High-molecular polymer and organic electroluminescent element
By developing high-molecular polymers containing electron-accepting groups and cross-linking groups for use in the charge injection/transport layer of OLEDs, the problems of high drive voltage and poor stability of components in the wet film-forming method have been solved, and low voltage has been achieved. and high-efficiency OLED performance.
Patent Information
- Application Number
- PCT/CN2024/071482
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-01-10
- Publication Date
- 2024-10-03
AI Technical Summary
In the existing OLED display process, components formed by the wet film formation method have problems with high driving voltage and poor stability, making it difficult to meet market demand.
Develop a high molecular polymer containing electron-accepting groups, fluorene, arylamine and carbazole compounds, and form a charge injection/transport layer with cross-linking groups through a wet film-forming method, using Suzuki reaction and Yamamoto reaction Wait for the transition metal catalyst coupling reaction to perform polymerization, reduce the driving voltage and improve the efficiency.
A low-voltage and high-efficiency OLED light-emitting element has been realized. Through the use of cross-linking groups, the charge transport and stability are improved, the startup voltage of the device is reduced, and the overall performance is improved.
Smart Images

Figure CN2024071482_03102024_PF_FP_ABST
Abstract
Description
A high molecular polymer and an organic electroluminescent element Technical Field
[0001] The present application relates to the field of OLED technology, specifically to a polymer that can be used to form an organic electroluminescent device (OLED), particularly as a charge injection / transport material. Furthermore, the present application relates to an organic electroluminescent device having a charge injection / transport layer formed using the polymer using a wet film formation method. Background Art
[0002] Organic light-emitting diodes (OLEDs) are gaining increasing attention in display and lighting applications due to their inherent self-luminescence, high contrast, wide color gamut, wide viewing angle, and fast response time. However, OLEDs struggle to meet market demand due to their high cost and difficulty in mass production. This is primarily due to the need for further technical refinement and improvement of their production processes.
[0003] There are two main OLED display process technologies: the more mature vapor deposition process and inkjet printing. These two processes differ significantly in terms of equipment, materials, and processes. Vapor deposition uses vacuum deposition to deposit small molecule OLED luminescent materials, but this is time-consuming and labor-intensive, with low material utilization and high costs. Inkjet printing uses solvents to dissolve OLED materials into a uniform solution, which is then directly sprayed onto the substrate surface to form the RGB organic light-emitting layer. This method boasts high material utilization and low costs. Due to its unique technical characteristics and manufacturing advantages, inkjet printing is gradually becoming the mainstream production process for OLED panels and will revolutionize the production model of the entire display industry.
[0004] Compared to elements formed by vacuum evaporation, wet film forming methods are difficult to stack and have poor driving stability. Therefore, in order to perform stacking using the wet film forming method, charge transport polymers with cross-linking groups have been developed. WO2009123269A1 and WO2013191088A1 disclose organic electroluminescent elements obtained by stacking polymers containing specific repeating units by wet film forming methods. US8974917B2 describes that in polymers having triarylamine repeating units, it is preferred that a fluorene ring be included in the main chain. In addition, it is described that the triplet energy of the polymer is increased by causing distortion by including a phenylene group having a substituent in the main chain of the polymer. TW201204687A discloses a compound in which a phenylene group having a substituent is connected between the nitrogen atoms of the main chain amine of an aromatic amine polymer or oligomer. WO2011099531A1 and CN102791768B disclose a polymer having an aromatic amine structure with a carbazole structure on the side chain. CN1882632B discloses a polymer comprising a fluorene repeating unit, wherein the fluorene repeating unit is substituted with a crosslinkable group, including a double bond, a triple bond, a precursor capable of forming a double bond in situ, or a heterocyclic addition polymerizable group. Benzocyclobutane (BCB) is disclosed as an exemplary crosslinkable group. WO2010013723A1 discloses a polymer comprising a double bond group and a BCB group. WO2012003485A2 and WO2012003482A2 disclose a hole transport layer formed by reacting a hole transport compound substituted with benzocyclobutane. CN101981086 A and WO2013191088A1 propose benzocyclobutene and styrene crosslinking groups as crosslinking groups for the polymer. However, benzocyclobutene crosslinking groups hinder charge transfer due to side reactions during crosslinking.
[0005] However, light-emitting elements manufactured using polymers have a problem of high driving voltage.
[0006] Summary of the Invention
[0007] The object of the present application is to provide a high molecular weight polymer useful for producing a light-emitting element having a low driving voltage.
[0008] The present application also aims to provide a light-emitting element containing the high molecular weight polymer.
[0009] From the perspective of lowering the voltage and increasing the efficiency of an organic electroluminescent element, in some embodiments, the high molecular weight polymer for an organic electroluminescent element of the present application contains an electron-accepting group. From the perspective of lowering the voltage of an organic electroluminescent element, in some embodiments, the high molecular weight polymer for an organic electroluminescent element of the present application further contains a fluorene, an aromatic amine, or a carbazole compound.
