Cr-Ni ALLOY TUBE

The Cr-Ni alloy tube achieves high strength and balanced mechanical properties through a specific chemical composition and heat treatment process, addressing the challenge of maintaining strength in harsh oil and gas well environments by minimizing the difference between compressive and tensile yield stresses.

WO2024201749A1PCT designated stage expired Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/012654
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Cr-Ni alloy tubes used in oil country tubular goods face challenges in maintaining high strength while minimizing the difference between compressive and tensile yield stresses, especially after cold working and heat treatment, which affects their performance in harsh oil and gas well environments.

Method used

A Cr-Ni alloy tube with specific chemical composition and heat treatment process, involving high-frequency induction heating and rapid cooling, to achieve a tensile yield stress of 780 MPa or more and a compressive yield stress ratio within 0.80 to 0.95 of the tensile yield stress, ensuring balanced mechanical properties.

Benefits of technology

The solution allows for a Cr-Ni alloy tube with high strength that maintains performance even in the event of softening in the weld zone, ensuring reliable use as oil country tubular goods by minimizing the difference between compressive and tensile yield stresses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a Cr-Ni alloy tube in which the tensile yield stress YSLT and the compressive yield stress YSLC in the tube axial direction of the Cr-Ni alloy tube and the tensile yield stress YSHT of a test piece after high-frequency induction heating and quenching satisfy [0.80 ≤ YSLC / YSLT < 0.95], [YS HT - 0.24 × YSLT ≥ 50.0], and [YSLT ≥ 443 × YSLT / YSLC + 2.28 × YSHT - 350], the test piece being collected from a thickness center position of the Cr-Ni alloy tube so that the longitudinal direction of the test piece is parallel to the tube axial direction.
Need to check novelty before this filing date? Find Prior Art

Description

Cr-Ni alloy tube

[0001] The present invention relates to a Cr-Ni alloy tube.

[0002] In recent years, the conditions for extracting oil wells and gas wells (hereinafter, oil wells and gas wells will be collectively referred to simply as "oil wells") from which crude oil, natural gas, etc. are extracted have become increasingly severe. For this reason, austenitic alloy pipes containing Cr and Ni and having excellent corrosion resistance (hereinafter, also referred to as "Cr-Ni alloy pipes") are sometimes used for oil country tubular goods used in oil wells.

[0003] In addition to excellent corrosion resistance, OCTG also requires high strength. The strength grade of OCTG is generally defined by the tensile yield stress in the axial direction of the tubing. OCTG users determine the environment of the well to be drilled (geologic pressure, temperature and pressure of the production fluid) through exploratory drilling and geological surveys, and then select OCTG with a strength grade that can withstand the conditions.

[0004] However, it is known that in cold-worked corrosion-resistant alloy pipes, the compressive yield strength in the pipe axis direction is smaller than the tensile yield stress in the pipe axis direction. As mentioned above, the strength grade of oil country tubular goods is generally determined by the tensile yield strength. Therefore, it is preferable that the difference between the compressive yield stress and the tensile yield stress is small.

[0005] Patent Document 1 discloses an austenitic alloy pipe that has small anisotropy in yield strength and can therefore withstand stress distributions that vary depending on the environment in which it is used.

[0006] International Publication No. 2012 / 128258

[0007] Incidentally, Cr-Ni alloy pipes as oil country tubular goods are sometimes welded to other alloy pipes or steel pipes. In this case, the welded portion of the Cr-Ni alloy pipe is softened by the welding heat. Therefore, it is necessary to select an oil country tubular good with a strength grade that can withstand the oil well environment in question, taking into consideration the softening at the welded portion.

[0008] In order to maintain high strength even when softening occurs in the weld, it is conceivable to increase the degree of cold working, but this is not desirable because it results in the compressive yield stress being significantly lower than the tensile yield stress.

[0009] SUMMARY OF THE INVENTION An object of the present invention is to solve the above problems and to provide a Cr-Ni alloy pipe having high strength while minimizing the difference between compressive yield stress and tensile yield stress.

[0010] The present invention has been made to solve the above problems, and the gist of the present invention is the following Cr-Ni alloy tube.

[0011] (1) A Cr-Ni alloy pipe, wherein the tensile yield stress YS in the pipe axis direction of the Cr-Ni alloy pipe LT and compressive yield stress YS LC The tensile yield stress YS of the test piece obtained by taking a specimen from the center position of the wall thickness of the Cr-Ni alloy pipe so that the longitudinal direction is parallel to the pipe axis direction, and using a high-frequency induction heating device, heating from room temperature to 1150°C at a heating rate of 100°C / s, subsequently heating to 1200°C at a heating rate of 25°C / s, and then holding at 1200°C for 180 seconds, and then spraying Ar gas to rapidly cool to room temperature under conditions where the cooling rate in the temperature range from 1200°C to 800°C is 50°C / s. HT A Cr-Ni alloy tube that satisfies the following formulas (i) to (iii): 0.80≦YS LC / YS LT <0.95...(i) YS HT -0.24 x YS LT ≧50.0...(ii) YS LT ≧443×YS LT / YS LC +2.28 x YS HT -350 (iii) where the meanings of the symbols in the above formula are as follows: YS LC : Compressive yield stress in the tube axial direction (MPa) YS LT : Tensile yield stress in the tube axial direction (MPa) YS HT : tensile yield stress (MPa) of the test piece after high-frequency induction heating and rapid cooling

[0012] (2) Tensile yield stress YS in the axial direction of the Cr-Ni alloy tube LT The Cr-Ni alloy pipe according to (1) above, wherein the strain is 780 MPa or more.

