Negative electrode material, preparation method thereof and electrochemical device

By using silicon-based material composite negative electrode material that regulates particle size and structure in electrochemical devices, the problem of volume expansion and fragmentation during the circulation of silicon-based materials is solved, and the circulation and rate performance of electrochemical devices is improved.

CN118943326AActive Publication Date: 2024-11-12NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202410992849.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The volume expansion and fragmentation of silicon-based materials during the circulation process in an electrochemical device leads to the destruction and growth of the solid electrolyte interface film, affecting the circulation and rate performance of the electrochemical device.

Method used

A negative electrode material is adopted, including a first silicon-based material, a second silicon-based material, passivated lithium powder and an organic polymer. By regulating the particle size and structure of each material, a composite structure of a core, a carbon layer and a lithium salt layer is formed. , secondary granulation is carried out in combination with polymer adhesive, to reduce the specific surface area of ​​silicon carbon particles and inhibit the growth of SEI film.

Benefits of technology

It effectively alleviates the fragmentation and powderization of silicon carbon anode material during the circulation process, reduces the volume expansion rate after cycling of the electrochemical device, and improves the circulation and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943326A_ABST
    Figure CN118943326A_ABST
Patent Text Reader

Abstract

The invention provides a negative electrode material, a preparation method thereof and an electrochemical device. The negative electrode material comprises a first silicon-based material, a second silicon-based material, passivated lithium powder and an organic polymer; the particle size Dv50 of the first silicon-based material is A, A is larger than or equal to 2 micrometers and smaller than or equal to 5 micrometers, and the particle size Dv50 of the second silicon-based material is B, alt; 20A, 20B; the particle size Dv50 of the passivated lithium powder is C, and C is more than or equal to 0.01 mu m and less than or equal to 0.1 mu m. According to the negative electrode material provided by the invention, the advantages of long cycle performance of the first silicon-based material and high rate performance of the second silicon-based material can be combined, fragmentation and pulverization of the silicon-carbon negative electrode material in the cycle process can be effectively relieved, growth of an SEI film is inhibited, and the volume expansion rate of an electrochemical device after circulation is reduced; and the cycle performance and the rate capability of the electrochemical device are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical energy storage, and particularly to a negative electrode material, a preparation method thereof, and an electrochemical device. Background Art

[0002] Graphite is the most widely used negative electrode material, which has advantages such as high efficiency and stable charge-discharge platform. However, its low specific capacity per gram hinders the further application of graphite. Compared with graphite, elemental silicon is considered an ideal negative electrode material that can replace graphite due to its high theoretical specific capacity and suitable working voltage.

[0003] However, the volume of silicon expands by up to 400% after lithium intercalation. The repeated expansion and contraction of silicon-based materials during cycling can lead to the destruction and growth of the solid electrolyte interface (SEI) film and the fragmentation of silicon-based negative electrode particles, resulting in huge electrode expansion and rapid capacity decay, affecting the cycling performance and rate performance of the electrochemical device and restricting the large-scale application of silicon negative electrode materials in electrochemical devices. Summary of the Invention

[0004] The object of the present invention is to provide a negative electrode material to improve the cycling performance and rate performance of an electrochemical device.

[0005] The first aspect of the present application provides a negative electrode material, which includes: a first silicon-based material, a second silicon-based material, passivated lithium powder, and an organic polymer; the Dv50 of the first silicon-based material is A, 2 μm ≤ A ≤ 5 μm, the Dv50 of the second silicon-based material is B, where 4B < A < 20B; the Dv50 of the passivated lithium powder is C, 0.01 μm ≤ C ≤ 0.1 μm.

[0006] In an embodiment of the present application, the first silicon-based negative electrode material and the second silicon-based material each include a core, a carbon layer outside the core, and a lithium salt layer outside the carbon layer.

[0007] In an embodiment of the present application, the negative electrode material satisfies at least one of the following: (1) the core includes at least one of silicon-carbon particles or silicon-oxygen particles; (2) the lithium salt includes at least one of LiF or Li 2 CO 3 ; (3) based on the mass of the first silicon-based material, the mass percentage content of the carbon layer of the first silicon-based particles is 1% to 5.2%, and the mass percentage content of the lithium salt layer is 0.53% to 2.1%; (4) based on the mass of the second silicon-based material, the mass percentage content of the carbon layer of the second silicon-based particles is 1% to 5.2%, and the mass percentage content of the lithium salt layer is 0.53% to 2.1%.

[0008] In one embodiment of the present application, the average size of silicon grains in the core of the first silicon-based material is a, and the average size of silicon grains in the core of the second silicon-based material is b; 1nm≤a≤1.5nm, 1.5nm≤b≤2nm, and a<b.

[0009] In one embodiment of the present application, 0.1 μm≤B≤0.5 μm.

[0010] In one embodiment of the present application, the mass of the first silicon-based material is m 1 g, the mass of the second silicon-based material is m 2 g, the mass of the passivated lithium powder is m 3 g, mass ratio meets: m 1 :m 2 :m 3 =100:10 to 40:0.5 to 5; based on the mass of the negative electrode material, the mass percentage of the organic polymer is 3% to 7%.

[0011] In one embodiment of the present application, the negative electrode material satisfies at least one of the following: (1) the Dv50 of the negative electrode material is 6 μm to 10 μm; (2) the Dv90 of the negative electrode material is less than or equal to 30 μm; (3) the organic polymer includes polyurethane; (4) based on the mass of the negative electrode material, the mass percentage of silicon element is 40% to 50%.

[0012] The second aspect of the present application provides a method for preparing the negative electrode material according to the first aspect of the present application, which comprises:

[0013] Providing a core of a first silicon-based material, carbon-coating the core to obtain a first intermediate, dispersing the first intermediate in water to obtain a first dispersion, adding an aqueous solution of a lithium source substance to the first dispersion to obtain a second dispersion, fully dispersing and stirring, and drying in an oven to obtain a first silicon-based material;

[0014] Providing a core of a second silicon-based material, carbon-coating the core to obtain a first intermediate, dispersing the first intermediate in water to obtain a first dispersion, adding an aqueous solution of a lithium source material to the first dispersion to obtain a second dispersion, fully dispersing and stirring, and drying in an oven to obtain a second silicon-based material;

[0015] The first silicon-based material, the second silicon-based material and the passivated lithium powder are dispersed and then deionized water is added to obtain a third dispersion; the polymer is dispersed in water to obtain a fourth dispersion, the fourth dispersion is added to the third dispersion, mixed and fully stirred, and the negative electrode material is obtained by spray drying.

[0016] The third aspect of the present application provides an electrochemical device, which includes a positive electrode sheet, a negative electrode sheet, and an electrolyte. The negative electrode sheet includes a negative electrode active material layer, and the negative electrode active material layer includes the negative electrode material described in the first aspect of the present application.

[0017] In one embodiment of the present application, the electrolyte includes at least one of lithium bis(trifluoromethylsulfonyl)imide or lithium bis(fluorosulfonyl)imide;

[0018] Based on the mass of the electrolyte, the mass percentage content of lithium bis(trifluoromethylsulfonyl)imide and / or lithium bis(fluorosulfonyl)imide is 0.1% to 5%.

[0019] The fourth aspect of the present application provides an electronic device, which includes the electrochemical device provided in the third aspect of the present application.

[0020] Advantageous effects of the embodiments of the present invention:

[0021] The present application provides a negative electrode material, which includes: a first silicon-based material, a second silicon-based material, passivated lithium powder, and an organic polymer; the Dv50 of the first silicon-based material is A, 2 μm ≤ A ≤ 5 μm, the Dv50 of the second silicon-based material is B, where 4B < A < 20B; the Dv50 of the passivated lithium powder is C, 0.01 μm ≤ C ≤ 0.1 μm. The negative electrode material includes a first silicon-based material, a second silicon-based material, passivated lithium powder, and an organic polymer, which can combine the advantages of the long cycle performance of the first silicon-based material and the high rate performance of the second silicon-based material, can effectively alleviate the fragmentation and pulverization of the silicon-carbon negative electrode material during the cycle and inhibit the growth of SEI, reduce the volume expansion rate after cycling of the electrochemical device, and improve the cycle performance and rate performance of the electrochemical device.

