Composite neutron scintillator and preparation method and application thereof
By using the composite technology of perovskite and neutron absorbing materials in neutron scintillator, the problems of low light yield and high cost of existing neutron scintillator are solved, and efficient neutron detection and gamma screening are achieved. The preparation process is simple and suitable for large scientific devices.
Patent Information
- Application Number
- CN202310324742.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
The existing neutron scintillator has low light yield, high cost, and complex preparation process, making it difficult to meet the needs of practical applications, especially in large scientific devices such as spallation neutron sources.
A composite neutron scintillator is used, including an organic polymer matrix, perovskite material powder and neutron absorption material powder. The perovskite material is selected from Cs3Cu2I5 and CsCu2I3, and the neutron absorption material is selected from Gd2O3 and 6LiF. Through ultrasonic stirring and solvent It is prepared by molding technology to form a large-area scintillator film, which has good plasticity and low cost.
It achieves high light yield and short attenuation lifetime, can effectively perform neutron/gamma discrimination, has a simple preparation process and low cost, and is suitable for neutron detectors and other applications.
Smart Images

Figure CN118725845A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of radiation detection, and in particular, to a composite neutron scintillator and a preparation method and application thereof. Background Art
[0002] Neutron detection plays an important role in basic physics, nuclear power, radioactive waste storage, homeland security, nuclear medicine and material analysis. Since neutrons are not charged and cannot be detected directly, indirect detection of neutrons is usually achieved by using nuclides that can react with neutrons. Currently, most neutron detection uses 3 He neutron detectors are expensive. Neutron scintillators are an alternative to expensive 3 The best solution for He neutron detectors is to use the nuclides contained in the scintillator material or composite material. 6 Li, 10 B. 157 Gd and other materials absorb neutrons to produce high-energy particles, or use gamma rays to excite scintillator materials to produce photons, and collect signals through photomultiplier tubes and electronic systems to achieve neutron detection.
[0003] However, the existing neutron scintillators have low light yield and high cost, which can hardly meet the actual application needs, especially for large scientific facilities such as spallation neutron sources. 6 Li glass:Ce (represented by GS20) has a short attenuation life and high transparency, but its light yield is low. Ce-doped potassium cryolite structure A2LiMX6:Ce (Cs2LiYCl6:Ce, Cs2LiYBr6:Ce, etc.) has a relatively high light yield, but its growth and preparation process is complex and the production cost is relatively high. The synthesis process of eutectic composite scintillators (LiF / SrF2:Ce, LiF / CaF2:Eu, etc.) mostly requires a high temperature and high pressure environment, and the preparation cost is also very high. In addition, the Eu-doped eutectic scintillator has a long life and is difficult to apply to position neutron detectors. The more mature technology currently used is the use of ZnS:Ag / 6 The LiF neutron scintillator screen has a relatively high light yield, but a relatively long attenuation life, and is bonded with an adhesive, so it has poor toughness and strength and is easily broken. Therefore, a neutron scintillator with a simple preparation process and meeting the requirements of neutron detection is needed. Summary of the invention
[0004] The purpose of the embodiments of the present application is to provide a composite neutron scintillator and a preparation method and application thereof. The neutron scintillator has the characteristics of high light yield, short decay life, and can effectively perform neutron / gamma discrimination, and the preparation process is simple and the cost is low.
[0005] In a first aspect, an embodiment of the present application provides a composite neutron scintillator, which includes an organic polymer matrix, and a perovskite material powder and a neutron absorption material powder dispersed in the organic polymer matrix, wherein the perovskite material is selected from at least one of Cs3Cu2I5 and CsCu2I3, and the neutron absorption material is selected from Gd2O3, 6 LiF, 10 At least one of B2O3.
[0006] In the above technical solution, the luminescent material of the composite neutron scintillator is a perovskite material, which is composited with a neutron absorbing material and embedded in an organic polymer matrix to form a large-area scintillator film with good plasticity.
[0007] In a possible implementation, the perovskite material is Cs3Cu2I5, and the neutron absorption material is 6 LiF.
[0008] In a possible implementation, the mass ratio of the perovskite material powder to the organic polymer matrix is 0.05-1:1.