[0010] A high molecular weight polymer containing at least one of the following three repeating units and terminated by Ar1 and Ar2,
[0011] wherein Ar1 and Ar2 independently represent C6-C36 aryl substituted or unsubstituted by R1 or R12, or C5-C36 heteroaryl substituted or unsubstituted by R1 or R12;
[0012] R1-R12 each independently represent hydrogen, substituted or unsubstituted C6-C36 aryl, substituted or unsubstituted C5-C36 heteroaryl, substituted or unsubstituted C1-C24 alkyl, substituted or unsubstituted C2-C24 alkenyl, substituted or unsubstituted C3-C24 cycloalkenyl, substituted or unsubstituted C6-C36 aryloxy, substituted or unsubstituted C5-C36 heteroaryloxy, substituted or unsubstituted C2-C24 alkane Oxycarbonyl, substituted or unsubstituted di-C1-C24 alkylamino, substituted or unsubstituted di-C6-C36 arylamino, substituted or unsubstituted C6-C36 aryl-C1-C24 alkylamino, substituted or unsubstituted C2-C24 alkanoyl, substituted or unsubstituted C8-C36 arylcycloalkyl, substituted or unsubstituted C3-C24 epoxy; wherein at least one of R1-R12 is a crosslinking group;
[0013] wherein the substitution in R1-R12 is substituted by halogen, C1-C8 alkyl, C3-C8 epoxy, C1-C8 alkoxy, C2-C8 alkenyl, C6-C10 aryl or C4-C10 cycloalkenylalkyl;
[0014] Wherein, m, n, and p represent the number of repeating units, m≥0, n≥0, and p≥0, and m and n are not zero at the same time, the weight average molecular weight Mw=10,000-1,000,000, and the dispersion degree PDI=1.0-3.0.
[0015] In some embodiments, the structure: has the structure of the following formula (I),
[0016] In some embodiments: R1-R12 are each independently hydrogen, substituted or unsubstituted C6-C24 aryl, substituted or unsubstituted C5-C24 heteroaryl, substituted or unsubstituted C1-C12 alkyl, substituted or unsubstituted C2-C12 alkenyl, substituted or unsubstituted C3-C12 cycloalkenyl, substituted or unsubstituted C6-C24 aryloxy, substituted or unsubstituted C5-C24 heteroaryloxy, substituted or unsubstituted C2-C12 alkoxycarbonyl, substituted or unsubstituted di-C1-C12 alkylamino, substituted or unsubstituted di-C6-C24 arylamino, substituted or unsubstituted C6-C24 aryl-C1-C12 alkylamino, substituted or unsubstituted C2-C12 alkanoyl, substituted or unsubstituted C8-C24 arylcycloalkyl, substituted or unsubstituted C3-C12 epoxy,
[0017] wherein the substitution in R1-R12 is substituted by halogen, C1-C6 alkyl, C3-C6 epoxy, C1-C6 alkoxy, C2-C6 alkenyl, C6-C10 aryl or C4-C10 cycloalkenylalkyl; m is greater than 0, n ≥ 0, and p ≥ 0;
[0018] Weight average molecular weight Mw = 20,000-800,000.
[0019] In some embodiments, R1, R4, R7, R10-R12 are each independently hydrogen, substituted or unsubstituted C6-C12 aryl, substituted or unsubstituted C5-C12 heteroaryl, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl, substituted or unsubstituted C3-C6 cycloalkenyl, substituted or unsubstituted C6-C12 aryloxy, substituted or unsubstituted C5-C12 heteroaryloxy, substituted or unsubstituted C 2-C6 alkoxycarbonyl, substituted or unsubstituted di-C1-C6 alkylamino, substituted or unsubstituted di-C6-C12 arylamino, substituted or unsubstituted C6-C12 aryl-C1-C6 alkylamino, substituted or unsubstituted C2-C6 alkanoyl, substituted or unsubstituted C8-C12 arylcycloalkyl, substituted or unsubstituted C3-C6 epoxy, and at least one of R1, R4, R7, R10-R12 is a crosslinking group,
[0020] R2-R3, R5-R6, R8-R9 each independently represent a substituted or unsubstituted C6-C12 aryl group, a substituted or unsubstituted C5-C12 heteroaryl group, or a substituted or unsubstituted C1-C6 alkyl group; Mw = 50,000-500,000, and dispersity PDI = 1.5-2.5.
[0021] The crosslinking group is R-substituted C8-C12 aryl and cycloalkyl, R-substituted C3-C6 epoxy, R-substituted C2-C6 alkenyl, C4-C10 cycloalkenyl substituted C8-C12 aryl, R-substituted vinyl phenylene, wherein R is hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, C6-C10 aryl.
