Method for manufacturing all-solid-state battery

The method of exposing the electrode laminate to a controlled environment and press-molding alleviates warping issues, ensuring stable battery characteristics and durability in all-solid-state batteries.

WO2024202311A1PCT designated stage expired Publication Date: 2024-10-03AESC JAPAN LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/045250
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-12-18
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

All-solid-state batteries face challenges in maintaining stable battery characteristics and durability due to warping of the electrode stack during the manufacturing process, which is exacerbated by exposure to moisture despite dew point control measures.

Method used

The method involves laminating a negative electrode, a solid electrolyte membrane, and a positive electrode to form an electrode laminate, then exposing it to an environment with a dew point of −40° C and water concentration of 127 ppm or less for 20 minutes or more, followed by press-molding to prevent warping and maintain ionic conductivity.

Benefits of technology

This approach results in a high-quality all-solid-state battery with stable electrical properties and durability, suppressing decreases in ionic conductivity and warping issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023045250_03102024_PF_FP_ABST
    Figure JP2023045250_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for manufacturing an all-solid-state battery with which warping of an electrode multilayer body is prevented, and deterioration of characteristics does not occur. The present invention provides a method for manufacturing an all-solid-state battery, the method comprising: a step for forming an electrode multilayer body by stacking a negative electrode, a positive electrode and a solid electrolyte membrane; a step for exposing the electrode multilayer body to an environment having a dew point temperature of -40°C and a moisture concentration of 127 ppm or less for 20 minutes or more; and a step for press molding the electrode multilayer body.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method for all-solid-state batteries

[0001] The present invention relates to a method for producing an all-solid-state electrolyte. The all-solid-state battery of the present invention includes a lithium-ion secondary battery.

[0002] In recent years, due to environmental considerations, development of secondary batteries that can be repeatedly charged and discharged has been progressing as an energy source for automobiles and homes. While the development of secondary batteries that can be expected to have high capacity and high output is expected, at the same time, greater emphasis must be placed on safety.

[0003] Among typical secondary batteries, lithium-ion secondary batteries, solid-state batteries using a solid electrolyte are known. An all-solid-state battery, which is one type of solid-state battery, includes a solid electrolyte layer, a positive electrode layer formed on one side of the solid electrolyte layer, a negative electrode layer formed on the other side, a positive electrode plate connected to the positive electrode layer, and a negative electrode plate connected to the negative electrode layer.

[0004] The positive electrode layer can be obtained by coating a positive electrode current collector with a slurry containing positive electrode active material particles, a binder, a solid electrolyte, and a solvent, followed by drying. Aluminum foil or the like can be used as the positive electrode current collector. On the other hand, the negative electrode can be obtained by coating a negative electrode current collector with a slurry containing negative electrode active material particles, a binder, a solid electrolyte, and a solvent, followed by drying. Copper foil can be used as the negative electrode current collector. Alternatively, a lithium metal layer formed on stainless steel foil can also be used as the negative electrode. The positive electrode layer or negative electrode layer can further contain a conductive additive.

[0005] The solid electrolyte layer can be formed by dispersing a solid electrolyte powder in a solvent to form a slurry, which is then applied and dried. For example, the solid electrolyte layer can be formed directly on the surface of the negative electrode layer or the positive electrode layer. Alternatively, the solid electrolyte layer can be formed on the surface of a substrate such as a polyethylene terephthalate (PET) film, and then the PET film can be peeled off.

[0006] The resulting positive and negative electrodes are stacked with a solid electrolyte sandwiched between them and pressurized to obtain an electrode laminate. A positive electrode terminal and a negative electrode terminal are attached to this electrode laminate, and the resultant is housed in an outer container and sealed so that one end of each terminal extends to the outside, thereby obtaining an all-solid-state battery.

[0007] A sulfide solid electrolyte is known as a solid electrolyte. It is known that sulfide solid electrolytes are chemically unstable and that their ionic conductivity decreases due to moisture when exposed to the atmosphere. Therefore, when using a sulfide solid electrolyte, the positive electrode or negative electrode active material and the solid electrolyte material itself are sufficiently dried in advance, and further, the dew point is strictly controlled during the lamination process of the positive electrode, negative electrode, and solid electrolyte layer, so that assembly can be carried out quickly under a low moisture concentration.

