Cold-rolled steel sheet, stamping member, and manufacturing method for cold-rolled steel sheet
By optimizing the chemical composition and hot rolling process, cold-rolled steel plates with high spheroidization rate and excellent hardenability are prepared, which solves the problems of insufficient hardenability and high production cost of existing steel materials, and achieves improvement in complex stamping performance and cost savings. .
Patent Information
- Application Number
- PCT/CN2024/084305
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Existing stamping steel materials have insufficient hardenability during heat treatment, resulting in dimensional deformation of parts and poor stamping performance. In addition, the existing process increases the number and time of spheroidizing annealing and increases production costs.
By optimizing the chemical composition ratio and hot rolling process, the cold-rolled steel plate is prepared. Its microstructure is uniformly distributed spherical cementite particles on a single-phase ferrite matrix, with a spheroidization rate of ≥90%. The bell annealing process is used to shorten the annealing. time and reduce production costs.
It achieves excellent hardenability and high spheroidization rate of cold-rolled steel plates during heat treatment, meets complex stamping requirements, and reduces manufacturing costs.
Smart Images

Figure CN2024084305_03102024_PF_FP_ABST
Abstract
Description
Cold-rolled steel plate, stamping part and manufacturing method thereof Technical Field
[0001] The present invention relates to a plate and a manufacturing method thereof, and in particular to a cold-rolled steel plate and a manufacturing method thereof. Background Art
[0002] Automotive stamping steel is widely used in the automotive parts manufacturing industry. Hot-rolled steel, due to its coarse pearlite lamellae, has high strength but poor plasticity, making it difficult to form directly. Furthermore, hot-rolled steel suffers from poor surface quality and thickness accuracy. Therefore, hot-rolled steel requires subsequent cold rolling and spheroidizing annealing before it can be used in the complex fine-blanking process.
[0003] The microstructure and properties of automotive stamping steel are essential for the stamping of complex parts. To achieve excellent stamping performance, the material requires high plasticity, low strength, and uniform properties. This is achieved by increasing the spheroidization rate. Key factors influencing spheroidization include the hot-rolled steel's original microstructure and the annealing process.
[0004] In the existing production process, the spheroidization rate of the material is usually improved by increasing the number of spheroidizing annealing times and extending the spheroidizing annealing time. However, the increase in the number of annealing times and the extension of the annealing time greatly increase the production cost.
[0005] In addition, for some materials or parts that require heat treatment, especially medium carbon steel, high carbon steel, alloy steel and other steels, the parts need to be heat treated after stamping. This requires the material to have good hardenability and be quenched under quenching media such as oil quenching to produce full martensite and improve the strength of the parts. However, due to the design of the alloy composition system, the existing steel grades generally require a faster cooling rate (≥30℃ / s) to quench into martensite. This places higher requirements on the thickness of the material and the cooling medium. At the same time, it is also necessary to consider related issues such as insufficient hardenability and dimensional deformation of the parts.
[0006] Based on this, it is desired to provide a cold-rolled steel sheet and a method for manufacturing the same, which can achieve a high spheroidization rate with a simple process.
[0007] Summary of the Invention
[0008] One of the purposes of the present invention is to provide a cold-rolled steel sheet having a high spheroidization rate, good plasticity and low strength, which can meet the requirements of complex stamping and has excellent hardenability during heat treatment.
[0009] In order to achieve the above object, the present invention provides a cold-rolled steel sheet containing Fe and unavoidable impurities, and further containing the following chemical elements in the following mass percentages:
[0010] C: 0.06~0.10wt%, Si: 0.01~0.5wt%, Mn: 1.6~2.5wt%, Al: 0.01~0.07wt%, Cr: 0.5~1.0wt%, Mo : 0.1~0.3wt%, Ti: 0.01~0.05wt%, Nb: 0.001~0.03wt%, B: 0.0001~0.005wt%, 0<N≤0.006wt%;
[0011] The microstructure of the cold-rolled steel plate is that spherical cementite particles are evenly distributed on a single-phase ferrite matrix, wherein the spheroidization rate of the spherical cementite is ≥90%.
