Porous ceramic framework and preparation method therefor, and double-bionic resin ceramic composite material

By designing a porous ceramic skeleton with a chamfered three-cylinder structure and preparing ceramic resin composite materials, the problem of unstable porosity and permeability of existing denture materials has been solved, a three-dimensional through-structure and high bionics have been achieved, and the denture materials have been improved. performance and application range.

WO2024198488A1PCT designated stage expired Publication Date: 2024-10-03AIDITE (QINHUANGDAO) TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/137096
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-12-07
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing denture materials have poor controllability of porosity, pore size, and pore distribution, and cannot achieve a three-dimensional through-structure, resulting in unstable permeability of resin materials and limiting the application of the material in the field of actual denture repair.

Method used

By designing a porous ceramic skeleton, using chamfered three-cylinder structure and cubic unit cell structure, the pore diameter is controlled to decrease step by step, forming a porous ceramic skeleton with a porosity that gradually changes from the bottom to the top, combined with the photo-curing 3D printing of ceramic resin slurry and Modification treatment was carried out to prepare double bionic resin ceramic composite materials.

Benefits of technology

It achieves controllability of the porosity, pore size, and pore distribution of the porous ceramic skeleton, improves the permeability and overall performance of the resin material, enhances the stability and bionics of the denture material, and is suitable for a wide range of denture repair applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023137096_03102024_PF_FP_ABST
    Figure CN2023137096_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A porous ceramic framework and a preparation method therefor, and a double-bionic resin ceramic composite material. The porous ceramic framework is of a three-dimensional structure formed by a plurality of unit cell structures arranged in an array; the unit cell structure is a cube provided with a through hole; the through hole is of a chamfered three-cylinder structure, the sizes of three cylinders in the three-cylinder structure are the same, and the length of the cylinders in the three-cylinder structure is the same as the side length of the cube. The porosity of hole units is controlled by changing a parameter D, a porous ceramic framework the porosity of which gradually changes from the bottom to the top is constructed, and bionics of a resin-infiltrated ceramic material and human teeth are achieved to the maximum extent in terms of physical performance; the porosity, pore diameter and pore distribution of the provided porous ceramic framework are highly controllable, a three-dimensional through structure can be realized, and the bionics of a resin-infiltrated ceramic material and human teeth is realized to the greatest extent in terms of structure.
Need to check novelty before this filing date? Find Prior Art

Description

A porous ceramic skeleton and its preparation method and a dual-bionic resin ceramic composite material

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 30, 2023, with application number CN202310322668.7 and invention name “A porous ceramic skeleton, its preparation method and a dual-bionic resin ceramic composite material”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the technical field of dentures, and in particular to a porous ceramic skeleton and a preparation method thereof, as well as a dual-bionic resin-ceramic composite material. Background Art

[0003] Dentures, commonly known as "false teeth", refer to restorations made after partial or complete loss of normal teeth in the upper and lower jaws of the human body. They can replace the missing teeth to achieve their normal chewing, vocalization, aesthetics and other functions, thereby alleviating the various inconveniences caused by tooth loss to patients.

[0004] At present, the denture materials used in clinical practice include ceramic-resin composite materials, in which porous ceramic skeletons are prepared by combining pore-forming agent method, freeze-drying method, foaming method, etc. with sintering method. The liquid resin is vacuum-impregnated and solidified into shape, thereby mimicking the material properties of natural teeth inorganic-organic composites.

[0005] Application document CN108743405A describes a process of preparing a slurry, freeze-casting, and vacuum freeze-drying to produce an oriented porous green body with a lamellar structure. The green body is then surface-modified and impregnated with a liquid resin monomer. After resin polymerization, the resulting biomimetic zirconia / resin composite material for dentures is obtained. This material has a flexural strength of 118 MPa to 282 MPa and a hardness of 1.8 to 3.4 GPa, with physical properties similar to those of natural teeth.

[0006] In the application document with publication number CN106830928A, a resin / ceramic composite material was prepared through compression molding, high-temperature sintering, surface treatment, infiltration treatment and resin polymerization steps. The material prepared by this method has a flexural strength of not less than 130 MPa, a compressive strength of not less than 300 MPa, an elastic modulus of not less than 8.8 GPa, and a hardness of 0.6 to 5.3 GPa.

[0007] However, the porosity, pore size, and pore distribution of the above composite materials are poorly controllable, and a three-dimensional through-hole structure cannot be achieved, resulting in a high degree of randomness in the penetration of the resin material, which in turn leads to insufficient stability in the performance of the material, and its application in the actual field of denture restoration is limited.

[0008] Summary of the Invention

[0009] In view of this, the purpose of the present application is to provide a porous ceramic skeleton and a preparation method thereof, as well as a dual-bionic resin-ceramic composite material. The present application controls the porosity of the pore unit by changing the parameter D to construct a porous ceramic skeleton whose porosity gradually changes from the bottom to the top. The porosity, pore size and pore distribution of the skeleton structure are highly controllable, and can achieve three-dimensional penetration, further control the permeability of the resin material, make the performance of the material stable, and realize wide application in the actual field of denture restoration.

[0010] In order to achieve the above-mentioned invention objectives, this application provides the following technical solutions:

[0011] The present application provides a porous ceramic skeleton, which is a three-dimensional structure formed by an array of multiple unit cell structures; the unit cell structure is a cube provided with a through hole, and the through hole is a three-cylinder structure with a chamfered corner, and the three cylinders in the three-cylinder structure have the same size, and the length of the cylinder in the three cylinders is the same as the side length of the cube;

[0012] In order from bottom to top, the pore size of the unit cell structure in the porous ceramic skeleton decreases step by step, each level has 1 to 5 layers, and the pore size of the unit cell structure in each level is the same; the pore size of the unit cell structure is measured by the diameter of the cylinder in the three cylinders;

[0013] The array is a unit cell structure in each level arranged in an array in the x-axis, y-axis and z-axis directions respectively.