[0008] Patent Document 1 discloses that in a slurry drying step for forming an electrode layer of an all-solid-state battery, drying is performed in an atmosphere with a volatile organic compound concentration of 100 ppm or less. Patent Document 2 discloses that a lithium ion conductive solid electrolyte is dried by heating in a temperature range of 80°C to 140°C.

[0009] JP 2019-200890 A JP 2008-103145 A

[0010] Even if an all-solid-state battery is assembled under dew point control, it is difficult to completely block exposure to moisture, so it is considered desirable to complete the process up to the stage of sealing the electrode stack in an outer container as quickly as possible. However, no matter how quickly the all-solid-state battery is assembled, the characteristics of the all-solid-state battery may deteriorate.

[0011] As a result of intensive research, the inventors have found that an all-solid-state battery with stable battery characteristics and durability cannot be obtained without further improvements to the manufacturing process of an electrode stack including a positive electrode, a solid electrolyte membrane, and a negative electrode. Specifically, there is a problem that the electrodes including the positive electrode and the negative electrode and the solid electrolyte membrane may warp due to the process of pressing them under high pressure. Simply assembling the electrode stack in a short time to prevent exposure of the solid electrolyte to moisture may not solve the problem of warping of the electrode stack.

[0012] The present invention provides a method for manufacturing an all-solid-state battery, comprising the steps of: laminating a negative electrode, a positive electrode, and a solid electrolyte membrane to form an electrode laminate; exposing the electrode laminate to an environment having a dew point temperature of −40° C. and a moisture concentration of 127 ppm or less for 20 minutes or more; and press-molding the electrode laminate.

[0013] According to the production method of the present invention, a high-quality all-solid-state battery can be obtained in which the solid electrolyte does not suffer from a decrease in ionic conductivity due to the influence of moisture, and in which the deterioration of electrical characteristics and durability due to warping of the electrode laminate is suppressed.

[0014] FIG. 1 is a flow chart showing an outline of an assembly process for an all-solid-state battery.

[0015] The following describes embodiments of the present invention, with reference to the accompanying drawings. Note that the present invention is not limited to the embodiments described below, and can be practiced within the scope of the present invention. The following is an example, and does not limit the present invention in any way.

[0016] <All-Solid-State Battery> In this specification, the term "all-solid-state battery" refers to a battery in which the electrolyte is a solid electrolyte, as described below. The term "all-solid-state battery" also includes secondary batteries and primary batteries. <Negative Electrode> The negative electrode can be any negative electrode used in non-aqueous secondary battery materials, and is not particularly limited. For example, the negative electrode includes a negative electrode current collector such as copper foil and a negative electrode layer containing a negative electrode active material and a solid electrolyte. The negative electrode layer preferably contains a binder. Alternatively, a stainless steel negative electrode current collector may be used instead of the copper foil negative electrode current collector, and a lithium metal layer may be formed on the surface of the negative electrode current collector by rolling or the like instead of the negative electrode active material. The negative electrode layer containing the negative electrode active material, solid electrolyte, and binder may be formed on at least one surface of the negative electrode current collector.

[0017] When using a negative electrode active material for the negative electrode, it is preferable to use a carbon-based active material. Examples of the carbon-based active material include natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, and any mixture thereof. Natural graphite includes natural graphite particles coated with amorphous carbon, while artificial graphite includes artificial graphite particles coated with amorphous carbon. These natural graphite and artificial graphite particles can be primary particles, particles formed by agglomeration of primary particles to form secondary particles, or mixtures thereof. Alternatively, a mixture of a carbon-based active material and a silicon-based active material may be used as the negative electrode active material. The negative electrode active material may also include metal materials such as aluminum, silver, bismuth, calcium, cerium, indium, magnesium, tin, zinc, and nickel.

[0018] Examples of binders used in the negative electrode layer include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF), conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles, synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR), and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin. Furthermore, examples of binders that can be used include polyacrylic acid, polymethacrylic acid, sodium polyacrylate, potassium polyacrylate, sodium polymethacrylate, potassium polymethacrylate, ethyl polyacrylate, ethyl polyacrylate, butyl polyacrylate, methyl polymethacrylate, ethyl polymethacrylate, butyl polymethacrylate, and any mixtures thereof. The binder content is preferably 1% by mass or more and less than 10% by mass of the total solid content of the negative electrode layer. If the binder content is too high, a large portion of the negative electrode active material surface will be covered with the binder, which may result in a decrease in ionic conductivity and electronic conductivity. If the binder content is too low, there is a risk that the negative electrode active material particles will not properly contact each other electrically.