[0012] Accordingly, the present invention also provides a cold-rolled steel sheet, wherein the mass percentages of the chemical elements are as follows:
[0013] C: 0.06-0.10wt%, Si: 0.01-0.5wt%, Mn: 1.6-2.5wt%, Al: 0.01-0.07wt%, Cr: 0.5-1.0wt%, Mo: 0.1-0.3wt%, Ti: 0.01-0.05wt%, Nb: 0.001-0.03wt%, B: 0.0001-0.005wt%, 0<N≤0.006wt%; the balance is Fe and unavoidable impurities;
[0014] The microstructure of the cold-rolled steel plate is spherical cementite particles uniformly distributed on a single-phase ferrite matrix, wherein the spheroidization rate of the spherical cementite is ≥90%.
[0015] The present invention reasonably controls carbon, manganese, chromium, molybdenum, boron and their contents and realizes the mutual coordination between the constituent elements, so that the cold-rolled steel plate obtains good hardenability, obtains martensitic structure at a lower cooling rate during heat treatment, and improves the strength and hardness of the material.
[0016] The reasons for designing the composition of each chemical component adopted in the present invention are as follows:
[0017] Carbon: In the technical solution described in the present invention, carbon is an important strengthening element, significantly increasing the strength of steel through solid solution strengthening. However, an excessively high carbon content not only significantly increases the carbon equivalent of the steel strip, reducing weldability, but also reduces its plasticity and increases its cold brittleness and aging sensitivity. Therefore, the carbon content should be kept to a minimum. Consequently, the carbon content in the cold-rolled steel sheet of the present invention is controlled to be between 0.06 and 0.10 wt%.
[0018] Silicon: Silicon is a ferrite solid solution strengthening element that can improve strength. However, adding silicon will increase the carbon equivalent, reduce weldability, and is also detrimental to phosphating properties. Therefore, the mass percentage of silicon in the cold-rolled steel sheet of the present invention is controlled at 0.01 to 0.5 wt%.
[0019] Manganese: Manganese has a strong solid solution strengthening effect and can effectively increase the strength of steel sheets. Therefore, to meet the high strength requirements after heat treatment, a certain amount of Mn is added to the cold-rolled steel sheets of the present invention. However, because an excessively high Mn content significantly increases the carbon equivalent of the steel sheet, reducing weldability and exacerbating segregation, it can negatively impact formability, such as plasticity, hole expansion, and bendability. Therefore, the Mn content in the cold-rolled steel sheets of the present invention is controlled to 1.6-2.5 wt%.
[0020] Aluminum: Al acts as a deoxidizer, combining with nitrogen to form AlN, which helps prevent austenite grain coarsening. However, when the Al content exceeds 0.07 wt%, the purity of the steel sheet decreases. Therefore, the cold-rolled steel sheet of the present invention controls the Al content to 0.01 to 0.07 wt%.
[0021] Chromium: Chromium in steel primarily serves to delay the austenite transformation incubation period, improve hardenability, and delay the transformation of ferrite and pearlite. This inhibits the formation of these structures during cooling, allowing the steel to enter the martensitic transformation zone directly without high cooling rates. Therefore, the chromium content in the cold-rolled steel sheet of the present invention is controlled to be between 0.5 and 1.0 wt%.
[0022] Molybdenum: Molybdenum's primary role in steel is solid solution strengthening. It also improves carbide stability, thereby increasing steel strength. It also enhances hardenability and hot resistance, preventing temper brittleness. Therefore, the molybdenum content in the cold-rolled steel sheet of the present invention is 0.1-0.3 wt%.
[0023] Titanium: In the present invention, Ti is a strong carbon and nitride-forming element with strong grain refinement and precipitation strengthening effects. The addition of Ti in the present invention also helps to reduce cracks in the edges and corners of slabs. Furthermore, compared to elemental Nb, the price of Ti is less than one-tenth of Nb, offering significant cost advantages. However, excessive addition of Ti reduces its strengthening effect. Therefore, the mass percentage of Ti in the high-strength cold-rolled steel strip described in the present invention is controlled to be between 0.01 and 0.05 wt%.
[0024] Niobium: Niobium is a strong carbon and nitride-forming element, exhibiting strong grain refinement and precipitation strengthening effects, contributing to improved strip strength. However, excessive Nb content can lead to carbon and nitride segregation, impairing the steel's workability. Furthermore, Nb is very expensive, and excessive addition increases costs. Therefore, the Nb content should be kept to a minimum. In the technical solution described herein, the Nb content is controlled to 0.001 to 0.03 wt%.
