Method for modifying bismuth oxyiodide-based composite solid polymer electrolyte and method for constructing lithium battery by using bismuth oxyiodide-based composite solid polymer electrolyte
Through the modification method of bismuth iodine-based composite solid polymer electrolyte, the problem of insufficient ion conductivity and interface stability of solid electrolyte is solved, and the improvement of high ion conductivity and mechanical strength is achieved, and high power and high energy are met. Demand for density lithium batteries.
Patent Information
- Application Number
- CN202411226238.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-07-11
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The existing solid polymer electrolyte has low ion conductivity and insufficient interfacial electrochemical stability, making it difficult to meet the requirements of high-power and high-energy density lithium batteries.
Modified bismuth iodine oxide-based composite solid polymer electrolyte is adopted to prepare modified bismuth iodine oxide by hydrothermal synthesis, and combined with lithium salt and polymer matrix to form a composite electrolyte with high ionic conductivity and high mechanical strength. Improve the interface contact between polymer and inorganic filler, improve conductivity and interface stability.
It significantly improves the ionic conductivity and cycle life of lithium batteries, enhances the mechanical strength and electrochemical stability of the batteries, and improves the energy density and power density of the batteries.
Smart Images

Figure CN119069819A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy battery materials, and specifically relates to a modification method of a bismuth oxyiodide-based composite solid polymer electrolyte, and also relates to a construction method of a lithium battery thereof. Background Art
[0002] Lithium-ion batteries are a common secondary battery widely used in various portable electronic devices, power tools, electric vehicles, energy storage systems, etc. They are widely favored for their high energy density, light weight, no memory effect, low self-discharge rate and long cycle life. However, traditional lithium-ion batteries contain liquid electrolytes, which have the risk of explosion under high temperature or high pressure. At the same time, they are prone to leakage during the cycle, reducing the safety and stability of the battery.
[0003] In view of this, it is necessary to use highly safe solid electrolytes to replace traditional liquid electrolytes. As an electrolyte material, solid polymer electrolytes have many advantages over traditional liquid electrolytes: first, solid electrolytes have higher safety because they do not leak or volatilize, thereby reducing the risk of battery accidents; second, solid electrolytes have higher chemical stability and can withstand a wider voltage range, thus making the battery cycle life longer; in addition, solid electrolytes also have higher ion transfer rates and lower internal resistance, which can improve the energy density and power density of the battery.
[0004] The research on solid polymer electrolytes began in the 1960s, initially focusing on the synthesis methods and performance regulation of polymer electrolytes. With the development of materials science and electrochemistry, the synthesis methods of solid polymer electrolytes have been continuously innovated, including solution impregnation, in-situ polymerization, interfacial polymerization, etc. At the same time, researchers are also constantly improving the ionic conductivity, mechanical properties and chemical stability of solid polymer electrolytes to meet the needs of different electrochemical devices.
[0005] At present, solid polymer electrolytes still have some defects. For example, the ionic conductivity of solid polymer electrolytes is still lower than that of liquid electrolytes. Although some progress has been made, its ionic conductivity still needs to be further improved to meet the requirements of high-power and high-energy density batteries. In addition, the interfacial stability between solid electrolytes and electrodes is one of the key factors affecting battery performance. Insufficient electrochemical stability of the interface may lead to electrolytic reactions of the electrolyte, dissolution of electrode materials and the formation of solid interfaces, thereby affecting the cycle life and safety of the battery. In response to these problems, current research focuses on finding new polymer materials, optimizing the structural design of electrolytes, improving preparation processes and improving battery interface engineering. Summary of the invention
[0006] The present invention aims at the technical status quo that the ion conductivity and interface electrochemical stability of the current solid electrolyte cannot meet the use requirements, and provides a modification method of a bismuth oxyiodide-based composite solid polymer electrolyte and a lithium battery construction method thereof.
[0007] The solid polymer electrolyte of the present invention is composited with an ion-conducting polymer and a metal iodine oxide, and the modification process is summarized as follows: first, a modified iodine oxide is prepared by a hydrothermal synthesis method, and the metal iodine oxide is modified by doping, calcination and the like; then, the modified iodine oxide is dispersed in an organic solvent, a lithium salt is added, and a polymer matrix is dispersed in the solvent, stirred until uniform, cast into a film, and vacuum dried to obtain a composite solid polymer electrolyte.