[0019] In addition to the above compounds, the binder component may further include carboxymethyl cellulose (referred to as "CMC"), which is a cellulose derivative, or a metal salt of carboxymethyl cellulose (e.g., sodium carboxymethyl cellulose, potassium carboxymethyl cellulose). When CMC or a metal salt of CMC is further added as a binder component, the content of CMC or the CMC metal salt is preferably 0.05 mass% or more and 1.5 mass% or less with respect to the total solid content of the negative electrode layer.

[0020] The negative electrode layer may further contain a conductive additive. The conductive additive is a material for reducing the resistance of the electrode. Examples of the conductive additive include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, carbon nanotubes, carbon nanofibers, carbon brushes, and other carbon fibers.

[0021] When carbon nanotubes or carbon nanofibers are used as the conductive additive, the content of these conductive additives is 0.01% by mass or more and 3% by mass or less, and preferably 0.03% by mass or more and 1% by mass or less, relative to the total solid content of the negative electrode layer.

[0022] In addition to the materials described above, the negative electrode layer may contain, as appropriate, electrode additives generally used for forming electrodes, such as thickeners, dispersants, and stabilizers.

[0023] <Solid Electrolyte Membrane> The negative electrode, solid electrolyte membrane, and positive electrode used in the manufacturing method of the embodiment include a solid electrolyte. Examples of the solid electrolyte used here include an oxide-based solid electrolyte and a sulfide-based solid electrolyte. As the oxide-based solid electrolyte, for example, a garnet-type, NASICON-type, or perovskite-type oxide-based material can be used. As the sulfide-based solid electrolyte, any known sulfide-based material can be used, for example, LiPO 4 -Li 2 S-SiS, 75% Li 2 S-25%P 2 S 5 mixture, Li 2 S-SiS 2 , Li 2 S-P 2 S 5 , Li 3 P.S. 4 , Li 3 P.O. 4 -Li 2 S-Si 2 S., Li. 3 P.O. 4 -Li 2 S-SiS 2 , LiI-Li 2 S-B 2 S 3, LiI-Li 2 S-SiS 2 , LiI-Li 2 S-P 2 S 5 , LiI-Li 2 S-P 2 O 5 , LiI-Li 3 P.O. 4 -P 2 S 5 Li 2 S-P 2 S 5 -LiCl, Li 6 P.S. 5 Cl, Li 10 GeP 2 S 12 , Li 3.25 Ge 0.25 P 0.75 S 4 and the like. In the embodiment, it is preferable to use a sulfide-based solid electrolyte. The solid electrolyte membrane used in the embodiment refers to a thin, flat surface having a predetermined area and made of a solid electrolyte. The solid electrolyte membrane may be a single layer (a solid electrolyte membrane made of one type of solid electrolyte) or a multi-layer (a solid electrolyte membrane in which two or more types of solid electrolyte membranes are stacked).

[0024] In the present invention, the solid electrolyte membrane is preferably formed to a thickness of 15 to 150 μm. If the membrane thickness is smaller than this, short circuits are likely to occur when the solid electrolyte is press-formed under high pressure. On the other hand, if the membrane thickness is larger than this, the cell volume will increase excessively, and the energy density per unit volume of the all-solid-state battery will not increase.

[0025] <Positive Electrode> The positive electrode can be any positive electrode used in non-aqueous secondary battery materials, and is not particularly limited. For example, the positive electrode includes a positive electrode current collector and a positive electrode layer containing a positive electrode active material and a solid electrolyte. The positive electrode layer preferably contains a binder. The positive electrode layer containing the positive electrode active material, the solid electrolyte, and the binder can be formed on at least one surface of the positive electrode current collector.

[0026] The positive electrode current collector can be made of stainless steel, aluminum, nickel, titanium, or a positive electrode current collector in which the surface of aluminum or stainless steel is surface-treated with carbon, nickel, titanium, or silver.