[0022] In some embodiments:
[0023] Wherein R is hydrogen, C1-C6 alkyl, or C6-C10 aryl.
[0024] Ar1 and Ar2 independently represent C6-C10 aryl groups which are substituted or unsubstituted by R1 or R12.
[0025] In some embodiments:
[0026] R1, R4, R7, R10-R12 are each independently hydrogen, substituted or unsubstituted C6-C12 aryl, substituted or unsubstituted C5-C12 heteroaryl, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl, substituted or unsubstituted C3-C6 cycloalkenyl, substituted or unsubstituted C8-C12 arylcycloalkyl, or substituted or unsubstituted C3-C6 epoxy;
[0027] R2 is the same as R3, R5 is the same as R6, and R8 is the same as R9;
[0028] Mw is 100,000-300,000, PDI=1.7-2.3.
[0029] The R1 and R12 are the same and are both crosslinking groups. The definitions of m, n, and p are the same as those in claim 1.
[0030] In some embodiments: n=0-1000, m=1, p=0-1000.
[0031] In some further embodiments: n=1-1000, m=1-1000, p=0-1000.
[0032] Further in some embodiments: n=1-1000, m=1-1000, p=1-1000.
[0033] R2 is the same as R3, R5 is the same as R6, R8 is the same as R9, and at least one of R4, R7, R10-R11 is a crosslinking group.
[0034] Application of the above-mentioned polymers in OLEDs.
[0035] The OLED comprises at least one of a light-emitting layer, a charge injection layer, and a charge transport layer, and the high molecular polymer is used as a material in the light-emitting layer, the charge injection layer, and / or the charge transport layer.
[0036] An organic electroluminescent element comprises at least one of a light-emitting layer, a charge injection layer and a charge transport layer, wherein the high molecular polymer is located in the light-emitting layer, the charge injection layer and / or the charge transport layer.
[0037] The high molecular polymer is fixed in the organic electroluminescent element through a wet film forming method.
[0038] The substituents R1 to R12 may include the following structures, but are not limited thereto.
[0039] For example, a linear, branched, or cyclic alkyl group having generally 1 or more, in some embodiments 4 or more and generally 24 or less, in some embodiments 12 or less, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-hexyl group, a cyclohexyl group, and a dodecyl group;
[0040] For example, an alkenyl group such as a vinyl group usually has 2 or more and usually has 24 or less carbon atoms, and in some embodiments, has 12 or less carbon atoms; an alkynyl group such as an ethynyl group usually has 2 or more and usually has 24 or less carbon atoms, and in some embodiments, has 12 or less carbon atoms;
[0041] For example, alkoxy groups such as methoxy and ethoxy groups generally have 1 or more carbon atoms and usually 24 or less, and in some embodiments, 12 or less carbon atoms;
[0042] For example, aryloxy or heteroaryloxy groups such as phenoxy, naphthyloxy, and pyridyloxy groups generally have 4 or more carbon atoms, in some embodiments 5 or more and generally 36 or less, and in some embodiments 24 carbon atoms;
[0043] For example, alkoxycarbonyl groups such as methoxycarbonyl and ethoxycarbonyl generally have 2 or more carbon atoms and usually 24 or less, and in some embodiments, 12 or less carbon atoms;
[0044] For example, dialkylamino groups such as dimethylamino and diethylamino groups generally have 2 or more carbon atoms and usually 24 or less, and in some embodiments, 12 or less carbon atoms;
[0045] For example, diarylamino groups such as diphenylamino, ditolylamino, and N-carbazolyl groups generally have 10 or more carbon atoms, in some embodiments 12 or more, and generally 36 or less, in some embodiments 24 or less carbon atoms;
[0046] For example, an arylalkylamino group having generally 7 or more carbon atoms and generally 36 or less, and in some embodiments, 24 or less carbon atoms, such as a phenylmethylamino group;
[0047] For example, acyl groups such as acetyl and benzoyl groups generally have 2 or more carbon atoms and usually 24 or less, and in some embodiments, 12 or less carbon atoms;
[0048] For example, aryl groups such as phenyl and naphthyl generally have 6 or more carbon atoms and usually 36 or less, and in some embodiments, 24 or less carbon atoms;
[0049] For example, heteroaryl groups such as thienyl and pyridyl usually have 3 or more carbon atoms, in some embodiments, 4 or more carbon atoms, and usually have 36 or less carbon atoms, in some embodiments, 24 or less carbon atoms.
[0050] In some embodiments, it is the above-mentioned alkyl group, alkoxy group, aryl group, or heteroaryl group. In some embodiments, it has no substituent, that is, is hydrogen, from the viewpoint of charge transport properties.
[0051] Examples of aryl and heteroaryl groups include, but are not limited to, the following structures.