[0013] (3) Chemical composition, in mass%, C: 0.030% or less, Si: 0.50% or less, Mn: 1.00% or less, P: 0.030% or less, S: 0.0050% or less, Cr: 19.00 to 32.00%, Ni: 29.50 to 55.00%, Mo: 2.50 to 12.00%, Cu: 3.00% or less, V: 0.01 to 0.50%, Nb + Ti: 0.002 to 1.000%, Al: 0.001 to 0.500%, N: 0.005 to 0.400%, W: 0 to 1.00%, Co: 0 to 1.00%, Sn: 0 to 0.010%, As: 0 to 0.010%, Zn: 0 to 0.010%, Pb: 0 to 0.010%, Sb: 0 to 0.010%, B: 0 to 0.0050%, Ca: 0 to 0.0200%, Mg: 0 to 0.0200%, REM: 0 to 0.100%, and the balance: Fe and impurities.

[0014] (4) The Cr-Ni alloy tube according to (3), wherein the chemical composition contains, in mass%, one or more elements selected from W: 0.01 to 1.00%, Co: 0.01 to 1.00%, Sn: 0.001 to 0.010%, As: 0.001 to 0.010%, Zn: 0.001 to 0.010%, Pb: 0.0005 to 0.010%, Sb: 0.0005 to 0.010%, B: 0.0001 to 0.0050%, Ca: 0.0005 to 0.0200%, Mg: 0.0001 to 0.0200%, and REM: 0.001 to 0.100%.

[0015] (5) The Cr-Ni alloy tube according to (3) or (4) above, wherein the chemical composition further satisfies the following formulas (iv) and (v): 9Mo+100N≧45.0 (iv) Ni+1.4Cu+Mo-0.9Cr-2Si-1.2Mn-5.7C+20N+90(0.15Nb+0.27V+0.3Ti)≦42.0 (v) where the element symbols in the formulas above represent the content (mass%) of each element in the alloy tube, and zero is substituted if the element is not contained.

[0016] (6) The Cr-Ni alloy tube according to any one of (3) to (5) above, wherein the chemical composition further satisfies the following formula (vi): 0.001×YS LT -0.820<N<0.001×YS LT −0.740 (vi) where the meanings of the symbols in the above formula are as follows: YS LC : Compressive yield stress in the tube axial direction (MPa) N: N content in the alloy tube (mass%)

[0017] According to the present invention, a Cr-Ni alloy pipe having high strength can be obtained while minimizing the difference between the compressive yield stress and the tensile yield stress.

[0018] Each of the requirements of the present invention will be described in detail below.

[0019] 1. Mechanical Properties The mechanical properties of the Cr—Ni alloy tube according to this embodiment will be described. The Cr—Ni alloy tube according to this embodiment has mechanical properties that satisfy the following formulas (i) to (iii). In the present invention, the Cr—Ni alloy tube refers to an austenitic alloy tube containing 19.00 to 32.00% Cr and 29.50 to 55.00% Ni.

[0020] <Strength Anisotropy> The Cr—Ni alloy tube according to this embodiment has improved strength due to work hardening caused by cold working, but if it is subsequently subjected to high-temperature heat treatment, its strength decreases and it is not possible to maintain the strength required in the usage environment. That is, the Cr—Ni alloy tube according to this embodiment is in an as-cold-worked state or in a state in which it has been subjected to low-temperature heat treatment after cold working. Therefore, the tensile yield stress in the axial direction of the Cr—Ni alloy tube is necessarily higher than the compressive yield stress in the axial direction.

[0021] However, if the difference between the compressive yield stress and the tensile yield stress in the axial direction of the pipe is excessive, even if the tensile yield stress is sufficient, the compressive yield stress will be insufficient and the pipe will not be usable as an oil country tubular good. Therefore, the compressive yield stress and the tensile yield stress in the axial direction of the pipe must satisfy the following formula (i): 0.80≦YS LC / YS LT <0.95 (i) where the meanings of the symbols in the above formula are as follows: YS LC : Compressive yield stress in the tube axial direction (MPa) YS LT : Tensile yield stress in the tube axial direction (MPa)

[0022] Y.S. LC / YS LT The value of YS is preferably 0.82 or more, more preferably 0.84 or more, and even more preferably 0.86 or more. LC / YS LT The value of may be 0.94 or less.

[0023] The tensile yield stress YS in the axial direction of the tube LT However, as described above, the Cr-Ni alloy pipe according to this embodiment is in the state of being cold worked or having been subjected to a low-temperature heat treatment after cold working, so that the tensile yield stress YS in the pipe axis direction is 780 MPa or more. LT is preferably 800 MPa or more, more preferably 820 MPa or more, even more preferably 840 MPa or more, and even more preferably 850 MPa or more.

[0024] Specifically, the compressive yield stress in the tube axial direction is determined by the following method. A compression test is performed according to ASTM E9 (2019). A cylindrical test piece for the compression test is prepared from the center of the wall thickness of the Cr-Ni alloy tube. The size of the cylindrical test piece is, for example, 4 mm in diameter at the parallel part and 8 mm in length. The longitudinal direction of the cylindrical test piece is parallel to the tube axial direction of the Cr-Ni alloy tube. A compression test is performed using the cylindrical test piece in air at room temperature (25°C), and the obtained 0.2% offset proof stress is used as the compressive yield stress YS in the tube axial direction. LC (MPa).

