Composite neutron scintillator, preparation method therefor, and use thereof

By using the composite technology of perovskite materials and neutron absorbing materials in neutron scintillator, the problems of low light yield and high cost of existing neutron scintillator are solved, and efficient neutron detection and low-cost preparation are achieved. Suitable for large scientific installations.

WO2024198169A1PCT designated stage expired Publication Date: 2024-10-03SONGSHAN LAKE MATERIALS LAB
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/108261
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-07-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The existing neutron scintillator has low light yield, high cost, and complex preparation process, making it difficult to meet the needs of practical applications, especially in large scientific devices such as spallation neutron sources.

Method used

A composite neutron scintillator is used, including perovskite material powder and neutron absorbing material powder in an organic polymer matrix. The perovskite material is selected from Cs3Cu2I5 and CsCu2I3, and the neutron absorbing material is selected from Gd2O3 and 6LiF. Through ultrasonic stirring and It is prepared by solvent molding method to form a large-area scintillator film, which has good plasticity and low cost.

Benefits of technology

It achieves high light yield and short attenuation life, can effectively perform neutron/gamma discrimination, has a simple preparation process and low cost, and is suitable for neutron detectors and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023108261_03102024_PF_FP_ABST
    Figure CN2023108261_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Embodiments of the present application provide a composite neutron scintillator, a preparation method therefor, and use thereof, relating to the field of radiation detection. The composite neutron scintillator comprises: an organic polymer matrix; and a perovskite material powder and a neutron absorption material powder which are dispersed in the organic polymer matrix. The perovskite material is selected from at least one of Cs3Cu2I5 and CsCu2I3, and the neutron absorption material is selected from at least one of Gd2O3, 6LiF, and 10B2O3. The preparation method mainly comprises: uniformly grinding the organic polymer, the perovskite material and the neutron absorption material to obtain a mixed powder; stirring and mixing the mixed powder with a solvent until the mixed powder is dissolved; and pouring the mixture into a mold for molding. The composite neutron scintillator is characterized by high light yield, shorter decay life, and capability of effectively performing neutron / gamma discrimination, and features a simple preparation process and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

A composite neutron scintillator and its preparation method and application Technical Field

[0001] The present application relates to the field of radiation detection, and in particular to a composite neutron scintillator and a preparation method and application thereof. Background Art

[0002] Neutron detection plays an important role in basic physics, nuclear power, radioactive waste storage, homeland security, nuclear medicine and material analysis. Since neutrons are not charged and cannot be detected directly, indirect detection is usually achieved by using nuclides that can react with neutrons. Currently, most neutron detection uses 3 He neutron detectors are expensive. Neutron scintillators are an alternative to expensive 3 The best solution for He neutron detectors is to use the nuclides contained in the scintillator material or composite material. 6 Li, 10 B. 157 Gd and other materials absorb neutrons to produce high-energy particles, or use gamma rays to excite scintillator materials to generate photons, and collect signals through photomultiplier tubes and electronic systems to achieve neutron detection.

[0003] However, the existing neutron scintillators have low light yield and high cost, which makes it difficult to meet the actual application needs, especially for large scientific facilities such as spallation neutron sources. 6 Li glass:Ce (represented by GS20) has a short attenuation life and high transparency, but its light yield is low. Ce-doped potassium cryolite structure A2LiMX6:Ce (Cs2LiYCl6:Ce, Cs2LiYBr6:Ce, etc.) has a relatively high light yield, but its growth and preparation process is complex and the production cost is relatively high. The synthesis process of eutectic composite scintillators (LiF / SrF2:Ce, LiF / CaF2:Eu, etc.) mostly requires a high temperature and high pressure environment, and the preparation cost is also very high. In addition, Eu-doped eutectic scintillators have a long life and are difficult to apply to position neutron detectors. The more mature technology currently used is the use of ZnS:Ag / 6 LiF neutron scintillator screens have a high light yield, but a long decay lifetime. Furthermore, they are bonded together with adhesives, resulting in poor toughness and strength, making them susceptible to breakage. Therefore, a neutron scintillator with a simple preparation process and that meets the requirements of neutron detection is needed.

[0004] Summary of the Invention

[0005] The purpose of the embodiments of the present application is to provide a composite neutron scintillator and its preparation method and application, which has the characteristics of high light yield, short decay life, and can effectively perform neutron / gamma discrimination, and has a simple preparation process and low cost.

