Layer structure for a MEMS mirror device, method for producing the layer structure, and MEMS mirror device
The use of high-strength materials like silicon carbide in MEMS mirror devices addresses material stress limitations, enhancing deflection frequencies and optical resolution while maintaining compactness and reducing dynamic deformations.
Patent Information
- Application Number
- PCT/EP2024/056101
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-03
AI Technical Summary
MEMS mirror devices face challenges in achieving high optical resolution and compact design due to material stress limitations with silicon technology, particularly in terms of mirror diameter, deflection frequencies, and mechanical deflection angles, leading to issues like spring suspension breakage and excessive dynamic deformations.
A layer structure for MEMS mirror devices using materials like silicon carbide (SiC), tungsten carbide (WC), or aluminum oxide (Al2O3) with higher breaking points and elastic moduli than silicon, which are used for the spring sections and mirror support to enhance mechanical resilience and reduce material stress.
The proposed solution allows for higher deflection frequencies, reduced dynamic deformations, and improved mirror flatness, enabling better optical resolution and longer service life while maintaining a compact design, as demonstrated by comparisons with silicon-based MEMS structures.
Smart Images

Figure EP2024056101_03102024_PF_FP_ABST
Abstract
Description
[0001] Layer structure for a MEMS mirror device, method for producing the layer structure, and MEMS mirror device
[0002] Description
[0003] The present disclosure relates to a layer structure for a MEMS mirror device, a method for producing the layer structure, and a MEMS mirror device having the layer structure.
[0004] background
[0005] MEMS devices are microsystems that typically comprise electronics including multiple sensors and actuators arranged on a substrate and have very small dimensions in the range of a few millimeters to sometimes sub-millimeter range.
[0006] MEMS devices are also used in the field of deflection of electromagnetic radiation, for example laser beams, although here too the requirements for such systems are constantly increasing.
[0007] Especially for applications such as compact laser projection displays, which must be small and compact enough for integration into wearables, i.e., electronic systems worn on the body, such as augmented reality smartglasses, the developer of such laser beam deflection systems faces extreme challenges. Typically, a laser beam for display applications must be deflected both horizontally and vertically using a movably suspended mirror.
[0008] One important requirement for such MEMS mirror systems, for example, is size and compactness. Typically, mirror diameters between 1 mm and 4 mm are desired. However, the chip sizes should be as small as possible compared to the mirror diameter to allow for a sufficiently small projector design. Generally, the larger the mirror diameter, the smaller the imaged spot / pixel can be and the higher the optical resolution can be. At the same time, however, there is the problem that the increase in dynamic deformation of the mirror is associated with the fifth power of the mirror diameter, thus severely limiting a larger mirror design.
[0009] Another important parameter is the deflection frequencies at which the MEMS mirror device can operate. For example, to ensure the highest possible resolution on a display, scan frequencies must also be as fast as possible. Typical frequencies are between 15 kHz and 60 kHz. High deflection frequencies are achieved by keeping the moment of inertia as low as possible and by high spring stiffness, since these movements are typically achieved in resonance mode. As the deflection frequency increases, the material stress in the spring mounts also increases, placing increasing strain on the material.
[0010] However, not only the deflection frequencies of the mirror are a significant parameter, but also the mirror's deflection angle. To achieve high optical resolution and a large field of view, the largest possible mechanical deflections / amplitudes of the mirror movement are required. Typical mechanical deflection angles are between + / -5° and + / -20°. However, with increasing deflections, the dynamic deformation of the mirror plate and the material stress in the spring suspensions also increase.
[0011] In addition to the deflection frequencies and deflection angles, mirror flatness is another crucial parameter for the MEMS mirror device. To ensure that the deflected laser beam retains its original quality as much as possible, the mirror must be extremely rigid. This can be achieved by choosing a thicker mirror, but this comes at the expense of the deflection frequencies. If these are to be kept unchanged, the spring stiffness must be increased as required, which leads to significantly increased material stress for the same deflections.
[0012] There are many other constraints that must be considered in a MEMS mirror device, such as constraints resulting from the manufacturing process itself.
[0013] However, when considering these parameters and requirements together, the problem is that silicon technology reaches its limits when it comes to meeting these requirements. This applies to both the use of single-crystal and polycrystalline silicon (silicon Si; for example, so-called "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg (electronic grade)). The material is subjected to such high stresses under these requirements that the spring suspensions may break in order to meet the desired high mirror diameters, deflection frequencies, and amplitudes, as silicon can no longer withstand these stress conditions. However, the occurrence of excessive dynamic mirror deformations is also a problem that should be avoided.
[0014] In view of the disadvantages described above, it is an object of the present application to provide an improved layer structure and an improved method for its production, with which the above-mentioned disadvantages are avoided.
[0015] Summary
[0016] The present disclosure relates to a layer structure for a MEMS mirror device, a method for producing the layer structure, and a MEMS mirror device having the layer structure.
[0017] In particular, to achieve the above-mentioned object, a layer structure for a MEMS mirror device according to independent claim 1, a method for producing the layer structure according to independent claim 18, and a MEMS mirror device according to independent claim 24 are proposed. The dependent claims relate to some exemplary preferred embodiments.
[0018] According to a first aspect, a layer structure for a MEMS mirror device is proposed, comprising: a layer structure section which has a mechanically effective functional layer with spring sections and a mirror support section which is oscillatingly movable in at least one dimension and is resiliently held by the spring sections, and wherein the layer structure section has a first material which has a higher fracture strength and / or an at least equally high modulus of elasticity than monocrystalline or polycrystalline silicon, in particular Si sg (Silicon solar grade) or Si eg (Silicon electronical grade).
[0019] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the fracture limit of the first material is at least 60%, preferably at least 100%, particularly preferably at least 500% higher than the fracture limit of single-crystalline or polycrystalline silicon, in particular Si sg (Silicon solar grade) or Si eg (Silicon electronical grade), and / or the modulus of elasticity of the first material is at least equal to, preferably at least 100%, particularly preferably at least 200% or particularly preferably at least 300% higher than the modulus of elasticity of single-crystal or polycrystalline silicon, in particular Si sg (Silicon solar grade) or Si eg (Silicon electronic grade).
[0020] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the first material comprises at least one material of silicon carbide (SiC), in particular 4H-SiC or 6H-SiC, tungsten carbide (WC), titanium carbide (TiC), chromium carbide (Cr3C2, Cr7C3, Cr 23 C6) or aluminum oxide (Al2O3), in particular made of a material of silicon carbide (SiC), in particular 4H-SiC or 6H-SiC, tungsten carbide (WC), titanium carbide (TiC), chromium carbide (Cr3C2, Cr7C3, Cr 23 C6) or aluminum oxide (Al2O3).
[0021] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the first material, in particular the silicon carbide, has a doping.
[0022] In some preferred embodiments, the layer structure can be advantageously further developed such that the mechanically active functional layer comprises the first material.
[0023] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the layer structure section has an additional layer in addition to the mechanically active functional layer, wherein at least the mechanically active functional layer or at least the additional layer has the first material.
[0024] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the mechanically effective functional layer is mechanically connected in direct contact with the additional layer.
[0025] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the mechanically active functional layer comprises the first material and the additional layer comprises a second material with a lower breaking point and / or a modulus of elasticity that is at most the same as the first material of the mechanically active functional layer.
[0026] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the additional layer comprises the first material and the mechanically active functional layer comprises a second material with a lower breaking point and / or a modulus of elasticity that is at most the same as the first material of the additional layer.
[0027] In some preferred embodiments, the layer structure can be advantageously further developed in that an intermediate layer is provided between the mechanically active functional layer and the additional layer, in particular an electrically insulating intermediate layer, wherein the additional layer and the mechanically active functional layer comprise the first material, in particular consist of the first material.
[0028] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that at least parts of the additional layer for stiffening the mechanically active functional layer are provided in the region of the mirror support section and / or in the region of the spring sections of the mechanically active functional layer and are accordingly mechanically connected to the mechanically active functional layer.
[0029] In some preferred embodiments, the layer structure can be advantageously further developed in that a reinforcement section comprising the first material is provided within the mechanically active functional layer, wherein the mechanically active functional layer, which surrounds the reinforcement section in at least two spatial directions, comprises a second material with a lower breaking point and / or a maximum equal modulus of elasticity as the first material of the reinforcement section.
[0030] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the reinforcement section is provided in the region of the mirror support section and / or the spring sections of the mechanically active functional layer within the mechanically active functional layer for reinforcing the mirror support section and / or the spring sections.
[0031] In some preferred embodiments, the layer structure can advantageously be further developed by a bottom wafer which is mechanically connected in direct contact with the layer structure section.
[0032] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the layer structure section is formed as a single layer and has the mechanically active functional layer, wherein the mechanically active functional layer has the first material, in particular consists of the first material, and is mechanically connected in direct contact with the base wafer.
[0033] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the layer structure section, in addition to a structuring for the mechanically active functional layer, further comprises a structuring of a stiffening structure, in particular in the region of the mirror support section and / or in the region of the spring sections of the mechanically active functional layer, so that the structuring for the mechanically active functional layer and the structuring of the stiffening structure are formed monolithically in the individual layer of the layer structure section.
[0034] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the layer structure, in addition to the layer structure section, has an electrically active section with at least one actuator and / or sensor, in particular with at least one actuator and / or sensor layer.
[0035] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the at least one actuator and / or sensor, in particular the at least one actuator and / or sensor layer, is designed as a piezo actuator and / or piezo sensor or as a piezoelectric layer.
[0036] In some preferred embodiments, the layer structure can advantageously be further developed by a light-transmitting element, in particular a glass dome, which is mechanically connected to the mechanically active functional layer or to the electrically active section.
[0037] In some preferred embodiments, the layer structure can be advantageously further developed in such a way that an electrical separation is provided between the layer structure section and the base wafer.
[0038] In some preferred embodiments, the layer structure can be advantageously further developed by an electrically active section that is mechanically connected in direct contact with the layer structure section and is configured to cause the resiliently held mirror support section of the mechanically active functional layer to oscillate and / or to perform measurements on the mechanically active functional layer. In some preferred embodiments, the layer structure can be advantageously further developed in such a way that the electrically active section has an electrically conductive layer, in particular a metallic layer, that is formed on the mechanically active functional layer.