[0025] Similarly, the tensile yield stress in the tube axial direction is determined by the following method. A tensile test is performed according to ASTM E8 / E8M (2021). A round bar test specimen for the tensile test is prepared from the center of the wall thickness of the Cr-Ni alloy tube. The size of the round bar test specimen is, for example, 4 mm in parallel diameter and 20 mm in gauge length. The longitudinal direction of the round bar test specimen is parallel to the tube axial direction of the Cr-Ni alloy tube. A tensile test is performed using the round bar test specimen at room temperature (25°C) in the air, and the obtained 0.2% offset proof stress is defined as the tensile yield stress YS LT (MPa).

[0026] <Base strength> As mentioned above, the strength of a Cr—Ni alloy tube can be improved by cold working, but excessive working leads to increased anisotropy. Therefore, in order to avoid excessive working, it is necessary to ensure sufficient strength before cold working, i.e., strength in a state without the effect of work hardening (hereinafter also referred to as "base strength"). As a result of the inventors' studies, they found that an index of base strength can be obtained from the tensile yield stress of a test specimen in which the effects of work hardening have been eliminated by high-frequency induction heating and rapid cooling, and the tensile yield stress in the axial direction of the Cr—Ni alloy tube.

[0027] Specifically, by satisfying the following formula (ii), the base strength is sufficient for use as an oil country tubular good. HT -0.24 x YS LT ≧50.0 (ii) where the meanings of the symbols in the above formula are as follows: YS LT : Tensile yield stress in the tube axial direction (MPa) YSHT : tensile yield stress (MPa) of the test piece after high-frequency induction heating and quenching

[0028] The test specimen after high-frequency induction heating and quenching is obtained by the following procedure. First, a test specimen is taken from the center of the wall thickness of the Cr-Ni alloy pipe so that its longitudinal direction is parallel to the pipe axis. The test specimen is prepared in accordance with ASTM E8 / E8M (2021). Specifically, when the wall thickness of the alloy pipe is 6 mm or more, a cylindrical test specimen with a diameter of 6 mm and a gauge length of 30 mm is used. When the wall thickness of the alloy pipe is less than 6 mm, a circular arc-shaped test specimen with the same thickness as the wall thickness of the alloy pipe and a gauge length of 50 mm is used.

[0029] Next, the cylindrical test piece is heated using a high-frequency induction heating device from room temperature to 1150°C at a heating rate of 100°C / s, and then to 1200°C at a heating rate of 25°C / s. At this time, the heating area by the high-frequency induction heating device is a region 3.5 mm from the center in the longitudinal direction of the test piece to both ends and 7.0 mm in the longitudinal direction. In addition, the temperature of the test piece is measured using a thermocouple installed in the center of the test piece in the longitudinal direction.

[0030] The test piece is then held at 1200°C for 180 seconds. Immediately after holding, Ar gas is sprayed onto the test piece, which is rapidly cooled to room temperature at a cooling rate of 50°C / s in the temperature range from 1200°C to 800°C. Then, using the test piece after high-frequency induction heating and rapid cooling, a tensile test is carried out in air at room temperature (25°C) in accordance with JIS Z 2241 (2011), and the obtained 0.2% offset proof stress is used as the tensile yield stress YS of the test piece after high-frequency induction heating and rapid cooling. HT (MPa).

[0031] <Work hardening ability> In order to improve strength by cold working while suppressing an increase in anisotropy, excellent work hardening ability is required, which allows efficient work hardening even with a small degree of working. As a result of intensive research by the present inventors, it was found that the YS LC / YS LT The reciprocal of YS LT / YS LCIt was also found that the tensile yield stress in the axial direction of the Cr-Ni alloy tube and the YS LT / YS LC and the tensile yield stress YS of the test piece after eliminating the influence of work hardening by high-frequency induction heating and rapid cooling. HT It was found that the following relationship is an index of work hardening capacity.

[0032] Specifically, by satisfying the following formula (iii), the steel has sufficient work hardening ability for use as an oil country tubular good. LT ≧443×YS LT / YS LC +2.28 x YS HT -350 (iii) where the meanings of the symbols in the above formula are as follows: YS LC : Compressive yield stress in the tube axial direction (MPa) YS LT : Tensile yield stress in the tube axial direction (MPa) YS HT : tensile yield stress (MPa) of the test piece after high-frequency induction heating and rapid cooling

[0033] As described above, from the three mechanical property values ​​of the tensile yield stress and compressive yield stress in the axial direction of the Cr-Ni alloy pipe, and the tensile yield stress of the test piece after high-frequency induction heating and quenching, it is possible to select a Cr-Ni alloy pipe that can maintain high strength even when softening occurs in the weld and is a highly reliable material for oil country tubular goods.

[0034] 2. Chemical Composition The chemical composition of the Cr-Ni alloy tube according to this embodiment is not particularly limited as long as it contains the predetermined amounts of Cr and Ni and has the above-mentioned mechanical properties. The Cr-Ni alloy tube according to this embodiment preferably has, for example, the chemical composition shown below. The reasons for limiting each element are as follows. In the following description, "%" in the content means "mass %."