[0009] In the above technical solution, if the amount of perovskite material used is too large, the transparency of the formed scintillator will decrease, resulting in severe light scattering, reduced transmittance, and reduced final light yield or detection efficiency.
[0010] In a possible implementation, the mass ratio of the perovskite material powder to the neutron absorption material powder is 0.05-1:1.
[0011] In the above technical solution, if the amount of perovskite material is too small relative to the neutron absorbing material, the energy emitted by the neutron absorbing material cannot be completely absorbed, resulting in a decrease in the final light yield of the scintillator or the neutron detection efficiency.
[0012] In a possible implementation, the material of the organic polymer matrix is selected from at least one of polymethyl methacrylate, polystyrene, polyvinyl chloride and polyphenylene oxide.
[0013] In a possible implementation, the composite neutron scintillator has a thickness of 0.2-2 mm, a light transmittance of 30%-90%, and a light yield of more than 20,000 photon / MeV.
[0014] In the above technical solution, the light transmittance of the scintillator is guaranteed to ensure its detection efficiency.
[0015] In a second aspect, an embodiment of the present application provides a method for preparing the composite neutron scintillator provided in the first aspect, comprising the following steps:
[0016] Grinding the organic polymer, the perovskite material and the neutron absorbing material uniformly to obtain a mixed powder;
[0017] The mixed powder is stirred with the solvent until dissolved, and then poured into a mold for forming.
[0018] In the above technical solution, the preparation process is simple, and compared with the traditional neutron scintillator, it does not require high-temperature preparation and has low cost.
[0019] In a possible implementation, the solvent is selected from at least one of dichloromethane, N,N-dimethylformamide, dimethyl sulfoxide, and alcohols;
[0020] And / or, the molding method is to allow the solvent to evaporate naturally, or to place the mixture at 10-24°C to allow the solvent to evaporate.
[0021] In a possible implementation, the method for preparing the perovskite material includes the following steps:
[0022] Adding CuI, CsI and a stabilizer into a solvent, stirring with ultrasound until all of them are dissolved in the solvent, to obtain a solution;
[0023] Allow the solvent in the solution to evaporate naturally until it is completely evaporated.
[0024] In a third aspect, an embodiment of the present application provides an application of the composite neutron scintillator provided in the first aspect, and the composite neutron scintillator can be used as a neutron scintillation material for wave-shifting optical fiber, Anger camera, imaging system, and neutron detector. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 A schematic diagram of the structure of a composite neutron scintillator provided in an embodiment of the present application;
[0027] Figure 2 Schematic diagram of a micrograph of the perovskite Cs3Cu2I5 crystal prepared in Example 1;
[0028] Figure 3 XRD pattern of the perovskite Cs3Cu2I5 crystal prepared in Example 1;
[0029] Figure 4 This is a fluorescence quantum efficiency diagram of the perovskite material Cs3Cu2I5 prepared in Example 1;
[0030] Figure 5The luminescence spectrum of the perovskite material Cs3Cu2I5 prepared in Example 1 under X-ray irradiation;
[0031] Figure 6 This is a comparison chart of the light yield of the neutron scintillator of Example 1 and the commercial GS20 scintillator;
[0032] Figure 7 is the neutron scintillator decay life curve of Example 1;
[0033] Figure 8 The neutron scintillator neutron gamma Identification chart;
[0034] Fig. 9 The following are the actual photos of different neutron scintillator samples;
[0035] Fig.10 Absorption spectra of different neutron scintillator samples. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0037] The composite neutron scintillator and its preparation method and application according to the embodiment of the present application are described in detail below.
[0038] Please see Figure 1 The embodiment of the present application provides a composite neutron scintillator, which includes an organic polymer matrix, and a perovskite material powder and a neutron absorption material powder dispersed in the organic polymer matrix. The material of the organic polymer matrix is selected from at least one of polymethyl methacrylate, polystyrene, polyvinyl chloride and polyphenylene oxide; the perovskite material is selected from at least one of Cs3Cu2I5 and CsCu2I3; the neutron absorption material is selected from Gd2O3, 6 LiF, 10 At least one of B2O3. The perovskite material is Cs3Cu2I5, and the neutron absorption material is 6 LiF.