[0027] The positive electrode active material preferably contains a lithium nickel-based composite oxide as the positive electrode active material. The lithium nickel-based composite oxide is represented by the general formula Li x Ni y Me (1-y) O 2 (wherein Me is at least one metal selected from the group consisting of Al, Mn, Na, Fe, Co, Cr, Cu, Zn, Ca, K, Mg, and Pb).) The positive electrode active material may also contain a lithium-manganese composite oxide. The lithium-manganese composite oxide may be, for example, lithium manganese oxide (LiMnO 2 ), spinel-type lithium manganese oxide (LiMn 2 O 4 The positive electrode active material is particularly a material represented by the general formula Li x Ni y Co z Mn (1-y-z) O 2 It is preferable that the cathode active material contains a lithium nickel manganese cobalt composite oxide having a layered crystal structure represented by the formula: where x in the general formula is 1≦x≦1.2, y and z are positive numbers satisfying y+z<1, and the value of y is 0.5 or greater. In order to obtain a high-capacity battery, it is particularly preferable that y>1-y-z and y>z. The lithium nickel composite oxide having this general formula is a lithium nickel cobalt manganese composite oxide. The lithium nickel cobalt manganese composite oxide is a lithium nickel composite oxide that is suitably used to increase the capacity of a battery. In addition, the cathode active material is a lithium nickel manganese composite oxide having the general formula LiMPO 4 (M is at least one selected from the group consisting of Mn, Fe, Co, and Ni). 3The buffer layer may be formed by coating the positive electrode layer with a material such as a fluorine-containing compound. The buffer layer can be formed to a thickness of 10 nm or less, thereby suppressing the interfacial resistance between the positive electrode layer and the solid electrolyte membrane. The buffer layer can be formed on the surface of the positive electrode layer by a sol-gel method or the like.

[0028] Examples of the binder that forms the positive electrode layer together with the positive electrode active material include fluororesins such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and polyvinyl fluoride (PVF); conductive polymers such as polyanilines, polythiophenes, polyacetylenes, and polypyrroles; synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), chloroprene rubber (CR), isoprene rubber (IR), and acrylonitrile butadiene rubber (NBR); and polysaccharides such as carboxymethyl cellulose (CMC), xanthan gum, guar gum, and pectin.

[0029] The positive electrode layer may also contain a conductive additive. Examples of the conductive additive include carbon black such as acetylene black and ketjen black, activated carbon, graphite, mesoporous carbon, fullerenes, and carbon fibers such as carbon nanofibers, carbon nanotubes, and carbon nanobrushes. In addition, electrode additives commonly used for electrode formation, such as thickeners, dispersants, and stabilizers, can be appropriately used in the positive electrode layer.

[0030] <Cell Creation> First, we will explain how to create the negative electrode. There are several methods for creating the negative electrode. Regardless of the method used, it is preferable to create the negative electrode in a low-moisture environment under dew point control in order to prevent water from being adsorbed onto the solid electrolyte.

[0031] <Preparation of Negative Electrode> When using a negative electrode in which a negative electrode active material is formed on a negative electrode current collector, a slurry in which the negative electrode active material, solid electrolyte, and binder are dispersed in a dehydrated organic solvent is applied to a portion or all of the surface of a negative electrode current collector such as copper foil, followed by drying to obtain a negative electrode precursor sheet. The obtained negative electrode precursor sheet is compressed using a press molding method such as a roll press, a uniaxial press, a rubber press, or an isostatic press (cold isostatic pressing [CIP] or warm isostatic pressing [WIP], with cold isostatic pressing being particularly preferred), to obtain a negative electrode sheet. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, all of which are preferably dehydrated.

[0032] Alternatively, a negative electrode precursor sheet can be obtained by transferring granules of the negative electrode active material, including at least the negative electrode active material, solid electrolyte, and binder, to a negative electrode current collector. A surface layer containing a polymer component, such as a binder, that enhances adhesion to the granules of the negative electrode active material may be preformed on the surface of the negative electrode current collector. The negative electrode layer may also contain a conductive additive. The resulting negative electrode precursor sheet can be compressed using a press molding method such as a roll press, uniaxial press, rubber press, or isostatic pressing (CIP, WIP) to obtain a negative electrode sheet.