[0025] Boron: Boron is an element that strongly segregates at the austenite grain boundaries in steel, reducing the grain boundary energy of austenite and inhibiting the formation of proeutectoid ferrite nuclei. Boron has three key advantages for improving the hardenability of steel: a strong ability to enhance hardenability, and requiring only minimal amounts of Boron, while conserving significant quantities of precious alloying elements. However, Boron has an optimal content for enhancing hardenability. Unlike general alloying elements, the effect of Boron on hardenability increases with its content in steel. To effectively enhance hardenability, the Boron content in the present invention must be above 0.0001 wt%. However, when the content exceeds 0.005 wt%, the effect of enhancing hardenability reaches saturation. Therefore, the Boron content in the present invention is controlled between 0.0001 and 0.005 wt%.
[0026] Nitrogen: In Ti-containing steels, appropriate amounts of nitrogen (N) react with titanium (Ti) to form TiN at high temperatures, strengthening the matrix and improving the weldability of the steel. However, excessive nitrogen content can cause TiN to coarsen or lead to excessive nitrogen solid solution, reducing the steel's plasticity and hole expansion and flanging properties. Furthermore, excessive nitrogen content can form AlN nitrides during hot rolling, reducing the blanking performance and hardenability of the base steel. Therefore, in the technical solution of the present invention, the nitrogen content is controlled within the range of 0 < N ≤ 0.006 wt%.
[0027] The unavoidable impurities in the present invention are mainly S and P. Among them, phosphorus increases the cold brittleness of steel, reduces the plasticity of steel, and also has an adverse effect on weldability. Therefore, in the cold-rolled steel sheet of the present invention, the lower the content of the impurity P, the better. However, considering the smelting cost, in some embodiments, the mass percentage of P can be controlled to P ≤ 0.015wt%.
[0028] Sulfur easily forms MnS with Mn in steel, deteriorating mechanical properties, hole expansion performance and other forming properties. Therefore, in the technical solution described in the present invention, the lower the S content, the better. Therefore, in some embodiments of the present invention, the mass percentage of S can be controlled to S≤0.01wt%.
[0029] Furthermore, in the cold-rolled steel sheet of the present invention, the grain size of ferrite is 7.0 to 11.0.
[0030] Furthermore, the spheroidization rate of spheroidized cementite in the cold-rolled steel sheet of the present invention is ≥95%.
[0031] Furthermore, the yield strength of the cold-rolled steel sheet of the present invention is 280-420 MPa, the tensile strength is 450-600 MPa, and the elongation after fracture A is 280-420 MPa. 50mm ≥25%.
[0032] In some embodiments, the yield strength of the cold-rolled steel sheet of the present invention is 380-420 MPa, for example, 389-420 MPa.
[0033] In some embodiments, the tensile strength of the cold-rolled steel sheet of the present invention is 482-600 MPa, for example, 498-600 MPa, 529-600 MPa, 568-600 MPa, or 597-600 MPa.
[0034] Furthermore, the microstructure of the cold-rolled steel sheet in the hot-rolled state is a mixed structure of ferrite+pearlite+martensite.
[0035] Another object of the present invention is to provide a method for manufacturing a cold-rolled steel sheet, wherein the cold-rolled steel sheet produced has a high spheroidization rate, good plasticity and low strength, can meet the requirements of complex stamping, and also has excellent hardenability during heat treatment.
[0036] Based on the above objectives, the present invention also provides a method for manufacturing the cold-rolled steel sheet as described above, which comprises the steps of:
[0037] Smelting and casting to obtain slabs;
[0038] Hot rolling: heating, rolling and coiling; the coiling temperature is 500-620℃;
[0039] Pickling and cold rolling;
[0040] Hood annealing: annealing soaking temperature is 660-710℃, annealing soaking time is 5-30h;
[0041] smooth.
[0042] In the manufacturing method of the present invention, the hot rolling step is a key step in improving the spheroidization rate of spheroidal cementite in the microstructure of the cold-rolled steel sheet. The existing technology generally adopts a medium-high temperature coiling temperature of 620-670°C, and the microstructure of the hot-rolled steel sheet obtained is banded ferrite + massive pearlite, and there will be banded structure. In order to obtain a product with spheroidal cementite with the highest possible spheroidization rate and spheroidal cementite uniformly dispersed in the ferrite matrix, the existing technology generally adopts a process of increasing the number of spheroidizing annealing times (2 times or more) and extending the spheroidizing annealing time to allow the cementite to fully diffuse and ultimately obtain dispersed spheroidal cementite particles. However, the increase in the number of annealing times and the extension of the annealing time greatly increase the production cost.