[0014] Preferably, the pore size of the unit cell structure is 0.01 to 1.9 mm;

[0015] The porosity of the porous ceramic skeleton is calculated by Formula I: P = 59.76D - 14.02 Formula I;

[0016] In formula I: D is the pore size of the unit cell structure, in mm; P is the porosity of the porous ceramic skeleton, in %.

[0017] Preferably, the porosity of the porous ceramic skeleton is 3-70%; and the pore size difference between two adjacent unit cell structures is 0.01-1 mm.

[0018] The present application also provides a method for preparing the porous ceramic skeleton described in the above technical solution, comprising the following steps:

[0019] According to the structural design model of the porous ceramic skeleton according to any one of claims 1 to 3, a ceramic resin slurry is then used for light-curing 3D printing to obtain the porous ceramic skeleton.

[0020] Preferably, the steps of constructing the model are:

[0021] (1) Cylindrical models with the same center point and the same diameter D1 were constructed in the x, y, and z directions to obtain a three-cylindrical structure model. Each cylindrical model was Boolean subtracted from a cube with a side length of 2 mm to obtain a porous ceramic skeleton unit body with a pore size of D1;

[0022] (2) chamfering the corners of the porous ceramic skeleton unit body with a radius of R = (2-D1) / 2 to obtain a unit cell structure with a pore size of D1;

[0023] (3) Arraying the unit cell structure in the x-, y-, and z-axis directions to obtain a unit cell structure skeleton with an aperture of D1;

[0024] (4) Repeat steps (1) to (3), replacing D1 with D2 to obtain a unit cell structure skeleton with a pore size of D2;

[0025] (5) Repeat step (4) n times, replacing D1 each time, and replacing D1 with D3, D4, ..., D according to the number of repetitions. n , n≥3, and D1~D n Increase or decrease in sequence to obtain an aperture of D3~D n The unit cell structure skeleton;

[0026] (6) Set the aperture to D1~D n The multi-layer unit cell structure skeleton is superimposed in the order of increasing or decreasing pore size to obtain a porous ceramic skeleton model.

[0027] Preferably, the ceramic resin slurry comprises the following components in percentage by mass:

[0028] Preferably, the ceramic material includes one or more of zirconium oxide powder, lithium disilicate ceramic particles, sodium aluminum silicate ceramic particles, alumina ceramics, feldspar ceramic powder, barium glass powder and hydroxyapatite;

[0029] The resin material includes one or more of dimethacrylate urethane, triethylene glycol dimethacrylate, bisphenol A glycidyl methacrylate, ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; the initiator includes one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, and 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyloxime);

[0030] The dispersant includes one or more of polyethylene glycol, Triton X100, polycaprolactone dispersant, polyacrylic acid, polyethyleneimine and sodium dodecylbenzenesulfonate;

[0031] The auxiliary agent includes one or more of a leveling agent, a defoaming agent and a color stabilizer.

[0032] The present application also provides a method for preparing a dual-bionic resin-ceramic composite material, comprising the following steps: subjecting the porous ceramic skeleton to debinding treatment, pre-sintering, modification, drying, infiltration treatment and post-curing treatment in sequence to obtain a dual-bionic resin-ceramic composite material; the modification modifier is a silane coupling agent.

[0033] Preferably, the temperature of the debinding treatment is 300-600°C and the time is 1-10 hours; the debinding treatment is carried out in air or nitrogen atmosphere; the modification is to immerse the pre-sintered porous ceramic skeleton in a silane coupling agent, and the immersion time is 4-6 hours; the post-curing treatment includes photocuring and thermal curing performed in sequence.

[0034] The present application also provides a dual-bionic resin-ceramic composite material prepared by the preparation method described in the above technical solution.

[0035] The present application provides a porous ceramic skeleton, which is a three-dimensional structure formed by an array of several unit cell structures; the unit cell structure is a cube provided with a through hole, and the through hole is a chamfered three-cylinder structure, the three cylinders in the three-cylinder structure have the same size, and the length of the cylinder in the three cylinders is the same as the side length of the cube; in order from bottom to top, the pore size of the unit cell structure in the porous ceramic skeleton decreases step by step, each level has 1 to 5 layers, and the pore size of the unit cell structure in each level is the same; the pore size of the unit cell structure is measured by the diameter of the cylinder in the three cylinders; the array is an array of unit cell structures in each level in the x, y and z axis directions respectively. The present application controls the pore units of each level of the porous ceramic skeleton by changing the pore size (D) of the unit cell structure, and then controls the porosity of the entire skeleton, thereby constructing a porous ceramic skeleton in which the porosity gradually changes from bottom to top, and realizes the bionics of resin-infiltrated ceramic materials and human teeth to the greatest extent in terms of physical properties; the porosity, pore size, and pore distribution of the porous ceramic skeleton provided by the present application are highly controllable, and can realize a three-dimensional through-structure, further control the permeability of the resin material, and stabilize the performance of the material, and structurally realize the bionics of resin-infiltrated ceramic materials and human teeth to the greatest extent, and ultimately achieve wide application in the actual field of denture restoration.