[0022] Of course, it is not necessary for any product or method implementing the present invention to achieve all the above-mentioned advantages simultaneously. Description of the Drawings

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following will briefly introduce the drawings required for the description of the embodiments or the prior art. Obviously, the following drawings are only some embodiments of the present invention, and those of ordinary skill in the art can also obtain other embodiments based on these drawings.

[0024] Figure 1 Schematic structural diagram of the negative electrode material prepared for Example 1-1;

[0025] Figure 2 Comparison chart of the cycle performance of the lithium-ion batteries of Example 2-1 and Comparative Examples 4 to 6 at 25°C;

[0026] Figure 3 This is a comparison chart of the cycle performance of the lithium-ion batteries of Example 2-1 and Comparative Examples 4 to 6 at 45°C;

[0027] Figure 4 It is a comparison diagram of the expansion rates of the lithium ion batteries of Example 2-1 and Comparative Examples 4 to 6 at 25° C.;

[0028] Figure 5 It is a comparison diagram of the expansion rates of the lithium ion batteries of Example 2-1 and Comparative Examples 4 to 6 at 45° C.;

[0029] Figure 6 1 is a comparison chart of the capacity retention rates of the lithium-ion batteries of Example 2-1 and Comparative Examples 4 to 6 at different rates at 25° C. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0031] It should be noted that in the specific embodiments of the present application, a lithium-ion battery is used as an example of an electrochemical device to explain the present application, but the electrochemical device of the present application is not limited to a lithium-ion battery.

[0032] The first aspect of the present application provides a negative electrode material, which comprises: a first silicon-based material, a second silicon-based material, passivated lithium powder, and an organic polymer; the particle size Dv50 of the first silicon-based material is A, 2 μm ≤ A ≤ 5 μm, the particle size Dv50 of the second silicon-based material is B, wherein, 4B < A < 20B; the particle size Dv50 of the passivated lithium powder is C, 0.01 μm ≤ C ≤ 0.1 μm. For example, the particle size Dv50 of the first silicon-based material is A, A can be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm or a range composed of any two of these values; the particle size Dv50 of the second silicon-based material is B, B can be 0.05A, 0.1A, 0.15A, 0.2A, 0.25A or a range composed of any two of these values; the particle size Dv50 of the passivated lithium powder is C, C can be 0.01 μm, 0.02 μm, 0.04 μm, 0.06 μm, 0.08 μm, 0.1 μm or a range composed of any two of these values. By controlling the particle size Dv50 of the first silicon-based material within the range of 2 μm to 5 μm, the first silicon-based material has relatively excellent cycling performance, but slightly poor rate performance and a relatively large specific surface area; by controlling the particle size Dv50 of the second silicon-based material within the above range, the second silicon-based material has excellent rate performance, but slightly poor cycling performance and a relatively large specific surface area. By controlling the particle size Dv50 of the first silicon-based material, the second silicon-based material, and the passivated lithium powder, and performing secondary granulation on the first silicon-based material, the second silicon-based material, and the passivated lithium powder after grading with the help of a polymer binder, the advantages of the long cycling performance of the first silicon-based material and the high rate performance of the second silicon-based material can be combined, and at the same time, the specific surface area of the silicon-carbon particles can be further reduced, which can effectively alleviate the fragmentation and pulverization of the silicon-carbon negative electrode material during cycling and inhibit the growth of the SEI film, reduce the volume expansion after cycling of the electrochemical device, and improve the cycling performance and rate performance of the electrochemical device.

[0033] In an embodiment of the present application, the first silicon-based material and the second silicon-based material each include a core, a carbon layer outside the core, and a lithium salt layer outside the carbon layer. Specifically, the structural schematic diagram of the negative electrode material is as Figure 1 shown, from the inside out are the core 11, the carbon layer 12, the lithium salt layer 13, the organic polymer 14, and the passivated lithium powder 15.

[0034] In an embodiment of the present application, the negative electrode material satisfies at least one of the following: (1) the core includes at least one of silicon-carbon particles or silicon-oxygen particles; (2) the lithium salt includes LiF or Li 2 CO 3At least one of; (3) based on the mass of the first silicon-based material, the mass percentage of the carbon layer of the first silicon-based particle is 1% to 5.2%, and the mass percentage of the lithium salt layer is 0.53% to 2.1%; (4) based on the mass of the second silicon-based material, the mass percentage of the carbon layer of the second silicon-based particle is 1% to 5.2%, and the mass percentage of the lithium salt layer is 0.53% to 2.1%. For example, based on the mass of the first silicon-based material or the second silicon-based material, the mass percentage of the carbon layer thereof can be 1%, 2%, 3%, 4%, 5%, 5.2%, or a range consisting of any two of the values, and the mass percentage of the lithium salt layer thereof can be 0.53%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.1%, or a range consisting of any two of the values. The introduction of the carbon layer protects the active silicon on the first silicon-based material and the second silicon-based material, reducing the gas production problem caused by the direct contact between water and active silicon during the stirring process; the introduction of lithium salts and organic polymers inhibits the direct contact between the electrolyte and the active silicon, and at the same time can change the composition of SEI, thereby improving the cycle performance of the electrochemical device.

[0035] In one embodiment of the present application, the average size of silicon grains in the core of the first silicon-based material is a, and the average size of silicon grains in the core of the second silicon-based material is b; 1nm≤a≤1.5nm, 1.5nm≤b≤2nm, and a<b. For example, the average size a of silicon grains in the core of the first silicon-based material can be 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, or a range consisting of any two of these values; the average size b of silicon grains in the core of the second silicon-based material can be 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, or a range consisting of any two of these values. By adjusting the average size of silicon grains in the core of the first silicon-based material to 1nm to 1.5nm, the first silicon-based material has excellent cycle performance, but slightly poor rate performance and a larger specific surface area; by adjusting the average size of silicon grains in the core of the second silicon-based material to 1.5nm to 2nm, the second silicon-based material has excellent rate performance, but slightly poor cycle performance and a larger specific surface area. After grading the first silicon-based material, the second silicon-based material and the passivated lithium powder, secondary granulation is performed with the help of a polymer adhesive, which can combine the advantages of the long cycle performance of the first silicon-based material and the high rate performance of the second silicon-based material, and further reduce the specific surface area of ​​the silicon-carbon material particles, which can effectively alleviate the fragmentation and pulverization of the silicon-carbon material during the cycle and inhibit the growth of the SEI film, reduce the volume expansion of the electrochemical device after the cycle, and improve the cycle performance and rate performance of the electrochemical device.

[0036] In one embodiment of the present application, 0.1 μm ≤ B ≤ 0.5 μm. For example, B can be 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm or a range consisting of any two of these values. By regulating the particle size Dv50 of the second silicon-based material within the above range, the first silicon-based material, the second silicon-based material and the passivated lithium powder are graded and then secondary granulated with the help of a polymer adhesive, which can combine the advantages of the long cycle performance of the first silicon-based material and the high rate performance of the second silicon-based material, and further reduce the specific surface area of ​​the silicon-carbon particles, which can effectively alleviate the fragmentation and pulverization of the silicon-carbon negative electrode material during the cycle and inhibit the growth of the SEI film, reduce the volume expansion of the electrochemical device after the cycle, and improve the cycle performance and rate performance of the electrochemical device.

[0037] In one embodiment of the present application, the mass of the first silicon-based material is m 1 g, the mass of the second silicon-based material is m 2 g, the mass of the passivated lithium powder is m 3 g, mass ratio meets: m 1 :m 2 :m 3 =100:10 to 40:0.5 to 5. For example, m 1 :m 2 :m 3 It can be 100:10:0.5, 100:15:0.5, 100:20:0.5, 100:25:0.5, 100:30:0.5, 100:35:0.5, 100:40:0.5, 100:10:1, 100:10:2, 100:10:3, 100:10:4, 100:10:5, 100:25:1, 100:25:2, 100:25:3, 100:25:4, 100:25:5 or a range consisting of any two of them. By regulating the mass ratio of the first silicon-based material, the second silicon-based material and the passivated lithium powder, secondary granulation is performed with the help of a polymer adhesive, which can combine the advantages of the long cycle performance of the first silicon-based material and the high rate performance of the second silicon-based material, while further reducing the specific surface area of ​​the silicon-carbon particles, which can effectively alleviate the fragmentation and pulverization of the silicon-carbon material during the cycle and inhibit the growth of SEI, reduce the volume expansion of the electrochemical device after the cycle, and improve the cycle performance and rate performance of the electrochemical device.