[0006] In a first aspect, an embodiment of the present application provides a composite neutron scintillator, which includes an organic polymer matrix, and a perovskite material powder and a neutron absorption material powder dispersed in the organic polymer matrix, wherein the perovskite material is selected from at least one of Cs3Cu2I5 and CsCu2I3, and the neutron absorption material is selected from Gd2O3, 6 LiF, 10 At least one of B2O3.

[0007] In the above technical solution, the luminescent material of the composite neutron scintillator is a perovskite material, which is composited with a neutron absorbing material and embedded in an organic polymer matrix to form a large-area scintillator film with good plasticity.

[0008] In one possible implementation, the perovskite material is Cs3Cu2I5, and the neutron absorption material is 6 LiF.

[0009] In a possible implementation, the mass ratio of the perovskite material powder to the organic polymer matrix is ​​0.05-1:1.

[0010] In the above technical solution, if the amount of perovskite material used is too large, the transparency of the formed scintillator will decrease, resulting in severe light scattering, reduced transmittance, and reduced final light yield or detection efficiency.

[0011] In a possible implementation, the mass ratio of the perovskite material powder to the neutron absorption material powder is 0.05-1:1.

[0012] In the above technical solution, if the amount of perovskite material relative to the neutron absorbing material is too small, the energy emitted by the neutron absorbing material cannot be completely absorbed, resulting in a decrease in the final light yield of the scintillator or the neutron detection efficiency.

[0013] In a possible implementation, the material of the organic polymer matrix is ​​selected from at least one of polymethyl methacrylate, polystyrene, polyvinyl chloride, and polyphenylene oxide.

[0014] In a possible implementation, the composite neutron scintillator has a thickness of 0.2-2 mm, a transmittance of 30%-90%, and a light yield of more than 20,000 photon / MeV.

[0015] In the above technical solution, only by ensuring the light transmittance of the scintillator can its detection efficiency be guaranteed.

[0016] In a second aspect, an embodiment of the present application provides a method for preparing the composite neutron scintillator provided in the first aspect, comprising the following steps:

[0017] Grinding the organic polymer, the perovskite material and the neutron absorbing material uniformly to obtain a mixed powder;

[0018] The mixed powder is stirred with the solvent until dissolved, and then poured into a mold for molding.

[0019] In the above technical solution, the preparation process is simple, and compared with traditional neutron scintillators, high-temperature preparation is not required, and the cost is low.

[0020] In one possible implementation, the solvent is selected from at least one of dichloromethane, N,N-dimethylformamide, dimethyl sulfoxide, and alcohols;

[0021] And / or, the molding method is to allow the solvent to evaporate naturally, or to place the mixture at 10-24° C. to allow the solvent to evaporate.

[0022] In one possible implementation, the method for preparing the perovskite material includes the following steps:

[0023] CuI, CsI and a stabilizer are added to a solvent and ultrasonically stirred until all of them are dissolved in the solvent to obtain a solution;

[0024] Allow the solvent in the solution to evaporate naturally until it is completely evaporated.

[0025] In a third aspect, an embodiment of the present application provides an application of the composite neutron scintillator provided in the first aspect. The composite neutron scintillator can be used as a neutron scintillation material for wave-shifting optical fibers, Anger cameras, imaging systems, and neutron detectors. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0027] FIG1 is a schematic structural diagram of a composite neutron scintillator provided in an embodiment of the present application;

[0028] FIG2 is a schematic diagram of a micrograph of the perovskite Cs3Cu2I5 crystal prepared in Example 1;

[0029] FIG3 is an XRD pattern of the perovskite Cs3Cu2I5 crystal obtained in Example 1;

[0030] FIG4 is a graph showing the fluorescence quantum efficiency of the perovskite material Cs3Cu2I5 prepared in Example 1;

[0031] FIG5 is a luminescence spectrum of the perovskite material Cs3Cu2I5 prepared in Example 1 under X-ray irradiation;

[0032] FIG6 is a comparison diagram of the light yield of the neutron scintillator of Example 1 and the commercial GS20 scintillator;

[0033] FIG7 is a neutron scintillator decay life curve of Example 1;

[0034] FIG8 is a neutron scintillator neutron gamma in Example 1 Identification chart;

[0035] FIG9 is a physical photograph of different neutron scintillator samples;

[0036] FIG10 shows the absorption spectra of different neutron scintillator samples. DETAILED DESCRIPTION

[0037] To make the purpose, technical solutions and advantages of the examples of the present application clearer, the technical solutions in the examples of the present application will be described clearly and completely below. Where specific conditions are not specified in the examples, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0038] The composite neutron scintillator and its preparation method and application in the embodiment of the present application are described in detail below.