[0036] The present application also provides a dual-bionic resin-ceramic composite material. The present application introduces the parameter D through structural design, and the porosity of the porous ceramic skeleton from the cut to the neck gradually increases, so as to achieve a hard outer and tough inner denture for the repaired denture, realize the dual bionics of structure and physical properties, improve the service performance of the denture, and extend the service life of the repaired denture; the composite material provided by the present application has moderate strength and hardness, is not easy to wear, and is not easy to wear human natural teeth; the composite material provided by the present application is less brittle and is not easy to break during the cutting process; the present application makes the resin and the porous ceramic body more tightly bonded through the inner hole surface design and the surface treatment of the porous ceramic body, thereby enhancing the stability of the composite material; the present application can realize the functionalization of the material, and different composite materials can be selected for repair of different repair parts. According to the data in the examples, the flexural strength of the dual-bionic resin-ceramic composite material provided by the present application is 205~946MPa, the elastic modulus is 13~80GPa, and the hardness is 0.35~3.6GPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] FIG1 is a morphology diagram of a porous ceramic skeleton unit body with a D of 0.9 mm;

[0038] FIG2 is a morphology diagram of a porous ceramic skeleton unit body with a D of 1 mm;

[0039] FIG3 is a morphology diagram of a porous ceramic skeleton unit body with a D of 1.1 mm;

[0040] FIG4 is a morphology diagram of a porous ceramic skeleton unit body with a D of 1.2 mm;

[0041] FIG5 is a morphology diagram of a porous ceramic skeleton unit body with a D of 1.3 mm;

[0042] FIG6 is a morphology diagram of a porous ceramic skeleton unit body with a D of 1.4 mm;

[0043] FIG7 is a diagram showing the construction process of a unit cell structure;

[0044] FIG8 is a skeleton diagram of a unit cell structure with a D of 1 mm obtained in Example 5. DETAILED DESCRIPTION

[0045] The present application provides a porous ceramic skeleton, which is a three-dimensional structure formed by an array of multiple unit cell structures; the unit cell structure is a cube provided with a through hole, and the through hole is a three-cylinder structure with a chamfered corner, and the three cylinders in the three-cylinder structure have the same size, and the length of the cylinder in the three cylinders is the same as the side length of the cube;

[0046] In order from bottom to top, the pore size of the unit cell structure in the porous ceramic skeleton decreases step by step, each level has 1 to 5 layers, and the pore size of the unit cell structure in each level is the same; the pore size of the unit cell structure is measured by the diameter of the cylinder in the three cylinders;

[0047] The array is a unit cell structure in each level arranged in an array in the x-axis, y-axis and z-axis directions respectively.

[0048] In the present application, the porosity of the porous ceramic skeleton is preferably 3-70%, more preferably 20-40%; the pore size difference between two adjacent unit cell structures is preferably 0.01-1 mm, more preferably 0.1-0.5 mm.

[0049] In the present application, the three cylinders are entities formed by the intersection of three vertical cylinders; the diameter of each cylinder in the three cylinders is preferably 0.01 to 1 mm, more preferably 0.1 to 0.5 mm; the porosity of the porous ceramic skeleton is preferably calculated by formula I: P = 59.76D-14.02 formula I; wherein D is the pore size of the unit cell structure, in mm, and has a value of 0.01 to 1.9 mm; P is the porosity of the porous ceramic skeleton, in %. In a specific embodiment of the present application, the D is preferably the aperture corresponding to a unit cell structure with a side length of 2 mm, and the value range of the D is preferably 0.01 to 1.9 mm, more preferably 0.01 to 1 mm or 0.25 to 1.9 mm, further preferably 0.5 to 1.5 mm, and specifically preferably 0.28 mm, 0.32 mm, 0.40 mm, 0.57 mm, 0.74 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm or 1.4 mm.

[0050] The present application also provides a method for preparing a porous ceramic skeleton, comprising the following steps:

[0051] According to the structural design model of the porous ceramic skeleton, a ceramic resin slurry is used for light-curing 3D printing to obtain the porous ceramic skeleton.

[0052] In this application, the steps of constructing the model are preferably:

[0053] (1) Cylindrical models with the same center point and the same diameter D1 were constructed in the x, y, and z directions to obtain a three-cylindrical structure model. Each cylindrical model was Boolean subtracted from a cube with a side length of 2 mm to obtain a porous ceramic skeleton unit body with a pore size of D1;

[0054] (2) chamfering the corners of the porous ceramic skeleton unit body with a radius of R = (2-D1) / 2 to obtain a unit cell structure with a pore size of D1;

[0055] (3) Arraying the unit cell structure in the x-, y-, and z-axis directions to obtain a unit cell structure skeleton with an aperture of D1;

[0056] (4) Repeat steps (1) to (3), replacing D1 with D2 to obtain a unit cell structure skeleton with a pore size of D2;

[0057] (5) Repeat step (4) n times, replacing D1 each time, and replacing D1 with D3, D4, ..., D according to the number of repetitions. n , n≥3, and D1~D n Increase or decrease in sequence to obtain the aperture D 3~ D n The unit cell structure skeleton;

[0058] (6) Set the aperture to D1~D n The multi-layer unit cell structure skeleton is superimposed in the order of increasing or decreasing pore size to obtain a porous ceramic skeleton model.

[0059] In this application, in step (1), the relationship between the parameter D of the porous ceramic skeleton unit body and the porosity P and pore morphology is shown in Table 1. From Table 1, it can be obtained that the relationship between the parameters D of the porous ceramic skeleton unit body and the porosity P and pore morphology is shown in Table 1. n ) under the conditions of porosity change of porous ceramic skeleton; when D is 0.9 mm, the morphology of the porous ceramic skeleton unit body is shown in FIG1 , when D is 1 mm, the morphology of the porous ceramic skeleton unit body is shown in FIG2 , when D is 1.1 mm, the morphology of the porous ceramic skeleton unit body is shown in FIG3 , when D is 1.2 mm, the morphology of the porous ceramic skeleton unit body is shown in FIG4 , when D is 1.3 mm, the morphology of the porous ceramic skeleton unit body is shown in FIG5 , and when D is 1.4 mm, the morphology of the porous ceramic skeleton unit body is shown in FIG6 .

[0060] Table 1 Relationship between the parameter D and porosity P of porous ceramic skeleton unit

[0061] In this application, the construction process of step (1) and step (2) is specifically shown in Figure 7. As can be seen from Figure 7, this application uses Boolean operations to subtract the three-cylinder structure from the cube, and then chamfers the remaining part to obtain a unit cell structure.