[0039] According to a second aspect, a method for producing a layer structure for a MEMS mirror device as described above is proposed, comprising: providing a base element for forming the layer structure section, and structuring the base element for forming the mechanically active functional layer of the layer structure section, wherein the mechanically active functional layer comprises the spring sections and the mirror support section, which is oscillatingly movable in at least one dimension and is resiliently held by the spring sections, wherein the base element comprises a first material which has a higher breaking point and / or an at least equally high modulus of elasticity than monocrystalline or polycrystalline silicon, in particular Si sg (Silicon solar grade) or Si eg (Silicon electronical grade).
[0040] In some preferred embodiments, the method can be advantageously further developed in that the layer structure section has an additional layer in addition to the mechanically active functional layer, wherein at least the mechanically active functional layer or at least the additional layer has the first material, and the mechanically active functional layer is mechanically connected to the additional layer.
[0041] In some preferred embodiments, the method can be advantageously further developed by structuring the additional layer such that the mirror support section and / or the spring sections of the mechanically active functional layer are substantially completely exposed from the side of the additional layer, wherein the mechanically active functional layer comprises the first material, in particular consists of the first material, or structuring the additional layer such that a part of the additional layer for stiffening the mechanically active functional layer remains in the region of the mirror support section and / or in the region of the spring sections of the mechanically active functional layer, wherein the additional layer and / or the mechanically active functional layer comprises the first material, in particular consists of the first material.
[0042] In some preferred embodiments, the method can be advantageously further developed in that the base element for forming the layer structure section is designed as a single layer, wherein the single layer of the base element comprises the first material, in particular consists of the first material.
[0043] In some preferred embodiments, the method can be advantageously further developed in such a way that, for the provision of the base element, a formation of the base element takes place, comprising: providing a base layer with an intermediate layer, applying a reinforcement layer to the intermediate layer, wherein the reinforcement layer comprises the first material, structuring the reinforcement layer to form the reinforcement section, wherein the reinforcement section partially covers a surface of the intermediate layer, and forming a functional layer on the intermediate layer and the formed reinforcement section, such that the reinforcement section is surrounded by the functional layer in at least two spatial directions, wherein the base layer with intermediate layer, the reinforcement section and the functional layer form the base element,and wherein, during structuring of the formed base element, the functional layer is formed into the mechanically effective functional layer.,
[0044] In some preferred embodiments, the method can be advantageously further developed in such a way that the reinforcement section is applied to the intermediate layer only in the region in which the mirror support section and / or the spring sections of the mechanically active functional layer are formed during the structuring of the functional layer to form the mechanically active functional layer.
[0045] In some preferred embodiments, the method can be advantageously further developed by structuring the base layer and the intermediate layer of the base element so that the mechanically active functional layer is substantially completely exposed from the side of the base layer.
[0046] In some preferred embodiments, the method can be advantageously further developed by providing an electrically active section which is mechanically connected in direct contact with the layer structure section and is configured to drive the mechanically active functional layer of the layer structure section and / or to carry out measurements on the mechanically active functional layer of the layer structure section, providing a light-transmissive element, and providing a base wafer, wherein the light-transmissive element, the electrically active section, the layer structure section and / or the base wafer are further configured to produce a vacuum encapsulation of the mirror support section and the spring sections of the mechanically active functional layer.
[0047] According to a third aspect, a MEMS mirror device is proposed, comprising a layer structure as described above.
[0048] Further aspects and their advantages as well as advantages and more specific embodiments of the aspects and features described above are described in the following, but in no way limiting, descriptions and explanations of the attached figures.
[0049] Short description of the characters
[0050] Fig. 1 shows an exemplary flowchart of a method for manufacturing a layer structure for a MEMS device according to a background example,
[0051] Figs. 2A-2C show exemplary sectional views of the layer structure during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 1,
[0052] Fig. 3 shows an exemplary flowchart of a method for manufacturing a layer structure for a MEMS device according to a first embodiment of the present disclosure,
[0053] Figs. 4A-4C show exemplary sectional views of the layer structure during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 3,
[0054] Fig. 5 shows an exemplary flowchart of a method for manufacturing a layer structure for a MEMS device according to a second embodiment of the present disclosure,
[0055] Figs. 6A-6C show exemplary sectional views of the layer structure during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 5,
[0056] Fig. 7 shows an exemplary flowchart of a method for manufacturing a layer structure for a MEMS device according to a third embodiment of the present disclosure, Figs. 8A-8C show exemplary sectional views of the layer structure during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 7,
[0057] Fig. 9 shows an exemplary flowchart of a method for manufacturing a layer structure for a MEMS device according to a fourth embodiment of the present disclosure,
[0058] Figs. 10A-10D show exemplary sectional views of the layer structure during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 9,
[0059] Fig. 11 shows an exemplary flowchart of a method for manufacturing a layer structure for a MEMS device according to a fifth embodiment of the present disclosure,
[0060] Figs. 12A-12C show exemplary sectional views of the layer structure during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 11,
[0061] Fig. 13 shows an exemplary 2D contour plot of the deflection amplitude of a MEMS structure for an exemplary comparison of the deflection frequencies / natural frequencies of the oscillating system when using silicon (Si, here polycrystalline silicon) and silicon carbide (SiC),
[0062] Fig. 14 shows an exemplary comparison of the dynamic deformation of the oscillating system of a MEMS device using a mirror plate 6a made of silicon (Si, here polycrystalline silicon) and a mirror plate made of silicon carbide (SiC),
[0063] Fig. 15 shows an exemplary comparison of the mechanical stresses (first principal stress) occurring in the region of the torsion spring clamps on the chip frame in relation to the exemplary fracture limit of the respective material of the oscillating system of the MEMS structure made of silicon (Si) and the MEMS structure made of silicon carbide (SiC). Detailed description of the figures and preferred embodiments
[0064] Examples and embodiments of the present disclosure are described in detail below with reference to the accompanying figures. Identical or similar elements in the figures may be designated by the same reference numerals, although sometimes different reference numerals may be used.
[0065] It should be emphasized, however, that the subject matter of the present disclosure is in no way limited or restricted to the exemplary embodiments and their embodiment features described below, but further comprises modifications of the exemplary embodiments, in particular those which are encompassed by modifications of the features of the described examples or by combination of one or more of the features of the described examples within the scope of protection of the independent claims.
[0066] First, a background example is described below with reference to Figs. 1 and 2A-2C, which is intended to facilitate the understanding of the embodiments and advantages described below.
[0067] Even if the following description with reference to Figs. 1 and 2A-2C refers to a background example, any described technical details and / or features of the method, the manufacturing sequence, the layer structure and in particular of individual steps and / or layers of the layer structure and / or of their possible materials may also relate to corresponding details and / or features of the embodiments described below, unless a difference is explicitly pointed out.
[0068] Fig. 1 shows an exemplary flowchart of a method for producing a layer structure for a MEMS device, in particular a MEMS mirror device, according to a background example, and Figs. 2A-2C show exemplary sectional views of the layer structure during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 1.
[0069] Referring to Fig. 1, in an exemplary step S101, a base element 10 is provided for forming a layer structure section 10a, wherein the base element 10 can be formed, for example, as an SOI wafer (silicon-on-insulator wafer) and comprises a base layer 1 (carrier wafer) and a functional layer 3. A corresponding exemplary base element 10 also forms the basis of the layer structure shown in Fig. 2A (i). In this case, for example, the base layer 1 and the functional layer 3 can have or consist of silicon (Si; for example, single-crystalline or polycrystalline silicon) as the material. In addition, the functional layer 3 can, for example, have a layer thickness of a few micrometers up to several hundred micrometers and / or can be formed, for example, to be electrically conductive (for example, by appropriate doping).
[0070] The base element 10 according to Fig. 2A (i) comprises, for example, an intermediate layer 2 (e.g., an electrically insulating passivation layer, for example, made of silicon dioxide), which is arranged, for example, between the base layer 1 and the functional layer 3, with the functional layer 3 being formed, for example, on the intermediate layer 2. The base layer 1, the intermediate layer 2, and the functional layer 3 together form, for example, the base element 10, which is designed as an SOI wafer.
[0071] In an exemplary step S102 of the method according to Fig. 1, a piezoelectric layer 4 is applied to the functional layer 3 of the base element 10. The layer structure according to Fig. 2A (i) thus comprises, according to steps S101 and S102, by way of example, a piezoelectric layer 4 formed on the functional layer 3 of the base element 10, wherein the piezoelectric layer 4 is applied, for example, in step S102 according to Fig. 1, on the base element 10 above the functional layer 3.In some cases, for example if the functional layer 3 is not electrically conductive (for example due to a lack of doping) and thus cannot serve as a bottom electrode for the piezoelectric layer 4, an electrically conductive, for example metallic, layer can first be applied to the functional layer 3 as a bottom electrode and only then can the piezoelectric layer 4 be applied to the additionally formed bottom electrode.
[0072] In a further exemplary step S103 of the method according to Fig. 1, the piezoelectric layer 4, which is applied on or above the functional layer 3 of the base element 10, is structured (for example, dry- or wet-chemically); see also Fig. 2A (ii).
[0073] In a further exemplary step S104 of the method according to Fig. 1, a dielectric layer 5 (for example made of silicon dioxide, aluminum oxide, or silicon nitride; the latter two materials can also be present as a mixture or as a two-layer stack to form the dielectric layer 5) is applied; see also Fig. 2A (iii). The dielectric layer 5 is applied, for example, to regions of the piezoelectric layer 4 according to Fig. 2A (iii) and is further applied, for example, to regions of the functional layer 3 that are open after structuring the piezoelectric layer 4.
[0074] In some embodiments, the applied dielectric layer 5 can be opened / structured in selected regions. According to Fig. 2A (iv), for example, in region 5b, the dielectric layer 5 is opened or structured toward the functional layer 3, in particular before applying an electrode layer (see below), in order to provide, for example, a region 5b intended for a later bonding pad for the bottom electrode or as an electrical contact to the functional layer 3.
[0075] In addition or alternatively, regions of the applied dielectric layer 5 can also be opened or structured, for example above the applied and / or structured piezoelectric layer 4 (not shown here), in order, for example, to directly contact the electrode layer 6 to be applied later (see, for example, the following steps S105 and S106) with the piezoelectric layer 4.