[0039] In some embodiments of the present application, the mass ratio of the perovskite material powder to the organic polymer matrix is generally 0.05-1:1, and can be optionally 0.5:1.
[0040] The mass ratio of the perovskite material powder to the neutron absorption material powder is 0.05-1:1, and can be optionally 1:1.
[0041] The mass ratio of the organic polymer matrix to the perovskite material powder and the neutron absorption material powder is 1:0.05-1:0.05-1. Exemplarily, the mass ratio of the three materials is: organic polymer / perovskite material / neutron absorption material=2:1:1.
[0042] The smaller the particle size of the perovskite material powder and the neutron absorption material powder, the better the effect. Considering the comprehensive cost, the particle size of the perovskite material powder is generally 20-500μm, which is easy to prepare; the particle size of the neutron absorption material powder is 1-5μm, which can be directly purchased and obtained by grinding.
[0043] The composite neutron scintillator has a thickness of 0.2-2 mm, a light transmittance of 30%-90%, and a light yield of more than 20,000 photon / MeV, illustratively, about 23,000 photon / MeV.
[0044] In addition, an embodiment of the present application provides a method for preparing the above-mentioned composite neutron scintillator, which comprises the following steps:
[0045] S1. Preparation of perovskite materials:
[0046] Adding CuI, CsI and a stabilizer to a solvent, stirring with ultrasound until all of them are dissolved in the solvent, to obtain a solution, wherein the solvent may be N,N-dimethylformamide or dimethyl sulfoxide;
[0047] Allow the solvent in the solution to evaporate naturally until it is completely evaporated.
[0048] S2, grinding the organic polymer, the perovskite material and the neutron absorbing material uniformly to obtain a mixed powder;
[0049] S3. Stirring the mixed powder and the solvent until dissolved, the solvent is selected from at least one of dichloromethane, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and alcohols. The mixed powder is dissolved in the solvent, subjected to ultrasonic dispersion treatment until uniformly dispersed, and poured into a mold for molding. The molding method is to allow the solvent to evaporate naturally, or to place the solvent at a certain temperature (such as 10-24°C) to evaporate.
[0050] The embodiment of the present application provides an application of the above-mentioned composite neutron scintillator, and the composite neutron scintillator can be used as a neutron scintillation material for wave-shifting optical fiber, Anger camera, imaging system, and neutron detector.
[0051] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0052] Example 1
[0053] This embodiment provides a neutron scintillator, and the preparation process thereof is as follows:
[0054] (1) Material preparation
[0055] S1. Add CuI, CsI and stabilizer into N,N-dimethylformamide (DMF) solvent in sequence.
[0056] Among them, the ratio of CuI and CsI is 2:3.
[0057] The stabilizer may be one of Tween 80, citric acid, oleic acid, ethylenediaminetetraacetic acid, polyvinylpyrrolidone, etc., and in this embodiment, Tween 80 is used.
[0058] S2. Ultrasonicate the above solution until the solvent is completely dissolved.
[0059] S3. Pour the above solution into a culture dish and place it in a fume hood to evaporate naturally.
[0060] S4. After the solvent is evaporated, a dry solid powder is obtained.
[0061] The solid powder is tested, and the microscopic photo of the solid powder is as follows: Figure 2 As shown, the XRD spectrum is Figure 3 shown.
[0062] from Figure 3 It can be seen that the phase structure of the crystal is Cs3Cu2I5 (corresponding to card PDF#45-0077), belonging to the Pbnm(62) space group.
[0063] The fluorescence quantum efficiency of the perovskite material Cs3Cu2I5 was tested by an integrating sphere with built-in BaSO4. The test chart is as follows Figure 4 As shown, after calculating the test results, the quantum efficiency is obtained to be 60.3%.
[0064] The luminescence spectrum of the perovskite material Cs3Cu2I5 under X-ray irradiation is as follows Figure 5 As shown, the luminescence peak is located at about 440nm, which is a typical blue luminescence (emitting bright blue light under X-ray irradiation). This luminescence band corresponds to the high quantum efficiency band of PMT, which is beneficial to neutron detection.
[0065] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:1 and pour into a mortar and grind.
[0066] (3) The uniformly ground powder is dissolved in a solvent and poured into a mold for molding.