[0062] The present application has no special requirements for the number of arrays in the x, y, and z-axis directions in step (3), and can be adjusted according to actual needs. In a specific embodiment of the present application, the number of arrays in the x and y-axis directions in step (3) is preferably more than 200, and the number of arrays in the z-axis direction is preferably 4 to 5. The present application utilizes the curvature of any point within the three-periodic minimal surface function to ensure the absolute smoothness of the internal structure of the ceramic skeleton to the greatest extent possible. Compared with an internal structure with edges and corners, the ceramic skeleton can be better bonded to the ceramic surface after the resin infiltrates the ceramic in the later stage, thereby improving the performance stability of the material.

[0063] In the present application, the ceramic resin slurry preferably comprises the following components in mass percentages:

[0064] In this application, unless otherwise specified, all substances mentioned are commercially available products well known to those skilled in the art.

[0065] In the present application, the mass fraction of the ceramic material in the ceramic resin slurry is preferably 35-86%, more preferably 50-85%, and further preferably 82-85%; the ceramic material preferably includes one or more of zirconia powder, lithium disilicate ceramic particles, sodium aluminum silicate ceramic particles, alumina ceramics, feldspar ceramic powder, barium glass powder and hydroxyapatite; the zirconia powder is preferably a single-particle zirconia powder or a multi-particle mixed zirconia powder, and the particle size of the zirconia powder is preferably 50nm-5μm; the lithium disilicate ceramic particles are preferably single-particle lithium disilicate ceramics or multi-particle mixed lithium disilicate ceramic particles, and the particle size of the lithium disilicate ceramic particles is preferably 50nm-5μm; the sodium aluminum silicate ceramic particles are preferably single-particle sodium aluminum silicate ceramics or multi-particle mixed sodium aluminum silicate ceramics. Ceramic particles, the particle size of the sodium aluminum silicate ceramic particles is preferably 50nm~5μm; the alumina ceramic preferably includes spherical alumina ceramic particles and fibrous alumina ceramic, the spherical alumina ceramic particles are preferably single-particle size spherical alumina ceramic particles or multi-particle size mixed spherical alumina ceramic particles, the particle size of the alumina ceramic is preferably 50nm~5μm; the feldspar ceramic powder preferably includes one or more of albite, calcium feldspar, barium feldspar, barium cryolite, microcline, orthoclase and sanidine, the feldspar ceramic powder is preferably single-particle size feldspar ceramic powder or multi-particle size mixed feldspar ceramic powder, the particle size of the feldspar ceramic powder is preferably 50nm~5μm; the particle size of the barium glass powder is preferably 0.1~0.7μm; the particle size of the hydroxyapatite is preferably 100nm~1μm.

[0066] In the present application, the mass fraction of the resin material in the ceramic resin slurry is preferably 9-60%, more preferably 10-30%, and further preferably 10-15%; the resin material preferably includes one or more of dimethacrylate urethane, triethylene glycol dimethacrylate, bisphenol A glycidyl methacrylate, ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate, more preferably a mixture of dimethacrylate urethane, triethylene glycol dimethacrylate and bisphenol A glycidyl methacrylate, and the mass ratio of dimethacrylate urethane, triethylene glycol dimethacrylate and bisphenol A glycidyl methacrylate in the mixture is preferably 1:0.4-0.8:0.1-0.3, more preferably 1:0.5-0.6:0.1-0.25.

[0067] In the present application, the mass fraction of the initiator in the ceramic resin slurry is preferably 1 to 4%, more preferably 1.5 to 3.5%, and further preferably 2 to 3%; the initiator preferably includes one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone and 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyloxime), more preferably 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0068] In the present application, the mass fraction of the dispersant in the ceramic resin slurry is preferably 0.01-1%, more preferably 0.3-0.9%, and further preferably 0.5-0.8%; the dispersant preferably includes one or more of polyethylene glycol, Triton X100, polycaprolactone dispersant, polyacrylic acid, polyethyleneimine and sodium dodecylbenzenesulfonate, more preferably one or more of polyethylene glycol 200, polyethylene glycol 400, polyethylene glycol 1000, polyethylene glycol 4000 and polyethylene glycol 6000; the model of the polyethylene glycol is preferably polyethylene glycol 400.

[0069] In the present application, the mass fraction of the additive in the ceramic resin slurry is preferably 0.01-1%, more preferably 0.3-0.9%, and further preferably 0.5-1%; the additive preferably includes one or more of a leveling agent, a defoaming agent, and a color stabilizer, more preferably one or two of a leveling agent and a defoaming agent; the leveling agent preferably includes one or more of AKN-1033 leveling agent (XUHUA), EFKA SL 3258 leveling agent (BASF), 616 leveling agent (Keying Chemical Company), and BYK-333 leveling agent (BYK Chemical Company); the defoaming agent preferably includes BYKA535 defoaming agent (BYK Chemical Company), TEGO FOAMEX One or more of 810 defoamer (Evonik, Germany), X-039 defoamer (Guangzhou Hongtai New Materials Co., Ltd.) and Z-3158 defoamer (Shanghai Yuewan New Materials); in the specific embodiment of the present application, the leveling agent was purchased from BYK Chemical, model BYK-333, and the defoaming agent was purchased from Evonik, Germany, model TEGO FOAMEX 810.

[0070] In this application, the printing speed of the light-curing 3D printing is preferably 0.01 to 0.1 mm / min, more preferably 0.05 mm / min, the curing time is preferably 3 to 8 seconds, more preferably 5 to 6 seconds, and the light intensity is preferably 60 to 100 PWM, more preferably 70 to 80 PWM; this application has no special requirements for the scaling ratio of light-curing 3D printing, as long as it meets practical application requirements. In this application, the relationship between the pore size d of the porous ceramic skeleton model (the pore size used in actual 3D printing) and the pore size D of the porous ceramic skeleton (the pore size used when designing the model) is d = D*λ, where λ is the scaling ratio.