[0043] Unlike the prior art, the manufacturing method of the present invention adopts a low-temperature coiling process of 500°C to 620°C in the hot rolling step. The microstructure of the prepared hot-rolled steel plate is a uniform ferrite + pearlite + bainite / martensite structure. The carbides in these structures are evenly distributed, so the diffusion distance required in the subsequent cold rolling step and spheroidizing annealing step is greatly shortened. Under the same spheroidizing annealing process, a better spheroidization rate structure can be obtained. Therefore, the manufacturing method of the present invention does not require multiple and long-term annealing to obtain well-spheroidized spherical cementite particles.
[0044] In the present invention, if the coiling temperature is below 500°C, the steel plate will be prone to cracking due to the high martensite content produced during coiling. Furthermore, low coiling temperatures lead to large fluctuations in temperature control, large fluctuations in properties, and significant microstructure differences, which can easily generate internal stress and lead to poor plate shape. Therefore, the present invention adopts a low-temperature coiling process of 500°C to 620°C.
[0045] Annealing is the process of slowly heating a metal to a certain temperature, holding it for a sufficient time, and then cooling it at an appropriate rate. The purpose is to reduce the hardness increase of the steel plate caused by the cold rolling step, so as to improve the fine blanking processing performance. In the manufacturing method of the present invention, a bell-type annealing furnace is used for annealing, and the annealing temperature is selected to be below the A1 point temperature (i.e., the temperature at which austenite, ferrite, and cementite coexist in equilibrium under equilibrium conditions). This is because: too low an annealing temperature requires further extension of the holding time to obtain a good spheroidizing effect, and too high an annealing temperature will cause the strip to enter the two-phase region, and in the subsequent cooling process, the phase will transform into an undesirable structure of massive pearlite. At the same time, it will also cause coarse ferrite grains and obvious surface decarburization, affecting the final use performance of the material. Therefore, in order to improve the spheroidizing annealing effect, the present invention sets the annealing soaking temperature of the cold-rolled steel plate in the bell-type annealing furnace to 660-710°C. The soaking time during annealing is also critical. If the soaking time is too short, fine spherical particles cannot be formed and a dispersed distribution of cementite particles cannot be achieved. If the soaking time is too long, the spherical pearlite will grow again and agglomerate, forming lamellar segregation, resulting in reduced material plasticity and hindering subsequent fine blanking processing. Therefore, to improve the spheroidizing annealing effect, the annealing soaking time of the cold-rolled steel sheet in the bell annealing step of the present invention is 5 to 30 hours.
[0046] Compared with the prior art, the above-mentioned annealing process of the present invention greatly saves manufacturing costs while retaining the high spheroidization rate of spheroidal cementite of the cold-rolled steel sheet obtained after annealing under the conditions of reducing the number of spheroidizing annealing times and shortening the spheroidizing annealing time. Therefore, the obtained cold-rolled steel sheet has the advantages of good plasticity and low strength, has good stamping performance, and can meet complex stamping requirements.
[0047] In some embodiments of the present invention, the smelting is carried out using a converter or an electric furnace, and the thickness of the slab can be 80 to 300 mm.
[0048] Furthermore, in the hot rolling step of the manufacturing method of the present invention, the slab heating temperature is controlled to be 1180-1280°C, and the finishing rolling temperature is controlled to be 870-940°C.
[0049] The slab heating temperature during the hot rolling step of the present invention is controlled between 1180°C and 1280°C. This is to ensure that the microalloying elements in the slab are fully dissolved, thereby facilitating their full potential in subsequent steps. Since final rolling must be performed in the single-phase region, i.e., not below the Ar3 transformation temperature (the temperature at which the austenite to ferrite transformation begins during cooling), the final rolling temperature is controlled between 870°C and 940°C. If the final rolling temperature exceeds 940°C, the resulting oxide scale becomes thicker, reducing pickling resistance, potentially causing a decarburized layer on the surface of the steel sheet, and increasing the ferrite grain size. If the final rolling temperature is below the Ar3 transformation point, mixed crystals will form and the rolling load on the rolling mill will increase significantly. Therefore, limiting the final rolling temperature to the range of 870°C to 940°C avoids problems such as mixed crystals and increased rolling difficulty caused by too low a final rolling temperature, or excessively large grains that affect strengthening due to too high a temperature.