[0035] C: 0.030% or less Carbon (C) is an element that has the effect of increasing the strength of an alloy. However, if C is contained in excess, Cr carbides are formed at the grain boundaries. Cr carbides increase the susceptibility to stress corrosion cracking (SCC) at the grain boundaries. Therefore, the C content is 0.030% or less. The C content is preferably less than 0.030%, more preferably 0.025%, and even more preferably 0.020% or less. The lower limit of the C content is preferably 0.001%, more preferably 0.003%, and even more preferably 0.005%.

[0036] Si: 0.50% or less Silicon (Si) is an element that has the effect of deoxidizing the alloy. However, if Si is contained in excess, the hot workability of the alloy will decrease. Therefore, the Si content is 0.50% or less. The preferred Si content is less than 0.50%. The preferred upper limit of the Si content is 0.45%, more preferably 0.40%. The preferred lower limit of the Si content is 0.05%, more preferably 0.10%.

[0037] Mn: 1.00% or less Manganese (Mn) is an element that deoxidizes the alloy. Mn is also an austenite-forming element and stabilizes the austenite phase. However, excessive Mn content reduces the hot workability of the alloy. Therefore, the Mn content is 1.00% or less. A preferred Mn content is less than 1.00%. A preferred upper limit of the Mn content is 0.90%, more preferably 0.80%. A preferred lower limit of the Mn content is 0.10%, more preferably 0.30%.

[0038] P: 0.030% or less Phosphorus (P) is an impurity element. P increases the stress corrosion cracking susceptibility of the alloy in a hydrogen sulfide environment. Therefore, a low P content is preferable, and the P content is 0.030% or less. The P content is preferably 0.025% or less, and more preferably 0.020% or less.

[0039] S: 0.0050% or less Sulfur (S) is an impurity element. S reduces the hot workability of the alloy. Therefore, a low S content is preferable, and the S content is 0.0050% or less. The S content is preferably 0.0030% or less, and more preferably 0.0010% or less.

[0040] Cr: 19.00 to 32.00% Chromium (Cr) is an element that, in the presence of Ni, has the effect of increasing the stress corrosion cracking resistance (SCC resistance) of the alloy. Cr also increases the strength of the alloy through solid solution strengthening. On the other hand, if Cr is contained in excess, this effect saturates and the hot workability of the alloy deteriorates. Therefore, the Cr content is 19.00 to 32.00%. A preferred lower limit of the Cr content is 21.00%, more preferably 23.00%. A preferred upper limit of the Cr content is 30.00%, more preferably 28.00%.

[0041] Ni: 29.50 to 55.00% Nickel (Ni) is an austenite-forming element and has the effect of stabilizing the austenite phase. Ni also improves SCC resistance. However, if Ni is contained in excess, this effect saturates. Therefore, the Ni content is 29.50 to 55.00%. A preferred lower limit of the Ni content is 34.00%, and more preferably 40.00%. A preferred upper limit of the Ni content is 53.00%, and more preferably 50.00%.

[0042] Mo: 2.50 to 12.00% Molybdenum (Mo) is an element that, in the presence of Cr and Ni, has the effect of increasing the SCC resistance of the alloy. Mo also increases the strength of the alloy through solid solution strengthening. However, if Mo is contained in excess, this effect saturates and the hot workability of the alloy decreases. Therefore, the Mo content is 2.50 to 12.00%. A preferred lower limit of the Mo content is 3.50%, more preferably 5.00%. A preferred upper limit of the Mo content is 10.00%, more preferably 8.00%.

[0043] Cu: 3.00% or less Copper (Cu) is effective in stabilizing the passive film and is an element effective in improving pitting corrosion resistance and general corrosion resistance. However, if Cu is contained in excess, this effect saturates and further, hot workability deteriorates. Therefore, the Cu content is 3.00% or less. The Cu content is preferably 2.00% or less, more preferably 1.20% or less. The lower limit of the Cu content is preferably 0.10%, more preferably 0.50%.

[0044] V: 0.01 to 0.50% Vanadium (V) is an element that enhances the strength of alloys by finely precipitating within grains as carbides, nitrides, or carbonitrides. It also has the effect of refining crystal grains by pinning grain boundaries. Furthermore, V increases the solubility of N in alloys, thereby suppressing the occurrence of pinholes near the surface when the N content is increased to enhance alloy strength. However, excessive V content results in excessive precipitates, which not only reduces toughness but also increases the risk of weld cracking in the heat-affected zone. Therefore, the V content is 0.01 to 0.50%. The preferred lower limit of the V content is 0.02%, more preferably 0.03%. The preferred upper limit of the V content is 0.35%, more preferably 0.20%.

[0045] Nb + Ti: 0.002 to 1.000% Niobium (Nb) and titanium (Ti) are elements that enhance the strength of alloys by finely precipitating within grains as carbides, nitrides, or carbonitrides. They also have the effect of refining crystal grains by pinning grain boundaries. Nb and Ti further increase the solubility of N in alloys, thereby suppressing the occurrence of pinholes near the surface when the N content is increased to increase the alloy strength. However, excessive Nb and / or Ti leads to excessive precipitates, which not only reduces toughness but also increases the risk of weld cracking in the heat-affected zone. Therefore, one or both of Nb and Ti are contained, and their total content is 0.002 to 1.000%. The preferred lower limit of the total content is 0.010%, more preferably 0.030%. The preferred upper limit of the total content is 0.500%, more preferably 0.300%.