[0071] The present application also provides a method for preparing a dual-bionic resin-ceramic composite material, comprising the following steps: subjecting the porous ceramic skeleton to debinding treatment, pre-sintering, modification, drying, infiltration treatment and post-curing treatment in sequence to obtain a dual-bionic resin-ceramic composite material; the modification modifier is preferably a silane coupling agent.

[0072] In the present application, the temperature of the debinding treatment is preferably 300-600°C, more preferably 300°C, and the time is preferably 1-10h, more preferably 10h; the debinding treatment is preferably carried out in air or nitrogen atmosphere; the equipment for the debinding treatment is preferably a Komei sintering furnace, and the heating and cooling rates of the debinding treatment are preferably 0.5-10°C / min, more preferably 5°C / min.

[0073] After the debinding process is completed, the present application preferably further comprises cooling the debinding product obtained to room temperature; the present application has no special limitation on the cooling, and a cooling method well known to those skilled in the art may be used, such as natural cooling.

[0074] In the present application, the pre-sintering temperature is preferably 1400-1700°C, more preferably 1700°C, and the duration is preferably 1-10 hours, more preferably 10 hours. The pre-sintering heating rate is preferably 0.5-10°C / min, more preferably 5-8°C / min, and the temperature is preferably increased from room temperature to the pre-sintering temperature. The pre-sintering is preferably performed in an air atmosphere. Pre-sintering is used in the present application to impart certain mechanical properties to the porous ceramic skeleton.

[0075] After the pre-sintering is completed, the present application preferably further includes cooling the obtained pre-sintered product to room temperature; the present application has no special limitation on the cooling, and a cooling method well known to those skilled in the art can be used, such as natural cooling.

[0076] In the present application, the modification preferably involves soaking the pre-sintered porous ceramic skeleton in a silane coupling agent for 4 to 6 hours, more preferably 5 hours. The silane coupling agent preferably includes one or more of Shuguang KH550, KH560, KH570, and Maitu A-137. The modification is preferably performed under vacuum conditions, preferably with a vacuum degree of -0.1 MPa. In a specific embodiment of the present application, the silane coupling agent is preferably KH570. By modifying the porous ceramic skeleton, the present application forms an organic coating film on the surface of the ceramic skeleton material, which facilitates better bonding between the resin and the ceramic skeleton.

[0077] In the present application, the drying temperature is preferably 110-130°C, more preferably 130°C, the time is preferably 1-5 hours, more preferably 1-3 hours, and the drying atmosphere is air or nitrogen; the present application has no special requirements for the drying method, and the method commonly used by those skilled in the art can be selected.

[0078] In the present application, the infiltration treatment is preferably to soak the dried porous ceramic skeleton in a polymer solution under vacuum conditions, release the vacuum and then soak it under normal pressure, repeat the vacuum soaking-releasing the vacuum-normal pressure soaking steps 3 to 4 times until the liquid level of the polymer solution remains unchanged and no bubbles are generated; the vacuum soaking and normal pressure soaking temperatures are independently preferably 30 to 60°C, more preferably 40 to 50°C; the time for a single vacuum soaking is preferably 30 to 120 minutes, more preferably 50 to 100 minutes; the vacuum degree of the vacuum condition is preferably -0.1 MPa; a single normal pressure soaking The pressure immersion time is preferably 10 to 60 minutes, more preferably 20 to 50 minutes; the components of the polymer solution preferably include a resin and an initiator; the resin preferably includes one or more of PMMA, UDMA, BIS-GMA, TEGDMA and HEMA, and the resin undergoes a cross-linking reaction under the action of the initiator, thereby achieving filling of the ceramic skeleton; the initiator preferably includes one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl) butanone; the mass fraction of the initiator in the polymer solution is preferably 1 to 3%, more preferably 2%; in a specific embodiment of the present application, the polymer solution is composed of 98% by mass of PMMA and 2% by mass of the initiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide.

[0079] In the present application, the post-curing treatment includes sequential photocuring and thermal curing. The photocuring device is preferably a photocuring light box. The photocuring is preferably performed by immersing the porous ceramic skeleton after the infiltration treatment in water and curing in the photocuring light box. The light used for the photocuring is preferably medium-high light. The wavelength of the medium-high light is preferably 385-460nm, more preferably 405nm. The photocuring time is preferably 20-60 minutes. In the present application, photocuring in water can absorb the heat released during the curing process and alleviate the stress concentration caused by local excessive heat. In the present application, the thermal curing is preferably sintering the porous ceramic skeleton after the photocuring. The sintering temperature is preferably 125-155°C, more preferably 130-140°C. The sintering time is preferably 12-14h, more preferably 13h. The sintering device is preferably an oven. After the sintering is completed, the present application preferably further includes cooling the resulting solid processing system to room temperature. The cooling rate is preferably 0.5-5°C / min, more preferably 1-3°C / min.

[0080] This application also provides a dual-bionic resin-ceramic composite material prepared by the preparation method described in the above scheme. The dual-bionic resin-ceramic composite material provided in this application has a porous ceramic skeleton with gradually increasing porosity from the incisal end (the upper part of the tooth, where the teeth contact each other), the neck (the part connecting the crown and the root), and the root (the root), achieving a hard exterior and tough interior for the repaired denture, achieving dual bionic structure and physical properties.