[0052] For example, groups such as phenyl, naphthyl, phenanthryl, thienyl, pyridyl, furyl, benzofuranyl, benzothienyl, pyrrolyl, pyrazolyl, imidazolyl, oxadiazolyl, indolyl, carbazolyl, pyrroloimidazolyl, pyrrolopyrrolyl, pyrrolopyrazolyl, thienopyrrolyl, thienothiphenyl, furopyrrolyl, furofuranyl, thienofuranyl, benzisoxazolyl, benzisothienyl, benzimidazolyl, pyridyl, pyrazinyl, pyridazinyl, pyrimidinyl, triazinyl, quinolyl, isoquinolyl, shinorine, quinoxalinyl, phenanthridinyl, benzimidazolyl, perylene diazaphenyl, quinazolinyl, quinazolinonyl, and azulenyl groups,
[0053] In addition, the above-mentioned substituents may be further substituted, for example, by the same groups as the above-mentioned substituents (substituents) or by crosslinking groups described below. In some embodiments, they are not further substituted, or are substituted by an alkyl group having 6 or less carbon atoms, an alkoxy group having 6 or less carbon atoms, a phenyl group, or a crosslinking group described below.
[0054] From the viewpoint of charge transport properties, in some embodiments, no further substitution is performed.
[0055] The polymer of the present application must have a crosslinking group. By having a crosslinking group, a large difference in solubility in a solvent can be generated before and after the reaction (insolubilization reaction) initiated by heat and / or irradiation with active energy rays.
[0056] The crosslinkable group refers to a group that reacts with the same or different group of another nearby molecule by heat and / or irradiation with active energy rays to form a new chemical bond.
[0057] The polymer of the present application has three repeated polymerization units, and there is no distinction between the order of the three repeating polymerization units. Formula (I) and formula (II) only represent the structure of the polymerization units.
[0058] The polymer of the present application, when used as a charge injection layer or transport layer material in an OLED device, has the characteristics of low starting voltage and high device efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 NMR spectrum of polymer compound 1,
[0060] Figure 2 NMR spectrum of polymer compound 2,
[0061] Figure 3 NMR spectrum of polymer compound 3,
[0062] Figure 4 NMR spectrum of polymer compound 4,
[0063] Figure 5 NMR spectrum of polymer compound 5,
[0064] Figure 6 NMR spectrum of polymer compound 6,
[0065] Figure 7 NMR spectrum of polymer compound 7. DETAILED DESCRIPTION
[0066] The present application is further described in detail below with reference to the embodiments.
[0067] All raw materials used are commercially available.
[0068] Method for producing polymer body
[0069] The polymer host can be produced using a known polymerization method described in Chem. Rev., 109, 897-1091, 2009, etc. Examples include polymerization methods using a coupling reaction using a transition metal catalyst such as Suzuki reaction, Yamamoto reaction, Buchwald reaction, Stille reaction, Negishi reaction, and Kumada reaction.
[0070] Example 1 (polymer compound 1)
[0071] In a 250 mL double-necked round-bottom flask, precisely weigh compound 1 (1.0 g, 1.431 mmol) and compound 2 (610 mg, 1.431 mmol). Toluene (50 mL) and 2M K₂CO₃ (10 mL) were then added at room temperature. The atmosphere was replaced with nitrogen three times, and then bubbled with nitrogen for 20 minutes. Next, 65.5 mg (0.072 mmol) of the catalyst Pd₂(dba)₃ and 68.2 mg (0.143 mmol) of the ligand x-phos were added. A drop of Aliquat 336 was added, and nitrogen bubbling continued for 20 minutes. The balloon was removed, the flask sealed, and heated to 96°C for 26 hours. 0.1 g of bromobenzene was dissolved in 1 mL of toluene and added to the reaction mixture with stirring for 1 hour to cap the reaction. 0.1 g of phenylboronic acid was dissolved in 1 mL of toluene and added to the reaction mixture with stirring for 1 hour to cap the reaction. After completion, 10 mL of saturated sodium diethyldithiocarbamate was added and stirring was continued for 14 h.
[0072] The reaction mixture was cooled to room temperature, and most of the toluene and water were dried at 80°C. Then, approximately 20 mL of toluene was added to completely dissolve the crude product. The product was then precipitated in 800 mL of methanol at room temperature, washed with water, and then dried. The product was concentrated and reprecipitated with dichloromethane to give a white, yellowish solid. The product was dried at 70°C for 24 h to yield 0.48 g, a 47.1% yield. The product had Mn = 68,800, Mw = 133,472, and PDI (Mw / Mn) = 1.94. n = 187 (133,472 / 712). The NMR spectra are shown in Figure 1.
