bake for 1 to 2 minutes. Use electron beam exposure to pattern the photoresist layer to form an m×n array, with a rectangular unit length of 200 to 800 nm, a rectangular unit width of 100 to 200 nm, and an electron exposure metering setting of 18 to 40 nC / cm 2 The electron beam current is adjusted to 50-150 pA. The exposed structure is developed by immersing it in AR300-47 developer for 100-120 seconds, and then soaking it in isopropyl alcohol for 30-60 seconds to wash away the developer on the surface.
[0103] The patterned resist layer was then used as a mask to etch the oxide substrate using inductively coupled plasma (ICP) etching at an etching power of 150-200W, an O2 gas flow rate of 30-50 sccm, and an etching time of 20-40 seconds, transferring the pattern of the photoresist layer to the oxide layer. Depending on the length, width, and etching depth of the pattern designed using electron beam exposure, a rectangular metasurface with a length of 200-800nm, a width of 100-200nm, and a height of 100-300nm was obtained. The substrate was immersed in an acetone solution, and the electron beam photoresist was removed using an ultrasonic bath. The acetone was then washed off with alcohol. Electron beam evaporation was then used to deposit 120-320nm of SiO2 on the sample. Rapid thermal annealing was then used at 1000-1200°C for 1-2 minutes to planarize the deposited SiO2 layer. Finally, the SiO2 is ground and polished using chemical mechanical polishing (CMP). The polishing slurry consists of abrasive particles (Al2O3, SiO2, or ZrO2), an acid or base (KOH or NH2OH), and pure water. The polishing thickness is 100 to 320 nm. The metasurface is then post-cleaned with deionized water to remove particles and other chemical contaminants. The metasurface is then dried in an oven at 60 to 120°C to obtain an oxide optical diffraction metasurface.
[0104] It should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly indicating the quantity of the technical features indicated. The terms "upper," "lower," "top," and "bottom," etc., indicating positions or location relationships, are based on the positions or location relationships shown in the accompanying drawings and are intended solely to facilitate the description of this application and simplify the description. They do not indicate or imply that the devices or components referred to must have a specific orientation, be constructed, or operate in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0105] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification and features of different embodiments or examples, unless they are contradictory.
[0106] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. An all-optical nonlinearly modulated metasurface diffraction optical computing device, in, The all-optical nonlinear modulated metasurface diffraction optical computing device comprises: Optical diffractive metasurfaces; A metal layer, the metal layer being located on one side of the optical diffraction metasurface; A first insulating layer, wherein the first insulating layer is located on a side of the metal layer away from the optical diffraction metasurface; a nonlinear two-dimensional material layer, wherein the nonlinear two-dimensional material layer is located on a side of the first insulating layer away from the metal layer; a second insulating layer, wherein the second insulating layer is located on a side of the nonlinear two-dimensional material layer away from the first insulating layer; Plasmons, wherein the plasmons are located on a side of the second insulating layer away from the nonlinear two-dimensional material layer; A protective layer is located on a side of the plasmon away from the second insulating layer.
2. The all-optical nonlinear modulated metasurface diffraction optical computing device according to claim 1, in, The optical diffraction metasurface comprises a substrate layer, an active layer and a flat layer; The active layer is located on one side of the base layer, the active layer includes a plurality of active units arranged in an array, and the metal layer is located on a side of the flat layer away from the base layer; The material forming the active layer includes any one of silicon and oxide; The material forming the planar layer includes silicon dioxide; The flat layer satisfies any one of the following conditions: The flat layer is located between adjacent active units, and the thickness of the flat layer is equal to the thickness of the active unit; The flat layer includes a first flat portion and a second flat portion, the first flat portion is located between adjacent active units, the thickness of the first flat portion is equal to the thickness of the active unit, the second flat portion covers the first flat portion and the active unit, and the thickness of the second flat portion is less than or equal to 20 nm.
3. The all-optical nonlinear modulated metasurface diffraction optical computing device according to claim 2, in, The all-optical nonlinearly modulated metasurface diffraction optical computing device satisfies at least one of the following conditions: The thickness of the base layer is 100 to 250 μm; The thickness of the active layer is 100 to 300 nm; The material forming the metal layer includes at least one of gold and silver; The thickness of the metal layer is 1 to 5 nm; The material forming the first insulating layer includes hexagonal boron nitride; The thickness of the first insulating layer is 5-10 nm.