[0008] The electrolyte has the characteristics of high ionic conductivity and high mechanical strength. Bismuth iodide can react with the lithium negative electrode in situ to form SEI with lithium iodide, inhibiting the growth of dendrites. By modifying bismuth iodide, the interface contact between the polymer and the inorganic filler can be improved, and the ionic conductivity of the composite electrolyte can be improved. The composite electrolyte can be matched with lithium iron phosphate, NCM811, and sulfur positive electrodes to achieve high conductivity and high stability solid-state batteries.
[0009] Specifically, the technical solution adopted by the present invention is as follows:
[0010] In a first aspect, the present invention provides a method for modifying a bismuth oxyiodide-based composite solid polymer electrolyte, comprising the following steps:
[0011] (1) Solution mixing
[0012] Add bismuth nitrate pentahydrate to an organic solvent, selectively dope other metal salt hydrates according to different proportions, heat and stir evenly at 50° C., and obtain a clear solution after fully dissolving; add iodide to an organic solvent, heat and stir until fully dissolved, and then slowly add it to the clear solution of the bismuth metal salt;
[0013] (2) Preparation of metallic iodine bismuth oxide compounds
[0014] After the mixed solution is fully stirred, the mixed solution is placed in a reaction kettle by a one-step solvent thermal synthesis method, and hydrothermally synthesized at 120-240° C. for 2-24 hours. After the reaction is completed, the mixed solution is washed with ethanol and deionized water for multiple times, and then dried at 80° C. to obtain a metal iodine bismuth oxide compound;
[0015] (3) Preparation of defective bismuth iodide compounds
[0016] The prepared metal iodine bismuth oxide compound is placed in a tube furnace, the temperature is gradually increased in an air or hydrogen atmosphere, and the iodine bismuth oxide compound is calcined at a constant temperature of 200 to 500° C. for 2 hours to obtain a defective iodine bismuth oxide compound after annealing;
[0017] (4) Preparation of solid polymer electrolyte
[0018] After the polymer matrix is vacuum dried at 60°C, the polymer matrix and lithium salt are stirred and mixed together in an organic solvent; a metal iodine bismuth oxide compound or a defective iodine bismuth oxide compound is added to the mixed solution in different mass ratios and magnetically stirred to obtain a slurry, the slurry is poured into a mold, and after vacuum drying at 60°C, a composite solid polymer electrolyte membrane is obtained.
[0019] The preferred scheme of the above steps is as follows:
[0020] In step (1), the concentration of bismuth nitrate pentahydrate is 0.1-0.5 mol / L, and the concentration of iodide is 0.1-0.5 mol / L;
[0021] The organic solvent is selected from ethylene glycol, propylene glycol or butylene glycol;
[0022] The dissolved salt hydrate of other doped metals includes any one or more combinations of cerium nitrate, lanthanum nitrate, titanium chloride, iron chloride, zinc nitrate hexahydrate, zirconium chloride octahydrate, molybdenum chloride, antimony chloride, and tungsten chloride;
[0023] The iodide is selected from any one of potassium iodide and sodium iodide;
[0024] The molar ratio between bismuth nitrate pentahydrate and other metal soluble salts is 9:1;
[0025] After adding iodide, the mixture was heated and stirred at 50°C for 20 min.
[0026] In step (4), the polymer matrix is selected from any one of polyethylene oxide, polyvinylidene-hexafluoropropylene, and polyacrylonitrile;
[0027] The lithium salt is selected from any one of lithium trifluoromethanesulfonate, lithium nitrate, lithium hexafluorophosphate, and lithium borohydride;
[0028] The organic solvent is selected from any one of acetonitrile, methanol and N-methylpyrrolidone;
[0029] The proportion of the metal iodine bismuth oxide compound or the defective iodine bismuth oxide compound in the polymer matrix is 0.01-30%wt;
[0030] The molar ratio between the polymer matrix and the lithium salt is 20:1 to 10:1.
[0031] The thickness of the composite solid polymer electrolyte membrane is 30-150 μm.
[0032] In a second aspect, the present invention provides a bismuth oxyiodide-based composite solid polymer electrolyte membrane, which is prepared by the method described above.