[0046] Al: 0.001 to 0.500% Aluminum (Al) is an element that has the effect of deoxidizing the alloy. However, excessive Al content impairs cleanliness and deteriorates workability and ductility. Therefore, the Al content is 0.001 to 0.500%. A preferred lower limit of the Al content is 0.005%, more preferably 0.010%. A preferred upper limit of the Al content is 0.300%, more preferably 0.100%. In the present invention, the Al content refers to the content of acid-soluble Al (so-called "sol. Al").

[0047] N: 0.005 to 0.400% Nitrogen (N) increases the strength of an alloy through solid-solution strengthening. Adding N and performing solution heat treatment results in a high-strength alloy pipe. Using a high-strength alloy pipe allows the desired strength to be achieved in the cold-worked alloy pipe, even with low cold working. However, excessive N content can easily cause pinholes to form near the surface during solidification of the alloy. Furthermore, N reduces the hot workability of the alloy. Therefore, the N content is 0.005 to 0.400%. The preferred lower limit of the N content is 0.010%, more preferably 0.030%, and even more preferably 0.060%. The preferred upper limit of the N content is 0.350%, more preferably 0.300%.

[0048] In addition to the above elements, the Cr—Ni alloy tube according to this embodiment may further contain one or more elements selected from W, Co, Sn, As, Zn, Pb, Sb, B, Ca, Mg, and REM. There is no need to set a lower limit for the content of any of the elements, and the content may be 0%.

[0049] W: 0 to 1.00% Tungsten (W) is an optional element. Therefore, W does not have to be contained. W has the effect of increasing SCC resistance, so it may be contained as needed. However, if W is contained in excess, this effect saturates and the hot workability deteriorates. Therefore, the W content is 1.00% or less. The W content is preferably 0.50% or less, and more preferably 0.30% or less. The lower limit of the W content is preferably 0.01%, and more preferably 0.05%.

[0050] Co: 0 to 1.00% Cobalt (Co) is an optional element. Therefore, Co does not have to be contained. Like Ni, Co has the effect of increasing the stability of the austenite phase, so it may be contained as needed. However, since Co is an extremely expensive element, a high content of Co leads to an increase in costs. Therefore, the Co content is 1.00% or less. The preferred Co content is 0.50% or less, and more preferably 0.30% or less. The preferred lower limit of the Co content is 0.01%, and more preferably 0.05%.

[0051] Sn: 0 to 0.010% Tin (Sn) is an optional element. Therefore, Sn does not have to be contained. Sn has the effect of affecting convection in the molten pool during welding, increasing the penetration depth, and improving weldability, so it may be contained as needed. However, excessive Sn not only increases weld cracking susceptibility but also reduces corrosion resistance. Therefore, the Sn content is 0.010% or less. The preferred Sn content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Sn content is 0.001%, and more preferably 0.002%.

[0052] As: 0 to 0.010% Arsenic (As) is an optional element. Therefore, As does not have to be contained. As has the effect of affecting convection in the molten pool during welding, increasing penetration depth, and improving weldability, so it may be contained as needed. However, excessive As content not only increases weld cracking susceptibility but also reduces corrosion resistance. Therefore, the As content is 0.010% or less. The preferred As content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the As content is 0.001%, and more preferably 0.002%.

[0053] Zn: 0 to 0.010% Zinc (Zn) is an optional element. Therefore, Zn does not have to be contained. Zn has the effect of affecting convection in the molten pool during welding, increasing penetration depth, and improving weldability, so it may be contained as needed. However, excessive Zn not only increases weld cracking susceptibility but also reduces corrosion resistance. Therefore, the Zn content is 0.010% or less. The preferred Zn content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Zn content is 0.001%, and more preferably 0.002%.

[0054] Pb: 0 to 0.010% Lead (Pb) is an optional element. Therefore, Pb does not have to be contained. Pb affects the convection of the molten pool during welding, increases the penetration depth, and improves weldability, so it may be contained as needed. However, excessive Pb not only increases weld cracking susceptibility but also reduces corrosion resistance. Therefore, the Pb content is 0.010% or less. The preferred Pb content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Pb content is 0.0005%, and more preferably 0.001%.

[0055] Sb: 0 to 0.010% Antimony (Sb) is an optional element. Therefore, Sb does not have to be contained. Sb has the effect of affecting convection in the molten pool during welding, increasing the penetration depth, and improving weldability, so it may be contained as needed. However, excessive Sb not only increases weld cracking susceptibility but also reduces corrosion resistance. Therefore, the Sb content is 0.010% or less. The preferred Sb content is 0.008% or less, and more preferably 0.006% or less. The preferred lower limit of the Sb content is 0.0005%, and more preferably 0.001%.

[0056] B: 0 to 0.0050% Boron (B) is an optional element. Therefore, B does not have to be contained. B is an element that contributes to grain boundary strengthening and improves hot workability, so it may be contained as needed. However, if B is contained in excess, the effect saturates, and further, liquation cracking occurs at the grain boundaries of the heat-affected zone during welding. Therefore, the B content is 0.0050% or less. The preferred B content is 0.0030% or less, and more preferably 0.0015% or less. The preferred lower limit of the B content is 0.0001%, and more preferably 0.0003%.