4. The all-optical nonlinear modulated metasurface diffraction optical computing device according to claim 2, in, The nonlinear two-dimensional material layer includes nonlinear two-dimensional material sublayers, and the number of the nonlinear two-dimensional material sublayers is 1-4; When the number of the nonlinear two-dimensional material sublayers is greater than one, a plurality of the nonlinear two-dimensional material sublayers are stacked; The materials forming the nonlinear two-dimensional material sublayer include black phosphorus, PdSe 2 、PdS 2 , InSe, MoS 2 , WS 2 ,WSe 2 Any of the following: The thickness of the nonlinear two-dimensional material sublayer is 0.5 to 20 nm.
5. The all-optical nonlinear modulated metasurface diffraction optical computing device according to any one of claims 1 to 4, in, When the number of the nonlinear two-dimensional material sublayers is greater than one, the materials of the plurality of nonlinear two-dimensional material sublayers are different from each other.
6. The all-optical nonlinear modulated metasurface diffraction optical computing device according to claim 4, in, When the material forming the active layer is silicon, the material forming the nonlinear two-dimensional material sublayer includes black phosphorus, PdSe 2 、PdS 2 , InSe; When the material forming the active layer is an oxide, the material forming the nonlinear two-dimensional material sublayer includes MoS 2 , WS 2 ,WSe 2 Any one of .
7. The all-optical nonlinear modulated metasurface diffraction optical computing device according to any one of claims 1 to 6, in, The all-optical nonlinearly modulated metasurface diffraction optical computing device satisfies at least one of the following conditions: The material forming the second insulating layer includes hexagonal boron nitride; The thickness of the second insulating layer is 1 to 5 nm; The material forming the plasmon includes WO 3-x , gold, silver; The material forming the plasmon includes at least one of nanowires and quantum dots; The length of the nanowire is 50 to 150 nm, and the width of the nanowire is 5 to 20 nm; The diameter of the quantum dots is less than 40 nm; The material forming the protective layer includes SiO 2 、Al 2 O 3 At least one of; The thickness of the protective layer is 15-50 nm.
8. A method for preparing a metasurface diffraction optical computing device with all-optical nonlinear modulation, in, The method comprises: Providing optical diffractive metasurfaces; forming a metal layer on one side of the optical diffractive metasurface; forming a first insulating layer on a side of the metal layer away from the optical diffractive metasurface; forming a nonlinear two-dimensional material layer on a side of the first insulating layer away from the metal layer; forming a second insulating layer on a side of the nonlinear two-dimensional material layer away from the first insulating layer; forming plasmons on a side of the second insulating layer away from the nonlinear two-dimensional material layer; A protection layer is formed on a side of the plasmon away from the second insulating layer.
9. The method according to claim 8, in, The optical diffraction metasurface is formed by: providing a composite structure having a substrate layer and an active material layer; forming a photoresist layer on a side of the active material layer away from the base layer; Performing patterning on the photoresist layer to obtain a structure having a patterned resist layer; Using the patterned glue layer as a mask, etching the structure having the patterned glue layer, so that the active material layer forms an active layer, wherein the active layer includes a plurality of active units arranged in an array, to obtain a structure having an active layer; Immersing the structure with the active layer in an acetone solution, removing the patterned adhesive layer using an ultrasonic bath, and obtaining a super surface with the active layer; A flat layer is formed on one side of the base layer so that the flat layer at least covers the area between adjacent active units to obtain an optical diffraction metasurface.
10. The method according to claim 8 or 9, in, The method satisfies at least one of the following conditions: The metal layer is formed by evaporation coating; The first insulating layer is formed on the metal layer by a fixed-point transfer method; The nonlinear two-dimensional material layer is formed on the first insulating layer by a fixed-point rotation method; The second insulating layer is formed on the nonlinear two-dimensional material layer by a fixed-point transfer method; The plasmon is formed by spin coating; Forming the plasmon includes: mixing the material for forming the plasmon with ethanol to prepare a coating solution, coating the coating solution on a side of the second insulating layer away from the nonlinear two-dimensional material layer, and drying to obtain the plasmon; The protective layer is formed by evaporation coating.
Citation Information
Patent Citations
Three-dimensional integrated metasurface device and preparation method and application thereof
CN111025463A
Optical graph neural classification network and method based on on-chip diffraction neural network
CN114519403A
On-chip optical diffraction calculation processor and all-optical image classification device
CN114815961A
Silicon light in-situ detection and modulation integrated device and preparation method and application thereof
CN115207152A
On-chip infrared sensing, storage and calculation integrated photoelectric device and preparation method thereof
CN115224156A