[0073] Example 2 (polymer compound 2)
[0074] In a 250 mL double-necked round-bottom flask, precisely weigh compound 1 (1.0 g, 1.431 mmol), compound 2 (244 mg, 0.572 mmol), and compound 3 (412 mg, 0.859 mmol). Toluene (50 mL) and 2M K₂CO₃ (10 mL) were then added at room temperature. The atmosphere was replaced with nitrogen three times, and then bubbled with nitrogen for 20 minutes. Next, 65.5 mg (0.072 mmol) of the catalyst Pd₂(dba)₃ and 68.2 mg (0.143 mmol) of the ligand x-phos were added. A drop of Aliquat 336 was added, and nitrogen bubbling continued for 20 minutes. The balloon was removed, the flask sealed, and heated to 96°C for 26 hours. 0.1 g of bromobenzene was dissolved in 1 mL of toluene and added to the reaction mixture, stirring for 1 hour to cap the reaction. Another 0.1 g of 4-vinylphenylboronic acid was dissolved in 1 mL of toluene and added to the reaction mixture, stirring for 1 h to cap the reaction. After completion, 10 mL of saturated sodium diethyldithiocarbamate was added and stirring continued for 14 h.
[0075] The reaction mixture was cooled to room temperature, and most of the toluene and water were dried at 80°C. Then, approximately 20 mL of toluene was added to completely dissolve the crude product. The product was then precipitated in 800 mL of methanol at room temperature, washed with water, and then dried. The product was concentrated and precipitated again using dichloromethane to obtain a white, yellowish solid. The product was dried at 70°C for 24 h to yield 0.53 g of product, a 45.8% yield. The product had a number-average molecular weight (Mn) of 115,100, a weight-average molecular weight (Mw) of 231,351, and a PDI (Mw / Mn) of 2.01. The NMR spectrum is shown in Figure 2.
[0076] Example 3 (polymer compound 3)
[0077] In a 250 mL double-necked round-bottom flask, precisely weigh compound 1 (1.0 g, 1.431 mmol), compound 2 (244 mg, 0.572 mmol), compound 3 (412 mg, 0.572 mmol), and compound 4 (134 mg, 0.287 mmol). Toluene (50 mL) and 2M K₂CO₃ (10 mL) were then added at room temperature. The atmosphere was replaced with nitrogen three times, and then bubbled with nitrogen for 20 minutes. Next, 65.5 mg (0.072 mmol) of the catalyst Pd₂(dba)₃ and 68.2 mg (0.143 mmol) of the ligand x-phos were added. A drop of Aliquat 336 was added, and nitrogen bubbling continued for 20 minutes. The balloon was removed, the flask sealed, and heated to 96°C for 26 hours. 0.1 g of bromobenzene was dissolved in 1 mL of toluene and added to the reaction mixture, stirring for 1 hour to cap the reaction. 0.1 g of 4-vinylphenylboronic acid was dissolved in 1 mL of toluene and added to the reaction mixture, stirring for 1 h to cap the reaction. After completion, 10 mL of saturated sodium diethyldithiocarbamate was added and stirring continued for 14 h.
[0078] The reaction mixture was cooled to room temperature, and most of the toluene and water were dried at 80°C. Then, approximately 20 mL of toluene was added to completely dissolve the crude product. The product was then precipitated in 800 mL of methanol at room temperature, washed with water, and dried. The product was concentrated and precipitated again using dichloromethane to obtain a white, yellowish solid. Drying at 70°C for 24 h yielded 0.58 g of the product, a 46.4% yield. Mn = 105,200, Mw = 207,244, PDI = 1.97. The NMR spectrum is shown in Figure 3.
[0079] Example 4-(Polymer Compound 4)
[0080] In a 250 mL double-necked round-bottom flask, precisely weigh compound 1 (1.0 g, 1.431 mmol), compound 3 (245 mg, 0.572 mmol), and compound 5 (412 mg, 0.859 mmol). Toluene (50 mL) and 2M K₂CO₃ (10 mL) were then added at room temperature. The atmosphere was replaced with nitrogen three times, and then bubbled with nitrogen for 20 minutes. Next, 65.5 mg (0.072 mmol) of the catalyst Pd₂(dba)₃ and 68.2 mg (0.143 mmol) of the ligand x-phos were added. A drop of Aliquat 336 was added, and nitrogen bubbling continued for 20 minutes. The balloon was removed, the apparatus sealed, and the reaction heated to 96°C for 26 hours.
[0081] Take a small amount of the reaction solution and add one drop each to methanol (1.5 mL) and n-hexane (1.5 mL). The precipitate is filamentous and the reaction solution is not rubbery. Dissolve 0.1 g of bromobenzene in 1 mL of toluene and add to the reaction solution, stirring for 1 hour to cap the end. Then, dissolve 0.1 g of phenylboric acid in 1 mL of toluene and add to the reaction solution, stirring for 1 hour to cap the end. After completion, add 10 mL of saturated sodium diethyldithiocarbamate and continue stirring for 14 hours.