[0038] In one embodiment of the present application, the mass percentage of the organic polymer is 3% to 7% based on the mass of the negative electrode material. For example, the mass percentage of the organic polymer can be 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7% or a range consisting of any two of these values. By regulating the mass percentage of the organic polymer within the above range, the polymer can play a role in secondary granulation, while inhibiting direct contact between the electrolyte and the active silicon, changing the composition of the SEI, and thus improving the cycle performance and rate performance of the electrochemical device.

[0039] In one embodiment of the present application, the negative electrode material satisfies at least one of the following: (1) the Dv50 of the negative electrode material is 6 μm to 10 μm; (2) the Dv90 of the negative electrode material is less than or equal to 30 μm; (3) the organic polymer includes polyurethane; (4) based on the mass of the negative electrode material, the mass percentage of silicon element is 40% to 50%.

[0040] In one embodiment of the present application, the Dv50 of the negative electrode material is 6 μm to 10 μm. For example, the Dv50 of the negative electrode material can be 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, or a range consisting of any two of these values. By adjusting the Dv50 of the negative electrode material within the above range, the particle size of the negative electrode material can be reduced, which helps to shorten the Li + The diffusion path of the negative electrode material is improved to improve the rate performance of the electrochemical device. However, the specific surface area increases as the particle size of the negative electrode material decreases, thereby increasing the contact area between the negative electrode material and the electrolyte, resulting in more side reactions and deteriorating the cycle performance. The inventors of this application have found that when the particle size Dv50 of the negative electrode material is 6μm to 10μm, when shortening the Li + A good balance is achieved between the diffusion path and the reduction of specific surface area, while improving the ionic conductivity of the negative electrode material and maintaining good cycle performance and rate performance.

[0041] In one embodiment of the present application, the Dv90 of the negative electrode material is less than or equal to 30μm. The Dv90 of the negative electrode material can be 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm or a range consisting of any two of these values. When the particle size Dv90 of the negative electrode material is too large (exceeding 30μm), it is not conducive to the processing of the negative electrode plate, and the negative electrode plate will have particle defects when coating the negative electrode plate; when the particle size Dv90 of the negative electrode material is less than or equal to 30μm, it can improve the dispersion uniformity of the slurry of the negative electrode material when preparing the negative electrode material layer, and improve Li+ transport, thereby improving the cycle performance and expansion performance of lithium-ion batteries.

[0042] In one embodiment of the present application, the organic polymer includes polyurethane. By selecting the above organic polymer, it can play a role in secondary granulation, while inhibiting direct contact between the electrolyte and the active silicon, changing the composition of SEI, thereby improving the cycle performance and rate performance of the electrochemical device.

[0043] In one embodiment of the present application, based on the mass of the negative electrode material, the mass percentage of silicon element is 40% to 50%. For example, the mass percentage of silicon element can be 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50% or a range consisting of any two of the values. By regulating the mass percentage of silicon element within the above range, the negative electrode material has a higher reversible capacity and first cycle efficiency, which is beneficial to improve the energy density, cycle performance and rate performance of the electrochemical device.

[0044] The second aspect of the present application provides a method for preparing the negative electrode material according to the first aspect of the present application, which comprises:

[0045] Providing a core of a first silicon-based material, carbon-coating the core to obtain a first intermediate, dispersing the first intermediate in water to obtain a first dispersion, adding an aqueous solution of a lithium source substance to the first dispersion to obtain a second dispersion, fully dispersing and stirring, and drying in an oven to obtain a first silicon-based material;

[0046] Providing a core of a second silicon-based material, carbon-coating the core to obtain a first intermediate, dispersing the first intermediate in water to obtain a first dispersion, adding an aqueous solution of a lithium source material to the first dispersion to obtain a second dispersion, fully dispersing and stirring, and drying in an oven to obtain a second silicon-based material;

[0047] The first silicon-based material, the second silicon-based material and the passivated lithium powder are dispersed and then deionized water is added to obtain a third dispersion; the polymer is dispersed in water to obtain a fourth dispersion, the fourth dispersion is added to the third dispersion, mixed and fully stirred, and the negative electrode material is obtained by spray drying.

[0048] In one embodiment of the present application, the core particle size Dv50 of the first silicon-based material is 1.985 μm to 4.985 μm, and the core particle size Dv50 of the second silicon-based material is 0.095 μm to 0.495 μm. For example, the core particle size Dv50 of the first silicon-based material can be 1.985μm, 2μm, 2.2μm, 2.4μm, 2.6μm, 2.8μm, 2.985μm, 3μm, 3.2μm, 3.4μm, 3.6μm, 3.8μm, 3.985μm, 4μm, 4.2μm, 4.4μm, 4.6μm, 4.985μm or a range consisting of any two of the values ​​therein; the core particle size Dv50 of the second silicon-based material can be 0.095μm, 0.1μm, 0.15μm, 0.2μm, 0.25μm, 0.3μm, 0.35μm, 0.4μm, 0.495μm or a range consisting of any two of the values ​​therein.

[0049] In one embodiment of the present application, the average size of silicon grains in the core of the first silicon-based material is a, and the average size of silicon grains in the core of the second silicon-based material is b; 1nm≤a≤1.5nm, 1.5nm≤b≤2nm, and a<b. For example, the average size a of silicon grains in the core of the first silicon-based material can be 1nm, 1.1nm, 1.2nm, 1.3nm, 1.4nm, 1.5nm, or a range consisting of any two of these values; the average size b of silicon grains in the core of the second silicon-based material can be 1.5nm, 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, or a range consisting of any two of these values.

[0050] In one embodiment of the present application, the first intermediate in preparing the first silicon-based material and the second silicon-based material is obtained by silane deposition at different temperatures of porous carbons of two different particle sizes obtained by airflow pulverization and classification. The present application has no particular limitation on the particle classification technology, as long as the purpose of the present application can be achieved, and the particle classification technology can be any known classification means in the art, such as jet classification and cyclone classification.

[0051] In one embodiment of the present application, the carbon coating process of the first silicon-based material is to place the core particles of the first silicon-based material in a fluidized bed at a temperature of 590°C to 610°C, and the carbon coating process of the second silicon-based material is to place the core particles of the second silicon-based material in a fluidized bed at a temperature of 540°C to 560°C. In the above case, a carbon source gas is introduced and reacted for 2h to 3h, wherein the carbon source gas contains at least one of acetylene, methane, and propylene. For example, the coating temperature of the first silicon-based material can be 590°C, 595°C, 600°C, 605°C, 610°C, or a range consisting of any two of the values ​​therein; the coating temperature of the second silicon-based material can be 540°C, 545°C, 550°C, 555°C, 560°C, or a range consisting of any two of the values ​​therein. For example, the coating time is 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, or a range consisting of any two of the values ​​therein. By controlling the time and temperature of carbon coating within the above range, the content of carbon material in the carbon coating process can be controlled. The carbon source gas is cracked at high temperature and then deposited on the outside of the core particle. In the appropriate temperature range, the higher the deposition temperature, the faster the cracking rate of the carbon source gas, the higher the utilization rate, and the faster the carbon layer grows; at the same deposition temperature, the length of deposition time determines the thickness and integrity of the carbon layer.

[0052] In one embodiment of the present application, the carbon source gas and the inert gas are mixed and introduced into the fluidized bed, and the inert gas includes at least one of nitrogen or argon; based on the volume of the mixed gas, the volume percentage of the carbon source gas is 10% to 50%. For example, the volume percentage of the carbon source gas can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of these values. The provision of the inert gas is conducive to improving the uniformity of the distribution of the carbon element in the carbon layer.

[0053] In one embodiment of the present application, the solid content of the first dispersion is 15% to 20%. For example, the solid content of the first dispersion can be 15%, 16%, 17%, 18%, 19%, 20%, or a range consisting of any two of these values. By regulating the solid content of the first intermediate in deionized water within the above range, the particle size distribution of the first silicon-based material particles and the second silicon-based material particles after spray drying can be controlled while taking into account the drying capacity and production capacity of the machine, effectively reducing the risk of particle size increase caused by particle adhesion.