[0067] The type of solvent can be dichloromethane, DMF, DMSO, alcohols, etc. The solvent in this embodiment is dichloromethane.
[0068] The molding process can be a natural volatilization of the solvent, or volatilization at a certain temperature. The volatilization temperature is determined by the boiling point of the selected solvent. In this embodiment, natural volatilization is used.
[0069] The shape of the mold can be cylindrical, square, etc. In this embodiment, the mold used is cylindrical.
[0070] (4) After the molded sample is demolded, the desired neutron scintillator is obtained.
[0071] The light yield comparison between this neutron scintillator and the commercial GS20 scintillator is shown in the figure below. Figure 6 As shown, the radiation source is 252 Cf, using commercial GS20 (whose light output is about 6000photons / MeV) as a calibration object, the test results show that the neutron scintillator Cs3Cu2I5 / 6 The light output of LiF / PMMA is about 4 times that of GS20, which is equivalent to a light output of about 23,000 photons / MeV.
[0072] The decay life curve of the neutron scintillator is as follows Figure 7 As shown, the radiation source is 252 Cf, the radiation decay lifetime is fitted and the decay lifetime is found to be about 253ns.
[0073] The neutron gamma Identification chart Figure 8 As shown, the identification method uses image Enter the non-negative matrix method: First, under different radiation sources ( 60 Co, 252 Cf, 137 Cs, background (Bg)) measures radiation reaction events, forms image signals from the measured events, and forms a two-dimensional image through an algorithm. Figure 8 Different shades of color represent signals generated by different events. Figure 8 The signals formed by neutron radiation and those formed by gamma radiation can be easily distinguished.
[0074] It can be seen that the neutron scintillator has a high light yield, a short life, and a high neutron gamma discrimination rate (2×10 5 ).
[0075] Example 2
[0076] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:
[0077] (2) The generated powder is mixed with organic polymer PDMS (polydimethylsiloxane), 6 LiF powder, according to PDMS / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:1 and pour into a mortar and grind.
[0078] (3) The uniformly ground powder is dissolved in ethyl acetate, poured into a cylindrical mold and placed at 60° C. for volatilization and molding.
[0079] (4) After the molded sample is demolded, the desired neutron scintillator is obtained.
[0080] Example 3
[0081] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:
[0082] (2) Mix the generated powder with organic polymer PMMA powder and Gd2O3 powder in a mass ratio of PMMA / Gd2O3 / Cs3Cu2I5=2:0.1:1, pour into a mortar and grind.
[0083] (3) The uniformly ground powder is dissolved in dichloromethane solvent and poured into a cylindrical mold to evaporate naturally.
[0084] Example 4
[0085] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:
[0086] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:0.1 and pour into a mortar and grind.
[0087] (3) The uniformly ground powder is dissolved in dichloromethane solvent and poured into a cylindrical mold to evaporate naturally.
[0088] (4) After the molded sample is demolded, the desired neutron scintillator is obtained.
[0089] Example 5
[0090] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:
[0091] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:0.3 and pour into a mortar and grind.
[0092] (3) The uniformly ground powder is dissolved in dichloromethane solvent and poured into a cylindrical mold to evaporate naturally.
[0093] (4) After the molded sample is demolded, the desired neutron scintillator is obtained.
[0094] Example 6
[0095] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:
[0096] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:0.5 and pour into a mortar and grind.
[0097] (3) The uniformly ground powder is dissolved in dichloromethane solvent and poured into a cylindrical mold to evaporate naturally.
[0098] (4) After the molded sample is demolded, the desired neutron scintillator is obtained.
[0099] Example 7
[0100] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:
[0101] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6 Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:2 and pour into a mortar and grind.
[0102] (3) The uniformly ground powder is dissolved in dichloromethane solvent and poured into a cylindrical mold to evaporate naturally.
[0103] (4) After the molded sample is demolded, the desired neutron scintillator is obtained.
[0104] Example 8
[0105] This embodiment provides a neutron scintillator, and its preparation process is different from that of embodiment 1 in that:
[0106] (2) The generated powder is mixed with organic polymer PMMA powder, 6 LiF powder, according to PMMA / 6Mix LiF / Cs3Cu2I5 in a mass ratio of 2:1:1.5 and pour into a mortar and grind.