[0033] In a third aspect, the present invention provides a method for constructing a bismuth oxyiodide-based composite solid-state lithium battery, comprising the following steps:
[0034] (1) 75 wt% of positive electrode active material, 10 wt% of carbon black and 15 wt% of PVDF were dispersed in N-methylpyrrolidone solvent, stirred evenly and coated on aluminum foil; then the solvent was removed under vacuum at 60°C and the foil was cut into discs of a certain diameter;
[0035] (2) A battery shell of suitable type is selected, and a 1 mm stainless steel sheet is used as the current collector. The battery is assembled in the order of lithium sheet, bismuth iodide-based composite solid polymer electrolyte membrane, positive electrode sheet, and current collector from the negative electrode to the positive electrode.
[0036] Preferably, the positive electrode active material is selected from any one of lithium iron phosphate, NCM811, and carbon / sulfur composite positive electrode materials;
[0037] The loading amount of the positive electrode is 2-4 mg / cm 2 .
[0038] In a fourth aspect, the present invention provides a corresponding bismuth oxyiodide-based composite solid-state lithium battery, which is constructed using the method described above.
[0039] Experimental test results show that the ionic conductivity of the battery constructed using the method of the present invention at room temperature is improved compared to the battery without adding metal iodine bismuth oxide compound filler, with the lowest improvement being 1.84 times.
[0040] Beneficial technical effects of the present invention:
[0041] (1) The modified iodine oxide filler solid polymer electrolyte prepared by the present invention has the characteristics of high ion conductivity and high mechanical strength. The glass transition temperature of the polymer is reduced by adding iodine oxide filler, so that the conductivity of the composite solid polymer electrolyte at room temperature is increased. The inorganic filler can adsorb trifluoromethanesulfonate anions, promote the dissociation of lithium salts, and improve the ion mobility of the solid electrolyte; at the same time, the addition of inorganic fillers also improves the mechanical strength of the composite solid polymer electrolyte, improving the disadvantage that the solid polymer electrolyte is difficult to process due to poor mechanical strength.
[0042] (2) The modified bismuth iodide filler solid polymer electrolyte of the present invention can improve the interface contact between the electrolyte and the lithium negative electrode. The lithium negative electrode and the bismuth iodide can form hard lithium iodide in situ at the interface, which can effectively inhibit the growth of dendrites and improve the cycle life of the solid-state battery.
[0043] (3) The modified bismuth iodide filler solid polymer electrolyte of the present invention can improve the cycle performance of the battery. The CEI buffer layer formed at the interface between the positive electrode and the polymer can effectively inhibit the structural damage and capacity attenuation of the positive electrode material at high temperature, thereby improving the stability of the battery under long cycles.
[0044] The projects on which this invention is based are as follows: Project type: Shanghai Science and Technology Commission, Basic Research Special Zone Plan; Project number: 22T01400100-18; Project name: Design, preparation and application of key materials for solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is a field emission scanning electron microscope photograph of the bismuth iodide oxide prepared in Example 1;
[0046] Figure 2 is a scanning electron microscope photograph of the composite solid polymer electrolyte prepared in Example 2;
[0047] Figure 3 is the EPR spectrum of the oxygen-deficient bismuth oxyiodide prepared in Example 3;
[0048] Figure 4 The cycle performance of the doped bismuth iodide oxide composite solid electrolyte symmetrical battery prepared in Example 3;
[0049] Figure 5 The volt-ampere characteristic curve of the bismuth oxyiodide composite solid polymer electrolyte lithium iron phosphate full battery constructed in Example 5;
[0050] Figure 6 A flow chart of the composite solid electrolyte of the present invention. DETAILED DESCRIPTION
[0051] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0052] Example 1
[0053] A. Modification and construction of bismuth iodide-based composite solid polymer electrolytes
[0054] (1) Add 4.85 g of bismuth nitrate pentahydrate (BiNO3·5H2O) to 30 ml of ethylene glycol, add 1.66 g of potassium iodide to 30 ml of ethylene glycol, stir thoroughly to dissolve, slowly pour the ethylene glycol solution of potassium iodide into the ethylene glycol solution of bismuth nitrate pentahydrate and mix thoroughly, heat and stir at 50°C for 20 min, then transfer the mixed solution to a hydrothermal reactor and perform a hydrothermal reaction at 180°C for 2 h.