[0076] In a further exemplary step S105 of the method, an electrode layer 6 is applied to the dielectric layer 5, which may optionally have been previously opened in regions (e.g., opened region 5b for a later bond pad and / or regions above the piezoelectric layer 4); see also Fig. 2B (v). During the application of the electrode layer 6, the region 5b previously opened in the dielectric layer 5 is also filled with the material of the electrode layer 6, for example, to form a bond pad. Aluminum, AlCu, gold, tungsten, molybdenum, or another electrically conductive material can be used, for example, as the material for the electrode layer 6.
[0077] In a further exemplary step S106 of the method according to Fig. 1, the electrode layer 6, which is applied on or above the dielectric layer 5, is structured; see also Fig. 2B (vi). For example, in the region 5b that was opened in the dielectric layer 5, a bonding pad 6b is formed with the material of the electrode layer 6, which provides electrical contact to the top side of the functional layer 3 of the base element 10 (and / or to the exemplary bottom electrode, which can be electrically connected to the underside of the structured regions of the piezoelectric layer 4). In the exemplary step S106 of structuring the electrode layer 6, the desired structure of the upper electrode (top electrode) for the upper electrical contacting of the piezoelectric layer 4 is formed.Furthermore, in step S106 of structuring the electrode layer 6, a mirror 6a (mirror layer 6a with a reflective surface) can be formed in the center of the layer structure according to Fig. 2B (vi), using the material of the electrode layer 6. It should be noted that, for example, pads and also the mirror plate / mirror 6a can be formed in a step (process) independent of step S106, for example, by an additional lithography process followed by etching or a process using shadow masks.
[0078] In such examples, for example, the electrode layer may comprise metal, in particular aluminum, so that the surface of the electrode layer 6 already has a reflective surface and is suitable for forming the mirror 6a. In further examples, it is possible to provide a non-reflective or non-metallic electrode layer (e.g., doped polycrystalline silicon), in which case a further, for example, metallic mirror layer (e.g., as a thin metal film) can then be applied in the region of the layer 6a. For example, molybdenum, which is electrically conductive and thus fundamentally suitable as an electrode layer 6, has poor reflection properties and is also not bondable, so that molybdenum is suitable neither as a material for the mirror plate / mirror 6a nor as a material for bond pads.
[0079] In a further exemplary step S107 of the method according to Fig. 1, the dielectric layer 5 is opened in regions 5a toward the functional layer 3, see also Fig. 2B (vii). These are, in particular, regions 5a of the dielectric layer 5 to be opened, in which the underlying functional layer 3 is structured to form the mechanically active structures / mechanically active functional layer 3 of the MEMS device, in particular the MEMS mirror device.
[0080] In relation to a MEMS, "mechanically effective" is to be understood in particular to mean that the mechanically effective layer or the at least one mechanically effective functional layer (device layer) of the MEMS layer structure preferably forms the layer which, according to its structuring, is designed or configured to execute an oscillatory movement, in particular a one-dimensional or two-dimensional oscillatory movement, or in such a way that one or more structures or bodies formed in the mechanically effective layer or mechanically effective functional layer can execute an oscillatory movement, in particular a one-dimensional or two-dimensional oscillatory movement (e.g., about an oscillation / torsion axis or about two oscillation / torsion axes which are preferably transverse or, in particular, perpendicular to one another, in particular, for example, for Lissajous scanning movements).
[0081] For this purpose, the holding and / or spring structure for the movable structures or bodies of the mechanically active layer or mechanically active functional layer can preferably also be formed in this mechanically active layer or mechanically active functional layer. In some embodiments, the spring structure can comprise spring / spring sections, particularly preferably bending and / or torsion springs, which are preferably designed to hold the mirror support element / mirror support section in such a way that the mirror support element can execute an oscillating rotational movement about the respective oscillation and / or torsion axis around the corresponding axis (e.g., torsional oscillations).
[0082] Furthermore, the formation of the mechanically active layer 3 or mechanically active functional layer 3 can preferably determine the resonance frequency or resonance frequencies of the MEMS and / or the deflection amplitudes / deflection angles.
[0083] With the opening of the dielectric layer 5 in the regions 5a toward the functional layer 3 according to step S107 of the method according to Fig. 1, as also shown in Fig. 2B (vii), an exemplary electrically active section 20 can be formed on the base element 10, which can, for example, comprise the piezoelectric layer 4, the dielectric layer 5, the electrode layer 6, as well as the mirror layer 6a and the bond pad 6b. Furthermore, if the mechanically active functional layer 3 is electrically non-conductive (for example, due to a lack of doping), the exemplary electrically active section 20 can further comprise an electrically conductive, for example, metallic layer, which is formed on the base element 10 (for example, on the functional layer 3), wherein the piezoelectric layer 4 is then further formed on the electrically conductive layer.The electrically active section 20 can be mechanically connected in direct contact with the functional layer 3 of the base element 10.
[0084] In a further exemplary step S108 of the method according to Fig. 1, the functional layer 3 is structured in regions 3a, see also Fig. 2B (viii). In particular, the mechanically active structures of the MEMS device or MEMS mirror device are formed in the functional layer 3 (mechanically active functional layer 3). This includes, for example, the formation or exposure of a mirror support element / mirror support section 3b (here, for example, the region of the functional layer 3 below the mirror layer 6a), which is formed, for example, from central regions of the functional layer 3, as well as any retaining webs formed from the functional layer 3, wherein the retaining webs act, for example, as spring structures / spring sections 3c (not shown here, see Fig. 13) and can hold the mirror support element 3b so that it can swing / resiliently move about one, two, or more oscillation or torsion axes.
[0085] For example, during the structuring of the functional layer 3 in step S108, the so-called high-rate etching or deep reactive ion etching (DRIE for short) can be used to form the deep trenches in the functional layer 3 (e.g. regions 3a in Fig. 2B (viii)).
[0086] In a further exemplary step S109 of the method according to Fig. 1, the base element 10 is opened at the rear to expose the functional layer 3 on the side opposite the piezoelectric layer 4; see also Fig. 2C (ix), in which, for example, the base layer 1 is opened at the rear toward the intermediate layer 2, and Fig. 2C (x), in which, for example, the intermediate layer 2 is opened at the rear toward the functional layer 3.
[0087] The layer structure 100 produced in this way, by way of example, comprises the layer structure section 10a with the electrically active section 20 provided or formed thereon. The electrically active section 20 is mechanically connected, by way of example, in direct contact with the layer structure section 10a, as shown in Fig. 2C (x), wherein the electrically active section 20 can further be configured to, for example, cause the resiliently held mirror support section 3b of the mechanically active functional layer 3 to vibrate and / or to perform measurements (for example, accelerations, strains of the material, etc.) on the mechanically active functional layer 3.
[0088] In a further exemplary step S110 of the method according to Fig. 1, the manufactured layer structure 100 is provided, by way of example, in a vacuum-packed MEMS device or MEMS mirror device 1100 according to Fig. 2C (xi). Here, the layer structure 100 was hermetically sealed from above with a light-transmissive element 40 (e.g., a glass dome) and from below with a base wafer 30 (e.g., with an integrated getter 31, which may comprise, for example, titanium or titanium-containing alloys) under a vacuum atmosphere. For example, glass frits can be used to join the light-transmissive element 40 and the base wafer 30 (as part of the layer structure 100) to the layer structure 100.
[0089] Thus, a vacuum-packed MEMS mirror device 1100 (e.g., a MEMS mirror scanner) comprising the fabricated layer structure 100 can be provided with piezoelectrically deflectable or controllable mirrors 6a, see, for example, Fig. 2C (xi).
[0090] The background example described here is intended to once again represent a typical manufacturing process of a layer structure 100, which is essentially produced from an SOI wafer as the base element 10 and has a silicon layer (for example made of monocrystalline silicon) as the handling wafer / handling layer and a silicon layer (for example made of polycrystalline silicon) for the later mechanically active functional layer 3.
[0091] Various exemplary embodiments are described below. Any details or exemplary features from the above examples, in particular regarding individual process steps and materials, may also apply analogously to the exemplary embodiments below, unless differences are explicitly pointed out. Furthermore, descriptions of details or exemplary features from the following exemplary embodiments, in particular regarding individual process steps and materials, may also apply analogously to other exemplary embodiments, unless differences are explicitly pointed out.
[0092] In contrast to the above background example, embodiments preferably provide for the use of a material that is more mechanically resilient than crystalline or polycrystalline silicon (Si; for example, so-called "solar silicon" Si sg (solar grade) or "semiconductor silicon" Sieg (electronical grade)), whereby of particular interest are the regions of the MEMS device that are exposed to high mechanical stress or high mechanical material tension, such as the mechanically active functional layer 3 and in particular the mirror support section 3b and the spring sections 3c (see, for example, Fig. 13). Alternatively or additionally, these materials can also support the mechanically active functional layer 3 made of this silicon (Si), particularly in the regions with high material stress, for example due to the high deflection frequencies and / or high deflection angles of the mechanically movable part (for example, the mirror support section 3b and / or the spring sections 3c) of the mechanically active functional layer 3.
[0093] The reason for replacing the material in the mechanically highly stressed areas is, as already described, that with regard to the requirements mentioned above, monocrystalline or polycrystalline silicon (Si) is reaching its material or mechanical limits. The mechanical properties of polycrystalline silicon (Si, such as "solar silicon" Si) can be sg (solar grade)), for example, the Young's modulus is around 160 GPa and the tensile strength is around 1.5 GPa. For single-crystal silicon (Si, such as "semiconductor silicon" Si eg(electronical grade)), the mechanical properties mentioned can also depend on the crystal orientation of the silicon. For example, for the principal crystal orientation (100) of silicon, the Young's modulus can be approximately 130 GPa, for the principal crystal orientation (110) of silicon, the Young's modulus can be approximately 169 GPa, and for the principal crystal orientation (111) of silicon, the Young's modulus can be approximately 188 GPa.
[0094] For the sake of completeness, it should be noted at this point that the values of Young's modulus and / or fracture strength listed here can be noticeably higher for a "perfect", ideal single-crystal Si. However, such values are not to be expected for technical applications of silicon, since, for example, even single-crystal silicon (with the highest purity) is doped with very small amounts of impurity atoms and / or contains defects in the crystal lattice (for example, due to mechanical processing of the silicon to prepare it for the respective technical application, etc.).