[0057] Ca: 0 to 0.0200% Calcium (Ca) is an optional element. Therefore, Ca does not necessarily have to be contained. Ca has the effect of fixing S as sulfides and improving the hot workability of the alloy, so it may be contained as needed. However, if Ca is contained in excess, coarse oxides are formed, which actually reduces the hot workability of the alloy. Therefore, the Ca content is 0.0200% or less. The preferred Ca content is 0.0100% or less, and more preferably 0.0050% or less. The preferred lower limit of the Ca content is 0.0005%, and more preferably 0.0010%.

[0058] Mg: 0 to 0.0200% Magnesium (Mg) is an optional element. Therefore, Mg does not necessarily need to be contained. Like Ca, Mg has the effect of fixing S as sulfides and improving the hot workability of the alloy, so it may be contained as needed. However, if Mg is contained in excess, coarse oxides are formed, which actually reduces the hot workability of the alloy. Therefore, the Mg content is 0.0200% or less. The preferred Mg content is 0.0100% or less, more preferably 0.0050% or less, and even more preferably 0.0020% or less. The preferred lower limit of the Mg content is 0.0001%, more preferably 0.0005%.

[0059] REM: 0 to 0.100% Rare earth elements (REM) are optional elements. Therefore, REM may not be included. Like Ca and Mg, REM has the effect of fixing S as sulfides and improving the hot workability of the alloy, so it may be included as needed. However, if REM is included in excess, coarse oxides are formed, which actually reduces the hot workability of the alloy. Therefore, the REM content is 0.100% or less. The preferred REM content is 0.050% or less, and more preferably 0.030% or less. The preferred lower limit of the REM content is 0.001%, and more preferably 0.005%.

[0060] In this embodiment, "REM" refers to a total of 17 elements, including Sc, Y, and lanthanides, and "REM content" refers to the content of one type of REM when there is one type of REM, and to the total content of two or more types of REM when there are two or more types of REM. REM is also generally supplied as misch metal, which is an alloy of multiple types of REM. Therefore, one or more individual elements may be added, or they may be added in the form of misch metal, for example.

[0061] The Cr—Ni alloy tube according to this embodiment contains the above-mentioned elements, with the balance being Fe and impurities. Here, the term “impurities” refers to components that are mixed in due to various factors in raw materials such as ores and scraps, or in the manufacturing process, when industrially manufacturing alloy materials, and are acceptable within a range that does not adversely affect the present invention.

[0062] The chemical composition of the Cr-Ni alloy tube according to this embodiment preferably further satisfies the following formulas (iv) and (v): 9Mo+100N≧45.0 (iv) Ni+1.4Cu+Mo-0.9Cr-2Si-1.2Mn-5.7C+20N+90(0.15Nb+0.27V+0.3Ti)≦42.0 (v) Note that the element symbols in the above formulas indicate the content (mass%) of each element, and zero is substituted if the element is not contained.

[0063] The present inventors analyzed the relationship between the mechanical properties and chemical composition of various Cr-Ni alloy pipes, and as a result, it became clear that in the above chemical composition, Mo and N particularly contribute to the base strength. It was also found that by satisfying the above formula (iv), a stable high base strength can be obtained.

[0064] It is not necessary to set an upper limit to the value of 9Mo+100N, but from the viewpoint of suppressing a decrease in hot workability, it is preferably 85.0 or less, and more preferably 83.0 or less.

[0065] In addition, by focusing on elements that affect stacking fault energy and analyzing the relationship between mechanical properties and chemical composition, it was found that stable and excellent work hardening ability can be obtained by satisfying the above formula (v).

[0066] There is no need to set a lower limit for the value on the left side of formula (v), and the lower the value, the better. However, considering the range of the content of each element, the substantial lower limit is 1.2.

[0067] The chemical composition of the Cr-Ni alloy tube according to this embodiment preferably further satisfies the following formula (vi). As mentioned above, anisotropy tends to increase when the degree of cold working is high. However, by adjusting the N content so as to satisfy the following formula (vi) in relation to the tensile yield stress in the axial direction of the Cr-Ni alloy tube, it becomes easier to suppress an increase in anisotropy even when the tube has a strength of 900 MPa or more. 0.001×YS LT -0.820<N<0.001×YS LT -0.740...(vi) YS LC : Compressive yield stress in the tube axial direction (MPa) N: N content in the alloy tube (mass%)

[0068] 3. Manufacturing Method An example of a method for manufacturing the Cr—Ni alloy pipe according to this embodiment will be described.

[0069] First, a molten austenitic alloy is melted to produce a molten metal. 2 A mixed gas bottom blown decarburization furnace (AOD furnace), a vacuum decarburization furnace (VOD furnace), etc. can be used.

[0070] The molten metal is then used to produce a casting material, such as an ingot, a slab, or a bloom. Specifically, an ingot is produced by an ingot casting method, or a slab or a bloom is produced by a continuous casting method.

[0071] Next, the cast material is hot worked to produce a round billet. Hot working is, for example, hot rolling or hot forging. The produced round billet is then hot worked to produce a mother pipe. Specifically, a mother pipe is produced from the round billet by an extrusion pipe-making method, such as the Ugine-Séjournet process. Alternatively, a mother pipe is produced from the round billet by the Mannesmann pipe-making process.