[0033] Alternatively, a metallic lithium layer such as lithium foil is placed on a part or all of a stainless steel negative electrode current collector, and these are then adhered together by rolling or the like to obtain a negative electrode sheet.

[0034] <Preparation of Solid Electrolyte Membrane> Next, a solid electrolyte membrane is formed on the surface of the negative electrode. Regardless of the method used to form the solid electrolyte membrane, it is preferable to prepare it in a low-moisture environment under dew point control in order to prevent moisture from being adsorbed onto the solid electrolyte.

[0035] A solid electrolyte film can be formed on the surface of the negative electrode by applying a slurry of a solid electrolyte dispersed in an organic solvent to the surface of a negative electrode layer formed on a copper foil or the surface of metallic lithium formed on a stainless steel foil and drying it. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, and it is preferable that all of them be dehydrated.

[0036] Alternatively, a solid electrolyte film can be formed on the surface of the negative electrode by applying a slurry in which a solid electrolyte is dispersed in an organic solvent to the surface of a polyester film containing polyester as the main component, drying the applied slurry, and then laminating the polyester film together with the polyester film so that the solid electrolyte film is in contact with the surface of the negative electrode layer or the surface of metallic lithium.

[0037] The laminated negative electrode and solid electrolyte membrane are compressed by a press molding method such as a roll press, a uniaxial press, a rubber press, or an isostatic press (CIP, WIP), to obtain a negative electrode-solid electrolyte membrane laminate. When the solid electrolyte is laminated together with a polyester sheet and pressurized, the polyester film is peeled off from the solid electrolyte membrane. In this case, it is also preferable to use a polyester film whose surface is coated with a release agent such as silicone, so that the polyester film can be easily peeled off from the solid electrolyte membrane.

[0038] <Preparation of Positive Electrode> Next, the preparation of the positive electrode will be described. Whichever method is used to prepare the positive electrode, it is preferable to prepare it in a low moisture environment under dew point control in order to suppress moisture adsorption.

[0039] A cathode sheet is obtained by dispersing a cathode active material, a solid electrolyte, and a binder in a dehydrated organic solvent, coating the resulting slurry on part or all of the surface of a cathode current collector such as aluminum, and then drying. Examples of organic solvents include acetonitrile, xylene, dimethoxyethane, dimethyl carbonate, tertiary amine solvents such as triethylamine, heptane, hexane, tetrahydrofuran, toluene, and N-methylpyrrolidone, as well as ether solvents, thiol solvents, and butyl butyrate, all of which are preferably dehydrated.

[0040] <Formation of Electrode Stack> A positive electrode sheet is laminated on a negative electrode-solid electrolyte membrane stack to obtain an electrode stack precursor. When a sulfide solid electrolyte is used as the solid electrolyte, exposure to moisture reduces the ionic conductivity of the solid electrolyte. Therefore, after obtaining the electrode stack precursor, it is desirable to compress the electrode stack precursor by a method such as roll pressing, uniaxial pressing, rubber pressing, or isostatic pressing (CIP, WIP) within a predetermined time to obtain an electrode stack. The predetermined time is, for example, within two days in an environment with a dew point of −40°C and a moisture concentration of 127 ppm or less. If a longer time has passed, there is a risk of performance degradation due to water absorption by the solid electrolyte, which is undesirable from the viewpoint of reducing the productivity of all-solid-state batteries.

[0041] The positive electrode can be first roll-pressed in the form of a thin sheet consisting of only a positive electrode layer formed on a positive electrode current collector, and then laminated onto the anode-solid electrolyte membrane laminate. Alternatively, from the viewpoint of production efficiency, the positive electrode sheet can be placed on the anode-solid electrolyte membrane laminate without applying pressure to the positive electrode sheet alone, or with only enough pressure to press the positive electrode sheet with the conveying arm of the laminator. This step is the step immediately before the isostatic pressing to form the electrode laminate.

[0042] When a positive electrode sheet is roll-pressed, the voids in the positive electrode active material and solid electrolyte are initially crushed, but the positive electrode is distorted by springback when the pressure applied to the compact is released. Because the positive electrode is extremely thin, it tends to warp immediately after pressing. However, if the positive electrode sheet is placed on the negative electrode-solid electrolyte membrane laminate in this state and then isostatically pressed immediately, the effects of springback will become significant after the electrode laminate is formed, potentially affecting battery performance, such as causing fine peeling at the interface between the positive electrode sheet and the solid electrolyte membrane.