[0039] Referring to FIG1 , an embodiment of the present application provides a composite neutron scintillator, which includes an organic polymer matrix, and a perovskite material powder and a neutron absorption material powder dispersed in the organic polymer matrix. The material of the organic polymer matrix is ​​selected from at least one of polymethyl methacrylate, polystyrene, polyvinyl chloride, and polyphenylene oxide; the perovskite material is selected from at least one of Cs3Cu2I5 and CsCu2I3; and the neutron absorption material is selected from Gd2O3, 6 LiF, 10 At least one of B2O3. The perovskite material is Cs3Cu2I5, and the neutron absorption material is 6 LiF.

[0040] In some embodiments of the present application, the mass ratio of the perovskite material powder to the organic polymer matrix is ​​generally 0.05-1:1, and can be optionally 0.5:1.

[0041] The mass ratio of the perovskite material powder to the neutron absorption material powder is 0.05-1:1, and can be optionally 1:1.

[0042] The mass ratio of the organic polymer matrix to the perovskite material powder and the neutron absorption material powder is 1:0.05-1:0.05-1. For example, the mass ratio of the three materials is: organic polymer / perovskite material / neutron absorption material = 2:1:1.

[0043] The smaller the particle size of the perovskite material powder and the neutron absorption material powder, the better the effect. Considering the comprehensive cost, the particle size of the perovskite material powder is generally 20-500μm, which is easy to prepare; the particle size of the neutron absorption material powder is 1-5μm, which can be purchased directly and obtained by grinding.

[0044] The composite neutron scintillator has a thickness of 0.2-2 mm, a transmittance of 30%-90%, and a light yield of more than 20,000 photon / MeV, illustratively, about 23,000 photon / MeV.

[0045] In addition, an embodiment of the present application provides a method for preparing the above-mentioned composite neutron scintillator, which comprises the following steps:

[0046] S1. Preparation of perovskite materials:

[0047] Adding CuI, CsI and a stabilizer to a solvent, stirring with ultrasound until all are dissolved in the solvent to obtain a solution, wherein the solvent may be N,N-dimethylformamide or dimethyl sulfoxide;

[0048] Allow the solvent in the solution to evaporate naturally until it is completely evaporated.

[0049] S2. Grinding the organic polymer, the perovskite material, and the neutron absorbing material uniformly to obtain a mixed powder;

[0050] S3. Stirring the mixed powder with a solvent until dissolved, wherein the solvent is selected from at least one of dichloromethane, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and alcohols. The mixed powder is dissolved in the solvent, subjected to ultrasonic dispersion treatment until uniformly dispersed, and poured into a mold for molding. The molding method is to allow the solvent to evaporate naturally, or to place the solvent at a certain temperature (e.g., 10-24°C) to evaporate the solvent.

[0051] The embodiment of the present application provides an application of the above-mentioned composite neutron scintillator, which can be used as a neutron scintillation material for wave-shifting optical fibers, Anger cameras, imaging systems, and neutron detectors.

[0052] The features and performance of the present application are further described in detail below with reference to the embodiments.

[0053] Example 1

[0054] This embodiment provides a neutron scintillator, the preparation process of which is as follows:

[0055] (1) Material preparation

[0056] S1. CuI, CsI and stabilizer are added to N,N-dimethylformamide (DMF) solvent in sequence.

[0057] Among them, the ratio of CuI and CsI is 2:3.

[0058] The stabilizer may be one of Tween 80, citric acid, oleic acid, ethylenediaminetetraacetic acid, polyvinylpyrrolidone, etc. In this embodiment, Tween 80 is used.

[0059] S2. Ultrasonicate the above solution until the solvent is completely dissolved.

[0060] S3. Pour the above solution into a culture dish and place it in a fume hood to evaporate naturally.

[0061] S4. After the solvent is evaporated, a dry solid powder is obtained.

[0062] The solid powder was tested. A micrograph of the solid powder is shown in FIG2 , and an XRD pattern is shown in FIG3 .

[0063] As can be seen from Figure 3, the phase structure of the crystal is Cs3Cu2I5 (corresponding to card PDF#45-0077), belonging to the Pbnm(62) space group.

[0064] The fluorescence quantum efficiency of the perovskite material Cs3Cu2I5 was tested using an integrating sphere with built-in BaSO4. The test graph is shown in FIG4 . After calculating the test results, the quantum efficiency was found to be 60.3%.

[0065] The luminescence spectrum of the perovskite material Cs3Cu2I5 under X-ray irradiation is shown in Figure 5. The luminescence peak is located at around 440nm, which is a typical blue luminescence (emitting bright blue light under X-ray irradiation). This luminescence band corresponds to the high quantum efficiency band of PMT, which is conducive to neutron detection.