[0055] (2) The mixed solution after the reaction was centrifuged and washed three times in ethanol and deionized water respectively, and then dried at 80° C. for 10 hours to obtain a bismuth iodide filler. The constructed bismuth iodide filler was examined under a microscope to obtain Figure 1 The field emission scanning electron microscope photograph shown shows that the prepared bismuth iodide oxide filler is in the shape of a flower ball and is self-assembled by stacked nanosheets.
[0056] (3) PEO was used as the polymer matrix, bismuth iodide as the filler, and LiTFSI as the lithium salt to prepare a PEO-based composite solid electrolyte membrane by solution casting: First, PEO was vacuum dried at 60°C for 2 h, 2 g PEO and 0.725 g LiTFSI were added to a stirring bottle, and an appropriate amount of acetonitrile was added to mix. 0.1 g bismuth iodide was added to the mixed solution and magnetically stirred for 12 h. After stirring, the obtained slurry was cast into a polytetrafluoroethylene mold in a glove box and placed in a vacuum drying oven at 60°C for 24 h to obtain a composite solid polymer electrolyte membrane.
[0057] B. Construction of bismuth iodide composite solid polymer electrolyte full battery
[0058] See the process Figure 6 , the main steps are as follows:
[0059] (1) 240 mg of NCM811 active substance, 30 mg of carbon black and 30 mg of PVDF were dispersed in N-methylpyrrolidone solvent, stirred evenly and coated on aluminum foil. The NMP solvent was then removed under vacuum at 60 °C and the foil was cut into 8 mm diameter discs. The active substance loading was about 2.4 mg / cm 2 .
[0060] (2) A 2032-type battery case was used, and a 1 mm stainless steel sheet was used as the current collector. The battery was assembled in the order of lithium sheet, polymer electrolyte sheet, positive electrode sheet, and current collector from the negative electrode to the positive electrode to conduct electrochemical performance testing.
[0061] Example 2
[0062] A. Modification and construction of bismuth iodide-based composite solid polymer electrolytes
[0063] (1) Add 4.85 g of bismuth nitrate pentahydrate (BiNO3·5H2O) to 30 ml of ethylene glycol, add 1.66 g of potassium iodide to 30 ml of ethylene glycol, stir thoroughly to dissolve, slowly pour the ethylene glycol solution of potassium iodide into the ethylene glycol solution of bismuth nitrate pentahydrate and mix thoroughly, heat and stir at 50°C for 20 min, then transfer the mixed solution to a hydrothermal reactor and perform a hydrothermal reaction at 120°C for 24 h.
[0064] (2) washing the mixed solution after the reaction in ethanol and deionized water by centrifugation three times respectively, and then drying at 80° C. for 10 hours to obtain bismuth iodide filler;
[0065] (3) placing the bismuth iodide filler in a tube furnace, calcining at a constant temperature of 500° C. for 2 hours in an air atmosphere, and annealing to obtain bismuth iodide with oxygen defects.
[0066] (4) Using PVDF-HFP as the polymer matrix, bismuth iodide as the filler, and LiTFSI as the lithium salt, a PVDF-HFP-based composite solid electrolyte membrane was prepared by solution casting: First, PVDF-HFP was vacuum dried at 60°C for 2h, 2g PVDF-HFP and 1g LiTFSI were added to a stirring bottle, and an appropriate amount of acetonitrile was added to mix. 0.2g bismuth iodide was added to the mixed solution and magnetically stirred for 12h. After stirring, the obtained slurry was cast into a polytetrafluoroethylene mold in a glove box and placed in a vacuum drying oven at 60°C for 24h to obtain a composite solid polymer electrolyte membrane.
[0067] The composite solid polymer electrolyte constructed in this example was examined under a microscope to obtain Figure 2 The field emission scanning electron microscope photo is shown. The results show that the surface of the prepared composite solid polymer electrolyte is smooth, indicating that the filler is evenly dispersed in the polymer film.