[0050] Furthermore, in the hot rolling step of the manufacturing method of the present invention, the slab heating temperature is controlled to be 1200-1250°C, and the final rolling temperature is controlled to be 890-930°C.
[0051] Furthermore, in the hot rolling step of the manufacturing method of the present invention, the coiling temperature is controlled to be 550-600°C.
[0052] In some embodiments of the present invention, in the hot rolling step, the slab heating temperature can be selected to be 1200-1250°C, the final rolling temperature is 890-930°C, and the coiling temperature is 500-620°C, thereby producing a bainite structure that is beneficial to improving the spheroidization rate, ultimately achieving the purpose of improving the spheroidization rate, improving the plasticity of cold-rolled steel, and reducing the strength. At the same time, it is beneficial to shorten the subsequent spheroidizing annealing time and reduce the number of subsequent spheroidizing annealing, thereby reducing manufacturing costs.
[0053] In some embodiments of the present invention, the finishing rolling step may further include water spray cooling to cool the steel plate to the coiling temperature at a set cooling rate for coiling, wherein the cooling rate may be >30°C / s.
[0054] Furthermore, in the cold rolling step of the manufacturing method of the present invention, the cold rolling reduction ratio of the cold-rolled steel sheet is controlled to be 20-60%.
[0055] The main parameter that determines the quality of cold-rolled steel sheets in the cold rolling step is the cold rolling reduction. An appropriate cold rolling reduction can generate distortion energy in the material and provide energy for the spheroidization transformation of pearlite. The present invention promotes the recrystallization of grains in the subsequent hood annealing step by cold rolling the hot-rolled steel sheets, obtains an appropriate grain size, and meets the requirements of continuous fine blanking processing. Therefore, it is necessary to set the reduction rate to more than 20%. On the other hand, if the reduction rate exceeds 60%, the steel sheet will harden due to excessive grain refinement, and the fine blanking performance of the obtained cold-rolled steel sheet will be reduced. At the same time, excessive deformation will cause excessive load on the cold rolling mill, increase the number of cold rolling passes, and increase the cold rolling cost.
[0056] Furthermore, in the cold rolling step of the manufacturing method of the present invention, the cold rolling reduction ratio of the cold-rolled steel sheet is controlled to be 30-50%.
[0057] The cold rolling reduction ratio is preferably controlled at 30-50% to further obtain a product with a target spheroidization ratio and grain size.
[0058] Furthermore, in the manufacturing method of the present invention, a flattening step is further performed after the hood annealing step, wherein the flattening elongation is controlled to be ≤2.5%.
[0059] Furthermore, in the manufacturing method of the present invention, the flattening elongation is controlled to be 0.5-2.0%, which can further obtain a suitable yield strength ratio, which is beneficial for subsequent precision stamping.
[0060] In some embodiments of the present invention, the surface of the obtained cold-rolled steel sheet is free of coating.
[0061] Another object of the present invention is to provide a stamping part (such as a stamping part for automobiles), which can be used for parts such as automobile engine systems, transmission systems, and automobile chassis systems.
[0062] Based on the above objectives, the present invention provides a stamping part (eg, a stamping part for automobiles), which is stamped by using the cold-rolled steel sheet described above.
[0063] Furthermore, the stamping part of the present invention is subjected to a heat treatment process with a heating temperature of 800-950° C. and a cooling rate of 10-30° C. / s to obtain a full martensitic structure.
[0064] Compared with the stamping parts in the prior art which require a cooling rate of ≥30°C / s to quench into martensite during heat treatment, the present invention can obtain full martensite even with a lower quenching cooling rate.
[0065] Furthermore, the automotive stamping parts of the present invention have a yield strength of 650-900 MPa, a tensile strength of 800-1100 MPa, and an elongation after fracture of A 50mm≥5.5%, e.g., ≥5.8%, ≥5.9%, ≥6.4%, ≥6.8%, ≥6.9%, ≥7.4% or ≥8%.
[0066] In some embodiments, the automotive stamping parts of the present invention have a yield strength of 663-900 MPa, such as 673-900 MPa, 735-900 MPa, 763-900 MPa, 858-900 MPa, or 868-900 MPa.
[0067] In some embodiments, the yield strength of the automotive stamping parts of the present invention is a tensile strength of 879-1100 MPa, for example, 976-1100 MPa, 998-1100 MPa, 1002-1100 MPa, 1055-1100 MPa, or 1078-1100 MPa.