[0066] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:1, pour into a mortar and grind.

[0067] (3) The powder after uniform grinding is dissolved in a solvent and poured into a mold for molding.

[0068] The type of solvent can be dichloromethane, DMF, DMSO, alcohols, etc. The solvent in this embodiment is dichloromethane.

[0069] The molding process can be a natural volatilization of the solvent, or volatilization at a certain temperature. The volatilization temperature is determined by the boiling point of the selected solvent. In this embodiment, natural volatilization is used.

[0070] The shape of the mold can be cylindrical, square, etc. In this embodiment, the mold used is cylindrical.

[0071] (4) After the molded sample is demoulded, the desired neutron scintillator is obtained.

[0072] The light yield comparison of this neutron scintillator and the commercial GS20 scintillator is shown in Figure 6, where the radiation source is 252 Cf, using commercial GS20 (whose light output is about 6000photons / MeV) as a calibration object, the test results show that the neutron scintillator Cs3Cu2I5 / 6 The light output of LiF / PMMA is about 4 times that of GS20, which is equivalent to a light output of about 23,000 photons / MeV.

[0073] The decay life curve of the neutron scintillator is shown in Figure 7. The radiation source is 252 Cf, the radiation decay lifetime is fitted and its decay lifetime is found to be about 253ns.

[0074] The neutron gamma The discrimination diagram is shown in Figure 8. The discrimination method uses image Enter the non-negative matrix method: First, under different radiation sources ( 60 Co, 252 Cf, 137 The system measures radiation reaction events (Cs, background (Bg)) and converts these events into image signals, which are then transformed into a two-dimensional image using an algorithm. The different shades of color in Figure 8 represent signals generated by different events. Figure 8 clearly shows how to distinguish between signals generated by neutron radiation and those generated by gamma radiation.

[0075] It can be seen that the neutron scintillator has a high light yield, a short lifespan, and a high neutron gamma discrimination rate (2×10 5 ).

[0076] Example 2

[0077] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:

[0078] (2) The generated powder is mixed with organic polymer PDMS (polydimethylsiloxane), 6 LiF powder, according to PDMS / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:1, pour into a mortar and grind.

[0079] (3) The powder after uniform grinding is dissolved in ethyl acetate solvent, poured into a cylindrical mold and placed at 60°C for volatilization and molding.

[0080] (4) After the molded sample is demoulded, the desired neutron scintillator is obtained.

[0081] Example 3

[0082] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:

[0083] (2) The generated powder was mixed with organic polymer PMMA powder and Gd2O3 powder in a mass ratio of PMMA / Gd2O3 / Cs3Cu2I5=2:0.1:1, and poured into a mortar and ground.

[0084] (3) The powder after uniform grinding is dissolved in dichloromethane solvent and poured into a cylindrical mold to evaporate naturally to form a shape.

[0085] Example 4

[0086] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:

[0087] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:0.1, pour into a mortar and grind.

[0088] (3) The powder after uniform grinding is dissolved in solvent dichloromethane and poured into a cylindrical mold to evaporate naturally to form a shape.

[0089] (4) After the molded sample is demoulded, the desired neutron scintillator is obtained.

[0090] Example 5

[0091] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:

[0092] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:0.3, pour into a mortar and grind.

[0093] (3) The powder after uniform grinding is dissolved in solvent dichloromethane and poured into a cylindrical mold to evaporate naturally to form a shape.

[0094] (4) After the molded sample is demoulded, the desired neutron scintillator is obtained.

[0095] Example 6

[0096] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:

[0097] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:0.5, pour into a mortar and grind.

[0098] (3) The powder after uniform grinding is dissolved in solvent dichloromethane and poured into a cylindrical mold to evaporate naturally to form a shape.

[0099] (4) After the molded sample is demoulded, the desired neutron scintillator is obtained.

[0100] Example 7

[0101] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:

[0102] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:2, pour into a mortar and grind.

[0103] (3) The powder after uniform grinding is dissolved in solvent dichloromethane and poured into a cylindrical mold to evaporate naturally to form a shape.

[0104] (4) After the molded sample is demoulded, the desired neutron scintillator is obtained.

[0105] Example 8

[0106] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:

[0107] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:1.5, pour into a mortar and grind.

[0108] (3) The powder after uniform grinding is dissolved in solvent dichloromethane and poured into a cylindrical mold to evaporate naturally to form a shape.

[0109] (4) After the molded sample is demoulded, the desired neutron scintillator is obtained.