[0068] B. Construction of bismuth iodide composite solid polymer electrolyte full battery
[0069] (1) Disperse 240 mg of lithium iron phosphate active material, 30 mg of carbon black and 30 mg of PVDF in N-methylpyrrolidone solvent, stir evenly and apply on aluminum foil. Then remove the NMP solvent under vacuum at 60°C and cut into discs with a diameter of 8 mm. The active material loading is about 2.4 mg / cm 2 .
[0070] (2) A 2032-type battery case was used, and a 1 mm stainless steel sheet was used as the current collector. The battery was assembled in the order of lithium sheet, polymer electrolyte sheet, positive electrode sheet, and current collector from the negative electrode to the positive electrode, and the electrochemical performance was tested.
[0071] Example 3
[0072] A. Modification and construction of bismuth iodide-based composite solid polymer electrolytes
[0073] (1) Add 4.85 g of bismuth nitrate pentahydrate (BiNO3·5H2O) to 30 ml of ethylene glycol, add 1.66 g of potassium iodide to 30 ml of ethylene glycol, stir thoroughly to dissolve, slowly pour the ethylene glycol solution of potassium iodide into the ethylene glycol solution of bismuth nitrate pentahydrate and mix thoroughly, heat and stir at 50°C for 20 min, then transfer the mixed solution to a hydrothermal reactor and perform a hydrothermal reaction at 180°C for 2 h.
[0074] (2) washing the mixed solution after the reaction in ethanol and deionized water by centrifugation three times respectively, and then drying at 80° C. for 10 hours to obtain bismuth iodide filler;
[0075] (3) placing the bismuth iodide filler in a tube furnace, calcining it at a constant temperature of 300° C. for 2 hours in a hydrogen atmosphere, and annealing it to obtain defective bismuth iodide.
[0076] The bismuth iodide prepared in this example was subjected to EPR testing, and the results were as follows: Figure 3 As shown, the characteristic peak of oxygen vacancy appears at the position of g=2.003 in bismuth iodide oxide reduced by hydrogen, indicating that oxygen vacancies are successfully introduced into bismuth iodide oxide through hydrogen reduction. The oxygen vacancies can adsorb trifluoromethanesulfonate anions as Lewis bases as Lewis acids, promoting the dissociation of lithium salts.
[0077] (4) Using PAN as the polymer matrix, bismuth iodide as the filler, and LiNO3 as the lithium salt,
[0078] The PEO-based composite solid electrolyte membrane was prepared by solution casting. First, PEO was vacuum dried at 60°C for 2h, 2g PAN and 0.725g LiNO3 were added to a stirring bottle, and an appropriate amount of acetonitrile was added to mix. 0.2g bismuth iodide oxide was added to the mixed solution and magnetically stirred for 12h. After stirring, the obtained slurry was cast into a polytetrafluoroethylene mold in a glove box and placed in a vacuum drying oven at 60°C for 24h to obtain a composite solid polymer electrolyte membrane.
[0079] B. Construction of bismuth iodide composite solid polymer electrolyte full battery
[0080] (1) 240 mg of sulfur / carbon active material, 30 mg of carbon black and 30 mg of PVDF were dispersed in N-methylpyrrolidone solvent, stirred evenly and coated on aluminum foil. The NMP solvent was then removed under vacuum at 60°C and the foil was cut into 8 mm diameter discs. The active material loading was about 2.4 mg / cm 2 .
[0081] (2) A 2032-type battery case was used, and a 1 mm stainless steel sheet was used as the current collector. The battery was assembled in the order of lithium sheet, polymer electrolyte sheet, positive electrode sheet, and current collector from the negative electrode to the positive electrode, and the electrochemical performance was tested.