[0082] The reaction mixture was cooled to room temperature, and most of the toluene and water were dried at 80°C. Then, approximately 20 mL of toluene was added to completely dissolve the crude product. The product was then precipitated in 800 mL of methanol at room temperature, washed with water, and dried. The product was concentrated and precipitated again using dichloromethane to obtain a white, yellowish solid. Drying at 70°C for 24 h yielded 0.48 g of the product, a 41.9% yield. Mn = 110,100, Mw = 199,281, and PDI = 1.81. The NMR spectrum is shown in Figure 4.
[0083] Example 5 (polymer compound 5)
[0084] In a 250 mL double-necked round-bottom flask, precisely weigh compound 1 (1.0 g, 1.431 mmol) and compound 3 (0.685 g, 1.431 mmol). Toluene (50 mL) and 2M K₂CO₃ (10 mL) were then added at room temperature. The atmosphere was replaced with nitrogen three times, and then bubbled with nitrogen for 20 minutes. Next, 65.5 mg (0.072 mmol) of the catalyst Pd₂(dba)₃ and 68.2 mg (0.143 mmol) of the ligand x-phos were added. A drop of Aliquat 336 was added, and nitrogen bubbling continued for 20 minutes. The balloon was removed, the flask sealed, and heated to 96°C for 26 hours. 0.07 g of compound 3 was dissolved in 1 mL of toluene and added to the reaction solution, stirring for 1 hour. 0.1 g of 4-vinylphenylboronic acid was dissolved in 1 mL of toluene and added to the reaction solution, stirring for 1 hour, to cap the reaction. After completion, 10 mL of saturated sodium diethyldithiocarbamate (metal chelator) was added and stirring was continued for 14 h.
[0085] The reaction mixture was cooled to room temperature, and most of the toluene and water were dried at 80°C. Then, approximately 20 mL of toluene was added to completely dissolve the crude product. The product was then precipitated in 800 mL of methanol at room temperature, washed with water, and then dried. The product was concentrated and precipitated again using dichloromethane to obtain a white, yellowish solid. The product was dried at 70°C for 24 h to yield 0.45 g, a 41.1% yield. The product had an Mn of 62,220, an Mw of 120,710, and a PDI (Mw / Mn) of 1.94. The NMR spectrum is shown in Figure 5.
[0086] Example 6 (Polymer Compound 6)
[0087] In a 250 mL double-necked round-bottom flask, precisely weigh compound 1 (1.0 g, 1.431 mmol) and compound 4 (0.668 g, 1.431 mmol). Toluene (50 mL) and 2M K₂CO₃ (10 mL) were then added at room temperature. The atmosphere was replaced with nitrogen three times, and then bubbled with nitrogen for 20 minutes. Next, 65.5 mg (0.072 mmol) of the catalyst Pd₂(dba)₃ and 68.2 mg (0.143 mmol) of the ligand x-phos were added. A drop of Aliquat 336 was added, and nitrogen bubbling continued for 20 minutes. The balloon was removed, the flask sealed, and heated to 96°C for 26 hours. 0.1 g of compound 4 was dissolved in 1 mL of toluene and added to the reaction solution, stirring for 1 hour. 0.1 g of 4-vinylphenylboronic acid was dissolved in 1 mL of toluene and added to the reaction solution, stirring for 1 hour, to cap the reaction. After completion, 10 mL of saturated sodium diethyldithiocarbamate (metal chelator) was added and stirring was continued for 14 h.
[0088] The reaction mixture was cooled to room temperature, and most of the toluene and water were dried at 80°C. Then, approximately 20 mL of toluene was added to completely dissolve the crude product. The product was then precipitated in 800 mL of methanol at room temperature, washed with water, and then dried. The product was concentrated and precipitated again using dichloromethane to obtain a white, yellowish solid. The product was dried at 70°C for 24 h to yield 0.47 g, a 43.3% yield. The product had an Mn of 57,700, an Mw of 109,640, and a PDI (Mw / Mn) of 1.90. The NMR spectrum is shown in Figure 6.
[0089] Example 7-Comparative Example 1 (Polymer Compound 7)
[0090] In a 250 mL double-necked round-bottom flask, precisely weigh compound 1 (1.0 g, 1.431 mmol) and compound 6 (0.785 mg, 1.431 mmol). Toluene (50 mL) and 2M K₂CO₃ (10 mL) were then added at room temperature. The atmosphere was replaced with nitrogen three times, and then bubbled with nitrogen for 20 minutes. Next, 65.5 mg (0.072 mmol) of the catalyst Pd₂(dba)₃ and 68.2 mg (0.143 mmol) of the ligand x-phos were added. A drop of Aliquat 336 was added, and nitrogen bubbling continued for 20 minutes. The balloon was removed, the flask sealed, and heated to 96°C for 26 hours. 0.1 g of p-bromostyrene was dissolved in 1 mL of toluene and added to the reaction mixture with stirring for 1 hour to cap the reaction. 0.1 g of 4-vinylphenylboronic acid was dissolved in 1 mL of toluene and added to the reaction mixture with stirring for 1 hour to cap the reaction. After completion, 10 mL of saturated sodium diethyldithiocarbamate (metal chelator) was added and stirring was continued for 14 h.