[0095] In addition, these described values, as well as the following values for the other materials, are generally average values and may, of course, deviate slightly from them in individual cases. In particular, the values of Young's modulus and fracture strength under tensile / compressive load of the individual materials given here should not be viewed as absolute values of the respective material, but rather as a classification of the materials with regard to strength and resistance to mechanical stress in comparison to the already described single-crystalline or polycrystalline silicon (Si; such as "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg (electronical grade)).
[0096] However, the limit values specified or known for silicon are no longer sufficient to meet the ever-increasing demands placed on MEMS devices or MEMS mirror devices, so that an alternative material to silicon should be used in order to still be able to meet the requirements.
[0097] An advantageous alternative to single-crystal or polycrystalline silicon (Si) can be silicon carbide (SiC). This material can exist in various phases, with the single-crystal 4H and 6H phases being particularly advantageous for demanding technical applications. For example, the Young's modulus of the 4H phase of SiC can range from approximately 380 to 430 GPa, and the 6H phase of SiC can have a Young's modulus of up to approximately 700 GPa. In terms of tensile strength, this material can, for example, have a fracture strength of approximately 10 GPa or more.
[0098] The higher strength values of silicon carbide (SiC) can advantageously enable a MEMS structure that was previously made of the aforementioned silicon (Si) to now be able to perform significantly higher deflection angles and significantly higher deflection frequencies / oscillation frequencies, which can lead to fewer flicker artifacts and higher frame rates without experiencing mechanical damage.
[0099] In addition, the higher strength values allow the MEMS structure to be made smaller or more delicate, while simultaneously enabling larger mirror diameters. This reduces both static (e.g., due to its own weight) and dynamic (due to high movement speeds) deformation, thus achieving significantly better mirror flatness. The use of silicon carbide (SiC) can significantly increase the design freedom of a MEMS structure and exceed the previously known limitations due to the comparatively low strength values of silicon (Si).
[0100] Another great advantage of silicon carbide (SiC) is that it has a comparatively low density of approximately 3.21 g / cm 3 and thus approximately in the range of single-crystalline or polycrystalline silicon with approx. 2.34 g / cm 3This may increase the moment of inertia of moving parts of the MEMS structure slightly compared to silicon, but the structure as a whole is still significantly more mechanically resilient.
[0101] In addition, silicon carbide can be made electrically conductive using a dopant without significantly affecting the mechanical properties of the silicon carbide.
[0102] With regard to structuring silicon carbide (SiC) with a typical plasma etching process, the structuring speeds (etch rates) can be significantly higher compared to silicon (Si; such as "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg(electronical grade)) may be significantly lower (for example, the etching rates in a plasma etching process of silicon carbide can be only around 800 nm per minute), but this can be at least partially counteracted, for example, by a laser-assisted wet-chemical etching process.
[0103] Although this does not quite achieve the etching rates achieved with silicon, since it is a wet-chemical etching process that can be carried out in a tank, multiple wafers can be processed simultaneously / in parallel (batch processing). Furthermore, this process eliminates the need for a complex hard mask, which would otherwise be very thick and partly made of silicon dioxide or using nickel, for example. This eliminates manufacturing steps or preparatory steps, which further compensates for the longer structuring times.
[0104] In addition, the laser-assisted wet-chemical etching process offers another advantage in the improved structuring of the mechanically effective functional layer, since, for example, the surfaces of the processed substrates can be healed and smoothed by the wet-chemical step following exposure, which in turn can benefit increased fracture strength.
[0105] In addition to silicon carbide (SiC) as an alternative to the aforementioned silicon (Si), other materials can also be used. For example, tungsten carbide (WC), which can exhibit a Young's modulus of up to 650 GPa and a tensile strength of up to 3.5 GPa. Tungsten carbide also has the advantageous property of being inherently electrically conductive, so that, for example, a mechanically active functional layer made of this material can simultaneously be used as an electrically conductive layer, for example, for electrically contacting the piezoelectric layer provided on the mechanically active functional layer.
[0106] In addition to the materials silicon carbide (SiC) and tungsten carbide (WC), both of which could potentially be used for electrically conductive layers, aluminum oxide (Al2O3), for example, can also be used advantageously as an electrically insulating material as an alternative to silicon (Si; for example, "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg (electronic grade)) for use in MEMS devices. Al2O3 has a Young's modulus of approximately 350 to 400 GPa and a fracture strength at compressive strength of approximately 2.5 to 4 GPa, depending on the purity of the aluminum oxide present. The Young's modulus and fracture strength increase with increasing material purity (e.g., Young's modulus of 350 GPa and fracture strength of 2.5 GPa at a purity of approximately 96%, and Young's modulus of 400 GPa and fracture strength of 4 GPa at a purity of approximately 99.8%).
[0107] It should be noted here that, in addition to the materials already mentioned, there are also other advantageous alternatives to silicon (Si). For example, titanium carbide (TiC), chromium carbide (e.g., Cr3C2), or even diamond (C) or diamond-like carbon (DLC) could also be used in MEMS devices, especially MEMS mirror devices.
[0108] The materials referred to below as "first material" include all materials that have a higher fracture strength and / or at least an equal, but usually higher, elastic modulus than monocrystalline or polycrystalline silicon (Si; such as "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg(electronical grade)), but in particular the materials already mentioned and described, such as silicon carbide (SiC), tungsten carbide (WC), aluminum oxide (Al2O3), titanium carbide (TiC) and chromium carbide (e.g. Cr3C2).
[0109] Fig. 3 shows an exemplary flowchart of a method for producing a layer structure 200 for a MEMS device 1200, in particular a MEMS mirror device 1200, according to a first embodiment, and Figs. 4A-4C show exemplary sectional views of the layer structure 200 during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 3.
[0110] In this first embodiment, in contrast to the exemplary background example according to Figs. 1 and 2A-2C, a base element 10 for forming the layer structure section 10a can first be provided (step S201 in Fig. 3), which, for example, has a base layer 1 (additional layer 1) with a layer 3 (here the functional layer 3) subsequently applied thereon (see Fig. 4A (i)). The base layer 1 can, for example, comprise the already described silicon (Si; second material; for example, "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg(electronical grade)) or consist of this, while the layer 3 subsequently applied to the base layer 1, for example, has the first material (for example silicon carbide (SiC), in particular doped silicon carbide (SiC)) or consists of this and thus, for example, has a higher breaking point and / or at least an equally high, preferably a higher, modulus of elasticity (E-modulus) than the silicon (Si) of the base layer 1.
[0111] An advantage of using the first material can already be seen here, since the intermediate layer 2 or the passivation layer 2 could be omitted, which already leads to simpler production of the base element 10, from which the layered construction section 10a is later formed. Furthermore, by omitting the intermediate layer 2, which can be formed, for example, as an oxide layer, the introduction of stress / material strains into the base element 10 is advantageously avoided.
[0112] For the formation / production of the base element 10 with the layers, each of which comprises different materials with different expansion coefficients, a deposition process (e.g. epitaxial deposition, sputtering, PLD, etc.) or a laser-assisted bonding process with only very limited, local heat input may be advantageous, since in this way, for example, possible effects of the different expansion coefficients of the different materials can be avoided.
[0113] The steps S202 to S208 in the manufacturing method of the layer structure 200 according to Fig. 3 are initially the same as the steps S102 to S108 of the background example according to Fig. 1.
[0114] Thus, a piezoelectric layer 4 can first be applied to the functional layer 3 of the base element 10 (step S202), as also shown in Fig. 4A (ii), and this layer can then be structured (step S203; see Fig. 4A (iii)). This can be followed by the application of a dielectric layer 5 on the structured piezoelectric layer 4 and the exposure of a region 5b or several regions (for example, above the structured piezoelectric layer 4) of the dielectric layer 5 for the subsequent bond pad or a subsequent contacting of the piezoelectric layer 4 (step S204; see Fig. 4A (iv) and Fig. 4B (v)).
[0115] An advantage of the combination of mechanically active functional layer 3 and the piezoelectric layer 4 applied directly thereon is that the piezoelectric layer 4, if provided, for example, in the region of the spring sections 3c (not shown here, see Fig. 13), contributes to additional stiffening of the spring sections 3c and can thus additionally advantageously influence the natural frequency of the oscillating system. Furthermore, the thermal expansion coefficients of, for example, silicon carbide (SiC) as the mechanically active functional layer 3 and the piezoelectric layer 4 (for example, AlN) can be closer to each other than for polycrystalline or monocrystalline silicon (Si), so that less stress is introduced into the mechanically active functional layer 3 in the event of temperature differences.
[0116] The use of a piezoelectric layer 4 on the mechanically active functional layer 3, especially if it comprises, for example, SiC or one of the other materials (such as tungsten carbide or aluminum oxide, etc.), also enables a very efficient coupling of the energy for driving the MEMS device into the mechanically active functional layer 3, so that the mechanical stress / tension can be generated very locally. This allows the structures of the mechanically active functional layer 3, in particular the structures of the spring sections 3c, to be very thin and yet still be driven via the directly adjacent piezoelectric layer 4.
[0117] The piezo material required for the piezoelectric layer 4 can advantageously be produced very precisely and locally on the functional layer 3 using semiconductor technology. Unlike other drive technologies (such as electrostatic or electromagnetic drives), it does not require any modifications to the functional layer 3 or complex additional structures. This allows a high degree of freedom in the design of the actual mechanical structures (e.g., the spring sections 3c and / or the mirror support section 3b) and, among other things, enables a very compact design of the geometric structures.
[0118] It should be noted that the advantages mentioned here of the combination of the mechanically active functional layer 3 and the piezoelectric layer 4 applied thereon also apply to the other layer structures 300 - 600, even if the functional layer 3, for example, initially comprises the second material, but a stiffening structure, for example by the base layer 1, is provided.
[0119] Furthermore, it should be noted that the following also applies to layer structures 200-600: if, for example, the functional layer 3 is not electrically conductive (for example, due to a lack of doping) and thus cannot serve as a bottom electrode for the piezoelectric layer 4, an electrically conductive layer, for example a metallic layer, can first be applied to the functional layer 3 as a bottom electrode, and only subsequently can the piezoelectric layer 4 be applied to the additionally formed bottom electrode. An electrode layer 6 can then be applied to the dielectric layer 5 (step S205; see Fig. 4B (vi)) and structured accordingly (step S206; see Fig. 4B (vii)) for the exemplary formation of the bond pad 6b, the mirror layer 6a, conductor tracks, and top electrode, for example for the piezoelectric layer 4.Thereafter, the dielectric layer 5 can be opened in certain regions 5a (step S207; see Fig. 4B (viii)) and the functional layer 3 can be structured (step S208; see Fig. 4C (ix)) to form the mirror support section 3b and the spring sections 3c (not shown here, see Fig. 13) of the mechanically active functional layer 3 (for example by the laser-assisted wet-chemical etching process already described).