[0082] Example 4
[0083] A. Modification and construction of bismuth iodide-based composite solid polymer electrolytes
[0084] (1) Add 4.365 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.326 g of cerium nitrate (CeNO3) to 30 ml of ethylene glycol, add 1.66 g of potassium iodide to 30 ml of ethylene glycol, stir thoroughly to dissolve, slowly pour the ethylene glycol solution of potassium iodide into the ethylene glycol solution of bismuth nitrate pentahydrate and mix thoroughly, heat and stir at 50°C for 20 min, then transfer the mixed solution to a hydrothermal reactor. Hydrothermally react at 180°C for 2 h;
[0085] (2) washing the mixed solution after the reaction in ethanol and deionized water by centrifugation three times respectively, and then drying at 80° C. for 10 hours to obtain a cerium-doped bismuth iodide filler;
[0086] (3) Using PEO as the polymer matrix, bismuth iodide as the filler, and LiTFSI as the lithium salt, a PEO-based composite solid electrolyte membrane was prepared by solution casting: First, PEO was vacuum dried at 60°C for 2 h, 2 g PEO and 0.725 g LiTFSI were added to a stirring bottle, and an appropriate amount of acetonitrile was added to mix. 0.1 g bismuth iodide was added to the mixed solution and magnetically stirred for 12 h. After stirring, the obtained slurry was cast into a polytetrafluoroethylene mold in a glove box and placed in a vacuum drying oven at 60°C for 24 h to obtain a composite solid polymer electrolyte membrane.
[0087] B. Construction of bismuth iodide composite solid polymer electrolyte full battery
[0088] (1) Disperse 240 mg of lithium iron phosphate active material, 30 mg of carbon black and 30 mg of PVDF in N-methylpyrrolidone solvent, stir evenly and apply on aluminum foil. Then remove the NMP solvent under vacuum at 60°C and cut into discs with a diameter of 8 mm. The active material loading is about 2.4 mg / cm 2 .
[0089] (2) A 2032-type battery case was used, and a 1 mm stainless steel sheet was used as the current collector. The battery was assembled in the order of lithium sheet, polymer electrolyte sheet, positive electrode sheet, and current collector from the negative electrode to the positive electrode, and the electrochemical performance was tested.
[0090] The voltammetric curves of the constructed full battery were tested at different scan rates. Figure 4 As shown, standard redox peaks appeared in the voltammetric characteristic curves at different scan rates, indicating that the full battery assembled by the solid composite polymer electrolyte has good electrochemical performance.
[0091] Example 5
[0092] A. Modification and construction of bismuth iodide-based composite solid polymer electrolytes
[0093] (1) Add 8.73 g of bismuth nitrate pentahydrate (BiNO3·5H2O) and 0.378 g of zinc nitrate (ZnNO3) to 30 ml of ethylene glycol, add 3.32 g of potassium iodide to 30 ml of ethylene glycol, stir thoroughly to dissolve, slowly pour the ethylene glycol solution of potassium iodide into the ethylene glycol solution of bismuth nitrate pentahydrate and mix thoroughly, heat and stir at 50°C for 20 min, then transfer the mixed solution to a hydrothermal reactor. Hydrothermally react at 180°C for 2 h;
[0094] (2) washing the mixed solution after the reaction in ethanol and deionized water by centrifugation three times respectively, and then drying at 80° C. for 10 hours to obtain a zinc-doped bismuth iodide filler;
[0095] (3) Using PAN as the polymer matrix, bismuth iodide as the filler, and LiPF6 as the lithium salt, a PEO-based composite solid electrolyte membrane was prepared by solution casting: First, PAN was vacuum dried at 60°C for 2h, 2g PAN and 0.9g LiPF6 were added to a stirring bottle, and 40ml methanol was added to mix. 0.1g zinc-doped bismuth iodide was added to the mixed solution and magnetically stirred for 12h. After stirring, the obtained slurry was cast into a polytetrafluoroethylene mold in a glove box and placed in a vacuum drying oven at 60°C for 24h to obtain a composite solid polymer electrolyte membrane.
[0096] B. Construction of bismuth iodide composite solid polymer electrolyte full battery
[0097] (1) 240 mg of NCM811 active substance, 30 mg of carbon black and 30 mg of PVDF were dispersed in N-methylpyrrolidone solvent, stirred evenly and coated on aluminum foil. The NMP solvent was then removed under vacuum at 60°C and the foil was cut into 8 mm diameter discs. The active substance loading was about 2.4 mg / cm 2 .
[0098] (2) A 2032-type battery case was used, and a 1 mm stainless steel sheet was used as the current collector. The battery was assembled in the order of lithium sheet, polymer electrolyte sheet, positive electrode sheet, and current collector from the negative electrode to the positive electrode, and the electrochemical performance was tested.