[0110] Example 1, Example 4-6, and Example 8 are neutron scintillator samples prepared by using different addition ratios of perovskite materials. FIG9 shows the neutron scintillator samples prepared by using different addition ratios of perovskite materials Cs3Cu2I5 (PMMA / 6 Figure 9 shows the actual images of neutron scintillator samples with LiF / Cs3Cu2I5=2:1:0.1, 2:1:0.3, 2:1:0.5, 2:1:1, and 2:1:1.5. As can be seen from Figure 9, excessive addition of perovskite material will reduce the transparency of the scintillator.

[0111] Example 1, Example 4-6, and Example 8 are neutron scintillator samples prepared by using different addition ratios of perovskite materials. FIG10 shows different addition ratios of perovskite materials Cs3Cu2I5 (PMMA / 6 Figure 10 shows the absorption spectra of neutron scintillator samples with LiF / Cs3Cu2I5 = 2:1:0.1, 2:1:0.3, 2:1:0.5, 2:1:1, and 2:1:1.5. As can be seen from Figure 10, as the Cs3Cu2I5 content in the composite neutron scintillator increases, its transmittance decreases.

[0112] In summary, the composite neutron scintillator of the embodiment of the present application has the characteristics of high light yield, short decay lifetime, and can effectively perform neutron / gamma discrimination, and has a simple preparation process and low cost.

[0113] The above description is merely an embodiment of the present application and is not intended to limit the scope of protection of the present application. For those skilled in the art, various modifications and variations of the present application are possible. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A composite neutron scintillator, It is characterized in that The invention comprises an organic polymer matrix, and a perovskite material powder and a neutron absorption material powder dispersed in the organic polymer matrix, wherein the perovskite material is selected from Cs 3 Cu 2 I 5 , CsCu 2 I 3 At least one of the neutron absorbing material is selected from Gd 2 O 3 , 6 LiF, 10 B 2 O 3 At least one of .

2. The composite neutron scintillator according to claim 1, It is characterized in that The perovskite material is Cs 3 Cu 2 I 5 , the neutron absorbing material is 6 LiF.

3. The composite neutron scintillator according to claim 1, It is characterized in that The mass ratio of the perovskite material powder to the organic polymer matrix is ​​0.05-1:

1.

4. The composite neutron scintillator according to claim 1, It is characterized in that The mass ratio of the perovskite material powder to the neutron absorption material powder is 0.05-1:

1.

5. The composite neutron scintillator according to claim 1, It is characterized in that The material of the organic polymer matrix is ​​selected from at least one of polymethyl methacrylate, polystyrene, polyvinyl chloride and polyphenylene oxide.

6. The composite neutron scintillator according to claim 1, It is characterized in that The composite neutron scintillator has a thickness of 0.2-2 mm, a light transmittance of 30%-90%, and a light yield of more than 20,000 photon / MeV.

7. A method for preparing the composite neutron scintillator according to claim 1, It is characterized in that It includes the following steps: Grinding the organic polymer, the perovskite material and the neutron absorbing material uniformly to obtain a mixed powder; The mixed powder is stirred and mixed with a solvent until dissolved, and poured into a mold for molding.

8. The method for preparing the composite neutron scintillator according to claim 7, It is characterized in that The solvent is selected from at least one of dichloromethane, N,N-dimethylformamide, dimethyl sulfoxide, and alcohols; And / or, the molding method is to allow the solvent to evaporate naturally, or to place the mixture at 10-24° C. to allow the solvent to evaporate.

9. The method for preparing the composite neutron scintillator according to claim 7, It is characterized in that The preparation method of the perovskite material comprises the following steps: Adding CuI, CsI and a stabilizer into a solvent, and stirring with ultrasound until all of them are dissolved in the solvent, to obtain a solution; The solvent in the solution is allowed to evaporate naturally until it is completely evaporated.

10. A use of the composite neutron scintillator as claimed in claim 1, It is characterized in that The composite neutron scintillator can be used as a neutron scintillation material for wave-shifting optical fibers, Anger cameras, imaging systems, and neutron detectors.

Citation Information

Patent Citations

  • Neutron and gamma ray monitor

    CN101443679A

  • Novel perovskite-like structure scintillator for neutron detection as well as preparation method and application of novel perovskite-like structure scintillator

    CN114411252A

  • Preparation method and application of lead-free perovskite polymer scintillator

    CN114774109A

  • Hydrogen-rich two-dimensional perovskite fast neutron scintillator material and preparation method and application thereof

    CN115074116A

  • Method for improving detection performance of powdery scintillator on high-energy rays

    CN115639587A