[0091] The reaction mixture was cooled to room temperature, and most of the toluene and water were dried at 80°C. Then, approximately 20 mL of toluene was added to completely dissolve the crude product. The product was then precipitated in 800 mL of methanol at room temperature, washed with water, and then dried. The product was concentrated and precipitated again using dichloromethane to obtain a white, yellowish solid. The product was dried at 70°C for 24 h to yield 0.67 g, a 56.3% yield. The product had an Mn of 77,900, an Mw of 148,100, and a PDI (Mw / Mn) of 1.90. The NMR spectrum is shown in Figure 7.
[0092] Example 8 Preparation of Device
[0093] Manufacturing of OLEDs 1 to 7
[0094] OLED devices OLED 1 to OLED 7 having a structure of ITO / hole injection layer / hole transport layer / EML / ETL / cathode were manufactured according to the following steps:
[0095] 1) 50 nm PEDOT (CleviosTM VP AI 4083) was coated on an ITO (indium tin oxide) glass substrate as a hole injection layer and dried by heating at 230° C. in air for 15 minutes.
[0096] 2) Spin coating of methyl benzoate solution (0.5 wt%) of polymer 1-7 in a glove box to coat 20
[0097] nm hole transport layer.
[0098] 3) The hole transport layer was dried by heating at 230° C. for 30 minutes in a glove box.
[0099] 4) Vapor deposition of 40nm EML / 35nm ETL / 1nm Yb / 100nm Ag.
[0100] 5) Encapsulating the device.
[0101] The device results of OLED1 to OLED8 are as follows
[0102] The results show that OLEDs 1-5 have better device efficiency and lower operating voltage than devices 6 and 7. OLEDs 2-3, in particular, have excellent performance across all performance indicators. This indicates that the choice of repeating unit has a direct impact on device performance.
[0103] From the device data of OLED4-7, it can be seen that the device of this application has added olefin groups as cross-linking groups, and its device has higher relative efficiency and lower relative starting voltage, which shows that the addition of cross-linking groups improves the performance of the polymer of this application.
Claims
1. A high molecular polymer comprising at least one of the following three repeating units and terminated by Ar1 and Ar2, in, Ar1 and Ar2 independently represent C6-C36 aryl substituted or unsubstituted by R1 or R12, or C5-C36 heteroaryl substituted or unsubstituted by R1 or R12; R1-R12 each independently represents hydrogen, substituted or unsubstituted C6-C36 aryl, substituted or unsubstituted C5-C36 heteroaryl, substituted or unsubstituted C1-C24 alkyl, substituted or unsubstituted C2-C24 alkenyl, substituted or unsubstituted C3-C24 cycloalkenyl, substituted or unsubstituted C6-C36 aryloxy, substituted or unsubstituted C5-C36 heteroaryloxy, substituted or unsubstituted C2-C24 alkane; Oxycarbonyl, substituted or unsubstituted di-C1-C24 alkylamino, substituted or unsubstituted di-C6-C36 arylamino, substituted or unsubstituted C6-C36 aryl-C1-C24 alkylamino, substituted or unsubstituted C2-C24 alkanoyl, substituted or unsubstituted C8-C36 arylcycloalkyl, substituted or unsubstituted C3-C24 epoxy; wherein at least one of R1-R12 is a crosslinking group; Wherein the substitution in R1-R12 is substitution by halogen, C1-C8 alkyl, C3-C8 epoxy, C1-C8 alkoxy, C2-C8 alkenyl, C6-C10 aryl or C4-C10 cycloalkenylalkyl; In the formula, m, n, and p represent the number of each repeating unit, m≥0, n≥0, and p≥0; and m and n are not zero at the same time; Weight average molecular weight Mw = 10000-1000000, dispersion degree PDI = 1.0-3.
0.
2. The high molecular weight polymer according to claim 1, having the structure described in the following formula (I), wherein R1-R12 each independently represents hydrogen, substituted or unsubstituted C6-C24 aryl, substituted or unsubstituted C5-C24 heteroaryl, substituted or unsubstituted C1-C12 alkyl, substituted or unsubstituted C2-C12 alkenyl, substituted or unsubstituted C3-C12 cycloalkenyl, substituted or unsubstituted C6-C24 aryloxy, substituted or unsubstituted C5-C24 heteroaryloxy, substituted or unsubstituted C2-C12 alkoxycarbonyl, substituted or unsubstituted di-C1-C12 alkylamino, substituted or unsubstituted di-C6-C24 arylamino, substituted or unsubstituted C6-C24 aryl-C1-C12 alkylamino, substituted or unsubstituted C2-C12 alkanoyl, substituted or unsubstituted C8-C24 arylcycloalkyl, substituted or unsubstituted C3-C12 epoxy, Mw is 20000-800000, wherein the substitution in R1-R12 is substituted by halogen, C1-C6 alkyl, C3-C6 epoxy, C1-C6 alkoxy, C2-C6 alkenyl, C6-C10 aryl or C4-C10 cycloalkenyl, The definitions of m, n and p are the same as those in claim 1.