[0043] On the other hand, if an attempt is made to laminate a positive electrode sheet onto an anode-solid electrolyte membrane laminate without applying substantial pressure to the positive electrode sheet and then perform isostatic pressing, the positive electrode sheet tends to warp due to the influence of gas present in the voids in the positive electrode layer when the laminate is vacuum-sealed as a pretreatment for isostatic pressing. In this case, the warping of the positive electrode also affects the electrode laminate, which may affect the electrode laminate and battery characteristics.

[0044] Therefore, it is preferable to leave a predetermined time or more between laminating the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate and performing press molding. In this way, the influence of warping of the positive electrode is mitigated, and distortion after isostatic pressing can be reduced. The predetermined time is, for example, 20 minutes or more in an environment with a dew point of −40°C and a moisture concentration of 127 ppm or less. This makes it possible to mitigate warping of the electrode laminate to a degree that does not cause any influence from press molding. When multiple negative electrodes, solid electrolyte membranes, and positive electrodes are stacked, it is preferable to finally stack the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate, and then perform press molding after a predetermined time has elapsed.

[0045] <Sealing of the Electrode Stack> The resulting electrode stack is desirably quickly sealed in an exterior case. One end of a rectangular metal plate serving as a negative electrode terminal is attached to the negative electrode current collector, and one end of a rectangular metal terminal serving as a positive electrode terminal is attached to the positive electrode current collector. The electrode stack is then housed in an aluminum exterior case. A resin layer, such as polyolefin, is preferably formed on at least the inner surface of the exterior case facing the electrode stack. The resin layer is heated to melt the resin and then solidified again, sealing the electrode stack in the aluminum exterior case. At this time, the other end of the positive electrode terminal and the other end of the negative electrode terminal are positioned so that they extend outside the exterior case. A layer of the same or a different type of resin as the resin used in the resin layer on the inner surface of the exterior case can be provided at the portions where the positive electrode terminal and the negative electrode terminal contact the resin layer on the inner surface of the exterior case to strengthen the adhesion of the exterior case at those locations.

[0046] A battery was fabricated according to the flow shown in the embodiment of the invention. Figure 1 is a flow diagram summarizing the embodiment of the invention.

[0047] [I] Formation of negative electrode-solid electrolyte film laminate (1) A foil (manufactured by Honjo Metals Co., Ltd.) was prepared as a negative electrode, in which a 20 μm thick metallic lithium layer was formed on the surface of a 10 μm thick stainless steel negative electrode current collector. (2) A solid electrolyte, Li, was dissolved in xylene as an organic solvent. 6 P.S. 5 A slurry containing Cl (D50: 8 μm) dispersed therein was applied to the surface of a polyester film primarily composed of polyester and dried to obtain a solid electrolyte membrane. The obtained solid electrolyte membrane was laminated together with a polyester film so as to be in contact with the surface of metallic lithium. (3) The anode-solid electrolyte membrane laminate obtained in (2) above was laminated and vacuum-sealed in a nylon vacuum pack and held at room temperature (25°C) under a pressure of 400 MPa for 1 minute. Thereafter, while still laminated and sealed, the anode-solid electrolyte membrane laminate was compressed by an isostatic pressing method to obtain an anode-solid electrolyte membrane laminate with a porosity of 7% in the anode layer. The size of the anode and solid electrolyte laminate was 50 mm × 70 mm. (4) The polyester film was peeled off from the solid electrolyte membrane to obtain an anode-solid electrolyte membrane laminate.

[0048] [II] Lamination of a positive electrode sheet and a negative electrode-solid electrolyte membrane laminate (1) LiNi as a positive electrode active material 0.8 Co 0.1 Mn 0.1 O 2 (D50: 8 μm) 70 mass % and Li as a solid electrolyte 6 P.S. 5 A slurry containing 25% by mass of Cl (average particle size 1 μm), 2% by mass of acetylene black (manufactured by Timcal Japan Co., Ltd.), and 3% by mass of styrene-butadiene rubber (SBR) as a binder dispersed in xylene, an organic solvent, was applied to a 10 μm thick aluminum foil (manufactured by UACJ Corporation) and dried to form a positive electrode layer, thereby obtaining a positive electrode. (2) The positive electrode obtained in (1) above was cut to 45 mm x 65 mm and laminated so that the positive electrode layer was in contact with the solid electrolyte membrane of the negative electrode-solid electrolyte membrane laminate prepared in [I], thereby obtaining an electrode laminate precursor. The number of stacked positive electrodes and negative electrode-solid electrolyte membrane laminates was one each.