[0072] The produced mother pipe is subjected to cold working. Cold working includes cold drawing and cold rolling, typified by pilger rolling. Either cold drawing or cold rolling may be employed in the present invention. Cold drawing imparts a larger tensile strain to the alloy pipe in the axial direction than cold rolling. Cold rolling imparts a larger strain to the mother pipe not only in the axial direction but also in the circumferential direction. Therefore, cold rolling imparts a larger compressive strain to the mother pipe in the circumferential direction than cold drawing.

[0073] The preferred area reduction rate during cold working is 15% or more. Here, the area reduction rate is defined by the following formula (I). The preferred lower limit of the area reduction rate is 20%. On the other hand, if the area reduction rate is too high, not only will the roundness of the alloy pipe decrease, but the anisotropy will become significant. Therefore, the preferred upper limit of the area reduction rate during cold working is 50%. Area reduction rate (%) = 100 x (cross-sectional area of ​​mother pipe before cold working - cross-sectional area of ​​mother pipe after cold working) / cross-sectional area of ​​mother pipe before cold working (I)

[0074] Other treatments may be performed between the hot working and the cold working. For example, a solution heat treatment may be performed on the hot-worked mother pipe. In this case, the mother pipe after the solution heat treatment is descaled to remove scale, and then cold working is performed. Furthermore, cold working may be performed multiple times. When cold working is performed multiple times, solution heat treatment may be performed as a softening heat treatment between cold working and the next cold working.

[0075] Furthermore, after cold working, in order to reduce anisotropy, straightening processing using an inclined roll straightener and / or low-temperature heat treatment may be performed. Either straightening processing or low-temperature heat treatment may be performed first. However, if the heat treatment temperature is too high, the yield stress will be excessively reduced, making it impossible to maintain the strength required in the usage environment. Therefore, when low-temperature heat treatment is performed, the heating temperature should be 300 to 550°C, and preferably 400 to 500°C.

[0076] There are no particular restrictions on the dimensions of the alloy pipe obtained by the above process, but from the viewpoint of maintaining the strength required in the usage environment, the wall thickness of the alloy pipe is preferably 4 mm or more, more preferably 6 mm or more, even more preferably 8 mm or more, and even more preferably 10 mm or more.

[0077] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.

[0078] An alloy having the chemical composition shown in Table 1 was melted and cast in a vacuum to obtain an ingot weighing 30 kg and having an outer diameter of 120 mm. This ingot was hot forged to a thickness of 50 mm. The temperature of the ingot before hot forging was 1200°C. Furthermore, the material was hot rolled. In this case, in order to change the product strength, the cold working ratio shown in Table 2 was applied, and the thickness of the intermediate alloy material (alloy plate) was determined by back-calculation so that the thickness after cold rolling was standardized to 11.5 mm. Subsequently, a softening heat treatment was performed by heat treatment for 10 minutes at the temperature shown in Table 2 followed by water cooling. Subsequently, the cold working ratio shown in Table 2 was applied to standardize the thickness to 11.5 mm. Tests Nos. 22 and 23 were further subjected to a solution heat treatment by heat treatment for 10 minutes at the temperature shown in Table 2 followed by water cooling after cold working. Test No. 24 was not subjected to cold working. In this example, an alloy plate was used instead of an alloy pipe in order to facilitate the experiment.

[0079]

[0080]

[0081] Next, the compressive yield stress YS in the tube axial direction is measured by the above-mentioned method. LC (MPa) and tensile yield stress YS LT (MPa) was determined. Specifically, cylindrical test pieces for compression tests and round bar test pieces for tensile tests were taken from the center of the plate thickness of the alloy plate of each test number so that the longitudinal direction was parallel to the rolling direction. The cylindrical test pieces had a parallel part diameter of 4 mm and a length of 8 mm. The round bar test pieces had a parallel part diameter of 4 mm and a gauge length of 20 mm. A compression test was performed on the cylindrical test pieces for compression tests in air at room temperature (25°C) using a method in accordance with ASTM E9 (2019). The 0.2% offset proof stress obtained by the compression test was used as the compressive yield stress YS in the axial direction of the tube. LC Furthermore, a tensile test was carried out on the round bar test specimens at room temperature (25°C) in the air in accordance with ASTM E8 / E8M (2013). The 0.2% offset yield strength obtained by the tensile test was used as the tensile yield stress YS in the axial direction of the pipe. LT (MPa).

[0082] Furthermore, the tensile yield stress YS of the test piece after high-frequency induction heating and rapid cooling was measured by the above-mentioned method. HT The strain (MPa) was determined. Specifically, a cylindrical test piece for high-frequency induction heating and quenching was taken from the center of the plate thickness of each alloy plate with each test number, with the longitudinal direction parallel to the rolling direction. The cylindrical test piece was prepared in accordance with ASTM E8 / E8M (2021) and had a diameter of 6 mm and a gauge length of 30 mm. The cylindrical test piece for high-frequency induction heating and quenching was heated from room temperature to 1150 ° C at a heating rate of 100 ° C / s using a high-frequency induction heating device, and then heated to 1200 ° C at a heating rate of 25 ° C / s. At this time, the heating region by the high-frequency induction heating device was a region of 3.5 mm from the center of the test piece to both ends in the longitudinal direction and 7.0 mm in the longitudinal direction. The temperature of the test piece was measured using a thermocouple installed in the center of the test piece in the longitudinal direction.