[0054] Without being limited to any theory, the lithium source material may be LiF. The inventors believe that by successively adding ammonium fluoride and an aqueous solution of a lithium source compound to the first dispersion and stirring the mixture sufficiently to react and generate lithium fluoride, the first intermediate can be more evenly coated on the outside thereof. The lithium source compound includes at least one of lithium acetate, lithium nitrate, and lithium sulfate.

[0055] Without being limited to any theory, the lithium source material may be Li 2 CO 3 The inventors believe that the lithium source compound is first dissolved in an aqueous solution, added to the first dispersion, and then carbon dioxide is introduced and stirred to react to generate lithium carbonate, which can be more evenly coated on the outside of the first intermediate. The lithium source compound includes lithium hydroxide.

[0056] In one embodiment of the present application, the concentration of the lithium source compound aqueous solution is 1% to 10%. For example, the concentration of the lithium source compound aqueous solution can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of these values.

[0057] In one embodiment of the present application, the lithium source material may include LiF and Li 2 CO 3 , LiF and Li 2 CO 3 The mass ratio is 1:1 to 10:1, and the concentration of the lithium source compound aqueous solution corresponding to the lithium source material is 1% to 10%. 2 CO 3 The mass ratio of can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1 or a range consisting of any two of them; for example, the concentration of the lithium source compound aqueous solution can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or a range consisting of any two of them. LiF and Li 2 CO 3 The introduction of can improve the composition of SEI, enhance the mechanical strength and ionic and electronic conductivity of SEI, thereby improving the cycle performance of lithium-ion batteries.

[0058] In one embodiment of the present application, the mass ratio of the first intermediate to the lithium salt is 100:0.5 to 100:3. For example, the mass ratio may be 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, or a range consisting of any two of the above values. By regulating the mass ratio of the first intermediate to the lithium salt within the above range, the composition of the SEI film can be changed and the thickness of the SEI can be reduced, the lithium ion mobility of the SEI can be increased, and the cycle performance of the electrochemical device can be improved, while the silicon content in the final negative electrode material will not be significantly reduced, thereby ensuring that the negative electrode material has sufficient reversible capacity.

[0059] In one embodiment of the present application, the solid content of the second dispersion is 8% to 20%, for example, the solid content of the second dispersion can be 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20% or a range consisting of any two of these values. By regulating the solid content within the above range, the particle size distribution of the secondary particles after spray drying can be controlled while taking into account the drying capacity and production capacity of the machine.

[0060] In one embodiment of the present application, the stirring and dispersing time of the second dispersion is 3 hours to 6 hours, for example, the stirring and dispersing time can be 3 hours, 4 hours, 5 hours, 6 hours or a range consisting of any two of the above values. By regulating the stirring and dispersing time within the above range, sufficient stirring can make the first intermediate and the lithium source material in the aqueous solution fully and uniformly contact, thereby improving the uniformity of the lithium salt layer.

[0061] In one embodiment of the present application, the temperature of the oven drying is 100°C to 150°C, and the drying time is 12h to 24h. For example, the drying temperature can be 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, or a range consisting of any two of the values; the drying time can be 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, or a range consisting of any two of the values. By regulating the parameters of the oven drying within the above range, the particle size distribution of the particles after drying can be controlled, and the risk of particle size increase caused by the adhesion of the particles can be effectively reduced.

[0062] In one embodiment of the present application, the solid content of the third dispersion is 15% to 30%. For example, the solid content can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, or a range consisting of any two of the above values. By regulating the solid content of the second intermediate in deionized water within the above range, the particle size distribution of the secondary particles after spray drying can be controlled while taking into account the drying capacity and production capacity of the machine.

[0063] In one embodiment of the present application, the mass ratio of the mixture of the first silicon-based material, the second silicon-based material, and the passivation lithium powder is m 1 :m 2 :m 3=100:10 to 40:0.5 to 5. For example, the mass ratio of the mixture of the first silicon-based material, the second silicon-based material, and the passivation lithium powder can be 100:10:0.5, 100:15:0.5, 100:20:0.5, 100:25:0.5, 100:30:0.5, 100:35:0.5, 100:40:0.5, 100:10:1, 100:10:2, 100:10:3, 100:10:4, 100:10:5, 100:25:1, 100:25:2, 100:25:3, 100:25:4, 100:25:5, or a range consisting of any two of the values.

[0064] In one embodiment of the present application, the solid content of the fourth dispersion is 18% to 22%. For example, the solid content may be 18%, 19%, 20%, 21%, 22% or a range consisting of any two of the above values.

[0065] In one embodiment of the present application, the solid content of the third dispersion after mixing with the fourth dispersion is 15% to 25%. For example, the solid content can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25% or a range consisting of any two of the above values.

[0066] In one embodiment of the present application, the stirring and dispersing time of the negative electrode material is 3 hours to 6 hours, for example, the stirring and dispersing time can be 3 hours, 4 hours, 5 hours, 6 hours or a range consisting of any two of the above values. Sufficient stirring can make the mixture of the first silicon-based material, the second silicon-based material, the passivated lithium powder, and the polyurethane in the aqueous solution fully and evenly contact, thereby improving the uniformity of the organic polymer on the outside of the negative electrode material.

[0067] In one embodiment of the present application, the inlet temperature of the spray drying of the negative electrode material is 200-230°C, and the outlet temperature is 100-110°C. For example, the inlet temperature of the spray drying of the negative electrode material can be 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, or a range consisting of any two values ​​therein; the outlet temperature can be 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, or a range consisting of any two values ​​therein. The parameters of the spray drying are within the above range, and the particle size distribution of the secondary particles after spray drying is controlled while taking into account the drying capacity and production capacity of the machine.

[0068] The third aspect of the present application provides an electrochemical device, which includes a positive electrode plate, a negative electrode plate and an electrolyte, the negative electrode plate includes a negative electrode active material layer, and the negative electrode active material layer includes the negative electrode material described in the first aspect of the present application.

[0069] In one embodiment of the present application, the electrolyte comprises at least one of lithium bis(trifluoromethylsulfonyl)imide or lithium bis(fluorosulfonyl)imide; based on the mass of the electrolyte, the mass percentage of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and / or lithium bis(fluorosulfonyl)imide (LiFSI) is 0.1% to 5%. For example, the mass percentage of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and / or lithium bis(fluorosulfonyl)imide (LiFSI) may be 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two of the values. By regulating within the above range, LiTFSI and / or LiFSI can improve the contact interface and improve the cycle performance and rate performance of the electrochemical device by interacting with the negative electrode material when the electrochemical device is cycled.

[0070] In the electrochemical device of the present application, the electrolyte further includes electrolyte lithium salt and a non-aqueous solvent.

[0071] In some embodiments of the present application, the electrolyte lithium salt is selected from lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ) lithium hexafluoroarsenate (LiAsF 6 ), lithium perchlorate (LiClO 4 ), lithium tetraphenylborate (LiB(C 6 H5) 4 ), lithium methanesulfonate (LiCH 3 SO 3 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 )、LiC(SO 2 CF 3 ) 3 、Lithium hexafluorosilicate (LiSiF 6 ), lithium bis(oxalatoborate) (LiBOB) and lithium difluoroborate (LiF 2 OB) in one or more. For example, the electrolyte lithium salt can be selected from LiPF 6 Because it has high ionic conductivity and improves cycle characteristics. Based on the mass of the electrolyte, the mass percentage of the electrolyte lithium salt can be 8% to 20%, for example, the mass percentage of the electrolyte lithium salt can be 8%, 10%, 12%, 14%, 16%, 18%, 20% or a range consisting of any two of these values.

[0072] The non-aqueous solvent may be a carbonate compound, a carboxylate compound, an ether compound, other organic solvents or a combination thereof.

[0073] The carbonate compound may be a linear carbonate compound, a cyclic carbonate compound, a fluorinated carbonate compound or a combination thereof. Examples of the linear carbonate compound are dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (EMC) and a combination thereof. Examples of the cyclic carbonate compound are ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC) and a combination thereof. Examples of the fluorinated carbonate compounds are fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate, and combinations thereof.