3. The high molecular polymer according to claim 2, wherein R1, R4, R7, R10-R12 are each independently hydrogen, substituted or unsubstituted C6-C12 aryl, substituted or unsubstituted C5-C12 heteroaryl, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl, substituted or unsubstituted C3-C6 cycloalkenyl, substituted or unsubstituted C6-C12 aryloxy, substituted or unsubstituted C5-C12 heteroaryloxy, substituted or unsubstituted C2-C6 alkoxycarbonyl, substituted or unsubstituted di-C1-C6 alkylamino, substituted or unsubstituted di-C6-C12 arylamino, substituted or unsubstituted C6-C12 aryl-C1-C6 alkylamino, substituted or unsubstituted C2-C6 alkanoyl, substituted or unsubstituted C8-C12 aryl-C1-C6 alkylamino, substituted or unsubstituted C2-C6 alkanoyl, substituted or unsubstituted C8-C12 aryl-cycloalkyl, substituted or unsubstituted C3-C6 epoxy, at least one of R1, R4, R7, R10-R12 is a crosslinking group, R2-R3, R5-R6, R8-R9 each independently represent a substituted or unsubstituted C6-C12 aryl group, a substituted or unsubstituted C5-C12 heteroaryl group, a substituted or unsubstituted C1-C6 alkyl group; Mw is 50000-500000, and the dispersion degree PDI = 1.5-2.
5.
4. The high molecular polymer according to claim 1, wherein the crosslinking group is R-substituted C8-C12 aryl and cycloalkyl, R-substituted C3-C6 epoxy, R-substituted C2-C6 alkenyl, C4-C10 cycloalkenyl substituted C8-C12 aryl, R-substituted vinylphenylene, wherein R is hydrogen, halogen, C1-C6 alkyl, C1-C6 alkoxy, C6-C10 aryl.
5. The high molecular polymer according to claim 4, wherein the crosslinking group is one of the following structures: Wherein R is hydrogen, C1-C6 alkyl, C6-C10 aryl.
6. The high molecular polymer according to any one of claims 1 to 5, wherein Ar1 and Ar2 are independently represented by C6-C10 aromatic groups substituted or unsubstituted by R1 or R12.
7. The high molecular polymer according to claim 6, whose structure is shown in formula (II), R1, R4, R7, R10-R12 are each independently hydrogen, substituted or unsubstituted C6-C12 aryl, substituted or unsubstituted C5-C12 heteroaryl, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl, substituted or unsubstituted C3-C6 cycloalkenyl, substituted or unsubstituted C8-C12 aryl and cycloalkyl, substituted or unsubstituted C3-C6 epoxy; R2 is the same as R3, R5 is the same as R6, and R8 is the same as R9; Mw is 100000-300000, and the dispersion degree PDI is 1.7-2.3; The definitions of m, n and p are the same as those in claim 1.
8. The high molecular polymer according to claim 7, wherein R1 and R12 are the same and are both cross-linking groups.
9. The high molecular weight polymer according to claim 1, wherein: m=1, n=0~1000, p=0~1000.
10. The high molecular polymer according to claim 2, wherein: m=1~1000, n=1~1000, p=0~1000.
11. The high molecular polymer according to claim 3, wherein: m=1~1000, n=1~1000, p=1~1000.
12. The high molecular weight polymer according to any one of claims 9 to 11, wherein: R2 is the same as R3, R5 is the same as R6, R8 is the same as R9, and at least one of R4, R7, R10-R11 is a crosslinking group.
13. An organic electroluminescent element, comprising the high molecular weight polymer according to any one of claims 1 to 12.
14. The organic electroluminescent element according to claim 13 comprises at least one of a light-emitting layer, a charge injection layer and a charge transport layer, wherein the high molecular polymer according to any one of claims 1 to 12 is located in the light-emitting layer, the charge injection layer and / or the charge transport layer. 15 . The organic electroluminescent device according to claim 14 , wherein the high molecular polymer is fixed in the organic electroluminescent device by a wet film forming method.
Citation Information
Patent Citations
Fluorine-carbazole co-polymer based organic electroluminescence device
CN101114698A
Polymer compound and polymer light-emitting device using the same
CN101516960A
Polymer, organic electroluminescence element material, composition for organic electroluminescence element, organic electroluminescence element, display device, and lighting device
CN102791768A
Methoxytriphenylamine-fluorene-containing copolymer, and preparation method and application thereof
CN103396533A
Cross-linking polymer and organic electroluminescent element using same
CN103717636A