[0081] This application performs fitting based on the pore size and mechanical property data of the dual-bionic resin-ceramic composite material to obtain a corresponding functional relationship. Those skilled in the art can derive the physical properties of the composite material prepared in Example 1 based on the fitting function. The flexural strength F of the dual-bionic resin-ceramic composite material is calculated by Formula II: F = -193.1D + 1178.3 Formula II,

[0082] In formula II: F is the flexural strength, in MPa, D is the pore size of the unit cell structure, in mm;

[0083] The elastic modulus of the dual-bionic resin ceramic composite material is calculated by formula III: G = 1.3571D 2 -25.043D+104.8 Formula III,

[0084] In formula II: G is the elastic modulus, in GPa, D is the pore size of the unit cell structure, in mm;

[0085] The hardness of the dual-bionic resin-ceramic composite material is calculated by Formula IV: H = -0.81D + 4.45 Formula IV,

[0086] In formula II: H is the hardness, the unit is GPa, D is the pore size of the unit cell structure, the unit is mm.

[0087] In order to further illustrate the present application, the porous ceramic skeleton and its preparation method as well as a dual-bionic resin ceramic composite material provided by the present application are described in detail below in combination with the examples, but they should not be understood as limiting the scope of protection of the present application.

[0088] Example 1

[0089] Construction of porous ceramic skeleton model:

[0090] (1) constructing cylindrical models with the same center point and the same diameter in the x, y, and z directions, respectively, wherein the diameter D is 0.74 mm, and performing Boolean subtraction between the cylindrical model and a cube with a side length of 2 mm to obtain a porous ceramic skeleton unit body with a pore diameter of 0.74 mm;

[0091] (2) chamfering the corners of the porous ceramic skeleton unit body with a radius R = 0.37 mm to obtain a unit cell structure with a pore diameter of 0.74 mm;

[0092] (3) Arraying the unit cell structure in the x-, y-, and z-axis directions to obtain a unit cell structure skeleton with an aperture of 0.74 mm, wherein 20 to 100 units are arrayed in the x- and y-axis directions, and the number of arrays in the two directions is the same, and 5 units are arrayed in the z-axis direction;

[0093] (4) Repeat steps (1) to (3), replacing 0.74 mm with 0.57 mm to obtain a single-cell structure skeleton with a pore size of 0.57 mm;

[0094] (5) Repeat steps (1) to (3), replacing 0.57 mm with 0.40 mm to obtain a single-cell structure skeleton with a pore size of 0.40 mm;

[0095] (6) Repeat steps (1) to (3), replacing 0.40 mm with 0.32 mm to obtain a single-cell structure skeleton with a pore size of 0.32 mm;

[0096] (7) Repeat steps (1) to (3), replacing 0.32 mm with 0.28 mm and replacing 5 arrays with 4 arrays in the z-axis direction to obtain a single-cell structure skeleton with an aperture of 0.28 mm;

[0097] (8) The single-cell structure skeleton with a pore size of 0.74 mm is used as the bottom layer, and the single-cell structure skeleton with a pore size of 0.57 mm, the single-cell structure skeleton with a pore size of 0.40 mm, the single-cell structure skeleton with a pore size of 0.32 mm and the single-cell structure skeleton with a pore size of 0.28 mm are stacked in sequence to obtain a porous ceramic skeleton model.

[0098] (i) Preparation of ceramic resin slurry:

[0099] 82% of zirconium oxide powder, 6% of ethoxylated bisphenol A dimethacrylate, 8% of 1,6-hexanediol diacrylate, 2% of initiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 0.5% of dispersant polyethylene glycol 400, 0.5% of Triton X100, 0.5% of leveling agent and 0.5% of deaerator are mixed and stirred uniformly to obtain a ceramic resin slurry, wherein the diameter of the zirconium oxide powder is 50 nm, the leveling agent is BYK-333 leveling agent, and the deaerator is TEGO FOAMEX 810 deaerator produced by Evonik of Germany. The above contents are in percentage by mass.

[0100] (ii) 3D printing of porous ceramic skeleton models:

[0101] According to the above-mentioned porous ceramic skeleton model, the above-mentioned ceramic resin slurry was used for light-curing 3D printing, wherein the scaling ratio was 2:1, that is, d=1 / 2D, and a porous ceramic skeleton with a size of 20~100mm×20~100mm×24mm was obtained. The pore diameters of the porous ceramic skeleton were 0.37mm, 0.285mm, 0.20mm, 0.16mm and 0.14mm from bottom to top, and the porosity of the porous ceramic skeleton was 30%, 20%, 10%, 5% and 3% from bottom to top; the printing speed was 0.05mm / min, the curing time was 5s, and the light intensity was 80PWM.

[0102] (iii) Preparation of dual biomimetic resin ceramic composites:

[0103] The porous ceramic skeleton was subjected to debinding treatment and then naturally cooled to room temperature. The debinding equipment was a Kemei sintering furnace, the debinding temperature was 300°C, the debinding time was 10h, the heating rate was 5°C / min, and the debinding atmosphere was air.

[0104] Then, the porous ceramic skeleton after debinding was pre-sintered and naturally cooled to room temperature. The pre-sintering temperature was 1700℃, the time was 10h, the heating rate was 5℃ / min, and the sintering atmosphere was air.

[0105] Then, the pre-sintered porous ceramic skeleton is modified by soaking the pre-sintered porous ceramic skeleton in a silane coupling agent for 5 hours at a soaking temperature of 40°C and a vacuum degree of -0.1 MPa, and the silane coupling agent is KH570;

[0106] The modified porous ceramic skeleton was then dried at a temperature of 130°C for 3 h in an air atmosphere.

[0107] The dried porous ceramic skeleton was then subjected to an infiltration treatment, which included vacuum immersing the dried porous ceramic skeleton in a polymer solution at 40°C and -0.1 MPa for 30 minutes, releasing the vacuum, and then continuing to immerse the skeleton at normal pressure for 10 minutes, repeating the vacuum immersion-release-normal pressure immersion steps four times; wherein the polymer solution consisted of 98% by mass of PMMA and 2% by mass of an initiator, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide;

[0108] Finally, the porous ceramic skeleton after infiltration treatment was post-cured. The post-curing treatment was first light curing and then heat curing. The light curing equipment was a Kemei light curing light box. Specifically, the porous ceramic skeleton after infiltration treatment and the light box were immersed in water and treated with 405nm ultraviolet light for 60 minutes. The heat curing equipment was an oven. The light-cured porous ceramic skeleton was placed in the oven. The heat curing temperature was 155°C, the time was 12h, and the cooling rate was 5°C / min to obtain a dual-bionic resin ceramic composite material.