[0074] Examples of the above carboxylic acid ester compounds are methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanoic acid lactone, valerolactone, mevalonolactone, caprolactone and combinations thereof.

[0075] Examples of the above ether compound are dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, ethoxymethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and combinations thereof.

[0076] Examples of the above other organic solvents are dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, formamide, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, trioctyl phosphate and phosphoric acid esters and combinations thereof.

[0077] In the present application, the electrochemical device also includes a negative electrode plate, which includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The above-mentioned "negative electrode active material layer is disposed on at least one surface of the negative electrode current collector" means that the negative electrode active material layer can be disposed on one surface of the negative electrode current collector along its own thickness direction, or it can be disposed on two surfaces of the negative electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of ​​the surface of the negative electrode current collector, or it can be a partial area of ​​the surface of the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved.

[0078] The present application has no particular limitation on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, it may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or a composite current collector. For example, the composite current collector may be a lithium-copper composite current collector, a carbon-copper composite current collector, a nickel-copper composite current collector, a titanium-copper composite current collector, etc.

[0079] The negative electrode active material layer also contains carbon material, which may include at least one of natural graphite, artificial graphite, hard carbon material, soft carbon material or mesophase microcarbon spheres, and the content of the carbon material ranges from 30% to 95% based on the mass of the negative electrode active material layer. For example, it may be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 70%, 80%, 90%, 95% or a range consisting of any two of these values.

[0080] In some embodiments of the present application, the negative electrode active material layer may also include a conductive agent and a binder. The present application does not particularly limit the types of conductive agents and binders, as long as the purpose of the present application can be achieved. For example, the binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon, etc. The conductive agent may include but is not limited to: carbon-based materials, metal-based materials, conductive polymers and mixtures thereof. Among them, the carbon-based material is selected from natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber or any combination thereof; the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum or silver; the conductive polymer is a polyphenylene derivative. The present application does not particularly limit the mass ratio of the negative electrode material, conductive agent and binder in the negative electrode active material layer, and those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved.

[0081] The present application has no particular limitation on the thickness of the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the single-sided negative electrode active material layer is 30 μm to 120 μm.

[0082] The present application has no particular limitation on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4 μm to 15 μm.

[0083] In the present application, the electrochemical device also includes a positive electrode plate, which includes a positive electrode collector and a positive electrode active material layer disposed on at least one surface of the positive electrode collector. The above-mentioned "positive electrode active material layer disposed on at least one surface of the positive electrode collector" means that the positive electrode active material layer can be disposed on one surface of the positive electrode collector along its own thickness direction, or on two surfaces of the positive electrode collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of ​​the surface of the positive electrode collector, or it can be a partial area of ​​the surface of the positive electrode collector. This application has no special restrictions, as long as the purpose of this application can be achieved.

[0084] The present application has no particular limitation on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, it may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector).

[0085] The present application has no particular restrictions on the positive electrode material, as long as the purpose of the present application can be achieved. For example, the positive electrode material may include but is not limited to at least one of lithium cobalt oxide, lithium nickel manganese cobalt oxide, lithium nickel manganese aluminum oxide, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, spinel lithium nickel manganese oxide and lithium titanate.

[0086] The positive electrode active material layer may also include a conductive agent and a binder. The present application has no particular restrictions on the types of the conductive agent and the binder, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the mass ratio of the positive electrode material, the conductive agent, and the binder in the positive electrode active material layer. Those skilled in the art can select according to actual needs, as long as the purpose of the present application can be achieved.

[0087] The present application has no particular limitation on the binder, as long as the purpose of the present application can be achieved. For example, the binder may include but is not limited to adhesive polymers, such as at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified polyvinylidene fluoride, modified styrene-butadiene rubber or polyurethane, wherein the polyolefin binder includes at least one of polyethylene, polypropylene, polyolefin ester, polyolefin alcohol or polyacrylic acid.

[0088] The present application has no particular restrictions on the conductive agent, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to carbon-based materials, metal-based materials, conductive polymers or mixtures thereof; wherein the carbon-based materials include natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black or carbon fiber; examples of metal-based materials include metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers include polyphenylene derivatives.

[0089] The present application has no particular limitation on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5 μm to 20 μm, and the thickness of the single-sided positive electrode active material layer is 30 μm to 120 μm.

[0090] Optionally, the positive electrode sheet may further include a conductive layer, which is located between the positive electrode current collector and the positive electrode active material layer. The composition of the conductive layer is not particularly limited, and it can be a conductive layer commonly used in the art. The conductive layer includes a conductive agent and a binder. The present application does not particularly limit the conductive agent and the binder in the conductive layer, for example, it can be at least one of the above conductive agent and the above binder.

[0091] In the present application, the electrochemical device also includes an isolation membrane. The present application has no particular restrictions on the isolation membrane, as long as the purpose of the present application can be achieved. For example, the material of the isolation membrane may include but is not limited to polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (e.g., polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or aramid. The type of isolation membrane may include at least one of a woven membrane, a non-woven membrane, a microporous membrane, a composite membrane, a rolled membrane or a spun membrane.

[0092] In some embodiments of the present application, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer may be a nonwoven fabric, a film or a composite film having a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be used.

[0093] Optionally, a surface treatment layer is disposed on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing a polymer and an inorganic layer.

[0094] In some embodiments of the present application, the inorganic layer includes inorganic particles and a binder. The present application is not particularly limited to inorganic particles, such as inorganic particles can include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application is not particularly limited to binders, such as binders can be at least one of the above-mentioned binders. In some embodiments of the present application, the polymer layer includes polymers, and the material of the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymers, polyacrylic acid, polyacrylates, polyvinyl pyrrolidone, polyvinyl ether or polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene).

[0095] In some embodiments of the present application, the inorganic layer may also include a thickener and a wetting agent. The present application has no particular restriction on the types of the thickener and the wetting agent, as long as the purpose of the present application can be achieved. For example, the thickener may include but is not limited to at least one of sodium carboxymethyl cellulose or lithium carboxymethyl cellulose; the wetting agent may include but is not limited to at least one of dimethyl siloxane, sodium dodecyl sulfate, trialkyl phosphate, methyl decanoate, and lauryl acetate.

[0096] In the present application, there is no particular limitation on the thickness of the isolation film, as long as the purpose of the present application can be achieved. For example, the thickness of the isolation film may be 4 μm to 30 μm.

[0097] The electrochemical device also includes a housing for accommodating a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, as well as other components known in the field of electrochemical devices, and this application does not limit the above-mentioned other components. This application does not particularly limit the housing, and it can be a housing known in the art, as long as the purpose of this application can be achieved. For example, the housing can be a hard shell housing or a flexible shell. The material of the hard shell housing can be metal, and this application does not limit the type of metal, and a metal hard shell housing known in the art can be used, as long as the purpose of this application can be achieved. The flexible housing can be a metal plastic film, such as an aluminum plastic film, a steel plastic film, etc.

[0098] The preparation process of the electrochemical device of the present application is well known to those skilled in the art, and the present application has no particular limitations. For example, the preparation process of the electrochemical device may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly with a wound structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain an electrochemical device. Alternatively, stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly with a stacked structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain an electrochemical device. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent pressure rise and overcharge and discharge inside the electrochemical device.

[0099] A fourth aspect of the present application provides an electronic device, which includes the electrochemical device provided in the third aspect of the present application.

[0100] The electronic device of the present application is not particularly limited, and it can be any electrical device known in the prior art. In some embodiments, the electrical device may include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.

[0101] Example

[0102] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0103] Test methods and equipment

[0104] Test of mass percentage of Si element

[0105] Prepare digestion samples: Take 0.1000g of silicon-based negative electrode particles or negative electrode materials, put them into a nickel crucible, add 1.5g of KOH and cover the crucible, heat the muffle furnace to 400℃, and the heating program is from room temperature to 300℃ within 2h, and then from 300℃ to 400℃ within 2h. Then start cooling, cool naturally to 80℃, and the digestion program is over. Take out the crucible, cool to room temperature, take out the digested sample and place it in an F4 beaker.