[0120] Now, for example, the opening of the layer structure 200 to expose the mechanically active functional layer 3 can be carried out by structuring / opening the base layer 1, for example by plasma-assisted etching such as deep reactive ion etching (DRIE for short) (step S209; see Fig. 4C (x)), which further forms the layer structure section 10a. Advantageously, the mechanically active functional layer 3 can now be exposed with just one etching process, since the intermediate layer 2 or the passivation layer 2 is missing and no longer needs to be removed at the corresponding locations.
[0121] On the other hand, the intermediate layer 2 can be dispensed with as an "etch stop layer" for the etching process, since the different materials (for example silicon and silicon carbide) of the base element 10 significantly change the speed of the etching process at the boundary between silicon and silicon carbide due to the selectivity in the etching process (in particular, silicon carbide is etched significantly more slowly than the described silicon), whereby the etching process is very well controllable and can be terminated accordingly, for example if etching has taken place through the silicon layer onto the silicon carbide layer.
[0122] Nevertheless, it should be noted that between the base layer 1 (additional layer 1) and the functional layer 3, for example, an intermediate layer 2 / passivation layer 2, as shown in the background example according to Figs. 2A to 2C, can be provided, so that the etching process initially on this passivation layer 2 (in particular if formed as an oxide layer) slows down so much that it virtually stops.
[0123] Subsequently, the translucent element 40 (for example the
[0124] glass dome or a flat element) and / or the bottom wafer 30 (for example with integrated getter 31) are joined (mechanically connected) to the layer structure section 10a and / or the electrically active section 20 of the layer structure 200 in order to provide the MEMS device 1200, in particular the MEMS mirror device 1200 (step S210; see Fig. 4C (xi)).Since the light-transmitting element 40 and the base wafer 30 are configured to pack the layer structure 200 in a vacuum-tight manner, the entire MEMS device 1200 can thereby be vacuum-packed, for example (for example with an internal pressure of less than 1 mbar, substantially less than 0.1 mbar, and in particular less than 0.01 mbar), so that the moving parts such as the mirror support section 3b including the mirror 6a and the spring sections 3c can oscillate substantially without resistance or damping (for example due to air / gases present in the MEMS), which, among other things, leads to more energy-efficient operation of the MEMS device 200, in particular the MEMS mirror device 200.
[0125] For joining the light-transmissive element 40 and the base wafer 30 to the layered structure section 10a and / or the electrically active section 20 of the layered structure 200, a low-temperature process can be advantageously used. For example, eutectic or transient liquid-phase wafer bonding can be used, which uses, for example, a joining material based on indium (In) (e.g., Auln or Culn). In such processes, joining can be carried out at a temperature of, for example, 160 to 200°C.
[0126] Alternatively, for joining the translucent element 40 and the base wafer 30 to the layer structure section 10a and / or the electrically active section 20 of the layer structure 200, a joining process can also be carried out at temperatures in the range of approximately 350 - 450°C, wherein the expansion behavior of the material pairs (for example silicon Si and silicon carbide SiC of the layer structure 200 or the layer structure section 10a) can advantageously be actively influenced and thus coordinated with one another in order to avoid, for example, unnecessary material stresses or even material damage due to the initially different expansion coefficients and the high heat input through the joining process.
[0127] Due to the mechanically effective functional layer 3 now made from the first material (for example silicon carbide (SiC)), in comparison to a mechanically effective functional layer 3 made from silicon (Si; such as "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg (electronic grade) significantly higher amplitudes and frequencies (thus fewer flicker artifacts and higher frame rates) of the mirror 6a of the MEMS mirror device 1200 can be achieved, while simultaneously improving the mirror flatness. Overall, this significantly improves the optical resolution and the illumination of the image surface of the image projected by the MEMS mirror device 1200, as well as the service life of the MEMS mirror device 1200.
[0128] It should be noted at this point that in addition to silicon carbide (SiC), other materials of the first material can also be used and can achieve such improvements compared to the silicon (Si) already described.
[0129] Fig. 5 shows an exemplary flowchart of a method for producing a layer structure 300 for a MEMS device 1300, in particular a MEMS mirror device 1300, according to a second exemplary embodiment, and Figs. 6A-6C show exemplary sectional views of the layer structure 300 during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 5.
[0130] In this second exemplary embodiment, in contrast to the exemplary background example according to Figs. 1 and 2A to 2C, a base element 10 for forming the layer structure section 10a can first be provided (step S301 in Fig. 5), which, for example, has the base layer 1 (additional layer 1) with the functional layer 3 subsequently applied thereto (see Fig. 6A (i)). In comparison to the first exemplary embodiment according to Fig. 3 or Figs. 4A to 4C, the base layer 1 can now comprise the first material or the base layer 1 can consist of the first material. The functional layer 3, on the other hand, can comprise a different material (second material) that has a lower fracture strength and / or at most an equal, but generally lower, modulus of elasticity than the first material of the base layer 1. Therefore, the functional layer 3 can, for example, comprise silicon (Si; such as, for example, "solar silicon"). sg (solar grade) or "semiconductor silicon" Sieg (electronical grade)), which may also be doped.
[0131] Here too, as already described under the first embodiment according to Fig. 3, 4A to 4B, for example, the intermediate layer 2 or the passivation layer 2 can be omitted for the reasons already mentioned.
[0132] The steps S302 to S308 in the manufacturing method of the layer structure 300 according to Fig. 5 are also the same as the steps S102 to S108 of the background example according to Fig. 1.
[0133] Thus, here too, a piezoelectric layer 4 can first be applied to the functional layer 3 (step S302), as is also shown in Fig. 6A (ii), and this can then be structured (step S303; see Fig. 6A (iii)). The application
[0134] REVISED SHEET (RULE 91) ISA / EP of a dielectric layer 5 on the structured piezoelectric layer 4 and the exposure / opening of one or more regions (for example the region 5b and / or regions above the piezoelectric layer 4) of the dielectric layer 5 for the later bonding pad or the contacting of the piezoelectric layer 4 (step S304; see Fig. 6A (iv) and Fig. 6B (v)).
[0135] An electrode layer 6 can now be applied to the dielectric layer 5 (step S305; see Fig. 6B (vi)) and structured accordingly (step S306; see Fig. 6B (vii)), for example to form the bond pad 6b, the mirror layer 6a, conductor tracks and top electrode, for example for the piezoelectric layer 4. Thereafter, the opening of the dielectric layer 5 can take place in certain regions 5a (step S307; see Fig. 6B (viii)) and the structuring of the functional layer 3 (step S308; see Fig. 6C (ix)) to form the mechanically active functional layer 3.
[0136] A significant difference from the first embodiment is, for example, that instead of completely opening the layer structure (as shown and described in the layer structure 200 of the first embodiment) to expose the mechanically effective functional layer 3 by appropriately structuring the base layer 1, only a partial opening of the layer structure, in particular the base layer 1 (additional layer 1), can take place (step S309; see Fig. 6C (x)).
[0137] As a result, in particular, parts of the base layer 1 (additional layer 1), which comprises or consists of the first material, can remain as a stiffening structure in the region of the mirror support section 3b and / or in the region of the spring sections 3c (not shown here, see Fig. 11) of the mechanically active functional layer 3. This can advantageously make it possible to reduce or avoid static and / or dynamic deformations of the mirror support section 3b and thus of the mirror 6a, even under high dynamic loads on the mirror 6a.
[0138] Furthermore, in particular by stiffening the spring sections 3c, an influence / tuning of the natural frequencies of the oscillating part of the MEMS device 1300 can be achieved, which can be extremely advantageous, for example, in multi-axis oscillating MEMS mirror devices 1300 that are used as resonators (for example as Lissajous scanners).
[0139] It should be noted at this point that a stiffening structure in the first exemplary embodiment (see layer structure 200 or MEMS device 1200), in which the base layer 1 comprises the second material (for example, silicon (Si)) and the mechanically active functional layer 3 comprises the first material (for example, silicon carbide (SiC)), is also possible due to only partial removal of the base layer 1. This also makes it possible to achieve the advantageous effects of stiffening, for example, the mirror support section 3b and / or the spring sections 3c.
[0140] In addition, the mechanically effective functional layer 3 can advantageously be exposed here with only one etching process (for example, the laser-assisted wet-chemical etching process here too), since the intermediate layer 2 or the passivation layer 2 is missing and this no longer has to be removed in a separate step.
[0141] After the mechanically active functional layer 3 has been exposed, whereby the layer structure section 10a has also been formed, the light-transmissive element 40 (for example the glass dome) and the base wafer 30 (for example with integrated getter 31) can also be joined (mechanically connected) to the layer structure section 10a and / or the electrically active section 20 of the layer structure 300, for example by means of the low-temperature process already described, in order to provide a MEMS device 1300, in particular a MEMS mirror device 1300 (step S310; see Fig. 6C (xi)). Since the light-transmissive element 40 and the base wafer 30 are also configured here to pack the layer structure 300 in a vacuum-tight manner, this MEMS device 1300 can also be vacuum-packed, for example, so that the movable parts such as the mirror support section 3b orMirror 6a and the spring sections 3c can oscillate essentially without resistance and damping.
[0142] Due to the stiffening structures comprising the first material (for example silicon carbide (SiC)) for stiffening the mechanically effective functional layer 3, in comparison to a mechanically effective functional layer 3 made of single-crystalline or polycrystalline silicon (Si; for example "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg (electronical grade)) higher amplitudes and frequencies (thus fewer flicker artifacts and higher frame rates) of the mirror 6a of the MEMS mirror device 1300 can be achieved with simultaneously better mirror flatness.
[0143] The use of a stiffening structure can also improve the overall optical resolution and illumination of the image surface of the image projected by the MEMS mirror device 1300. Fig. 7 shows an exemplary flowchart of a method for producing a layer structure 400 for a MEMS device 1400, in particular a MEMS mirror device 1400, according to a third exemplary embodiment, and Figs. 8A-8C show exemplary sectional views of the layer structure 400 during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 7.