[0107] (3) The uniformly ground powder is dissolved in dichloromethane solvent and poured into a cylindrical mold to evaporate naturally.
[0108] (4) After the molded sample is demolded, the desired neutron scintillator is obtained.
[0109] Embodiment 1, Embodiment 4-6, and Embodiment 8 are neutron scintillator samples prepared by using different addition ratios of perovskite materials. Fig. 9 Different addition ratios of perovskite material Cs3Cu2I5 (PMMA / 6 Physical picture of neutron scintillator samples of LiF / Cs3Cu2I5=2:1:0.1、2:1:0.3、2:1:0.5、2:1:1、2:1:1.5). Fig. 9 It can be seen that if the addition ratio of perovskite material is too large, the transparency of the scintillator will be reduced.
[0110] Embodiment 1, Embodiment 4-6, and Embodiment 8 are neutron scintillator samples prepared by using different addition ratios of perovskite materials. Fig.10 Different addition ratios of perovskite material Cs3Cu2I5 (PMMA / 6 The absorption spectra of neutron scintillator samples with LiF / Cs3Cu2I5=2:1:0.1, 2:1:0.3, 2:1:0.5, 2:1:1, 2:1:1.5). Fig.10 It can be seen that with the increase of Cs3Cu2I5 content in the composite neutron scintillator, its transmittance becomes lower and lower.
[0111] In summary, the composite neutron scintillator of the embodiment of the present application has the characteristics of high light yield, short decay life, and can effectively perform neutron / gamma discrimination, and has a simple preparation process and low cost.
[0112] The above description is only an embodiment of the present application and is not intended to limit the protection scope of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A composite neutron scintillator, characterized in that: The invention comprises an organic polymer matrix, and a perovskite material powder and a neutron absorption material powder dispersed in the organic polymer matrix, wherein the perovskite material is selected from at least one of Cs3Cu2I5 and CsCu2I3, and the neutron absorption material is selected from Gd2O3, 6 LiF, 10 At least one of B2O3.
2. The composite neutron scintillator according to claim 1, characterized in that: The perovskite material is Cs3Cu2I5, and the neutron absorption material is 6 LiF.
3. The composite neutron scintillator according to claim 1, characterized in that: The mass ratio of the perovskite material powder to the organic polymer matrix is 0.05-1:
1.
4. The composite neutron scintillator according to claim 1, characterized in that: The mass ratio of the perovskite material powder to the neutron absorption material powder is 0.05-1:
1.
5. The composite neutron scintillator according to claim 1, characterized in that: The material of the organic polymer matrix is selected from at least one of polymethyl methacrylate, polystyrene, polyvinyl chloride and polyphenylene oxide.
6. The composite neutron scintillator according to claim 1, characterized in that: The composite neutron scintillator has a thickness of 0.2-2 mm, a light transmittance of 30%-90%, and a light yield of more than 20,000 photon / MeV.
7. A method for preparing a composite neutron scintillator according to claim 1, characterized in that: It includes the following steps: Grinding the organic polymer, the perovskite material and the neutron absorbing material uniformly to obtain a mixed powder; The mixed powder is stirred and mixed with a solvent until dissolved, and poured into a mold for molding.
8. The method for preparing a composite neutron scintillator according to claim 7, characterized in that: The solvent is selected from at least one of dichloromethane, N,N-dimethylformamide, dimethyl sulfoxide, and alcohols; And / or, the molding method is to allow the solvent to evaporate naturally, or to place the mixture at 10-24° C. to allow the solvent to evaporate.
9. The method for preparing a composite neutron scintillator according to claim 7, characterized in that: The preparation method of the perovskite material comprises the following steps: Adding CuI, CsI and a stabilizer into a solvent, and stirring with ultrasound until all of them are dissolved in the solvent, to obtain a solution; The solvent in the solution is allowed to evaporate naturally until it is completely evaporated.
10. An application of the composite neutron scintillator according to claim 1, characterized in that: The composite neutron scintillator can be used as a neutron scintillation material for wave-shifting optical fibers, Anger cameras, imaging systems, and neutron detectors.
Citation Information
Cited By
Preparation method of meter-scale oversized boron nitride neutron scintillation screen