[0106] Titration of the digested sample with sodium hydroxide standard solution: Add 30mL of boiling water to the F4 beaker, soak for 1h, then use tweezers to pick up the crucible and clean it, control the volume to 50mL, and then filter the above solution and transfer it to a 400mL beaker. After the filtration is completed, add 20mL of concentrated nitric acid to the beaker to neutralize the solution and make the solution acidic. After the solution is cooled to room temperature, add solid KCl to saturation while stirring continuously, and use an excess of 2g. Then add 10mL of potassium fluoride solution, a white precipitate appears, age for 15min, filter with medium-speed quantitative filter paper, wash the beaker and precipitate with 8mL of potassium chloride solution each time, and wash three times in total. Remove the filter paper and put it back to the original beaker, add 20mL of potassium chloride ethanol solution and 10 drops of phenolphthalein, then neutralize the residual acid with sodium hydroxide standard solution, stir the filter paper and wipe the cup wall until the solution is light red, and use a glass rod to break up the pulp during this process, and react for 1h. Add 200 mL of neutralized boiling water into the cup (add 10 drops of phenolphthalein after boiling, and neutralize with sodium hydroxide standard solution until it turns slightly red), titrate with sodium hydroxide standard solution until it turns light red as the end point, and record the volume V of sodium hydroxide standard solution consumed in the titration.

[0107] Titration of blank sample with sodium hydroxide standard solution: except that the digested sample is not added, the remaining steps are the same as those of the titration of the digested sample with sodium hydroxide standard solution. Prepare a blank sample and record the volume V of sodium hydroxide standard solution consumed in the titration of the blank sample. 0 .

[0108] The mass percentage of silicon is calculated according to the following formula: Si =(VV 0 )×c×7.02 / m×100%, where: c is the concentration of sodium hydroxide standard solution, in mol / L; V is the volume of sodium hydroxide standard solution consumed in titration, in L; V 0 is the volume of sodium hydroxide standard solution consumed by the blank sample, in L; 7.02 is the molar mass of 1 / 4Si, in g / mol; m is the mass of the sample, in g.

[0109] Carbon mass percentage test

[0110] Take the negative electrode material and heat it at high temperature in a high-frequency furnace under oxygen-rich conditions to oxidize carbon into carbon dioxide. After treatment, the gas enters the corresponding absorption cell, absorbs the corresponding infrared radiation, and then is converted into a corresponding signal by the detector. This signal is sampled by a computer, converted into a value proportional to the concentration of carbon dioxide after linear correction, and then the values ​​of the entire analysis process are accumulated. After the analysis is completed, this accumulated value is divided by the weight value in the computer, multiplied by the correction coefficient, and the blank is deducted to obtain the mass percentage of carbon. The test is carried out using a high-frequency infrared carbon and sulfur analyzer (Shanghai Dekai HCS-140).

[0111] Powder conductivity test

[0112] The conductivity of each synthesized negative electrode material was tested in a drying room using a powder resistivity meter to obtain the conductivity, the reciprocal of which is the resistance of the negative electrode material.

[0113] Particle size testing

[0114] The Mastersizer 3000 particle size tester produced by Malvern was used to measure the Dv50 and Dv90 of the first silicon-based material, the second silicon-based material particles and the negative electrode material.

[0115] XRD test and silicon grain size calculation

[0116] The first silicon-based material and the second silicon-based material powders were placed on the sample stage of an XRD test instrument (the instrument model is Bruker D8 ADVANCE), and an XRD diffraction pattern was obtained using a scanning rate of 2° / min, a scanning angle range of 10° to 90°, and Cu Kα rays. The silicon grain size was obtained by fitting and calculating the XRD diffraction data in the test software according to the Scherrer formula.

[0117] The preparation process of button half-cell includes:

[0118] (1) Preparation process of positive electrode sheet: The negative electrode material prepared in the embodiment or comparative example is used as the active material, acetylene black is used as the conductive agent, and sodium alginate is used as the binder. The mass ratio of active material, acetylene black and sodium alginate is 90:5:5. The active material and acetylene black are fully mixed in proportion and ground evenly, and sodium alginate aqueous solution is added in proportion and stirred for 4 hours. Finally, the mixture slurry is evenly coated on the copper foil, and vacuum dried at 70°C, and punched into a circular electrode sheet with a diameter of 10 mm.

[0119] Electrolyte and isolation membrane: In an argon atmosphere glove box with a water content of <10ppm, propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) were mixed in a ratio of 1:1:1 to obtain a base solvent, and lithium salt LiPF was added. 6 Dissolve and mix evenly to obtain an electrolyte; wherein, based on the total mass of the electrolyte, the lithium salt LiPF 6 The mass percentage of the solvent is 12.5%, and the balance is the base solvent. A PE / PP composite film with a thickness of 8 μm is used as the isolation membrane.

[0120] (2) Assembly of button half-cell: In an argon atmosphere glove box with a water content of less than 10 ppm, a lithium metal sheet is used as the negative electrode sheet. The negative electrode sheet, the isolation membrane prepared above, and the positive electrode sheet are stacked in order, so that the isolation membrane is located between the positive electrode sheet and the negative electrode sheet to play an isolating role. After assembly, the electrolyte prepared above is injected to obtain a button half-cell.

[0121] The test methods for the first cycle charge and discharge specific capacity include:

[0122] At 25°C and normal pressure, the prepared button half-cell was discharged at a constant current of 0.1C to 0.01V, and then left to stand for 5 minutes. The discharge specific capacity at this time was recorded, which was the first cycle discharge specific capacity.

[0123] Then charge at a constant current of 0.1C to 1.5V, then charge at a constant voltage to a current of 0.05C, and then let it stand for 5 minutes. This is a cyclic charge and discharge process. Record the charging capacity at this time, which is the first cycle charging capacity.

[0124] First cycle charge and discharge efficiency = first cycle charge specific capacity / first cycle discharge specific capacity × 100%.

[0125] Lithium-ion battery cycle performance test

[0126] For the lithium-ion battery of the embodiment or comparative example, the test temperature is 25°C / 45°C, and the battery is charged to 4.4V at 3.4C constant current, charged to 0.025C at constant voltage, and discharged to 3.0V at 0.5C after standing for 5 minutes. The capacity obtained in this step is taken as the initial capacity, and a cycle test is performed at 3.4C charging / 0.5C discharging, and the cycle is repeated 500 times. The capacity of each step is compared with the initial capacity to obtain a cycle performance comparison chart. Figure 2 and Figure 3 .

[0127] The number of cycles at 25°C until the capacity retention rate reaches 90% is recorded as the room temperature cycle performance of the battery;

[0128] The number of cycles at 45° C. until the capacity retention rate reaches 80% is recorded as the high-temperature cycle performance of the battery. The cycle performance of the lithium-ion battery is compared by comparing the number of cycles in the above two cases.

[0129] Lithium-ion battery rate cycle capacity retention test

[0130] Place the lithium-ion battery in a 25℃ constant temperature box for 1 hour to allow the lithium-ion battery to reach a constant temperature; charge it to 4.4V at a constant current of 0.2C, charge it to 0.025C at a constant voltage, and place it for 30 minutes; discharge it to 3.0V at 0.2C, and place it for 30 minutes. The capacity (D 0 ) as a benchmark;

[0131] At 25℃, charge to 4.4V at 0.7C constant current, charge to 0.025C constant voltage, and let stand for 30 minutes; discharge to 3.0V at different rates of 0.2C / 0.5C / 0.7C / 1C / 1.5C / 2C, and record the capacity at different rates as D x (x is 0.2, 0.5, 0.7, 1, 1.5 or 2). Discharge capacity ratio at different rates = D x / D 0 × 100%, and the capacity retention rate curve is drawn, that is, Figure 6 The 2C rate discharge capacity ratio is the 2C capacity retention rate.

[0132] Lithium-ion battery cycle expansion rate test

[0133] For lithium-ion batteries, the relative difference between the thickness of the battery after 400 cycles of discharge to 3.0V at 25°C and the original battery thickness divided by the original battery thickness is recorded as the room temperature cycle expansion rate of the battery;

[0134] The relative difference between the thickness of the battery after 400 cycles of discharge to 3.0 V at 45°C and the thickness of the original battery divided by the thickness of the original battery is recorded as the high-temperature cycle expansion rate of the battery.