[0099] Comparative Example 1
[0100] The composite solid polymer electrolyte was prepared and a battery was constructed by the method of Example 1, except that no modified bismuth iodide oxide composite was added in this comparative example 1.
[0101] A. Modification and construction of composite solid polymer electrolytes
[0102] (1) PEO was used as the polymer matrix and LiTFSI was used as the lithium salt to prepare a PEO-based solid electrolyte membrane by solution casting. First, PEO was vacuum dried at 60°C for 2 h, 2 g PEO and 0.1 g LiTFSI were added to a stirring bottle, and 40 ml acetonitrile was added to mix. After stirring, the obtained slurry was cast into a polytetrafluoroethylene mold in a glove box and placed in a vacuum drying oven at 60°C for 24 h to obtain a composite solid polymer electrolyte membrane.
[0103] B. Construction of composite solid polymer electrolyte full battery
[0104] (1) Disperse 240 mg of lithium iron phosphate active material, 30 mg of carbon black and 30 mg of PVDF in N-methylpyrrolidone solvent, stir evenly and apply on aluminum foil. Then remove the NMP solvent under vacuum at 60°C and cut into discs with a diameter of 8 mm. The active material loading is about 2.4 mg / cm 2 .
[0105] (2) A 2032-type battery case was used, and a 1 mm stainless steel sheet was used as the current collector. The battery was assembled in the order of lithium sheet, polymer electrolyte sheet, positive electrode sheet, and current collector from the negative electrode to the positive electrode to conduct electrochemical performance testing.
[0106] The conductivity of the PEO solid electrolytes prepared in Examples 1 to 5 and Comparative Example 1 was tested under the same conditions. The results are shown in Table 1 below. The conductivity of the PEO solid electrolytes added with the modified bismuth oxyiodide composite filler in Examples 1 to 5 is significantly better than that in Comparative Example 1. The improvement of the conductivity of the PEO solid electrolyte by the defective bismuth oxyiodide composite is better than that of the bismuth oxyiodide composite without defective modification. The oxygen-defective bismuth oxyiodide has the best improvement effect, followed by the zinc-doped bismuth oxyiodide.
[0107] Table 1. Test results of conductivity of PEO solid electrolytes prepared in Examples 1 to 5 and Comparative Example 1
[0108]
[0109] In summary, the addition of bismuth oxyiodide filler significantly improved the ionic conductivity of the PEO solid polymer electrolyte. Targeted modification and design of bismuth oxyiodide can improve the interfacial contact between bismuth oxyiodide and PEO, further improving the ionic conductivity.
[0110] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A method for modifying a bismuth oxyiodide-based composite solid polymer electrolyte, It is characterized in that The steps include: (1) Solution mixing Add bismuth nitrate pentahydrate to an organic solvent, selectively dope other metal hydrates according to different proportions, heat and stir evenly at 50° C., and obtain a clear solution after it is fully dissolved; The iodide is added to an organic solvent, heated and stirred to fully dissolve, and then slowly added to the clear solution of the bismuth metal salt; (2) Preparation of metallic iodine bismuth oxide compounds After the mixed solution is fully stirred, the mixed solution is placed in a reaction kettle by a one-step solvent thermal synthesis method, and hydrothermally synthesized at 120-240° C. for 2-24 hours. After the reaction is completed, the mixed solution is washed with ethanol and deionized water for multiple times, and then dried at 80° C. to obtain a metal iodine bismuth oxide compound; (3) Preparation of defective bismuth iodide compounds The prepared metal iodine bismuth oxide compound is placed in a tube furnace, the temperature is gradually increased in an air or hydrogen atmosphere, and the iodine bismuth oxide compound is calcined at a constant temperature of 200 to 500° C. for a certain period of time to obtain a defective iodine bismuth oxide compound after annealing; (4) Preparation of solid polymer electrolyte After the polymer matrix is dried under vacuum at 60° C., the polymer matrix and the lithium salt are stirred and mixed in an organic solvent; A metal iodine bismuth oxide compound or a defective iodine bismuth oxide compound is added to a mixed solution in different mass ratios and magnetically stirred to obtain a slurry. The slurry is poured into a mold and vacuum dried at 60° C. to obtain a composite solid polymer electrolyte membrane.