[0049] [III] Mitigation of Warpage of Positive Electrode Sheets Until press-molding, the electrode laminate precursor obtained in [II] above was stored in a space where the atmosphere was controlled to a dew point temperature of −40° C. and a moisture concentration of 127 ppm or less. The time between laminating the last positive electrode sheet and press-molding was the time shown in Table 1 (Examples 1 to 3 and Comparative Examples 1 and 2).

[0050] [IV] Pressurization of Electrode Laminate (1) The electrode laminate precursor obtained in each Example was laminated and vacuum-sealed in a nylon vacuum pack, and held at room temperature (25° C.) under a pressure of 400 MPa for 1 minute. Next, while still laminated and sealed, the electrode laminate precursor was compressed by an isostatic pressing method to obtain an electrode laminate with a positive electrode layer having a porosity of 5%.

[0051] [V] Encapsulation into an outer case (1) The electrode laminate obtained in [IV] above was enclosed in an outer case by the method described in the embodiment, and a battery was obtained in which the positive electrode terminal and the negative electrode terminal were extended to the outside of an aluminum outer case (manufactured by Dai Nippon Printing Co., Ltd.).

[0052] The resulting battery was charged at a constant current of 0.05 C to 4.25 V, then switched to constant voltage charging, and the charging was cut off at 0.005 C. The average discharge operating voltage was then obtained when the battery was discharged at a constant current of 0.05 C to 2.5 V. Table 1 shows the average discharge operating voltages of other examples and comparative examples, with the average discharge operating voltage of Example 1 defined as 1. Furthermore, for "wrinkles after pressing" in Table 1, the electrode laminate precursor was compressed by isostatic pressing, and the resulting electrode laminate was visually observed. If wrinkles were observed, the result was rated as "present," and if no wrinkles were observed, the result was rated as "absent."

[0053] From Table 1, it can be said that it is preferable to leave a time of 20 minutes or more between the final lamination of the positive electrode sheet and the negative electrode-solid electrolyte membrane laminate and the press molding.

[0054] The examples in the present invention are merely examples and are not intended to limit the scope of the present invention. For example, an aluminum laminate film was used for the exterior case, but a strong aluminum can case or a cylindrical case may also be used. 6 P.S. 5 Although Cl is used in this invention, the present invention can be applied to any sulfide-based solid electrolyte that has low chemical stability with water. The positive and negative electrodes are pre-adjusted to a predetermined size, but they may be stacked and then quickly cut into a predetermined shape. Needless to say, other design changes are possible within the scope of the invention.

Claims

1. A method for manufacturing an all-solid-state battery, comprising: laminating a negative electrode, a positive electrode, and a solid electrolyte membrane to form an electrode laminate; exposing the electrode laminate to an environment having a dew point temperature of -40°C and a moisture concentration of 127 ppm or less for 20 minutes or more; and press-molding the electrode laminate.

2. The method for producing an all-solid-state battery according to claim 1, wherein the electrode laminate is exposed to an environment having a dew point temperature of -40°C and a moisture concentration of 127 ppm or less for 2 days or less.

3. The method for producing an all-solid-state battery according to claim 1 or 2, wherein the electrode laminate is press-molded by an isostatic pressing method.

4. The method for producing an all-solid-state battery according to claim 3, wherein the isostatic pressing method is cold isostatic pressing method.

5. The method for producing an all-solid-state battery according to any one of claims 1 to 4, wherein the solid electrolyte is a sulfide-based solid electrolyte.

Citation Information

Patent Citations

  • Battery material manufacturing method and all-solid battery

    JP2008103145A

  • Method for manufacturing electrode layer

    JP2019200890A

  • Nonaqueous electrolyte battery

    JP2013175412A

  • Method of manufacturing all solid state battery and all solid state battery

    JP2018125268A

  • All-solid state battery

    JP2020155301A