[0135] The thickness of the film was discharged to 3.0V after 400 cycles at 25℃, and the thickness of each step was compared with the original thickness. The thickness of the film was discharged to 3.0V after 400 cycles at 45℃, and the thickness of the film after 0, 50, 100, 150, 200, 300, and 400 cycles was compared with the original thickness to obtain the expansion rate comparison chart. Figure 4 and Figure 5 .

[0136] Example 1

[0137] <Preparation of negative electrode materials>

[0138] (1) 200 kg of silicon-carbon particles are taken and classified by jet classification (or cyclone classification) to obtain core particles of the first silicon-based material.

[0139] (2) Take 1 kg of silicon-carbon particles, the core particles of the first silicon-based material, with a Dv50 of 2.985 μm and a silicon grain size of 1.31 nm, and transfer 1 kg of silicon-carbon particles into the fluidized bed through high-pressure transmission. After standing for about 30 minutes, close the fluidized bed air inlet valve and tail gas valve and evacuate. When the chamber pressure reaches -101 kPa, close the vacuum and introduce nitrogen at a rate of 10 L / min to positive pressure. Repeat the vacuum and nitrogen introduction for more than 5 times, and then detect the oxygen content inside the chamber. When the oxygen content drops below 10 ppm, open the tail gas valve, start the fluidized bed stirring paddle, rotate at 150 rpm, introduce nitrogen at a rate of 20 L / min, heat to 600 ° C at a heating rate of 5 ° C / min, and keep warm for 1 hour. After the heat preservation is completed, the valve of the fluidized bed air inlet pipeline is switched to introduce acetylene / nitrogen mixed gas into the fluidized bed, with acetylene accounting for 25% by volume, gas flow rate of 20L / min, and reaction time of 150min. After the reaction is completed, nitrogen is introduced at a flow rate of 15L / min, and the stirring blade speed is adjusted to 100 rpm to cool down, and the material is discharged when it drops to room temperature to obtain the first intermediate of the first silicon-based material.

[0140] (3) Prepare 508.8 g of lithium acetate aqueous solution with a lithium acetate concentration of 10%, prepare 285.5 g of ammonium fluoride aqueous solution with a ammonium fluoride concentration of 10%, and prepare 64.8 g of lithium hydroxide aqueous solution with a lithium hydroxide concentration of 10%.

[0141] (4) Prepare 5 kg of deionized water, add 1 kg of the first intermediate, stir thoroughly to obtain a first dispersion, pour 508.8 g of 10% lithium acetate aqueous solution into the first dispersion while stirring, stir thoroughly for 1 hour; slowly pour 285.5 g of 10% ammonium fluoride aqueous solution while stirring, and react thoroughly for 2 hours; slowly pour 64.8 g of 10% lithium hydroxide aqueous solution while stirring, and stir thoroughly for 1 hour; introduce CO at a rate of 5 L / min while stirring. 2 The gas was stirred for 2 hours and fully stirred for 3 hours to obtain a second dispersion. The second dispersion was filtered and washed 3 times, and then placed in a 100°C oven (a constant vacuum drying oven, DZF-6020) for drying for 24 hours to obtain a first silicon-based material.

[0142] (5) Using jet classification (or cyclone classification) to perform classification treatment, a core particle of a second silicon-based material is obtained. 1 kg of the core particles of the second silicon-based material with a Dv50 of 0.295 μm and a silicon grain size of 1.8 nm are taken, and steps (2) to (4) are repeated, wherein the coating temperature of the carbon coating is reduced to 550° C., to obtain a second silicon-based material.

[0143] (6) Take 1000g of the first silicon-based material, 300g of the second silicon-based material, and 30g of passivated lithium powder, put them into 7kg of deionized water, and stir them thoroughly for 2h to obtain the third dispersion. Add 333g of the fourth dispersion with a solid content of 20% (the solute is polyurethane and the solvent is deionized water) to the third dispersion while stirring, and stir them thoroughly for 3h. Start the spray dryer, set the inlet temperature to 220℃ and the outlet temperature to 105℃. After the inlet temperature and outlet temperature reach the set range, first supply deionized water at a supply rate of 300mL / min. After stable operation for about 30min, switch to supply slurry. The dry negative electrode material after secondary granulation is obtained at the discharge port.

[0144] Among them, in the first silicon-based material, the mass percentage of the carbon layer is 3%, LiF and Li 2 CO 3 The total mass percentage is 2% (the mass percentage of LiF is 1.4%, Li 2 CO 3 The mass percentage of the first silicon-based material is 0.6%), the particle size Dv50 of the first silicon-based material is 3 μm; in the second silicon-based material, the mass percentage of the carbon layer is 3%, LiF and Li 2 CO 3 The total mass percentage is 2% (the mass percentage of LiF is 1.4%, Li 2 CO 3 The mass percentage is 0.6%), the particle size Dv50 of the second silicon-based material is 0.3 μm; the Dv50 of the passivated lithium powder is 0.07 μm;

[0145] The mass ratio of the first silicon-based material, the second silicon-based material, and the passivation lithium powder satisfies: m 1 :m 2 :m 3 =100:30:3, based on the mass of the negative electrode material, the mass percentage of polyurethane is 4.6%.

[0146] The negative electrode material prepared in Example 1-1 has a Dv50 of 7.6 μm and a Dv90 of 26.7 μm, and the structural schematic diagram is shown in FIG1 .

[0147] Example 1-2 to Example 1-4

[0148] Except that the particle size Dv50 of the first silicon-based material is adjusted according to Table 1 and the average size of the core silicon grains changes accordingly, the rest is the same as Example 1-1.

[0149] Examples 1-5

[0150] Except for synchronously adjusting the mass percentage of the carbon layer of the first silicon-based material and the second silicon-based material to 1%, and keeping the mass percentage of the lithium salt unchanged, the rest is the same as Example 1-1.

[0151] Examples 1-6

[0152] Except for synchronously adjusting the mass percentage of the carbon layer of the first silicon-based material and the second silicon-based material to 5.2% and keeping the mass percentage of the lithium salt unchanged, the rest is the same as Example 1-1.

[0153] Examples 1-7

[0154] In addition to synchronously adjusting the mass percentage of lithium salts of the first silicon-based material and the second silicon-based material to 1.2% (the mass percentage of LiF is 0.6%, Li 2 CO 3 The mass percentage of the carbon layer is 0.6%), and the rest is the same as Example 1-1.

[0155] Examples 1-8

[0156] In addition to synchronously adjusting the mass percentage of lithium salts of the first silicon-based material and the second silicon-based material to 0.6% (the mass percentage of LiF is 0.3%, Li 2 CO 3 The mass percentage of the carbon layer is 0.3%, and the rest is the same as Example 1-1.

[0157] Examples 1-9

[0158] Except for synchronously adjusting the type of lithium salt of the first silicon-based material and the second silicon-based material to LiF, the mass percentage content is 2%, and the mass percentage content of the carbon layer remains unchanged, the rest is the same as Example 1-1.

[0159] Example 1-10 to Example 1-23

[0160] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-1.

[0161] Comparative Example 1

[0162] Except that the first silicon-based material is not added according to Table 1, the rest is the same as Example 1-1.

[0163] Comparative Example 2

[0164] Except that the second silicon-based material is not added according to Table 1, the rest is the same as Example 1-1.

[0165] Comparative Example 3

[0166] Except for adjusting the relevant parameters according to Table 1, the rest is the same as Example 1-1.

[0167] Example 2-1

[0168] <Preparation of negative electrode sheet>

[0169] Graphite, the negative electrode material prepared according to Example 1-1, and a conductive agent (conductive carbon black, Super ) and binder polyacrylic acid (PAA) are dissolved in deionized water in a ratio of 80:10:5:5 and mixed evenly to form a negative electrode slurry with a solid content of 70wt%, and deionized water is added to adjust the viscosity of the slurry to 5000Pa·s to form a negative electrode slurry. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 120°C to obtain a negative electrode sheet with a single-sided coating of a negative electrode material layer. The coating weight of the negative electrode material layer is 142mg / 1540mm 2 Then repeat the above steps on the other surface of the copper foil to obtain a negative electrode sheet with a negative electrode material layer coated on both sides. After drying at 120°C, cold pressing, cutting and welding the tabs, a negative electrode sheet with a specification of 78mm×875mm is obtained for standby use. Among them, the thickness of the single-sided negative electrode active material layer is 54.5μm.