[0068] The cold-rolled steel sheet and the manufacturing method thereof of the present invention have the following advantages and beneficial effects:
[0069] The cold-rolled steel sheet of the present invention optimizes the chemical composition ratio and the hot rolling process so that the microstructure of the hot-rolled steel sheet is a uniform ferrite + pearlite + martensite mixed structure. Furthermore, the microstructure of the cold-rolled steel sheet after cold rolling and spheroidizing annealing is spheroidal cementite particles uniformly dispersed on a ferrite matrix, and the spheroidization rate of the spheroidal cementite is ≥90%. Therefore, the cold-rolled steel has a high spheroidization rate, good plasticity, and low strength, meeting the requirements of precision blanking.
[0070] The manufacturing method of the present invention adopts a low-temperature coiling process of 500°C to 620°C in the hot rolling step. The microstructure of the prepared hot-rolled steel plate is a uniform mixed structure of ferrite, pearlite and martensite. The carbides in these structures are evenly distributed, so the diffusion distance required in the subsequent cold rolling step and spheroidizing annealing step is greatly shortened. Under the same spheroidizing annealing process, a better spheroidization rate structure can be obtained. Therefore, in the manufacturing method of the present invention, well-spheroidized spherical cementite particles can be obtained without multiple and long annealing.
[0071] The manufacturing method described in the present invention greatly saves manufacturing costs while retaining the high spheroidization rate of spheroidal cementite of the cold-rolled steel plate obtained after annealing, while reducing the number of spheroidizing annealing times and shortening the spheroidizing annealing time. Therefore, the obtained cold-rolled steel plate has the advantages of good plasticity and low strength, has good stamping performance, and can meet complex stamping requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] FIG1 shows a metallographic microstructure of a hot-rolled steel plate according to Example 1 of the present invention.
[0073] FIG2 shows a metallographic microstructure diagram of the cold-rolled steel sheet according to Example 1 of the present invention.
[0074] FIG3 shows a metallographic microstructure diagram of the stamping part after heat treatment according to Example 1 of the present invention. DETAILED DESCRIPTION
[0075] The cold-rolled steel sheet, its manufacturing method and the stamping parts described in the present invention will be further explained and illustrated below in conjunction with specific embodiments and the accompanying drawings. However, such explanation and illustration do not constitute an undue limitation to the technical solution of the present invention.
[0076] Examples 1-6 and Comparative Examples 1-2
[0077] Table 1 lists the mass percentages of various chemical elements in the cold-rolled steel sheets of Examples 1-6 and the comparative steel sheets of Comparative Examples 1-2.
[0078] Table 1. (wt%, the balance is Fe and other inevitable impurities except P and S)
[0079] The cold-rolled steel sheets of Examples 1-6 of the present invention are all prepared by the following steps:
[0080] (1) Smelting and casting according to the chemical composition shown in Table 1 to obtain slabs with a thickness of 80 to 300 mm.
[0081] (2) Hot rolling: the slab heating temperature is controlled to be 1180-1280°C, the final rolling temperature is 870-940°C, and water cooling is performed after final rolling at a cooling rate of >30°C / s, so that the steel plate temperature is cooled to a coiling temperature of 500-620°C for coiling; preferably, the slab heating temperature is controlled to be 1200-1250°C, the final rolling temperature is 890-930°C, and the coiling temperature is 560-620°C.
[0082] (3) Pickling and cold rolling: Pickling is performed to remove surface iron oxide scale. After the pickling step, a cold rolling step is performed, and the cold rolling reduction rate is controlled to be 20-60%, preferably 30-50%.
[0083] (4) Hood annealing: Control the annealing soaking temperature to 660-710℃ and the annealing soaking time to 5-30h.
[0084] (5) Smoothing: The smoothing rate is controlled to be ≤2.5%, preferably 0.5-2.0%.
[0085] Although the comparative steels of Comparative Examples 1-2 were also produced using the above-mentioned manufacturing process, their chemical composition design and specific manufacturing process parameters did not meet the design requirements of the present invention.
[0086] Table 2 lists the specific process parameters of the cold-rolled steel sheets of Examples 1-6 and the comparative steel sheets of Comparative Examples 1-2 in the steps of the above-mentioned manufacturing method.
[0087] Table 2.
[0088] In order to observe the microstructural changes of the present invention, the inventors also sampled the hot-rolled plates of Examples 1-6 after the hot rolling step and observed their microstructures. FIG1 shows a metallographic microstructure of the hot-rolled steel plate of Example 1 of the present invention.