[0144] In this third exemplary embodiment, in contrast to the exemplary background example according to Figs. 1 and 2A to 2C, a base element 10 for forming the layer structure section 10a can first be provided (step S401 in Fig. 7), which, for example, has the base layer 1 (additional layer 1) with the functional layer 3 subsequently applied thereto and an intermediate layer 2 provided between the base layer 1 and the functional layer 3 (see Fig. 8A (i)). In comparison to the first exemplary embodiment according to Fig. 3 or Figs. 4A to 4C and to the second exemplary embodiment according to Figs. 5 or Figs. 6A to 6C, the base layer 1 and the functional layer 3 can now comprise the first material, or the base layer 1 and the functional layer 3 can consist of the first material. Therefore, it can be advantageous to provide the intermediate layer 2, which can also be electrically insulating, between these two layers.
[0145] It should be noted at this point that the intermediate layer 2 can also be provided between a functional layer 3, which comprises or consists of the first material, and a base layer 1, which comprises or consists of the second material, in order, for example, to enable electrical insulation of the two layers. Conversely, if the functional layer 3 comprises or consists of the second material and the base layer 1 comprises or consists of the first material, the intermediate layer 2 can of course also be provided accordingly between these two layers.
[0146] The steps S402 to S408 in the manufacturing method of the layer structure 400 according to Fig. 7 are also the same as the steps S102 to S108 of the background example according to Fig. 1.
[0147] Thus, here too, a piezoelectric layer 4 can first be applied to the functional layer 3 (step S402), as also shown in Fig. 8A (ii), and this can then be structured (step S403; see Fig. 8A (iii)). This can be followed by the application of a dielectric layer 5 on the structured piezoelectric layer 4 and the exposure / opening of one or more regions (for example, region 5b and / or regions above the piezoelectric layer 4) of the dielectric layer 5 for the subsequent bond pad or the contacting of the piezoelectric layer 4 (step S404; see
[0148] Fig. 8A (iv) and Fig. 8B (v)).
[0149] An electrode layer 6 can now be applied to the dielectric layer 5 (step S405; see Fig. 8B (vi)) and structured accordingly (step S406; see Fig. 8B (vii)), for example to form the bond pad 6b, the mirror layer 6a, conductor tracks and top electrode, for example for the piezoelectric layer 4. Thereafter, the opening of the dielectric layer 5 can take place in certain regions 5a (step S407; see Fig. 8B (viii)) and the structuring of the functional layer 3 (step S408; see Fig. 8C (ix)) to form the mechanically active functional layer 3.
[0150] A key difference from the first and second exemplary embodiments is that, when the layer structure is opened at the rear, in addition to parts of the base layer 1, a part of the intermediate layer 2 can also remain as a reinforcement or stiffening structure in the region of the mirror support section 3b and / or in the region of the spring sections 3c (not shown here, see Fig. 13) of the mechanically active functional layer 3 (step S409; see Fig. 8C (x)). In this case, the base layer 1 and the intermediate layer 2 can be partially removed by exemplary process steps (for example, by etching) (see also the background example according to Fig. 2C (ix), in which, by way of example, the base layer 1 is opened at the rear towards the intermediate layer 2, and Fig. 2C (x), in which, by way of example, the intermediate layer 2 is opened at the rear towards the functional layer 3).
[0151] This also advantageously makes it possible to reduce or avoid static and / or dynamic deformations of the mirror support section 3b and thus of the mirror 6a even under high dynamic loads on the mirror 6a, and to change / tune the natural frequencies of the oscillating part of the MEMS device 1400 by stiffening the spring sections 3c (particularly advantageous when using the MEMS device / MEMS mirror device as a resonator or as a Lissajous scanner).
[0152] After the mechanically active functional layer 3 has been exposed, whereby the layer structure section 10a has also been formed, the light-transmissive element 40 (for example the glass dome) and the base wafer 30 (for example with integrated getter 31) can also be joined (mechanically connected) to the layer structure section 10a and / or the electrically active section 20 of the layer structure 400, for example by means of the low-temperature process already described, in order to provide a MEMS device 1400, in particular a MEMS mirror device 1400 (step S410; see Fig. 8C (xi)). Since the light-transmissive element 40 and the base wafer 30 are also configured here to pack the layer structure 400 in a vacuum-tight manner, this MEMS device 1400 can also be vacuum-packed, for example, so that the movable parts such as the mirror support section 3b orMirror 6a and the spring sections 3c can oscillate essentially without resistance and damping.
[0153] Fig. 9 shows an exemplary flowchart of a method for producing a layer structure 500 for a MEMS device 1500, in particular a MEMS mirror device 1500, according to a fourth exemplary embodiment, and Figs. 10A-10D show exemplary sectional views of the layer structure 500 during the manufacturing process according to an exemplary manufacturing sequence based on the method according to Fig. 9.
[0154] In this fourth embodiment, for example, a base layer 1 (for example comprising silicon (Si; for example "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg(electronical grade)) or consisting thereof) with a passivation layer 2 applied thereon (for example comprising or consisting of silicon dioxide) (step S501 in Fig. 9).
[0155] For example, a reinforcement layer 32 comprising the first material or consisting of it can now be applied to the passivation layer 2 (for example by deposition; step S502 in Fig. 9), as already shown in Fig. 10A (i). This reinforcement layer 32 can now be structured by a structuring step (step S503 in Fig. 9) such that, for example - locally - in areas of the later mirror support section 3b and / or the later spring sections 3c (not shown here, see, for example, Fig. 13) of the mechanically active functional layer 3, parts of the reinforcement layer 32 remain as reinforcement sections 3d. This can result in a prepared substrate, as already shown in Fig. 10A (ii).
[0156] In a further step, the reinforcement section 3d and the surface of the passivation layer 2 can now be covered with the functional layer 3 (for example by epitaxial growth of, for example, polycrystalline silicon; step S504 in Fig. 9), so that, for example, the reinforcement section 3d is surrounded by the functional layer 3 in at least two spatial directions. As a result, the base element 10 for the formation of the layer construction section 10a could now be formed, wherein the functional layer 3 comprises a material (second material, for example silicon (Si; for example Si sg or Si eg ) or doped silicon (Si; for example Si sg or Si eg )) which has a lower breaking strength and / or a maximum equal modulus of elasticity as the first material of the reinforcing section 3d.
[0157] Subsequently, steps S505 to S512 according to Fig. 9 and Figs. 10A (iii) to 10D (xii) can be carried out, which are identical to steps S102 to S109 according to Fig. 1 and Figs. 2A (i) to 2C (x) of the background example, for forming / producing the layer structure 500.
[0158] Thus, here too, a piezoelectric layer 4 can first be applied to the functional layer 3 of the base element 10 (step S505), as also shown in Fig. 10A (iii), and this can then be structured (step S506; see Fig. 10A (iv)). Here, too, the application of a dielectric layer 5 on the structured piezoelectric layer 4 and the exposure of one or more regions (for example, region 5b and / or regions above the structured piezoelectric layer 4) of the dielectric layer 5 for the subsequent bond pad and / or the subsequent contacting of the piezoelectric layer 4 can follow (step S507; see Fig. 10B (v) and Fig. 10B (vi)).
[0159] An electrode layer 6 can now be applied to the dielectric layer 5 (step S508; see Fig. 10B (vii)) and structured accordingly (step S509; see Fig. 10C (viii)) for the exemplary formation of the bond pad 6b, the mirror layer 6a, conductor tracks and top electrode, for example for the piezoelectric layer 4. Thereafter, the opening of the dielectric layer 5 can take place in certain regions 5a (step S510; see Fig. 10C (ix)) and the structuring of the functional layer 3 (step S511; see Fig. 10C (x)) to form the mirror support section 3b and the spring sections 3c (not shown here, see Fig. 13) of the mechanically active functional layer 3.
[0160] In a further exemplary step S512 of the method according to Fig. 9, the base element 10 is opened at the rear to expose the functional layer 3 on the side opposite the piezoelectric layer 4; see also Fig. 10D (xi), in which, for example, the base layer 1 is opened at the rear toward the intermediate layer 2, and Fig. 10D (xii), in which, for example, the intermediate layer 2 is opened at the rear toward the functional layer 3, thereby forming the layer construction section 10a. Subsequently, the light-transmitting element 40 (for example, the glass dome) and the bottom wafer 30 (for example, with integrated getter 31) can again be provided on the layer structure section 10a and / or the electrically active section 20 of the layer structure 500 in order to provide a MEMS device 1500, in particular a MEMS mirror device 1500 (step S513; see Fig. 10D (xiii)).Since here too the light-transmitting element 40 and the base wafer 30 are configured to pack the layer structure 500 in a vacuum-tight manner, this MEMS device 1500 can also be vacuum-packed, for example, so that the moving parts such as the mirror support section 3b or mirror 6a and the spring sections 3c can oscillate essentially without resistance and damping.
[0161] Advantageously, the provision of a reinforcement section 3d (for example made of silicon carbide (SiC) or tungsten carbide (WC), etc.) in the areas of the mirror support section 3b and / or the spring sections 3c can lead to better mirror flatness with regard to static and dynamic deformation (thus again better optical resolution of the projected image) and enable a targeted influencing, in particular an increase in the natural frequencies of the oscillating system of the MEMS mirror device 1500 (which leads to improved illumination of the image surface of the projected image) while maintaining the same lateral geometry of the mechanically active functional layer 3 or the MEMS chip.
[0162] Fig. 11 shows an exemplary flowchart of a method for producing a layer structure 600 for a MEMS device 1600, in particular a MEMS mirror device 1600, according to a fifth exemplary embodiment, and Figs. 12A-12C show exemplary sectional views of the layer structure 600 during the manufacturing method according to an exemplary manufacturing sequence based on the method according to Fig. 11.
[0163] In this fifth embodiment, in contrast to the exemplary background example according to Figs. 1 and 2A to 2C, a base element 10 can be provided (step S601 in Fig. 11) which, for example, exclusively comprises the functional layer 3 or consists of the functional layer 3 (see Fig. 12A (i)). In this case, the functional layer 3 can comprise the first material or the functional layer 3 can consist of the first material.