[0170] <Preparation of positive electrode sheet>

[0171] The positive electrode active material LiCoO 2 , conductive carbon black and polyvinylidene fluoride (PVDF) were fully stirred and mixed in an N-methylpyrrolidone solvent system at a mass ratio of 95:2.5:2.5 to prepare a positive electrode slurry. The positive electrode slurry was evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10 μm, and dried at 120°C to obtain a positive electrode sheet coated with a positive electrode material layer on one side. The coating weight of the positive electrode material layer was 267.8 mg / 1540 mm 2 Then repeat the above steps on the other surface of the aluminum foil to obtain a positive electrode sheet with a positive electrode material layer coated on both sides. After drying at 120°C, cold pressing, cutting and welding the tabs, a positive electrode sheet with a specification of 74mm×867mm is obtained for standby use. The thickness of the single-sided positive electrode material layer is 42μm.

[0172] <Preparation of Electrolyte>

[0173] In a dry argon environment, propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) were mixed in a ratio of 1:1:1 to obtain a base solvent, and lithium salt LiPF was added. 6 Mix evenly, dissolve and mix evenly to obtain an electrolyte; wherein, based on the total mass of the electrolyte, the lithium salt LiPF 6 The mass percentage is 12.5%, and the balance is the base solvent.

[0174] <Isolation film>

[0175] 8μm PE / PP composite film is used as the isolation membrane.

[0176] <Preparation of lithium-ion batteries>

[0177] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and the bare battery cell is wound. The bare battery cell is placed in an outer package, the electrolyte is injected, and the package is encapsulated. After the formation, degassing, trimming and other process flows, a lithium-ion battery is obtained.

[0178] Example 2-2 to Example 2-23

[0179] Except that the negative electrode materials in <Preparation of Negative Electrode Sheet> are selected from the negative electrode materials prepared in corresponding Examples 1-2 to 1-23 according to Table 2, the rest are the same as Example 2-1.

[0180] Comparative Examples 4 to 6

[0181] Except that the negative electrode material in <Preparation of Negative Electrode Sheet> is selected from the negative electrode materials prepared in Comparative Examples 1 to 3 according to Table 2, the rest is the same as Example 2-1.

[0182] Example 3-1 to Example 3-9

[0183] In addition to adding LiTFSI and LiFSI to the electrolyte according to Table 3 in <Preparation of Electrolyte>, and adjusting the mass percentage of LiTFSI and LiFSI, the mass percentage of the base solvent is changed accordingly, and the lithium salt LiPF 6 Except that the mass percentage content is changed accordingly, the rest is the same as Example 2-21.

[0184] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 3.

[0185]

[0186]

[0187]

[0188]

[0189] Table 3

[0190]

[0191] Note: “ / ” in Table 3 indicates that there is no corresponding preparation parameter, substance or performance parameter.

[0192] The mass percentage and type of additives in the electrolyte will affect the cycle performance and rate performance of the lithium-ion battery. It can be seen from Examples 2-21 and 3-1 to 3-9 that when the mass percentage of lithium bis(trifluoromethylsulfonyl)imide and / or lithium bis(fluorosulfonyl)imide in the electrolyte is within 0.1% to 5%, the lithium-ion battery prepared using the negative electrode material provided by the present application has a lower room temperature cycle expansion rate, high temperature cycle expansion rate and higher room temperature cycle performance, high temperature cycle performance, and 2C capacity retention rate.

[0193] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0194] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

Claims

1. A negative electrode material comprising: a first silicon-based material, a second silicon-based material, passivated lithium powder and an organic polymer; The particle size Dv50 of the first silicon-based material is A, 2μm≤A≤5μm, and the particle size Dv50 of the second silicon-based material is B, wherein, 4B <A<20B; The particle size Dv50 of the passivated lithium powder is C, 0.01 μm≤C≤0.1 μm.

2. The negative electrode material according to claim 1, wherein The first silicon-based material and the second silicon-based material respectively include a core, a carbon layer outside the core, and a lithium salt layer outside the carbon layer.

3. The negative electrode material according to claim 2, wherein The negative electrode material satisfies at least one of the following: (1) The core comprises at least one of silicon-carbon particles or silicon-oxygen particles; (2) The lithium salt includes at least one of LiF or Li2CO3; (3) Based on the mass of the first silicon-based material, the mass percentage of the carbon layer of the first silicon-based particle is 1% to 5.2%, and the mass percentage of the lithium salt layer is 0.53% to 2.1%; (4) Based on the mass of the second silicon-based material, the mass percentage of the carbon layer of the second silicon-based particle is 1% to 5.2%, and the mass percentage of the lithium salt layer is 0.53% to 2.1%.

4. The negative electrode material according to claim 2, wherein The average size of silicon grains in the core of the first silicon-based material is a, and the average size of silicon grains in the core of the second silicon-based material is b; 1nm≤a≤1.5nm, 1.5nm≤b≤2nm, and a<b.

5. The negative electrode material according to claim 1, wherein 0.1μm≤B≤0.5μm.

6. The negative electrode material according to claim 1, wherein The mass of the first silicon-based material is m1 g, the mass of the second silicon-based material is m2 g, the mass of the passivation lithium powder is m3 g, and the mass ratio satisfies: m1:m2:m3=100:10 to 40:0.5 to 5; Based on the mass of the negative electrode material, the mass percentage of the organic polymer is 3% to 7%.

7. The negative electrode material according to any one of claims 1 to 6, wherein The negative electrode material satisfies at least one of the following: (1) The Dv50 of the negative electrode material is 6 μm to 10 μm; (2) The Dv90 of the negative electrode material is less than or equal to 30 μm; (3) The organic polymer comprises polyurethane; (4) Based on the mass of the negative electrode material, the mass percentage of silicon element is 40% to 50%.

8. An electrochemical device comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the negative electrode sheet comprises a negative electrode active material layer, and the negative electrode active material layer comprises the negative electrode material according to any one of claims 1 to 7.

9. The electrochemical device according to claim 8, wherein: The electrolyte comprises at least one of lithium bis(trifluoromethylsulfonyl)imide or lithium bis(fluorosulfonyl)imide; Based on the mass of the electrolyte, the mass percentage of the lithium bis(trifluoromethylsulfonyl)imide and / or the lithium bis(fluorosulfonyl)imide is 0.1% to 5%.

10. A method for preparing the negative electrode material according to any one of claims 1 to 7, comprising: Providing a core of a first silicon-based material, carbon-coating the core to obtain a first intermediate, dispersing the first intermediate in water to obtain a first dispersion, adding an aqueous solution of a lithium source substance to the first dispersion to obtain a second dispersion, fully dispersing and stirring, and drying in an oven to obtain a first silicon-based material; Providing a core of a second silicon-based material, carbon-coating the core to obtain a first intermediate, dispersing the first intermediate in water to obtain a first dispersion, adding an aqueous solution of a lithium source substance to the first dispersion to obtain a second dispersion, fully dispersing and stirring, and drying in an oven to obtain a second silicon-based material; The first silicon-based material, the second silicon-based material and the passivated lithium powder are dispersed and then added with deionized water to obtain a third dispersion; a polymer is dispersed in water to obtain a fourth dispersion, the fourth dispersion is added to the third dispersion, mixed and fully stirred, and a negative electrode material is obtained by spray drying.

Citation Information

Patent Citations

  • Negative active material, preparation method thereof and lithium ion battery

    CN113113579A

  • Pre-lithiated silicon-based negative electrode material and preparation method thereof, negative electrode and battery

    CN117673287A

  • Negative pole piece as well as preparation method and application thereof

    CN118198270A

  • Negative electrode material and preparation method thereof, negative electrode plate, electrode assembly and battery

    CN118352514A

  • Negative active material for rechargeable lithium battery, negative electrode including the same and method of preparing the same, and rechargeable lithium battery including the same

    US20130045419A1

Cited By

  • Composite material, secondary battery and electronic device

    WO2026107648A1