[0109] By changing the pore diameter D and the scaling ratio λ, the present application can control the porosity, pore diameter and pore morphology of the pore unit, construct a porous ceramic skeleton with a porosity gradually decreasing from the bottom to the top, and realize a three-dimensional through-structure. Therefore, the dual-bionic resin-ceramic composite material provided by the present application realizes the bionics of resin-infiltrated ceramic material and human teeth to the greatest extent in structure.

[0110] Example 2

[0111] Construction of porous ceramic skeleton model:

[0112] The dual-bionic resin-ceramic composite material was prepared according to the steps of constructing the porous ceramic skeleton model, preparing the ceramic resin slurry, 3D printing the porous ceramic skeleton model, and preparing the dual-bionic resin-ceramic composite material provided in Example 1, except that the zirconium oxide powder was replaced with lithium disilicate ceramic, and the pre-sintering temperature was 820°C.

[0113] Example 3

[0114] Construction of porous ceramic skeleton model:

[0115] The dual-bionic resin-ceramic composite material was prepared according to the steps of constructing the porous ceramic skeleton model, preparing the ceramic resin slurry, 3D printing the porous ceramic skeleton model, and preparing the dual-bionic resin-ceramic composite material provided in Example 1, except that the zirconium oxide powder was replaced with sodium aluminum silicate ceramic, and the pre-sintering temperature was 850°C.

[0116] Example 4

[0117] Construction of porous ceramic skeleton model:

[0118] The dual-bionic resin-ceramic composite material was prepared according to the steps of constructing the porous ceramic skeleton model, preparing the ceramic resin slurry, 3D printing the porous ceramic skeleton model, and preparing the dual-bionic resin-ceramic composite material provided in Example 1, except that the zirconia powder was replaced with feldspar ceramic and the pre-sintering temperature was 850°C.

[0119] Example 5

[0120] Construction of porous ceramic skeleton model:

[0121] (1) constructing cylindrical models with the same center point and the same diameter in the x, y, and z directions, respectively, wherein the diameter D is 1 mm, and performing Boolean subtraction between the cylindrical model and a cube with a side length of 2 mm to obtain a porous ceramic skeleton unit body with a pore diameter of 1 mm;

[0122] (2) chamfering the corners of the porous ceramic skeleton unit body with a radius R = 0.5 mm to obtain a unit cell structure with a pore diameter of 1 mm;

[0123] (3) The unit cell structures are arrayed in the x-, y-, and z-axis directions to obtain a unit cell structure skeleton with an aperture of 1 mm, wherein 5 units are arrayed in the x- and y-axis directions, and 4 units are arrayed in the z-axis direction.

[0124] FIG8 is a diagram of a unit cell structure skeleton with a D of 1 mm obtained in Example 5, which can realize a three-dimensional through-structure.

[0125] Test Case

[0126] Performance test of dual bionic resin ceramic composite materials

[0127] The performance test was conducted on each unit cell structure skeleton layer of the dual-bionic resin ceramic composite material prepared in Examples 1 to 4. The test results are shown in Tables 2 to 5:

[0128] Table 2 Performance test results of the dual-bionic resin ceramic composite material prepared in Example 1

[0129] Table 3 Performance test results of the dual-bionic resin ceramic composite material prepared in Example 2

[0130] Table 4 Performance test results of the dual-bionic resin ceramic composite material prepared in Example 3

[0131] Table 5 Performance test results of the dual-bionic resin ceramic composite material prepared in Example 4

[0132] As can be seen from Tables 2 to 5, the dual-bionic resin-ceramic composite material provided by the present application is soft and tough at the bottom and strong and hard at the top, and realizes the bionics of the resin-infiltrated ceramic material and human teeth to the greatest extent in terms of physical properties.

[0133] The above is only a preferred embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.

Claims

1. A porous ceramic skeleton, It is characterized in that The porous ceramic skeleton is a three-dimensional structure formed by an array of several unit cell structures; the unit cell structure is a cube provided with a through hole, the through hole is a chamfered three-cylinder structure, the three cylinders in the three-cylinder structure have the same size, and the length of the cylinder in the three cylinders is the same as the side length of the cube; In order from bottom to top, the pore size of the unit cell structure in the porous ceramic skeleton decreases step by step, each level has 1 to 5 layers, and the pore size of the unit cell structure in each level is the same; the pore size of the unit cell structure is measured by the diameter of the cylinder in the three cylinders; The array is that the unit cell structures in each level are arranged in an array in the x-axis, y-axis and z-axis directions respectively.

2. The porous ceramic skeleton according to claim 1, It is characterized in that The pore size of the unit cell structure is 0.01 to 1.9 mm; The porosity of the porous ceramic skeleton is calculated by formula I: P = 59.76D-14.02 Formula I; In formula I: D is the pore size of the unit cell structure, in mm; P is the porosity of the porous ceramic skeleton, in %.

3. The porous ceramic skeleton according to claim 1, It is characterized in that The porosity of the porous ceramic skeleton is 3-70%; the pore size difference between two adjacent unit cell structures is 0.01-1 mm.

4. The porous ceramic skeleton according to claim 1, It is characterized in that The three cylinders are entities formed by the intersection of three vertical cylinders; the diameter of each cylinder in the three cylinders is 0.01-1 mm.