[0089] As can be seen from Figure 1, the hot rolled microstructure is ferrite + pearlite + martensite. The microstructures of the hot rolled steel sheets of Examples 2-6 after the hot rolling step are all ferrite + pearlite + martensite.
[0090] The inventors also sampled the cold-rolled steel sheets produced in Examples 1-6 and Comparative Examples 1-2 and observed their microstructures using an optical microscope. The spheroidization rate of spheroidized cementite was measured under the optical microscope according to the SEP15203 series rating standard, and the results are listed in Table 3. The ferrite grain size was evaluated according to GB / T 6394, and the results are listed in Table 3.
[0091] Table 3 lists the metallographic microstructure observation results of the cold-rolled steel sheets of Examples 1-6 and the cold-rolled steel sheets of Comparative Examples 1-2.
[0092] Table 3.
[0093] It can be seen from Table 3 above that the microstructures of the cold-rolled steel sheets in Examples 1-6 are all composed of spherical cementite particles evenly distributed on a single-phase ferrite matrix, wherein the spheroidization rate of the spherical cementite is ≥90%.
[0094] In addition, FIG2 also shows a metallographic microstructure diagram of the cold-rolled steel sheet according to Example 1 of the present invention.
[0095] As shown in FIG2 , the microstructure shows a uniform distribution of ferrite and a dispersed distribution of spherical cementite, wherein the spheroidization rate of the spherical cementite is 99%.
[0096] The inventors also conducted mechanical property tests on the cold-rolled steel sheets used in the Examples and Comparative Examples. The composition of the Examples and Comparative Examples was determined according to GB / T 223. Yield strength, tensile strength, and elongation were tested according to GB / T 228-2002, with an elongation gauge length of 50 μm. Hole expansion performance was tested according to GB / T 15825.4-2008. The final results of these tests are listed in Table 4 below.
[0097] Table 4 lists the performance test results of the cold-rolled steel sheets of Examples 1-6 and the cold-rolled steel sheets of Comparative Examples 1-2.
[0098] Table 4.
[0099] As can be seen from Table 4, in the present invention, the yield strength of the cold-rolled steel sheets of Examples 1-6 is greater than 280 MPa, the tensile strength is greater than 450 MPa, and the elongation after fracture is greater than 0. 50mm All greater than 25%.
[0100] It can be seen from the above embodiments that the present invention can obtain cold-rolled steel sheets with good plasticity and low strength through appropriate chemical composition design and optimized manufacturing process, which can meet the requirements of subsequent complex stamping.
[0101] In order to further verify the stamping performance of the cold-rolled steel sheet of the present invention, each embodiment and comparative example was stamped into automotive stamping parts, and heat treated under the heat treatment process parameters of heating temperature 800-950°C and cooling speed 10°C / s-30°C / s (i.e. quenching speed). The tensile performance test was carried out according to GB / T228-2002 to obtain the yield strength, tensile strength and elongation A of the stamping parts. 50mm The microstructure of the stamped parts was observed using an optical microscope. The results are listed in Table 5.
[0102] Table 5.
[0103] As can be seen from Table 5, the embodiments of the present invention can obtain a fully martensitic microstructure at a quenching cooling rate of at least 10°C / s, while Comparative Examples 1 and 2 still cannot obtain a fully martensitic microstructure at quenching cooling rates of 10°C / s and 20°C / s, which makes the strength of Comparative Examples 1 and 2 lower than that of the embodiments of the present invention.
[0104] Figure 3 shows the microstructure of the stamped part after heat treatment obtained in Example 1. As can be seen from Figure 3, the stamped part is a fully martensitic structure.
[0105] It should be noted that the prior art within the scope of protection of the present invention is not limited to the embodiments given in this application document. All prior art that does not contradict the solutions of the present invention, including but not limited to prior patent documents, prior publications, prior public uses, etc., can be included in the scope of protection of the present invention.
[0106] In addition, the combination of the various technical features in this case is not limited to the combination described in the claims of this case or the combination described in the specific embodiments. All technical features recorded in this case can be freely combined or combined in any way unless there is a contradiction between them.
[0107] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made therefrom that can be directly derived from or easily conceived by those skilled in the art based on the disclosure of the present invention are intended to fall within the scope of protection of the present invention.