[0083] The test specimen was then held at 1200°C for 180 seconds. Immediately after holding, Ar gas was sprayed onto the specimen, and the specimen was rapidly cooled to room temperature at a cooling rate of 50°C / s in the temperature range from 1200°C to 800°C. Then, using the test specimen after high-frequency induction heating and rapid cooling, a tensile test was carried out in air at room temperature (25°C) in accordance with JIS Z 2241 (2011), and the obtained 0.2% offset proof stress was used as the tensile yield stress YS of the test specimen after high-frequency induction heating and rapid cooling. HT (MPa).

[0084] The results are also shown in Table 2. As shown in Table 2, alloy materials that satisfy all the requirements of the present invention have a high tensile yield stress of 780 MPa or more and a YS LC / YS LT It is possible to set the value to 0.80 or more.

[0085] According to the present invention, a Cr—Ni alloy pipe having high strength can be obtained while minimizing the difference between the compressive yield stress and the tensile yield stress. Therefore, by selecting the Cr—Ni alloy pipe according to the present invention as a material for oil country tubular goods, it is possible to obtain highly reliable oil country tubular goods that can maintain high strength even when softening occurs at the weld.

Claims

1. A Cr-Ni alloy tube, comprising: a tensile yield stress YS in the tube axis direction of the Cr-Ni alloy tube; LT and compressive yield stress YS LC The tensile yield stress YS of a test piece obtained by taking a specimen from the center position of the wall thickness of the Cr-Ni alloy pipe so that the longitudinal direction is parallel to the tube axis direction, heating the specimen from room temperature to 1150°C at a heating rate of 100°C / s using a high-frequency induction heating device, subsequently heating the specimen to 1200°C at a heating rate of 25°C / s, holding the specimen at 1200°C for 180 seconds, and then quenching the specimen to room temperature under conditions in which the cooling rate in the temperature range from 1200°C to 800°C is 50°C / s by blowing Ar gas. HT A Cr-Ni alloy tube that satisfies the following formulas (i) to (iii): 0.80≦YS LC / Y.S. LT <0.95...(i) YS HT -0.24 x YS LT ≧50.0...(ii) YS LT ≧443×YS LT / Y.S. LC +2.28 x YS HT −350 (iii) where the symbols in the above formula have the following meanings: LC : Compressive yield stress in the tube axial direction (MPa) YS LT : Tensile yield stress in the tube axial direction (MPa) YS HT : Tensile yield stress (MPa) of the test piece after high-frequency induction heating and quenching 2. Tensile yield stress YS in the axial direction of the Cr-Ni alloy tube LT The Cr-Ni alloy tube according to claim 1, wherein the strain is 780 MPa or more.

3. Chemical composition, by mass%, is: C: 0.030% or less, Si: 0.50% or less, Mn: 1.00% or less, P: 0.030% or less, S: 0.0050% or less, Cr: 19.00-32.00%, Ni: 29.50-55.00%, Mo: 2.50-12.00%, Cu: 3.00% or less, V: 0.01-0.50%, Nb+Ti: 0.002-1.000%, Al: 0.001-0.500%, N: 0.005-0.400%, W: 0-1.00%, Co: 0-1.00%, Sn: 0-0.010%, As: 0-0.010%, 3. The Cr-Ni alloy tube according to claim 1, comprising: Zn: 0-0.010%, Pb: 0-0.010%, Sb: 0-0.010%, B: 0-0.0050%, Ca: 0-0.0200%, Mg: 0-0.0200%, REM: 0-0.100%, and the balance being Fe and impurities.

4. The Cr-Ni alloy tube according to claim 3, wherein the chemical composition contains, in mass%, one or more selected from W: 0.01-1.00%, Co: 0.01-1.00%, Sn: 0.001-0.010%, As: 0.001-0.010%, Zn: 0.001-0.010%, Pb: 0.0005-0.010%, Sb: 0.0005-0.010%, B: 0.0001-0.0050%, Ca: 0.0005-0.0200%, Mg: 0.0001-0.0200%, and REM: 0.001-0.100%.

5. The Cr-Ni alloy tube according to claim 3 or 4, wherein the chemical composition further satisfies the following formulas (iv) and (v): 9Mo+100N≧45.0 ... (iv) Ni+1.4Cu+Mo-0.9Cr-2Si-1.2Mn-5.7C+20N+90(0.15Nb+0.27V+0.3Ti)≦42.0 ... (v) where the element symbols in the above formulas indicate the content (mass%) of each element in the alloy tube, and zero is substituted if the element is not contained.

6. The Cr-Ni alloy tube according to any one of claims 3 to 5, wherein the chemical composition further satisfies the following formula (vi): 0.001×YS LT -0.820<N<0.001×YS LT −0.740 (vi) where the symbols in the above formula have the following meanings: YS LC : Compressive yield stress in the tube axial direction (MPa) N: N content in the alloy tube (mass%)

Citation Information

Patent Citations

  • ANTICORROSIVE ALLOY OF HIGH Ni EXCELLENT IN INTERGRANULAR CORROSION RESISTANCE OR CORROSION RESISTANCE, AND EXCELLENT IN HOT WORKABILITY AND COLD WORKABILITY

    JP2020094235A

  • Austenite system alloy pipe and manufacturing method thereof

    WO2012128258A1

  • Austenitic alloy pipe and method for manufacturing same

    WO2018225869A1

  • Alloy material and seamless pipe for oil well

    WO2021070735A1

  • Alloy pipe and method for manufacturing same

    WO2021256128A1