[0164] In particular, the single-layer base element 10 (single layer) for forming the layered construction section 10a is possible because the first material, such as silicon carbide (SiC), has a significantly higher modulus of elasticity and a significantly higher fracture strength than silicon (Si; such as "solar silicon" Si sg (solar grade) or "semiconductor silicon" Si eg (electronic grade)), which is otherwise preferably used. As a result, the single layer of the base element 10 can be partially provided with a thickness of, for example, only 150 pm (with a diameter of, for example, 8" of the single SiC layer / single-layer SiC wafer), without requiring an additional layer (such as the base layer 1 of the layer structure 200 to 500 of the first to fourth embodiments) for supporting / handling the functional layer 3.
[0165] In addition, all steps (e.g., etching processes) for exposing the structured functional layer 3 (mechanically active functional layer 3) can be omitted, such as step S109 in Fig. 1 and Figs. 2C (ix) and 2C (x) of the background example or, for example, step S209 in Fig. 3 and Fig. 4C (x) of the first exemplary embodiment, since, in addition to the functional layer 3, there is no further layer that would first have to be removed for the function of the mechanically active functional layer 3. This advantageously makes it possible, for example, to reduce manufacturing time and resource utilization, which at least partially compensates for the longer time required to structure the first material of the functional layer 3 (to form the mechanically active functional layer 3).
[0166] The steps S602 to S608 in the manufacturing method of the layer structure 600 according to Fig. 11 are the same as the steps S102 to S108 of the background example according to Fig. 1.
[0167] First, a piezoelectric layer 4 can be applied to the base element 10 (step S602), as also shown in Fig. 12A (ii), and then structured (step S603; see Fig. 12A (iii)). This can be followed by the application of a dielectric layer 5 on the structured piezoelectric layer 4 and the exposure of one or more regions (for example, region 5b or regions above the piezoelectric layer 4) of the dielectric layer 5 for the subsequent bond pad and / or for the contact of the piezoelectric layer 4 (step S604; see Fig. 12A (iv) and Fig. 12B (v)).
[0168] Now, an electrode layer 6 can be applied to the dielectric layer 5 (step S605; see Fig. 12B (vi)) and structured accordingly (step S606; see Fig. 12B (vii)) for the exemplary formation of the bond pad 6b, the mirror layer 6a, conductor tracks and top electrode, for example for the piezoelectric layer 4. Thereafter, the dielectric layer 5 can be opened again in certain regions 5a (step S607; see Fig. 12B (viii)) and the functional layer 3 can be structured (step S608; see Fig. 12C (ix)) to form the mirror carrier section 3b and the spring sections 3c (not shown here, see Fig. 13) of the mechanically active functional layer 3, whereby the layer structure section 10a is formed.
[0169] It should be noted at this point that the structuring of the functional layer 3 can also have, for example, a (rear-side) structuring for forming stiffening structures, for example in the region of the mirror support section 3b and / or the spring sections 3c (not shown here, see Fig. 13) of the mechanically active functional layer 3, so that a monolithic structure consisting of a structure of the mechanically active functional layer 3 and a stiffening structure for stiffening the structure of the mechanically active functional layer 3 can be formed.
[0170] Thus, as already described, the layer structure 600 has already been formed with the layer structure section 10a and the electrically active section 20 arranged thereon, so that further elements (for example, light-transmitting element 40 and bottom wafer 30 with, for example, integrated getter 31) can now be joined to the layer structure section 10a and / or the electrically active section 20 of the layer structure 600 (here too, for example, using the low-temperature process already described), as is also shown in Fig. 12C (x).
[0171] As a result, the MEMS device 1600, in particular the MEMS mirror device 1600, can now be provided (step S609; see Fig. 12C (x)). Since the light-transmissive element 40 and the base wafer 30 are also configured to vacuum-tightly package the layer structure 600, this MEMS device 1600 can also be vacuum-packed, for example, so that the moving parts, such as the mirror support section 3b including the mirror 6a and the spring sections 3c of the mechanically active functional layer 3, can oscillate essentially without resistance and damping.
[0172] Fig. 13 shows a 2D contour plot of the deflection amplitude (here, for example, a small relative angle) of a MEMS structure for an exemplary comparison of the deflection frequencies / natural frequencies of the oscillating system when using silicon (Si, here polycrystalline silicon) and silicon carbide (SiC). The MEMS structure (here, the mechanically active functional layer 3) comprises a circular mirror plate with a diameter of approximately 1 mm, which is suspended from a chip frame via torsion spring sections of equal length (spring sections 3c, each approximately 0.02 mm wide and approximately 0.5 mm long). This mechanically active functional layer 3 has a layer thickness of approximately 0.05 mm.
[0173] The mechanically active functional layer 3 was then simulated to determine at which frequencies the MEMS structure exhibits essentially the same deflection amplitude when using silicon (Si; here, for example, polycrystalline silicon) and when using silicon carbide (SiC). Figure 13 shows the deflection / deflection amplitude of the mirror support section 3b with torsion of the spring sections 3c of the MEMS structure simulated with the two different materials.
[0174] For example, a significant deviation in the natural frequencies / deflection frequencies between the two materials was observed, with the MEMS structure made of silicon (Si; here, for example, polycrystalline silicon) having a natural frequency of approximately 25.7 kHz, while the same MEMS structure made of silicon carbide (SiC) had a natural frequency of approximately 35 kHz.
[0175] Conversely, this means that, with constant parameters such as chip size (structure size) and deflection amplitude or deflection angle, the MEMS structure made of silicon carbide (SiC) has a natural frequency (also called scan frequency) that is approximately 40% higher than the MEMS structure made of silicon (Si; here, for example, polycrystalline silicon), so that the MEMS device with silicon carbide (SiC) as the mechanically effective functional layer 3 can be operated in resonance significantly faster due to the higher Young's modulus of SiC. This, in turn, has a positive effect on the illumination of the projected image, whereby the material stress in the spring sections 3c generated by the higher frequencies does not pose a problem for the silicon carbide (SiC), as is also shown and described further in Fig. 15.
[0176] Fig. 14 shows an exemplary comparison of the dynamic deformation of the oscillating system of a MEMS device using a mirror plate 6a made of silicon (Si, here polycrystalline silicon) and a mirror plate 6a made of silicon carbide (SiC).
[0177] Both mirror plates 6a have a diameter of approximately 1 mm and the spring width of the spring sections 3c of the MEMS structure made of silicon (Si; here, for example, polycrystalline silicon) is still approximately 0.02 mm, while the spring width of the spring sections 3c of the MEMS structure made of silicon carbide (SiC) is approximately 0.015 mm.
[0178] Otherwise, in a modification of the comparison of the different materials of the MEMS structure described in Fig. 13, the simulated natural frequencies with which the two mirror plates 6a are deflected are approximately 25.7 kHz and the simulated mechanical deflection angles are approximately 12.5°.
[0179] As can be seen in the comparison of the two contour plots of the mirror plate 6a made of silicon (Si; see Fig. 14 (i)) and the mirror plate 6a made of silicon carbide (SiC; see Fig. 14 (ii)), the value (peak-valley value; shown here as a relative value for the comparison of the values of the dynamic deformation with each other) of the dynamic deformation of the two mirror plates 6a in this exemplary comparison is approximately 2 times lower for the mirror plate 6a made of silicon carbide (SiC; here the peak-valley value was approximately 271) than for the mirror plate 6a made of silicon (Si; here the peak-valley value was approximately 502), although the spring width of the spring sections 3c of the MEMS structure made of silicon carbide (SiC) is already approximately 25% narrower than the spring width of the spring sections 3c of the MEMS structure made of silicon (Si; here polycrystalline silicon is used as an example).
[0180] The use of, for example, silicon carbide for the mechanically active functional layer 3 advantageously leads to a significantly lower dynamic deformation of the mirror plate 6a and thus also to a better optical quality of the beam deflection, in particular to an improved optical resolution of the image projected by the mirror plate 6a of the MEMS device, in particular MEMS mirror device.
[0181] Fig. 15 shows an exemplary comparison of the mechanical stresses (mechanical stress; first principal stress) occurring in the region of the clamping of the torsion springs / spring sections 3c on the chip frame in relation to the exemplary fracture limit of the respective material of the oscillating system of the MEMS structure made of silicon (Si, here polycrystalline silicon) and the MEMS structure made of silicon carbide (SiC) according to Fig. 13.
[0182] The design of the two MEMS structures is identical, as already described in Fig. 13, and both MEMS structures are simulated with a deflection angle of approximately 12.5°.
[0183] It is clear that the breaking point of the MEMS structure made of silicon (Si, here polycrystalline silicon) is already very strongly exploited, namely in places up to 65% / 70% of the breaking point (see Fig. 15 (i), especially in the middle area of the spring section 3c shown), which for example is the case with polycrystalline silicon (Si; for example "solar silicon" Si sg (solar grade)) with a value of approximately 1.5 GPa.
[0184] In contrast, the mechanical stresses (first principal stress) in relation to the fracture strength of the MEMS structure made of silicon carbide (SiC), which is calculated to be approximately 10 GPa, are only 25% (see Fig. 15 (ii), especially in the middle area of the spring section 3c shown).
[0185] While in the MEMS structure made of silicon (Si, here polycrystalline silicon) the mechanical stresses only have a safety factor of approximately 1.4 compared to the material-specific fracture limit, this safety factor is approximately 4 for the MEMS structure made of silicon carbide (SiC).
[0186] This significantly higher safety factor for silicon carbide (SiC) leads, among other things, to a significantly longer lifetime (greater number of vibration cycles until fatigue failure) of the MEMS device, in particular MEMS mirror device, or can be used to allow higher vibration amplitudes (with higher mechanical stress in the spring sections) in the MEMS device / MEMS mirror device, thereby again increasing the optical resolution and also the field of view of the image projected by the MEMS device.