Claims
1. A cold-rolled steel sheet, characterized in that: The cold-rolled steel sheet contains Fe and inevitable impurities, and further contains the following chemical elements in the following mass percentages: C: 0.06~0.10wt%, Si: 0.01~0.5wt%, Mn: 1.6~2.5wt%, Al: 0.01~0.07wt%, Cr: 0.5~1.0wt%, Mo : 0.1~0.3wt%, Ti: 0.01~0.05wt%, Nb: 0.001~0.03wt%, B: 0.0001~0.005wt%, 0<N≤0.006wt%; The microstructure of the cold-rolled steel sheet is that spherical cementite particles are evenly distributed on a single-phase ferrite matrix, wherein the spheroidization rate of the spherical cementite is ≥90%.
2. The cold-rolled steel sheet according to claim 1, characterized in that: The mass percentage of each chemical element in the cold-rolled steel sheet is: C: 0.06~0.10wt%, Si: 0.01~0.5wt%, Mn: 1.6~2.5wt%, Al: 0.01~0.07wt%, Cr: 0.5~1.0wt%, Mo: 0.1~0.3wt%, Ti: 0.01~0.05wt%, Nb: 0.001~0.03wt%, B: 0.0001~0.005wt%, 0<N≤0.006wt%; the balance is Fe and unavoidable impurities.
3. The cold-rolled steel sheet according to claim 1 or 2, characterized in that: The grain size of ferrite is 7.0 to 11.
0.
4. The cold-rolled steel sheet according to claim 1 or 2, characterized in that: The spheroidization rate of spheroidized cementite in the cold-rolled steel sheet is ≥95%.
5. The cold-rolled steel sheet according to claim 1 or 2, characterized in that: The yield strength of the cold-rolled steel sheet is 280-420 MPa, the tensile strength is 450-600 MPa, and the elongation after fracture is A 50mm ≥25%.
6. The cold-rolled steel sheet according to claim 1 or 2, characterized in that: The microstructure of the cold-rolled steel sheet in the hot-rolled state is ferrite+pearlite+martensite.
7. The method for manufacturing a cold-rolled steel sheet according to any one of claims 1 to 6, characterized in that: The method for manufacturing the cold-rolled steel sheet comprises the following steps: Smelting and casting to obtain slabs; Hot rolling: heating, rolling and coiling; the coiling temperature is 500-620℃; Pickling and cold rolling; Hood annealing: annealing soaking temperature is 660-710℃, annealing soaking time is 5-30h; smooth.
8. The manufacturing method according to claim 7, characterized in that: In the hot rolling step, the slab heating temperature is controlled to be 1180-1280°C, and the final rolling temperature is controlled to be 870-940°C.
9. The manufacturing method according to claim 7, characterized in that: In the hot rolling step, the coiling temperature is controlled to be 550-600°C.
10. The manufacturing method according to claim 9, characterized in that: In the hot rolling step, the slab heating temperature is controlled to be 1200-1250°C, and the final rolling temperature is controlled to be 890-930°C.
11. The manufacturing method according to claim 7, characterized in that: In the cold rolling step, the cold rolling reduction ratio is controlled to be 20 to 60%.
12. The manufacturing method according to claim 7, characterized in that: In the cold rolling step, the cold rolling reduction ratio is controlled to be 30 to 50%.
13. The manufacturing method according to claim 7, characterized in that: In the leveling step, the leveling elongation is controlled to be ≤2.5%.
14. A stamping part for automobile, characterized in that: The automobile stamping parts are obtained by stamping the cold-rolled steel sheets as claimed in any one of claims 1 to 6.
15. The automobile stamping part according to claim 14, characterized in that: The automobile stamping parts are subjected to a heat treatment process at a heating temperature of 800 to 950° C. and a cooling rate of 10 to 30° C. / s to obtain a full martensitic structure; and / or The automotive stamping parts have a yield strength of 650-900 MPa, a tensile strength of 800-1100 MPa, and an elongation after fracture of 50mm ≥5.5%.
Citation Information
Patent Citations
High-strength steel sheet and its production method
CN101460644A
Cold-rolled steel sheet, manufacturing method thereof and blanking part for automobile
CN114058941A
Cold-rolled annealed steel sheet and manufacturing method
CN114829131A
Cold-rolled steel sheet, stamping part and manufacturing method of stamping part
CN117363972A
High tensile strength cold rolled steel sheet having excellent workability, production method thereof and working method thereof
JP2003321732A