5. A method for preparing the porous ceramic skeleton according to any one of claims 1 to 4, It is characterized in that The following steps are involved: According to the structural design model of the porous ceramic skeleton according to any one of claims 1 to 4, a ceramic resin slurry is then used for photocuring 3D printing to obtain a porous ceramic skeleton.

6. The preparation method according to claim 5, It is characterized in that The steps for building the model are: (1) Construct the same center point and the same diameter D in the x, y and z axes respectively 1 The cylindrical model is obtained to obtain a three-cylinder structure model. Each cylindrical model is subtracted from a cube with a side length of 2 mm by Boolean to obtain an aperture of D 1 A porous ceramic skeleton unit body; (2) The corners of the porous ceramic skeleton unit body are formed with a radius R = (2-D 1 ) / 2 chamfer, The aperture is D 1 The unit cell structure of (3) Arrange the unit cell structure in the x, y and z directions respectively to obtain an aperture of D 1 The unit cell structure skeleton; (4) Repeat steps (1) to (3) to convert D 1 Replace with D 2 , and the aperture is D 2 The unit cell structure skeleton; (5) Repeat step (4) n times, and change D 1 Replace, and replace D in turn according to the number of repetitions. 1 Replace with D 3 , D 4 ...D n , n≥3, and D 1 ~D n Increase or decrease successively to obtain the aperture D 3 ~D n The unit cell structure skeleton; (6) Set the aperture to D 1 ~D n The multi-layer unit cell structure skeleton is superimposed in the order of increasing or decreasing pore sizes to obtain a porous ceramic skeleton model.

7. The preparation method according to claim 6, It is characterized in that In step (3), the number of arrays in the x- and y-axis directions is more than 200, and the number of arrays in the z-axis direction is 4 to 5.

8. The preparation method according to claim 4, It is characterized in that The ceramic resin slurry comprises the following components in percentage by mass:

9. The preparation method according to claim 8, It is characterized in that The ceramic material includes one or more of zirconium oxide powder, lithium disilicate ceramic particles, sodium aluminum silicate ceramic particles, alumina ceramics, feldspar ceramic powder, barium glass powder and hydroxyapatite; The resin material includes one or more of dimethacrylate carbamate, triethylene glycol dimethacrylate, bisphenol A glycidyl methacrylate, ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate; the initiator includes one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone and 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyl oxime); The dispersant includes polyethylene glycol, Triton X100, polycaprolactone dispersant, polypropylene One or more of acid, polyethyleneimine and sodium dodecylbenzenesulfonate; The auxiliary agent includes one or more of a leveling agent, a defoaming agent and a color stabilizer.

10. The preparation method according to claim 8, It is characterized in that The initiator includes one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone and 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyloxime).

11. The preparation method according to claim 5, 8, 9 or 10, It is characterized in that The speed of the light-curing 3D printing is 0.01-0.1 mm / min, the curing time is 3-8 s, and the light intensity is 60-100 PWM.

12. A method for preparing a dual bionic resin ceramic composite material, It is characterized in that The method comprises the following steps: subjecting the porous ceramic skeleton described in any one of claims 1 to 4 or the porous ceramic skeleton prepared by the preparation method described in any one of claims 5 to 11 to debinding treatment, pre-sintering, modification, drying, infiltration treatment and post-curing treatment in sequence to obtain a dual-bionic resin ceramic composite material; the modification agent is a silane coupling agent.

13. The preparation method according to claim 12, It is characterized in that The temperature of the debinding treatment is 300-600°C, and the time is 1-10 hours; the debinding treatment is carried out in air or nitrogen atmosphere; the modification is to immerse the pre-sintered porous ceramic skeleton in a silane coupling agent, and the immersion time is 4-6 hours; the post-curing treatment includes sequential photocuring and thermal curing.

14. The preparation method according to claim 13, It is characterized in that The light used for the photocuring is medium-high light, the wavelength of the medium-high light is 385-460nm, the time of the photocuring is 20-60min, and the photocuring is carried out in water; The thermal curing is to sinter the porous ceramic skeleton after light curing, and the sintering temperature is 125-155° C. and the time is 12-14 hours.

15. The preparation method according to claim 12 or 13, It is characterized in that The pre-sintering temperature is 1400-1700° C. and the time is 1-10 hours.

16. The preparation method according to claim 12, It is characterized in that The infiltration treatment is to immerse the dried porous ceramic skeleton in a polymer solution under vacuum conditions, release the vacuum and then immerse it at normal pressure, and repeat the above steps of vacuum immersion-releasing the vacuum-normal pressure immersion 3 to 4 times until the liquid level of the polymer solution remains unchanged and no bubbles are generated.

17. The preparation method according to claim 16, It is characterized in that The components of the polymer solution include resin and initiator; The resin includes one or more of PMMA, UDMA, BIS-GMA, TEGDMA and HEMA; The initiator in the polymer solution includes one or more of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, ethyl 2,4,6-trimethylbenzoylphenylphosphonate and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone; the mass fraction of the initiator in the polymer solution is 1-3%.

18. The preparation method according to claim 16 or 17, It is characterized in that The vacuum immersion and normal pressure immersion temperatures are independently 30-60° C.; the time for a single vacuum immersion is 30-120 min; the vacuum degree of the vacuum condition is -0.1 MPa; and the time for a single normal pressure immersion is 10-60 min.

19. The dual-bionic resin ceramic composite material prepared by the preparation method according to any one of claims 12 to 18.

Citation Information

Patent Citations

  • Silicon nitride-resin double continuous phase composite ceramic material and preparation method and application thereof

    CN107056319A

  • Zirconia-resin bicontinuous composite material, application and preparation method thereof

    CN110327220A

  • Mathematical modeling method of controllable porous bone tissue engineering scaffold

    CN111899346A

  • Bone repairstentfor directionally inducing bone tissue differentiation

    CN113577379A

  • Gradient bionic dental ceramic

    CN114213021A