[0187] It should be noted that only examples or exemplary embodiments of the present disclosure, as well as technical advantages, have been described above in detail with reference to the accompanying figures. However, the present disclosure is in no way limited or restricted to the exemplary embodiments described above and their design features or their described combinations, but further encompasses modifications of the exemplary embodiments, in particular those encompassed by modifications of the features of the described examples or by combination or partial combination of individual or several of the features of the described examples within the scope of the independent claims. List of reference symbols
[0188] 1 base layer / additional layer
[0189] 2 Intermediate layer / passivation layer
[0190] 3 Functional layer / mechanically effective functional layer
[0191] 3a Trenches or structured areas of the functional layer
[0192] 3b Mirror support section
[0193] 3c Spring sections
[0194] 3d reinforcement section
[0195] 4 piezoelectric layer
[0196] 5 dielectric layer
[0197] 5a opened area of the dielectric layer
[0198] 5b opened area of the dielectric layer
[0199] 6 Electrode layer
[0200] 6a Mirror / Mirror layer / Mirror plate
[0201] 6b Bond pad
[0202] 10 Basic element
[0203] 10a Layer structure section
[0204] 20 electrically active section
[0205] 30 bottom wafers
[0206] 31 getters
[0207] 32 Reinforcement layer
[0208] 40 translucent element / glass dome
[0209] 100 Layer structure of the background example
[0210] 200 Layer structure of the first embodiment 300 Layer structure of the second embodiment
[0211] 400 Layer structure of the third embodiment
[0212] 500 Layer structure of the fourth embodiment
[0213] 600 Layer structure of the fifth embodiment
[0214] 1100 MEMS mirror device of the background example
[0215] 1200 MEMS mirror device of the first embodiment
[0216] 1300 MEMS mirror device of the second embodiment
[0217] 1400 MEMS mirror device of the third embodiment
[0218] 1500 MEMS mirror device of the fourth embodiment
[0219] 1600 MEMS mirror device of the fifth embodiment
Claims
Patent claims 1. Layer structure (200, 300, 400, 500, 600) for a MEMS mirror device (1200, 1300, 1400, 1500, 1600), comprising: a layer structure section (10a) which has a mechanically active functional layer (3) with spring sections (3c) and a mirror support section (3b) which is oscillatingly movable in at least one dimension and is resiliently held by the spring sections (3c), and wherein the layer structure section (10a) has a first material which has a higher fracture strength and / or an at least equally high modulus of elasticity than monocrystalline or polycrystalline silicon (Si), in particular Si sg (Silicon solar grade) or Si eg (Silicon electronical grade).
2. Layer structure (200, 300, 400, 500, 600) according to claim 1, wherein the fracture limit of the first material is at least 60%, preferably at least 100%, particularly preferably at least 500% higher than the fracture limit of single-crystalline or polycrystalline silicon (Si), in particular Si sg (Silicon solar grade) or Si eg (Silicon electronical grade), and / or the modulus of elasticity of the first material is at least equal to, preferably at least 100%, particularly preferably at least 200% or particularly preferably at least 300% higher than the modulus of elasticity of single-crystalline or polycrystalline silicon (Si), in particular Si sg (Silicon solar grade) or Si eg (Silicon electronic grade).
3. Layer structure (200, 300, 400, 500, 600) according to claim 1 or 2, wherein the first material is at least one of silicon carbide (SiC), in particular 4H-SiC or 6H-SiC, tungsten carbide (WC), titanium carbide (TiC), chromium carbide (Cr3C2, Cr7C3, Cr23 C6) or aluminum oxide (Al2O3), in particular made of a material of silicon carbide (SiC), in particular 4H-SiC or 6H-SiC, tungsten carbide (WC), titanium carbide (TiC), chromium carbide (Cr3C2, Cr7C3, Cr 23 C6) or aluminum oxide (Al2O3).
4. Layer structure (200, 300, 400, 500, 600) according to one of the preceding claims, wherein the first material has a doping.
5. Layer structure (200, 400, 500, 600) according to one of the preceding claims, wherein the mechanically active functional layer (3) comprises the first material.
6. Layer structure (200, 300, 400, 500) according to one of claims 1 to 4, wherein the layer structure section (10a) has an additional layer (1) in addition to the mechanically active functional layer (3), wherein at least the mechanically active functional layer (3) or at least the additional layer (1) has the first material.
7. Layer structure (200, 300) according to claim 6, wherein the mechanically effective functional layer (3) is mechanically connected in direct contact with the additional layer (1).
8. Layer structure (200) according to claim 6 or 7, wherein the mechanically active functional layer (3) comprises the first material and the additional layer (1) comprises a second material with a lower breaking point and / or a maximum equal modulus of elasticity as the first material of the mechanically active functional layer (3).
9. Layer structure (300) according to claim 6 or 7, wherein the additional layer (1) comprises the first material and the mechanically active functional layer (3) comprises a second material with a lower breaking point and / or a modulus of elasticity at most equal to that of the first material of the additional layer (1).
10. Layer structure (400) according to claim 6, wherein an intermediate layer (2) is provided between the mechanically active functional layer (3) and the additional layer (1), in particular an electrically insulating intermediate layer (2), wherein the additional layer (1) and the mechanically active functional layer (3) comprise the first material, in particular consist of the first material.
11. Layer structure (200, 300, 400) according to one of claims 8 to 10, wherein at least parts of the additional layer (1) for stiffening the mechanically active functional layer (3) in the region of the mirror support section (3b) and / or in the region of the Spring sections (3c) of the mechanically active functional layer (3) are provided and are mechanically connected to the mechanically active functional layer (3).
12. Layer structure (500) according to claim 5, wherein a reinforcing section (3d) comprising the first material is provided within the mechanically active functional layer (3), wherein the mechanically active functional layer (3) surrounding the reinforcing section (3d) in at least two spatial directions comprises a second material having a lower breaking point and / or a modulus of elasticity at most equal to that of the first material of the reinforcing section (3d).
13. Layer structure (500) according to claim 12, wherein the reinforcement section (3d) is provided in the region of the mirror support section (3b) and / or the spring sections (3c) of the mechanically active functional layer (3) within the mechanically active functional layer (3) for reinforcing the mirror support section (3b) and / or the spring sections (3c).
14. Layer structure (600) according to one of claims 1 to 5, further comprising: a bottom wafer (30) which is mechanically connected in direct contact with the layer structure section (10a), and the layer structure section (10a) is formed as a single layer and has the mechanically active functional layer (3), wherein the mechanically active functional layer (3) has the first material, in particular consists of the first material, and is mechanically connected in direct contact with the bottom wafer (30).
15. Layer structure (200, 300, 400, 500, 600) according to one of the preceding claims, wherein the layer structure (200, 300, 400, 500, 600) has, in addition to the layer structure section (10a), an electrically active section (20) with at least one actuator and / or sensor, in particular with at least one actuator and / or sensor layer.
16. Layer structure (200, 300, 400, 500, 600) according to claim 15, wherein the at least one actuator and / or sensor, in particular the at least one actuator and / or sensor layer, is designed as a piezo actuator and / or piezo sensor or as a piezoelectric layer (4).
17. Layer structure (200, 300, 400, 500, 600) according to claim 15 or 16, further comprising: a light-transmitting element (40), in particular a glass dome, which is mechanically connected to the mechanically active functional layer (3) or to the electrically active section (20).
18. A method for producing a layer structure (200, 300, 400, 500, 600) for a MEMS mirror device (1200, 1300, 1400, 1500, 1600) according to one of the preceding claims, comprising: - providing a base element (10) for forming the layered construction section (10a), and - Structuring the base element (10) to form the mechanically active functional layer (3) of the layer construction section (10a), wherein the mechanically active functional layer (3) has the spring sections (3c) and the mirror support section (3b), which is oscillatingly movable in at least one dimension and is resiliently held by the spring sections (3c), wherein the base element (10) has a first material which has a higher breaking point and / or an at least equally high modulus of elasticity than monocrystalline or polycrystalline silicon (Si), in particular Si sg (Silicon solar grade) or Si eg (Silicon electronical grade).
19. The method according to claim 18, wherein the layer structure section (10a) has an additional layer (1) in addition to the mechanically active functional layer (3), wherein at least the mechanically active functional layer (3) or at least the additional layer (1) has the first material, and the mechanically active functional layer (3) is mechanically connected to the additional layer (1).
20. The method of claim 19, further comprising: - Structuring the additional layer (1) so that the mirror support section (3b) and / or the spring sections (3c) of the mechanically active functional layer (3) are projecting from the side of the Additional layer (1) is substantially completely exposed, wherein the mechanically effective functional layer (3) comprises the first material, in particular consists of the first material, or - Structuring the additional layer (1) so that a part of the additional layer (1) for stiffening the mechanically active functional layer (3) remains in the region of the mirror support section (3b) and / or in the region of the spring sections (3c) of the mechanically active functional layer (3), wherein the additional layer (1) and / or the mechanically active functional layer (3) comprises the first material, in particular consists of the first material.
21. The method according to claim 18, wherein the base element (10) for forming the layer structure section (10a) is designed as a single layer, wherein the single layer of the base element (10) comprises the first material, in particular consists of the first material.
22. The method according to claim 18, wherein the provision of the base element (10) comprises forming the base element (10), comprising: - Providing a base layer (1) with an intermediate layer (2), - applying a reinforcing layer (32) to the intermediate layer (2), wherein the reinforcing layer (32) comprises the first material, - structuring the reinforcing layer (32) to form the reinforcing section (3d), wherein the reinforcing section (3d) partially covers a surface of the intermediate layer (2), and - forming the functional layer (3) on the intermediate layer (2) and the formed reinforcement section (3d) such that the reinforcement section (3d) is surrounded by the functional layer (3) in at least two spatial directions, wherein the base layer (1) with intermediate layer (2), the reinforcement section (3d) and the functional layer (3) form the base element (10), and wherein during the structuring of the formed base element (10) the functional layer (3) is formed into the mechanically effective functional layer (3).
23. The method according to claim 18, wherein the reinforcement section (3d) is applied to the intermediate layer (2) only in the area in which, during the structuring of the functional layer (3), the mechanical effective functional layer (3) the mirror support section (3b) and / or the spring sections (3c) of the mechanically effective functional layer (3) are formed.
24. MEMS mirror device (1200, 1300, 1400, 1500, 1600), comprising a layer structure (200, 300, 400, 500) according to one of claims 1 to 17.
Citation Information
Patent Citations
GLASS-SUBSTRATED MEMS MIRROR DEVICE AND METHOD FOR ITS MANUFACTURING
DE102020008076A1
Multi-axis magnetically actuated device
US20020171901A1
Micromachined torsional scanner
US5629790A
Cited By
MEMS micromirror, optical apparatus, and terminal device
WO2026113304A1