2. The method for modifying the bismuth oxyiodide-based composite solid polymer electrolyte according to claim 1, characterized in that: in, In step (1), the concentration of bismuth nitrate pentahydrate is 0.1-0.5 mol / L, and the concentration of iodide is 0.1-0.5 mol / L; The organic solvent is selected from ethylene glycol, propylene glycol or butylene glycol; The dissolved salt hydrate of other doped metals includes any one or more combinations of cerium nitrate, lanthanum nitrate, titanium chloride, iron chloride, zinc nitrate hexahydrate, zirconium chloride octahydrate, molybdenum chloride, antimony chloride, and tungsten chloride; The iodide is selected from any one of potassium iodide and sodium iodide.
3. The method for modifying the bismuth oxyiodide-based composite solid polymer electrolyte according to claim 2, characterized in that: in, The molar ratio between bismuth nitrate pentahydrate and other metal soluble salts is 9:1; After adding iodide, the mixture was heated and stirred at 50°C for 20 min.
4. The method for modifying the bismuth oxyiodide-based composite solid polymer electrolyte according to claim 1, characterized in that: in, In step (3), the constant temperature calcination time is 2 hours.
5. The method for modifying the bismuth oxyiodide-based composite solid polymer electrolyte according to claim 1, characterized in that: in, In step (4), the polymer matrix is selected from any one of polyethylene oxide, polyvinylidene-hexafluoropropylene, and polyacrylonitrile; The lithium salt is selected from any one of lithium trifluoromethanesulfonate, lithium nitrate, lithium hexafluorophosphate, and lithium borohydride; The organic solvent is selected from any one of acetonitrile, methanol and N-methylpyrrolidone.
6. The method for modifying the bismuth oxyiodide-based composite solid polymer electrolyte according to claim 1, characterized in that: in, The proportion of the metal iodine bismuth oxide compound or the defective iodine bismuth oxide compound in the polymer matrix is 0.01-30%wt; The molar ratio between the polymer matrix and the lithium salt is 20:1 to 10:1, The thickness of the composite solid polymer electrolyte membrane is 30-150 μm.
7. A bismuth iodide-based composite solid polymer electrolyte membrane, It is characterized in that The method is used to prepare the product according to any one of claims 1 to 6.
8. A method for constructing a bismuth iodide-based composite solid-state lithium battery, It is characterized in that The steps include: (1) 75 wt% of positive electrode active material, 10 wt% of carbon black and 15 wt% of PVDF were dispersed in N-methylpyrrolidone solvent, stirred evenly and coated on aluminum foil; then the solvent was removed under vacuum at 60°C and the foil was cut into discs of a certain diameter; (2) A battery shell of suitable type is selected, and a 1 mm stainless steel sheet is used as the current collector. The battery is assembled in the order of lithium sheet, bismuth iodide-based composite solid polymer electrolyte membrane, positive electrode sheet, and current collector from the negative electrode to the positive electrode.
9. The method for constructing a bismuth oxyiodine-based composite solid-state lithium battery according to claim 8, characterized in that: in, The positive electrode active material is selected from any one of lithium iron phosphate, NCM811, and carbon / sulfur composite positive electrode materials; The loading amount of the positive electrode sheet is 2-4 mg / cm 2 .
10. A bismuth iodide-based composite solid-state lithium battery, It is characterized in that The method according to claim 8 or 9 is used to construct the product.
Citation Information
Patent Citations
Applications of nanometer lamellar BiOI as electrode material
CN108483494A
Composite solid electrolyte, preparation thereof and application of composite solid electrolyte in lithium battery
CN118040057A
Method for designing BiOCl chloride ion solid electrolyte based on Mg doping
CN118062885A
Solid electrolyte battery
JP1984009862A
Cited By
Bismuth oxide halide-polyvinylidene fluoride based composite solid electrolyte membrane for high-energy density battery and preparation method of bismuth oxide halide-polyvinylidene fluoride based composite solid electrolyte membrane
CN119764550A
Method for in-situ preparation of bismuth oxyhalide-PVDF-based composite solid electrolyte membrane
CN119764551A
A method for in-situ preparation of bismuth oxyhalide-pvdf-based composite solid electrolyte membrane
CN119764551B
Composite solid electrolyte, preparation method thereof and solid lithium metal battery
CN121307157A